Austenitic stainless steel containing carbon and nitrogen
An austenitic stainless steel with optimized chromium, manganese, nickel, carbon, and nitrogen content stabilizes the austenite phase, enhancing corrosion resistance and cryogenic toughness, addressing the high-cost nickel reliance of conventional steels and meeting LNG vessel requirements.
Patent Information
- Application Number
- US19/724871
- Authority / Receiving Office
- US · United States
- Patent Type
- Applications(United States)
- Current Assignee / Owner
- Priority Date
- 2024-01-15
- Filing Date
- 2026-06-30
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional austenitic stainless steels like STS 304 and STS 316 rely heavily on high-cost nickel for cryogenic performance, necessitating the development of low-cost alternatives that maintain a stable austenite phase and meet stringent mechanical safety and corrosion resistance requirements for LNG vessel applications.
An austenitic stainless steel composition with 16 to 20 wt% chromium, 4.5 to 9 wt% manganese, 3 to 6 wt% nickel, 0.05 to 0.12 wt% carbon, and 0.15 to 0.30 wt% nitrogen, with a combined carbon and nitrogen content of 0.25 to 0.32 wt%, optimized to stabilize the austenite phase and enhance corrosion resistance and cryogenic toughness.
The alloy achieves superior corrosion resistance and cryogenic toughness, with reduced corrosion-induced weight loss and impact absorbed energy exceeding 41 J at -196 °C, meeting IMO regulatory standards and offering cost-competitiveness.
Smart Images

Figure US20260357404A1-D00001 
Figure US20260357404A1-D00002 
Figure US20260357404A1-D00003
Abstract
Description
CROSS REFERENCE TO RELATED APPLICATIONS
[0001] This application is a continuation application filed under 35 U.S.C. § 111(a) and claims the benefit under 35 U.S.C. §§ 120 and 365(c) of International Application No. PCT / KR 2025 / 000905, filed on Jan. 15, 2025, which claims priority to Korean Patent Application No. 10-2024-0006022, filed on Jan. 15, 2024, the disclosures of which are incorporated herein by reference in their entireties.BACKGROUNDTechnical Field
[0002] Exemplary embodiments relate to an austenitic stainless steel containing carbon and nitrogen.Description of the Related Art
[0003] Conventional austenitic stainless steels, such as STS 304 and STS 316 materials, are widely utilized in liquefied natural gas (LNG) storage vessels because they maintain a stable austenite phase even at ultra-low or cryogenic temperatures. However, these conventional materials heavily rely on nickel (Ni) as a primary austenite-stabilizing alloying element. Because nickel is a high-cost commodity, its extensive inclusion imposes a significant economic burden on manufacturing.
[0004] Consequently, a need exists for alternative structural materials that offer superior cost competitiveness relative to STS 304 and STS 316 without compromising cryogenic performance. To achieve this, low-cost austenite-stabilizing elements—such as manganese (Mn), carbon (C), and nitrogen (N)—must be strategically alloyed to reduce the absolute nickel content while successfully maintaining a stable austenite single-phase microstructure at ambient and cryogenic temperatures.
[0005] Furthermore, under International Maritime Organization (IMO) regulations, structural materials designated for LNG vessel applications must meet stringent mechanical safety thresholds, including an impact absorbed energy of at least 41 J at a cryogenic temperature of −196 °C. Accordingly, there is a need to optimize the chemical composition of an austenitic stainless steel material that satisfies these strict cryogenic toughness requirements while concurrently exhibiting a resistance to corrosion-induced weight loss that is comparable or superior to that of conventional STS 304 and STS 316.SUMMARY
[0006] Aspects of one or more exemplary embodiments provide an austenitic stainless steel having improved resistance to corrosion-induced weight loss through the incorporation of carbon and nitrogen.
[0007] Additional aspects will be set forth in part in the description which follows and, in part, will become apparent from the description, or may be learned by practice of the exemplary embodiments.
[0008] According to an aspect of an exemplary embodiment, there is provided an austenitic stainless steel, including: 16 to 20 wt % of chromium (Cr); 4.5 to 9 wt % of manganese (Mn); 3 to 6 wt % of nickel (Ni); 0.05 to 0.12 wt % of carbon (C); 0.15 to 0.30 wt % of nitrogen (N); and a balance of iron (Fe) and inevitable impurities.
[0009] A combined content of the carbon and the nitrogen (C+N) may be in a range 0.25 to 0.32 wt %.
[0010] The combined content of the carbon and the nitrogen (C+N) may be in a ran of 0.25 to 0.28 wt %.
[0011] The austenitic stainless steel may have a corrosion-induced weight loss of 10 to 200 g / m2 as measured by a ferric chloride immersion test in accordance with ASTM G48-11.
[0012] The corrosion-induced weight loss may be in a range of 60 to 120 g / m2.
[0013] The austenitic stainless steel may have an impact absorbed energy of 41 to 200 J at a temperature of −196 °C.
[0014] The impact absorbed energy may be in a range of 105 to 140 J at −196 °C
[0015] The chromium (Cr) content may be in a range of 17 to 19 wt %.
[0016] The manganese (Mn) content may be in a range of 5.5 to 7.5 wt %.
[0017] The austenitic stainless steel may be in a hot-rolled state and may have a nominal thickness of 11.5 mm.
[0018] According to the present disclosure, an austenitic stainless steel provides several technical advantages. By incorporating low-cost carbon (C) and nitrogen (N) as interstitial alloying elements in a specific combined range (C+N) of 0.25 to 0.32 wt %, the austenitic stainless steel exhibits enhanced cost-competitiveness and equivalent or superior localized corrosion resistance compared to conventional STS 304 and STS 316, as characterized by reduced corrosion-induced weight loss under ASTM G48-11 immersion testing. The austenitic stainless steel further demonstrates excellent cryogenic toughness, with an impact absorbed energy of at least 41 J at an ultra-low temperature of −196 °C.BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The above and other aspects will become more apparent from the following description of the exemplary embodiments with reference to the accompanying drawings, in which:
[0020] FIG. 1 illustrates images showing experimental results of corrosion tests according to an exemplary embodiment;
[0021] FIG. 2 is a graph illustrating the results of corrosion tests according to an exemplary embodiment; and
[0022] FIG. 3 is a graph illustrating impact absorbed energy evaluation results according to an exemplary embodiment.DETAILED DESCRIPTION
[0023] Various modifications and various embodiments will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily carry out the disclosure. However, it is to be understood that the various embodiments are not limited to the scope of the disclosure to the specific exemplary embodiments, but they should be interpreted to include all modifications, equivalents, and substitutions of the embodiments included in the spirit and the scope disclosed herein. In the following description, like reference numerals refer to like components, even in different drawings. In certain embodiments, detailed descriptions of known functions and configurations which are deemed to make the gist of the present disclosure obscure will be omitted. For the same reason, some elements in the accompanying drawings may be exaggerated, omitted, or simplified.
[0024] Terms such as “first” and “second” may be used to describe various elements, but these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. The use of such ordinal numbers should not be construed as limiting the meaning of the term. For instance, the elements associated with such an ordinal number should not be limited in the order of use, placement order, or the like. If necessary, each ordinal number may be used interchangeably.
[0025] Terms used herein are only for illustrative purposes of specific embodiments and are not intended to limit the present disclosure. The singular forms include the plural forms where not contrary to the context. It will be further understood that the terms such as “comprise”, “include”, and “have / has” specify the presence of stated features, integers, steps, operations, elements, components, and / or combinations thereof but do not preclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or combinations thereof.
[0026] Unless otherwise defined, all terms including technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs. It will be further understood that terms, such as those defined in commonly used dictionaries, may be interpreted as having meanings consistent with their ordinary meaning in the context of the relevant art, and will not be interpreted in an idealized or overly formal sense unless expressly defined otherwise herein.
[0027] An austenitic stainless steel according to an exemplary embodiment may include 16 to 20 wt % of chromium (Cr), 4.5 to 9 wt % of manganese (Mn), 3 to 6 wt % of nickel (Ni), 0.05 to 0.12 wt % of carbon (C), and 0.15 to 0.30 wt % of nitrogen (N), with the balance being iron (Fe) and inevitable impurities.
[0028] In an exemplary embodiment, the austenitic stainless steel may include carbon and nitrogen in a combined amount of 0.25 to 0.32 wt %.
[0029] In an exemplary embodiment, the austenitic stainless steel may include carbon and nitrogen in a combined amount of 0.25 to 0.28 wt %.
[0030] Hereinafter, reasons for the numerical limitations of the present disclosure will be described.(1) Chromium (Cr): in the Range of 16 to 20 wt %
[0031] Chromium is an essential alloying element that imparts corrosion resistance t the austenitic stainless steel by forming a passive film on the alloy surface. To ensure sufficient corrosion resistance and structural integrity under aggressive operating environments, the austenitic stainless steel must include chromium in an amount of at least 16 wt %. However, chromium acts as a ferrite-stabilizing element. If the chromium content exceeds 20 wt %, the excessive chromium content can disrupt the phase stability of the alloy, promoting the precipitation of a sigma phase. The formation of the sigma phase drastically reduces localized corrosion resistance due to localized chromium depletion and severely compromises the cryogenic impact toughness of the material. Therefore, to balance passive film stability against the risk of deleterious phase precipitation, the austenitic stainless steel may include chromium in an amount of 16 to 20 wt %. Within this range, the chromium content may be restricted to a preferred sub-range of 17 to 19 wt %, and more preferably to a sub-range of 17.5 to 18.5 wt %.(2) Manganese (Mn): in the Range of 4.5 to 9 wt %
[0032] Manganese is a key alloying element that serves as an effective, low-cost substitute for nickel to stabilize the austenite phase. Additionally, manganese increases the solid solubility of nitrogen within the alloy matrix, thereby preventing nitrogen outgassing and stabilizing the microstructure. To achieve these austenite-stabilizing and nitrogen-retaining effects, the austenitic stainless steel must include manganese in an amount of at least 4.5 wt %. However, when the manganese content exceeds 9 wt %, excessive manganese may react with impurities such as sulfur(S) or oxygen (O) to form coarse non-metallic inclusions, such as manganese sulfides (MnS) or manganese oxides (MnO), which may degrade the corrosion resistance and mechanical properties of the austenitic stainless steel. Therefore, to suppress the formation of deleterious non-metallic inclusions while ensuring a stable austenitic phase, it is preferable that the austenitic stainless steel includes manganese in an amount of 4.5 to 9 wt %. Within this range, the manganese content may be restricted to a preferred sub-range of 5.5 to 7.5 wt %.(3) Nickel (Ni): in the Range of 3 to 6 wt %
[0033] Nickel is a powerful austenite-stabilizing element that expands the austenite phase and significantly enhances the cryogenic toughness, ductility, and formability of the alloy. To ensure that the alloy achieves the required mechanical properties and exhibits sufficient impact absorbed energy at a cryogenic temperature of −196 °C, the austenitic stainless steel must include nickel in an amount of at least 3 wt %. However, because nickel is a high-cost commodity element, excessive additions may significantly increase raw material and manufacturing costs, undermining the economic advantages of the alloy. Therefore, to maximize cryogenic impact toughness and general corrosion resistance while minimizing manufacturing expenditures, it is preferable that the austenitic stainless steel includes nickel in an amount of 3 to 6 wt %.(4) Carbon (C): in the Range of 0.05 to 0.12 wt %
[0034] Carbon is an alloying element that significantly contributes to the stabilization of the austenite phase and suppresses deformation-induced martensitic transformation under cryogenic strain. To ensure sufficient phase stability and adequate base mechanical strength, the austenitic stainless steel must include carbon in an amount of at least 0.05 wt %. However, when the carbon content exceeds 0.12 wt %, the excessive carbon may promote the formation of carbides, which may reduce corrosion resistance. Therefore, to suppress grain-boundary sensitization while retaining strong austenite stabilization, it is preferable that the austenitic stainless steel includes carbon in an amount of 0.05 to 0.12 wt %.(5) Nitrogen (N): in the Range of 0.15 to 0.30 wt %
[0035] Nitrogen is an effective interstitial alloying element that acts as a powerful austenite stabilizer, serving as an efficient and cost-effective partial substitute for nickel. To ensure sufficient matrix stabilization and to achieve a high resistance to localized corrosion, the austenitic stainless steel must include nitrogen in an amount of at least 0.15 wt %. However, when the nitrogen content exceeds 0.30 wt %, the excessive nitrogen may promote the formation of nitrides, which may reduce corrosion resistance and toughness. Therefore, to maximize solid-solution strengthening and phase stability while avoiding harmful nitride precipitation or casting defects, it is preferable that the austenitic stainless steel includes nitrogen in an amount of 0.15 to 0.30 wt %.(6) Combined Carbon and Nitrogen (C+N): in the Range of 0.25 to 0.32 wt %
[0036] The total interstitial alloy content, defined as the combined weight percentage of carbon and nitrogen (C+N), is controlled to exploit a critical, synergistic interstitial strengthening and passivation mechanism. Within the designated range, carbon and nitrogen interact synergistically to improve the corrosion resistance of the austenitic stainless steel, as evidenced by a reduction in weight loss measured by ferric chloride immersion testing in accordance with ASTM G48-11 standards. As the combined content of carbon and nitrogen increases, the corrosion-induced weight loss as measured by ferric chloride immersion testing may decrease in a highly predictable, substantially linear manner. This linear correlation demonstrates that the interstitial interaction between carbon and nitrogen effectively alters the passivation kinetics of the alloy surface, enhancing the overall chemical and mechanical properties of the stainless steel.
[0037] When the combined content of carbon and nitrogen (C+N) is less than 0.25 wt %, the resulting reduction in corrosion-induced weight loss is insufficient to protect the alloy from localized galvanic attack under aggressive chloride or marine conditions. Conversely, when the combined content of carbon and nitrogen exceeds 0.32 wt %, it may accelerate the formation of carbides and nitrides, thereby deteriorating the physical properties of the stainless steel. Accordingly, to maximize surface passivation while mitigating the risk of deleterious carbide and nitride formation, the combined content of carbon and nitrogen (C+N) is within a range of 0.25 wt % to 0.32 wt %.
[0038] In one embodiment, the austenitic stainless steel is characterized by a corrosion-induced weight loss ranging from 10 to 200 g / m2, as measured by ferric chloride immersion testing in accordance withASTM G48-11 standard guidelines. In a preferred embodiment, the austenitic stainless steel limits this corrosion-induced weight loss to a narrow range of 60 to 120 g / m2.
[0039] In one embodiment, the austenitic stainless steel exhibits an impact absorbed energy ranging from 41 to 200 J at an ultra-low cryogenic temperature of −196 °C. In a preferred embodiment, the alloy achieves a cryogenic impact absorbed energy of 105 to 140 J at −196 °C. An impact absorbed energy threshold of at least 41 J at −196 °C is strictly required to satisfy International Maritime Organization (IMO) regulatory mandates for structural materials deployed in LNG vessel containment systems and cryogenic piping networks. If the impact absorbed energy falls below 41 J under these extreme cryogenic conditions, the material becomes susceptible to low-temperature embrittlement and catastrophic crack propagation, rendering it structurally unsuitable for LNG vessel applications.
[0040] The following Examples are provided to illustrate specific embodiments of the present disclosure in further detail. However, it should be understood by those skilled in the art that these Examples are merely illustrative, exemplary, and non-exhaustive in nature. The specific technical configurations, chemical compositions, processing parameters, and experimental results described below do not limit the scope of the present disclosure. Thus, the Examples are provided to enable those skilled in the art to fully understand and practice the present disclosure.Example 1
[0041] An austenitic stainless steel ingot was fabricated utilizing a vacuum induction melting (VIM) furnace. High-purity raw materials—including electrolytic iron, chromium, manganese, nickel, molybdenum, and carbon powder, each having a chemical purity of at least 95%, along with required master alloys—were charged into the VIM furnace. To introduce and alloy nitrogen into the melt, the furnace chamber was evacuated and subsequently backfilled with a controlled partial pressure of nitrogen (N2) gas. The total dissolved nitrogen content within the resulting molten steel was precisely adjusted by controlling the volumetric flow rate of the introduced nitrogen gas, the chamber pressure, and the liquid-metal reaction dwell time.
[0042] The molten alloy was subsequently cast into a laboratory-scale steel ingot. This steel ingot was soaked and heated at a target temperature of 1200 °C for a predetermined duration, and then hot-rolled into a structural plate having a nominal thickness of 11.5 mm. In this exemplary embodiment, the chemical processing parameters were controlled such that the final hot-rolled plate exhibited a combined carbon and nitrogen content (C+N) of 0.2469 wt %.Example 2
[0043] An austenitic stainless steel structural plate was fabricated in the same manner as described in Example 1, with the exception that the chemical processing parameters and the partial pressure of nitrogen gas (N2) introduced into the vacuum induction melting (VIM) furnace were adjusted to alter the interstitial alloy content. Specifically, the processing parameters were controlled such that the resulting hot-rolled plate of Example 2 exhibited a combined carbon and nitrogen content (C+N) of 0.253 wt %.Example 3
[0044] An austenitic stainless steel structural plate was fabricated in the same manner as described in Example 1, with the exception that the chemical processing parameters and the partial pressure of nitrogen gas (N2) introduced into the vacuum induction melting (VIM) furnace were adjusted to alter the interstitial alloy content. Specifically, the processing parameters were controlled such that the resulting hot-rolled plate of Example 3 exhibited a combined carbon and nitrogen content (C+N) of 0.2795 wt %.Example 4
[0045] An austenitic stainless steel structural plate was fabricated in the same manner as described in Example 1, with the exception that the chemical processing parameters and the partial pressure of nitrogen gas (N2) introduced into the vacuum induction melting (VIM) furnace were adjusted to alter the interstitial alloy content. Specifically, the processing parameters were controlled such that the resulting hot-rolled plate of Example 4 exhibited a combined carbon and nitrogen content (C+N) of 0.3134 wt %.Comparative Example 1
[0046] A commercially available STS 304 was obtained and prepared as a baseline comparative material.Comparative Example 2
[0047] A commercially available STS 316 was obtained and prepared as a baseline comparative material.Experimental Example 1
[0048] Electrochemical and mechanical performance evaluations were conducted on the alloys prepared according to Examples 1 to 4 and Comparative Examples 1 to 2 to characterize their localized corrosion resistance profiles and ultra-low temperature structural integrity.
[0049] To evaluate pitting and crevice corrosion resistance, corrosion testing was conducted in accordance with ASTM G48-11. Test specimens harvested from the hot-rolled plates of Examples 1 to 4 and Comparative Examples 1 to 2 were fully immersed in an aqueous ferric chloride hexahydrate (FeCl3·6H2O) solution. The solution temperature was continuously maintained within a range of 21 °C to 23 °C for an exposure duration of 72 hours.
[0050] FIG. 1 illustrates images showing experimental results of corrosion tests (ASTM G48-11) according to an exemplary embodiment, and FIG. 2 is a graph illustrating the results of corrosion tests according to an exemplary embodiment. As confirmed by the experimental results in FIGS. 1 and 2, the austenitic stainless steel specimens prepared according to the Examples exhibited corrosion-induced weight loss profile that is highly comparable to, or lower than, the benchmark profiles of conventional STS 304 and STS 316, demonstrating excellent passivation stability.
[0051] FIG. 3 is a graph illustrating the evaluation results of impact absorbed energy according to an exemplary embodiment. Cryogenic mechanical properties were evaluated by measuring Charpy V-notch impact absorbed energy in accordance with ASTM A370 standard test methods for the mechanical testing of steel products. Standardized sub-size or full-size V-notch specimens were tested utilizing a calibrated pendulum Charpy impact tester (e.g., a Tinius Olsen, IT542E system). To qualify materials for structural deployment in LNG vessels and cryogenic piping networks, structural regulations generally mandate a minimum baseline impact absorbed energy of at least 41 J at cryogenic temperature of −196 °C. As graphically illustrated in FIG. 3, all specimens prepared according to Examples 1 to 4 significantly exceeded this safety threshold, consistently demonstrating superior cryogenic impact absorbed energy values of greater than 100 J at −196 °C.
[0052] While one or more exemplary embodiments have been described with reference to the accompanying drawings, it will be understood by those skilled in the art that various modifications in form and details may be made therein without departing from the idea and scope as defined in the appended claims.
Claims
1. An austenitic stainless steel, comprising:16 to 20 wt % of chromium (Cr);4.5 to 9 wt % of manganese (Mn);3 to 6 wt % of nickel (Ni);0.05 to 0.12 wt % of carbon (C);0.15 to 0.30 wt % of nitrogen (N); anda balance of iron (Fe) and inevitable impurities.
2. The austenitic stainless steel of claim 1, wherein a combined content of the carbon and the nitrogen (C+N) is in a range of 0.25 to 0.32 wt %.
3. The austenitic stainless steel of claim 2, wherein the combined content of the carbon and the nitrogen (C+N) is in a range of 0.25 to 0.28 wt %.
4. The austenitic stainless steel of claim 1, wherein the austenitic stainless steel has a corrosion-induced weight loss of 10 to 200 g / m2 as measured by a ferric chloride immersion test in accordance withASTM G48-11.
5. The austenitic stainless steel of claim 4, wherein the corrosion-induced weight loss is in a range of 60 to 120 g / m2.
6. The austenitic stainless steel of claim 1, wherein the austenitic stainless steel has an impact absorbed energy of 41 to 200 J at a temperature of −196 °C.
7. The austenitic stainless steel of claim 6, wherein the impact absorbed energy is in a range of 105 to 140 J at −196 °C.
8. The austenitic stainless steel of claim 1, wherein the chromium (Cr) content is in a range of 17 to 19 wt %.
9. The austenitic stainless steel of claim 1, wherein the manganese (Mn) content is in a range of 5.5 to 7.5 wt %.