Composition and cured product thereof

The composition of an olefin-aromatic vinyl compound-aromatic polyene copolymer with controlled boron and aluminum content addresses the need for low dielectric loss tangents and uniformity in high-frequency applications, enhancing the performance of insulating materials in multilayer substrates by reducing dielectric loss and maintaining transparency.

WO2024190873A1PCT designated stage expired Publication Date: 2024-09-19DENKA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010017
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-03-14
Publication Date
2024-09-19

AI Technical Summary

Technical Problem

As communication frequencies shift to higher bands, there is a need for insulating materials in multilayer substrates with low dielectric properties and reduced viscosity to minimize dielectric loss tangents and ensure uniform composition, particularly in high-frequency applications where signal frequencies are expected to increase and wiring becomes finer.

Method used

A composition comprising an olefin-aromatic vinyl compound-aromatic polyene copolymer with specific molecular weight and monomer unit ratios, combined with boron and aluminum content within precise ranges, is used to achieve low dielectric loss tangents and maintain transparency, employing a coordination polymerization catalyst and boron promoter to control impurities and molecular weight.

Benefits of technology

The solution effectively reduces dielectric loss tangents and maintains solution transparency without the need to remove aluminum, achieving suitable dielectric properties for high-frequency applications while ensuring uniform composition and low viscosity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The present disclosure provide an approach that does not require the removal of aluminum from inside a system, and that does not compromise the dielectric loss tangent or solution transparency. A composition according to the present disclosure comprises: (A) an olefin-aromatic vinyl compound-aromatic polyene copolymer, (B) 0.2 ppm or more of boron, as measured by ICP emission spectroscopy in conformance with JIS K 0116:2014, and (C) 100 ppm to 2000 ppm of aluminum, as measured by ICP emission spectroscopy in conformance with JIS K 0116:2014, said composition having a number average molecular weight of 40,000 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Composition and cured product thereof

[0001] The present invention relates to, for example, a curable composition and a cured product thereof.

[0002] As communication frequencies move into the gigahertz band and higher, there is an increasing need for multilayer substrates, transmission lines, antennas, etc., made of CCL or FCCL containing insulating materials with low dielectric properties. For use in such multilayer substrates, the insulating material must have good impregnation properties, so there is a need for even lower viscosity.

[0003] Patent Document 1 discloses a cured product obtained from a specific coordination polymerization catalyst and consisting of an ethylene-olefin (aromatic vinyl compound)-aromatic polyene copolymer and a non-polar vinyl compound copolymer having a specific composition and blend. In this technology, only one of the two vinyl groups of the aromatic polyene (divinylbenzene) is selectively copolymerized, and the remaining vinyl group is preserved, making it easy to obtain a crosslinkable hydrocarbon copolymer macromonomer having an aromatic vinyl group functional group.

[0004] In order to achieve low viscosity for multilayer substrate applications such as CCL, it has been necessary to reduce the molecular weight. As disclosed in Patent Document 2, it is known that a low molecular weight copolymer can be obtained by using a single-site coordination polymerization catalyst with a small ligand and relatively low polymerization activity.

[0005] A method for producing an ethylene-olefin (aromatic vinyl compound)-aromatic polyene copolymer using a coordination polymerization catalyst and a boron cocatalyst is also known (Patent Document 3).

[0006] JP 2009-161743 A International Publication No. 2022 / 014599 International Publication No. 2017 / 122295

[0007] However, signal frequencies are expected to become higher in the future, necessitating the development of insulating materials with lower dielectric loss tangents. Furthermore, particularly as package substrates become increasingly high-frequency and their wiring becomes finer, there is growing demand for insulating materials with low dielectric loss tangents yet a more uniform composition at the microscopic level. This insulating material is generally supplied in the form of a solvent-containing varnish and is concentrated (the solvent is removed) during the substrate manufacturing process before use. However, it is considered important that the material remains transparent even in its highly concentrated state during solvent removal, i.e., that it has a uniform composition that does not cause light scattering. The present inventors focused on the impurity content of this copolymer and discovered that by limiting the impurity content within a certain range, the uniformity (transparency) of the high-concentration solution of this copolymer is maintained and the dielectric loss tangent of the resulting cured product is further reduced, thereby completing the present invention.

[0008] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have come to the conclusion that the above-mentioned problems can be solved by controlling the content of specific elements in a composition, and have thus completed the present invention. That is, the present invention provides various specific embodiments as shown below.

[0009] Aspect 1. A composition comprising: (A) an olefin-aromatic vinyl compound-aromatic polyene copolymer; (B) boron having a content of 0.2 ppm or more as measured by ICP atomic emission spectroscopy in accordance with JIS K0116:2014; and (C) aluminum having a content of 100 ppm or more and 2,000 ppm or less as measured by ICP atomic emission spectroscopy in accordance with JIS K0116:2014; and having a number average molecular weight of 40,000 or less.

[0010] Aspect 2. The composition according to Aspect 1, wherein the component (A) satisfies the following conditions (1) to (4): (1) the number average molecular weight of the copolymer is 5,000 or more and 40,000 or less; (2) the aromatic vinyl compound monomer unit is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0 to 70 mass%; (3) the aromatic polyene monomer unit is one or more selected from polyenes having 5 to 20 carbon atoms and having multiple vinyl groups and / or vinylene groups in the molecule; (4) the olefin monomer unit is one or more selected from olefins having 2 to 20 carbon atoms, and the total of the olefin monomer unit, aromatic vinyl compound monomer unit, and aromatic polyene monomer unit is 100 mass%.

[0011] Aspect 3. The composition according to Aspect 2, wherein the above (3) satisfies the following condition (3a): (3a) the aromatic polyene monomer unit is one or more polyenes selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene monomer unit is 1.5 to 20 per number average molecular weight.

[0012] Aspect 4. The composition according to aspect 1, wherein the content of component (B) measured by ICP atomic emission spectroscopy in accordance with JIS K0116:2014 is in the range of 0.2 ppm to 10 ppm.

[0013] Aspect 5. The composition according to aspect 1 or 2, wherein the content of component (C) is in the range of 100 ppm to 1500 ppm.

[0014] Aspect 6. The composition according to aspect 5, wherein the content of component (C) is in the range of 100 ppm to 1100 ppm.

[0015] Aspect 7. The composition according to any one of Aspects 1 to 6, wherein the ratio Mw / Mn of the number average molecular weight (Mn) to the weight average molecular weight (Mw) is 10 or less.

[0016] Aspect 8. A cured product of the composition according to any one of aspects 1 to 7.

[0017] Aspect 9. A CCL substrate, an FCCL substrate, an interlayer insulating material, or a coverlay, comprising the cured product according to aspect 8.

[0018] According to the present invention, there are obtained effects such as the fact that the dielectric loss tangent and the transparency of the solution are not impaired without the need to remove aluminum from the system.

[0019] Hereinafter, embodiments of the present invention will be described in detail. However, the following embodiments are merely examples for explaining the present invention, and the present invention is not limited thereto. In other words, the present invention can be implemented with any modifications within the scope of the gist thereof. In this specification, a numerical range such as "1 to 100" includes both the lower limit "1" and the upper limit "100." The same applies to other numerical ranges. In this specification, the term "sheet" also includes the concept of "film." Furthermore, the term "film" in this specification also includes the concept of "sheet." In this specification, the term "composition" includes the concept of "varnish." In other words, a liquid composition is particularly referred to as "varnish." In this specification, the term "interlayer insulating material" includes the concept of "interlayer adhesive." In this specification, a numerical range includes both its lower and upper limits unless otherwise specified.

[0020] A composition provided by one embodiment of the present invention contains (A) an olefin-aromatic vinyl compound-aromatic polyene copolymer, (B) a boron content of 0.2 ppm or more as measured by ICP atomic emission spectroscopy in accordance with JIS K0116:2014, and (C) an aluminum content of 100 ppm to 2000 ppm as measured by ICP atomic emission spectroscopy in accordance with JIS K0116:2014, and is characterized by having a number-average molecular weight within a predetermined range. Component (A) is the main component of the composition. By blending component (A) with predetermined amounts of components (B) and (C), the synergistic effect of these components suppresses loss of solution transparency and reduces the dielectric dissipation factor. This composition is classified as an LDM (Low Dielectric Material) resin in the art.

[0021] Component (B) may be derived from any molecule containing a boron atom, preferably from the catalyst and / or co-catalyst, and more preferably from the co-catalyst.

[0022] The content of component (B) in the composition is 0.2 ppm or more, preferably 0.2 ppm or more and 10 ppm or less, and more preferably 0.2 ppm or more and 5.0 ppm or less. Throughout this specification, the amounts of component (B) and component (C) described below are measured by ICP atomic emission spectroscopy in accordance with JIS K0116:2014.

[0023] Examples of compounds that can contain component (B) include organic boron compounds and inorganic boron compounds. Examples of organic boron compounds include, but are not limited to, tris(perfluorophenyl)borane (FAB), tritium tetra(perfluorophenyl)borate (TRI-FABA, also known as triphenylmethylium tetrakis(pentafluorophenyl)borate or tritium tetrakis(pentafluorophenyl)borate), N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate (DAN-FABA), tris(pentafluorophenyl)borane (TPB), tris(pentafluorophenyl)borane trihydrate (TPB-3W), and triethyl borate. Examples of inorganic boron compounds include, but are not limited to, boric acid, sodium borate, nickel boron, manganese(II) borate, ammonium pentaborate, and potassium fluoroborate. Organic boron compounds are preferred.

[0024] Preferably, a co-catalyst containing component (B) containing fluorine atoms can be used. While not wishing to be bound by any particular theory, it is believed that a co-catalyst containing both boron and fluorine atoms may trap the aluminum atoms of component (C) and form a structure similar to an aluminum-boron cluster compound, which is likely to help suppress the adverse effects of a predetermined amount of component (C), as described below. Although this is merely a hypothesis, it is believed that the formation of such a cluster compound facilitates the dispersion of molecules in an organic solvent, making it easier to improve the transparency of the solution. It is believed that this effect cannot be achieved if the amount of component (C) is outside this predetermined range.

[0025] Component (C) may be derived from any molecule containing an aluminum atom, and is preferably derived from a catalyst, a co-catalyst, and / or a scavenger. In this specification, the term "scavenger" refers to a compound added to a system to remove impurities (such as water) that may adversely affect the polymerization reaction.

[0026] The content of component (C) in the present composition must be 100 ppm or more and 2000 ppm or less. If the amount of component (C) is outside this range, problems such as insufficient polymerization reaction of the system, deterioration of dielectric properties, or deterioration of transparency tend to occur. Preferably, the content of component (C) may be 100 ppm or more and 1500 ppm or less, more preferably 100 ppm or more and 1300 ppm or less, and even more preferably 100 ppm or more and 1100 ppm or less.

[0027] Examples of compounds that may contain component (C) include organoaluminum compounds. Examples of organoaluminum compounds include, but are not limited to, alkylaluminum compounds that can be used as scavengers or cocatalysts, such as triisobutylaluminum (TIBAL) and triethylaluminum (TEA). Other examples include aluminum compounds that can be used as cocatalysts, such as methylaluminoxane (also referred to as methylalumoxane or MAO), modified methylaluminoxane (also referred to as modified MAO or MMAO), and solid polymethylaluminoxane (also referred to as SMAO). These cocatalysts are commercially available from Tosoh Finechem Corporation under the trade names TMAO-312, TMAO-211, TMAO-212, MMAO-3A, ​​TMAO-341, and solid MAO. In a preferred embodiment, an alkylaluminum compound is used as the compound that may contain component (C), and aluminoxanes are not used.

[0028] In addition to components (B) and (C), the present composition may further contain another metal element, preferably a transition metal element, more preferably zirconium and / or hafnium, and even more preferably zirconium. The compound providing such a metal element may be a compound usable as a catalyst or co-catalyst. Examples of such compounds include, but are not limited to, dimethylmethylenebiscyclopentadienylzirconium dichloride, diphenylmethylenebiscyclopentadienylzirconium dichloride, dimethylmethylene(cyclopentadienyl)(1-indenyl)zirconium dichloride, and diphenylmethylene(cyclopentadienyl)(1-indenyl)zirconium dichloride.

[0029] Examples of compounds that provide other metal elements include transition metal compounds represented by the following general formula (I). In the above formula, M is an element selected from zirconium or hafnium. Cp1 and Cp2 are unsubstituted cyclopentadienyl groups, or cyclopentadienyl groups having one or two alkyl substituents (preferably having 1 to 3 carbon atoms) without a cyclic structure. Cp1 and Cp2 may be the same or different. One of the Cp1 and Cp2 groups may be an unsubstituted indenyl group, or an indenyl group having one or two alkyl substituents (preferably having 1 to 3 carbon atoms) without a cyclic structure. Y is bonded to Cp1 and Cp2 and is an element selected from carbon, silicon, germanium, or boron having a hydrogen atom or a substituent, and the substituents (preferably alkyl groups, phenyl groups, etc.) may be different or the same and may have a cyclic structure (cyclohexyl structure, etc.). X are each independently selected from the group consisting of hydrogen, halogen, alkyl groups, and aryl groups, or two Xs combine to form a diene group.

[0030] Further examples of these compounds (catalysts or co-catalysts) may include those described in European Patent Application Publication No. 0872492A2, Japanese Patent Application Publication No. H11-130808, Japanese Patent Application Publication No. H9-309925, International Publication No. 00 / 20426, European Patent Application Publication No. 0985689, Japanese Patent Application Publication No. H6-184179, and the like.

[0031] In a preferred embodiment, the composition may contain zirconium in an amount of 1.0 ppm to 1000 ppm, more preferably 1.0 ppm to 100 ppm. Preferably, the mass ratio of zirconium to aluminum (Zr / Al ratio) contained in the composition may be in the range of 0.013 to 0.5, more preferably 0.013 to 0.1. When the Zr / Al ratio is within this range, the effect of improving dielectric properties and transparency tends to be easily obtained.

[0032] The component (A) contained in the present composition is preferably an olefin-aromatic vinyl compound-aromatic polyene copolymer (hereinafter also simply referred to as "copolymer") that satisfies all of the following conditions. Component (A) is a component that imparts curability to the present composition through crosslinking. (1) The number-average molecular weight of the copolymer is 5,000 to 40,000. (2) The aromatic vinyl compound monomer unit is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0 to 70 mass%, preferably more than 0 mass% to 70 mass%. (3) The aromatic polyene monomer unit is one or more types selected from polyenes having 5 to 20 carbon atoms and having multiple vinyl groups and / or vinylene groups in the molecule. (4) The olefin monomer unit is one or more selected from olefins having 2 to 20 carbon atoms, and the total of the olefin monomer unit, aromatic vinyl compound monomer unit, and aromatic polyene monomer unit is 100 mass%.

[0033] It is more preferable that the above condition (3) satisfies the following condition (3a): (3a) the aromatic polyene monomer unit is one or more polyenes selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of vinyl groups and / or vinylene groups derived from the aromatic polyene monomer unit is 1.5 to 20 per number average molecular weight.

[0034] In this specification, the average molecular weight (Mn, Mw) of a composition that satisfies the above-mentioned conditions for the amounts of components (B) and (C) (i.e., the amounts of components (B) and (C) are minute compared to the amount of component (A)) can be considered to be substantially equal to the average molecular weight (Mn, Mw) of component (A) contained in the composition.

[0035] In this specification, the term "olefin monomer unit" refers to one or more compounds (units) selected from α-olefins having 2 to 20 carbon atoms and cyclic olefins having 5 to 20 carbon atoms, which are substantially free of oxygen, nitrogen, and halogens and are composed of carbon and hydrogen. Examples of α-olefins having 2 to 20 carbon atoms include, but are not limited to, ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, and 3,5,5-trimethyl-1-hexene. Examples of cyclic olefins having 5 to 20 carbon atoms include, but are not limited to, norbornene and cyclopentene. A preferred olefin monomer unit may be a combination of ethylene with an α-olefin other than ethylene or with a cyclic olefin. In a preferred embodiment, the olefin monomer unit may contain one or more compounds selected from the group consisting of ethylene and α-olefins having 3 or more carbon atoms.

[0036] In this specification, the term "aromatic vinyl compound monomer unit" refers to an aromatic vinyl compound (unit) having from 8 to 20 carbon atoms. Examples of the aromatic vinyl compound monomer unit include, but are not limited to, styrene, paramethylstyrene, paraisobutylstyrene, various vinylnaphthalenes, and various vinylanthracenes.

[0037] In this specification, the term "aromatic polyene monomer unit" refers to a polyene compound (unit) having 5 to 20 carbon atoms and containing multiple vinyl groups and / or vinylene groups in its molecule. Examples of the aromatic polyene monomer unit include, but are not limited to, various ortho-, meta-, and para-divinylbenzenes or mixtures thereof, and compounds having an aromatic vinyl structure, such as divinylnaphthalene, divinylanthracene, p-2-propenylstyrene, and p-3-butenylstyrene, which are substantially free of oxygen, nitrogen, and halogens and are composed of carbon and hydrogen. Furthermore, the aromatic polyene monomer unit may include, but is not limited to, bifunctional aromatic vinyl compounds such as 1,2-bis(vinylphenyl)ethane (abbreviation: BVPE), as described in JP 2004-087639 A. Among these, various ortho-, meta-, and para-divinylbenzenes or mixtures thereof are preferably used, and a mixture of meta-divinylbenzene and para-divinylbenzene is preferably used. In this specification, these divinylbenzenes are referred to as "divinylbenzenes." When divinylbenzenes are used as aromatic polyenes, they are preferred because they have high curing efficiency and are easy to cure when subjected to a curing treatment.

[0038] In the copolymer, the content of vinyl groups and / or vinylene groups (preferably vinyl groups) derived from aromatic polyene monomer units may be 1.5 or more and 20 or less than 1.5 and 20, preferably 2 or more and less than 7, per number average molecular weight. When the content of vinyl groups and / or vinylene groups is 1.5 or more, crosslinking efficiency is high, and a cured product with sufficient crosslinking density tends to be easily obtained. The content of vinyl groups derived from aromatic polyene units (divinylbenzene units) per number average molecular weight in the copolymer can be calculated, for example, by the number average molecular weight (Mn) calculated in terms of standard polystyrene obtained by GPC (gel permeation chromatography) known to those skilled in the art and 1 It can be obtained by comparing the vinyl group content derived from aromatic polyene units obtained by H-NMR measurement with the vinyl group content derived from aromatic polyene units obtained by H-NMR measurement. 1By comparing the intensities of each peak area obtained by H-NMR measurement, if the content of vinyl groups derived from aromatic polyene units (divinylbenzene units) in the copolymer is 0.6% by mass and the number average molecular weight calculated as polystyrene by GPC measurement is 49,000, the molecular weight of vinyl groups derived from aromatic polyene units in the number average molecular weight is the product of these, 299, which is divided by the formula weight of the vinyl groups, 130, to obtain 2.3. In other words, the content of vinyl groups derived from aromatic polyene units per number average molecular weight in this copolymer is determined to be 2.3. 1 The assignment of peaks obtained by H-NMR measurement is known from literature. 1 A method for determining the composition of a copolymer from a comparison of peak areas obtained by H-NMR measurement is also known. 1 The measurement was performed in a known quantitative mode using a H-NMR measurement method. 13 It is also possible to improve the accuracy of the composition by adding data on the peak areas and ratios of the C-NMR spectrum. In this specification, the content of divinylbenzene units in the copolymer is determined based on the peak intensity ( 1 In other words, the content of divinylbenzene units is calculated from the content of vinyl groups derived from divinylbenzene units, assuming that one vinyl group is derived from one divinylbenzene unit in the copolymer.

[0039] The number average molecular weight (Mn) and weight average molecular weight (Mw) in this specification are calculated as molecular weights converted into standard polystyrene, obtained by GPC (gel permeation chromatography).

[0040] The number average molecular weight (Mn) of the present composition is 40,000 or less, preferably 5,000 or more and 40,000 or less, more preferably 5,000 or more and 30,000 or less, and even more preferably 5,000 or more and 20,000 or less.

[0041] From the viewpoint of improving dielectric properties, the present composition may preferably have a weight average molecular weight (Mw) of 18,000 or more, and more preferably, Mw of 18,000 or more and 100,000 or less.

[0042] In a preferred embodiment, the ratio Mw / Mn of the number average molecular weight (Mn) to the weight average molecular weight (Mw) of the composition can be appropriately set depending on the desired performance, and is not particularly limited, but may be preferably 10 or less, more preferably 1 or more and 10 or less, and even more preferably 2 or more and 10 or less. When Mw / Mn is 10 or less, the molecular weight distribution is optimized, and appropriate dielectric properties can be obtained.

[0043] In some embodiments of the present invention, the composition may further comprise one or more of the following: (a) a curing agent; (b) one or more resins selected from a hydrocarbon-based elastomer, a polyether-based resin, and an aromatic polyene-based resin; (c) a monomer; and (d) an olefin-aromatic vinyl compound-aromatic polyene copolymer other than the above copolymers, which satisfies all of the following conditions (i) to (iv): (i) the number-average molecular weight of the copolymer is 500 or more and 100,000 or less, preferably 500 or more and less than 5,000, or more than 40,000 and 100,000 or less. (ii) The aromatic vinyl compound monomer unit is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 70% by mass or less, preferably more than 0% by mass and 70% by mass or less. (iii) The aromatic polyene monomer unit has a plurality of vinyl groups and / or vinylene groups in the molecule. (iv) The olefin monomer unit is one or more selected from olefins having from 2 to 20 carbon atoms, the content of the olefin monomer unit is 30% by mass or more, and the total of the olefin monomer unit, aromatic vinyl compound monomer unit, and aromatic polyene monomer unit is 100% by mass. It is preferable that the above (iii) satisfies the following condition (iiia): (iiia) The aromatic polyene monomer unit is one or more selected from polyenes having from 5 to 20 carbon atoms and having multiple vinyl groups and / or vinylene groups in the molecule, and the content of vinyl groups and / or vinylene groups derived from the aromatic polyene monomer unit is 1.5 to 20 per number average molecular weight.

[0044] Such other copolymers may be those described in, for example, WO 2021 / 112087, WO 2021 / 112088, and WO 2022 / 014599. Another olefin-aromatic vinyl compound-aromatic polyene copolymer that satisfies all of the above-mentioned specific conditions tends to be soft and exhibit a low dielectric constant and a low dielectric dissipation factor, so by combining it with the above-mentioned compound of component (A) to form a composition, it is possible to provide a cured product with a low dielectric constant and a low dielectric dissipation factor that covers a wide range of physical properties.

[0045] <Curing Agent> The curing agent that may be included in the present composition may be any known curing agent that has been used for the polymerization or curing of aromatic polyenes or aromatic vinyl compounds. Examples of such curing agents include radical polymerization initiators (radical generators), cationic polymerization initiators, and anionic polymerization initiators. Radical polymerization initiators are preferred, but the type is not particularly limited. Organic peroxides, azo polymerization initiators, dicumene initiators (e.g., 2,3-dimethyl-2,3-diphenylbutane), and the like are more preferred, and can be freely selected depending on the application and conditions. For example, dicumene initiators require high temperatures for reaction, making them less susceptible to side reactions during preparation of the cured product and easier to handle. A catalog listing organic peroxides can be downloaded from the NOF Corporation website, for example, https: / / www.nof.co.jp / business / functional-materials / functional-materials-product09. Organic peroxides listed in catalogs from Fujifilm Wako Pure Chemical Industries, Ltd. and Tokyo Chemical Industry Co., Ltd. may also be used. Also, known photopolymerization initiators that use light, ultraviolet light, or radiation can be used as a curing agent. Examples of photopolymerization initiators include photoradical polymerization initiators, photocationic polymerization initiators, and photoanionic polymerization initiators. Such photopolymerization initiators are available from, for example, Tokyo Chemical Industry Co., Ltd. Furthermore, curing by radiation or electron beams themselves is also possible. Furthermore, crosslinking and curing by thermal polymerization of the raw materials contained therein can also be performed without using a curing agent.

[0046] There are no particular restrictions on the amount of curing agent used, but for example, 0.01 to 10 parts by mass of the curing agent may be used per 100 parts by mass of the present compound (component (A)). When using a curing agent such as a peroxide, an azo-based polymerization initiator, or a dicumene initiator, the curing treatment should be carried out at an appropriate temperature and time, taking into account its half-life. In this case, the conditions can be determined according to the curing agent, but a temperature range of about 50°C to 200°C, and more preferably a temperature range of about 50°C to 300°C, is generally appropriate.

[0047] <Hydrocarbon Elastomer> The amount of hydrocarbon elastomer that may be contained in the composition can be appropriately set depending on the desired performance and is not particularly limited, but is preferably 1 to 200 parts by mass, more preferably 1 to 100 parts by mass, and most preferably 1 to 50 parts by mass, per 100 parts by mass of the present compound of component (A). The hydrocarbon elastomer preferably has a number average molecular weight of 100 or more and 100,000 or less, more preferably 1,000 or more and 4,500 or less. Preferred examples of the hydrocarbon elastomer include, but are not limited to, one or more elastomers selected from ethylene-based or propylene-based elastomers, conjugated diene-based polymers, block copolymers or random copolymers of aromatic vinyl compounds and conjugated dienes, and hydrogenated products thereof. Examples of the ethylene-based elastomer include ethylene-α-olefin copolymers such as ethylene-octene copolymer and ethylene-1-hexene copolymer, EPR, EPDM, etc., and examples of the propylene-based elastomer include atactic polypropylene, low stereoregular polypropylene, propylene-α-olefin copolymers such as propylene-1-butene copolymer, etc., but are not particularly limited to these.

[0048] Examples of conjugated diene polymers include, but are not limited to, polybutadiene and 1,2-polybutadiene. Examples of aromatic vinyl compound-conjugated diene block or random copolymers and their hydrogenated products (hydrogenated products) include, but are not limited to, SBS, SIS, SEBS, SEPS, SEEPS, and SEEBS. Suitable 1,2-polybutadiene is available, for example, from Nippon Soda Co., Ltd. under the product names B-1000, 2000, and 3000 as liquid polybutadiene. Another suitable copolymer containing a 1,2-polybutadiene structure is "Ricon 100" manufactured by TOTAL CRAY VALLEY. When the resin or resins selected from these hydrocarbon elastomers are liquid (approximately 300,000 mPa s or less) at room temperature (25°C), in particular, the amount used may be preferably 150 parts by mass or less, more preferably 1 to 30 parts by mass, and most preferably 1 to 20 parts by mass, per 100 parts by mass of the compound of component (A), from the viewpoint of the handleability and moldability of the present composition in an uncured state (handleability as a thermoplastic resin).

[0049] <Polyether-based resin> Examples of polyether-based resins that may be contained in the present composition include polyphenylene ether and polyether. As the polyphenylene ether, commercially available known polyphenylene ethers can be used, and the type is not particularly limited. The number average molecular weight of the polyphenylene ether is arbitrary and can be appropriately set depending on the desired performance, and is not particularly limited. However, in consideration of the moldability of the composition, the number average molecular weight (Mn) is preferably 10,000 or less, most preferably 5,000 or less. The number average molecular weight may preferably be 500 or more.

[0050] Furthermore, when the additive is added for the purpose of curing the present composition, it is preferable that the molecular terminals of the polyether-based resin, such as polyphenylene ether, be modified with a functional group. Furthermore, when the additive is added for the purpose of curing the present composition, it is preferable that the polyether-based resin, such as polyphenylene ether, have multiple functional groups in one molecule. For example, the polyether-based resin may be a modified polyphenylene ether. Examples of the functional group include radically polymerizable functional groups and functional groups such as epoxy groups, and preferably radically polymerizable functional groups. A preferred radically polymerizable functional group is a vinyl group. As the vinyl group, one or more of the group consisting of an allyl group, a (meth)acryloyl group, and an aromatic vinyl group are preferred, and one or more of the group consisting of a (meth)acryloyl group and an aromatic vinyl group are more preferred, with an aromatic vinyl group being the most preferred. In other words, in the composition of this embodiment, a bifunctional polyphenylene ether in which both molecular chain terminals are modified with radically polymerizable functional groups is particularly preferred. Examples of such polyphenylene ethers include Noryl (trademark) SA9000 manufactured by SABIC (modified polyphenylene ether having methacryloyl groups at both ends, number average molecular weight 2200) and bifunctional polyphenylene ether oligomer manufactured by Mitsubishi Gas Chemical Company, Inc. (OPE-2St, modified polyphenylene ether having vinylbenzyl groups at both ends, number average molecular weight 1200). Allylated PPE manufactured by Asahi Kasei Corporation can also be used. Of these, the bifunctional polyphenylene ether oligomer manufactured by Mitsubishi Gas Chemical Company, Inc. (OPE-2St) is preferred.

[0051] The polyether resin may also be an aromatic polyether (ELPAC HC-F series) manufactured by JSR Corp. The amount of polyphenylene ether or other polyether resin used in the composition can be appropriately determined depending on the desired performance and is not particularly limited, but is preferably 1 to 200 parts by mass, and more preferably 1 to 100 parts by mass, per 100 parts by mass of component (A).

[0052] <Aromatic Polyene Resin> The aromatic polyene resin that may be contained in the present composition includes divinylbenzene-based reactive hyperbranched copolymer (PDV) manufactured by Nippon Steel Chemical & Material Co., Ltd. Such PDV is described, for example, in the literature "Synthesis of Polyfunctional Aromatic Vinyl Copolymer and Development of a New IPN-Type Low Dielectric Loss Material Using the Same" (Kawabe Masanao, Journal of the Institute of Electronics Packaging, Vol. 12, No. 2 (2009) p. 125). The amount of aromatic polyene resin used in the present composition can be appropriately determined depending on the desired performance and is not particularly limited. However, it is preferably 1 to 200 parts by weight, more preferably 1 to 100 parts by weight, and most preferably 1 to 50 parts by weight per 100 parts by weight of the present compound (component (A)). Using an amount of aromatic polyene resin within these preferred ranges is preferable to prevent a decrease in adhesion to other components and a decrease in toughness.

[0053] <Monomer> The amount of monomer that may be contained in the composition may preferably be 100 parts by mass or less per 100 parts by mass of the present compound of component (A), or the composition may be substantially free of monomers. In this specification, a monomer refers to a monomer that can be polymerized by either radical polymerization, cationic polymerization, or anionic polymerization, and is preferably a radically polymerizable monomer. Its molecular weight is preferably 5,000 or less, more preferably less than 5,000, more preferably 1,000 or less, more preferably less than 1,000, even more preferably 500 or less, and even more preferably less than 500. The monomer may include a monomer having the same structure as the monomer unit of the above-mentioned "aromatic vinyl compound" or "aromatic polyene." Preferably, the monomer may include the following polar monomer.

[0054] <Polar Monomer> The amount of polar monomer that may be contained in the present composition can be appropriately set depending on the desired performance and is not particularly limited. However, it may be preferably 100 parts by mass or less, more preferably 0.1 to 20 parts by mass, and even more preferably 0.1 to 10 parts by mass, per 100 parts by mass of the present compound of component (A). Using an amount within this preferred range tends to prevent the dielectric constant and dielectric dissipation factor of the resulting cured product from becoming too high. In this specification, a polar monomer refers to a monomer containing one or more atoms selected from oxygen, nitrogen, phosphorus, and sulfur in the molecule. Suitable polar monomers have a molecular weight of less than 5,000, more preferably less than 1,000, and even more preferably less than 500. As the polar monomer, a polar monomer that can be polymerized using a radical polymerization initiator is preferred. Examples of polar monomers include, but are not limited to, various maleimides, bismaleimides, maleic anhydride, triallyl isocyanurate, glycidyl (meth)acrylate, tri(meth)acrylic isocyanurate, and trimethylolpropane tri(meth)acrylate. Maleimides and bismaleimides that can be used in the present embodiment are described, for example, in International Publication No. 2016 / 114287 and Japanese Patent Application Laid-Open No. 2008-291227, and can be purchased from, for example, Daiwa Chemical Industry Co., Ltd., Nippon Kayaku Co., Ltd., and Designer Molecules Inc. Furthermore, the bismaleimide resin "SLK" manufactured by Shin-Etsu Chemical Co., Ltd. can also be used. Of these maleimide group-containing compounds, bismaleimides are preferred from the viewpoints of solubility in organic solvents, high-frequency characteristics, high adhesion to conductors, and moldability of prepregs. These maleimide group-containing compounds may be used as polyaminobismaleimide compounds from the viewpoints of solubility in organic solvents, high-frequency characteristics, high adhesion to conductors, moldability of prepregs, etc. Polyaminobismaleimide compounds can be obtained, for example, by subjecting a compound having two maleimide groups at its terminals to a Michael addition reaction with an aromatic diamine compound having two primary amino groups in the molecule.When attempting to obtain high crosslinking efficiency with the addition of a small amount, it is preferable to use a polar monomer having a multifunctional group of two or more functional groups. Examples of such polar monomers include bismaleimides, triallyl isocyanurate (TAIC), trimethylolpropane tri(meth)acrylate, etc.

[0055] <Another Olefin-Aromatic Vinyl Compound-Aromatic Polyene Copolymer> The present composition may contain one or more olefin-aromatic vinyl compound-aromatic polyene copolymers other than the copolymers described above, and may satisfy any of the following conditions: (i) The number-average molecular weight of the copolymer is 500 or more and 100,000 or less, preferably 500 or more but less than 5,000, or more than 40,000 and 100,000 or less. (ii) The aromatic vinyl compound monomer units are aromatic vinyl compounds having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer units is 70% by mass or less, preferably more than 0% by mass and 70% by mass or less. (iii) The aromatic polyene monomer units are one or more selected from polyenes having 5 to 20 carbon atoms and having multiple vinyl groups and / or vinylene groups in the molecule, and the content of vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 to 20 per number-average molecular weight. (iv) The olefin monomer unit is one or more olefins selected from olefins having from 2 to 20 carbon atoms, the content of the olefin monomer units is 30% by mass or more, and the total of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units is 100% by mass.

[0056] <Production Method> The present composition can be produced by applying known production methods, and the production method is not particularly limited. For example, the composition can be produced based on the methods described in JP 2009-161743 A, JP 2010-280771 A, WO 00 / 37517, etc. In addition, the use of a single-site coordination polymerization catalyst composed of a transition metal compound and a co-catalyst is preferred because it allows for efficient production of an olefin-aromatic vinyl compound-aromatic polyene copolymer. In this production method, the transition metal compound represented by the above-mentioned general formula (I) can be added as a catalyst to raw materials containing an olefin monomer, an aromatic vinyl compound monomer, and an aromatic polyene monomer.

[0057] Furthermore, a co-catalyst containing one or more compounds selected from the group consisting of organoaluminum compounds and boron compounds may be added to form an active species consisting of the catalyst and the co-catalyst, which then initiates a single-site coordination polymerization reaction of the raw materials, thereby producing the composition.

[0058] <Varnish> In one embodiment of the present invention, a varnish containing the above-described composition and a solvent can be provided. In this specification, the term "varnish" refers to a substance that is liquid due to the inclusion of a solvent.

[0059] As described above, the varnish has an appropriate viscosity and is a viscous liquid. The varnish can be applied, impregnated, filled, or dripped onto other materials by an appropriate method, followed by removal of the solvent to form a molded product. It can then be cured with heat or light to obtain the desired cured product. These properties are useful because they can be used to form insulating coatings or layers by various transfer molding (pressure molding), application onto or between substrates or semiconductor device materials, or extrusion lamination or spin coating to form sheets or films, followed by curing. Furthermore, the polymerization liquid used to produce the present copolymer compound (which generally contains, in addition to the present copolymer compound, a solvent used in polymerization, such as toluene, ethylbenzene, cyclohexane, or methylcyclohexane; residual monomers, such as styrene or divinylbenzene; and residual monomers, such as olefin monomers; and catalyst and co-catalyst components) can also be used as a varnish. Alternatively, a varnish can be obtained by distilling off some or all of the solvent and residual monomers from the present polymerization liquid under reduced pressure, followed by diluting with the above-mentioned solvent as needed. That is, the present varnish may contain residual monomers from the polymerization and the solvent used in the polymerization.

[0060] <Solvent> An appropriate solvent may be added to the composition as needed. The amount of solvent used is not particularly limited. The solvent is used to adjust the viscosity and fluidity of the composition. In particular, when the resin composition of this embodiment is in the form of a varnish, a solvent is preferably used. A solvent with a high boiling point at atmospheric pressure, i.e., low volatility, results in a uniform thickness of the applied film. Therefore, a solvent having a boiling point of at least a certain level is preferred. The boiling point is preferably approximately 75°C or higher at atmospheric pressure, more preferably 100°C or higher and 300°C or lower, and even more preferably 130°C or higher and 300°C or lower. Solvents known in the art can be used, and are not particularly limited. Examples of solvents that can be used include cyclohexane, cyclohexanone, methyl ethyl ketone (MEK), toluene, ethylbenzene, xylene, mesitylene, tetralin, acetone, limonene, mixed alkanes, and mixed aromatic solvents. The amount of the solvent used in the composition of the present embodiment can be appropriately set depending on the desired performance, and is arbitrary. However, the amount is preferably 5 to 500 parts by mass, more preferably 10 to 300 parts by mass, and most preferably 50 to 150 parts by mass, relative to 100 parts by mass of the present compound, which is a copolymer.

[0061] When a raw material that is poorly soluble in toluene or other aromatic solvents, such as a specific bismaleimide, is used as a component of the present composition, methyl ethyl ketone (MEK) can be used as the solvent.

[0062] The composition and varnish may contain additives that are commonly used in resins in the industry, such as antioxidants, weathering agents, light stabilizers, lubricants, compatibilizers, antistatic agents, etc., to the extent that the desired effects and purposes are not impaired. The composition and varnish of the present embodiment are obtained by mixing, dissolving, or melting the various additives described above, and any known method can be used for mixing, dissolving, or melting.

[0063] The present composition can be mixed by a known kneading method, for example, a twin-screw kneader, various rolls, various kneaders, etc. When the composition is a varnish, it may be mixed by adding it to the varnish and stirring.

[0064] In one embodiment of the present invention, a cured product of the above-described composition or varnish can be provided. The cured product can be used to manufacture a CCL substrate, an FCCL substrate, an interlayer insulating material, or a coverlay. That is, the composition is particularly suitable as an electrical insulating material for high-frequency signals.

[0065] <Molded Articles> Molded articles obtained from the present composition and the like can have any shape. These compositions can exhibit the properties of thermoplastic resins. Therefore, under conditions that do not cause crosslinking, they can be molded into shapes such as sheets, tubes, strips, pellets, etc. in a substantially uncured state using known molding methods for thermoplastic resins, such as extrusion molding, injection molding, press molding, and inflation molding, and then crosslinked (cured). For example, when the composition is a varnish, it is generally obtained as a sheet or film-like molded article by applying it to a substrate and removing the solvent by heating, reducing pressure, air-drying, etc. These methods can produce uncured sheets and films. Alternatively, composites can be obtained by impregnating a porous substrate, woven fabric, or nonwoven fabric with the present varnish and removing the solvent. Dropping the composition onto a substrate and removing the solvent can also produce shapes such as hemispherical shapes. The sheet may be uncured (semi-cured) to the extent that it can maintain its sheet shape, or it may be fully cured. The degree of curing of the composition can be quantitatively measured using known dynamic mechanical analysis (DMA).

[0066] <Curing> The curing of a molded article obtained from the present composition, etc. can be carried out by a known method, taking into consideration the curing conditions (temperature, time, pressure) of the raw materials and curing agent contained therein. When the curing agent used is a peroxide, the curing conditions can be determined by taking into consideration the half-life temperature, etc. disclosed for each peroxide.

[0067] The cured product of the molded article obtained from the present composition is sufficiently cured, and the gel content (gel fraction) measured in accordance with ASTM is not particularly limited, but may be 90 mass% or more. The dielectric loss tangent of the cured product measured at a frequency of 40 GHz and 23°C is not particularly limited, but is preferably 0.003 or less, more preferably 0.002 or less, and even more preferably 0.001 or less.

[0068] In an embodiment of the present invention, it is also possible to provide a CCL substrate, an FCCL substrate, an interlayer insulating material, a coverlay, etc., which contain the above-mentioned cured product.

[0069] The features of the present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. That is, the materials, amounts used, ratios, processing details, processing procedures, etc. shown in the following examples can be appropriately changed as long as they do not deviate from the spirit of the present invention. Furthermore, the values ​​of various production conditions and evaluation results in the following examples represent preferred upper or lower limits in the embodiments of the present invention, and preferred numerical ranges may be defined by combining the above-mentioned upper or lower limits with the values ​​of the following examples or values ​​between the examples.

[0070] Examples 1 to 6 and Comparative Examples 1 to 3 Examples 1 to 6 and Comparative Examples 1 to 3 were prepared based on the raw material compositions (shown in mol% or ppm in the tables) shown in the following tables. Each copolymer was produced based on the production methods described in JP-A-2009-161743 and JP-A-2010-280771.

[0071] The following catalysts were used. The following symbols are used in the table to indicate the catalysts: Catalyst A: dimethylmethylenebiscyclopentadienylzirconium dichloride (Zr catalyst) Catalyst B: diphenylmethylene(1-indenyl)cyclopentadienylzirconium dichloride

[0072] The co-catalysts used were tritium tetrakis(pentafluorophenyl)borate ("TRI-FABA" manufactured by Tosoh Finechem Co., Ltd.), N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate ("DAN-FABA" manufactured by Tosoh Finechem Co., Ltd.), and modified methylaluminoxane ("MMAO" manufactured by Tosoh Finechem Co., Ltd.). Product names are used in the table.

[0073] Triisobutylaluminum ("TIBAL" manufactured by Tosoh Finechem Co., Ltd.) was used as a scavenger. The amount of scavenger added was adjusted by back-calculating from the target amount of aluminum.

[0074] Toluene was used as the solvent. Ethylene (Et), styrene (St), divinylbenzene (DVB), and in some examples, 1-hexene were used as raw material monomers. A 10 L polymerization vessel equipped with a stirrer and a heating / cooling jacket was used. The catalyst and co-catalyst were added and polymerization was carried out for 2 hours at the polymerization temperature shown in the table, followed by the addition of isopropanol, to obtain an LDM resin solution. The mixture was heated at 80°C under reduced pressure with stirring for 2 hours, and then concentrated to obtain the compositions of the Examples and Comparative Examples.

[0075]

[0076] The copolymers and compositions obtained above were analyzed by the following methods.

[0077] <Analysis of Chemical Structure of Compound> The composition ratio of each component is shown in the table. The composition ratio of ethylene (Et), α-olefin (1-hexene in this example), styrene (St), and divinylbenzene (DVB) in the copolymer, the content of vinyl group units derived from divinylbenzene, and the ratio of terminal vinyl groups to terminal vinylidene groups were calculated using the following formula: 1 The determination was made from the peak area intensity assigned to each component in H-NMR (using the method described above). The sample was dissolved in deuterated 1,1,2,2-tetrachloroethane, and the measurement was carried out at 23°C.

[0078] The NMR spectrum peaks were as follows: 0.7 to 1.02 ppm: α-olefin CH3, 3H 0.5 to 2.1 ppm: St + DVB + Et + α-olefin CH2, 2H 4.5 to 4.7 ppm: terminal vinylidene CH2, 2H … Vd 4.8 to 5.0 ppm: terminal vinyl CH2, 2H … Vn(2) 5.12 to 5.35, 5.6 to 5.8 ppm: DVB vinyl CH2,2H … 2Vn 6.6 to 6.8 ppm: DVB vinyl CH,1H 6.8 to 7.4 ppm: St aromatic ring C6H5,5H, DVB aromatic ring C6H4,4h

[0079] <Measurement of the Amounts of Component (B) and Component (C)> Measurement was performed by ICP atomic emission spectroscopy under the following conditions in accordance with JIS K0116:2014. 0.5 g of the composition was weighed into a platinum crucible and incinerated on a hot plate, an electric stove, and an electric furnace (gradually heated to 600°C). 0.5 ml of HCl (1+1) (a 1:1 volumetric mixture of hydrochloric acid and water) and ultrapure water were added to the residue, and after heating and dissolution, the mixture was adjusted to a constant volume of 5 ml to form a test solution, which was then quantitatively analyzed by ICP atomic emission spectroscopy (using an Agilent 5110VDV).

[0080] <Molecular Weight Measurement> The molecular weight of the copolymer was determined by GPC (gel permeation chromatography) to determine the number average molecular weight (Mn) and weight average molecular weight (Mw) converted to standard polystyrene, and the ratio (Mw / Mn) was also determined. Measurements were carried out under the following conditions. Column: Two TSK-GEL MultiporeHXL-M φ7.8 × 300 mm (manufactured by Tosoh Corporation) connected in series were used. Column temperature: 40°C Solvent: THF (tetrahydrofuran) Flow rate: 1.0 ml / min Detector: RI detector

[0081] <Solution Transparency> Each composition was dissolved in toluene to prepare a 60% by mass solution. A blank piece of paper with a cross written on it in black oil-based ink was placed under a 30 mL glass beaker conforming to JIS R3503:1994, and 30 mL of the prepared solution was poured into the beaker. If the cross was visible to the naked eye from above the beaker, the transparency was judged to be good, and if it was not visible, the transparency was judged to be NG.

[0082] Each composition was cured according to the following procedure, and the physical properties of the cured product were measured as follows. Using a vessel equipped with a heating and cooling jacket and a stirring blade, the composition prepared above and a solvent (toluene) were heated to approximately 60°C and stirred to dissolve the compound. Furthermore, 1 part by mass of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne-3 (Perhexyne 25B, manufactured by NOF Corporation) was added as a curing agent per 100 parts by mass of the composition, dissolved, stirred, and mixed to obtain a varnish-like composition. The resulting composition was poured into a silicone mold (frame length 7 cm, width 7 cm, thickness 0.2 mm) on a Teflon (registered trademark) sheet placed on a glass plate, air-dried, and then further dried in a vacuum dryer at 60°C for at least 3 hours to obtain an uncured sheet. Furthermore, a Teflon sheet and an SUS mold were placed under a load of 5 MPa in a press, and heat treatment was carried out at 120°C for 30 minutes, 150°C for 30 minutes, and then 200°C for 120 minutes.The Teflon sheet and the SUS mold were then removed to obtain a cured sheet.

[0083] <Dielectric Constant and Dielectric Loss (Dielectric Loss Tangent)> The dielectric loss tangent was measured at 23°C and 40 GHz using a cavity resonator perturbation method (Agilent Technologies 8722ES Network Analyzer, Keysight Technologies 40 GHz split cylinder resonator) using a 0.2 mm × 25 mm × 30 mm sample cut out from the sheet.

[0084] <Storage modulus> Measurements were made using a dynamic mechanical analysis (DMA) device (RSA-III, manufactured by Rheometrics) at a frequency of 1 Hz and in the temperature range of 20°C to +300°C. Measurement samples (3 mm x 40 mm) were cut out from films approximately 0.2 mm thick and measured to determine the storage modulus at 25°C. The main measurement parameters involved in the measurement were as follows: Measurement frequency 1 Hz Heating rate 3°C / min Sample measurement length 13 mm Test Type = Dynamic Temperature Ramp (DTempRamp) Initial Static Force 5.0 g Auto Tension Sensitivity 1.0 g Max Auto Tension Rate 0.033 mm / s Max Applied Strain 1.5% Min Allowed Force 1.0 g Strain 0.1%

[0085] All of the compositions according to Examples 1 to 6 were excellent in terms of dielectric properties, storage modulus, and solution transparency.

[0086] On the other hand, in Comparative Examples 1 to 3, which did not contain component (B), the transparency of the solution was poor.

Claims

1. A composition comprising: (A) an olefin-aromatic vinyl compound-aromatic polyene copolymer; (B) boron having a content of 0.2 ppm or more as measured by inductively coupled plasma atomic emission spectroscopy in accordance with JIS K0116:2014; and (C) aluminum having a content of 100 ppm or more and 2,000 ppm or less as measured by inductively coupled plasma atomic emission spectroscopy in accordance with JIS K0116:2014; and having a number average molecular weight of 40,000 or less.

2. The composition according to claim 1, wherein the component (A) satisfies the following conditions (1) to (4): (1) the number average molecular weight of the copolymer is 5,000 to 40,000; (2) the aromatic vinyl compound monomer unit is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0 to 70 mass%; (3) the aromatic polyene monomer unit is one or more selected from polyenes having 5 to 20 carbon atoms and having multiple vinyl groups and / or vinylene groups in the molecule; (4) the olefin monomer unit is a single or multiple units selected from olefins having 2 to 20 carbon atoms, and the total of the olefin monomer unit, the aromatic vinyl compound monomer unit, and the aromatic polyene monomer unit is 100 mass%.

3. The composition according to claim 2, wherein the above (3) satisfies the following condition (3a): (3a) the aromatic polyene monomer unit is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene monomer unit is 1.5 to 20 per number average molecular weight.

4. The composition according to claim 1, wherein the content of the component (B) measured by ICP atomic emission spectroscopy in accordance with JIS K0116:2014 is in the range of 0.2 ppm or more and 10 ppm or less.

5. The composition according to claim 1, wherein the content of component (C) is in the range of 100 ppm or more and 1500 ppm or less.

6. The composition according to claim 5, wherein the content of component (C) is in the range of 100 ppm or more and 1100 ppm or less.

7. The composition according to claim 1, wherein the ratio of number average molecular weight (Mn) to weight average molecular weight (Mw), Mw / Mn, is 10 or less.

8. A cured product of the composition according to any one of claims 1 to 7.

9. A CCL substrate, an FCCL substrate, an interlayer insulating material, or a coverlay, comprising the cured product according to claim 8.

Citation Information

Patent Citations

  • Copolymer, its production and product molded therefrom

    JP2000313724A

  • Method for producing heat-resistant cross copolymer, heat-resistant cross copolymer obtained, and its usage

    JP2009167387A

  • Cross-copolymer and method for producing the same

    JP2017222822A

  • Cross-copolymer, and resin composition

    WO2015152343A1

  • Process for producing (olefin / aromatic vinyl)-based copolymer and process for producing cross-copolymer

    WO2017122295A1