Packaging bag

The packaging bag's laminate structure with a fluororesin-based water vapor barrier layer addresses the issue of barrier property deterioration due to water vapor absorption, ensuring effective oxygen and water vapor barrier performance for maintaining content integrity.

WO2024190875A1PCT designated stage expired Publication Date: 2024-09-19FUJIMORI KOGYO CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010032
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-16
Filing Date
2024-03-14
Publication Date
2024-09-19

AI Technical Summary

Technical Problem

Packaging bags with water vapor barrier resin layers face issues where water vapor absorption leads to deterioration of barrier properties, affecting both oxygen and water vapor barrier performance, which is critical for maintaining the integrity of contents like pharmaceuticals and cosmetics.

Method used

A packaging bag design featuring a laminate structure with a sealant layer, an oxygen barrier layer, and a water vapor barrier layer in sequence, where the water vapor barrier layer contains fluororesin, such as polychlorotrifluoroethylene (PCTFE), to maintain low water vapor permeability and prevent absorption, thereby preserving oxygen barrier properties.

Benefits of technology

The packaging bag effectively maintains both oxygen and water vapor barrier properties, ensuring the contents remain protected from oxidation and moisture absorption, even when exposed to water vapor, thus extending the shelf life and quality of the packaged items.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010032_19092024_PF_FP_ABST
    Figure JP2024010032_19092024_PF_FP_ABST
Patent Text Reader

Abstract

A packaging bag according to the present invention comprises a bag body including: a bonded part that is obtained by layering laminates, each of which includes a sealant layer, an oxygen barrier layer, and a water vapor barrier layer in the stated order, such that the sealant layer sides thereof face each other, and fusing the outer peripheral edges of both laminates together; and a storage chamber that is defined by the laminates and the bonded part, and that can be filled with contents. The water vapor barrier layer contains a fluorine-based resin.
Need to check novelty before this filing date? Find Prior Art

Description

packaging bag

[0001] The present invention relates to a packaging bag.

[0002] BACKGROUND ART In various fields such as the medical, food, and cosmetic fields, bag-shaped packages formed by stacking laminates of multiple types of resin films and joining the outer periphery by heat sealing or the like are used as packages for filling contents such as medicines, food products, and cosmetics.

[0003] As such a packaging body, for example, a packaging material having a water vapor permeability of 20 g / (m) on both sides of an oxygen barrier resin layer made of a highly hydrogen-bonding resin containing an inorganic layered compound is used. 2 d) A packaging bag formed using a gas barrier film having a gas barrier layer in which the following water vapor barrier resin layer is disposed has been disclosed (for example, Patent Document 1).

[0004] Japanese Patent Application Publication No. 2015-36215

[0005] However, in the packaging bag of Patent Document 1, the barrier property may be reduced when the water vapor barrier resin layer absorbs water vapor. When water vapor passes through the water vapor barrier resin layer and reaches the oxygen barrier resin layer, the oxygen barrier resin layer absorbs the water vapor, resulting in a problem of reduced oxygen barrier property.

[0006] It is important that the packaging bag maintains low oxygen permeability and oxygen barrier properties so that the contents will not oxidize and deteriorate until they are used, and that it also maintains low water vapor permeability and water vapor barrier properties so that the concentration of the contents does not change.

[0007] An object of one aspect of the present invention is to provide a packaging bag that can maintain oxygen barrier properties and water vapor barrier properties.

[0008] One aspect of the present invention provides a packaging bag having a bag body including a joint formed by overlapping laminates having a sealant layer, an oxygen barrier layer, and a water vapor barrier layer in this order with the sealant layer sides facing each other and welding the outer peripheral edges of the laminates together, and a storage chamber defined by the laminates and the joint and filled with contents, wherein the water vapor barrier layer contains a fluorine-based resin.

[0009] According to one aspect of the present invention, a packaging bag capable of maintaining oxygen barrier properties and water vapor barrier properties is provided.

[0010] Fig. 2 is a plan view of a packaging bag according to a first embodiment of the present invention. Fig. 3 is a cross-sectional view taken along the line II in Fig. 1. Fig. 4 is a cross-sectional view of a packaging bag according to a second embodiment of the present invention.

[0011] Hereinafter, embodiments of the present invention will be described in detail. To facilitate understanding of the description, the same components in each drawing are denoted by the same reference numerals, and duplicate descriptions will be omitted. The scale of each component in the drawings may differ from the actual scale. In this specification, unless otherwise specified, the symbol "to" indicating a range of values ​​means that the values ​​before and after it are included as the lower and upper limits.

[0012] <First embodiment> [Packaging bag] A packaging bag according to a first embodiment of the present invention will be described. Fig. 1 is a plan view of the packaging bag according to this embodiment, and Fig. 2 is a cross-sectional view taken along the line II in Fig. 1. As shown in Fig. 1, the packaging bag 1A according to this embodiment has a bag main body 10A and may have a spout 20 joined to the bag main body 10A. The packaging bag 1A accommodates contents within the bag main body 10A. In this embodiment, the packaging bag 1A is composed of the bag main body 10A and the spout 20, but may also have other components.

[0013] Examples of the contents include pharmaceuticals (drugs), cells, tissues, organs, biomaterials, blood, body fluids, enzymes, antibodies, beauty products, nutrients, health supplements, cosmetics, and foods. Of these, pharmaceuticals are preferred. Preferred examples of pharmaceuticals include biopharmaceuticals. Preferred examples of biopharmaceuticals include protein preparations.

[0014] The form of the contents is not particularly limited and may be, for example, a solid, liquid, gas, powder, granules, a mixture, a composition, a dispersion, etc. Furthermore, when the contents are liquid, the liquid may be an aqueous solution containing a drug.

[0015] When the contents are placed in the bag body 10A, the bag body 10A may be filled with an inert gas such as nitrogen or a liquid.

[0016] The packaging bag 1A is a pouch, but the shape of the packaging bag 1A is not particularly limited and may be, for example, a three-sided bag, a four-sided bag, a seamed bag, a gusset bag, a self-standing bag, an inner bag for a bag-in-box, an inner bag for a drum can, etc.

[0017] As shown in FIG. 2, the bag body 10A is formed of a pair of laminates 11A, and is formed into a bag shape by stacking the pair of laminates 11A facing each other and bonding their outer peripheral edges together.

[0018] The bag body 10A has a joint 101 formed by stacking a pair of laminated bodies 11A facing each other and welding their outer peripheral edges together, and a storage chamber 102 defined by the pair of laminated bodies 11A and the joint 101.

[0019] The joint 101 is provided in a closed ring shape on the periphery of the bag body 10A. The joint 101 has a first joint 101-1 where the laminate 11A and the spout 20 are joined, and a second joint 101-2 where the laminates 11A are joined to each other. In a plan view of the bag body 10A, the first joint 101-1 and the second joint 101-2 are formed continuously.

[0020] The storage chamber 102 is a space into which the contents are filled. Note that the specific state, shape, etc. of the contents are not shown in the drawings. Before filling the contents, the bag body 10A may have a filling port, for example, in a part of the joint 101, for filling the contents into the storage chamber 102.

[0021] 2, the laminate 11A includes a sealant layer 111, an oxygen barrier layer 112, and a water vapor barrier layer 113 laminated in this order. The bag body 10A is formed by placing the sealant layers 111 of a pair of laminates 11A opposite each other and bonding the outer peripheral edges of the sealant layers 111 together.

[0022] (Sealant Layer) The sealant layer 111 is used when the laminate 11A is bonded together by heat sealing or the like to form a bag shape. The sealant layer 111 faces the storage chamber 102 and is a layer that comes into contact with the contents.

[0023] The sealant layer 111 preferably contains a cyclic olefin resin because it has non-adsorption properties.

[0024] Examples of cyclic olefin resins include cyclic olefin polymers (COP), cyclic olefin copolymers (COC), etc. The resin component constituting the sealant layer 111 may be one or more types of cyclic olefin resins, or may be a mixture of a cyclic olefin resin with another resin or elastomer, etc.

[0025] Examples of COPs include a homopolymer of a cyclic olefin, a copolymer of two or more types of cyclic olefins, or a hydrogenated product thereof. The COP is preferably an amorphous polymer, and more preferably a ring-opening polymer of a cyclic olefin obtained by metathesis or the like, or a hydrogenated product thereof. Compared to cyclic olefin copolymers and the like, COPs contain a higher proportion of alicyclic structures and have excellent non-adsorption properties for the contents contained in the storage chamber 102.

[0026] Examples of COC include copolymers of one or more cyclic olefins and one or more acyclic olefins, or hydrogenated products thereof. The cyclic olefin copolymer is preferably an amorphous polymer, and more preferably a copolymer of a cyclic olefin and ethylene, or a hydrogenated product thereof.

[0027] The cyclic olefin used as a constituent monomer of the cyclic olefin resin is an unsaturated hydrocarbon (olefin) having at least one ring structure. Examples include vinylcycloalkanes having a cycloalkane with 3 to 20 carbon atoms and derivatives thereof, monocycloalkenes having 3 to 20 carbon atoms and derivatives thereof, and cyclic olefins having a norbornene skeleton (norbornene-based monomers).

[0028] Examples of norbornene-based monomers include bicyclo[2.2.1]-2-heptene (norbornene) and its derivatives. Derivatives include compounds having a substituent such as an alkyl group, compounds having two or more unsaturated bonds such as norbornadiene, and compounds having three or more ring structures, two of which constitute a norbornene skeleton. Examples of norbornene-based monomers having three or more ring structures include tricyclo[5.2.1.0]-2-heptene (norbornene). 2,6 ]decene (dihydrodicyclopentadiene), compounds in which one or more molecules of cyclopentadiene are added to norbornene or dihydrodicyclopentadiene by Diels-Alder reaction (e.g., tetracyclododecene, pentacyclopentadecene, hexacycloheptadecene, etc.), hydrogenated products thereof, isomers with different double bond positions, alkyl-substituted products, etc.

[0029] Examples of acyclic olefins used as constituent monomers of COC include α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene, and alkenes such as 3-decene and 3-dodecene.

[0030] The thickness of the sealant layer 111 is preferably 10 μm to 100 μm, more preferably 20 μm to 60 μm, and even more preferably 30 μm to 50 μm. If the thickness of the sealant layer 111 is 10 μm to 100 μm, the sealant layers 111 of the laminate 11A can be bonded together by heat sealing or the like to form the laminate 11A into a bag shape. The upper and lower limits of the thickness of the sealant layer 111 may be combined in any desired manner.

[0031] When the sealant layer 111 contains a cyclic olefin resin, the thicker the sealant layer 111, the lower the water vapor permeability (water vapor transmission rate) of the bag body 10A tends to be. On the other hand, the thicker the sealant layer 111, the more likely the sealant layer 111 is to crack. When the sealant layer 111 contains a cyclic olefin resin, if the thickness of the sealant layer 111 is 20 μm to 60 μm, the sealant layer 111 can reduce the water vapor permeability while suppressing a decrease in strength.

[0032] In this specification, the thickness of the sealant layer 111 refers to the length in the direction perpendicular to the main surface of the sealant layer 111. The thickness of the sealant layer 111 may be, for example, the thickness measured at an arbitrary location on the cross section of the sealant layer 111, or may be the average value of measurements measured at several arbitrary locations. Hereinafter, the definition of thickness is similar for other members.

[0033] (Oxygen Barrier Layer) The oxygen barrier layer 112 is provided between the water vapor barrier layer 113 and the sealant layer 111 .

[0034] Materials that can be used to form the oxygen barrier layer 112 include ethylene-vinyl alcohol copolymer (EVOH) and vinylidene chloride. These may be used alone or in combination of two or more. Among these, it is preferable that the oxygen barrier layer 112 contains EVOH. By including EVOH in the oxygen barrier layer 112, the bag body 10A can have excellent mechanical strength and optical properties and low water vapor permeability.

[0035] The ethylene content of the EVOH is not particularly limited, but in order for the oxygen barrier layer 112 to exhibit oxygen barrier properties, it is preferably 1% to 50%, more preferably 30% to 46%, and even more preferably 32% to 44%.

[0036] When heat-sealing the pair of laminates 11A with the sealant layer 111, it is necessary to heat the sealant layer 111 until the resin contained in the sealant layer 111 melts. At this time, in order to suppress deformation and deterioration of the laminate 11A, the heating temperature during heat-sealing needs to be lower than the melting temperature of the resin contained in the oxygen barrier layer 112. Therefore, the type of resin contained in the sealant layer 111 is limited depending on the type of resin contained in the oxygen barrier layer 112. In the laminate 11A of this embodiment, by using a fluororesin with a higher glass transition temperature Tg than resins that have traditionally been used for water vapor barrier layers, the options for materials for forming the sealant layer 111 can be broadened.

[0037] The oxygen permeability of the oxygen barrier layer 112 is 15 cc / (m2 The oxygen barrier property of the oxygen barrier layer 112 is preferably 15 cc / (m 2 The lower limit of the oxygen barrier property of the oxygen barrier layer 112 is not particularly limited, and may be any thickness appropriate for the intended use of the packaging bag 1A.

[0038] The thickness of the oxygen barrier layer 112 may be 15 μm or more. If the thickness of the oxygen barrier layer 112 is 15 μm or more, the laminate 11A has an oxygen permeability of 15 cc / (m 2 The upper limit of the thickness of the oxygen barrier layer 112 is not particularly limited, and may be set to any appropriate thickness depending on the type of oxygen barrier layer 112, the intended use of the packaging bag 1A, and the like.

[0039] The oxygen barrier layer 112 may be a single layer made up of one layer, or may be a laminate of two or more layers.

[0040] (Water Vapor Barrier Layer) The water vapor barrier layer 113 is a layer exposed to the outside of the accommodation chamber 102, and contains a fluorine-based resin.

[0041] As fluorine-based resin, polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether (EPA), tetrafluoroethylene-ethylene copolymer (ETFE), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), chlorotrifluoroethylene-ethylene copolymer (ECTFE) etc. can be enumerated.Among these, polychlorotrifluoroethylene (PCTFE) is preferred.The above-mentioned resin can be used alone or in combination of two or more kinds.

[0042] The water vapor barrier layer 113 may be formed by including, in addition to a fluorine-based resin, a material that is generally used as a material having water vapor barrier properties. Examples of materials having water vapor barrier properties other than a fluorine-based resin include metal foils such as aluminum foil; vapor-deposited layers formed by vapor-depositing inorganic materials such as aluminum, silica, and alumina; and resin layers made of polyolefin-based resins, ethylene-vinyl alcohol copolymers (EVOH), polyvinylidene chloride (PVDC), and fluorine-based resins. These may be used alone or in combination of two or more.

[0043] Examples of the olefin-based resin include polyethylene-based resin, cyclic olefin-based polymer, etc. Examples of the polyethylene-based resin include polypropylene (PP), high-density polyethylene (HDPE), linear low-density polyethylene (LLDPE), etc.

[0044] The water vapor barrier layer 113 contains a fluororesin, and preferably contains PCTFE among the fluororesins. By including a fluororesin in the water vapor barrier layer 113, the bag body 10A has excellent mechanical strength and optical properties, a low water vapor permeability, and can suppress deterioration of the barrier properties due to absorption of water vapor.

[0045] Furthermore, the water vapor barrier layer 113 is preferably formed from a resin having a melting point higher than the sealing temperature of the sealant layer 111. Fluorine-based resins generally have a higher melting temperature than the resins used in the sealant layer 111. Therefore, by forming the water vapor barrier layer 113 containing a fluorine-based resin, the layer can function as a base material when the pair of laminates 11A are heat-sealed with the sealant layer 111, and the choice of materials for forming the sealant layer 111 can be broadened.

[0046] The thickness of the water vapor barrier layer 113 is preferably 10 μm to 100 μm, more preferably 15 μm to 80 μm, and even more preferably 20 μm to 60 μm. If the thickness of the water vapor barrier layer 113 is 10 μm to 100 μm, the laminate 11A can be easily formed into a bag shape.

[0047] The water vapor barrier layer 113 may be a single layer or may be a laminate of two or more layers.

[0048] (Other Layers) The laminate 11A may include other layers between any of the sealant layer 111, the oxygen barrier layer 112, and the water vapor barrier layer 113, or on the surface of any of these layers. The type of other layer can be selected appropriately, and examples thereof include a reinforcing layer, a light-shielding layer, a printed layer, a metal foil, synthetic paper, etc.

[0049] Examples of the reinforcing layer include reinforcing resin layers such as biaxially oriented polyethylene terephthalate (O-PET), biaxially oriented nylon (O-Ny), and biaxially oriented polypropylene (OPP).

[0050] The laminate 11A may have a printed layer or a coated layer on the surface (front surface) 113 a of the water vapor barrier layer 113 opposite to the oxygen barrier layer 112 .

[0051] The printing layer can impart distinctiveness and design to the packaging bag 1A by printing ink on the surface 113a of the water vapor barrier layer 113.

[0052] The coating layer is intended to protect the water vapor barrier layer 113 or other layers, such as a printed layer, provided on the water vapor barrier layer 113. Examples of such a coating layer include a thin-film resin layer (resin film) and an ultraviolet-curable resin.

[0053] As described above, the joint 101 is formed by overlapping a pair of laminates 11A so as to face each other, and is formed by fusing together the resins contained in the sealant layers 111 of the pair of laminates 11A. The joint 101 has a layered configuration in which the layers are stacked in the following order from the surface side of one water vapor barrier layer 113 of the laminate 11A toward the surface side of the other water vapor barrier layer 113: water vapor barrier layer 113 / oxygen barrier layer 112 / sealant layer 111 / sealant layer 111 / oxygen barrier layer 112 / water vapor barrier layer 113.

[0054] [Pouring Outlet] As shown in Figure 2, the pouring outlet 20 is sandwiched and joined between opposing sealant layers 111. The pouring outlet 20 preferably contains a cyclic olefin resin, and preferably contains a cyclic olefin resin at least in the portion that comes into contact with the contents. Examples of the cyclic olefin resin that forms the pouring outlet 20 include the same cyclic olefin resins that form the sealant layer 111. The material that forms the pouring outlet 20 and the material that forms the sealant layer 111 may be the same or different, but it is preferable that the pouring outlet 20 and the sealant layer 111 are formed from the same material. The molded product may be a single-color molded product or a multi-color molded product such as a two-color molded product.

[0055] Spout 20 has a cylindrical shape and has a flow path 201 therein for removing the contents. Spout 20 has at least a portion that is housed in storage chamber 102. Spout 20 preferably contains a cyclic olefin resin or a polyolefin resin as a forming material, and more preferably contains a cyclic olefin resin. When spout 20 is formed from a cyclic olefin resin, spout 20 can have excellent non-adsorption properties for the contents.

[0056] The polyolefin resin may be a homopolymer of one type of olefin or a copolymer of two or more types of olefins. Examples of olefins include acyclic olefins such as ethylene, propylene, 1-butene, 1-hexene, 1-octene, and α-olefins. Specific examples of polyolefins include polyethylene, polypropylene, and ethylene-α-olefin copolymers. These polyolefins may also be copolymers containing small amounts of non-olefin vinyl monomers such as vinyl acetate, vinyl chloride, and vinyl alcohol. The olefin may be derived from petroleum-derived olefins, plant-derived olefins, or a combination of both.

[0057] When the polyolefin resin forming the spout 20 is polyethylene, the polyethylene is preferably linear low-density polyethylene (LLDPE). When the spout 20 is formed from LLDPE, the spout 20 can be easily joined to the laminate 11A forming the bag body 10A, improving the handleability and durability of the packaging bag 1A.

[0058] First bonding portion 101-1 is formed by fusing together the resin contained in sealant layer 111 of each of a pair of laminates 11A and spout 20. In first bonding portion 101-1, the layer structure of the joint between laminate 11A and spout 20 is in the following order from the surface side of one water vapor barrier layer 113 of laminate 11A toward the surface side of the other water vapor barrier layer 113: water vapor barrier layer 113 / oxygen barrier layer 112 / sealant layer 111 / spout 20 / sealant layer 111 / oxygen barrier layer 112 / water vapor barrier layer 113.

[0059] As shown in FIG. 2, the laminate 11A may have a portion that joins with the spout 20 at the first joint 101-1.

[0060] Furthermore, the packaging bag 1A may have accessories such as a pouring port, a cock, a label, an opening tab, a handle, etc. in addition to the spout 20. When the accessories are resin molded products, they may have the same configuration as the spout 20 described above.

[0061] [Method for manufacturing packaging bag] An example of a method for manufacturing packaging bag 1A will be described. In the method for manufacturing packaging bag 1A, a resin that is a raw material for water vapor barrier layer 113, a resin that is a raw material for oxygen barrier layer 112, and a resin that is a raw material for sealant layer 111 are laminated in this order to form laminate 11A (step of forming laminate 11A).

[0062] The sealant layer 111, the oxygen barrier layer 112, and the water vapor barrier layer 113 may be laminated by a method such as dry lamination or extrusion lamination to form the laminate 11A.

[0063] Next, the laminate 11A and the spout 20 are joined together (joining step).

[0064] First, the spout 20 is sandwiched between the laminates 11A with the sealant layers 111 of the laminates 11A facing each other.

[0065] Next, the laminate 11A and the spout 20 are joined together to form the first joint 101-1.

[0066] Next, the stacked bodies 11A are joined together to form the second joint portion 101-2.

[0067] In this way, the packaging bag 1A is manufactured.

[0068] As described above, the packaging bag 1A has a bag body 10A including a joint 101 and a storage chamber 102, and the water vapor barrier layer 113 included in the laminate 11A constituting the bag body 10A contains a fluorine-based resin with low water vapor permeability as its forming material. This allows the water vapor barrier layer 113 to have a sufficiently low water vapor permeability and to suppress a decrease in its barrier property against water vapor (water vapor barrier property). This prevents the oxygen barrier layer 112 located inside the storage chamber 102 of the water vapor barrier layer 113 from absorbing water vapor that has passed through the water vapor barrier layer 113. Therefore, the packaging bag 1A can maintain low oxygen permeability to maintain its barrier property against oxygen (oxygen barrier property), and can maintain low water vapor permeability to maintain its water vapor barrier property.

[0069] Packaging bag 1A can contain EVOH in oxygen barrier layer 112. This allows oxygen barrier layer 112 to have low oxygen permeability, allowing packaging bag 1A to reliably exhibit oxygen barrier properties.

[0070] The packaging bag 1A can contain PCTFE as the fluororesin contained in the water vapor barrier layer 113. Among fluororesins, PCTFE has a particularly low water vapor permeability, suppresses moisture absorption, and can maintain water vapor barrier properties. Therefore, if PCTFE is used as the fluororesin contained in the water vapor barrier layer 113, the packaging bag 1A can reliably suppress moisture absorption in the water vapor barrier layer 113, and can more reliably suppress deterioration in the water vapor barrier properties of the water vapor barrier layer 113 and the oxygen barrier properties of the oxygen barrier layer 112. Therefore, the packaging bag 1A can more reliably maintain its oxygen barrier properties and water vapor barrier properties.

[0071] The thickness of the water vapor barrier layer 113 of the packaging bag 1A can be set to 10 μm to 100 μm. This allows the water vapor barrier layer 113 to reduce water vapor permeability while providing flexibility to the packaging bag 1A. Therefore, the packaging bag 1A exhibits water vapor barrier properties and can be easily formed into a bag shape.

[0072] The thickness of the oxygen barrier layer 112 of the packaging bag 1A can be set to 15 μm or more. This allows the oxygen barrier layer 112 to keep the oxygen permeability low while providing flexibility to the packaging bag 1A. Therefore, the packaging bag 1A exhibits oxygen barrier properties and can be easily formed into a bag shape.

[0073] The packaging bag 1A has a spout 20, which can be joined while being sandwiched between the opposing sealant layers 111 of a pair of opposing laminates 11A. This prevents water vapor and air from entering the storage chamber 102 from the outside through the gap between the spout 20 and the sealant layer 111, allowing the packaging bag 1A to maintain its water vapor barrier properties and oxygen barrier properties. Furthermore, the spout 20 can be formed from a cyclic olefin resin such as COP or COC, just like the sealant layer 111, so the packaging bag 1A can more reliably improve its non-adsorption properties for the contents.

[0074] As described above, since the packaging bag 1A has the above-mentioned characteristics, it can be suitably used as an infusion bag that contains medicines (drugs), nutrients, food and beverages, medical containers, medical equipment, medical supplies, cosmetics, etc. and is subjected to sterilization.

[0075] Second Embodiment A packaging bag according to a second embodiment of the present invention will now be described. Fig. 3 is a cross-sectional view of the packaging bag according to this embodiment, taken along the line II in Fig. 1. As shown in Fig. 3, the packaging bag 1B according to this embodiment is obtained by replacing the laminate 11A constituting the bag body 10A of the packaging bag 1A according to the first embodiment shown in Fig. 1 with a laminate 11B.

[0076] The laminate 11B has an adhesive layer (adhesive resin layer) 114 between each of the sealant layer 111 , the oxygen barrier layer 112 , and the water vapor barrier layer 113 .

[0077] [Adhesive Layer] The adhesive layer 114 includes an adhesive layer 114A provided between the sealant layer 111 and the oxygen barrier layer 112, and an adhesive layer 114B provided between the oxygen barrier layer 112 and the water vapor barrier layer 113. The adhesive layer 114A and the adhesive layer 114B may be formed of the same type of material or different types of materials.

[0078] The adhesive layer 114 is preferably a first adhesive layer containing a polyethylene-based resin and a modified polyethylene-based resin, or a second adhesive layer containing a polyethylene-based resin, an elastomer component, and a resin composition containing an epoxy group.

[0079] (First adhesive layer) Examples of the polyethylene resin contained in the first adhesive layer include linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), and low-density polyethylene is preferred.

[0080] The modified polyethylene resin contained in the first adhesive layer is a polyethylene resin modified with an unsaturated carboxylic acid or a derivative thereof, and has an acid functional group such as a carboxy group or a carboxylic anhydride group in the polyethylene resin. The modified polyethylene resin contained in the first adhesive layer is preferably obtained by acid-modifying a polyethylene resin.

[0081] The acid modification method includes graft modification in which a polyethylene resin and an acid functional group-containing monomer are melt-kneaded in the presence of a radical polymerization initiator such as an organic peroxide or an aliphatic azo compound.

[0082] The polyethylene-based resin material before modification is not limited as long as it contains ethylene as a raw material monomer, and known polyethylene-based resins can be used appropriately. Specific examples of the polyethylene-based resin include, in addition to the examples described above, ethylene-α-olefin copolymers such as ethylene-propylene copolymer, ethylene-1-butene copolymer, ethylene-4-methyl-1-pentene copolymer, ethylene-1-hexene copolymer, and ethylene-1-octene copolymer; and ethylene-based copolymer resins such as ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, and ethylene-(meth)acrylic acid ester copolymer.

[0083] The acid functional group-containing monomer is a compound having an ethylenic double bond and a carboxy group or a carboxylic acid anhydride group in the same molecule, and examples thereof include various unsaturated monocarboxylic acids, dicarboxylic acids, and acid anhydrides of dicarboxylic acids.

[0084] Examples of the acid functional group-containing monomer having a carboxy group (carboxy group-containing monomer) include α,β-unsaturated carboxylic acid monomers such as acrylic acid, methacrylic acid, maleic acid, nadic acid, fumaric acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, tetrahydrophthalic acid, and endo-bicyclo[2.2.1]-5-heptene-2,3-dicarboxylic acid (endic acid).

[0085] Examples of the acid functional group-containing monomer having a carboxylic acid anhydride group (carboxylic acid anhydride group-containing monomer) include unsaturated dicarboxylic acid anhydride monomers such as maleic anhydride, nadic anhydride, itaconic anhydride, citraconic anhydride, and endic anhydride.

[0086] These acid functional group-containing monomers may be used alone or in combination of two or more types in the components constituting the oxygen barrier layer 112 .

[0087] Among these, as the acid functional group-containing monomer, an acid functional group-containing monomer having an acid anhydride group is preferred, a carboxylic acid anhydride group-containing monomer is more preferred, and maleic anhydride is particularly preferred.

[0088] When a portion of the acid functional group-containing monomer used for the acid modification remains unreacted, it is preferable to use a resin from which the unreacted acid functional group-containing monomer has been removed in advance in order to prevent a decrease in adhesive strength due to the unreacted acid functional group-containing monomer.

[0089] The modified polyethylene resin contained in the first adhesive layer is preferably maleic anhydride modified polyethylene.

[0090] In the first adhesive layer, when the total of the polyethylene resin and the modified polyethylene resin is taken as 100% by mass, the lower limit of the ratio of the polyethylene resin to the total amount of the polyethylene resin and the modified polyethylene resin is preferably 10% or more, more preferably 20% or more. The upper limit of the ratio of the polyethylene resin to the total amount of the polyethylene resin and the modified polyethylene resin is preferably 70% or less, more preferably 60% or less. For example, the mixing ratio of the polyethylene resin to the modified polyethylene resin can be 20:80 to 60:40.

[0091] By using a mixed material of a polyethylene-based resin and a modified polyethylene-based resin for the oxygen barrier layer 112, adhesion between the sealant layer 111, the oxygen barrier layer 112, and the water vapor barrier layer 113 is improved. This makes it possible to prevent delamination of the oxygen barrier layer 112.

[0092] (Second Adhesive Layer) The second adhesive layer contains a resin composition that includes a polyethylene resin, an elastomer component, and a component having an epoxy group.

[0093] The polyethylene-based resin contained in the second adhesive layer is the same as the polyethylene-based resin contained in the mixture of the polyethylene-based resin and the modified polyethylene-based resin. The polyethylene-based resin contained in the resin composition may be biomass polyethylene, petroleum-derived polyethylene, or a mixture of both.

[0094] The polyethylene resin contained in the second adhesive layer is preferably polyethylene polymerized using a metallocene catalyst. Among these, suitable examples include ethylene-α-olefin copolymers such as C4-LLDPE, C6-LLDPE, and C8-LLDPE polymerized using a metallocene catalyst, and long-chain branched polyethylene.

[0095] Polyethylene resins polymerized with methacerone catalysts tend to have narrow molecular weight distributions, which means they contain fewer low-molecular-weight components that can inhibit adhesion, and are thought to provide high adhesive properties when used as adhesives.

[0096] The density of the polyethylene resin in the resin composition is 0.890 g / cm 3 0.940g / cm or more 3 Preferably, 0.910 g / cm or less 3 0.930g / cm or more 3 The following is more preferred:

[0097] The content of the polyethylene resin in the resin composition is 55 parts by mass to 90 parts by mass, and preferably 60 parts by mass to 80 parts by mass. When the content of the polyethylene resin is 90 parts by mass or less, the resin exhibits adhesiveness with the elastomer component described below, and the adhesiveness is enhanced.

[0098] Examples of the elastomer component contained in the second adhesive layer include styrene-based elastomers, acrylic-based elastomers, urethane-based elastomers, ester-based elastomers, etc. However, the elastomer component does not include a component having an epoxy group, which will be described later.

[0099] Among these, styrene-based elastomers are preferred, and examples thereof include block copolymers having a hard segment made of polystyrene or the like and a soft segment made of polyethylene, polybutadiene, polyisoprene, etc. Examples of styrene-based polymers that can be used for the styrene-based elastomer include aromatic olefin-aliphatic olefin copolymers such as styrene-butadiene copolymer, styrene-isoprene copolymer, and styrene-ethylene copolymer.

[0100] The styrene elastomer is preferably a styrene-ethylene-butylene-styrene copolymer (SEBS) obtained by hydrogenating a styrene-butylene-styrene copolymer (SBS) to completely open the unsaturated bonds in the molecule.

[0101] The styrene content is preferably 8% by mass to 24% by mass, more preferably 10% by mass to 20% by mass. When the styrene content is 20% by mass or less, curing of the resin can be suppressed, and a decrease in adhesiveness can be suppressed.

[0102] Specific examples of the elastomer component contained in the second adhesive layer include Dynaron from JSR Corporation, Tuftec H series from Asahi Kasei Chemicals Corporation, and Kraton G Polymer from Kraton Polymers, Inc.

[0103] In the second adhesive layer, the content of the elastomer component is 10 parts by mass to 45 parts by mass, and preferably 20 parts by mass to 40 parts by mass. When the content of the elastomer component is 45 parts by mass or less, a decrease in tensile strength when the second adhesive layer is formed can be suppressed, and a decrease in adhesive strength can be prevented.

[0104] The total amount of the polyethylene resin and the elastomer component is 100 parts by mass.

[0105] The component having an epoxy group contained in the second adhesive layer is preferably a component having an epoxy group and a vinyl group. The component having an epoxy group and a vinyl group is preferably a component having a 1,2-vinyl structure, and is preferably an epoxidized polybutadiene obtained by partially epoxidizing butadiene. Partially epoxidized 1,2-polybutadiene is particularly preferred.

[0106] Specific examples of components having an epoxy group include liquid polybutadiene JP-100 and JP-200 from Nippon Soda Co., Ltd., and Adeka Cizer BF-1000 from Adeka Corporation.

[0107] The number average molecular weight of the component having an epoxy group is preferably 500 to 4000. When the number average molecular weight of the component having an epoxy group is 4000 or less, it is possible to suppress a decrease in adhesiveness due to the component becoming a solid at room temperature, and it is possible to prevent a decrease in adhesiveness.

[0108] In the present embodiment, the number average molecular weight is a value calculated as polystyrene measured by GPC (gel permeation chromatography).

[0109] In the second adhesive layer, the content of the component having an epoxy group is 0.1 to 1.5 parts by mass, preferably 0.5 to 1.0 part by mass, relative to 100 parts by mass of the total amount of the polyethylene resin and the elastomer component. When the content of the component having an epoxy group is 1.5 parts by mass or less, low-molecular-weight components in the resin composition that cause adhesion inhibition can be reduced.

[0110] In the second adhesive layer, the elastomer component and the component having an epoxy group have a common repeating unit and are compatible with each other. The elastomer component and the component having an epoxy group are preferably a combination of styrene-based elastomers or acrylic-based elastomers.

[0111] The resin composition of the second adhesive layer may be a mixture of a polyethylene resin, an elastomer component, and a component having an epoxy group, each mixed in a specific blending ratio. The resin composition of the second adhesive layer has excellent adhesion to fluororesins because the epoxy groups in the component having an epoxy group are compatible with the fluorine component of the fluororesin. The presence of epoxy groups also enables adhesion to metal materials.

[0112] In the second adhesive layer, a polyethylene resin, an elastomer component, and an epoxy group-containing component are mixed in specific blending ratios to form a so-called sea-island structure, with the polyethylene resin representing the "sea" and the elastomer component representing the "islands." Furthermore, the epoxy group-containing component is compatible with the elastomer component, allowing the epoxy group-containing component to be uniformly dispersed in the resin composition. This is thought to protect the epoxy groups between the polyethylene resin and the elastomer component, preventing ring-opening of the epoxy groups due to moisture.

[0113] By using a mixed material of a polyethylene resin, an elastomer component, and a component having an epoxy group for the oxygen barrier layer 112, the adhesion between the sealant layer 111, the oxygen barrier layer 112, and the water vapor barrier layer 113 is improved, making it possible to make the laminate 11A less susceptible to delamination.

[0114] In this way, the packaging bag 1B can maintain its oxygen barrier properties and water vapor barrier properties while suppressing interlayer delamination between the sealant layer 111, the oxygen barrier layer 112, and the water vapor barrier layer 113, because the laminate 11B of the bag body 10A includes the adhesive layer 114.

[0115] Although the embodiments have been described above, they are presented as examples and the present invention is not limited to the above embodiments. The above embodiments can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the spirit of the invention. These embodiments and their modifications are included within the scope and spirit of the invention, and are also included in the inventions and their equivalents as set forth in the claims.

[0116] The present embodiment will be described below using examples, but the present embodiment is not limited to these examples.

[0117] <Preparation of Laminates (Laminate Films)> [Example 1] Cycloolefin polymer (COP), ethylene-vinyl alcohol copolymer (referred to as "EVOH1"; ethylene content: 32%), polychlorotrifluoroethylene resin (PCTFE), and maleic anhydride-modified polyethylene adhesive resin were used to form the sealant layer, oxygen barrier layer, water vapor barrier layer, and adhesive layer (AD) that constitute the laminate (laminated film), respectively. Using a T-die type multilayer film-forming machine, the COP, AD, EVOH1, AD, and PCTFE were extruded by a coextrusion method to prepare a laminate film in which the sealant layer, adhesive layer, oxygen barrier layer, adhesive layer, and water vapor barrier layer were laminated in this order so that their respective thicknesses were as shown in Table 1.

[0118] [Example 2] A laminated film was produced in the same manner as in Example 1, except that in the oxygen barrier layer, EVOH having an ethylene content different from that of EVOH1 (referred to as "EVOH2"; ethylene content: 44%) was used instead of EVOH1.

[0119] Example 3 A laminated film was produced in the same manner as in Example 2, except that the thickness of the sealant layer was changed to 16 μm.

[0120] [Example 4] A laminated film was produced in the same manner as in Example 1, except that the oxygen barrier layer was made of an aromatic polyamide resin (relative viscosity: 2.65, melt viscosity: 500 Pa sec, water content: 300 ppm) obtained by polymerizing metaxylylenediamine and adipic acid instead of EVOH1.

[0121] [Example 5] A laminate film was produced in the same manner as in Example 1, except that the resin forming the water vapor barrier layer in Example 1 was changed to COP and the thickness of the water vapor barrier layer was changed to the thickness shown in Table 1.

[0122] [Example 6] The same procedure as in Example 1 was carried out, except that the laminated film was composed of three layers: a sealant layer, an adhesive layer, and an oxygen barrier layer. A laminated film was produced in which the sealant layer, the adhesive layer, and the oxygen barrier layer were laminated in this order.

[0123] [Example 7] A laminate film was produced in the same manner as in Example 1, except that in Example 2, the resin forming the water vapor barrier layer was changed to COP and the thickness of the water vapor barrier layer was changed to the thickness shown in Table 1.

[0124] [Example 8] The same procedure as in Example 2 was carried out, except that the laminated film was composed of three layers: a sealant layer, an adhesive layer, and an oxygen barrier layer. A laminated film was produced in which the sealant layer, the adhesive layer, and the oxygen barrier layer were laminated in this order.

[0125] In each example, the type and thickness of the material of each layer constituting the laminated film are shown in Table 1.

[0126] <Evaluation> The oxygen permeability and water vapor permeability of the laminated film of each example were measured, and the oxygen barrier property and water vapor barrier property were evaluated.

[0127] [Oxygen Permeability] Oxygen gas was passed through the resulting laminate film at a temperature of 40°C and a relative humidity of 70% RH using an oxygen permeability measuring device in accordance with the electrolytic sensor method (Appendix A) of JIS K 7126-2:2006, "Plastics - Films and Sheets - Gas Permeability Measurement - Part 2: Isobaric Method (Mocon Method)." The amount of oxygen gas that permeated the laminate film (oxygen permeability) was measured using the electrolytic sensor method. The laminate film was positioned so that the sealant layer side faced the chamber into which oxygen gas was introduced, and oxygen gas was allowed to permeate from the sealant layer side of the laminate film to the water vapor barrier layer side. Because oxygen permeates the laminate film, the oxygen permeability of the laminate film was considered to be the oxygen permeability of the package. The measurement results of the oxygen permeability of the laminate film for each example are shown in Table 1.

[0128] [Water Vapor Permeability] The water vapor permeability of the resulting laminate film was measured using an infrared sensor method (MOCON method). Specifically, in accordance with JIS K 7129-2008 Method B, water vapor was allowed to permeate the resulting laminate film under conditions of a temperature of 40°C and a relative humidity of 100% RH using a water vapor permeability measuring device. The amount of water vapor permeating the laminate film was detected with the infrared sensor, and the water vapor permeability was calculated. The laminate film was positioned so that the water vapor barrier layer side faced the chamber into which water vapor was introduced, and water vapor was allowed to permeate from the water vapor barrier layer side of the laminate film to the sealant layer side. Because water vapor permeates the laminate film, the water vapor permeability of the laminate film was considered to be the water vapor permeability of the package. The measurement results of the water vapor permeability of the laminate film for each example are shown in Table 1.

[0129]

[0130] As shown in Table 1, the laminate film of Example 1 had lower oxygen permeability and water vapor permeability and was superior in oxygen barrier property and water vapor barrier property than the laminate films of Examples 5 and 6. This is thought to be because the water vapor barrier layer of the laminate films of Examples 5 and 6 absorbed moisture more than the laminate film of Example 1, resulting in inferior moisture resistance, and the oxygen barrier layer absorbing water vapor that had passed through the water vapor barrier layer, resulting in a decrease in oxygen barrier performance.

[0131] The laminate films of Examples 2 to 4 had lower oxygen permeability and water vapor permeability and were superior in oxygen barrier property and water vapor barrier property than the laminate films of Examples 7 and 8. This is thought to be because the water vapor barrier layer of the laminate films of Examples 7 and 8 absorbed moisture more than the laminate films of Examples 2 to 4, resulting in inferior moisture resistance, and the oxygen barrier layer absorbing water vapor that had passed through the water vapor barrier layer, resulting in a decrease in oxygen barrier performance.

[0132] Therefore, if PCTFE is used in the water vapor barrier layer that constitutes the laminate film, the deterioration of the water vapor barrier layer and oxygen barrier layer can be suppressed, and excellent water vapor barrier properties and oxygen barrier properties can be exhibited.

[0133] Note that aspects according to the present invention are, for example, as follows. <1> A packaging bag having a bag main body including a joint formed by overlapping laminates having a sealant layer, an oxygen barrier layer, and a water vapor barrier layer in this order with the sealant layer sides facing each other and welding the outer peripheral edges of the laminates together, and a storage chamber defined by the laminates and the joint and filled with contents, wherein the water vapor barrier layer contains a fluorine-based resin. <2> The packaging bag according to <1>, wherein the oxygen barrier layer contains an ethylene-vinyl alcohol copolymer. <3> The packaging bag according to <1> or <2>, wherein the fluorine-based resin contains polychlorotrifluoroethylene. <4> The packaging bag according to any one of <1> to <3>, wherein the thickness of the water vapor barrier layer is 10 μm to 100 μm. <5> The packaging bag according to any one of <1> to <4>, wherein the thickness of the oxygen barrier layer is 15 μm or more. <6> The packaging bag according to any one of <1> to <5>, which has a pouring outlet joined to the bag body, and the pouring outlet is sandwiched and joined between the opposing sealant layers. <7> The packaging bag according to any one of <1> to <6>, wherein the contents are a pharmaceutical product. <8> The packaging bag according to any one of <1> to <7>, wherein the packaging bag is an infusion bag.

[0134] This application claims priority based on Japanese Patent Application No. 2023-42338, filed with the Japan Patent Office on March 16, 2023, and incorporates the entire contents of said application by reference.

[0135] 1A, 1B Packaging bag 10A, 10B Bag body 101 Joint 101-1 First joint 101-2 Second joint 102 Storage chamber 11A, 11B Laminate 111 Sealant layer 112 Oxygen barrier layer 113 Water vapor barrier layer 114 Adhesive layer 20 Spout

Claims

1. A packaging bag comprising a bag body including a joint formed by overlapping a laminate having a sealant layer, an oxygen barrier layer, and a water vapor barrier layer in that order with the sealant layer sides facing each other and welding the outer peripheral edges of the laminate, and a storage chamber defined by the laminate and the joint and filled with contents, wherein the water vapor barrier layer contains a fluorine-based resin.

2. The packaging bag according to claim 1, wherein the oxygen barrier layer comprises an ethylene-vinyl alcohol copolymer.

3. The packaging bag according to claim 1, wherein the fluororesin contains polychlorotrifluoroethylene.

4. The packaging bag according to claim 1, wherein the water vapor barrier layer has a thickness of 10 μm to 100 μm.

5. The packaging bag according to claim 1, wherein the oxygen barrier layer has a thickness of 15 μm or more.

6. The packaging bag according to claim 1, further comprising a spout joined to the bag body, the spout being sandwiched and joined between opposing sealant layers.

7. The packaging bag according to claim 1, wherein the contents are medicines.

8. The packaging bag according to claim 1, which is an infusion bag.

Citation Information

Patent Citations

  • Gas barrier layer and gas barrier film

    JP2015036215A

  • Power generator and power generation method

    JP2023042338A

  • Packaging bag

    JP2018188189A

  • Laminate and packaging bag

    JP2020019212A

  • Oxygen-absorbing laminate containing plant-derived material

    JP2022014237A