Electrode for extracting lithium from salt lake by electrochemical deintercalation method, preparation method therefor and use thereof
By superoleophobic and superhydrophilic local modification of the ion screen pores, a hydrophilic and oleophobic film is formed, which solves the problems of electrode hydrophilicity and lithium extraction amount, and achieves efficient lithium ion adsorption effect, saturated adsorption amount and time. promote.
Patent Information
- Application Number
- PCT/CN2023/084574
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
When existing electrochemical deintercalation salt lake lithium extraction electrodes use hydrophilic inorganic nano-oxides and binders, the amounts are difficult to control, resulting in an insignificant improvement in the hydrophilic performance of the electrode or a too low proportion of active materials, which results in lithium extraction per unit area. Volume decreases.
By locally modifying the pores of the ion screen with super-oleophobic and super-hydrophilic properties, epoxy-modified silica powder and adhesives are used to locally modify the ion screen to form a hydrophilic and oleophobic film to improve the mass transfer effect of the solution. Avoid the decrease in the proportion of active materials and the amount of lithium extracted per unit area caused by adding too much hydrophilic substances.
It improves the mass transfer effect of the solution in the electrode pores, enhances the hydrophilicity of the electrode, avoids the decrease in the proportion of electrode active materials and the amount of lithium extracted per unit area, and the saturated adsorption capacity reaches more than 32.1mg/g, and the time required for saturated adsorption It can reach less than 14.9h.
Smart Images

Figure PCTCN2023084574-FTAPPB-I100001 
Figure PCTCN2023084574-FTAPPB-I100002
Abstract
Description
Electrochemical deintercalation method for lithium extraction from salt lakes, preparation method, and application thereof Technical Field
[0001] The present application belongs to the field of lithium extraction from salt lakes, for example, an electrochemical deintercalation method for lithium extraction from salt lakes electrode and its preparation method and application. Background Art
[0002] Over the past few years, supported by national policies, the new energy vehicle industry has experienced rapid growth, leading to a growing demand for lithium and a growing interest in lithium extraction technologies. my country is a major consumer of lithium, and lithium resources are a crucial strategic resource for its industrial development. my country's lithium resources are primarily found in salt lake brines, making the development of suitable lithium extraction technologies of great economic and strategic significance. Currently, developed methods for lithium extraction from salt lakes include adsorption, solution extraction, electrodialysis, and electrochemical deintercalation.
[0003] The electrochemical deintercalation method uses LiFePO4 / FePO4 electrodes as anodes / cathodes, and drives lithium ions to be embedded in the FePO4 electrode material through an external circuit to achieve selective lithium extraction. The mass transfer effect of lithium ions in the electrode is a key factor affecting the lithium extraction rate of the electrochemical deintercalation method. Generally, the electrodes are modified by introducing hydrophilic inorganic nano-oxides and binders to improve the hydrophilicity of the electrodes to the solution and reduce the concentration difference expansion during the lithium extraction process. The amount of hydrophilic inorganic nano-oxides and binders is difficult to control. Adding too little will result in a negligible improvement in the hydrophilicity of the electrode and the mass transfer effect of the solution. Adding too much will result in a low proportion of electrode active material, resulting in a decrease in the amount of lithium extracted per unit area.
[0004] CN113293290A discloses an electrode material for lithium extraction from salt lakes, its preparation method, and its application. By coating the surface of the electrode active material with a graphene oxide / manganese ion sieve composite, the selectivity and hydrophilicity of the electrode active material are improved. Using this modified electrode active material as raw material, an inorganic nano-oxide is introduced during the electrode preparation process to modify the binder. A pore-forming agent is added to create a porous electrode, further improving the electrode's affinity for the solution. The porous structure enhances mass transfer within the electrode, reducing concentration differential expansion during the lithium extraction process and improving the electrode's electrochemical performance.
[0005] CN113265538A discloses a method for preparing highly conductive porous electrodes for lithium extraction from salt lakes. The method involves modifying the binder used in the electrode preparation process by blending inorganic nanoparticles with polar hydrophilic polymers to increase the binder's hydrophilicity. During the electrode slurry preparation process, an inorganic salt pore-forming agent is added to form pores of varying sizes during drying, enhancing mass transfer within the electrode plate. Finally, the prepared electrode material undergoes surface chemical modification in a conductive polymer monomer solution.
[0006] The amount of hydrophilic inorganic nano-oxides and binders used in the above scheme is difficult to control. Adding too little will result in an insignificant improvement in the hydrophilicity of the electrode and the mass transfer effect of the solution. Adding too much will lead to a too low proportion of electrode active substances, resulting in a decrease in lithium extraction per unit area.
[0007] Summary of the Invention
[0008] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0009] The present application provides an electrochemical deintercalation method for extracting lithium from salt lakes, as well as a preparation method and application thereof. The present application aims to improve the hydrophilicity of the mass transfer channels and the mass transfer effect of the solution by locally modifying the pores of the ion sieve to be superoleophobic and superhydrophilic. In addition, the present application successfully avoids the decrease in the proportion of electrode active substances and the decrease in adsorption capacity due to excessive addition of hydrophilic substances.
[0010] To achieve the purpose of this application, this application adopts the following technical solutions:
[0011] In a first aspect, an embodiment of the present application provides a method for preparing a lithium-extraction electrode from a salt lake using an electrochemical deintercalation method, the preparation method comprising the following steps:
[0012] (1) mixing a silicon source, a silane coupling agent, and a solvent to obtain a mixed solution, adding an acid solution to the mixed solution to obtain a sol, ultrasonically treating and aging to obtain an epoxy-modified silica sol, and freeze-drying to obtain epoxy-modified silica powder;
[0013] (2) mixing the ion sieve, epoxy-modified silica powder and a binder, grinding and separating to obtain a partially modified ion sieve;
[0014] (3) The locally modified ion sieve, a binder and a conductive agent are mixed with a solvent to obtain an electrode slurry, and the electrode slurry is coated on the surface of a titanium mesh to obtain the electrochemical deintercalation method salt lake lithium extraction electrode.
[0015] The embodiment of the present application improves the hydrophilicity of the pores and thus enhances the mass transfer of the solution in the pores by locally modifying the pores of the ion sieve to be superoleophobic and superhydrophilic. This preparation method avoids the excessive addition of hydrophilic substances, which leads to a decrease in the proportion of electrode active materials and the amount of lithium extracted per unit area.
[0016] In one embodiment, the silicon source in step (1) includes ethyl orthosilicate.
[0017] In one embodiment, the silane coupling agent includes KH-560.
[0018] In one embodiment, the solvent comprises anhydrous ethanol.
[0019] In one embodiment, the mass ratio of the silicon source, the silane coupling agent and the solvent is (1.5-2.5):1:(4-6), for example: 1.5:1:4, 1.8:1:5, 2:1:5, 2.2:1:5.2 or 2.5:1:6, etc.
[0020] In one embodiment, the acid solution in step (1) comprises nitric acid.
[0021] In one embodiment, the mass ratio of the mixed solution to the acid solution is (3.2-3.5):1, for example: 3.2:1, 3.3:1, 3.4:1 or 3.5:1.
[0022] In one embodiment, the ultrasound duration is 1.5 to 3 hours, for example, 1.5 hours, 1.8 hours, 2 hours, 2.5 hours or 3 hours.
[0023] In one embodiment, the freeze-drying process comprises first freezing at -4°C for 12 hours and then freezing at -40°C for 24 hours.
[0024] In one embodiment, the adhesive in step (2) comprises epoxy resin.
[0025] In one embodiment, the ion sieve includes any one of an iron phosphate ion sieve and a lithium titanate ion sieve, or a combination of the two.
[0026] In one embodiment, the mass ratio of the epoxy-modified silica powder to the ion sieve is (0.2-1):100, for example: 0.2:100, 0.4:100, 0.6:100, 0.8:100 or 1:100.
[0027] The epoxy-modified silica described in the examples of this application exhibits excellent hydrophilic and oleophobic properties. When a hydrophilic and oleophobic film of epoxy-modified silica forms within the pores of the ion sieve, it improves the mass transfer efficiency of the solution within the pores. This preparation method successfully avoids the reduction in the proportion of electrode active material and the amount of lithium extracted per unit area caused by the addition of excessive hydrophilic substances.
[0028] In one embodiment, the mass ratio of the binder to the epoxy-modified silica powder is (0.02-0.1):100, for example: 0.02:100, 0.04:100, 0.06:100, 0.08:100 or 0.1:100, etc.
[0029] Under the action of the adhesive, epoxy-modified silica will form a hydrophilic and oleophobic film in the pores of the ion sieve at high temperatures. This local modification avoids the excessive addition of hydrophilic substances, which leads to a decrease in the proportion of electrode active materials and the amount of lithium extracted per unit area, and improves the mass transfer effect of the solution.
[0030] In one embodiment, the grinding speed in step (2) is 100-200 rpm, for example, 100 rpm, 120 rpm, 150 rpm, 180 rpm or 200 rpm.
[0031] In the embodiment of the present application, when the ball mill is running at high speed, the epoxy-modified silica and epoxy resin will enter the pores of the ion sieve; in addition, by controlling the rotational speed of the high-speed ball mill, the amount of epoxy-modified silica and epoxy resin entering the pores of the positive electrode material can be controlled.
[0032] In one embodiment, the separation comprises air flow separation.
[0033] In one embodiment, the air flow separation velocity is 10-15 m / s, for example, 10 m / s, 11 m / s, 12 m / s, 13 m / s, 14 m / s or 15 m / s.
[0034] In the embodiment of the present application, the evenly mixed particles are sent to an air flow separation device, and the separation of large and small particles is achieved by controlling the wind speed and utilizing the different centrifugal forces exerted on the large and small particles.
[0035] In one embodiment, the binder in step (3) includes polyvinylidene fluoride.
[0036] In one embodiment, the conductive agent includes acetylene black.
[0037] In one embodiment, the solvent comprises N-methylpyrrolidone.
[0038] In one embodiment, the mass ratio of the locally modified ion sieve, binder and conductive agent is (6-8):1:(1.5-2.5), for example: 6:1:1.5, 6.5:1:1.8, 7:1:2, 7.5:1:2.2 or 8:1:2.5, etc.
[0039] In one embodiment, the coating area in step (3) is 1500 to 1800 cm2 , for example: 1500cm 2 , 1550cm 2 , 1600cm 2 , 1700cm 2 , 1750cm 2 or 1800cm 2 wait.
[0040] In one embodiment, the coating density is 70-90 mg / cm 2 , for example: 70mg / cm 2 , 75mg / cm 2 、80mg / cm 2 、85mg / cm 2 or 90 mg / cm 2 wait.
[0041] In a second aspect, an embodiment of the present application provides an electrode for extracting lithium from salt lakes using an electrochemical deintercalation method, wherein the electrode for extracting lithium from salt lakes using an electrochemical deintercalation method is prepared by the method described in the first aspect.
[0042] Compared with the related art, this application has the following beneficial effects:
[0043] (1) This application aims to improve the hydrophilicity of the mass transfer channels and the mass transfer function of the solution by locally modifying the pores of the ion sieve to be superoleophobic and superhydrophilic; in addition, it successfully avoids the decrease in the proportion of electrode active materials and the decrease in adsorption capacity caused by excessive addition of hydrophilic substances.
[0044] (2) When the ball mill is running at high speed, the epoxy-modified silica and epoxy resin will enter the pores of the large particle ion sieve; in addition, by controlling the speed of the high-speed ball mill, the amount of epoxy-modified silica and epoxy resin entering the pores of the positive electrode material can be controlled. When the speed of the cylinder is low, most of the epoxy-modified silica and epoxy resin accumulate on the surface of the particles and are difficult to enter the cracks and defects on the surface of the particles. Subsequently, the epoxy-modified silica and epoxy resin remaining on the surface of the particles will be separated by the air flow separation device.
[0045] (3) The saturated adsorption capacity of the salt lake lithium extraction electrode prepared by the electrochemical deintercalation method described in this application can reach more than 32.1 mg / g, and the time required for saturated adsorption can reach less than 14.9 hours.
[0046] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION
[0047] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.
[0048] Example 1
[0049] This embodiment provides an electrochemical deintercalation method for extracting lithium from salt lakes. The preparation method of the electrochemical deintercalation method for extracting lithium from salt lakes is as follows:
[0050] (1) Tetraethyl orthosilicate, silane coupling agent KH-560 and anhydrous ethanol were mixed and stirred in a mass ratio of 2:1:5 for 10 minutes to obtain a mixed solution A; 0.21% (volume fraction) dilute nitric acid was added dropwise into the mixed solution A and stirred for hydrolysis for 2 hours to obtain a sol (wherein the mass ratio of the mixed solution A to the nitric acid was 3.4:1); after ultrasonic treatment for 2 hours, the sol was aged at room temperature for 3 to 4 weeks to obtain an epoxy-modified silica sol; finally, the sol was placed in a -4°C refrigerator for 12 hours, and then placed in a -40°C freeze dryer for 24 hours to obtain an epoxy-modified silica powder;
[0051] (2) Take the iron phosphate ion sieve, epoxy modified silica, and epoxy resin and fully ball mill them in a high-speed ball mill. After ball milling for 1 hour, send the materials into an air flow separation device to separate the iron phosphate ion sieve and the epoxy modified silica that is not embedded in the pores of the positive electrode material. Finally, place the iron phosphate ion sieve in a 100°C oven to dry to obtain a partially modified iron phosphate ion sieve, wherein the mass ratio of the epoxy modified silica to the positive electrode material is 0.5%; the speed of the ball mill is 150rpm; the air flow velocity in the air flow separation device is 12m / s; the mass ratio of the epoxy resin adhesive to the epoxy modified silica is 0.05%;
[0052] (3) Partially modified iron phosphate ion screen, PVDF, and acetylene black were weighed in a mass ratio of 7:1:2, mixed thoroughly, and then added with N-methylpyrrolidone (NMP) and stirred in a vacuum for 6 h to obtain an electrode slurry; the slurry was coated on a titanium mesh by a doctor blade method, and finally dried in a vacuum drying oven at 80°C for 12 h. The slurry coating area was 1680 cm 2 , coating density is 80mg / cm 2 , and obtain the electrochemical deintercalation method salt lake lithium extraction electrode.
[0053] Example 2
[0054] This embodiment provides an electrochemical deintercalation method for extracting lithium from salt lakes. The preparation method of the electrochemical deintercalation method for extracting lithium from salt lakes is as follows:
[0055] (1) Tetraethyl orthosilicate, silane coupling agent KH-560 and anhydrous ethanol were mixed and stirred in a mass ratio of 2.2:1:5.2 for 10 minutes to obtain a mixed solution A; 0.21% (volume fraction) dilute nitric acid was added dropwise into the mixed solution A and stirred for hydrolysis for 2 hours to obtain a sol (wherein the mass ratio of the mixed solution A to nitric acid was 3.5:1); after ultrasonic treatment for 2 hours, the sol was aged at room temperature for 3 to 4 weeks to obtain an epoxy-modified silica sol; finally, the sol was placed in a -4°C refrigerator for 12 hours, and then placed in a -40°C freeze dryer for 24 hours to obtain an epoxy-modified silica powder;
[0056] (2) Take the iron phosphate ion sieve, epoxy modified silica, and epoxy resin and fully ball mill them in a high-speed ball mill. After ball milling for 1 hour, send the materials into an air flow separation device to separate the iron phosphate ion sieve and the epoxy modified silica that is not embedded in the pores of the positive electrode material. Finally, place the iron phosphate ion sieve in a 100°C oven to dry to obtain a partially modified iron phosphate ion sieve, wherein the mass ratio of the epoxy modified silica to the positive electrode material is 0.6%; the speed of the ball mill is 100 rpm; the air flow velocity in the air flow separation device is 14 m / s; the mass ratio of the epoxy resin binder to the epoxy modified silica is 0.06%;
[0057] (3) Partially modified iron phosphate ion screen, PVDF, and acetylene black were weighed in a mass ratio of 7:1:2, mixed thoroughly, and then added with N-methylpyrrolidone (NMP) and stirred in a vacuum for 6 h to obtain an electrode slurry; the slurry was coated on a titanium mesh by a doctor blade method, and finally dried in a vacuum drying oven at 80°C for 12 h. The slurry coating area was 1680 cm 2 , coating density is 80mg / cm 2 , and obtain the electrochemical deintercalation method salt lake lithium extraction electrode.
[0058] Example 3
[0059] The only difference between this embodiment and embodiment 1 is that the speed of the ball mill is 50 rpm, the air flow speed of the air flow separation device is 15 m / s, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0060] Example 4
[0061] The only difference between this embodiment and embodiment 1 is that the speed of the ball mill is 200 rpm, the air flow speed of the air flow separation device is 10 m / s, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0062] Comparative Example 1
[0063] The only difference between this comparative example and Example 1 is that the ion sieve is not modified, and the other conditions and parameters are exactly the same as those in Example 1, namely:
[0064] Ferric phosphate ion sieve, PVDF and acetylene black were weighed in a mass ratio of 7:1:2, mixed thoroughly, added with N-methylpyrrolidone (NMP) and stirred in a vacuum for 6 h to obtain an electrode slurry; the slurry was coated on a titanium mesh by a doctor blade method and finally dried in a vacuum drying oven at 80°C for 12 h. The slurry coating area was 1680 cm 2 , coating density is 80mg / cm 2 , and obtain the electrochemical deintercalation method salt lake lithium extraction electrode.
[0065] Comparative Example 2
[0066] The difference between Comparative Example 2 and Comparative Example 1 is that in step (2), hydrophilic nano-silica accounting for 30% of the total mass is additionally added.
[0067] Performance testing:
[0068] The iron phosphate electrode prepared in Examples 1-6 and Comparative Examples 1-2 was placed as the cathode in a cathode chamber containing 15 g / L LiCl solution, and the lithium iron phosphate electrode was placed as the anode in an anode chamber containing 30 g / L NaCl solution. Lithium insertion / delithiation was performed using a constant current followed by a constant voltage process until the current was less than 2 A / m 2 , the test results are shown in Table 1:
[0069] Table 1
[0070] As can be seen from Table 1, according to Examples 1-2, the saturated adsorption capacity of the salt lake lithium extraction electrode prepared by the electrochemical deintercalation method described in the present application can reach more than 32.1 mg / g, and the time required for saturated adsorption can reach less than 14.9 h.
[0071] By comparing Example 1 and Examples 3-4, it can be seen that as the speed of the ball mill mixer becomes faster and faster, more epoxy-modified silica and epoxy resin adhesive are embedded in the pores of the ion sieve, and the hydrophilic and superoleophobic effects in the pores become better and better, allowing the solution to flow freely and unhindered in the electrode pores (the solution diffusion resistance is small), thereby improving the mass transfer effect of the solution and increasing the adsorption capacity of the electrode for lithium ions.
[0072] By comparing Example 1 and Comparative Example 1, it can be seen that the present application improves the hydrophilicity of the pores and thus improves the mass transfer of the solution in the pores by locally modifying the pores of the ion sieve to be superoleophobic and superhydrophilic, thereby significantly shortening the time required for saturated adsorption.
[0073] A comparison of Example 1 and Comparative Example 2 demonstrates that the epoxy-modified silica described herein exhibits excellent hydrophilic and oleophobic properties. The formation of a hydrophilic and oleophobic film within the pores of the ion sieve improves mass transfer within the solution. This preparation method successfully avoids the reduction in the proportion of electrode active material and lithium extraction per unit area caused by excessive addition of hydrophilic material.
Claims
1. A method for preparing a lithium-extraction electrode from a salt lake by an electrochemical deintercalation method, the method comprising the following steps: (1) mixing a silicon source, a silane coupling agent and a solvent to obtain a mixed solution, adding an acid solution to the mixed solution to obtain a sol, subjecting the mixed solution to ultrasonic treatment and aging to obtain an epoxy-modified silica sol, and subjecting the mixed solution to freeze-drying to obtain an epoxy-modified silica powder; (2) mixing the ion sieve, epoxy-modified silica powder and a binder, grinding and separating to obtain a partially modified ion sieve; (3) The locally modified ion sieve, a binder and a conductive agent are mixed with a solvent to obtain an electrode slurry, and the electrode slurry is coated on the surface of a titanium mesh to obtain the electrochemical deintercalation method salt lake lithium extraction electrode.
2. The preparation method according to claim 1, wherein The silicon source in step (1) includes tetraethyl orthosilicate.
3. The preparation method according to claim 1 or 2, wherein: The silane coupling agent includes KH-560.
4. The preparation method according to any one of claims 1 to 3, wherein The solvent includes anhydrous ethanol.
5. The preparation method according to any one of claims 1 to 4, wherein: The mass ratio of the silicon source, the silane coupling agent and the solvent is (1.5-2.5):1:(4-6).
6. The preparation method according to any one of claims 1 to 5, wherein: The acid solution in step (1) includes nitric acid.
7. The preparation method according to any one of claims 1 to 6, wherein: The mass ratio of the mixed solution to the acid solution is (3.2-3.5):
1.
8. The preparation method according to any one of claims 1 to 7, wherein: The ultrasonic treatment time in step (1) is 1.5 to 3 hours.
9. The preparation method according to any one of claims 1 to 8, wherein: The freeze-drying process includes first freezing at -4°C for 12 hours and then freezing at -40°C for 24 hours.
10. The preparation method according to any one of claims 1 to 9, wherein: The adhesive in step (2) includes epoxy resin.
11. The preparation method according to any one of claims 1 to 10, wherein: The ion sieve includes any one of an iron phosphate ion sieve and a lithium titanate ion sieve or a combination of the two.
12. The preparation method according to any one of claims 1 to 11, wherein: The mass ratio of the epoxy-modified silica powder to the ion sieve in step (2) is (0.2-1):
100.
13. The preparation method according to any one of claims 1 to 12, wherein: The mass ratio of the adhesive to the epoxy-modified silica powder is (0.02-0.1):
100.
14. The preparation method according to any one of claims 1 to 13, wherein: The grinding speed in step (2) is 100-200 rpm; Optionally, the separation comprises airflow separation; Optionally, the air flow velocity of the air flow separation is 10 to 15 m / s.
15. The preparation method according to any one of claims 1 to 14, wherein: The binder in step (3) comprises polyvinylidene fluoride; Optionally, the conductive agent includes acetylene black; Optionally, the solvent comprises N-methylpyrrolidone; Optionally, the mass ratio of the partially modified ion sieve, the binder and the conductive agent is (6-8):1:(1.5-2.5).
16. The preparation method according to any one of claims 1 to 15, wherein: The coating area in step (3) is 1500-1800cm 2 ; Optionally, the coating density is 70-90 mg / cm 2 .
17. An electrode for extracting lithium from salt lakes using an electrochemical deintercalation method, wherein the electrode is prepared by the method according to any one of claims 1 to 16.
Citation Information
Patent Citations
Organic-inorganic hybridization ultraviolet cured paint for protecting metallic surface
CN101307194A
Hydrophilic coating agent, hydrophilic coating film, and hydrophilic base
CN101809101A
Preparation method of hydrophilic lithium extraction electrode
CN113293289A
Manganese ion sieve electric control lithium extraction membrane electrode surface hydrophilic modification method
CN114864876A
High-selectivity and hydrophilic electrode for lithium extraction and preparation method therefor