Glass ceramic solid electrolyte mixture, glass ceramic solid electrolyte and method of producing the same, and solid state battery and method of producing the same

TWI945772BActive Publication Date: 2026-11-11BELENOS CLEAN POWER HLDG
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
TW114113151
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2024-05-08
Filing Date
2025-04-08
Publication Date
2026-11-11
Estimated Expiration
2045-04-07

AI Technical Summary

Technical Problem

Conventional methods for producing inorganic-based solid electrolytes require high temperatures and long processing times, leading to high energy consumption and contact losses between electrodes, limiting the lifespan of batteries, and existing glass-ceramic synthesis methods still require impractical high sintering temperatures, resulting in low ionic conductivity at room temperature.

Method used

A glass-ceramic solid electrolyte mixture comprising borate, Li₂SO₄, and lithium halide is sintered at lower temperatures (600°C to 1000°C) to achieve high ionic conductivity (10⁻⁵ to 10⁻⁹ S/cm) between room temperature and 100°C, allowing for the assembly and sintering of anode and cathode components together, reducing energy consumption and process complexity.

Benefits of technology

The method produces a glass-ceramic solid electrolyte with improved ionic conductivity at practical temperatures, enabling the production of all-ceramic solid-state batteries with reduced energy consumption and simplified manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure TWG2TB001920524_001
    Figure TWG2TB001920524_001
  • Figure TWG2TB001920524_002
    Figure TWG2TB001920524_002
  • Figure TWG2TB001920524_003
    Figure TWG2TB001920524_003
Patent Text Reader

Abstract

This invention relates to a glass-ceramic solid electrolyte mixture comprising a glass-ceramic solid electrolyte, wherein the glass-ceramic solid electrolyte comprises a ternary glass-ceramic of borate, Li₂SO₄, and lithium halide. The invention further relates to a glass-ceramic solid electrolyte obtained from the mixture, a solid-state battery comprising the glass-ceramic solid electrolyte, and a method for producing the glass-ceramic solid electrolyte and the solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a glass-ceramic solid electrolyte and a solid-state battery comprising the glass-ceramic solid electrolyte, particularly a lithium-ion battery. The invention further relates to a method for producing the glass-ceramic solid electrolyte. [Previous Technology]

[0002] Inorganic materials, such as ceramics, are widely used in electronics, energy storage, and extreme environments due to their high thermal, mechanical, and chemical stability. The conventional synthesis of such inorganic materials typically involves solid-state reactions to form inorganic components from precursors, and sintering the inorganic components to obtain a solid (inorganic) composition. Each step typically requires high temperatures and long processing times.

[0003] Long processing times are also a problem with conventional methods for producing inorganic-based (e.g., ceramic-based) solid electrolytes (SSEs). Such SSEs are promising alternatives to liquid electrolytes, which may leak from the battery, posing safety concerns. In particular, materials such as phosphorus oxynitride and thiolated LixAl-yMyS4 (A being Si or Ge and M being P, Al, Zn, Ga, or Sb) are promising materials for SSEs exhibiting excellent ionic conductivity in the range of 10⁻⁴ S / cm. However, these materials have high production costs, particularly regarding high energy consumption due to high sintering temperatures, and note the frequent contact losses between the electrodes and the SSE after prolonged charge / discharge cycles, thus limiting the lifespan of batteries containing these solid electrolytes.

[0004] Therefore, glass and glass-ceramic solid electrolytes have attracted attention because they are known to be sintered at relatively low but still fairly high temperatures. In particular, borate-based glass-ceramics have attracted attention, and they are known to include two component phases using B2O3, LiBO2, and occasionally Li3BO3.

[0005] Study of electrical conductivity of Li2O-B2O3-SiO2-Li2SO4 glasses and glass-ceramics, SS Gundale, VV Behare et al., Solid State Ionics, Volume 298 (2016), pages 57-62 discloses the synthesis of glasses and glass-ceramics for SSE in the Li2O-B2O3-SiO2-Li2SO4 system. This method includes melt-quenching and single-stage heat treatment. The highest electrical conductivity (4.08 * 10-4 S / cm) was measured at 250 °C for the synthesized glass with a composition of 40Li2O:30B2O3:15SiO2:15Li2SO4, while noting that the ionic conductivity of the glass-ceramics was lower than that of the glass.

[0006] The disadvantage of the above method lies in its complexity, requiring a suitable environment and equipment for melt quenching. Another disadvantage is that high temperatures are required during the heat treatment process due to the presence of SiO2 (silicone), which has a high melting point.

[0007] Optimization of a heterogeneous ternary Li3PO4-Li3BO3---Li2SO4 mixture for Li-ion conductivity by machine learning, Kenji Homma, Yu Liu, et al., The Journal of Physical Chemistry C 124, 24 (2020), pages 12865-12870, reveals the optimization of the composition ratio of the ternary Li3PO4-Li3BO3-Li2SO4 mixture for lithium-ion conductivity using machine learning. After determining the optimal composition (25:14:61 Li3PO4:Li3BO3:Li2SO4, in moles), the mixture was prepared and sintered at temperatures determined by the melting point and phase transition of the mixture (for 12 hours in the range of 620 to 1000 °C). The lithium-ion conductivity of this mixture at 300 °C was 4.9 × 10⁻⁴ S / cm.

[0008] The disadvantage of the above method is that it still requires a relatively high sintering temperature, which is believed to be due to the use of Li3PO4 with a high melting point.

[0009] While the ionic conductivity values ​​of the two publications mentioned above appear acceptable, it is worth noting that these values ​​were obtained only at 250°C and 300°C, respectively, temperatures that are impractical for batteries. It is known in the art that ionic conductivity decreases with decreasing test temperature, meaning that at temperatures between room temperature and 100°C, the ionic conductivity values ​​of the sintered material can be expected to be unacceptably low, making the material unsuitable for use as a solid electrolyte in batteries. [Summary of the Invention]

[0010] The purpose of this invention is to overcome one or more of the above-mentioned disadvantages. The purpose of this invention is to provide a glass-ceramic solid electrolyte (i.e., solid electrolyte, SSE) that, when used in a battery, exhibits good total ionic conductivity at both room temperature and high temperature.

[0011] Simultaneously, an object of the present invention is to provide a method for producing glass-ceramic SSEs that consumes less energy compared to methods known in the art. A further object is to provide a method for producing glass-ceramic SSEs comprising sintering at a temperature lower than that of prior art sintering methods, wherein the obtained SSE has properties equal to or better than those of glass-ceramic SSEs obtained through conventional high-temperature sintering processes, particularly in terms of total ionic conductivity when used in batteries.

[0012] A further objective is to provide a method for producing solid-state batteries (SSBs), particularly all-ceramic SSBs, in which some or all of the components (including the anode and / or cathode) can be assembled and then sintered together, thereby reducing the overall energy consumption of the method for producing SSBs, as well as the complexity of the process and the number of steps required.

[0013] According to a first aspect of this disclosure, a glass-ceramic solid electrolyte mixture as described in the appended claims is provided.

[0014] The glass-ceramic solid electrolyte mixture comprises ternary glass-ceramics of borate, Li2SO4 and lithium halide or is substantially composed of ternary glass-ceramics of borate, Li2SO4 and lithium halide.

[0015] Advantageously, based on the total weight of the glass-ceramic solid electrolyte mixture, the glass-ceramic solid electrolyte mixture contains between 50 and 85% by weight, preferably between 60 and 80% by weight, more preferably between 65 and 75% by weight, for example 70% by weight of borate.

[0016] Advantageously, based on the total weight of the glass-ceramic solid electrolyte mixture, the glass-ceramic solid electrolyte mixture contains between 10 and 40% by weight, preferably between 15 and 35% by weight, more preferably between 20 and 30% by weight, for example 25% by weight of Li2SO4.

[0017] Advantageously, based on the total weight of the glass-ceramic solid electrolyte mixture, the glass-ceramic solid electrolyte mixture contains between 1 and 10% by weight, preferably between 2 and 8% by weight, more preferably between 3 and 7% by weight, for example 5% by weight of lithium halide.

[0018] Advantageously, based on the total weight of the glass-ceramic solid electrolyte mixture, the glass-ceramic solid electrolyte mixture comprises between 50 and 85% by weight of borate, between 10 and 40% by weight of Li2SO4 and between 1 and 10% by weight of lithium halide, preferably between 65 and 75% by weight of borate, between 20 and 30% by weight of Li2SO4 and between 3 and 7% by weight of lithium halide.

[0019] Advantageously, the borate contains or is substantially composed of Li3BO3.

[0020] Advantageously, the lithium halide is LiCl, that is, the halide is advantageously a chloride.

[0021] According to a second aspect of this disclosure, a glass-ceramic solid electrolyte as described in the appended claims is provided.

[0022] Advantageously, the glass-ceramic solid electrolyte is obtained or is obtainable by sintering a glass-ceramic solid electrolyte mixture of the first aspect.

[0023] The glass-ceramic solid electrolyte comprises a ternary glass-ceramic of borate, Li2SO4 and lithium halide or is substantially composed of a ternary glass-ceramic of borate, Li2SO4 and lithium halide, wherein the borate and the lithium halide are as described above.

[0024] Advantageously, the glass-ceramic solid electrolyte comprises or is substantially composed of a matrix, which comprises or is substantially composed of a borate. Advantageously, the lithium halide and Li2SO4 are dispersed in the matrix.

[0025] Advantageously, the borate is at least partially present in or included in the glass-ceramic solid electrolyte as a glass phase (e.g., a glass network).

[0026] The term “at least partially present or contained as a glass phase” as used in this disclosure means that at least 25%, preferably at least 50%, and more preferably at least 75% of the borate is present in the glass-ceramic solid electrolyte as a glass phase.

[0027] Advantageously, the glass-ceramic solid electrolyte has a total ionic conductivity between 10⁻⁵ and 10⁻⁹ S / cm, preferably between 10⁻⁵ and 10⁻⁸ S / cm, at a temperature between room temperature and 100°C.

[0028] According to a third aspect of this disclosure, a solid-state battery as described in the appended claims is provided.

[0029] The solid-state battery includes an electrolyte according to the second aspect of the present disclosure, namely an electrolyte comprising a ternary glass-ceramic containing borate, Li2SO4 and lithium halide or an electrolyte substantially composed of a ternary glass-ceramic containing borate, Li2SO4 and lithium halide, or an electrolyte obtained by sintering a glass-ceramic solid electrolyte mixture according to the first aspect of the present disclosure.

[0030] Advantageously, the solid-state battery is an all-ceramic solid-state battery. Advantageously, the solid-state battery is a rechargeable battery.

[0031] According to a fourth aspect of this disclosure, a method for producing a glass-ceramic solid electrolyte as described in the appended claims is provided.

[0032] Advantageously, the glass-ceramic solid electrolyte produced is, according to the second aspect of this disclosure, a ternary glass-ceramic comprising borate, Li2SO4 and lithium halide or essentially composed of borate, Li2SO4 and lithium halide, wherein the borate and the lithium halide are as described above.

[0033] The method comprises a sintered glass-ceramic solid electrolyte mixture comprising a ternary glass-ceramic of borate, Li₂SO₄, and lithium halide, or substantially composed of a ternary glass-ceramic of borate, Li₂SO₄, and lithium halide, wherein the borate and the lithium halide are as described above. Advantageously, the glass-ceramic solid electrolyte mixture is according to the first aspect of this disclosure.

[0034] The mixture is sintered in an inert atmosphere at a temperature between 600°C and 1000°C, preferably between 700°C and 900°C, and even more preferably between 750°C and 850°C.

[0035] According to a fifth aspect of this disclosure, a method for producing a solid-state battery as described in the appended claims is provided. Advantageously, the solid-state battery is, according to a third aspect of this disclosure, an all-ceramic solid-state battery.

[0036] According to a first embodiment, the method comprises: - applying a glass-ceramic solid electrolyte mixture according to the first aspect of the present disclosure to the surface of an anode or cathode; - sintering the mixture-anode or mixture-cathode assembly in an inert atmosphere at a temperature between 600°C and 1000°C, preferably between 700°C and 900°C, and more preferably between 750°C and 850°C; and - providing a cathode or anode on the exposed surface of the sintered mixture, thereby obtaining the solid-state battery.

[0037] According to a second embodiment, the method includes providing a glass-ceramic solid electrolyte mixture according to the first aspect of this disclosure between an anode and a cathode, and sintering an anode-mixture-cathode assembly, wherein sintering is carried out at the temperature and atmosphere as described above with respect to the first embodiment.

[0038] The inventors unexpectedly discovered that the presence of lithium halide in the glass-ceramic solid electrolyte mixture allows for a significant reduction in the sintering temperature of ternary glass-ceramics containing borate compounds, for example, from temperatures between 950°C and 1050°C or even higher to temperatures between 800°C and 850°C. Not wishing to be bound by any theory, the inventors believe that the lower sintering temperature is achievable because lithium halide, having a melting temperature below its sintering temperature (e.g., 605°C for LiCl), remains molten during sintering, resulting in so-called liquid-phase sintering or liquid-assisted sintering. The presence of the liquid (molten lithium halide) accelerates the bonding between other components, thus allowing for the lower sintering temperature.

[0039] The advantage of this significantly lower sintering temperature is that the mixture can be co-sintered with one or both of the anode and cathode, making the production of solid-state batteries (especially all-ceramic solid-state batteries) less complex and less energy-intensive. It is known that for all ceramic SSBs, the anode and / or cathode contain materials that need to be sintered at temperatures below 1000°C, preferably even below 900°C, to avoid any degradation or damage that would lead to a decrease in battery quality.

[0040] Therefore, since the method of the present invention and the glass-ceramic solid electrolyte mixture allow sintering at temperatures below 1000°C, the anode and / or cathode can be assembled with the glass-ceramic solid electrolyte mixture first, followed by a single sintering step. This contrasts with prior art methods, which on the one hand require separate sintering steps for the anode and / or cathode at temperatures below 1000°C, and on the other hand require separate sintering steps for the SSE at temperatures above 1000°C.

[0041] Therefore, the advantages of the method of the present invention and the glass-ceramic solid electrolyte mixture include lower energy consumption during the sintering process and a less complex process for producing solid-state batteries (especially all-ceramic solid-state batteries).

Implementation Method

[0043] The glass-ceramic solid electrolyte mixture disclosed herein and the glass-ceramic solid electrolyte comprising ternary glass-ceramics of borate, Li2SO4 and lithium halide or substantially composed of ternary glass-ceramics of borate, Li2SO4 and lithium halide.

[0044] Advantageously, the borate comprises or is substantially composed of Li3BO3. Alternatively or additionally, and still advantageously, the borate may comprise one or more of B2O3, LiBO2, Li4B2O5, and Li6B4O9.

[0045] The halide can be any one of chloride, bromide, iodide, and fluoride, preferably chloride or fluoride, and more preferably chloride. Therefore, the lithium halide can be any one of LiCl, LiBr, LiI, and LiF, preferably LiCl or LiF, and more preferably LiCl. The glass-ceramic solid electrolyte can contain two or more lithium halides, advantageously two or more of LiCl, LiBr, LiI, and LiF.

[0046] Advantageously, based on the total weight of the glass-ceramic solid electrolyte, the glass-ceramic solid electrolyte contains between 50 and 85% by weight, preferably between 60 and 80% by weight, more preferably between 65 and 75% by weight, for example 70% by weight of borate.

[0047] Advantageously, based on the total weight of the glass-ceramic solid electrolyte, the glass-ceramic solid electrolyte contains between 10 and 40% by weight, preferably between 15 and 35% by weight, more preferably between 20 and 30% by weight, for example 25% by weight of Li2SO4.

[0048] Advantageously, based on the total weight of the glass-ceramic solid electrolyte, the glass-ceramic solid electrolyte contains between 1 and 10% by weight, preferably between 2 and 8% by weight, more preferably between 3 and 7% by weight, for example 5% by weight of lithium halide.

[0049] Advantageously, based on the total weight of the glass-ceramic solid electrolyte, the glass-ceramic solid electrolyte comprises between 50 and 85% by weight of borate, between 10 and 40% by weight of Li2SO4, and between 1 and 10% by weight of lithium halide, preferably between 65 and 75% by weight of borate, between 20 and 30% by weight of Li2SO4, and between 3 and 7% by weight of lithium halide.

[0050] Advantageously, the glass-ceramic solid electrolyte disclosed herein is a dense electrolyte, i.e., an electrolyte with low porosity. More specifically, the electrolyte advantageously has a density equal to or higher than 70% of its theoretical density. The theoretical density is calculated based on the density of the compounds contained in the electrolyte and the composition of the electrolyte (the amount of each compound). The density of the electrolyte is calculated by dividing its weight by its volume.

[0051] The present invention further relates to solid-state batteries (i.e., all-solid-state batteries) (SSB), particularly secondary batteries, which include the glass-ceramic solid electrolyte of the present invention.

[0052] Advantageously, the battery further comprises a cathode, which may be any suitable cathode known in the art. Advantageously, the battery further comprises an anode, which may be any suitable anode known in the art.

[0053] Advantageously, the SSB is an all-ceramic SSB, that is, an SSB in which all components (anode, cathode and electrolyte) are made of ceramic materials.

[0054] This invention also relates to a method for producing glass-ceramic SSE. This method advantageously includes operations for preparing a mixture, molding, and sintering.

[0055] Advantageously, the mixture preparation operation comprises mixing a borate, Li2SO4, and a lithium halide, wherein the borate and the lithium halide are as described above. To obtain a homogeneous mixture, mixing techniques known in the art, such as ball milling or pearl milling, can be used.

[0056] Advantageously, based on the total weight of the mixture, the mixture comprises between 50 and 85% by weight of borate (preferably Li3BO3), between 10 and 40% by weight of Li2SO4, and between 1 and 10% by weight of lithium halide (preferably LiCl), preferably between 65 and 75% by weight of borate, between 20 and 30% by weight of Li2SO4, and between 3 and 7% by weight of lithium halide.

[0057] Advantageously, the mixture is shaped during the molding operation. Molding can be carried out by methods known in the art, such as by pressing the mixture into a predetermined shape or by laser cutting the mixture into a predetermined shape. After molding, a green body is obtained. The green body can have various shapes, such as flakes, granules, discs, etc., wherein the shape is defined by the desired shape of the composite solid electrolyte.

[0058] The green blank is then sintered during a sintering operation. The sintering operation includes heating the green blank to a sintering temperature and maintaining the green blank at the sintering temperature for a predetermined sintering duration, during which the green blank is sintered.

[0059] Advantageously, the sintering operation is carried out in an atmosphere known in the art. Preferably, the sintering operation is carried out in an inert atmosphere, more preferably in an inert atmosphere containing argon or consisting essentially of argon.

[0060] Advantageously, the sintering temperature is between 600°C and 1000°C, more preferably between 700°C and 900°C, and even more preferably between 750°C and 850°C.

[0061] Advantageously, the green blank is heated to a sintering temperature at a heating rate between 5°C / s and 500°C / s, which can be carried out at a conventional heating rate or an ultrafast heating rate.

[0062] Advantageously, the sintering duration is between 5 seconds and 600 seconds, more preferably between 10 seconds and 300 seconds, even more preferably between 20 seconds and 200 seconds, for example between 30 seconds and 150 seconds, or between 45 seconds and 100 seconds.

[0063] It should be understood that the sintering duration depends on the heating rate, sintering temperature, and the equipment used, etc. Example 1

[0064] A mixture of 7.0 g Li3BO3, 2.5 g Li2SO4 and 0.5 g LiCl was ball-milled at 400 rpm for 2 hours under an argon atmosphere. The mixture was then pressed into green pellets using a uniaxial press.

[0065] The green particles were then heated to 825°C and sintered at 825°C for 100 seconds, and then cooled to room temperature. The resulting glass-ceramic solid electrolyte particles were then partially ground into powder and partially cut into fragments for analysis.

[0066] Figure 1 shows the X-ray diffraction (XRD) patterns of Li2SO4, Li3BO3, and glass-ceramic solid electrolyte powders (labeled 1, 2, and 3, respectively). The comparison of the XRD patterns clearly shows the presence of Li2SO4 and Li3BO3 in the electrolyte. The signal between 0°2θ and 20°2θ further indicates the presence of a glass phase, which is believed to be formed by Li3BO3.

[0067] The glass-ceramic solid electrolyte fragments were analyzed by scanning electron microscopy (SEM) under high vacuum using a high-resolution scanning electron microscope FEI (Teneo). Figures 2 and 3 show SEM images of the cross-section of the glass-ceramic solid electrolyte at different magnifications. At low magnification (Figure 2), a dense structure is visible. At high magnification (Figure 3), the glassy matrix (contributed by Li3BO3) is clearly visible, in which crystalline phases are dispersed.

[0068] Figure 4 shows the energy-dispersive X-ray diffraction (EDX) analysis of the cross-section of the electrolyte. All elements of Li3BO3, Li2SO4, and LiCl were detected. This confirms that all components of the mixture are retained in the resulting glass-ceramic solid electrolyte. Example 2

[0069] A Li-Li symmetric battery comprising the glass-ceramic solid electrolyte of Example 1 was prepared to measure the total ionic conductivity and electrochemical performance. The Li-Li symmetric battery of the present invention was prepared using 800 μm thick glass-ceramic solid electrolyte particles prepared in Example 1, 50 μm thick lithium metal as electrodes, and 5 to 8 μm thick copper foil as current collectors.

[0070] Figure 5 shows the total ionic conductivity as a function of temperature between room temperature and 100°C. At room temperature, the total ionic conductivity is 2 * 10⁻⁸ S / cm, while at 100°C, the total ionic conductivity is 4 * 10⁻⁷ S / cm.

[0071] The Li-Li symmetric cell of the present invention was also subjected to constant current cycling at 100°C and a current density of 0.1 mA / cm². As can be clearly seen from Figure 6, the cycle stability was maintained for more than 4500 seconds. Nomenclature: 1. XRD pattern of Li₂SO₄; 2. XRD pattern of Li₃BO₃; 3. XRD pattern of the glass-ceramic solid electrolyte of the present invention. [Simplified Explanation of the Diagram]

[0042] Aspects of the invention will now be described in more detail with reference to the accompanying drawings, wherein like reference numerals denote like features, and wherein: [Figure 1] shows an X-ray diffraction (XRD) pattern of the glass-ceramic solid electrolyte of the invention after it has been ground into powder; [Figures 2 and 3] show scanning electron microscope (SEM) images of the cross-section of the glass-ceramic solid electrolyte of the invention at different magnifications; [Figure 4] shows energy dispersive X-ray (EDX) analysis of the cross-section of the glass-ceramic solid electrolyte of the invention; [Figure 5] shows the total ionic conductivity of a Li-Li symmetric cell containing the glass-ceramic solid electrolyte of the invention; and [Figure 6] shows the galvanostatic cycling of the cell of the invention.

Claims

1. A glass-ceramic solid electrolyte mixture comprising Li3BO3, Li2SO4, and LiCl, wherein, The glass-ceramic solid electrolyte mixture contains, based on its total weight, 50 to 85% by weight of Li3BO3, 10 to 40% by weight of Li2SO4, and 1 to 10% by weight of LiCl.

2. A glass-ceramic solid electrolyte that can be obtained by sintering a glass-ceramic solid electrolyte mixture as claimed in claim 1, wherein the glass-ceramic solid electrolyte mixture is sintered in an inert atmosphere at a temperature between 600°C and 1000°C.

3. The glass-ceramic solid electrolyte of claim 2, comprising a matrix including Li3BO3, wherein LiCl and Li2SO4 are dispersed in the matrix.

4. The glass-ceramic solid electrolyte of claim 2, wherein Li3BO3 is at least partially contained in the electrolyte as a glass phase.

5. The glass-ceramic solid electrolyte of claim 2, having a total ionic conductivity between 10⁻⁵ and 10⁻⁹ S / cm at a temperature between room temperature and 100°C.

6. A solid-state battery comprising a glass-ceramic solid electrolyte as claimed in claim 2.

7. The solid-state battery in Request 6 is an all-ceramic solid-state battery.

8. A method for producing a glass-ceramic solid electrolyte comprising a ternary glass-ceramic of Li3BO3, Li2SO4 and LiCl, the method comprising sintering the mixture of claim 1 at a temperature between 600°C and 1000°C in an inert atmosphere.

9. A method for producing a solid-state battery comprising a glass-ceramic solid electrolyte as claimed in claim 2 or a glass-ceramic solid electrolyte obtained by the method of claim 8, the method comprising: - applying a mixture of glass-ceramic solid electrolytes as claimed in claim 1 to a surface of an anode or cathode; - sintering in an inert atmosphere at a temperature between 600°C and 1000°C; and - providing a cathode or anode on the exposed surface of the sintered mixture, thereby obtaining the solid-state battery.

10. The method of producing a solid-state battery as claimed in claim 9, wherein the anode and the cathode are provided prior to sintering, thereby providing the glass-ceramic solid electrode mixture between the anode and the cathode, and wherein sintering comprises sintering an anode-mixture-cathode assembly.

Citation Information

Patent Citations

  • Solid electrolyte, method for preparing the same, and battery using the same

    US20040151986A1