Secondary battery functional material, preparation method therefor and use thereof
By evenly distributing active materials in the pores of the carrier material and catalyzing the reaction at a specific voltage, the problem of irreversible active ion consumption in secondary batteries is solved, and the energy density and service life of the battery are improved.
Patent Information
- Application Number
- PCT/CN2023/100109
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-06-14
- Publication Date
- 2024-10-03
AI Technical Summary
Existing lithium-ion batteries and sodium-ion batteries have irreversible active ion consumption during the first charge and discharge process, resulting in low Coulombic efficiency in the first week of the battery, affecting energy density and service life.
By mixing the precursor solution containing lithium or sodium active material with the carrier material, and through physical processes such as shaking and dispersion, the active material is evenly distributed in the pores and surface of the carrier material to form a composite material. The carrier material operates at 2.0V-4.8 The catalytic active material reacts under V voltage, reducing the reaction activation energy and increasing the reaction area.
It improves the replenishment capacity of active ions in the secondary battery during the charge and discharge cycle, prolongs the cycle life of the battery and increases the capacity.
Smart Images

Figure CN2023100109_03102024_PF_FP_ABST
Abstract
Description
A secondary battery functional material and its preparation method and application
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on March 27, 2023, with application number 202310300406.0 and invention name “A secondary battery functional material, its preparation method and application”. Technical Field
[0002] The present invention relates to the technical field of secondary battery materials, and in particular to a secondary battery functional material and a preparation method and application thereof. Background Art
[0003] In recent years, as people become more aware of the environmental impact of fossil fuels, the shift to electric energy in mobile devices, industrial tools, and electric vehicles has led to a rapid increase in demand for high-efficiency secondary batteries. The widespread use of these batteries requires them to possess high energy density, excellent safety performance, and a long service life.
[0004] Lithium-ion and sodium-ion batteries are two key battery types in energy storage and electronic product systems. Although some products have been commercialized, their energy density, service life, and safety still cannot fully meet people's usage needs. For example, current lithium-ion and sodium-ion batteries experience irreversible consumption of active ions during the initial charge and discharge process, resulting in low coulombic efficiency in the first cycle, which in turn affects the battery's energy density and service life.
[0005] In order to solve the above problems, a functional material with excellent performance is developed to replenish the consumed irreversible active ions, so as to solve the problem of irreversible consumption of active ions in the first charge and discharge process of secondary batteries, which leads to low coulombic efficiency in the first cycle of the battery, thereby affecting the energy density and service life of the battery.
[0006] Summary of the Invention
[0007] An embodiment of the present invention provides a secondary battery functional material, a preparation method and application thereof, wherein a solution of a precursor containing a lithium or sodium active material is mixed with a carrier material, and then the active material is uniformly distributed in the pores and on the surface of the carrier material in the form of small particles through a physical process (such as shaking, dispersing and stirring, etc.), thereby obtaining a secondary battery functional material; the secondary battery functional material is obtained by adsorbing the active material in the pores of the carrier material, thereby compounding the two materials, the active material and the carrier material, wherein the carrier material can catalyze the reaction of the active material under a voltage of 2.0V-4.8V, thereby reducing the reaction activation energy of the active material; at the same time, because the active material exists in the form of small particles, the reaction sites are increased, the reaction area is increased, and the overall reaction activity of the material is improved; the secondary battery functional material provided by the embodiment of the present invention is applied to a secondary battery, which can provide more active ions, replenish the irreversible active ions consumed by the secondary battery during the charge and discharge cycle, and enable the secondary battery to have the advantages of high capacity and long cycle life.
[0008] In a first aspect, an embodiment of the present invention provides a secondary battery functional material, the secondary battery functional material comprising: a carrier material and an active material;
[0009] The carrier material is a porous material that produces a catalytic effect on the active material at a voltage of 2.0V-4.8V; the carrier material includes: one or more of a porous metal material, a porous ceramic material, a porous carbon material, a porous plastic, and a molecular sieve;
[0010] The active material includes: a compound containing lithium or a compound containing sodium; the active material is uniformly distributed in the pores or on the surface of the carrier material in the form of fine particles;
[0011] The particle size Dv50 of the active material is between 0.1nm-10μm; the particle size Dv50 of the carrier material is between 1nm-100μm; the particle size Dv50 of the secondary battery functional material is between 1nm-120μm;
[0012] The lithium-containing compound includes one or more of lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium formate, lithium oxide, lithium peroxide, lithium sulfide, lithium fluoride, and lithium nitride;
[0013] The sodium-containing compound includes one or more of sodium carbonate, sodium hydroxide, sodium oxalate, sodium acetate, sodium formate, sodium oxide, sodium peroxide, sodium sulfide, and sodium fluoride;
[0014] The porous metal material includes: one or more of aluminum, copper, iron, silver, titanium, nickel, tungsten, cobalt, molybdenum, platinum, magnesium, lead, zinc or alloy materials of the above metals;
[0015] The porous ceramic material includes one or more of porous alumina, porous zirconia, porous magnesia, porous silicon carbide, porous silicon nitride, cordierite, high-siliceous silicate, aluminosilicate, and aluminum titanate;
[0016] The porous carbon material includes one or more of activated carbon, expanded graphite, activated carbon fiber, carbon nanotubes, and porous acetylene black;
[0017] The porous plastic includes one or more of porous polyethylene, porous polystyrene, porous polyvinyl chloride, porous polypropylene, porous polyurethane, and porous phenolic resin;
[0018] The molecular sieve comprises: one or more of cross-linked dextran, carbon molecular sieve or zeolite;
[0019] The secondary battery functional material is obtained by adsorbing a clear solution containing a precursor of the active material into the pores of the carrier material and performing a drying process; the drying process is performed at a temperature of 60° C. to 300° C.
[0020] Preferably, the pore size of the support material is between 0.1 nm and 20 μm;
[0021] The specific surface area of the carrier material is 5m 2 / g-3000m 2 / g between;
[0022] The mass ratio of the active material to the carrier material is 0.1:1-100:1.
[0023] In a second aspect, an embodiment of the present invention provides a method for preparing the secondary battery functional material according to the first aspect, the method comprising:
[0024] Dissolve a certain amount of active material precursor in a solvent and stir evenly to obtain a clear solution;
[0025] Adding a certain amount of carrier material to the clear solution and fully dispersing it evenly so that the clear solution is adsorbed into the pores of the carrier material to obtain a composite material solution;
[0026] The composite material solution is dried to remove the solvent, and the clear solution in the pores of the composite material is crystallized to form fine particles of active material, thereby finally obtaining a functional material for a secondary battery;
[0027] Wherein, the carrier material includes: one or more of porous metal materials, porous ceramic materials, porous carbon materials, porous plastics, and molecular sieves;
[0028] The active material includes: a compound containing lithium element or a compound containing sodium element;.
[0029] Preferably, the lithium-containing compound includes one or more of lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium formate, lithium oxide, lithium peroxide, lithium sulfide, lithium fluoride, and lithium nitride;
[0030] The sodium-containing compound includes one or more of sodium carbonate, sodium hydroxide, sodium oxalate, sodium acetate, sodium formate, sodium oxide, sodium peroxide, sodium sulfide, and sodium fluoride;
[0031] The solvent includes one or more of deionized water, ethanol, ether, acetone, N-methylpyrrolidone NMP, N,N-dimethylformamide DMF, ethyl acetate, benzene, and chloroform;
[0032] The mass ratio of the solvent to the active material is 5:1-200:1.
[0033] Preferably, the porous metal material comprises: one or more of the elements of aluminum, copper, iron, silver, titanium, nickel, tungsten, cobalt, molybdenum, platinum, magnesium, lead, and zinc, or alloys of the aforementioned metals;
[0034] The porous ceramic material includes one or more of porous alumina, porous zirconia, porous magnesia, porous silicon carbide, porous silicon nitride, cordierite, high-siliceous silicate, aluminosilicate, and aluminum titanate;
[0035] The porous carbon material includes one or more of activated carbon, expanded graphite, activated carbon fiber, carbon nanotubes, and porous acetylene black;
[0036] The porous plastic includes one or more of porous polyethylene, porous polystyrene, porous polyvinyl chloride, porous polypropylene, porous polyurethane, and porous phenolic resin;
[0037] The molecular sieve comprises one or more of cross-linked dextran, carbon molecular sieve or zeolite.
[0038] Preferably, the method of fully dispersing includes: a combination of one or more of shaking dispersion, stirring dispersion, ultrasonic dispersion, and ball milling dispersion;
[0039] The fully dispersed equipment includes: a combination of one or more equipment selected from the group consisting of a shaker, a blender, an ultrasonic disperser, and a ball mill;
[0040] The sufficient dispersion time is between 0.5 hours and 72 hours.
[0041] Preferably, the drying method includes: a combination of one or more methods selected from the group consisting of rotary evaporation drying, stirring and heating drying, spray drying, vacuum heating drying, and filtration followed by air drying.
[0042] The drying process is carried out at a temperature of 60° C. to 300° C. and for a time of 0.5 hours to 48 hours.
[0043] In a third aspect, an embodiment of the present invention provides a positive electrode plate, wherein the positive electrode plate includes the secondary battery functional material described in the first aspect.
[0044] In a fourth aspect, an embodiment of the present invention provides a secondary battery, comprising the positive electrode sheet described in the third aspect.
[0045] An embodiment of the present invention provides a secondary battery functional material, a preparation method and application thereof, wherein a solution of a precursor containing a lithium or sodium active material is mixed with a carrier material, and then the active material is uniformly distributed in the pores and on the surface of the carrier material in the form of small particles through a physical process (such as shaking, dispersing and stirring, etc.), thereby obtaining a secondary battery functional material; the secondary battery functional material is obtained by adsorbing the active material in the pores of the carrier material, thereby compounding the two materials, the active material and the carrier material, wherein the carrier material can catalyze the reaction of the active material under voltage, thereby reducing the reaction activation energy of the active material, and at the same time, because the active material exists in the form of small particles, the reaction sites are increased, the reaction area is increased, and the overall reaction activity of the material is improved; the secondary battery functional material provided by the embodiment of the present invention is applied to a secondary battery, which can provide more active ions, replenish the irreversible active ions consumed by the secondary battery during the charge and discharge cycle, and make the secondary battery have the advantages of high capacity and long cycle life.
[0046] The method for preparing a secondary battery functional material provided by the embodiment of the present invention is simple to operate, low in cost, and applicable to large-scale batch production. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] The technical solutions of the embodiments of the present invention are further described in detail below through the accompanying drawings and examples.
[0048] FIG1 is a flow chart of a method for preparing a secondary battery functional material provided by an embodiment of the present invention.
[0049] FIG2 is a scanning electron microscope (SEM) image of the secondary battery functional material provided in Example 1 of the present invention.
[0050] FIG3 is a charge-discharge curve diagram of the first cycle of the secondary battery functional material provided in Example 1 of the present invention.
[0051] FIG4 is an X-ray diffraction (XRD) pattern of the secondary battery functional material and active material lithium oxalate provided in Example 2 of the present invention.
[0052] FIG5 is a charge-discharge curve diagram of the first cycle of the secondary battery functional material provided by Example 2 of the present invention.
[0053] FIG6 is a comparison diagram of the first-week charge and discharge curves of the CR2032 button batteries assembled in Example 3 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0054] The present invention will be further described in detail below through the accompanying drawings and specific examples, but it should be understood that these examples are only used for more detailed explanation and should not be understood as limiting the present invention in any form, that is, they are not intended to limit the scope of protection of the present invention.
[0055] An embodiment of the present invention provides a secondary battery functional material, including: a carrier material and an active material; the mass ratio of the active material to the carrier material is [0.1:1]-[100:1]; the active material is uniformly distributed in the pores or on the surface of the carrier material in the form of fine particles.
[0056] The carrier material is a porous material that catalyzes the active material at a voltage of 2.0V-4.8V. Specifically, the carrier material has strong ion adsorption, which can reduce the activation energy of the reaction and accelerate the release of active ions, thereby achieving catalysis. The particle size Dv50 of the carrier material is between 1nm-100μm; the particle size Dv50 of the secondary battery functional material is between 1nm-120μm; the pore size of the carrier material is between 0.1nm-20μm; the specific surface area of the carrier material is between 5m 2 / g-3000m 2 / g.
[0057] The carrier material includes: one or more of porous metal materials, porous ceramic materials, porous carbon materials, porous plastics, and molecular sieves; the porous metal material includes: one or more of single substances or alloy materials of aluminum, copper, iron, silver, titanium, nickel, tungsten, cobalt, molybdenum, platinum, magnesium, lead, and zinc; the porous ceramic material includes: one or more of porous alumina, porous zirconia, porous magnesium oxide, porous silicon carbide, porous silicon nitride, cordierite, high-siliceous silicate, aluminosilicate, and aluminum titanate; the porous carbon material includes: one or more of activated carbon, expanded graphite, activated carbon fiber, carbon nanotubes, and porous acetylene black; the porous plastic includes: one or more of porous polyethylene, porous polystyrene, porous polyvinyl chloride, porous polypropylene, porous polyurethane, and porous phenolic resin; the molecular sieve includes: one or more of cross-linked dextran, carbon molecular sieve, or zeolite.
[0058] The active material includes: a lithium-containing compound or a sodium-containing inorganic compound; the lithium-containing inorganic compound includes: one or more of lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium formate, lithium oxide, lithium peroxide, lithium sulfide, lithium fluoride, and lithium nitride; the sodium-containing compound includes: one or more of sodium carbonate, sodium hydroxide, sodium oxalate, sodium acetate, sodium formate, sodium oxide, sodium peroxide, sodium sulfide, and sodium fluoride; the particle size Dv50 of the active material is between 0.1 nm and 10 μm.
[0059] An embodiment of the present invention provides a method for preparing the above-mentioned secondary battery functional material, as shown in FIG1 , which specifically includes the following steps.
[0060] Step 110 : dissolving a certain amount of active material precursor into a solvent and stirring the mixture to obtain a clear solution.
[0061] Among them, the precursor of the active material includes: a raw material of a lithium-containing compound or a raw material of a sodium-containing compound; the lithium-containing compound includes: one or more of lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium formate, lithium oxide, lithium peroxide, lithium sulfide, lithium fluoride, and lithium nitride; the sodium-containing compound includes: one or more of sodium carbonate, sodium hydroxide, sodium oxalate, sodium acetate, sodium formate, sodium oxide, sodium peroxide, sodium sulfide, and sodium fluoride.
[0062] The solvent includes one or more of deionized water, ethanol, ether, acetone, N-methylpyrrolidone NMP, N,N-dimethylformamide DMF, ethyl acetate, benzene, and chloroform.
[0063] The mass ratio of solvent to active material is [5:1]-[200:1].
[0064] The stirring method in this step is a conventional method to uniformly mix the active material and the solvent. The stirring equipment includes but is not limited to any one of a blender, an ultrasonic disperser, and a high-pressure mixer.
[0065] Step 120 , adding a certain amount of carrier material to the clarified solution and fully and evenly dispersing the clarified solution so that the clarified solution is adsorbed into the pores of the carrier material to obtain a composite material solution.
[0066] The carrier material includes one or more of porous metal materials, porous ceramic materials, porous carbon materials, porous plastics, and molecular sieves. Since the carrier material has a porous structure, it has a stronger adsorption capacity for the solute in the clarified solution when adsorbing the clarified solution.
[0067] The porous metal material includes one or more of the simple substances or alloy materials of aluminum, copper, iron, silver, titanium, nickel, tungsten, cobalt, molybdenum, platinum, magnesium, lead, and zinc.
[0068] The porous ceramic material includes one or more of porous alumina, porous zirconia, porous magnesia, porous silicon carbide, porous silicon nitride, cordierite, high-siliceous silicate, aluminosilicate, and aluminum titanate.
[0069] The porous carbon material includes one or more of activated carbon, expanded graphite, activated carbon fiber, carbon nanotube, and porous acetylene black.
[0070] The porous plastic includes one or more of porous polyethylene, porous polystyrene, porous polyvinyl chloride, porous polypropylene, porous polyurethane, and porous phenolic resin.
[0071] The molecular sieve includes one or more of cross-linked dextran, carbon molecular sieve or zeolite.
[0072] The method of sufficient dispersion includes: a combination of one or more of oscillation dispersion, stirring dispersion, ultrasonic dispersion, and ball milling dispersion; the equipment for sufficient dispersion includes: a combination of one or more of an oscillating shaker, a stirrer, an ultrasonic disperser, or a ball mill; and the time for sufficient dispersion is between 0.5 hours and 72 hours.
[0073] Step 130 , drying the composite material solution to remove the solvent, and allowing the clarified solution in the pores of the composite material to crystallize into fine particles of active material, ultimately obtaining a functional material for a secondary battery.
[0074] The drying method includes: a combination of one or more methods of rotary evaporation drying, stirring and heating drying, spray drying, vacuum heating drying, and filtration followed by air drying; the drying temperature is 60°C-300°C, and the drying time is 0.5 hours-48 hours.
[0075] In the secondary battery functional material prepared in the embodiment of the present invention, the active material is mainly evenly distributed in the pores of the carrier material in the form of fine particles, and is partially distributed on the surface of the carrier material without forming a coating structure.
[0076] The secondary battery functional material prepared by the above-mentioned preparation method in the embodiment of the present invention can be used as an additive for positive electrode active materials in the preparation of positive electrode sheets.
[0077] Among them, the above-mentioned positive electrode sheet mainly includes a positive electrode current collector, a positive electrode active material, a secondary battery functional material, a conductive agent and a binder.
[0078] The positive electrode current collector includes but is not limited to aluminum foil.
[0079] The positive electrode active material includes any one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, nickel cobalt lithium manganese oxide ternary material, sodium cobalt oxide, vanadium pentoxide, Prussian blue, olivine structure sodium iron phosphate, NASICON structure Na3V2(PO4)3, and layered structure sodium nickel iron manganese oxide.
[0080] The conductive agent includes, but is not limited to, one or more of carbon black, carbon nanotubes, acetylene black, and Ketjen black.
[0081] The binder includes, but is not limited to, one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, carboxymethyl cellulose, sodium carboxymethyl cellulose, polymethyl methacrylate, polyacrylate, polyacrylonitrile, styrene-butadiene rubber, polyvinyl alcohol, polytetrafluoroethylene, polyacrylamide, polyvinyl acetate, and polyurethane.
[0082] An embodiment of the present invention provides a secondary battery, which includes a lithium-ion battery or a sodium-ion battery.
[0083] Specifically, the secondary battery is composed of the above-mentioned positive electrode plate containing the secondary battery functional material, a separator, an electrolyte or a solid electrolyte, and a negative electrode plate.
[0084] Among them, the diaphragm includes but is not limited to any one of a double-sided alumina diaphragm, a diaphragm containing a sodium ion solid electrolyte, and a diaphragm containing a lithium ion solid electrolyte; the base film of the diaphragm includes: any one of a polyolefin film, a non-woven fabric diaphragm, a fiber diaphragm, and a polyaramid diaphragm.
[0085] The negative electrode plate includes any one of a lithium sheet, a sodium sheet or a negative electrode current collector containing a negative electrode active material; specifically, the negative electrode current collector includes but is not limited to copper foil or titanium foil, and the active material layer on the surface of the negative electrode current collector also contains a conductive agent and a binder; the negative electrode active material includes but is not limited to any one of a carbon material, a tin-based negative electrode material, a silicon-based negative electrode material, a silicon-carbon composite material, a nano-oxide material, and a titanate negative electrode material; the carbon material includes any one of graphite, hard carbon, carbon fiber, petroleum coke, and mesophase carbon microbeads.
[0086] The electrolyte consists of a solute and a solvent.
[0087] The solute is a conductive salt, including any one of sodium perchlorate (NaClO4), sodium tetrafluoroborate (NaBF4), sodium hexafluorophosphate (NaPF6), sodium hexafluoroarsenate (NaAsF6), sodium trifluoroacetate (CF3COONa), lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium hexafluoroborate (LiBF6), and lithium hexafluoroarsenate (LiAsF6).
[0088] The solvent includes: ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), γ-butyrolactone (BL), methyl propionate (MP), methyl butyrate (MB), ethyl acetate (EA), ethyl propionate (EP), propyl propionate (PP), ethyl butyrate (EB), 1,3-dioxolane (DOL), ethylene glycol dimethyl ether (DME), diethylene glycol dimethyl ether (DEGDME), triethylene glycol dimethyl ether (TRGDME), tetraethylene glycol dimethyl ether (TEGDME), ethyl methanesulfonate (EMS) or dimethyl sulfoxide (DMSO).
[0089] In order to better understand the technical solution provided by the present invention, the preparation process and characteristics of the secondary battery functional material of the present invention are respectively described below with multiple specific examples.
[0090] Example 1
[0091] This embodiment provides a preparation process and performance test of a secondary battery functional material. The specific preparation steps are as follows.
[0092] In step 110 , 120 g of deionized water is weighed and placed in a beaker, 8 g of sodium fluoride with a particle size Dv50 of 1 μm is dissolved in the 120 g of deionized water, and the mixture is stirred evenly using a magnetic stirrer to obtain a clear solution.
[0093] Step 120, 8 grams of particles with a Dv50 of 20 μm and a specific surface area of 850 m 2 / g of porous zirconium oxide was added to the above clarified solution, and then placed in an oscillating shaker at a frequency of 80 Hz for 48 hours to allow the active material to be adsorbed into the pores of the carrier material to obtain a composite material solution.
[0094] Step 130: Place the composite material solution in a rotary evaporation device, perform rotary evaporation drying to concentrate the solution into a thick liquid, and then transfer it to a blast drying oven and dry it at 120° C. for 1 hour. After taking it out, grind and sieve it to obtain a functional material for a secondary battery in which sodium fluoride is adsorbed in the pores and on the surface of porous zirconia, wherein the particle size Dv50 of the functional material for a secondary battery is 20.2 μm.
[0095] FIG2 is a SEM image of the functional material for a secondary battery prepared in Example 1 of the present invention. As can be seen from FIG2 , the functional material for a secondary battery is irregular in shape as a whole, and slightly larger pores can be observed on the surface of the material.
[0096] The secondary battery functional material prepared in this embodiment was used as a positive electrode active material to prepare a positive electrode sheet, and a sodium ion battery was assembled, and then the electrochemical performance of the sodium ion battery was tested, specifically:
[0097] Preparation of sodium ion battery: The secondary battery functional material prepared in this example is mixed with polyvinylidene fluoride (PVDF) and conductive carbon black (SP) in a mass ratio of 8:1:1 to form a slurry, which is then coated on aluminum foil to prepare a positive electrode sheet. It is then assembled with a sodium sheet, a double-sided alumina separator and an electrolyte according to a conventional method to form a CR2032 button battery, wherein the electrolyte is a 1 mol / L sodium hexafluorophosphate NaPF6 solution of ethylene carbonate (EC) / dimethyl carbonate (DEC) (volume ratio 1:1).
[0098] Test method: The test was performed according to the procedure of charging to 4.0V at a rate of 0.1C, then charging to 0.02C at a constant voltage of 4.0V, and then discharging to 2V at a rate of 0.1C. The charge and discharge test curve of the first week is shown in Figure 3. It can be seen from the figure that the battery's first-week charging capacity is 296.9mAh / g, and the discharge capacity is 58.3mAh / g, indicating that the battery prepared in this embodiment only uses secondary battery functional materials as the positive electrode active material. It can release more active sodium ions during the first week of charging, further illustrating that the secondary battery functional materials provided in the embodiment of the present invention can be used as functional materials for supplementing active sodium ions in sodium ion batteries.
[0099] Control group experiment of Example 1
[0100] In this comparative example, sodium fluoride, the active material of Example 1, was used as the positive electrode active material to prepare a positive electrode sheet, and a sodium ion battery was assembled. The sodium ion battery was then subjected to an electrochemical performance test. The battery assembly and testing methods were the same as those in Example 1. The first-week charge capacity of the test battery was 0.42 mAh / g, and the discharge capacity was 0.39 mAh / g, which were much smaller than the test values of the first-week charge and discharge capacity of Example 1. This further illustrates that the secondary battery functional material prepared in Example 1 of the present invention can release more active sodium ions during the first-week charging process.
[0101] Example 2
[0102] This embodiment provides a preparation process and performance test of a secondary battery functional material. The specific preparation steps are as follows.
[0103] Step 110: dissolve 12 g of lithium oxalate with a particle size Dv50 of 6 μm in 200 g of deionized water, place the solution in a disperser, and stir the solution at 500 rpm for 30 minutes to obtain a clear solution.
[0104] Step 120, 8 grams of particles with a Dv50 of 2 μm and a specific surface area of 920 m2 / g of porous polyurethane was added to the above clarified solution, and then continued to disperse and stir in a disperser for 40 hours to allow the active material to be adsorbed into the pores of the carrier material to obtain a composite material solution.
[0105] Step 130: Transfer the composite material solution to a heating mixer, heat and stir to concentrate the solution into a thick liquid, then transfer it to a blast drying oven and dry it at 110°C for 2 hours. After taking it out, grind and sieve it to obtain a functional material for a secondary battery with lithium oxalate adsorbed in the pores and on the surface of the porous polyurethane, wherein the particle size Dv50 of the functional material for a secondary battery is 2 μm.
[0106] FIG4 shows an XRD pattern of the functional material for a secondary battery prepared in Example 2 of the present invention. FIG4 shows that the characteristic peaks of the functional material for a secondary battery are consistent with the characteristic peaks of the active material lithium oxalate, indicating that the crystal structure of the active material lithium oxalate does not change after the active material lithium oxalate is loaded into the porous polyurethane carrier material.
[0107] The secondary battery functional material prepared in this embodiment was used to prepare positive electrode sheets to assemble lithium-ion batteries, and electrochemical performance tests were conducted, specifically:
[0108] Preparation of lithium-ion battery: The secondary battery functional material prepared in this example is mixed with polyvinylidene fluoride (PVDF) and conductive carbon black (SP) in a mass ratio of 8:1:1 to form a slurry, which is then coated on aluminum foil to prepare a positive electrode sheet. Then, it is assembled with a lithium sheet, a double-sided alumina separator and an electrolyte according to a conventional method to form a CR2032 button battery, wherein the electrolyte is a 1 mol / L LiPF6 ethylene carbonate EC / dimethyl carbonate DEC (the volume ratio of EC to DEC is 1:1) solution.
[0109] Test method: The test was carried out according to the procedure of charging to 4.4V at a rate of 0.1C, then charging to 0.02C at a constant voltage of 4.4V, and then discharging to 3V at a rate of 0.1C. The charge and discharge test curve of the first week is shown in Figure 5. It can be seen that the first-week charging capacity of the material is 461.7mAh / g, and the discharge capacity is 32.6mAh / g, indicating that the lithium-ion battery prepared in this embodiment only uses secondary battery functional materials as the positive electrode active material. It can release more active lithium ions during the first week of charging, further illustrating that the secondary battery functional materials provided in the embodiment of the present invention can be used as functional materials for supplementing active lithium ions in lithium-ion batteries.
[0110] Control group experiment of Example 2
[0111] In this comparative example, the active material lithium oxalate of Example 2 was used as the positive electrode active material to prepare a positive electrode sheet, and a lithium-ion battery was assembled. The lithium-ion battery was then subjected to an electrochemical performance test. The battery assembly and testing methods were the same as those in Example 2. The first-week charge capacity of the test battery was 36.8 mAh / g, and the discharge capacity was 1.2 mAh / g, which were much smaller than the test values of the first-week charge and discharge capacity of Example 2. This further illustrates that the secondary battery functional material prepared in Example 2 of the present invention can release more active lithium ions during the first-week charging process.
[0112] Example 3
[0113] This embodiment provides a preparation process and performance test of a secondary battery functional material. The specific preparation steps are as follows.
[0114] In step 110, 1.8 kg of lithium carbonate with a particle size Dv50 of 500 nm and 20 kg of deionized water are placed in a stirring tank and stirred for 2 hours until the lithium carbonate is completely dissolved to obtain a clear solution.
[0115] Step 120: 1.2 kg of particles with a Dv50 of 5 μm and a specific surface area of 880 m 2 / g of cross-linked dextran was added to the above clear solution, and the solution was stirred in a stirring tank for 24 hours to allow the active material lithium carbonate to be adsorbed into the pores of the carrier material cross-linked dextran to obtain a composite material solution.
[0116] Step 130: Place the composite material solution in a spray dryer with an inlet temperature of 250°C and an outlet temperature of 120°C, and spray granulate to obtain a functional material for a secondary battery in which lithium carbonate is adsorbed in the pores and on the surface of the cross-linked dextran, wherein the particle size Dv50 of the functional material for a secondary battery is 5 μm.
[0117] The secondary battery functional material prepared in this embodiment was used to prepare positive electrode sheets to assemble lithium-ion batteries, and electrochemical performance tests were conducted, specifically:
[0118] Preparation of lithium-ion battery: The secondary battery functional material prepared in this embodiment is mixed with polyvinylidene fluoride (PVDF), conductive carbon black (SP) and ternary positive electrode material NCM811 in a mass ratio of 5:2:2:91 to form a slurry, which is then coated on aluminum foil to prepare a positive electrode sheet. It is then assembled with a lithium sheet, a double-sided alumina separator and an electrolyte according to a conventional method to form a CR2032 button battery, wherein the electrolyte is a 1 mol / L LiPF6 ethylene carbonate EC / dimethyl carbonate DEC (the volume ratio of EC to DEC is 1:1) solution.
[0119] Test method: The test was carried out according to the procedure of charging to 4.4V at a rate of 0.1C, then charging to 0.02C at a constant voltage of 4.4V, and then discharging to 3V at a rate of 0.1C. The charge and discharge test curve of the first week is shown in Figure 6. It can be seen from the figure that the material's first-week charge capacity is 239.5mAh / g, the discharge capacity is 210.4mAh / g, and the coulombic efficiency of the first week is 87.8%.
[0120] In order to better illustrate the effects of the embodiments of the present invention, comparative example 1 is compared with embodiment 3.
[0121] Comparative Example 1
[0122] This comparative example differs from Example 3 in that functional materials for secondary batteries are not used to prepare the positive electrode sheets. The other battery assembly methods are the same: PVDF, SP and the ternary positive electrode material NCM811 are taken and uniformly formed into a slurry in a mass ratio of 2:2:96, and then coated and prepared into positive electrode sheets. The CR2032 button batteries are assembled in the manner of Example 3 and tested according to the procedures of Example 3.
[0123] The charge and discharge curves of the battery assembled in this comparative example in the first week of testing are shown in FIG6 . As can be seen from the figure, the first week charge capacity of the material is 225.2 mAh / g, the discharge capacity is 209.8 mAh / g, and the first week coulombic efficiency is 93.2%.
[0124] The first-week charging capacity of the battery in Example 3 is greater than that of the material in Comparative Example 1, indicating that the material can release more active lithium ions during the first-week charging process. Although the first-week coulombic efficiency of Example 3 appears to be lower than that of Comparative Example 1, in the half-cell test, with the same lithium insertion capacity, the battery in Example 3 using secondary battery functional materials has a larger lithium removal capacity, so the first-week efficiency appears to be lower, indicating that the secondary battery functional material has played a role. The difference in the charging capacity between the two is 14.3 mAh / g, which is equivalent to 511.2 mAh / g for the secondary battery functional material, indicating that the secondary battery functional material in Example 3 has a higher supplementary specific capacity.
[0125] Example 4
[0126] This embodiment provides a preparation process and performance test of a secondary battery functional material. The specific preparation steps are as follows:
[0127] Step 110: dissolve 5 g of sodium acetate with a particle size Dv50 of 1 μm in 180 g of ethanol, place the mixture in a disperser and stir for 20 min until uniform, to obtain a clear solution.
[0128] Step 120, 15 g of particles with a Dv50 of 20 μm and a specific surface area of 80 m 2 / g of cordierite was added to the above clarified solution, and then placed in a ball mill for dispersion for 16 hours, so that the active material sodium acetate was adsorbed into the pores of the carrier material cordierite to obtain a composite material solution.
[0129] Step 130: Transfer the composite material solution to a heating mixer, heat and stir to concentrate the solution into a thick liquid, then transfer it to a blast drying oven and dry it at 90°C for 1 hour. After taking it out, grind and sieve it to obtain a functional material for a secondary battery in which sodium acetate is adsorbed in the pores and on the surface of cordierite, wherein the particle size Dv50 of the functional material for a secondary battery is 6 μm.
[0130] The secondary battery functional material prepared in this embodiment was used to prepare a positive electrode sheet to assemble a sodium ion battery, and the electrochemical performance test was carried out. The preparation process and testing method of the sodium ion battery were the same as those in Example 1. The first-week charging capacity of the sodium ion battery was 353.3 mAh / g, indicating that the sodium removal capacity was large.
[0131] In order to better illustrate the effects of the embodiments of the present invention, Comparative Example 2 is compared with Example 4.
[0132] Comparative Example 2
[0133] The difference between this comparative example and Example 4 is that functional materials for secondary batteries are not used to prepare the positive electrode plates. The other battery assembly methods are the same: sodium acetate powder material is taken, PVDF and SP are uniformly mixed in a ratio of 8:1:1 to form a slurry, and then coated and prepared into plates. The plates are assembled into batteries in the same manner as in Example 4, and tested according to the procedures of Example 4. The test results show that the first-week charging capacity of the material is only 0.92 mAh / g. This is because no functional materials for secondary batteries are used in Comparative Example 2, and no catalytic effect is produced on sodium acetate. Therefore, sodium acetate is not decomposed and its capacity cannot be exerted.
[0134] By comparing the first-week charging capacity results of Example 4 and Comparative Example 2, it can be found that the functional material of Example 4 has a larger sodium removal capacity, and when loaded onto the porous ceramic material cordierite, it has a good catalytic decomposition effect on the decomposition of the active ingredients.
[0135] Example 5
[0136] This embodiment provides a preparation process and performance test of a secondary battery functional material. The specific preparation steps are as follows:
[0137] Step 110: Weigh 250 g of benzene and place it in a conical flask. Then add 10 g of lithium nitride with a particle size Dv50 of 3 μm. Place the flask in an ultrasonic disperser and perform ultrasonic dispersion for 1 hour to completely dissolve the lithium nitride in the benzene to obtain a clear solution.
[0138] Step 120, 15 g of particles with a Dv50 of 720 nm and a specific surface area of 670 m 2 / g of porous titanium was added to the above clarified solution, and then dispersed in an ultrasonic disperser for 24 hours to allow the active material lithium nitride to be adsorbed into the pores of the carrier material porous titanium to obtain a composite material solution.
[0139] Step 130: Transfer the composite material solution to a rotary evaporator, dry it by vacuum rotary evaporation, take it out, grind it, and sieve it to obtain a functional material for a secondary battery in which lithium nitride is adsorbed in the pores and on the surface of porous titanium, wherein the particle size Dv50 of the functional material for a secondary battery is 746 nm.
[0140] An embodiment of the present invention provides a secondary battery functional material, a preparation method and application thereof, wherein a solution of a precursor containing a lithium or sodium active material is mixed with a carrier material, and then the active material is uniformly distributed in the pores and on the surface of the carrier material in the form of small particles through a physical process (such as shaking, dispersing and stirring, etc.), thereby obtaining a secondary battery functional material; the secondary battery functional material is obtained by adsorbing the active material in the pores of the carrier material so as to composite the two materials, the active material and the carrier material, wherein the carrier material can catalyze the reaction of the active material under voltage, thereby reducing the reaction activation energy of the active material; at the same time, because the active material exists in the form of small particles, the reaction sites are increased, the reaction area is increased, and the overall reaction activity of the material is improved; the secondary battery functional material provided by the embodiment of the present invention is applied to a secondary battery, which can provide more active ions, replenish the irreversible active ions consumed by the secondary battery during the charge and discharge cycle, and enable the secondary battery to have the advantages of high capacity and long cycle life.
[0141] The method for preparing a secondary battery functional material provided by the embodiment of the present invention is simple to operate, low in cost, and applicable to large-scale batch production.
[0142] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A secondary battery functional material, characterized in that: The secondary battery functional material includes: a carrier material and an active material; The carrier material is a porous material that produces a catalytic effect on the active material at a voltage of 2.0V-4.8V; the carrier material includes: one or more of a porous metal material, a porous ceramic material, a porous carbon material, a porous plastic, and a molecular sieve; The active material comprises: a compound containing lithium or a compound containing sodium; the active material is uniformly distributed in the pores or on the surface of the carrier material in the form of fine particles; The particle size Dv50 of the active material is between 0.1nm-10μm; the particle size Dv50 of the carrier material is between 1nm-100μm; the particle size Dv50 of the secondary battery functional material is between 1nm-120μm; The lithium-containing compound includes one or more of lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium formate, lithium oxide, lithium peroxide, lithium sulfide, lithium fluoride, and lithium nitride; The compound containing sodium element includes: one or more of sodium carbonate, sodium hydroxide, sodium oxalate, sodium acetate, sodium formate, sodium oxide, sodium peroxide, sodium sulfide, and sodium fluoride; The porous metal material includes: one or more of the single substances of aluminum, copper, iron, silver, titanium, nickel, tungsten, cobalt, molybdenum, platinum, magnesium, lead, zinc or alloy materials of the aforementioned metals; The porous ceramic material includes: one or more of porous alumina, porous zirconia, porous magnesia, porous silicon carbide, porous silicon nitride, cordierite, high-siliceous silicate, aluminosilicate, and aluminum titanate; The porous carbon material includes: one or more of activated carbon, expanded graphite, activated carbon fiber, carbon nanotubes, and porous acetylene black; The porous plastic includes: one or more of porous polyethylene, porous polystyrene, porous polyvinyl chloride, porous polypropylene, porous polyurethane, and porous phenolic resin; The molecular sieve comprises: one or more of cross-linked dextran, carbon molecular sieve or zeolite; The secondary battery functional material is obtained by adsorbing a clear solution containing a precursor of the active material into the pores of the carrier material and drying the solution; the drying temperature is 60° C.-300° C.
2. The secondary battery functional material according to claim 1, characterized in that: The pore size of the carrier material is between 0.1 nm and 20 μm; The specific surface area of the carrier material is 5m 2 / g-3000m 2 / g between; The mass ratio of the active material to the carrier material is 0.1:1-100:
1.
3. A method for preparing a secondary battery functional material according to any one of claims 1-2, characterized in that: The preparation method comprises: Dissolving a certain amount of the precursor of the active material into the solvent and stirring evenly to obtain a clear solution; Adding a certain amount of carrier material to the clear solution and dispersing it evenly, so that the clear solution is adsorbed into the pores of the carrier material to obtain a composite material solution; The composite material solution is dried to remove the solvent, and the clear solution in the pores of the composite material is crystallized to form fine particle-shaped active materials, and finally a functional material for a secondary battery is obtained; Wherein, the carrier material includes: one or more of porous metal materials, porous ceramic materials, porous carbon materials, porous plastics, and molecular sieves; The precursor of the active material includes: a compound raw material containing lithium element or a compound raw material containing sodium element.
4. The preparation method according to claim 3, characterized in that: The compound raw material containing lithium element includes: one or more of lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium formate, lithium oxide, lithium peroxide, lithium sulfide, lithium fluoride, and lithium nitride; The compound raw material containing sodium element includes: one or more of sodium carbonate, sodium hydroxide, sodium oxalate, sodium acetate, sodium formate, sodium oxide, sodium peroxide, sodium sulfide, and sodium fluoride; The solvent includes: one or more of deionized water, ethanol, ether, acetone, N-methylpyrrolidone NMP, N,N-dimethylformamide DMF, ethyl acetate, benzene, and chloroform; The mass ratio of the solvent to the active material is 5:1-200:
1.
5. The preparation method according to claim 3, characterized in that: The porous metal material includes: one or more of the single substances of aluminum, copper, iron, silver, titanium, nickel, tungsten, cobalt, molybdenum, platinum, magnesium, lead, zinc or alloy materials of the aforementioned metals; The porous ceramic material includes: one or more of porous alumina, porous zirconia, porous magnesia, porous silicon carbide, porous silicon nitride, cordierite, high-siliceous silicate, aluminosilicate, and aluminum titanate; The porous carbon material includes: one or more of activated carbon, expanded graphite, activated carbon fiber, carbon nanotubes, and porous acetylene black; The porous plastic includes: one or more of porous polyethylene, porous polystyrene, porous polyvinyl chloride, porous polypropylene, porous polyurethane, and porous phenolic resin; The molecular sieve comprises: one or more of cross-linked dextran, carbon molecular sieve or zeolite.
6. The preparation method according to claim 3, characterized in that: The method of fully dispersing includes: a combination of one or more of shaking dispersion, stirring dispersion, ultrasonic dispersion, and ball milling dispersion; The fully dispersed equipment includes: a combination of one or more equipments such as a shaking table, a stirrer, an ultrasonic disperser or a ball mill; The sufficient dispersion time is between 0.5 hours and 72 hours.
7. The preparation method according to claim 3, characterized in that: The drying method includes: a combination of one or more of rotary evaporation drying, stirring and heating drying, spray drying, vacuum heating drying, and blast drying after filtration; The drying process is carried out at a temperature of 60° C. to 300° C. and for a time of 0.5 hour to 48 hours.
8. A positive electrode sheet, characterized in that: The positive electrode plate comprises the secondary battery functional material described in any one of claims 1-2.
9. A secondary battery, characterized in that: The secondary battery comprises the positive electrode sheet as claimed in claim 8.
Citation Information
Patent Citations
Lithium sulfide-porpous carbon compound positive material for lithium ion battery and preparation method thereof
CN102163720A
Composite material for positive electrode of lithium-sulfur battery and preparation method and application of composite material
CN106920930A
Metal monoatom-doped carbon nanomaterial catalytic carrier, and preparation method and application thereof
CN109248712A
High-safety and high-energy quasi-solid-state lithium secondary battery based on lithium sulfide positive electrode and preparation method thereof
CN112271274A
Alkali metal fluoride / carbon composite material and preparation and application thereof