Steel sheet

A steel sheet with controlled composition and microstructure addresses bendability and hydrogen embrittlement issues, enhancing the performance of machine parts made from high-carbon steel.

US20260357395A1Pending Publication Date: 2026-11-12NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
US19/139271
Authority / Receiving Office
US · United States
Patent Type
Applications(United States)
Current Assignee / Owner
Priority Date
2022-12-16
Filing Date
2023-12-14
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

High-carbon steel sheets used as starting materials for machine parts like springs and washers require high bendability and hydrogen embrittlement resistance, which are not adequately addressed in existing technologies.

Method used

A steel sheet composition with C: 0.50 to 0.90%, Si: 0.10 to 0.50%, Mn: 0.20 to 1.30%, and a microstructure of 95% ferrite and cementite particles with specific size and spheroidization ratios, along with controlled C concentration gradients, to enhance hardenability, bendability, and hydrogen embrittlement resistance.

Benefits of technology

The steel sheet achieves excellent bendability, hardenability, and hydrogen embrittlement resistance when formed into machine parts, ensuring high strength and durability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A steel sheet according to the present disclosure has the chemical composition described in the specification. In the steel sheet, a total area fraction of ferrite and cementite particles is 95% or more, the mean grain size of the ferrite is 20.0 μm or less, the mean particle size of the cementite particles is 1.50 μm or less, and a spheroidization ratio of the cementite particles is 85% or more. When the content of C at a position at a depth of 50 μm in the thickness direction from a surface of the steel sheet is represented by “[C]s”, and a content of C at a center position in the thickness direction of the steel sheet is represented by “[C]c”, a C concentration ratio F1 defined by Formula (1) is 0.50 or less.F1=[C]s / [C]c  (1)
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present disclosure relates to a steel sheet, and more particularly relates to a steel sheet that can be utilized as a starting material for machine parts typified by automotive parts.BACKGROUND ART

[0002] Steel sheets that have a high content of C (high-carbon steel sheets) are utilized as a starting material for machine parts typified by automotive parts. A method for producing these machine parts using such kind of steel sheet as a starting material is as follows. The steel sheet is subjected to cold working to form the steel sheet into the shape of the relevant machine part. After the cold working, the steel sheet is subjected to quenching and tempering. A high-strength machine part is produced by the above production process.

[0003] To increase the strength of a machine part, it is required to increase hardenability of the steel sheet that serves as the starting material for the machine part. Therefore, steel sheets in which the hardenability is increased are proposed in Patent Literature 1 and Patent Literature 2.

[0004] Patent Literature 1 discloses a steel sheet having a composition containing, in mass %, C: 0.20 to 0.40%, Si: 0.10% or less, Mn: 0.50% or less, P: 0.03% or less, S: 0.010% or less, sol. Al: 0.10% or less, N: 0.0050% or less, and B: 0.0005 to 0.0050%, and further containing one or more kinds of element among Sb, Sn, Bi, Ge, Te, and Se in a total content of 0.002 to 0.030%, with the balance being Fe and unavoidable impurities. In this steel sheet, the proportion that an amount of dissolved B accounts for in the content of B is 70% or more. Further, the microstructure is composed of ferrite and cementite. In addition, the cementite density in ferrite grains is 0.08 pieces / μm2 or less. In the steel sheet of Patent Literature 1, hardenability is increased by ensuring the amount of dissolved B.

[0005] Patent Literature 2 discloses a steel sheet that has a chemical composition containing, in mass %, C: 0.10% or more to 0.33% or less, Si: 0.01% or more to 0.50% or less, Mn: 0.40% or more to 1.25% or less, P: 0.03% or less, S: 0.01% or less, sol. Al: 0.10% or less, N: 0.01% or less, and Cr: 0.50% or more to 1.50% or less, with the balance being Fe and unavoidable impurities, and has a microstructure containing ferrite and carbides. A ratio of the volume accounted for by ferrite and carbides to the volume of the entire microstructure is 90% or more, and a ratio of the volume accounted for by pro-eutectoid ferrite to the volume of the entire microstructure is 20% or more to 80% or less. The Mn concentration in the carbides is 0.10% or more by mass to 0.50% or less by mass, and a proportion accounted for by the number of carbides having a grain size of 1 μm or more among the total number of carbides is 30% or more to 60% or less. In the steel sheet of Patent Literature 2, the Mn concentration in carbides is reduced. By this means, the dissolution of carbides during quenching is facilitated. As a result, hardenability increases.CITATION LISTPatent LiteraturePatent Literature 1: International Application Publication No. WO2015 / 146173

[0007] Patent Literature 2: International Application Publication No. WO2020 / 175665SUMMARY OF INVENTIONTechnical Problem

[0008] In this connection, among high-carbon steel sheets, steel sheets in which the content of C is 0.50% or more are often used as a starting material for machine parts such as springs and washers. In a process for producing machine parts such as springs and washers, the steel sheet that is the starting material is subjected to bending. Therefore, the steel sheet that is the starting material is required to have high bendability.

[0009] Further, machine parts after quenching have high strength. Therefore, the machine parts are required to have high hydrogen embrittlement resistance. In Patent Literature 1 and Patent Literature 2, bendability and hydrogen embrittlement resistance are not investigated.

[0010] An objective of the present disclosure is to provide a steel sheet in which excellent bendability and excellent hardenability are obtained, and with which excellent hydrogen embrittlement resistance is obtained when made into a machine part.Solution to Problem

[0011] A steel sheet according to the present disclosure consists of, in mass %,

[0012] C: 0.50 to 0.90%,

[0013] Si: 0.10 to 0.50%,

[0014] Mn: 0.20 to 1.30%,

[0015] P: 0.100% or less,

[0016] S: 0.100% or less,

[0017] Al: 0.100% or less,

[0018] Cr: 0.01 to 1.20%,

[0019] N: 0.0150% or less,

[0020] Mo: 0 to 0.500%,

[0021] Ni: 0 to 1.000%,

[0022] B: 0 to 0.0100%,

[0023] V: 0 to 0.500%,

[0024] Nb: 0 to 0.500%,

[0025] Ti: 0 to 0.150%,

[0026] Cu: 0 to 0.15%,

[0027] W: 0 to 0.15%,

[0028] Ta: 0 to 0.15%,

[0029] Sn: 0 to 0.050%,

[0030] Sb: 0 to 0.050%,

[0031] Co: 0 to 0.050%,

[0032] As: 0 to 0.050%,

[0033] Mg: 0 to 0.050%,

[0034] Y: 0 to 0.050%,

[0035] Zr: 0 to 0.050%,

[0036] La: 0 to 0.050%,

[0037] Ce: 0 to 0.050%, and

[0038] Ca: 0 to 0.050%,

[0039] with the balance being Fe and impurities,

[0040] wherein:

[0041] in the microstructure, a total area fraction of ferrite and cementite particles is 95% or more;

[0042] a mean grain size of the ferrite is 20.0 μm or less;

[0043] a mean particle size of the cementite particles is 1.50 μm or less;

[0044] among the cementite particles, when the cementite particles having an aspect ratio of 3.0 or less are defined as “spheroidal cementite particles”, a spheroidization ratio that is a ratio of a total number of the spheroidal cementite particles to a total number of the cementite particles is 85% or more; and

[0045] when a content of C at a position at a depth of 50 μm in a thickness direction from a surface of the steel sheet is represented by “[C]s”, and a content of C at a center position in the thickness direction of the steel sheet is represented by “[C]c”, a C concentration ratio F1 defined by Formula (1) is 0.50 or less.F1=[C]s / [C]c  (1)Advantageous Effects of Invention

[0046] According to the steel sheet of the present disclosure, excellent bendability and excellent hardenability are obtained, and excellent hydrogen embrittlement resistance is obtained when the steel sheet is made into a machine part.DESCRIPTION OF EMBODIMENTS

[0047] The present inventors have conducted studies regarding a steel sheet that has excellent hardenability and excellent bendability, and with which excellent hydrogen embrittlement resistance can be obtained when the steel sheet is made into a machine part. As a result, the present inventors obtained the following findings.

[0048] First, the present inventors conducted studies from the viewpoint of the chemical composition with respect to enhancing hardenability and bendability in a steel sheet in which the content of C is 0.50% or more and also enhancing hydrogen embrittlement resistance when the steel sheet is made into a machine part. As a result, the present inventors have considered that if a steel sheet has a chemical composition consisting of, in mass %, C: 0.50 to 0.90%, Si: 0.10 to 0.50%, Mn: 0.20 to 1.30%, P: 0.100% or less, S: 0.100% or less, Al: 0.100% or less, Cr: 0.01 to 1.20%, N: 0.0150% or less, Mo: 0 to 0.500%, Ni: 0 to 1.000%, B: 0 to 0.0100%, V: 0 to 0.500%, Nb: 0 to 0.500%, Ti: 0 to 0.150%, Cu: 0 to 0.15%, W: 0 to 0.15%, Ta: 0 to 0.15%, Sn: 0 to 0.050%, Sb: 0 to 0.050%, Co: 0 to 0.050%, As: 0 to 0.050%, Mg: 0 to 0.050%, Y: 0 to 0.050%, Zr: 0 to 0.050%, La: 0 to 0.050%, Ce: 0 to 0.050%, Ca: 0 to 0.050%, and the balance: Fe and impurities, there is a possibility that enhancement of hardenability and bendability of the steel sheet, and also enhancement of the hydrogen embrittlement resistance when the steel sheet is made into a machine part can be realized. Therefore, the present inventors have also conducted studies from the viewpoint of the microstructure with regard to means that can enhance the hardenability, bendability, and hydrogen embrittlement resistance in a steel sheet having the chemical composition described above.

[0049] First, with regard to the microstructure of the steel sheet, the present inventors have conducted studies regarding means that contributes to enhancement of hardenability during quenching. The microstructure of a steel sheet having the chemical composition described above is a structure that is substantially composed of ferrite and cementite particles. In order to enhance hardenability of the steel sheet during quenching in a production process when producing a machine part using the steel sheet as a starting material, it is preferable that cementite particles in the steel sheet are easily dissolved during quenching. In order to increase the solubility of cementite particles during quenching, it is preferable that the particle size of the cementite particles is small. In the case of a steel sheet having the chemical composition described above, it is effective to make the mean particle size of cementite particles 1.50 μm or less.

[0050] In addition, with respect to the microstructure of the steel sheet, the present inventors have also conducted studies regarding means that contributes to enhancing bendability. In order to increase the bendability of the steel sheet, it is effective to increase the spheroidization ratio of the cementite particles and to make the mean grain size of the ferrite an appropriate size. Therefore, in the steel sheet of the present embodiment, the spheroidization ratio of cementite particles is made 85% or more, and the mean grain size of ferrite is made 20.0 μm or less.

[0051] However, even when steel sheets were composed as described above, there were still cases where excellent bendability and excellent hydrogen embrittlement resistance were not obtained. Therefore, the present inventors conducted further studies. Here, the present inventors focused on the strength of the outer layer of the steel sheet. If the strength of the outer layer of a steel sheet is equally as high as the strength of the interior of the steel sheet, sufficient bendability will not be obtained, and sufficient hydrogen embrittlement resistance will not be obtained when the steel sheet is formed into a machine part. If the C concentration in the outer layer of the steel sheet is lower than the C concentration in the interior of the steel sheet apart than the outer layer, the bendability of the steel sheet will increase, and the hydrogen embrittlement resistance will also increase while ensuring the strength of a machine part produced using the steel sheet as a starting material.

[0052] The present inventors conducted further studies based on the technical idea described above. As a result, the present inventors have found that when the content of C at a position at a depth of 50 μm in the thickness direction from the surface of a steel sheet is represented by “[C]s”, and the content of C at the center position in the thickness direction of the steel sheet is represented by “[C]c”, if a C concentration ratio F1 defined by Formula (1) is 0.50 or less, excellent bendability is obtained in the steel sheet and, furthermore, excellent hydrogen embrittlement resistance is obtained in a machine part produced using the steel sheet as a starting material.F1=[C]s / [C]c  (1)

[0053] The steel sheet of the present embodiment was completed based on the technical idea described above, and is as follows.

[0054] A steel sheet of a first aspect consists of, in mass %,

[0055] C: 0.50 to 0.90%,

[0056] Si: 0.10 to 0.50%,

[0057] Mn: 0.20 to 1.30%,

[0058] P: 0.100% or less,

[0059] S: 0.100% or less,

[0060] Al: 0.100% or less,

[0061] Cr: 0.01 to 1.20%,

[0062] N: 0.0150% or less,

[0063] Mo: 0 to 0.500%,

[0064] Ni: 0 to 1.000%,

[0065] B: 0 to 0.0100%,

[0066] V: 0 to 0.500%,

[0067] Nb: 0 to 0.500%,

[0068] Ti: 0 to 0.150%,

[0069] Cu: 0 to 0.15%,

[0070] W: 0 to 0.15%,

[0071] Ta: 0 to 0.15%,

[0072] Sn: 0 to 0.050%,

[0073] Sb: 0 to 0.050%,

[0074] Co: 0 to 0.050%,

[0075] As: 0 to 0.050%,

[0076] Mg: 0 to 0.050%,

[0077] Y: 0 to 0.050%,

[0078] Zr: 0 to 0.050%,

[0079] La: 0 to 0.050%,

[0080] Ce: 0 to 0.050%, and

[0081] Ca: 0 to 0.050%,

[0082] with the balance being Fe and impurities,

[0083] wherein:

[0084] in the microstructure, a total area fraction of ferrite and cementite particles is 95% or more;

[0085] a mean grain size of the ferrite is 20.0 μm or less;

[0086] a mean particle size of the cementite particles is 1.50 μm or less;

[0087] among the cementite particles, when the cementite particles having an aspect ratio of 3.0 or less are defined as “spheroidal cementite particles”, a spheroidization ratio that is a ratio of a total number of the spheroidal cementite particles to a total number of the cementite particles is 85% or more; and

[0088] when a content of C at a position at a depth of 50 μm in a thickness direction from a surface of the steel sheet is represented by “[C]s”, and a content of C at a center position in the thickness direction of the steel sheet is represented by “[C]c”, a C concentration ratio F1 defined by Formula (1) is 0.50 or less.F1=[C]s / [C]c  (1)

[0089] A steel sheet of a second aspect is in accordance with the steel sheet of the first aspect, wherein the steel sheet contains one or more kinds of element selected from a group consisting of:

[0090] Mo: 0.001 to 0.500%,

[0091] Ni: 0.001 to 1.000%, and

[0092] B: 0.0001 to 0.0100%.

[0093] A steel sheet of a third aspect is in accordance with the steel sheet of the first or second aspect, wherein the steel sheet contains one or more kinds of element selected from a group consisting of:

[0094] V: 0.001 to 0.500%,

[0095] Nb: 0.001 to 0.500%, and

[0096] Ti: 0.001 to 0.150%.

[0097] A steel sheet of a fourth aspect is in accordance with the steel sheet of any one of the first to third aspects, wherein the steel sheet contains one or more kinds of element selected from a group consisting of:

[0098] Cu: 0.01 to 0.15%,

[0099] W: 0.01 to 0.15%,

[0100] Ta: 0.01 to 0.15%,

[0101] Sn: 0.001 to 0.050%,

[0102] Sb: 0.001 to 0.050%,

[0103] Co: 0.001 to 0.050%,

[0104] As: 0.001 to 0.050%,

[0105] Mg: 0.001 to 0.050%,

[0106] Y: 0.001 to 0.050%,

[0107] Zr: 0.001 to 0.050%,

[0108] La: 0.001 to 0.050%,

[0109] Ce: 0.001 to 0.050%, and

[0110] Ca: 0.001 to 0.050%.

[0111] Hereunder, the steel sheet of the present embodiment is described in detail. Note that, the symbol “%” relating to an element means “mass percent” unless otherwise noted.[Features of Steel Sheet of Present Embodiment]

[0112] The steel sheet of the present embodiment satisfies the following feature 1 to feature 6.(Feature 1)

[0113] The chemical composition consists of, in mass %, C: 0.50 to 0.90%, Si: 0.10 to 0.50%, Mn: 0.20 to 1.30%, P: 0.100% or less, S: 0.100% or less, Al: 0.100% or less, Cr: 0.01 to 1.20%, N: 0.0150% or less, Mo: 0 to 0.500%, Ni: 0 to 1.000%, B: 0 to 0.0100%, V: 0 to 0.500%, Nb: 0 to 0.500%, Ti: 0 to 0.150%, Cu: 0 to 0.15%, W: 0 to 0.15%, Ta: 0 to 0.15%, Sn: 0 to 0.050%, Sb: 0 to 0.050%, Co: 0 to 0.050%, As: 0 to 0.050%, Mg: 0 to 0.050%, Y: 0 to 0.050%, Zr: 0 to 0.050%, La: 0 to 0.050%, Ce: 0 to 0.050%, Ca: 0 to 0.050%, and the balance: Fe and impurities.(Feature 2)

[0114] In the microstructure, the total area fraction of ferrite and cementite particles is 95% or more.(Feature 3)

[0115] The mean grain size of the ferrite is 20.0 μm or less.(Feature 4)

[0116] The mean particle size of the cementite particles is 1.50 μm or less.(Feature 5)

[0117] Among the cementite particles, when the cementite particles having an aspect ratio of 3.0 or less are defined as “spheroidal cementite particles”, a spheroidization ratio that is a ratio of the total number of the spheroidal cementite particles to the total number of the cementite particles is 85% or more.(Feature 6)

[0118] When a content of C at a position at a depth of 50 μm in a thickness direction from a surface of the steel sheet is represented by “[C]s”, and a content of C at a center position in the thickness direction of the steel sheet is represented by “[C]c”, a C concentration ratio F1 defined by Formula (1) is 0.50 or less.F1=[C]s / [C]c  (1)

[0119] Feature 1 to feature 6 are described hereunder.[(Feature 1) Regarding Chemical Composition]

[0120] The chemical composition of the steel sheet of the present embodiment contains the following elements.C: 0.50 to 0.90%

[0121] Carbon (C) increases hardenability of the steel sheet. As a result, by performing quenching in a process for producing a machine part with the steel sheet as a starting material, the strength of the machine part is increased. If the content of C is less than 0.50%, the aforementioned advantageous effect will not be sufficiently obtained. On the other hand, if the content of C is more than 0.90%, the bendability and hydrogen embrittlement resistance of the steel sheet will decrease. Therefore, the content of C is 0.50 to 0.90%.

[0122] A preferable lower limit of the content of C is 0.52%, more preferably is 0.55%, and further preferably is 0.60%.

[0123] A preferable upper limit of the content of C is 0.88%, more preferably is 0.85%, and further preferably is 0.80%.

[0124] A preferable range of the content of C is, for example, 0.52 to 0.88%, more preferably is 0.55 to 0.85%, and further preferably is 0.60 to 0.80%.Si: 0.10 to 0.50%

[0125] Silicon (Si) deoxidizes the steel at the steelmaking stage in the process for producing the steel sheet. Si also increases temper softening resistance of the steel sheet in a case where tempering is performed in a process for producing a machine part with the steel sheet as a starting material. In addition, Si promotes decarburization of the outer layer of the steel sheet during cold-rolled sheet annealing. If the content of Si is less than 0.10%, the aforementioned advantageous effects will not be sufficiently obtained. On the other hand, if the content of Si is more than 0.50%, the strength of the steel sheet will be excessively high due to solid-solution strengthening. Consequently, the bendability of the steel sheet will decrease. Therefore, the content of Si is 0.10 to 0.50%.

[0126] A preferable lower limit of the content of Si is 0.12%, more preferably is 0.15%, and further preferably is 0.20%.

[0127] A preferable upper limit of the content of Si is 0.48%, more preferably is 0.44%, and further preferably is 0.40%.

[0128] A preferable range of the content of Si is, for example, 0.12 to 0.48%, more preferably is 0.15 to 0.44%, and further preferably is 0.20 to 0.40%.Mn: 0.20 to 1.30%

[0129] Manganese (Mn) increases hardenability of the steel sheet. As a result, by performing quenching in a process for producing a machine part with the steel sheet as a starting material, the strength of the machine part is increased. If the content of Mn is less than 0.20%, the aforementioned advantageous effect will not be sufficiently obtained. On the other hand, if the content of Mn is more than 1.30%, the strength of the steel sheet will be excessively high due to solid-solution strengthening. Consequently, the bendability of the steel sheet will decrease. Therefore, the content of Mn is 0.20 to 1.30%.

[0130] A preferable lower limit of the content of Mn is 0.25%, more preferably is 0.30%, and further preferably is 0.35%.

[0131] A preferable upper limit of the content of Mn is 1.25%, more preferably is 1.20%, and further preferably is 1.15%.

[0132] A preferable range of the content of Mn is, for example, 0.25 to 1.25%, more preferably is 0.30 to 1.20%, and further preferably is 0.35 to 1.15%.P: 0.100% or Less

[0133] Phosphorus (P) is an impurity. The content of P may be 0%. If the content of P is more than 0.100%, toughness of the steel sheet will decrease. Therefore, the content of P is 0.100% or less.

[0134] The content of P is preferably as low as possible. That is, preferably the content of P is 0%. However, excessively reducing the content of P will significantly increase the production cost. Therefore, when industrial manufacturing is taken into consideration, a preferable lower limit of the content of P is 0.001%, more preferably is 0.003%, and further preferably is 0.005%.

[0135] A preferable upper limit of the content of P is 0.090%, more preferably is 0.080%, and further preferably is 0.050%.

[0136] A preferable range of the content of P is, for example, 0.001 to 0.090%, more preferably is 0.003 to 0.080%, and further preferably is 0.005 to 0.050%.S: 0.100% or Less

[0137] Sulfur(S) is an impurity. The content of S may be 0%. If the content of S is more than 0.100%, S will form an excessively large amount of sulfides. Consequently, the bendability of the steel sheet will decrease. Therefore, the content of S is 0.100% or less.

[0138] The content of S is preferably as low as possible. That is, preferably the content of S is 0%. However, excessively reducing the content of S will significantly increase the production cost. Therefore, when industrial manufacturing is taken into consideration, a preferable lower limit of the content of S is 0.001%, more preferably is 0.003%, and further preferably is 0.005%.

[0139] A preferable upper limit of the content of S is 0.090%, more preferably is 0.080%, and further preferably is 0.050%.

[0140] A preferable range of the content of S is, for example, 0.001 to 0.090%, more preferably is 0.003 to 0.080%, and further preferably is 0.005 to 0.050%.Al: 0.100% or Less

[0141] Aluminum (Al) is an impurity. The content of Al may be 0%. Al combines with N to form AlN. The AlN refines austenite grains during heating when performing quenching in a process for producing a machine part using the steel sheet as a starting material. Refining of the austenite grains reduces hardenability of the steel sheet. If the content of Al is more than 0.100%, austenite grains will be excessively refined during heating when performing quenching, and hardenability of the steel sheet will markedly decrease. Therefore, the content of Al is 0.100% or less.

[0142] A preferable lower limit of the content of Al is 0.001%, more preferably is 0.005%, and further preferably is 0.010%.

[0143] A preferable upper limit of the content of Al is 0.090%, more preferably is 0.080%, further preferably is 0.070%, and further preferably is 0.050%.

[0144] A preferable range of the content of Al is, for example, 0.001 to 0.090%, more preferably is 0.005 to 0.070%, and further preferably is 0.010 to 0.050%.

[0145] In the chemical composition of the steel sheet of the present embodiment, the term “content of Al” means the content of acid-soluble Al (sol. Al).Cr: 0.01 to 1.20%

[0146] Chromium (Cr) increases hardenability of the steel sheet. As a result, by performing quenching in a process for producing a machine part with the steel sheet as a starting material, the strength of the machine part is increased. If the content of Cr is less than 0.01%, the aforementioned advantageous effect will not be sufficiently obtained. On the other hand, if the content of Cr is more than 1.20%, the strength of the steel sheet will be excessively high. Consequently, the bendability of the steel sheet will decrease. Therefore, the content of Cr is 0.01 to 1.20%.

[0147] A preferable lower limit of the content of Cr is 0.02%, more preferably is 0.03%, and further preferably is 0.05%.

[0148] A preferable upper limit of the content of Cr is 1.15%, more preferably is 1.10%, further preferably is 1.00%, further preferably is 0.70%, and further preferably is 0.50%.

[0149] A preferable range of the content of Cr is, for example, 0.02 to 1.15%, more preferably is 0.03 to 1.10%, and further preferably is 0.05 to 0.50%.N: 0.0150% or Less

[0150] Nitrogen (N) is an impurity that is unavoidably contained. That is, the content of N is more than 0%. N combines with Al to form AlN. The AlN refines austenite grains during heating when performing quenching in a process for producing a machine part using the steel sheet as a starting material. Refining of the austenite grains reduces hardenability of the steel sheet. If the content of N is more than 0.0150%, austenite grains will be excessively refined during heating when performing quenching, and hardenability of the steel sheet will markedly decrease. Therefore, the content of N is 0.0150% or less.

[0151] A preferable lower limit of the content of N is 0.0001%, and more preferably is 0.0005%.

[0152] A preferable upper limit of the content of N is 0.0140%, and more preferably is 0.0130%.

[0153] A preferable range of the content of N is, for example, 0.0001 to 0.0140%, and more preferably is 0.0005 to 0.0130%.

[0154] The balance of the chemical composition of the steel sheet according to the present embodiment is Fe and impurities. Here, the term “impurities” with respect to the chemical composition means substances which are mixed in from ore and scrap as the raw material or from the production environment or the like when industrially producing the steel sheet, and which are permitted within a range that does not adversely affect the steel sheet according to the present embodiment.[Regarding Optional Elements]

[0155] The chemical composition of the steel sheet of the present embodiment may further contain one or more kinds of element selected from the group consisting of a first group to a third group in lieu of a part of Fe.[First Group]

[0156] One or more kinds of element selected from the group consisting of:

[0157] Mo: 0 to 0.500%,

[0158] Ni: 0 to 1.000%, and

[0159] B: 0 to 0.0100%.[Second Group]

[0160] One or more kinds of element selected from the group consisting of:

[0161] V: 0 to 0.500%,

[0162] Nb: 0 to 0.500%, and

[0163] Ti: 0 to 0.150%.[Third Group]

[0164] One or more kinds of element selected from the group consisting of:

[0165] Cu: 0 to 0.15%,

[0166] W: 0 to 0.15%,

[0167] Ta: 0 to 0.15%,

[0168] Sn: 0 to 0.050%,

[0169] Sb: 0 to 0.050%,

[0170] Co: 0 to 0.050%,

[0171] As: 0 to 0.050%,

[0172] Mg: 0 to 0.050%,

[0173] Y: 0 to 0.050%,

[0174] Zr: 0 to 0.050%,

[0175] La: 0 to 0.050%,

[0176] Ce: 0 to 0.050%, and

[0177] Ca: 0 to 0.050%.

[0178] These optional elements are described hereunder.[Regarding First Group (Mo, Ni, and B)]

[0179] The chemical composition of the steel sheet according to the present embodiment may further contain one or more kinds of element selected from the group consisting of Mo, Ni, and B in lieu of a part of Fe. Each of these elements is an optional element, and does not have to be contained. When contained, each of Mo, Ni, and B increases hardenability of the steel sheet.Mo: 0 to 0.500%

[0180] Molybdenum (Mo) is an optional element, and does not have to be contained. That is, the content of Mo may be 0%.

[0181] When Mo is contained, that is, when the content of Mo is more than 0%, Mo increases hardenability of the steel sheet. Therefore, by performing quenching in a process for producing a machine part with the steel sheet as a starting material, the strength of the machine part is increased. In addition, Mo increases the temper softening resistance of the steel sheet in a case where tempering is performed in a process for producing a machine part with the steel sheet as a starting material. If even a small amount of Mo is contained, the aforementioned advantageous effects will be obtained to a certain extent. However, if the content of Mo is more than 0.500%, the strength of the steel sheet will be excessively high. Consequently, the bendability of the steel sheet will decrease. Therefore, the content of Mo is 0 to 0.500%.

[0182] A preferable lower limit of the content of Mo is 0.001%, more preferably is 0.003%, further preferably is 0.005%, and further preferably is 0.010%.

[0183] A preferable upper limit of the content of Mo is 0.450%, more preferably is 0.400%, further preferably is 0.350%, and further preferably is 0.300%.

[0184] A preferable range of the content of Mo is, for example, 0.001 to 0.450%, more preferably is 0.003 to 0.400%, further preferably is 0.005 to 0.350%, and further preferably is 0.010 to 0.300%.Ni: 0 to 1.000%

[0185] Nickel (Ni) is an optional element, and does not have to be contained. That is, the content of Ni may be 0%.

[0186] When Ni is contained, that is, when the content of Ni is more than 0%, Ni increases hardenability of the steel sheet. Therefore, by performing quenching in a process for producing a machine part with the steel sheet as a starting material, the strength of the machine part is increased. In addition, Ni increases the temper softening resistance of the steel sheet in a case where tempering is performed in a process for producing a machine part with the steel sheet as a starting material. If even a small amount of Ni is contained, the aforementioned advantageous effects will be obtained to a certain extent. However, if the content of Ni is more than 1.000%, the strength of the steel sheet will be excessively high. Consequently, the bendability of the steel sheet will decrease. Therefore, the content of Ni is 0 to 1.000%.

[0187] A preferable lower limit of the content of Ni is 0.001%, more preferably is 0.005%, further preferably is 0.007%, and further preferably is 0.010%.

[0188] A preferable upper limit of the content of Ni is 0.950%, more preferably is 0.900%, further preferably is 0.800%, further preferably is 0.700%, and further preferably is 0.600%.

[0189] A preferable range of the content of Ni is, for example, 0.001 to 0.950%, more preferably is 0.005 to 0.900%, further preferably is 0.007 to 0.800%, further preferably is 0.010 to 0.700%, and further preferably is 0.010 to 0.600%.B: 0 to 0.0100%

[0190] Boron (B) is an optional element, and does not have to be contained. That is, the content of B may be 0%.

[0191] When B is contained, that is, when the content of B is more than 0%, B increases hardenability of the steel sheet. Therefore, by performing quenching in a process for producing a machine part with the steel sheet as a starting material, the strength of the machine part is increased. If even a small amount of B is contained, the aforementioned advantageous effect will be obtained to a certain extent. However, if the content of B is more than 0.0100%, B compounds will form. In such case, the strength of the steel sheet will be excessively high. Consequently, the bendability of the steel sheet will decrease. Therefore, the content of B is 0 to 0.0100%.

[0192] A preferable lower limit of the content of B is 0.0001%, more preferably is 0.0003%, and further preferably is 0.0005%.

[0193] A preferable upper limit of the content of B is 0.0090%, more preferably is 0.0080%, further preferably is 0.0070%, further preferably is 0.0060%, and further preferably is 0.0050%.

[0194] A preferable range of the content of B is, for example, 0.0001 to 0.0090%, more preferably is 0.0003 to 0.0080%, further preferably is 0.0005 to 0.0070%, further preferably is 0.0005 to 0.0060%, and further preferably is 0.0005 to 0.0050%.[Regarding Second Group (V, Nb, and Ti)]

[0195] The chemical composition of the steel sheet according to the present embodiment may further contain one or more kinds of element selected from the group consisting of V, Nb, and Ti in lieu of a part of Fe. Each of these elements is an optional element, and does not have to be contained. When contained, each of V, Nb, and Ti forms carbides and thereby suppresses coarsening of austenite grains during quenching heating in a process for producing a machine part with the steel sheet as a starting material. Consequently, the toughness of the machine part is enhanced.V: 0 to 0.500%

[0196] Vanadium (V) is an optional element, and does not have to be contained. That is, the content of V may be 0%.

[0197] When V is contained, that is, when the content of V is more than 0%, V forms carbides and thereby suppresses coarsening of austenite grains during quenching heating in a process for producing a machine part with the steel sheet as a starting material. Consequently, the toughness of the machine part is enhanced. If even a small amount of V is contained, the aforementioned advantageous effect will be obtained to a certain extent. However, if the content of V is more than 0.500%, carbides will excessively form and precipitation strengthen the steel sheet. Consequently, the bendability of the steel sheet will decrease. Therefore, the content of V is 0 to 0.500%.

[0198] A preferable lower limit of the content of V is 0.001%, more preferably is 0.003%, and further preferably is 0.005%.

[0199] A preferable upper limit of the content of V is 0.480%, more preferably is 0.450%, and further preferably is 0.400%.

[0200] A preferable range of the content of V is, for example, 0.001 to 0.480%, more preferably is 0.003 to 0.450%, and further preferably is 0.005 to 0.400%.Nb: 0 to 0.500%

[0201] Niobium (Nb) is an optional element, and does not have to be contained. That is, the content of Nb may be 0%.

[0202] When Nb is contained, that is, when the content of Nb is more than 0%, Nb forms carbides and thereby suppresses coarsening of austenite grains during quenching heating in a process for producing a machine part with the steel sheet as a starting material. Consequently, the toughness of the machine part is enhanced. Further, Nb combines with N and thereby suppresses the formation of nitrides by dissolved B. As a result, hardenability of the steel sheet is increased by the dissolved B. If even a small amount of Nb is contained, the aforementioned advantageous effects will be obtained to a certain extent. However, if the content of Nb is more than 0.500%, carbides will excessively form and precipitation strengthen the steel sheet. Consequently, the bendability of the steel sheet will decrease. Therefore, the content of Nb is 0 to 0.500%.

[0203] A preferable lower limit of the content of Nb is 0.001%, more preferably is 0.003%, and further preferably is 0.005%.

[0204] A preferable upper limit of the content of Nb is 0.480%, more preferably is 0.450%, further preferably is 0.400%, further preferably is 0.350%, and further preferably is 0.300%.

[0205] A preferable range of the content of Nb is, for example, 0.001 to 0.480%, more preferably is 0.003 to 0.450%, further preferably is 0.005 to 0.400%, further preferably is 0.005 to 0.350%, and further preferably is 0.005 to 0.300%.Ti: 0 to 0.150%

[0206] Titanium (Ti) is an optional element, and does not have to be contained. That is, the content of Ti may be 0%.

[0207] When Ti is contained, that is, when the content of Ti is more than 0%, Ti forms carbides and thereby suppresses coarsening of austenite grains during quenching heating in a process for producing a machine part with the steel sheet as a starting material. Consequently, the toughness of the machine part is enhanced. Further, Ti combines with N and thereby suppresses the formation of nitrides by dissolved B. As a result, hardenability of the steel sheet is increased by the dissolved B. If even a small amount of Ti is contained, the aforementioned advantageous effect will be obtained to a certain extent. However, if the content of Ti is more than 0.150%, carbides will excessively form and precipitation strengthen the steel sheet. Consequently, the cold workability of the steel sheet will decrease. Therefore, the content of Ti is 0 to 0.150%.

[0208] A preferable lower limit of the content of Ti is 0.001%, more preferably is 0.003%, and further preferably is 0.005%.

[0209] A preferable upper limit of the content of Ti is 0.145%, more preferably is 0.130%, further preferably is 0.120%, further preferably is 0.100%, and further preferably is 0.080%.

[0210] A preferable range of the content of Ti is 0.001 to 0.145%, more preferably is 0.003 to 0.130%, further preferably is 0.005 to 0.120%, further preferably is 0.005 to 0.100%, and further preferably is 0.005 to 0.080%.[Regarding Third Group (Cu, W, Ta, Sn, Sb, Co, As, Mg, Y, Zr, La, Ce, and Ca)]

[0211] The chemical composition of the steel sheet according to the present embodiment may further contain one or more kinds of element selected from the group consisting of Cu, W, Ta, Sn, Sb, Co, As, Mg, Y, Zr, La, Ce, and Ca in lieu of a part of Fe. Each of these elements is an optional element, and does not have to be contained. That is, the content of these elements may be 0%.

[0212] Each of these elements is a tramp element, and is considered an impurity in the present invention. Therefore, the content of Cu is 0 to 0.15%, the content of W is 0 to 0.15%, Ta: 0 to 0.15%, Sn: 0 to 0.050%, Sb: 0 to 0.050%, Co: 0 to 0.050%, As: 0 to 0.050%, Mg: 0 to 0.050%, Y: 0 to 0.050%, Zr: 0 to 0.050%, La: 0 to 0.050%, Ce: 0 to 0.050%, and Ca: 0 to 0.050%.

[0213] A preferable lower limit of the content of Cu is 0.01%, and more preferably is 0.03%.

[0214] A preferable upper limit of the content of Cu is 0.13%, and more preferably is 0.10%.

[0215] A preferable range of the content of Cu is, for example, 0.01 to 0.13%, and more preferably is 0.03 to 0.10%.

[0216] A preferable lower limit of the content of W is 0.01%, and more preferably is 0.03%.

[0217] A preferable upper limit of the content of W is 0.13%, and more preferably is 0.10%.

[0218] A preferable range of the content of W is, for example, 0.01 to 0.13%, and more preferably is 0.03 to 0.10%.

[0219] A preferable lower limit of the content of Ta is 0.01%, and more preferably is 0.03%.

[0220] A preferable upper limit of the content of Ta is 0.13%, and more preferably is 0.10%.

[0221] A preferable range of the content of Ta is, for example, 0.01 to 0.13%, and more preferably is 0.03 to 0.10%.

[0222] A preferable lower limit of the content of Sn is 0.001%, more preferably is 0.005%, and further preferably is 0.010%.

[0223] A preferable upper limit of the content of Sn is 0.045%, more preferably is 0.040%, and further preferably is 0.035%.

[0224] A preferable range of the content of Sn is, for example, 0.001 to 0.045%, more preferably is 0.005 to 0.040%, and further preferably is 0.010 to 0.035%.

[0225] A preferable lower limit of the content of Sb is 0.001%, more preferably is 0.005%, and further preferably is 0.010%.

[0226] A preferable upper limit of the content of Sb is 0.045%, more preferably is 0.040%, and further preferably is 0.035%.

[0227] A preferable range of the content of Sb is, for example, 0.001 to 0.045%, more preferably is 0.005 to 0.040%, and further preferably is 0.010 to 0.035%.

[0228] A preferable lower limit of the content of Co is 0.001%, more preferably is 0.005%, and further preferably is 0.010%.

[0229] A preferable upper limit of the content of Co is 0.045%, more preferably is 0.040%, and further preferably is 0.035%.

[0230] A preferable range of the content of Co is, for example, 0.001 to 0.045%, more preferably is 0.005 to 0.040%, and further preferably is 0.010 to 0.035%.

[0231] A preferable lower limit of the content of As is 0.001%, more preferably is 0.005%, and further preferably is 0.010%.

[0232] A preferable upper limit of the content of As is 0.045%, more preferably is 0.040%, and further preferably is 0.035%.

[0233] A preferable range of the content of As is, for example, 0.001 to 0.045%, more preferably is 0.005 to 0.040%, and further preferably is 0.010 to 0.035%.

[0234] A preferable lower limit of the content of Mg is 0.001%, more preferably is 0.005%, and further preferably is 0.010%.

[0235] A preferable upper limit of the content of Mg is 0.045%, more preferably is 0.040%, and further preferably is 0.035%.

[0236] A preferable range of the content of Mg is, for example, 0.001 to 0.045%, more preferably is 0.005 to 0.040%, and further preferably is 0.010 to 0.035%.

[0237] A preferable lower limit of the content of Y is 0.001%, more preferably is 0.005%, and further preferably is 0.010%.

[0238] A preferable upper limit of the content of Y is 0.045%, more preferably is 0.040%, and further preferably is 0.035%.

[0239] A preferable range of the content of Y is, for example, 0.001 to 0.045%, more preferably is 0.005 to 0.040%, and further preferably is 0.010 to 0.035%.

[0240] A preferable lower limit of the content of Zr is 0.001%, more preferably is 0.005%, and further preferably is 0.010%.

[0241] A preferable upper limit of the content of Zr is 0.045%, more preferably is 0.040%, and further preferably is 0.035%.

[0242] A preferable range of the content of Zr is, for example, 0.001 to 0.045%, more preferably is 0.005 to 0.040%, and further preferably is 0.010 to 0.035%.

[0243] A preferable lower limit of the content of La is 0.001%, more preferably is 0.005%, and further preferably is 0.010%.

[0244] A preferable upper limit of the content of La is 0.045%, more preferably is 0.040%, and further preferably is 0.035%.

[0245] A preferable range of the content of La is, for example, 0.001 to 0.045%, more preferably is 0.005 to 0.040%, and further preferably is 0.010 to 0.035%.

[0246] A preferable lower limit of the content of Ce is 0.001%, more preferably is 0.005%, and further preferably is 0.010%.

[0247] A preferable upper limit of the content of Ce is 0.045%, more preferably is 0.040%, and further preferably is 0.035%.

[0248] A preferable range of the content of Ce is, for example, 0.001 to 0.045%, more preferably is 0.005 to 0.040%, and further preferably is 0.010 to 0.035%.

[0249] A preferable lower limit of the content of Ca is 0.001%, more preferably is 0.005%, and further preferably is 0.010%.

[0250] A preferable upper limit of the content of Ca is 0.045%, more preferably is 0.040%, and further preferably is 0.035%.

[0251] A preferable range of the content of Ca is, for example, 0.001 to 0.045%, more preferably is 0.005 to 0.040%, and further preferably is 0.010 to 0.035%.[Method for Measuring Chemical Composition of Steel Sheet]

[0252] The chemical composition of the steel sheet of the present embodiment can be measured by a well-known composition analysis method. Specifically, a drill is used to collect a machined chip from a position at a depth of 0.1 mm or more on the inner side from the surface of the steel sheet. The collected machined chip is dissolved in acid to obtain a liquid solution. The liquid solution is subjected to ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry) to perform elementary analysis of the chemical composition. The content of C and the content of S are determined by a well-known high-frequency combustion method (combustion-infrared absorption method). The content of N is determined using a well-known inert gas fusion-thermal conductivity method.

[0253] Note that, the content of each element is taken as a numerical value up to the least significant digit of the content of each element defined in the present embodiment that is obtained by rounding off a fraction of the measured numerical value based on the significant figures defined in the present embodiment. For example, the content of C in the steel sheet of the present embodiment is defined as a numerical value up to the second decimal place. Therefore, the content of C is taken as a numerical value up to the second decimal place that is obtained by rounding off the third decimal place of the measured numerical value.

[0254] Similarly, for the content of each element other than the content of C in the steel sheet of the present embodiment also, a value obtained by rounding off a fraction of the numerical value of the measured value up to the least significant digit defined in the present embodiment is taken as the content of the relevant element. Note that, the term “rounding off” means rounding down if the fraction is less than 5, and rounding up if the fraction is 5 or more.[(Feature 2) Regarding Microstructure]

[0255] In the microstructure of the steel sheet of the present embodiment, the total area fraction of ferrite and cementite particles is 95% or more. That is, the microstructure of the steel sheet of the present embodiment is substantially composed of ferrite and cementite particles.

[0256] In the microstructure, the structure other than the ferrite and the cementite particles is, for example, one or more types selected from the group consisting of bainite, martensite, and pearlite.

[0257] Preferably, the total area fraction of ferrite and cementite particles in the microstructure is 96% or more, more preferably is 97% or more, further preferably is 98% or more, and further preferably is 99% or more. The microstructure may be a structure that consists of ferrite and cementite particles.

[0258] A preferable range of the total area fraction of ferrite and cementite particles is 96 to 100%, more preferably is 97 to 100%, further preferably is 98 to 100%, and further preferably is 99 to 100%.

[0259] If the total area fraction of ferrite and cementite particles is 95% or more, on the precondition that feature 1 and feature 3 to feature 6 are satisfied, excellent bendability will be obtained, and high hydrogen embrittlement resistance will be obtained when the steel sheet is made into a machine part.[Method for Measuring Total Area Fraction of Ferrite and Cementite Particles in Microstructure]

[0260] The total area fraction of ferrite and cementite particles in the microstructure can be measured by the following method.

[0261] A test specimen with dimensions of 15 mm in the rolling elongation direction of the steel sheet×10 mm in the sheet width direction×the sheet thickness is taken from the center part of the width of the steel sheet. Among the surfaces of the test specimen, a surface with dimensions of 15 mm in the rolling elongation direction×the sheet thickness is defined as an observation surface. The observation surface of the test specimen is mirror-polished. The mirror-polished observation surface is subjected to etching using a 3% nitric acid alcohol (nital etching reagent). Secondary electron images of an arbitrary five observation visual fields on the etched observation surface are observed using a scanning electron microscope (SEM) at a magnification of 1000×. Each observation field is set as a rectangle with dimensions of 100 μm×120 μm.

[0262] In the observation visual fields, ferrite and cementite particles exhibit different contrast and different morphology from other structures (bainite, martensite, pearlite, and the like). Therefore, the ferrite and the cementite particles in the observation visual fields are identified based on contrast and morphology.

[0263] The total area fraction (%) of ferrite and cementite particles is determined based on the total area of ferrite and the total area of cementite particles in the five observation visual fields, and the total area of the five observation visual fields.[(Feature 3) Regarding Mean Grain Size of Ferrite]

[0264] In the steel sheet of the present embodiment, in addition, the mean grain size of ferrite is 20.0 μm or less.

[0265] If the mean grain size of the ferrite is more than 20.0 μm, bendability will decrease. Furthermore, if the mean grain size of the ferrite is more than 20.0 μm, the annealing time will be long due to coarsening of the ferrite grains. In such case, concentration of alloying elements into the cementite will progress and hardenability will decrease. Therefore, the mean grain size of the ferrite is 20.0 μm or less.

[0266] A preferable upper limit of the mean grain size of the ferrite is 19.5 μm, more preferably is 19.0 μm, further preferably is 18.5 μm, and further preferably is 18.0 μm.

[0267] The lower limit of the mean grain size of the ferrite is not particularly limited. However, excessive refinement of ferrite will excessively increase the yield strength of the steel sheet. In such case, the machining load during bending will excessively increase. Therefore, a preferable lower limit of the mean grain size of the ferrite is 5.0 μm. A more preferable lower limit of the mean grain size of the ferrite is 5.2 μm, further preferably is 5.5 μm, further preferably is 5.7 μm, further preferably is 6.0 μm, and further preferably is 6.5 μm.

[0268] A preferable range of the mean grain size of the ferrite is, for example, 5.0 to 20.0 μm, more preferably is 5.2 to 19.5 μm, further preferably is 5.5 to 19.0 μm, further preferably is 5.7 to 18.5 μm, further preferably is 6.0 to 18.0 μm, and further preferably is 6.5 to 18.0 μm.[Method for Measuring Mean Grain Size of Ferrite]

[0269] The mean grain size of the ferrite can be measured by the following method.

[0270] A test specimen with dimensions of 15 mm in the rolling elongation direction of the steel sheet×10 mm in the sheet width direction×the sheet thickness is taken from the center part of the width of the steel sheet. Among the surfaces of the test specimen, a surface with dimensions of 15 mm in the rolling elongation direction×the sheet thickness is defined as an observation surface. The observation surface of the test specimen is mirror-polished. After mirror polishing, the observation surface is subjected to etching using a 3% nital etching reagent. On the etched observation surface, secondary electron images are captured using a scanning electron microscope (SEM) in an arbitrary five observation visual fields at a position at a depth of ¼ of the thickness from the surface of the steel sheet. The grain size number of the ferrite is determined by the intercept method in accordance with JIS G 0551:2020. At such time, the magnification of the SEM is selected within the range of 500 to 3000× so that the number of ferrite grains intercepted by one line segment is at least 10 or more in one visual field. An intercept length is determined for each of the five observation visual fields. The grain size number of ferrite is determined based on the arithmetic average value of the intercept lengths for the five observation visual fields. The mean grain size (μm) of the ferrite is determined from the obtained grain size number.

[0271] A value obtained by rounding off the second decimal place of the obtained value (that is, the value to the first decimal place) is adopted as the mean grain size of ferrite.[(Feature 4) Regarding Mean Particle Size of Cementite Particles]

[0272] In the steel sheet of the present embodiment, the mean particle size of the cementite particles is 1.50 μm or less.

[0273] If the mean particle size of the cementite particles is large, bendability of the steel sheet will decrease. Furthermore, if the mean particle size of the cementite particles is large, the cementite particles will not sufficiently dissolve during heating in a quenching process in a process for producing a machine part with the steel sheet as a starting material. In such case, sufficient hardenability will not be obtained in the steel sheet. As a result, sufficient strength will not be obtained in a machine part produced using the steel sheet as a starting material.

[0274] If the mean particle size of the cementite particles is 1.50 μm or less, the cementite particles will be sufficiently small. Therefore, sufficient bendability will be obtained in the steel sheet. Furthermore, the cementite particles will sufficiently dissolve during heating in a quenching process, and the hardenability of the steel sheet will increase.

[0275] A preferable upper limit of the mean particle size of the cementite particles is 1.45 μm, more preferably is 1.40 μm, further preferably is 1.35 μm, and further preferably is 1.30 μm.

[0276] To enhance hardenability, a small mean particle size of the cementite particles is preferable. However, if the mean particle size of the cementite particles is too small, the hardness of the steel sheet will be too high and the cold workability will decrease. Therefore, a preferable lower limit of the mean particle size of the cementite particles is 0.05 μm, more preferably is 0.10 μm, further preferably is 0.15 μm, and further preferably is 0.20 μm.

[0277] A preferable range of the mean particle size of the cementite particles is, for example, 0.05 to 1.50 μm, more preferably is 0.10 to 1.45 μm, further preferably is 0.15 to 1.40 μm, further preferably is 0.20 to 1.35 μm, and further preferably is 0.20 to 1.30 μm.[Method for Measuring Mean Particle Size of Cementite Particles]

[0278] The mean particle size of the cementite particles can be determined by the following method.

[0279] A test specimen with dimensions of 15 mm in the rolling elongation direction of the steel sheet×10 mm in the sheet width direction×the sheet thickness is taken from a position that is at the center part of the width of the steel sheet. Among the surfaces of the test specimen, a surface with dimensions of 15 mm in the rolling elongation direction×the sheet thickness is defined as an observation surface.

[0280] The observation surface of the test specimen is mirror-polished. After mirror polishing, the observation surface is subjected to etching using picral etchant. On the etched observation surface, secondary electron images are captured in an arbitrary five observation visual fields at a position at a depth of ¼ of the sheet thickness from the surface of the steel sheet. Specifically, the five observation visual fields are observed at a magnification of 2000× using a scanning electron microscope (SEM), and the aforementioned secondary electron images are captured. Each observation field is set as a rectangle with dimensions of 50 μm×60 μm.

[0281] In each secondary electron image, cementite particles are identified based on contrast. The area of each identified cementite particle is determined, and the equivalent circular diameter of each cementite particle is determined based on the area. The determined equivalent circular diameter is taken as the particle size of the relevant cementite particle. Note that, well-known image processing software is used to determine the particle size.

[0282] The arithmetic average value of the particle sizes of the cementite particles obtained in the five observation visual fields is taken as the mean particle size (μm) of the cementite particles.

[0283] A value obtained by rounding off the third decimal place of the obtained value (that is, the value to the second decimal place) is adopted as the mean particle size of the cementite particles.[(Feature 5) Regarding Spheroidization Ratio]

[0284] In the steel sheet of the present embodiment, among a plurality of cementite particles, cementite particles having an aspect ratio of 3.0 or less are defined as spheroidal cementite particles. A spheroidization ratio that is a ratio of the total number of the spheroidal cementite particles to the total number of the plurality of cementite particles is 85% or more.

[0285] If the spheroidization ratio is 85% or more, on the precondition that feature 1 to feature 4 and feature 6 are satisfied, excellent bendability will be obtained in the steel sheet. Therefore, in the steel sheet of the present embodiment, the spheroidization ratio is 85% or more.

[0286] A higher spheroidization ratio is preferable. A preferable lower limit of the spheroidization ratio is 87%, more preferably is 89%, further preferably is 91%, and further preferably is 95%.

[0287] A preferable range of the spheroidization ratio is, for example, 85 to 100%, more preferably is 87 to 100%, further preferably is 89 to 100%, further preferably is 91 to 100%, and further preferably is 95 to 100%.[Method for Measuring Spheroidization Ratio]

[0288] The spheroidization ratio can be measured by the following method.

[0289] The aspect ratio of each of a plurality of cementite particles identified in five observation visual fields by the above-described [Method for measuring mean particle size of cementite particles] is determined. Specifically, the maximum distance obtained when the contour of a cementite particle is positioned between two parallel line segments is defined as the major axis. In addition, when the contour of the relevant cementite particle is positioned between two line segments that are two line segments parallel to the major axis, the distance between the relevant two line segments (in other words, the width in a direction perpendicular to the major axis) is defined as the minor axis.

[0290] The aspect ratio of each cementite particle (=major axis / minor axis) is determined based on the obtained major axis and minor axis. Among all of the cementite particles in the five observation visual fields, cementite particles having an aspect ratio of 3.0 or less are identified as “spheroidal cementite particles”. The ratio of the total number of spheroidal cementite particles to the total number of the plurality of cementite particles in the five observation visual fields is defined as the spheroidization ratio (%).

[0291] A value obtained by rounding off the first decimal place of the obtained value (that is, an integer) is adopted as the spheroidization ratio.[(Feature 6) Regarding C Concentration Ratio F1]

[0292] In the steel sheet of the present embodiment, when the content of C at a position at a depth of 50 μm in the thickness direction from the surface of the steel sheet is represented by “[C]s”, and the content of C at the center position in the thickness direction of the steel sheet is represented by “[C]c”, a C concentration ratio F1 defined by Formula (1) is 0.50 or less.F1=[C]s / [C]c  (1)

[0293] Note that, the center position in the thickness direction of the steel sheet is located further inside the steel sheet than the position at a depth of 50 μm in the thickness direction from the surface of the steel sheet.

[0294] If the C concentration ratio F1 is higher than 0.50, the strength of the outer layer portion of the steel sheet will be high, and the strength of an outer layer portion of a machine part produced using the steel sheet as a starting material will also be high. In such case, the bendability of the steel sheet will decrease, and furthermore, the hydrogen embrittlement resistance of the machine part produced using the steel sheet as a starting material will decrease.

[0295] If the C concentration ratio F1 is 0.50 or less, the strength of the outer layer portion of the steel sheet can be sufficiently suppressed. Therefore, excellent bendability will be obtained in the steel sheet. In addition, excellent hydrogen embrittlement resistance will be obtained in a machine part produced using the steel sheet as a starting material.

[0296] A preferable upper limit of the C concentration ratio F1 is 0.49, more preferably is 0.48, further preferably is 0.47, further preferably is 0.46, and further preferably is 0.45.

[0297] The lower limit of the C concentration ratio F1 is not particularly limited. In a steel sheet satisfying feature 1 to feature 6, the lower limit of the C concentration ratio F1 is, for example, 0.05, more preferably is 0.10, and further preferably is 0.15.

[0298] A preferable range of the C concentration ratio F1 is, for example, 0.05 to 0.50, more preferably is 0.10 to 0.49, further preferably is 0.15 to 0.48, further preferably is 0.15 to 0.47, further preferably is 0.15 to 0.46, and further preferably is 0.15 to 0.45.[Method for Measuring C Concentration Ratio F1]

[0299] The C concentration ratio F1 can be measured by the following method.

[0300] A test specimen with dimensions of 15 mm in the rolling elongation direction of the steel sheet×10 mm in the sheet width direction×the sheet thickness is taken from the center part of the width of the steel sheet. Among the surfaces of the test specimen, a surface with dimensions of 15 mm in the rolling elongation direction×the sheet thickness is defined as an observation surface. The observation surface of the test specimen is mirror-polished. On the observation surface after mirror polishing, the content of C (mass %) at a position at a depth of 50 μm in the thickness direction from the steel sheet surface is measured at 300 measurement positions at a pitch of 1 μm in the longitudinal direction of the steel sheet using an electron probe micro analyzer (EPMA). The arithmetic average value of the contents of C (mass %) obtained at the 300 points is defined as [C]s. In addition, at the center position in the thickness direction of the steel sheet, the content of C (mass %) is measured at 300 measurement positions at a pitch of 1 μm in the longitudinal direction of the steel sheet using an electron probe micro analyzer (EPMA). The arithmetic average value of the contents of C (mass %) obtained at the 300 points is defined as [C]c. The C concentration ratio F1 is determined based on Formula (1) using the obtained [C]s and [C]c. Note that, measurement by the EPMA is performed under the following conditions.

[0301] Acceleration voltage: 15.0 kV

[0302] Irradiation current: 0.30 μA

[0303] Irradiation time: 50 ms

[0304] Beam diameter: 1 μm

[0305] A value obtained by rounding off the third decimal place of the relevant obtained value (that is, the value to the second decimal place) is adopted as [C]s (mass %) and [C]c (mass %), respectively. A value obtained by rounding off the third decimal place of the relevant obtained value (that is, the value to the second decimal place) is adopted as the C concentration ratio F1.[Advantageous Effects of Steel Sheet of Present Embodiment]

[0306] Excellent bendability is obtained in the steel sheet of the present embodiment that satisfies feature 1 to feature 6 described above. Further, with the steel sheet of the present embodiment, sufficient hardenability is obtained when performing quenching during a process for producing a machine part with the steel sheet as a starting material. In addition, excellent hydrogen embrittlement resistance is obtained in a machine part produced using the steel sheet of the present embodiment as a starting material.[Regarding Bendability]

[0307] Bendability is evaluated by the following method.[Bendability Evaluation Method]

[0308] A sheet-like test specimen is taken from a center part of the width of the steel sheet. With regard to the shape of the sheet-like test specimen, the test specimen is taken so as to have dimensions of 15 mm in the rolling elongation direction of the steel sheet×30 mm in the sheet width direction×the sheet thickness. The sheet-like test specimen is subjected to a 90° V-bending test. Specifically, a die and a pushing punch are used to perform a 90° V-bending process at the center position of the width (30 mm) of the sheet-like test specimen. A folding line formed in the sheet-like test specimen by the V bending is to be made parallel to the rolling elongation direction of the steel sheet (L-axis bending). The R of the pushing punch used in the 90° V-bending test is to be made 0.1 mm. The presence or absence of a crack in the surface of the sheet-like test specimen after the 90° V-bending test is confirmed by visual observation. If no crack is confirmed, it is determined that excellent bendability is obtained.[Regarding Hardenability]

[0309] Hardenability is evaluated by the following method.[Hardenability Evaluation Method](Ac1 Transformation Point Measurement)

[0310] A cylindrical test specimen with a diameter of 3 mm and a length of 10 mm is taken from the center part of the width of the steel sheet. The longitudinal direction of the cylindrical test specimen is to be parallel to the rolling elongation direction of the steel sheet. The thermal expansion coefficient during heating is measured using a Formaster tester. The Ac1 transformation point is determined based on the obtained thermal expansion coefficient.(Maximum Quenching Hardness Measurement)

[0311] A sheet-like test specimen is taken from the center part of the width of the steel sheet. With regard to the shape of the sheet-like test specimen, the test specimen is taken so as to have dimensions of 15 mm in the rolling elongation direction of the steel sheet×30 mm in the sheet width direction×the sheet thickness.

[0312] The sheet-like test specimen is heated at 1000 °C for 20 minutes using a salt bath. Thereafter, the sheet-like test specimen is immersed in water in a water tank to quench the sheet-like test specimen. After quenching, the sheet-like test specimen is cut into two equal parts in the width direction of the steel sheet. The cut surface is mirror-polished. A Vickers hardness test in accordance with JIS Z 2244:2009 is carried out at three arbitrary points at the center position in the thickness direction of the cut surface after mirror polishing. At such time, the test force is set to 98 N. The arithmetic average value of the obtained Vickers hardnesses is defined as a maximum quenching hardness HD0 (HV).(Hardenability Evaluation)

[0313] A sheet-like test specimen is taken from a center part of the width of the steel sheet. With regard to the shape of the sheet-like test specimen, the test specimen is taken so as to have dimensions of 15 mm in the rolling elongation direction of the steel sheet×30 mm in the sheet width direction×the sheet thickness.

[0314] The sheet-like test specimen is immersed in a salt bath at a temperature of the Ac1 transformation point+80 °C for 10 minutes. Thereafter, the sheet-like test specimen that has been taken out from the salt bath is immersed in water in a water tank for quenching. After quenching, the sheet-like test specimen is cut into two equal parts in the sheet width direction. The cut surface is mirror-polished. A Vickers hardness test in accordance with JIS Z 2244:2009 is carried out at three arbitrary points at the center position in the thickness direction of the cut surface after mirror polishing. At such time, the test force is set to 98 N. The arithmetic average value of the obtained Vickers hardnesses is defined as a quenching hardness HD1 (HV). If the obtained quenching hardness HD1 is 0.95 times or more the maximum quenching hardness HD0, it is determined that sufficient hardenability is obtained in the steel sheet.[Regarding Hydrogen Embrittlement Resistance]

[0315] The hydrogen embrittlement resistance is evaluated by the following method.[Hydrogen Embrittlement Resistance Evaluation Method]

[0316] A sheet-like test specimen is taken from the center position of the width of the steel sheet. With regard to the shape of the sheet-like test specimen, the test specimen is taken so as to have dimensions of 30 mm in the rolling elongation direction of the steel sheet×100 mm in the sheet width direction×the sheet thickness. The sheet-like test specimen is subjected to bending into a U-shape by a pressing bend method to prepare a U-bend test specimen with a curvature radius R of 2.0 mm. Specifically, U-bending is performed at the center position of the width (100 mm) of the sheet-like test specimen. The bend line formed in the sheet-like test specimen by the U-bending is to be parallel to the rolling elongation direction of the steel sheet (L-axis bending).

[0317] The U-bend test specimen is immersed in a salt bath at a temperature of the Ac1 point+80 °C for 10 minutes. After immersion, the U-bend test specimen is removed from the salt bath and immersed in a water tank for quenching. After quenching, the U-bend test specimen is subjected to tempering at 250 °C for one hour. In the U-bend test specimen after tempering, a pair of ends of unbent parts of the U-bend test specimen are fastened with a bolt to cause elastic deformation so that opposing unbent parts become parallel to each other.

[0318] The U-bend test specimen in which the unbent parts were made parallel is subjected to a delayed fracture promoting test. Specifically, the U-bend test specimen is immersed for 100 hours in hydrochloric acid with a pH of 1. After 100 hours elapse, the presence or absence of a crack in the bent part of the U-bend test specimen is confirmed by visual observation. If no crack is confirmed, it is determined that excellent hydrogen embrittlement resistance is obtained.[Uses of Steel Sheet]

[0319] The steel sheet of the present embodiment is suitable as a starting material for machine parts typified by automotive parts. The machine parts are, for example, springs and washers of automobiles. Note that, the steel sheet of the present embodiment may also be used for uses other than machine parts in which bendability and hydrogen embrittlement resistance are required.[Method for Producing Steel Sheet]

[0320] An example of a method for producing the steel sheet of the present embodiment will now be described. The method for producing the steel sheet described hereunder is one example for producing the steel sheet of the present embodiment. Accordingly, a steel sheet composed as described above may also be produced by a production method other than the production method described hereunder. However, the production method described hereunder is a preferable example of a method for producing the steel sheet of the present embodiment.

[0321] One example of a method for producing the steel sheet of the present embodiment includes the following steps.

[0322] (Step 1) Starting material preparation process

[0323] (Step 2) Hot rolling process

[0324] (Step 3) Hot-rolled sheet annealing process

[0325] (Step 4) Cold rolling process

[0326] (Step 5) Cold-rolled sheet annealing process

[0327] Each of these steps is described hereunder.[(Step 1) Starting Material Preparation Process]

[0328] In the starting material preparation process, a starting material satisfying feature 1 is prepared. The starting material is produced, for example, by the following method. A molten steel in which the content of each element in the chemical composition is within the range of the present embodiment is produced. The molten steel is used to produce a starting material (a slab or an ingot) by a casting process. For example, the molten steel is used to produce a slab by a well-known continuous casting process. Alternatively, the molten steel is used to produce an ingot by a well-known ingot-making process.[(Step 2) Hot Rolling Process]

[0329] In the hot rolling process, the prepared starting material (slab or ingot) is subjected to hot rolling to produce a steel sheet. The hot rolling process includes a rough rolling process of subjecting the starting material to rough rolling to produce a sheet bar (intermediate steel sheet), and a finish rolling process of subjecting the sheet bar to finish rolling to produce a steel sheet.

[0330] In the rough rolling process, the starting material (slab or ingot) is heated in a reheating furnace. The heated starting material is rolled using a roughing mill to produce a sheet bar. The heating temperature of the starting material in the rough rolling process is, for example, 1100 to 1250 °C. The furnace time of the starting material in the reheating furnace is 30 mins or more, and preferably is 60 mins or more. Although the upper limit of the furnace time is not particularly limited, for example, the furnace time is 300 minutes.

[0331] In the finish rolling process, the sheet bar is subjected to further rolling (finish rolling) using a finish rolling mill to thereby produce a steel sheet. The finish rolling mill includes a plurality of stands arranged in a row. Each stand includes a pair of work rolls. The surface temperature of the steel sheet on the exit side of the stand which is the last stand to perform rolling of the steel sheet among the plurality of stands of the finish rolling mill is defined as the rolling finishing temperature (°C). In the present embodiment, the rolling finishing temperature is 830 to 950 °C. Further, among the plurality of stands arranged in a row in the finish rolling mill, the rolling reduction at the rearmost stand which subjects the steel sheet to rolling reduction is defined as the rolling reduction in the final pass (%). In the present embodiment, the rolling reduction in the final pass is 5 to 25%. The hot-rolled steel sheet after finish rolling is coiled into a coil shape. The coiling temperature CT will be described later. The hot-rolled steel sheet in a coil shape is cooled to normal temperature.[(Step 3) Hot-Rolled Sheet Annealing Process]

[0332] In the hot-rolled sheet annealing process, the hot-rolled steel sheet is subjected to hot-rolled sheet annealing under well-known conditions. In the hot-rolled sheet annealing process, the annealing temperature is, for example, 500 to 770 °C, and the holding time at the annealing temperature is, for example, 5 to 80 hours. In the hot-rolled sheet annealing process, so-called “batch annealing” is performed. Further, the annealing is performed in a reducing atmosphere.[(Step 4) Cold Rolling Process]

[0333] In the cold rolling process, the steel sheet after the hot-rolled sheet annealing process is subjected to cold rolling. The cold rolling is performed using a cold rolling mill. A cold rolling reduction CR in the cold rolling process is described later.[(Step 5) Cold-Rolled Sheet Annealing Process]

[0334] In the cold-rolled sheet annealing process, the cold-rolled steel sheet after the cold rolling process is subjected to cold-rolled sheet annealing. In the cold-rolled sheet annealing process of the present embodiment, open coil annealing (OCA) is applied. The cold-rolled steel sheet is subjected to annealing using an open coil annealing furnace under conditions which satisfy conditions 3 to 6 to be described later. By this means, the degree of recrystallization of ferrite and the degree of precipitation of cementite particles are adjusted. In addition, the C concentration ratio F1 is adjusted.[Regarding Condition 1 to Condition 6]

[0335] In the above-described step 1 to step 5, the following condition 1 to condition 6 are to be satisfied.

[0336] (Condition 1) Coiling temperature CT in step 2:550 to 750 °C

[0337] (Condition 2) Cold rolling reduction CR in step 4: more than 35 to 60%

[0338] (Condition 3) Annealing temperature T1 in step 5:650 to 750 °C

[0339] (Condition 4) Holding time t1 in step 5:5 to 40 hours

[0340] (Condition 5) Atmosphere in annealing furnace in step 5:93 to 97% by volume hydrogen-3 to 7% by volume nitrogen atmosphere

[0341] (Condition 6) Dew point of annealing furnace in step 5: +25 to +65 °C.

[0342] Each condition is described hereunder.[(Condition 1) Regarding Coiling Temperature CT]

[0343] In the hot rolling process, the coiling temperature CT influences the spheroidization ratio of cementite particles. If the coiling temperature CT is 750 °C or less, the cementite particles formed in the hot-rolled steel sheet will be distributed sufficiently evenly. In such case, the spheroidization ratio of the cementite particles will be increased by performing annealing. Therefore, it is preferable to set the coiling temperature CT to 750 °C or less. On the other hand, the lower limit of the coiling temperature CT is not particularly limited. However, in consideration of equipment constraints, a preferable lower limit of the coiling temperature CT is 550 °C.[(Condition 2) Regarding Cold Rolling Reduction CR]

[0344] In the cold rolling process, the cold rolling reduction CR is defined by the following formula.Cold rolling reduction CR (%)=(1−(thickness of cold-rolled steel sheet after cold rolling process / thickness of hot-rolled steel sheet before cold rolling process))×100

[0345] If the cold rolling reduction CR is more than 35%, sufficient strain will be introduced into the steel sheet. In such case, in the annealing process that is the next process, spheroidization of cementite particles will be promoted and the spheroidization ratio will be 85% or more. On the other hand, if the cold rolling reduction CR is 60% or less, the strain introduced into the steel sheet will be appropriate. In such case, the ferrite will be moderately refined, and the mean grain size of the ferrite will be 5.0 μm or more.[(Condition 3) Regarding Annealing Temperature T1]

[0346] In the cold-rolled sheet annealing process, an annealing temperature T1 adjusts the spheroidization ratio of cementite particles in the steel sheet. If the annealing temperature T1 is less than 650 °C, spheroidization of cementite particles will be insufficient and the spheroidization ratio of cementite particles will be less than 85%. In addition, the C concentration ratio F1 will be more than 0.50. On the other hand, if the annealing temperature T1 is more than 750 °C, the annealing temperature will be too high. In such case, spheroidization of cementite will be insufficient, and the spheroidization ratio of cementite particles will be less than 85%.[(Condition 4) Regarding holding time t1 at annealing temperature T1]

[0347] In the cold-rolled sheet annealing process, a holding time t1 at the annealing temperature T1 influences the size of the ferrite and the size of the cementite particles in the steel sheet. Specifically, if the holding time t1 is less than five hours, cementite particles will not spheroidize sufficiently. On the other hand, if the holding time t1 is more than 40 hours, the ferrite and the cementite particles will coarsen because the holding time is too long. As a result, the mean grain size of the ferrite may become more than 20.0 μm and the mean particle size of the cementite particles may become more than 1.50 μm.[(Condition 5) Regarding Atmosphere in Annealing Furnace]

[0348] The atmosphere in the open coil annealing furnace in the cold-rolled sheet annealing process is to be made a 93 to 97% by volume hydrogen-3 to 7% by volume nitrogen atmosphere. In this case, the C concentration ratio F1 can be made 0.50 or less.[(Condition 6) Regarding Dew Point in Annealing Furnace]

[0349] The dew point in the atmosphere in the open coil annealing furnace in the cold-rolled sheet annealing process is to be made +25 to +65 °C. Specifically, the dew point is adjusted to within the above dew point range using humidified nitrogen. If the dew point is less than +25 °C, the C concentration ratio F1 will be more than 0.50. On the other hand, if the dew point is more than +65 °C, the equipment load will be excessive. Therefore, the dew point in the cold-rolled sheet annealing process is to be within the range of +25 to +65 °C.

[0350] A steel sheet satisfying feature 1 to feature 6 can be produced by the above production process.

[0351] Note that, if annealing is performed in the hot-rolled sheet annealing process so as to satisfy condition 5 and condition 6 instead of in a reducing atmosphere, and in addition, annealing is performed in the cold-rolled sheet annealing process in a reducing atmosphere, a steel sheet satisfying feature 1 to feature 6 cannot be obtained. If annealing that satisfies condition 5 and condition 6 is performed in the hot-rolled sheet annealing process, a decarburized layer will be formed in the steel sheet after the hot-rolled sheet annealing process. However, the decarburized layer will be extended by the cold rolling process after the hot-rolled sheet annealing process. As a result, the decarburized layer will be made thinner by the cold rolling process. Furthermore, when the cold-rolled sheet annealing process is performed, C in the steel sheet will be diffused and recarburization will occur, and the C concentration will be made uniform throughout the steel sheet. As a result, a steel sheet satisfying feature 6 will not be obtained.

[0352] According to the present embodiment, in the hot-rolled sheet annealing process, annealing is performed in a reducing atmosphere, and in addition, in the cold-rolled sheet annealing process that is the final step, annealing is performed under conditions that satisfy condition 3 to condition 6. By this means, a steel sheet in which the C concentration ratio is 0.50 or less, and which satisfies feature 1 to feature 6 can be produced.

[0353] The advantageous effects of steel sheet of the present embodiment will now be described more specifically by way of examples. The conditions adopted in the following examples are one example of conditions adopted for confirming the feasibility and advantageous effects of the steel sheet of the present embodiment. Accordingly, the steel sheet of the present embodiment is not limited to this one example of conditions.EXAMPLES

[0354] Steel sheets having the chemical compositions shown in Table 1-1 and Table 1-2 were produced.TABLE 1-1Chemical Composition (unit is mass percent; balance isSteelFe and impurities)NumberCSiMnPSAlCrN10.660.460.960.0160.0770.0070.550.002920.810.450.210.0530.0030.0320.630.009530.770.130.720.0420.0930.0160.440.002140.650.310.410.0090.0310.0540.340.008550.540.111.190.0450.0050.0760.410.012260.780.500.390.0420.0650.0950.360.010770.560.480.860.0780.0040.0830.680.001880.650.120.430.0320.0420.0470.240.001890.820.411.200.0460.0090.0900.450.0148100.730.120.920.0550.0710.0530.550.0130110.730.250.410.0480.0570.0640.440.0125120.580.131.090.0630.0440.0070.650.0004130.660.141.030.0060.0650.0270.470.0012140.550.440.260.0130.0620.0440.650.0129150.840.150.930.0410.0970.0550.320.0069160.590.230.240.0770.0890.0010.270.0095170.770.141.150.0720.0290.0670.240.0139180.730.151.250.0790.0850.0820.470.0067190.570.171.280.0050.0720.0450.260.0032200.850.101.280.0210.0450.0460.360.0012210.610.130.540.0720.0320.0730.580.0118220.760.190.880.0550.0690.0730.640.0085230.820.420.930.005—0.0490.450.0070240.830.430.220.0640.0650.0120.230.0069250.720.350.540.0660.0600.0660.410.0136260.770.120.980.0620.0140.0250.270.0062270.530.490.820.0060.0840.0080.350.0052280.620.260.360.0690.0580.0730.250.0079290.630.110.890.0780.0250.0640.330.0135300.690.490.900.0470.0360.0720.460.0046310.780.420.820.0540.0490.0360.670.0112320.940.360.450.0180.0600.0220.480.0012330.310.131.250.0580.0140.0450.310.0088340.530.081.230.0560.0060.0870.380.0098350.711.190.740.0040.0580.0590.430.0058360.820.170.110.0370.0510.0260.640.0043370.620.271.980.0410.0040.0350.250.0111380.700.461.050.0740.0610.0371.980.0071390.830.190.250.0420.0790.0670.660.0097TABLE 1-2Chemical Composition (unit is mass percent;balance is Fe and impurities)MaximumOptional ElementsQuenchingSteelFirst GroupSecond GroupAC1HardnessNumberMoNiBVNbTiOtherPointHD0 (HV)1———————7358372———————7448813——0.0008——0.043—7278734——0.0024——0.032—7338335———————7207756———————7398757———————73978780.025——————72683390.360——————73088310—0.095—————72486211—0.832—————71986212———0.009———72679813———0.425———72483714————0.008——74478115————0.427——72388616—————0.012—73280417—————0.143—71987318——0.0073————72286219——————Cu: 0.1471979320——————W: 0.1271888721——————Ta: 0.1273181422——————Sn: 0.04373087123——————Sb: 0.03873388324——————Co: 0.04573788425——————As: 0.04173485926——————Mg: 0.04172187327——————Y: 0.03973476928——————Zr: 0.03773181929——————La: 0.03572282430——————Ce: 0.03373584931——————Ca: 0.04073887532———————73789333———————71959734———————71976935———————75785636———————73888337———————71481938———————759852391.010——————737884Specifically, molten steels were subjected to continuous casting to produce slabs with a thickness of 250 mm. Each slab was subjected to a hot rolling process. Specifically, the slab was heated for 120 mins at 1100 to 1250 °C. After heating, the slab was subjected to rolling with a roughing mill to produce a sheet bar. Further, the sheet bar was rolled using a finish rolling mill to produce a hot-rolled steel sheet having a thickness of 3.5 mm. The rolling finishing temperature of each test number was 830 to 950 °C. The rolling reduction in the final pass was in the range of 5 to 25%. The hot-rolled steel sheet after the finish rolling was coiled into a coil shape. The hot-rolled steel sheet in a coiled shape was allowed to cool to normal temperature. The coiling temperature CT in the hot rolling process of each test number was as shown in Table 2.TABLE 2HotColdCold-Rolled SheetRollingRollingAnnealingCoilingCold RollingDewTestSteelTemperatureReductionT1t1PointNumberNumberCT (°C)CR (%)(°C)(h)(°C)11648507102536226424571025403364650710204544635507003041546485571025436564550690304275632507002544866365071020439663050710253510664250710253111763945710303812863450710204413964850710254414106414571025421511650507102544161263255710254217136375070025431814650507102542191563445700254220166425071025442117645557002541221864150710254123196394569030412420640507102545252164255710254226226374571020422723646506903044282463250710254029256445070030443026642557102042312763250690253032286484571025423329648557102543343063550710253235316365070030423632635457102043373463750710252938356385069030423936639557102541403764650690254341386425071020454239635457102544432632506908042442063050710704345364845690300468631557102504721638507102504856403071025424966343070025435023630307103042519755407002042529655406402044The hot-rolled steel sheet was subjected to a hot-rolled sheet annealing process. In the hot-rolled sheet annealing process, the annealing temperature was 500 to 770 °C, and the holding time at the annealing temperature was 5 to 80 hours. The hot-rolled sheet annealing was performed in a reducing atmosphere. The hot-rolled steel sheet after the hot-rolled sheet annealing process was subjected to a cold rolling process to produce a cold-rolled steel sheet. The cold rolling reduction CR in the cold rolling process was as shown in Table 2. The cold-rolled steel sheet after cold rolling was subjected to a cold-rolled sheet annealing process. In the cold-rolled sheet annealing process, open coil annealing was performed. The annealing temperature T1, holding time t1, and dew point in the cold-rolled sheet annealing process were as shown in Table 2. Note that, for each test number, the atmosphere in the open coil annealing furnace was made an atmosphere composed of 95% by volume hydrogen and 5% by volume nitrogen. Steel sheets were produced by the above production process.[Evaluation Tests]

[0357] The produced steel sheet of each test number was subjected to the following tests.

[0358] (Test 1) Chemical composition measurement test

[0359] (Test 2) Test to measure total area fraction of ferrite and cementite particles

[0360] (Test 3) Test to measure mean grain size of ferrite

[0361] (Test 4) Test to measure mean particle size of cementite particles

[0362] (Test 5) Test to measure spheroidization ratio of cementite particles

[0363] (Test 6) Test to measure C concentration ratio F1

[0364] (Test 7) Bendability evaluation test

[0365] (Test 8) Hardenability evaluation test

[0366] (Test 9) Hydrogen embrittlement resistance evaluation test

[0367] Hereunder, test 1 to test 9 are described.[(Test 1) Chemical Composition Measurement Test]

[0368] The chemical composition of the steel sheet of each steel number was measured based on the method described above in the section [Method for measuring chemical composition of steel sheet]. The chemical composition of the steel sheet of each steel number determined as a result was as described in Table 1-1 and Table 1-2.[(Test 2) Test to Measure Total Area Fraction of Ferrite and Cementite Particles]

[0369] The total area fraction of ferrite and cementite particles in the steel sheet of each test number was determined based on the method described above in the section [Method for measuring total area fraction of ferrite and cementite particles in microstructure]. As a result, it was determined that the total area fraction of ferrite and cementite particles was 95% or more in the steel sheet of each test number.[(Test 3) Test to Measure Mean Grain Size of Ferrite]

[0370] The mean grain size of ferrite in the steel sheet of each test number was determined based on the method described above in the section [Method for measuring mean grain size of ferrite]. The determined results are shown in Table 3.TABLE 3MaximumFerriteCementiteQuenchingGrainParticleSpheroidizationQuenchingHardnessTestSteelSizeSizeRatioHardnessHD0NumberNumber(μm)(μm)(%)F1 ≤0.50HD1 (HV)(HV)1117.10.6197T8158372210.30.3697T864881339.60.4596T863873448.60.3287T830833549.70.3195T829833659.30.2595T7437757512.50.7886T737775867.50.2888T837875968.50.6190T8648751067.80.7586T8438751177.60.4498T7607871289.30.3595T8018331397.70.3097T876883141010.20.3195T85486215119.50.3386T85286216128.30.3296T79679817139.20.3294T807837181410.40.2992T780781191512.40.3190T878886201610.70.3387T78980421179.50.3190T83487322189.20.2986T836862231910.30.3387T78479324209.50.3288T84788725217.10.2994T791814262213.50.3195T850871272310.60.3498T842883282410.30.3390T87188429258.10.3291T833859302610.40.3197T860873312710.70.3398T765769322810.00.3198T80481933297.60.3199T80182434308.60.3293T83884935319.40.3391T83787536328.90.3095T88989337349.20.2696F74276938358.70.2688T842856393610.10.2289T55588340377.70.2692T80281941389.10.3595T712852423912.40.2995T77888443222.41.5999T821881442021.61.5897T82988745310.60.5695F8548734689.50.4294F82783347218.20.3692F79481448510.10.2680T7747754969.50.2983T85087550238.30.3078T8768835198.90.2682T8318835297.60.2483F878883QuenchingHardnessLowerHydrogenTestLimitEmbrittlementNumber(HV)HardenabilityBendabilityResistanceRemarks1795EEEInventiveExample2837EEEInventiveExample3829EEEInventiveExample4791EEEInventiveExample5791EEEInventiveExample6736EEEInventiveExample7736EEEInventiveExample8831EEEInventiveExample9831EEEInventiveExample10831EEEInventiveExample11748EEEInventiveExample12791EEEInventiveExample13839EEEInventiveExample14819EEEInventiveExample15819EEEInventiveExample16758EEEInventiveExample17795EEEInventiveExample18742EEEInventiveExample19842EEEInventiveExample20763EEEInventiveExample21829EEEInventiveExample22819EEEInventiveExample23753EEEInventiveExample24843EEEInventiveExample25773EEEInventiveExample26827EEEInventiveExample27839EEEInventiveExample28840EEEInventiveExample29816EEEInventiveExample30829EEEInventiveExample31730EEEInventiveExample32778EEEInventiveExample33783EEEInventiveExample34806EEEInventiveExample35831EEEInventiveExample36848EBBComparativeExample37730EBBComparativeExample38813EBEComparativeExample39839BEEComparativeExample40778EBEComparativeExample41810BBEComparativeExample42840BBEComparativeExample43837BBEComparativeExample44843BBEComparativeExample45829EBBComparativeExample46791EBBComparativeExample47773EBBComparativeExample48736EBEComparativeExample49831EBEComparativeExample50839EBEComparativeExample51839BBEComparativeExample52839EBBComparativeExample[(Test 4) Test to Measure Mean Particle Size of Cementite Particles]

[0371] The mean particle size of cementite particles (μm) in the steel sheet of each test number was determined based on the method described above in the section [Method for measuring mean particle size of cementite particles]. The determined mean particle size of cementite particles (μm) is shown in Table 3.[(Test 5) Test to Measure Spheroidization Ratio of Cementite Particles]

[0372] The spheroidization ratio of cementite particles in the steel sheet of each test number was determined based on the method described above in the section [Method for measuring spheroidization ratio]. The determined spheroidization ratio is shown in Table 3.[(Test 6) Test to Measure C Concentration Ratio F1]

[0373] The C concentration ratio F1 in the steel sheet of each test number was determined based on the method described above in the section [Method for measuring C concentration ratio F1]. The determined C concentration ratio F1 is shown in Table 3. In Table 3, “T (True)” in the column “F1≤0.50” indicates that F1 was 0.50 or less, and “F (False)” indicates that F1 was more than 0.50.[(Test 7) Bendability Evaluation Test]

[0374] The bendability of the steel sheet of each test number was evaluated based on the method described above in the section [Bendability evaluation method]. The evaluation result is shown in the column “Bendability” in Table 3. If the result of visually confirming whether or not a crack was present in the surface of the sheet-like test specimen after the 90° V-bending test was that no crack was confirmed, it was determined that excellent bendability was obtained (indicated by “E (Excellent)” in the column “Bendability” in Table 3). On the other hand, if a crack was confirmed, it was determined that excellent bendability was not obtained (indicated by “B (Bad)” in the column “Bendability” in Table 3).[(Test 8) Hardenability Evaluation Test]

[0375] The hardenability during quenching of the steel sheet of each test number was evaluated based on the method described above in the section [Hardenability evaluation method]. The column “Quenching Hardness Lower Limit (HV)” in Table 3 shows the value of the maximum quenching hardness HD0×0.95. If the quenching hardness HD1 was equal to or more than the quenching hardness lower limit, it was determined that sufficient hardenability was obtained (indicated by “E (Excellent)” in the column “Hardenability” in Table 3). On the other hand, if the quenching hardness HD1 was less than the quenching hardness lower limit, it was determined that sufficient hardenability was not obtained (indicated by “B (Bad)” in the column “Hardenability” in Table 3). In addition, if the maximum quenching hardness HD0 in the steel sheet was less than 600 HV, it was determined that sufficient strength as a machine part was not obtained.[(Test 9) Hydrogen Embrittlement Resistance Evaluation Test]

[0376] The hydrogen embrittlement resistance of a simulated machine part (U-bend test specimen) based on the assumption of producing a machine part using the steel sheet of the respective test numbers as a starting material was evaluated based on the method described above in the section [Hydrogen embrittlement resistance evaluation method]. The evaluation result is shown in the column “Hydrogen Embrittlement Resistance” in Table 3. The presence or absence of a crack at the bent part of the U-bend test specimen was confirmed by visual observation. If no crack was confirmed, it was determined that excellent hydrogen embrittlement resistance was obtained (indicated by “E (Excellent)” in the column “Hydrogen Embrittlement Resistance” in Table 3). On the other hand, if a crack was confirmed, it was determined that excellent hydrogen embrittlement resistance was not obtained (indicated by “B (Bad)” in the column “Hydrogen Embrittlement Resistance” in Table 3).[Evaluation Results]

[0377] Referring to Table 1-1, Table 1-2, Table 2, and Table 3, in Test Nos. 1 to 35, the chemical composition was appropriate and the production conditions were also appropriate. Therefore, the steel sheets of these test numbers satisfied feature 1 to feature 6. As a result, excellent hardenability, excellent bendability, and excellent hydrogen embrittlement resistance were obtained.

[0378] On the other hand, in Steel No. 33, the content of C was too low. Therefore, the maximum quenching hardness HD0 was a low hardness of less than 600 HV, and sufficient strength required as a part was not obtained.

[0379] In Test No. 36, the content of C was too high. Therefore, sufficient bendability and sufficient hydrogen embrittlement resistance were not obtained.

[0380] In Test No. 37, the content of Si was too low. Therefore, decarburization during cold-rolled sheet annealing was insufficient, and the C concentration ratio F1 was more than 0.50. As a result, sufficient bendability and sufficient hydrogen embrittlement resistance were not obtained.

[0381] In Test No. 38, the content of Si was too high. Therefore, the strength of the steel sheet became excessively high due to solid-solution strengthening, and sufficient bendability was not obtained.

[0382] In Test No. 39, the content of Mn was too low. Therefore, sufficient hardenability was not obtained.

[0383] In Test No. 40, the content of Mn was too high. Therefore, the strength of the steel sheet became excessively high due to solid-solution strengthening, and sufficient bendability was not obtained.

[0384] In Test No. 41, the content of Cr was too high. Therefore, sufficient hardenability was not obtained. In addition, sufficient bendability was not obtained.

[0385] In Test No. 42, the content of Mo was too high. Therefore, sufficient hardenability was not obtained. In addition, sufficient bendability was not obtained.

[0386] In Test Nos. 43 and 44, although the chemical composition was appropriate, the holding time t1 at the tempering temperature T1 in the cold-rolled sheet annealing process was too long. Therefore, the mean grain size of the ferrite was more than 20.0 μm, and the mean particle size of the cementite particles was more than 1.50 μm. As a result, sufficient hardenability could not be obtained, and sufficient bendability was not obtained.

[0387] In Test Nos. 45 to 47, although the chemical composition was appropriate, the dew point during cold-rolled sheet annealing was less than 25 °C. Therefore, the C concentration ratio F1 was more than 0.50. As a result, sufficient bendability and sufficient hydrogen embrittlement resistance were not obtained.

[0388] In Test Nos. 48 to 50, although the chemical composition was appropriate, the cold rolling reduction CR was 35% or less, which was low. Therefore, the spheroidization ratio of cementite particles was less than 85%, which was too low. As a result, sufficient bendability was not obtained.

[0389] In Test No. 51, although the chemical composition was appropriate, the coiling temperature CT was too high. Therefore, the spheroidization ratio of cementite particles was less than 85%, which was too low. As a result, sufficient hardenability and sufficient bendability were not obtained.

[0390] In Test No. 52, although the chemical composition was appropriate, the annealing temperature T1 in the cold-rolled sheet annealing process was too low. Therefore, the spheroidization ratio of cementite particles was less than 85%, which was too low. In addition, the C concentration ratio F1 was more than 0.50. As a result, sufficient bendability and sufficient hydrogen embrittlement resistance were not obtained.

[0391] An embodiment of the present disclosure has been described above. However, the embodiment described above is merely an example for carrying out the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiment, and can be implemented by appropriately modifying the above-described embodiment within a range not departing from the gist thereof.

Claims

1-4. (canceled)5. A steel sheet, comprising, in mass %,C: 0.50 to 0.90%,Si: 0.10 to 0.50%,Mn: 0.20 to 1.30%,P: 0.100% or less,S: 0.100% or less,Al: 0.100% or less,Cr: 0.01 to 1.20%,N: 0.0150% or less,Mo: 0 to 0.500%,Ni: 0 to 1.000%,B: 0 to 0.0100%,V: 0 to 0.500%,Nb: 0 to 0.500%,Ti: 0 to 0.150%,Cu: 0 to 0.15%,W: 0 to 0.15%,Ta: 0 to 0.15%,Sn: 0 to 0.050%,Sb: 0 to 0.050%,Co: 0 to 0.050%,As: 0 to 0.050%,Mg: 0 to 0.050%,Y: 0 to 0.050%,Zr: 0 to 0.050%,La: 0 to 0.050%,Ce: 0 to 0.050%, andCa: 0 to 0.050%,with the balance being Fe and impurities,wherein:in the microstructure, a total area fraction of ferrite and cementite particles is 95% or more;a mean grain size of the ferrite is 20.0 μm or less;a mean particle size of the cementite particles is 1.50 μm or less;among the cementite particles, when the cementite particles having an aspect ratio of 3.0 or less are defined as “spheroidal cementite particles”, a spheroidization ratio that is a ratio of a total number of the spheroidal cementite particles to a total number of the cementite particles is 85% or more; andwhen a content of C at a position at a depth of 50 μm in a thickness direction from a surface of the steel sheet is represented by “[C]s”, and a content of C at a center position in the thickness direction of the steel sheet is represented by “[C]c”, a C concentration ratio F1 defined by Formula (1) is 0.50 or less,F1=[C]s / [C]c  (1).

6. The steel sheet according to claim 5, comprising one or more of:Mo: 0.001 to 0.500%,Ni: 0.001 to 1.000%, andB: 0.0001 to 0.0100%.

7. The steel sheet according to claim 5, comprising one or more of:V: 0.001 to 0.500%,Nb: 0.001 to 0.500%, andTi: 0.001 to 0.150%.

8. The steel sheet according to claim 6, comprising one or more of:V: 0.001 to 0.500%,Nb: 0.001 to 0.500%, andTi: 0.001 to 0.150%.

9. The steel sheet according to claim 5, comprising one or more of:Cu: 0.01 to 0.15%,W: 0.01 to 0.15%,Ta: 0.01 to 0.15%,Sn: 0.001 to 0.050%,Sb: 0.001 to 0.050%,Co: 0.001 to 0.050%,As: 0.001 to 0.050%,Mg: 0.001 to 0.050%,Y: 0.001 to 0.050%,Zr: 0.001 to 0.050%,La: 0.001 to 0.050%,Ce: 0.001 to 0.050%, andCa: 0.001 to 0.050%.

10. The steel sheet according to claim 6, comprising one or more of:Cu: 0.01 to 0.15%,W: 0.01 to 0.15%,Ta: 0.01 to 0.15%,Sn: 0.001 to 0.050%,Sb: 0.001 to 0.050%,Co: 0.001 to 0.050%,As: 0.001 to 0.050%,Mg: 0.001 to 0.050%,Y: 0.001 to 0.050%,Zr: 0.001 to 0.050%,La: 0.001 to 0.050%,Ce: 0.001 to 0.050%, andCa: 0.001 to 0.050%.

11. The steel sheet according to claim 7, comprising one or more of:Cu: 0.01 to 0.15%,W: 0.01 to 0.15%,Ta: 0.01 to 0.15%,Sn: 0.001 to 0.050%,Sb: 0.001 to 0.050%,Co: 0.001 to 0.050%,As: 0.001 to 0.050%,Mg: 0.001 to 0.050%,Y: 0.001 to 0.050%,Zr: 0.001 to 0.050%,La: 0.001 to 0.050%,Ce: 0.001 to 0.050%, andCa: 0.001 to 0.050%.

12. The steel sheet according to claim 8, comprising one or more of:Cu: 0.01 to 0.15%,W: 0.01 to 0.15%,Ta: 0.01 to 0.15%,Sn: 0.001 to 0.050%,Sb: 0.001 to 0.050%,Co: 0.001 to 0.050%,As: 0.001 to 0.050%,Mg: 0.001 to 0.050%,Y: 0.001 to 0.050%,Zr: 0.001 to 0.050%,La: 0.001 to 0.050%,Ce: 0.001 to 0.050%, andCa: 0.001 to 0.050%.