Corrosion-resistant free-cutting brass alloy, manufacturing method and application
The corrosion-resistant free-cutting brass alloy with a balanced composition of Si, Ni, Mn, and B, forming a composite κ phase, addresses the limitations of existing brass alloys by enhancing cutting performance, corrosion resistance, and mechanical properties, while being environmentally friendly.
Patent Information
- Application Number
- US19/716196
- Authority / Receiving Office
- US · United States
- Patent Type
- Applications(United States)
- Current Assignee / Owner
- Priority Date
- 2025-10-16
- Filing Date
- 2026-06-23
- Publication Date
- 2026-11-12
AI Technical Summary
Existing brass alloys face challenges such as toxicity, lack of environmental friendliness, insufficient cutting performance, corrosion resistance, and mechanical properties, particularly due to issues like hot and cold cracking, dezincification corrosion, and poor thermal conductivity.
A corrosion-resistant free-cutting brass alloy composed of Cu: 58.0 to 62.5%, Si: 0.3 to 1.2%, Ni: 0.1 to 0.5%, Mn: 0.3 to 0.7%, B: 0.005 to 0.025%, with a synergistic optimization index (Γ) of 0.1 to 0.4, forming a composite κ phase (Cu, Ni, Mn)5ZnSi to enhance strength, cutting performance, and corrosion resistance, while controlling impurities <0.3%.
The alloy achieves excellent cutting performance, corrosion resistance, and mechanical properties, with yield strength >200 MPa, tensile strength >500 MPa, elongation >22%, dezincification corrosion depth <410 μm, and main cutting force <100 N, meeting environmental protection requirements.
Smart Images

Figure US20260357381A1-D00001 
Figure US20260357381A1-D00002 
Figure US20260357381A1-D00003
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the field of alloys, and in particular, to a corrosion-resistant free-cutting brass alloy, manufacturing method and application thereof.DESCRIPTION OF RELATED ART
[0002] Traditional free-cutting brass is widely used in the industrial field, and its core modification element is lead. The lead element exists in the form of free lead particles in the brass matrix. During the cutting process, the lead particles can play a good role in chip breaking, thereby significantly improving the cutting performance of the material. For example, a common C3604 alloy usually has a lead content up to 1.8 to 3.7%, and during cutting processing, a cutting force is relatively small, a tool wear rate is slow, and the processing efficiency is high.
[0003] However, with the improvement of environmental awareness and the increasingly strict environmental regulations, the toxicity problem of lead is gradually highlighted. In order to cope with the environmental protection problem of traditional lead-containing brass, researchers have proposed a series of lead-free alternatives. CN101701304B discloses a bismuth-based brass, which improves the cutting performance of copper zinc alloys by adding bismuth as a substitute for lead, and adds arsenic to improve the dezincification corrosion resistance of the alloy, thereby achieving the purposes of corrosion resistance, lead-free and free-cutting. However, bismuth-based brass is prone to hot cracking and cold cracking problems during hot working and subsequent processing. Hot cracking often occurs during the casting or high-temperature forming stage, which is caused by the brittleness of bismuth and the difference in thermal expansion from the copper matrix; cold cracking is mostly caused by stress concentration during cooling, cold working or storage. The cracking problem significantly affects the yield, mechanical reliability and processing efficiency of the material, and limits its wider application. Moreover, arsenic is toxic and cannot fundamentally solve the toxicity problem in the use of alloys.
[0004] In the research and development of lead-free brass, antimony has also been used as one of the substitute elements for lead. CN100503854C discloses a low-lead-boron free-cutting antimony brass alloy, in which antimony can form hard particles, which is conducive to chip breaking, thereby improving the cutting performance of the material. However, the antimony-based brass has obvious limitations: on the one hand, antimony has a certain biotoxicity, which may be dissolved during the use of products, posing a safety risk in drinking water scenarios; on the other hand, antimony will reduce the thermal conductivity and thermoplasticity of alloys, and is prone to surface cracks and internal defects during hot rolling or hot forging, which seriously affects the thermal processing yield and mechanical properties of materials.
[0005] Compared with bismuth and antimony elements, silicon, as an environmentally friendly substitute element, has attracted extensive attention in brass research and development.
[0006] EP3985136A1 discloses a lead-free copper alloy, containing Cu: 70.0 to 83.0%, Si: 2.0 to 2.9%, P: 0.05 to 0.10%, Sn: 0.01 to 0.30%, balance: Zn and inevitable impurities. Although the high Si content can improve the cutting performance of the alloy, it will reduce the plasticity of the alloy, and also aggravate the oxidation burning loss in the smelting process, making it more difficult to control the melt quality and the casting billet uniformity. In addition, the Cu content far beyond the conventional brass standard results in a significant rise in cost.
[0007] DE102022002927B4 discloses a malleable material made of copper-zinc alloy, containing Cu: 58.0 to 63.0%, Si: 0.04 to 0.32%, P: 0.05 to 0.20%, balance: Zn and inevitable impurities. Low Si content makes it difficult to form a sufficient number of hard silicide phases, resulting in limited improvement of cutting performance. At the same time, although the addition of P helps to improve the cutting performance, its solid solution strengthening effect is limited, and it tends to segregate at grain boundaries, weakening the grain boundary cohesion. In addition, the composition of the alloy determines that the alloy has poor dezincification corrosion resistance, which makes it difficult for the alloy to meet the requirements of high-performance application scenarios.
[0008] In summary, the brass alloy materials in the prior art generally have problems such as toxicity, lack of environmental friendliness, insufficient cutting performance, corrosion resistance or mechanical properties.SUMMARY
[0009] An object of the present disclosure is to provide a corrosion-resistant free-cutting brass alloy, manufacturing method and application thereof. The corrosion-resistant free-cutting brass alloy of the present disclosure has excellent cutting performance, corrosion resistance and mechanical properties, achieving a balance of comprehensive performance, and is free of lead, which meets environmental protection requirements and can meet the application requirements of brass alloy materials in different fields.
[0010] A first aspect of the present disclosure provides a corrosion-resistant free-cutting brass alloy, composed of the following components in percentage by mass: Cu: 58.0 to 62.5%, Si: 0.3 to 1.2%, Ni: 0.1 to 0.5%, Mn: 0.3 to 0.7%, B: 0.005 to 0.025%, and the balance of Zn and inevitable impurity elements, wherein a total content of the inevitable impurity elements is <0.3%.
[0011] The present disclosure synergistically improves the cutting performance, corrosion resistance and mechanical properties of brass alloys by adding elements such as Si, Ni, Mn and controlling the content of each element.
[0012] The zinc equivalent coefficient of Si is high, and adding an appropriate amount of Si to brass can shift the β phase boundary in the Cu—Zn phase diagram to the left, thereby improving the strength and cutting performance of the alloy.
[0013] Ni and Cu can form an infinite solid solution, which enhances the strength and toughness of the alloy through solid solution strengthening. The addition of Ni can change the electrode potential on the surface of the alloy, inhibit the common dezincification corrosion in brass, and significantly improve the resistance of the alloy to seawater, salt fog and chloride.
[0014] Mn can improve the strength and hardness of the alloy through a solid solution strengthening mechanism, while reducing the thermal brittleness of the alloy and improving its hot workability. In addition, during hot working, Mn inhibits the formation of harmful phases, reduce the occurrence of cracks, and make the alloy easier to form at high temperatures.
[0015] In the alloy of the present disclosure, the Si content is 0.3 to 1.2%. If Si<0.3%, it cannot effectively promote chip fracture, resulting in the generation of continuous long chips during the processing. Long chips can not only wrap around the tool, affecting machining operations, but also scratch the already machined surface, reducing surface quality. When Si>1.2%, more brittle reticulated 7 phases are formed in the alloy, the coarse 7 phases are distributed at the grain boundaries, segmenting the matrix, which can significantly reduce the plasticity and toughness of the alloy. During the cutting process, the material is prone to cracking, especially during precision machining, which seriously affects the machining accuracy and causes dimensional deviation.
[0016] In the alloy of the present disclosure, the Ni content is 0.1 to 0.5%. Ni has the effect of inhibiting dezincification corrosion and promoting grain refinement in the alloy, and a small amount of addition can significantly enhance the corrosion resistance of the alloy. When Ni<0.1%, the effect of inhibiting dezincification corrosion is not obvious, and in a marine environment or an atmospheric environment containing salt fog, the alloy is prone to dezincification corrosion, which shortens the service life of the material; when Ni>0.5%, hard and brittle phases such as Ni2Si are prone to precipitate in the alloy, which are distributed at grain boundaries, resulting in increased brittleness of the material. In addition, Ni is a relatively expensive metal, and an excessively high Ni content will increase production costs.
[0017] In the alloy of the present disclosure, the Mn content is controlled at 0.3 to 0.7%. Within this range, Mn can be fully solid dissolved in the copper matrix, which effectively plays a solid solution strengthening role and improves the strength and hardness of the alloy. If Mn<0.3%, the solid solution strengthening effect will be significantly weakened, resulting in insufficient overall strength and hardness of the alloy; moreover, it may also cause composition segregation, which adversely affects the dynamic recrystallization behavior during the hot working process and reduces the material forming consistency; when Mn>0.7%, a coarse hard and brittle manganese compound phase is easily formed at the grain boundary, seriously disrupting the continuity of the matrix. During the hot working process, the hard and brittle manganese compound phase can become a stress concentration point, which is easy to cause cracks, resulting in a decrease in the thermal plasticity and poor formability of the alloy.
[0018] In the alloy of the present disclosure, B as a modifier plays a crucial role during the solidification process of the alloy. Its core function is to refine the solidification structure, improve element segregation, enhance structure uniformity, and provide a good billet foundation for subsequent hot working.
[0019] In order to avoid the uncontrollable influence of impurities on the alloy properties, the present disclosure controls the total content of impurity elements in the brass alloy to be <0.3%. In particular, Pb<0.05% and Bi<0.008% in the inevitable impurities. By controlling Pb<0.05%, the present disclosure can ensure that the environmental protection requirements are met; by controlling Bi<0.008%, the alloy is prevented from segregating at the grain boundary and being distributed in a network or thin film shape during the solidification process, resulting in the cold / hot brittleness phenomenon, which adversely affects the processability and mechanical properties.
[0020] Preferably, the brass alloy has an α phase, a β phase and a composite κ phase in particle form, and the area proportions of the α phase, the β phase and the composite κ phase are 28 to 72%, 26 to 67% and 1 to 5% of the total area of these three phases, respectively; wherein the composite κ phase is (Cu, Ni, Mn)5ZnSi, has an average particle size of 0.5 to 1.5 μm, and is dispersively distributed in the β phase.
[0021] The traditional silicon brass microstructure is composed of α+β+γ phase, wherein the γ phase (Cu5Si) precipitates in a continuous or semi-continuous network form along the grain boundary of the α phase, and the γ phase will significantly reduce the plasticity of the brass alloy material. In order to solve this problem, the present disclosure adjusts and optimizes the Si content in the silicon brass, adds a proper amount of Ni and Mn elements, and through the synergistic action among the three elements, innovatively introduces a composite κ phase, which can be expressed as (Cu, Ni, Mn)5ZnSi, ((Cu, Ni, Mn) indicates that Ni and Mn replace part of Cu atoms in the κ phase (Cu5ZnSi)), thus avoiding the formation of γ phase in the silicon brass alloy. The composite κ phase of the present disclosure is uniformly distributed in the β phase in the form of finely dispersed particles, and this crystal phase distribution enables the alloy to have good strength while maintaining excellent cutting performance, while avoiding the plastic deterioration problem caused by the brittle network phase in alloys containing the γ phase. In addition, the Ni and Mn elements rich in the composite κ phase interface can effectively inhibit the high-temperature coarsening of the crystal phase, so that the material has slower performance degradation and higher reliability at high temperature.
[0022] The formation of the composite κ phase occurs in the melting and casting stage, and during the melting and casting process, the mechanism of forming the composite κ phase by the synergistic action of elements Si, Ni and Mn is as follows:
[0023] (1) in the nucleation stage, during the cooling process after solidification of the alloy, when the temperature drops to the formation zone of the κ phase (Cu5ZnSi), the κ phase nucleates and precipitates in the β phase. This is mainly because the complex cubic structure of the κ phase has higher compatibility with the body-centered cubic structure of the β phase, and the interface energy difference between the two is smaller, which significantly reduces the energy barrier required for nucleation, making nucleation easier and faster;
[0024] (2) in the growth stage, Ni and Mn atoms dissolve in solid solution into the lattice of the κ phase, partially replace Cu atoms, this initiates lattice distortion, generates a solid-solution strengthening effect, and promotes the formation and dispersive distribution of the composite κ phase, and form a thermodynamically more stable composite compound (Cu, Ni, Mn)5ZnSi, that is, the composite κ phase;
[0025] (3) in the stabilization stage, solute atoms such as Ni and Mn (especially Ni) segregate at the interface of the composite κ phase, which effectively hinders the migration of the interface and the diffusion of elements, thereby significantly inhibiting the coarsening process of the composite κ phase particles at high temperature, so that the composite κ phase particles can maintain fine size and dispersive distribution state.
[0026] The α phase is a copper-rich face-centered cubic (FCC) solid solution based on copper-zinc, and its main function is to provide excellent ductility, toughness and cold working performance. The α phase structure is soft, can coordinate plastic deformation, and effectively inhibits the initiation and propagation of cracks, thereby ensuring that the alloy is not prone to cracking during cold working. Meanwhile, the α phase also has good corrosion resistance, which is the basis for maintaining the overall corrosion resistance of the alloy. If the content of the α phase is <28%, the alloy will exhibit obvious brittleness tendency due to excessive hardening, and its ductility cannot meet the processing and use requirements; if the content is >72%, although the alloy has high plasticity, its strength, hardness and wear resistance will be significantly insufficient, making it difficult to bear structural loads.
[0027] The β phase is a body-centered cubic (BCC) solid solution based on copper-zinc, serving as a strengthening phase in an alloy, provides the necessary strength and hardness for a material, and is a core source of load-bearing capacity. However, the β phase is sensitive to dezincification corrosion due to its high zinc content and specific crystal structure. Its content range of 26 to 67% balances mechanical properties and corrosion resistance. When the content of β phase is <26%, the dezincification corrosion resistant effect of the alloy is better, but the strength and hardness are insufficient, and it is difficult to meet the application requirements; if the content is >67%, the strength is improved, but the toughness and brittle fracture resistance of the alloy are sharply reduced, increasing the risk of cold cracking. More importantly, the dezincification corrosion resistance of the alloy will be seriously deteriorated at this time.
[0028] The composite κ phase is an intermetallic compound formed by elements such as Si, Ni, Mn, and is a hard and brittle dispersed precipitate phase, which functions to improve the cutting performance and mechanical properties of the alloy. During cutting, the composite κ phase can promote chip fracture, reduce tool adhesion and vibration, thereby reducing cutting force, reducing tool wear, and obtaining a good surface finish. The content of the composite κ phase is strictly controlled at 1% to 5% to balance the cutting performance and mechanical properties. When the content is <1%, the effect of improving the cutting performance is not obvious; when the content is >5%, too much composite κ phase will become a stress concentration point, which significantly damages the plasticity and toughness of the material and causes the alloy to become brittle.
[0029] In the brass alloy of the present disclosure, the average particle size of the composite κ phase is 0.5 to 1.5 μm, and within this particle size range, the composite κ phase can effectively serve as both a dispersed strengthening phase and a cutting performance improvement phase, thereby achieving a perfect balance between mechanical properties and cutting performance. When the average particle size is <0.5 μm, the composite κ phase is difficult to achieve a chip breaking effect, and the main cutting force is increased, resulting in a decrease in the cutting performance of the alloy; and when the average particle size is >1.5 μm, the composite κ phase hinders dislocation movement, resulting in local stress concentration, which leads to a deterioration in the plasticity of the alloy.
[0030] It should be noted that the addition of element B plays a key role in regulating the morphology and distribution of the composite κ phase. B preferentially forms fine boride particles with Ni and Mn elements in the alloy during solidification. On the one hand, high-melting-point boride particles serve as heterogeneous nucleation cores to refine as-cast grains; on the other hand, they are adsorbed on grain boundaries and phase boundaries to produce pinning effects on grain boundary migration. This pinning effect can effectively inhibit excessive growth and coarsening of the composite κ phase during subsequent solidification and heat treatment, and promote the composite κ phase to be uniformly distributed in the matrix in a finer and more dispersed form, thereby significantly improving the strength, hardness and hot workability of the alloy. At the same time, by refining the grains and inhibiting the coarsening of the composite κ phase, the element B also helps to reduce the hot cracking tendency of the alloy and improve the integrity and structure uniformity of the casting billet.
[0031] Preferably, the brass alloy of the present disclosure has a yield strength of >200 MPa, a tensile strength of >500 MPa, an elongation of >22%, a main cutting force Fz during cutting of <100 N, a transverse average dezincification corrosion depth of <410 μm, and a longitudinal average dezincification corrosion depth of <520 μm.
[0032] Due to the complex synergistic interaction between Si, Ni, and Mn elements, in order to make the alloy obtain excellent comprehensive performance, we propose a synergistic optimization index (F), and the core purpose of the synergistic optimization index is to accurately characterize the structure-activity relationship between multi-component and performance through a unified quantitative index, breaking through the limitation of the traditional single-variable optimization method. As a core basis for the composition design of the alloy of the present disclosure, the index can effectively guide the ratio of each element, promote the dispersed precipitation of the composite κ phase, thereby improving the cutting performance, dezincification corrosion resistance and mechanical properties of the alloy, and achieving the synergistic optimization of multiple performance indexes. The calculation formula of the synergistic optimization index Γ is as follows (Γ: the ratio of the product of the Ni content and the Mn content to the 1.2th power of the Si content, in mass percentage):Γ=Ni·MnSi1.2(Formula 1)
[0033] In order to make the alloy obtain good comprehensive properties, in the content range of each component, the present disclosure strictly controls the synergistic optimization index Γ within the range of 0.1 to 0.4, which is the key to realize the synergistic optimization of multiple properties. Within this range, the proportions of the key components such as Si, Ni and Mn are in the best synergistic state. Each element can not only strengthen the matrix by fully solid solution, but also promote the precipitation of the composite κ phase in a fine and dispersed ideal form, thereby significantly improving the comprehensive performance of the alloy.
[0034] When Γ<0.1, it means that the content of Si elements in the alloy composition is relatively high or the content of Ni and Mn elements is relatively insufficient. This ratio imbalance will lead to the inability to form an effective synergistic strengthening mechanism between elements: excessive Si is easy to form Si-rich phases, resulting in a decrease in plasticity; insufficient Ni content will reduce the corrosion stability between phase interfaces and weaken its ability to inhibit anode dissolution, resulting in a significant increase in the depth of dezincification corrosion, seriously deteriorating corrosion resistance; insufficient Mn content will weaken the distortion effect on the matrix lattice, reduce the dislocation movement resistance, and affect the mechanical properties of the alloy; if the cooperation of Ni and Mn elements is insufficient, the mechanical properties and the dezincification corrosion resistance of the alloy will be damaged at the same time, resulting in that the comprehensive performance cannot meet the standard.
[0035] When Γ>0.4, it means that the content of Ni and Mn elements in the alloy composition is relatively high or the content of Si element is relatively insufficient. Excessive Ni and Mn aggravate the lattice distortion of the matrix and improve the solid solution strengthening effect, but easily lead to a decrease in material plasticity.
[0036] In the brass alloy of the present disclosure, the content of Si is preferably 0.5 to 1.2% in percentage by mass. The present disclosure further improves the mechanical properties, cutting performance and dezincification corrosion resistance of the material by regulating the Si content.
[0037] On the basis of the above preferred components, in combination with the subsequent processing process, the area proportions of the α phase, the β phase and the composite κ phase in the alloy of the present disclosure are further adjusted to obtain the brass alloy with the area proportions of the α phase, the β phase and the composite κ phase of 28 to 60%, 40 to 67% and 2.5 to 4.6% of the total area of these three phases, respectively, thereby further improving the comprehensive performance of the alloy.
[0038] Further preferably, the brass alloy of the present disclosure has a yield strength of >255 MPa, a tensile strength of >560 MPa, an elongation of >22%, a main cutting force Fz during cutting of <88 N, a transverse average dezincification corrosion depth of <305 μm, and a longitudinal average dezincification corrosion depth of <420 km.
[0039] In practical use, the brass alloy of the present disclosure has various forms, such as stick-shaped, wire-shaped, pipe-shaped, plate-shaped, strip-shaped, rod-shaped or block-shaped.
[0040] A second aspect of the present disclosure provides the application of the corrosion-resistant free-cutting brass alloy in the fields of bathroom valves, plumbing connectors, spare parts and accessories for refrigeration or automobiles.
[0041] A third aspect of the present disclosure provides a method for manufacturing the corrosion-resistant free-cutting brass alloy, comprising the following steps: batching and smelting according to target components, and then casting to obtain an ingot; and subjecting the ingot to a processing treatment to manufacture a brass alloy.
[0042] The raw materials for manufacturing the brass alloy in the form of stick-shaped, wire-shaped, pipe-shaped, plate-shaped, strip-shaped, rod-shaped or block-shaped etc. of the present disclosure can be selected from high-purity cathode copper or bright wire, zinc ingot, intermediate alloy containing Si, Ni, Mn and B elements, etc. In the present disclosure, the mass proportions of Si, Ni, Mn and B in the intermediate alloy are not limited, as long as the content of each element after batching meets the target components of the product.
[0043] The casting process of the present disclosure can be semi-continuous casting or horizontal continuous casting, etc., which is specifically determined according to the type of the target product. In the present disclosure, the smelting temperature is set to 1050 to 1100 °C, and the casting temperature is set to 1030 to 1080 °C.
[0044] When manufacturing a stick-shaped form brass alloy articles, a semi-continuous casting process is preferably used, and a low-frequency electromagnetic stirring is applied during the casting process. The stirring frequency is controlled at 10 to 30 Hz with a current intensity of 20 to 40 A. Through electromagnetic stirring, dendrites can be effectively broken and the mass transfer process in the liquid phase can be promoted, thereby reducing macroscopic segregation and refining the grains of solidification structure.
[0045] The processing treatment of the present disclosure comprises hot working, cold working and heat treating, etc., and can not only adopt existing mature processing technologies, but also optimize and adjust process parameters or develop new processing methods according to specific product performance requirements and application scenarios, so as to meet the diversified requirements of different industries for brass alloy materials.
[0046] In some examples of the present disclosure, when the brass alloy article has a stick-shaped form, the processing treatment comprises the following steps:
[0047] (1) hot extruding: heating the ingot to 650 to 700 °C before extruding, then extruding at an extrusion speed of 10 to 15 mm / s, and cooling at a cooling rate not lower than 30 °C / min after extruding;
[0048] (2) stretching: stretching the hot extruded stick; and
[0049] (3) final annealing: annealing the stretched stick at 260 to 330 °C for 120 to 240 min.
[0050] Preferably, in the hot extruding, the ingot is heated to 650 to 700 °C by graded gradient heating before extruding, and the graded gradient heating sequentially includes a low-temperature preheating stage, a medium-temperature heating stage and a high-temperature soaking stage;
[0051] the low-temperature preheating stage is: heating the ingot to 300 to 400 °C within 50 to 60 min;
[0052] the medium-temperature heating stage is: heating the ingot to 500 to 600 °C within 40 to 50 min;
[0053] the high-temperature soaking stage is: heating the ingot to 650 to 700 °C within 30 to 40 min.
[0054] In the low-temperature preheating stage (300 to 400 °C), the ingot slowly and uniformly absorbs heat, initially increasing the overall temperature and releasing the stress of the ingot slowly and uniformly, avoiding the risk of cracking and reducing ingot dendrite segregation, making the alloy composition more uniform.
[0055] The medium-temperature heating stage (500 to 600 °C) is a dissolution window for many low melting eutectic phases or unstable transition phases. Within this temperature range, the harmful phases (such as Cu5Zn8) formed during casting and distributed at the grain boundary can be dissolved or spheroidized, thereby purifying the grain boundary, improving the high-temperature plasticity, and preventing grain boundary cracking during hot working. More importantly, this stage provides sufficient diffusion power and time for the composite κ phase to be homogenized and spheroidized, and the composite κ phase changes from an irregular shape in an as-cast state to a dispersed and rounded particle state, thereby optimizing its strengthening effect and reducing the deformation resistance.
[0056] The temperature range of the high-temperature soaking stage (650 to 700 °C) is located in the α+β two-phase region, and the alloy has excellent plasticity, low flow stress, and is easy to extrusion forming. More importantly, the composite κ phase has extremely high thermal stability at this temperature without dissolution and coarsening. The present disclosure controls the heating time at this stage to be 30 to 40 min, so as to avoid the problem of severe grain coarsening caused by excessive heating time and the generation of microcracks inside the alloy during extrusion.
[0057] The extrusion speed is controlled at 10 to 15 mm / s, which can not only ensure high extrusion efficiency, but also avoid thermal defects caused by heat accumulation due to material deformation. After extrusion, rapid cooling is immediately carried out with a cooling rate of not less than 30 °C / min. Controlling the cooling rate at 30 °C / min or higher helps to obtain a more uniform microstructure, thereby ensuring more excellent mechanical properties of the alloy. When the cooling rate is lower than 30 °C / min, the alloy material cannot be rapidly and effectively cooled, which will easily lead to coarse particles and poor mechanical properties.
[0058] Preferably, in the present disclosure, after the hot extrusion process, the obtained copper stick is subjected to acid washing to remove the oxide layer on the alloy surface, after acid washing, the surface of the copper stick is rinsed with water, then naturally dried, and then subjected to a stretching process.
[0059] Preferably, the stretching process adopts cold stretching, the cold stretching pass is at least 1 pass, the deformation amount of each pass is controlled at 15 to 35%, when the deformation amount is too small, the deformation of the surface layer and the core of the alloy is uneven; when the deformation amount is too large, the alloy is prone to cracks or even brittle fracture. It should be noted that when the cold stretching pass is 1 pass, the final annealing can be performed directly after the stretching process. When the cold stretching passes are more than 1 pass, stress relief annealing needs to be performed on the stick between the passes, the stress relief annealing temperature is 200 to 250 °C, and the annealing time is 60 to 90 min. This process not only controls the product dimensions, but also further improves the strength of the material through cold stretching cold work hardening.
[0060] In the present disclosure, the stretched copper stick is annealed at 260 to 330 °C for 120 to 240 min to eliminate the cold stretching stress, promote the recovery process, adjust the distribution of the composite κ phase, and distribute the composite κ phase uniformly and dispersedly in the β phase, thereby achieving a good match between the strength and plasticity of the alloy and improving the comprehensive performance.BRIEF DESCRIPTION OF DRAWINGS
[0061] FIG. 1 is a SEM image (FIG. 1(a)) and an EDS distribution image (FIG. 1(b), FIG. 1(c), FIG. 1(d), FIG. 1(e), FIG. 1(f)) of the brass alloy of Example 2.
[0062] FIGS. 2(a)-2(f) are SEM image (FIG. 2(a)) and EDS distribution image (FIG. 2(b), FIG. 2(c), FIG. 2(d), FIG. 2(e), FIG. 2(f)) of the brass alloy of Example 4.
[0063] FIG. 3 is a SEM image (FIG. 3(a)) and an EDS distribution image (FIG. 3(b), FIG. 3(c), FIG. 3(d), FIG. 3(e), FIG. 3(f)) of the brass alloy of Comparative Example 2.
[0064] FIG. 4 is a main cutting force-time graph (FIG. 4(a)) and a chip morphology graph (FIG. 4(b)) of the brass alloy of Example 2.
[0065] FIG. 5 is a main cutting force-time graph (FIG. 5(a)) and a chip morphology graph (FIG. 5(b)) of the brass alloy of Example 4.
[0066] FIG. 6 is a main cutting force-time graph (FIG. 6(a)) and a chip morphology graph (FIG. 6(b)) of the brass alloy of Comparative Example 1.
[0067] FIG. 7 is an EDS energy spectrum of a composite κ phase at Point A in FIG. 1(a) and Point B in FIG. 2(a).DETAILED DESCRIPTION
[0068] To make the objectives, technical solutions, and advantages of this application clearer, the following will provide a clear and complete description of the technical solution of this application in conjunction with the Examples. Obviously, the described Examples are a part of the Examples of this application, not all of them. The present disclosure will be further described in detail below with reference to Examples.
[0069] The present disclosure is described by taking the manufacturing of a brass alloy product in a stick-shaped form as an example. 12 groups of Examples and 4 groups of Comparative examples were manufactured under different process conditions, and the specific components of the Examples and Comparative examples were shown in Table 1. The specific manufacturing method of the stick-shaped brass alloy product was as follows:
[0070] (1) Batching: the ingredients in Table 1 were batched, high-purity cathode copper or bright wire with a purity of >99.9%, and 0 # zinc ingot were selected as raw materials, and the remaining elements, Si, Ni, Mn, B etc. were added in the form of Cu-24% Si (mass proportion), Cu-20% Ni (mass proportion), Cu-29% Mn (mass proportion), Cu-4% B (mass proportion) intermediate alloy.
[0071] (2) Smelting: the smelting was carried out in a power frequency induction furnace. During smelting, dry charcoal was used to cover the liquid surface, and the thickness of the covering layer was controlled to be 180 to 220 mm to isolate air and reduce the melt oxidation and the loss of volatile elements. The smelting temperature was strictly controlled at 1050 to 1100 °C, during which the alloy elements were uniformly distributed by sufficient stirring.
[0072] (3) Semi-continuous casting: the casting temperature was controlled at 1030 to 1080 °C, and the speed was maintained at 50 to 80 mm / min by using the dummy bar traction mode. In the process, a low-frequency electromagnetic stirring device was used, with a frequency set to 10 to 30 Hz and a current of 20 to 40 A.
[0073] (4) Hot extrusion: the ingot was thermally deformed using a horizontal reverse extruder. Before extrusion, the ingot was heated to 650 to 700 °C by graded gradient heating. The graded gradient heating process sequentially included:
[0074] a low-temperature preheating stage: heating the ingot to 300 to 400 °C within 50 to 60 min;
[0075] a medium-temperature heating stage: heating the ingot to 500 to 600 °C within 40 to 50 min;
[0076] a high-temperature soaking stage: heating the ingot to 650 to 700 °C within 30 to 40 min.
[0077] (5) Pickling: the extruded stick was lifted into a pickling tank to wash off the surface oxide layer, and the pickling solution was a mixed solution of sulfuric acid, nitric acid and water (the volume ratio of sulfuric acid, nitric acid and water was 13:1:10). The pickling time was 3 to 10 min. After pickling, the surface of the bar was rinsed with water, and then dried naturally.
[0078] (6) Stretching: the hot extruded bar was subjected to one-pass cold stretching processing, with a deformation amount of each pass stretching controlled at 15 to 35%.
[0079] (7) The final annealing: the low-temperature annealing treatment was carried out at 260 to 330 °C for 120 to 240 min.
[0080] The key process parameters of Examples and Comparative examples of the present disclosure were shown in Table 2.
[0081] The manufactured alloys of Examples and Comparative examples were subjected to performance tests such as microstructure, mechanical properties, cutting performance and dezincification corrosion at room temperature. The alloy performance target values were as follows: alloy yield strength>200 MPa, tensile strength>500 MPa, elongation>22%, main cutting force Fz<100 N, chip morphology at II grade and above, and dezincification corrosion resistance: transverse average dezincification corrosion depth<410 μm, and longitudinal average dezincification corrosion depth<520 μm.
[0082] A Supra55 type field emission scanning electron microscopy (SEM) produced by Zeiss company, Germany was used to observe and characterize the microstructure of the alloy, and the composition of the phase present in the alloy was analyzed by its matched energy dispersive X-ray spectroscopy (EDS).
[0083] The mechanical properties were tested by a room-temperature tensile test, in accordance with GB / T 228.1~2010 Metallic materials—Tensile testing—Part 1: Method of test at room temperature, on an electronic universal mechanical property testing machine with a strain rate of 1×10−3 s−1.
[0084] The cutting performance of the alloy was evaluated by a turning test. The testing machine tool was a HTC150II type CNC lathe, equipped with a piezoelectric dynamometer to measure the cutting force, using a cemented carbide tool with a rake angle of 10° and a clearance angle of 6°. The cutting parameters were as follows: the rotation speed of the spindle was 1000 r / min, the feed amount was 0.16 mm / r, and the cutting depth was 1.0 mm during external turning. During the test, the equipment was debugged first and a pre-cutting was conducted, then the actual cutting was conducted according to the parameters and the data were recorded, and the process was repeated three times for the same sample to take the average value (during each stable cutting period, the average value of the cutting force was taken as one measurement). The main cutting force Fz of each inventive alloy was measured experimentally. According to chip morphology, chips were classified into three grades. Grade I (excellent): broken chips, such as collapsed chips, needle-shaped chips, and other similar morphologies; grade II (qualified): semi-continuous chips, such as short spiral chips, C-shaped chips, and other similar morphologies; grade III (unqualified): long continuous chips, such as long tightly coiled chips, spiral chips, and other similar morphologies.
[0085] The brass was processed into a specification of 10 mm×10 mm×10 mm, and a dezincification corrosion experiment was performed according to GB / T 10119-2008 standard.
[0086] The test results of microstructure and related performance were shown in Table 3 and Table 4, and FIG. 1 to FIG. 7.
[0087] As shown in Tables 1 and 4, and FIGS. 4 and 5, when the composition and mass percentage of elements satisfied Cu: 58.0 to 62.5%, Si: 0.3 to 1.2%, Ni: 0.1 to 0.5%, Mn: 0.3 to 0.7%, B: 0.005 to 0.025%, and the balance of Zn, the mechanical properties, cutting performance, and corrosion resistance of the alloys of Examples all satisfied the target values, the comprehensive performance of the alloys of the Examples were superior to those of the Comparative examples 1 to 4, the cutting performance of the Comparative example 1 and the Comparative example 3 (H62 alloy) did not satisfy the target values, and the mechanical properties of the Comparative example 2 and the Comparative example 4 (C3604 alloy) did not satisfy the target values.
[0088] As shown in Table 3, the alloys of Examples and Comparative Examples 1, 2 all had an α phase, a β phase and a composite κ phase in particle form, and unlike the traditional silicon brass materials, the γ phase was not detected in the alloys of the present disclosure, but a composite κ phase (Cu, Ni, Mn)5ZnSi was formed, which was dispersed in the β phase (as shown in FIGS. 1 to 3 and FIG. 7). It could be clearly observed that in Examples 1 to 12, the area proportions of the α phase, the β phase and the composite κ phase were 28 to 72%, 26 to 67% and 1 to 5% of the total area of these three phases, respectively, and the average particle size of the composite κ phase was 0.5 to 1.5 μm. Different from Examples 1 to 12, the area proportion and the average particle size of the composite κ phase in Comparative examples 1 to 2 were not within the ranges of Examples 1 to 12, the area proportion of the composite κ phase thereof was 0.8% and 5.6%, respectively, while the area proportion of the α phase in Comparative example 2 was only 5.6%, and the average particle size reached 3.5 μm, which was due to the difference in Si content. In Comparative example 1, the Si content was 0.21%, which was lower than the lower limit of the present disclosure, and the relatively insufficient Si content seriously hindered the effective formation of the composite κ phase, resulting in insufficient total quantity and unsatisfactory distribution state thereof, and insufficient quantity of the composite κ phase significantly weakened the effect of promoting chip fracture, so that the material was easy to generate continuous chips during machining, and the cutting resistance was increased. When the Si content exceeded the upper limit of the present disclosure (Comparative example 2), excess Si was prone to form a Si-rich phase, resulting in an increase in the particle size of the composite κ phase and a decrease in plasticity, which was consistent with the results shown in Table 4 and FIG. 6.
[0089] Si, Ni, and Mn were key constituent elements for forming a composite κ phase. In the present disclosure, by controlling the addition amounts of Si, Ni and Mn and the subsequent processing process, the proportions and sizes of the α phase, the β phase and the composite κ phase in the alloy were controlled to improve the comprehensive performance of the alloy. As shown in the experimental results of Table 1, when the contents of Ni, Mn and Si satisfied Formula 1, and the synergistic optimization index I′ was in the range of 0.10 to 0.40 (Examples 1 to 11), the alloy obtained a relatively ideal microstructure: the composite κ phase was uniformly distributed in the β phase in a fine dispersed form, with the area proportion of 1.0 to 5.0% of the total area of the three phases, and the average particle size of 0.5 to 1.5 μm; meanwhile, the area proportions of the α phase and β phase were maintained within the optimized equilibrium ranges of 28 to 72% and 26 to 67%, respectively.
[0090] Under this structural feature, the alloy had good mechanical properties, cutting performance and dezincification corrosion resistance at the same time. As shown in Table 4, the alloy had a yield strength>200 MPa, a tensile strength>500 MPa, and an elongation>22%, and the alloy had good strength and plasticity. In terms of cutting performance, the main cutting force Fz of the alloy was <100 N, and the chip morphology was at grade II and above. The improvement of the dezincification corrosion resistance was particularly obvious, with a transverse average dezincification corrosion depth of <305 μm and a longitudinal average dezincification corrosion depth of <420 μm.
[0091] Conversely, instability of the Γ value led to structure deterioration.
[0092] Comparative example 1 (Γ=0.601) was unable to provide sufficient Si atoms for the formation of the composite κ phase due to the severe lack of Si content (0.21%), resulting in an area proportion of the composite κ phase of only 0.8%. Correspondingly, the strength of the alloy was low, and its yield strength and tensile strength were 191 MPa and 498 MPa, respectively. Moreover, the cutting performance was poor, the main cutting force Fz of the alloy was increased to 116.5 N, and the chip level was grade III.
[0093] In Comparative Example 2 (Γ=0.097), due to excessive Si (1.58%), the composite κ phase area proportion reached 5.6%, and the area proportion of β phase was significantly increased (88.8%); under this microstructure, although the alloy had good strength (yield strength 362 MPa, tensile strength 651 MPa) and cutting performance (Fz=89.3, grade II chip), the plasticity of the alloy was seriously deteriorated, and the elongation was only 15%.
[0094] The synergistic optimization index Γ was in the range of [0.1, 0.4], and the alloy had good comprehensive performance.
[0095] In Examples 2 to 5, the content of Si element increased from 0.39% to 1.19%, the microstructure of the alloy changed significantly, the area proportion of α phase decreased from 59.1% to 28.6%, the area proportion of β phase increased correspondingly from 39.1% to 66.9%, and the area proportion of composite κ phase increased from 1.8% to 4.5%. The change of Si content led to obvious changes in the mechanical properties and cutting performance of the alloy, the tensile strength was increased from 531 MPa to 621 MPa, and the elongation was decreased from 31% to 23%; the main cutting force Fz was decreased from 88.9 N to 80.1 N, and the chip grade was changed from grade II to grade I.
[0096] Comparing Example 6 and Example 7, the Ni element content was increased from 0.16% to 0.5%. Although the microstructure of the alloy changed little, the dezincification corrosion resistance of the alloy changed significantly. The transverse average dezincification corrosion depth decreased from 303.5 μm to 98.5 μm, and the longitudinal average dezincification corrosion depth decreased from 411.3 μm to 165.1 μm. In contrast, the mechanical properties and cutting performance of the alloys varied less.
[0097] Comparing Example 8 and Example 9, the content of Mn element increased from 0.35% to 0.68%. Similar to the Ni element, the change in Mn element content did not cause a significant change in the alloy microstructure. At this time, the strength of the alloy was slightly increased, and the plasticity was slightly decreased. The dezincification corrosion resistance was also slightly increased, while the cutting performance remained almost unchanged.
[0098] In Example 12, the Si content (0.65%) was moderate, and compared with Example 6, the contents of Ni (0.12%) and Mn (0.33%) were reduced, resulting in a reduction of the synergistic optimization index Γ to 0.066, so that the synergistic effect of elements Si, Ni, Mn and the like failed to reach the optimum. Compared with Example 6, the mechanical properties (yield strength of 251 MPa and tensile strength of 556 MPa) of Example 12 did not change significantly, but its cutting performance and dezincification corrosion resistance were relatively poor.
[0099] In Comparative example 2, the Si content was too high and no B element was added, the average particle size of the composite κ phase of the alloy was 3.5 μm, which was significantly larger than the average particle size of the composite κ phase in other Examples and Comparative examples. Obviously, compared with Example 5, the addition of element B played a key role in refining the composite κ phase. The alloy of the present disclosure was compared with H62 lead-free brass and C3604 lead brass in combination with Comparative example 3 and Comparative example 4. The experimental results showed that although H62 brass had good dezincification corrosion resistant effect, the cutting performance was extremely poor; C3604 brass had very good cutting performance, but its dezincification corrosion resistant effect was extremely poor.
[0100] The corrosion-resistant free-cutting brass alloy material of the present disclosure can be made not only into sticks, but also into wires, pipes, plates, strips, rods or blocks, etc. Through further processing of wires, pipes, plates, strips, rods, or blocks, they can be made into parts for bathroom valves, plumbing connectors, refrigeration, or automobiles. In different application scenarios, brass materials with different ratios of Si, Ni and Mn can be selected, for example, if high corrosion resistance is required, the composition ratio of Example 7 can be selected; if more attention is paid to the mechanical properties of the product, the composition ratio of Example 5 can be selected. In any case, within the composition and content range of the present disclosure, the alloy material of the present disclosure achieves a balance of comprehensive performance.TABLE 1The composition and synergistic optimization index Γof Examples and Comparative examples of the present disclosure.SynergisticComponents / wt %optimizationNO.CuSiNiMnBPbBiZnindex ΓExample 158.520.320.180.310.0120.0060.003Balance0.219Example 259.560.390.300.410.0160.0080.001Balance0.381Example 359.510.610.320.460.0190.0050.004Balance0.266Example 459.490.930.350.440.0180.0030.003Balance0.168Example 559.561.190.360.470.0200.0090.002Balance0.137Example 659.550.620.160.450.0130.0030.003Balance0.128Example 759.480.610.500.410.0150.0060.002Balance0.371Example 859.510.630.300.350.0160.0050.001Balance0.183Example 959.530.650.330.680.0180.0020.002Balance0.376Example 1061.580.310.200.330.0110.0060.003Balance0.269Example 1162.260.350.210.310.0210.0080.003Balance0.229Example 1259.510.650.120.330.0130.0020.006Balance0.066Comparative Example 159.520.210.280.330.0100.0030.002Balance0.601Comparative Example 259.521.580.380.44—0.0050.001Balance0.097Comparative Example 361.50——————Balance—(H62)Comparative Example 457.81————2.68—Balance—(C3604)TABLE 2The key process parameters of Examples and Comparative Examples of the present disclosureHot ExtrusionCastingLow-TemperatureMedium-TemperatureHigh-TemperatureFinalTractionPreheatingHeatingSoakingExtrusionAnnealingTemperature / Speed / Temperature / Time / Temperature / Time / Temperature / Time / Speed / Temperature / Time / NO.°Cmm / min°Cmin°Cmin°Cminmm / s°CminExample 110408034052530456603015280180Example 210507035052530456703015300180Example 310507036055560456703213300180Example 410507036055560486703013300180Example 510507037055560456703013300180Example 610507037055560456703013300180Example 710606038055570456803013320160Example 810606038055570456803014320160Example 910606036055560456803814320160Example 1010606038058560457003014320160Example 1110606038058590457003014320160Example 1210606038055590457003014320160Comparative10407035055560456703013300140Example 1Comparative10605038055590457003011280180Example 2Comparative105010036055570456803015300160Example 3(H62)Comparative105012034055550456603015300160Example 4(C3604)TABLE 3 Microstructure of Examples and ComparativeExamples of the present disclosureArea Proportion / %α-Cuβ-CuZnComposite κAverage Particle Size / μmNO.PhasePhasePhaseComposite κ PhaseExample 162.536.01.50.8Example 259.139.11.81.0Example 350.646.82.60.9Example 443.153.23.71.1Example 528.666.94.51.0Example 652.644.43.00.9Example 750.046.53.51.2Example 856.140.73.21.3Example 955.640.83.61.1Example 1068.230.51.31.2Example 1171.626.81.61.3Example 1255.141.92.90.9Comparative53.645.60.81.1Example 1Comparative5.688.85.63.5Example 2Comparative67.932.1——Example 3(H62)Comparative60.539.5——Example 4(C3604)TABLE 4Related performance of Examples and Comparative Examples of the present disclosureDezincification CorrosionCuttingResistant PerformancePerformanceTransverseLongitudinalMechanical PropertiesMainAverageAverageYieldTensileCuttingDezincificationDezincificationStrength / Strength / Elongation / ForceChipCorrosionCorrosionNO.MPaMPa%Fz / NGradeDepth / μmDepth / μmExample 12285203389.9II286.3391.6Example 22365313188.9II239.7336.1Example 32655762986.3I268.5361.8Example 42986122683.5I268.2344.6Example 53356212380.1I221.6332.1Example 62595612885.8I303.5411.3Example 72685812987.1I98.5165.1Example 82615753086.2I251.2356.1Example 92765892785.1I221.1315.6Example 102115153495.2II162.2226.7Example 112025083698.5II118.9181.6Example 122515563090.0II408512.6Comparative19149835116.5III251.8352.6Example 1Comparative3626511589.3II298.1361.8Example 2Comparative20843138180III191.6286.2Example 3(H62)Comparative1914663167.8I>1000>1000Example 4(C3604)
Claims
1. A corrosion-resistant free-cutting brass alloy, which is composed of the following components in percentage by mass: Cu: 58.0 to 62.5%, Si: 0.3 to 1.2%, Ni: 0.1 to 0.5%, Mn:0.3 to 0.7%, B: 0.005 to 0.025%, and the balance of Zn and inevitable impurity elements, wherein a total content of the inevitable impurity elements is <0.3%, wherein the brass alloy has an α phase, a β phase and a composite κ phase in particle form, and the area proportions of the α phase, the β phase and the composite κ phase are 28 to 72%, 26 to 67% and 1 to 5% of the total area of these three phases, respectively; wherein the composite κ phase is (Cu, Ni, Mn)5ZnSi, has an average particle size of 0.5 to 1.5 μm, and is dispersively distributed in the β phase.
2. The corrosion-resistant free-cutting brass alloy according to claim 1, wherein the brass alloy has a yield strength of >200 MPa, a tensile strength of >500 MPa, an elongation of >22%, a main cutting force during cutting of <100 N, a transverse average dezincification corrosion depth of <410 μm, and a longitudinal average dezincification corrosion depth of <520 μm.
3. The corrosion-resistant free-cutting brass alloy according to claim 1, wherein a mass ratio of Ni, Mn and Si in the brass alloy satisfies:0.1≤Ni·MnSi1.2≤0.4.
4. The corrosion-resistant free-cutting brass alloy according to claim 3, wherein the content of Si is 0.5 to 1.2% in percentage by mass.
5. The corrosion-resistant free-cutting brass alloy according to claim 4, wherein in the brass alloy, the area proportions of the α phase, the β phase and the composite κ phase are 28 to 60%, 40 to 67% and 2.5 to 4.6% of the total area of these three phases, respectively.
6. The corrosion-resistant free-cutting brass alloy according to claim 5, wherein the brass alloy has a yield strength of >255 MPa, a tensile strength of >560 MPa, an elongation of >22%, a main cutting force during cutting of <88 N, a transverse average dezincification corrosion depth of <305 μm, and a longitudinal average dezincification corrosion depth of <420 μm.
7. The corrosion-resistant free-cutting brass alloy according to claim 1, which is composed of the following components in percentage by mass: Si: 0.61 to 1.19%, and / or Ni: 0.16 to 0.50%, and / or Mn: 0.35 to 0.68%, and / or B: 0.013 to 0.020%.
8. The corrosion-resistant free-cutting brass alloy according to claim 1, wherein the α phase is 28.6 to 56.1%, and / or the β phase is 40.7 to 66.9%, and / or the composite κ phase is 2.6 to 4.5%, and / or the average particle size is 0.9 to 1.3 μm.
9. The corrosion-resistant free-cutting brass alloy according to claim 1, which is composed of the following components in percentage by mass: Cu: 59.55%, Si: 0.62%, Ni: 0.16%, Mn: 0.45%, B: 0.013%.
10. The corrosion-resistant free-cutting brass alloy according to claim 1, which is composed of the following components in percentage by mass: Cu: 59.48%, Si: 0.61%, Ni: 0.50%, Mn: 0.41%, B: 0.015%.
11. The corrosion-resistant free-cutting brass alloy according to claim 1, which is composed of the following components in percentage by mass: Cu: 59.53%, Si: 0.65%, Ni: 0.33%, Mn: 0.68%, B: 0.018%.
12. The corrosion-resistant free-cutting brass alloy according to claim 1, wherein the form of the brass alloy is stick-shaped, wire-shaped, pipe-shaped, plate-shaped, strip-shaped, rod-shaped or block-shaped.
13. Application of the corrosion-resistant free-cutting brass alloy according to claim 1 in bathroom valves, plumbing connectors, spare parts and accessories for refrigeration or automobiles.
14. A method for manufacturing a corrosion-resistant free-cutting brass alloy according to claim 1, comprising the following steps: batching and smelting according to target components, and then casting to obtain an ingot; and subjecting the ingot to a processing treatment to manufacture a brass alloy.
15. The method for manufacturing a corrosion-resistant free-cutting brass alloy according to claim 14, wherein the brass alloy is in a stick shaped form, the processing treatment comp rises the following steps:(1) hot extruding: heating the ingot to 650 to 700 °C before extruding, then extruding at an extrusion speed of 10 to 15 mm / s, and cooling at a cooling rate not lower than 30 °C / min after extruding;(2) stretching: stretching the hot extruded stick; and(3) final annealing: annealing the stretched stick at 260 to 330 °C for 120 to 240 min.
16. The method for manufacturing a corrosion-resistant free-cutting brass alloy according to claim 15, wherein in the hot extruding, the ingot is subjected to graded gradient heating before extruding, and the graded gradient heating sequentially comprises:a low-temperature preheating stage: heating the ingot to 300 to 400 °C within 50 to 60 min;a medium-temperature heating stage: heating the ingot to 500 to 600 °C within 40 to 50 min;a high-temperature soaking stage: heating the ingot to 650 to 700 °C within 30 to 40 min.
17. The method for manufacturing a corrosion-resistant free-cutting brass alloy according to claim 16, wherein the stretching is a cold stretching, the cold stretching pass is at least 1 pass, with a deformation amount of each pass controlled within 15 to 35%.
18. The method for manufacturing a corrosion-resistant free-cutting brass alloy according to claim 17, wherein the cold stretching pass is more than 1 pass, and the alloy is subjected to a stress relief annealing between the passes, with an annealing temperature of 200 to 250 °C and an annealing time of 60 to 90 min.