Lithium iron phosphate conductive agent, lithium iron phosphate positive electrode sheet using same, and battery
By using nitrogen-doped carbon nanotubes in lithium iron phosphate materials to form a conductive network structure, the problem of poor conductivity of lithium iron phosphate materials is solved, the transmission capacity of lithium ions and the cycle performance of the battery are improved, and the polarization phenomenon is reduced.
Patent Information
- Application Number
- PCT/CN2023/137107
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2023-12-07
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium iron phosphate material has poor conductivity, resulting in slow lithium ion diffusion, high internal resistance, poor rate performance, and prone to polarization, which limits the performance of lithium-ion batteries.
Nitrogen-doped carbon nanotubes are used as conductive agents. By doping nitrogen elements in the carbon nanotubes, an efficient conductive network structure is formed, which improves the conductivity and tap density of lithium iron phosphate materials and enhances the transmission capacity of lithium ions.
It significantly improves the conductivity and high-rate performance of lithium iron phosphate materials, reduces polarization phenomena, improves the reversible capacity and cycle performance of the battery, and uses nitrogen-doped carbon nanotubes with high purity and stability.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
A lithium iron phosphate conductive agent and a lithium iron phosphate positive electrode sheet and battery using the same
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on March 30, 2023, with application number 2023103283020. The entire contents of the above application are incorporated by reference into this application. Technical Field
[0002] The present application belongs to the field of lithium battery conductive agents, and specifically relates to a lithium iron phosphate conductive agent and a lithium iron phosphate positive electrode sheet and battery using the same. Background Art
[0003] Energy shortages and global environmental pressures have driven the development and application of lithium batteries. Today, lithium batteries, with their unique performance advantages, are present in every corner of our lives. Currently, the main cathode materials for lithium-ion power batteries are lithium iron phosphate and ternary materials. Despite fierce competition among companies, the degree of iron-lithium conversion remains very high. The performance of the cathode material directly affects the performance of lithium-ion batteries. Lithium iron phosphate, with its excellent properties such as high voltage, high capacity, low power consumption, high safety, and long cycle life, has become the cathode of choice in the lithium-ion battery industry. However, due to its inherent structure, lithium iron phosphate has a low tap density, poor inter-particle adhesion, and lithium ions only deintercalate in one dimension, resulting in poor conductivity. This is primarily because when lithium ions are deintercalated and intercalated into the cathode, LiFePO4 exists as a lithium-rich phase (LiFePO4) and a lithium-poor phase (FePO4). During this phase transition, the crystal undergoes only a slight volume contraction. Therefore, lithium ions will only diffuse along one-dimensional direction, but the transformation of LiFePO4 to FePO4 will occur during the process of extraction and embedding, and the PO4 tetrahedron between LiO6 octahedron and FeO6 octahedron limits the volume change in this transformation, thereby affecting the Li + In addition, since there are no continuous FeO6 octahedrons in the structure, electrons cannot be transmitted continuously and can only be conducted through the Fe-O-Fe method, resulting in poor electronic conductivity.
[0004] However, due to the poor conductivity of lithium iron phosphate materials themselves and the slow diffusion of lithium ions, problems such as large internal resistance and poor rate performance are prone to occur during battery use. In addition, polarization is often easily generated during high-rate charge and discharge, reducing the utilization of capacity. Therefore, it is necessary to study the impact of the composition of conductive additives on battery performance. In conventional production, Super P and KS-6 conductive additives are generally used to improve the conductivity and flexibility of lithium iron phosphate electrodes. There are also some methods that directly modify LiFePO4. Common LiFePO4 modification methods mainly include carbon coating modification, morphology control modification, and doping modification. Technical issues
[0005] In order to solve the problems and deficiencies in the prior art, the present application provides a lithium iron phosphate conductive agent, which is nitrogen-doped carbon nanotubes, to improve the conductivity and high-rate performance of the lithium iron phosphate material and improve the electrochemical performance of the battery.
[0006] Technical Solution
[0007] In a first aspect, the present application provides a lithium iron phosphate conductive agent comprising nitrogen-doped carbon nanotubes, wherein the nitrogen content of the nitrogen-doped carbon nanotubes is 0.8 to 1.5 wt % of the total mass of the nitrogen-doped carbon nanotubes. The nitrogen content of the nitrogen-doped carbon nanotubes can be, for example, 0.8 wt %, 1.0 wt %, 1.2 wt %, 1.4 wt %, or 1.5 wt %, but is not limited to these values, and other values within this range are also applicable.
[0008] In a second aspect, the present application provides a method for preparing the above-mentioned lithium iron phosphate conductive agent, which is prepared according to the following steps:
[0009] S1. Using a silicon wafer as a substrate, deposit a 0.5-1.5 nm gold thin film layer on the substrate by thermal evaporation to obtain a gold-coated silicon wafer.
[0010] S2.
[0011] S2.1. Wash the gold-containing thin film silicon wafer with ethanol and blow dry with gas. Place the nitrogen source powder, carbon source powder, and gold-containing thin film silicon wafer in the reaction chamber in that order. Place the nitrogen source powder near the gas inlet. The distance between the nitrogen source powder and the carbon source powder is 10-12 cm, and the distance between the carbon source powder and the gold-containing thin film silicon wafer is 10-12 cm.
[0012] S2.2. The reaction chamber is evacuated for 5 to 10 minutes, and the vacuum degree of the reaction chamber is maintained at 0.05 to 0.2 Pa;
[0013] S2.3. Under heating and high pressure conditions, inert gas and nitrogen are introduced. Under heating and high pressure conditions, the gold thin film layer on the gold-containing silicon wafer forms alloy droplets that act as a catalyst. Through a gas-liquid-solid reaction, nitrogen-doped carbon nanotubes are precipitated on the silicon substrate.
[0014] S3. After the reaction chamber cools to room temperature, remove the silicon wafer containing the reactants, scrape the reactants off the silicon wafer, soak them in acid, and neutralize them with alkali to obtain a suspension. The suspension is filtered, washed, and dried to obtain nitrogen-doped carbon nanotubes.
[0015] In a third aspect, the present application provides a positive electrode sheet, which includes a positive electrode current collector and a positive electrode active material layer, the positive electrode active material layer includes a positive electrode active material and the above-mentioned lithium iron phosphate conductive agent; the positive electrode active material includes lithium iron phosphate.
[0016] In a fourth aspect, the present application provides a battery comprising the above-mentioned positive electrode sheet, negative electrode sheet, separator and electrolyte. Beneficial effects
[0017] Generally speaking, in order to improve the conductivity of lithium iron phosphate materials, traditional conductive additives such as acetylene black, SP, SuperS, Ketjen black, etc. are currently mainly used. However, although this type of conductive agent can improve the conductivity of lithium iron phosphate materials to a certain extent, it cannot effectively improve the structural defects of lithium iron phosphate itself, such as the low tap density. Therefore, this type of conductive agent has certain limitations on improving the conductivity of lithium iron phosphate. Carbon nanotubes are a new type of carbon material that are widely used in the fields of catalytic modification, hydrogen storage performance modification, capacitor modification, etc. Although some reports mention that carbon nanotubes have good conductivity and that doping modification of carbon nanotubes is beneficial to improving properties such as conductivity, such as nitrogen-doped carbon nanotubes, their use in improving the conductivity of lithium iron phosphate is less involved.
[0018] There are no continuous FeO6 octahedrons in the lithium iron phosphate structure, so electrons cannot be transmitted continuously and can only be conducted in the form of Fe-O-Fe, resulting in poor electronic conductivity. Compared with non-nitrogen-doped carbon nanotubes, the nitrogen-doped carbon nanotubes in this solution use nitrogen doping to reduce the band gap of the carbon nanotubes, reducing the energy required for electron transition to the conduction band, which can well compensate for the defects in the structure of the lithium iron phosphate itself and enhance the conductivity and storage capacity of the lithium iron phosphate. In addition, the size of nitrogen atoms is not much different from that of carbon atoms, and they can more easily enter the lattice of carbon nanotubes during the synthesis of carbon nanotubes, which greatly improves the physical and chemical properties of carbon nanotubes. Therefore, the nitrogen-doped carbon nanotubes of this application can more effectively improve the defects of the structure of the lithium iron phosphate material itself, enhance the tap density of lithium iron phosphate and the viscosity between particles, enable lithium ions to be not limited to the deintercalation in one-dimensional direction, reduce the lithium ion diffusion barrier, and improve the transmission capacity of lithium ions, thereby improving the cycle performance of lithium iron phosphate. Furthermore, when the nitrogen-doped carbon nanotubes in the present application modify the lithium iron phosphate material, in the three-dimensional network structure formed between them, the hollow fiber structure of the nitrogen-doped carbon nanotubes can firmly entangle the lithium iron phosphate nanoparticles, and they are closely connected. The large specific surface area between the two can enable good contact, ensuring that the amount of conductive agent in each active material is evenly distributed, and the nitrogen-doped carbon nanotubes have a lower band gap width. Such a uniform and mutually cross-linked structure can enhance the activity of electron transitions in the lithium iron phosphate material, so that electrons can be transmitted more quickly with the help of nitrogen-doped carbon nanotubes, thereby improving the conductivity and high-rate performance of the lithium iron phosphate material.
[0019] Furthermore, when the nitrogen doping level meets the aforementioned characteristics, nitrogen-doped carbon nanotubes not only effectively reduce the carbon nanotube band gap and enhance conductivity, but also significantly improve the physical and chemical properties of the carbon nanotubes, even with a relatively low nitrogen doping level. However, too little nitrogen doping has little effect on enhancing the carbon nanotubes' conductivity, while too much nitrogen doping can weaken the carbon nanotubes' inherent properties, disrupting some of the carbon nanotubes' lattices and reducing their structural stability, thereby affecting the performance of the active material.
[0020] The nitrogen-doped carbon nanotubes prepared by chemical vapor deposition (CVD) are directly co-doped with the carbon source in situ to form nitrogen-doped carbon nanotubes. This allows nitrogen atoms to be smoothly doped into the lattice of the carbon nanotubes during their growth and formation, thereby improving lattice defects, enhancing the structural stability of the carbon nanotubes, and improving the electrical conductivity and other physical and chemical properties of the carbon nanotubes. Furthermore, when the nitrogen-doped carbon nanotubes prepared by the above method are used to modify lithium iron phosphate materials, their stable lattice structure can fully compensate for the structural defects of the lithium iron phosphate itself. When the nitrogen-doped carbon nanotubes prepared by the above method are dispersed in the lithium iron phosphate material, the hollow fiber structure formed by the stable lattice structure is more conducive to firmly entrapping the lithium iron phosphate particles. This not only facilitates the good dispersion of the nitrogen-doped carbon nanotubes in the lithium iron phosphate material, but also helps to increase the tap density of the lithium iron phosphate material and increase the compaction between the lithium iron phosphate particles, thereby improving the electrical conductivity and other electrochemical properties of the lithium iron phosphate material.
[0021] In S1, the thickness of the gold thin film layer can be, for example, 0.5 nm, 1 nm, or 1.5 nm (the thickness can be controlled by the evaporation time); the current during gold plating can be, for example, 120 A, 130 A, 140 A, or 150 A. The reaction conditions described in S1 are not limited to the values listed above; other values not listed within the numerical range are also applicable. The gold thin film layer deposited on the silicon wafer serves as a catalyst for the subsequent formation of nitrogen-doped carbon nanotubes, exhibiting higher catalytic activity. Furthermore, a thinner gold thin film layer can reduce the catalyst content in the formed nitrogen-doped carbon nanotubes, thereby increasing the purity of the nitrogen-doped carbon nanotubes and reducing the adverse effects of the metal catalyst on the nitrogen-doped carbon nanotubes.
[0022] The nitrogen-doped carbon nanotubes in this scheme are used as the conductive agent of the lithium iron phosphate positive electrode sheet, which improves the poor conductivity of the lithium iron phosphate positive electrode active material, increases its lithium ion conduction rate at high rate, reduces the occurrence of polarization phenomenon, and improves the high rate performance of the battery.
[0023] In the battery in the present application, the active material layer of the positive electrode sheet includes lithium iron phosphate active material and the nitrogen-doped carbon nanotube conductive agent in this solution. Compared with the combination of lithium iron phosphate active material and ordinary conductive agent, the nitrogen-doped carbon nanotube conductive agent in this solution is more obvious in enhancing the conductivity of the lithium iron phosphate active material, and can significantly improve the capacity of the lithium iron phosphate positive electrode sheet and improve the reversible capacity and cycle performance of the battery.
[0024] In summary, the nitrogen-doped carbon nanotubes obtained by the preparation method in this application can significantly improve the poor conductivity of active materials such as lithium iron phosphate positive electrode materials, and reduce the polarization phenomenon caused by slow lithium ion conduction during high-rate discharge of lithium iron phosphate positive electrode materials. Compared with laser evaporation and arc discharge methods, the chemical vapor deposition method used in this scheme to prepare nitrogen-doped carbon nanotubes has lower energy consumption and simple operation, and the purity of the obtained nitrogen-doped carbon nanotubes is higher. Modes for Carrying Out the Invention
[0025] In one embodiment, in the nitrogen-doped carbon nanotubes, nitrogen accounts for 1.2 wt % of the total mass of the nitrogen-doped carbon nanotubes.
[0026] In one embodiment, the nitrogen-doped carbon nanotubes have a pore diameter of 5 to 10 nm and an aspect ratio of 800 to 1100:1. The pore diameter of the nitrogen-doped carbon nanotubes can be, for example, 5 nm, 6 nm, 7 nm, 8 nm, or 9 nm; the aspect ratio can be, for example, 800:1, 900:1, 1000:1, or 1100:1. The structural parameters of the nitrogen-doped carbon nanotubes are not limited to the values listed above, and other values not listed within the numerical range are also applicable. Because the aspect ratio of carbon nanotubes affects the dispersion of carbon nanotubes in the medium, nitrogen-doped carbon nanotubes that meet the above characteristics have better dispersion in lithium iron phosphate materials, can reduce the entanglement of nitrogen-doped carbon nanotubes, and prevent nitrogen-doped carbon nanotubes from being doped in the gaps between active particles in the form of agglomerates. At the same time, they can form a three-dimensional conductive network with the lithium iron phosphate material, increasing the contact area between the nitrogen-doped carbon nanotubes and the lithium iron phosphate material, thereby improving the conductivity of the lithium iron phosphate material.
[0027] In one embodiment, the pore diameter of the nitrogen-doped carbon nanotubes is 7 nm, and the aspect ratio is 1000:1.
[0028] In one embodiment, in S2.1, the inert gas includes argon.
[0029] In S2.1 above, the distance between the nitrogen source powder and the carbon source powder can be, for example, 10 cm, 11 cm, or 12 cm; the distance between the carbon source powder and the gold-containing thin film silicon wafer can be, for example, 10 cm, 11 cm, or 12 cm. The reaction conditions described in S2.1 above are not limited to the values listed, and other values within the numerical range not listed are equally applicable. When the gas is introduced, the nitrogen source powder and the carbon source powder can be transported with the gas to the downstream location of the gold-containing thin film silicon wafer, allowing the nitrogen source powder and the carbon source powder to fully contact the gold-containing thin film silicon wafer, increasing the reaction contact area and improving the degree of reaction. Maintaining a certain distance between the nitrogen source powder, the carbon source powder, and the gold-containing thin film can control the carbon source and nitrogen source to mix and react at an appropriate rate as the gas is transported, ensuring sufficient reaction between the nitrogen source and the carbon source, allowing sufficient time for nitrogen to be doped into the carbon nanotube lattice, improving the dispersion of nitrogen in the carbon nanotubes, effectively enhancing and reducing the band gap of the carbon nanotubes, and further improving the conductivity and other physical and chemical properties of the nitrogen-doped carbon nanotubes.
[0030] In S2.2 above, the evacuation time can be 5 minutes, 10 minutes, or 15 minutes; the vacuum level maintained in the reaction chamber can be 0.05 Pa, 0.1 Pa, 0.15 Pa, or 0.2 Pa. The process conditions described in S2.2 above are not limited to the values listed above; other values not listed within the numerical range are also applicable. Evacuating the reaction chamber is performed to remove impurities within the reaction chamber to prevent them from affecting the subsequent nitrogen-doped carbon nanotube production process and causing quality defects in the nitrogen-doped carbon nanotubes.
[0031] In one embodiment, in S2.3, the high-pressure heating conditions are a heating temperature of 750-850°C, a pressure of 400-600 mbar, and a reaction time of 15-60 minutes. The heating temperature in S2.3 can be 750°C, 800°C, or 850°C; the pressure can be 400 mbar, 450 mbar, 500 mbar, 550 mbar, or 600 mbar; and the reaction time can be 15 minutes, 20 minutes, 30 minutes, 40 minutes, or 50 minutes. The reaction conditions in S2.3 are not limited to the listed values; other values within the numerical range not listed are also applicable.
[0032] In one embodiment, in S3, the acid soaking time is 30 to 40 minutes. The acid soaking time can be, for example, 30 minutes, 35 minutes, or 40 minutes, but is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0033] In one embodiment, the nitrogen source powder includes at least one of melamine and ammonium carbonate.
[0034] In one embodiment, the carbon source powder includes at least one of graphite, cellulose, and camphor.
[0035] In one embodiment, the nitrogen source is melamine and the carbon source is graphite. Using these two nitrogen and carbon source materials allows for better coordination and interaction during the formation of nitrogen-doped carbon nanotubes, resulting in a smaller bandgap and, consequently, superior electrical conductivity. Furthermore, the nitrogen-doped carbon nanotubes formed from these two materials have fewer lattice defects, a uniform morphology, a stable structure, and improved physical and chemical properties.
[0036] In one embodiment, the lithium iron phosphate conductive agent accounts for 3.2 wt% of the total mass of the positive electrode active material layer (2.5% carbon black, 0.7% nitrogen-doped carbon nanotubes). Using the nitrogen-doped carbon nanotube conductive agent in this embodiment, a relatively small amount can significantly enhance the conductivity of the lithium iron phosphate material. Within the aforementioned content range, the nitrogen-doped carbon nanotube conductive agent has the best modification effect on the lithium iron phosphate, enhancing the conductivity of the lithium iron phosphate material while maintaining or enhancing other properties of the lithium iron phosphate as a positive electrode material.
[0037] Example 1
[0038] (1) Preparation of nitrogen-doped carbon nanotubes
[0039] The nitrogen-doped carbon nanotubes of this embodiment were prepared according to the following method:
[0040] S1.
[0041] S1.1. The silicon wafer is rinsed with acetone and ethanol to remove impurities on the surface of the silicon wafer. In this step, the silicon wafer can also be placed in acetone and ethanol and then ultrasonically cleaned to remove impurities on the surface of the silicon wafer.
[0042] S1.2. Place gold particles in a thermal evaporation groove and control the thermal evaporation to form a 1nm thick gold film on the silicon wafer, resulting in a gold-coated silicon wafer. The gold plating current is 120A.
[0043] S2.
[0044] S2.1. Wash the gold-containing thin film silicon wafer with ethanol and blow dry with gas. Place nitrogen source powder, carbon source powder, and the gold-containing thin film silicon wafer in a tube furnace, with the nitrogen source powder near the gas inlet. The nitrogen source powder and carbon source powder are 11 cm apart, and the carbon source powder and gold-containing thin film silicon wafer are 11 cm apart.
[0045] S2.2. Evacuate the tube furnace for 10 minutes and maintain a vacuum of 0.1 Pa in the quartz tube;
[0046] S2.3. A mixed argon / nitrogen gas mixture is introduced into the tube furnace for 10 minutes. The furnace is then heated to 750°C and the pressure within the furnace is increased to 500 mbar. This mixture transports nitrogen and carbon source powders downstream to the location of the gold-containing thin film silicon wafer. The gold thin film on the gold-containing thin film silicon wafer melts at high temperature to form alloy droplets, which serve as a catalyst. The nitrogen and carbon source powders undergo a gas-liquid-solid reaction for 30 minutes, precipitating nitrogen-doped carbon nanotubes on the silicon substrate.
[0047] S3. After the tube furnace cools to room temperature, remove the silicon wafer containing the reactants, rinse it with ethanol, and blow dry it. Then, scrape the reactants off the wafer and soak it in an acidic solution. After stirring and reacting for 35 minutes, neutralize it with an alkaline solution to obtain a suspension. Filter the suspension to obtain a solid product. Wash the solid product with distilled water and ethanol, and then dry it to obtain nitrogen-doped carbon nanotubes.
[0048] In this example, by controlling the feed ratio of nitrogen source powder to carbon source powder in S2, the nitrogen doping level of the generated nitrogen-doped carbon nanotubes was controlled to 1.2 wt%, where the nitrogen doping level represents the mass fraction of nitrogen in the nitrogen-doped carbon nanotubes. Furthermore, the nitrogen-doped carbon nanotubes in this example had a pore diameter of 7 nm and a length of 7 μm, resulting in an aspect ratio of 1000:1. In this example, the nitrogen source powder was melamine, and the carbon source powder was graphite.
[0049] (2) Preparation of lithium iron phosphate positive electrode
[0050] The lithium iron phosphate active material, carbon black, the nitrogen-doped carbon nanotubes, and PVDF (polytetrafluoroethylene) are mixed in a mass ratio of 95:2.5:0.7:1.8, and NMP (N-methylpyrrolidone) is added thereto to obtain a positive electrode slurry. The positive electrode slurry is coated on the surface of the positive electrode collector, dried, and pressed to obtain a lithium iron phosphate positive electrode sheet. After the positive electrode slurry is dried, a positive electrode active material layer is formed on the surface of the positive electrode collector. In this embodiment, the nitrogen-doped carbon nanotubes account for 0.7 wt% of the total mass of the positive electrode active material layer.
[0051] (3) Battery preparation
[0052] The lithium iron phosphate positive electrode sheet, negative electrode sheet, and separator are assembled into a cell, and an electrolyte is injected into the cell to obtain a battery.
[0053] Example 2
[0054] (1) Preparation of nitrogen-doped carbon nanotubes
[0055] The difference between the preparation of nitrogen-doped carbon nanotubes in this embodiment and that in embodiment 1 is that the nitrogen doping amount in the nitrogen-doped carbon nanotubes is 0.8 wt % by controlling the feed ratio of the nitrogen source powder and the carbon source powder in S2; the rest is the same as in embodiment 1.
[0056] (2) Preparation of lithium iron phosphate positive electrode
[0057] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0058] (3) Battery preparation
[0059] The preparation of the battery in this example is the same as that in Example 1.
[0060] Example 3
[0061] (1) Preparation of nitrogen-doped carbon nanotubes
[0062] The difference between the preparation of nitrogen-doped carbon nanotubes in this embodiment and that in embodiment 1 is that the nitrogen doping amount in the nitrogen-doped carbon nanotubes is 1.5 wt % by controlling the feed ratio of the nitrogen source powder and the carbon source powder in S2; the rest is the same as in embodiment 1.
[0063] (2) Preparation of lithium iron phosphate positive electrode
[0064] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0065] (3) Battery preparation
[0066] The preparation of the battery in this example is the same as that in Example 1.
[0067] Example 4
[0068] (1) Preparation of nitrogen-doped carbon nanotubes
[0069] The difference between the preparation of nitrogen-doped carbon nanotubes in this embodiment and that in Example 1 is that in S2.3, the heat preservation reaction time is 15 minutes, the pore diameter of the obtained nitrogen-doped nanotubes is 5 nm, the length is 4 μm, and the aspect ratio is 800:1; the rest is the same as in Example 1.
[0070] (2) Preparation of lithium iron phosphate positive electrode
[0071] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0072] (3) Battery preparation
[0073] The preparation of the battery in this example is the same as that in Example 1.
[0074] Example 5
[0075] (1) Preparation of nitrogen-doped carbon nanotubes
[0076] The difference between the preparation of nitrogen-doped carbon nanotubes in this embodiment and that in Example 1 is that in S2.3, the heat preservation reaction time is 50 minutes, the pore diameter of the obtained nitrogen-doped nanotubes is 10 nm, the length is 11 μm, and the aspect ratio is 11:1; the rest is the same as in Example 1.
[0077] (2) Preparation of lithium iron phosphate positive electrode
[0078] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0079] (3) Battery preparation
[0080] The preparation of the battery in this example is the same as that in Example 1.
[0081] Example 6
[0082] (1) Preparation of nitrogen-doped carbon nanotubes
[0083] The difference between the preparation of nitrogen-doped carbon nanotubes in this embodiment and that in Example 1 is that in S2.3, the heat preservation reaction time is 10 minutes, the pore diameter of the obtained nitrogen-doped nanotubes is 5 nm, the length is 3.5 μm, and the aspect ratio is 700:1; the rest is the same as in Example 1.
[0084] (2) Preparation of lithium iron phosphate positive electrode
[0085] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0086] (3) Battery preparation
[0087] The preparation of the battery in this example is the same as that in Example 1.
[0088] Example 7
[0089] (1) Preparation of nitrogen-doped carbon nanotubes
[0090] The difference between the preparation of nitrogen-doped carbon nanotubes in this embodiment and that in Example 1 is that in S2.3, the heat preservation reaction time is 60 minutes, the pore diameter of the obtained nitrogen-doped nanotubes is 8 nm, the length is 9.6 μm, and the aspect ratio is 1200:1; the rest is the same as in Example 1.
[0091] (2) Preparation of lithium iron phosphate positive electrode
[0092] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0093] (3) Battery preparation
[0094] The preparation of the battery in this example is the same as that in Example 1.
[0095] Example 8
[0096] (1) Preparation of nitrogen-doped carbon nanotubes
[0097] The difference between the preparation of nitrogen-doped carbon nanotubes in this embodiment and that in embodiment 1 lies in the different material combinations of the nitrogen source powder and the carbon source powder used. The nitrogen source and carbon source used in this embodiment are ammonium carbonate and graphite, respectively; the rest are the same as in embodiment 1.
[0098] (2) Preparation of lithium iron phosphate positive electrode
[0099] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0100] (3) Battery preparation
[0101] The preparation of the battery in this example is the same as that in Example 1.
[0102] Example 9
[0103] (1) Preparation of nitrogen-doped carbon nanotubes
[0104] The difference between the preparation of nitrogen-doped carbon nanotubes in this embodiment and that in embodiment 1 lies in the different material combinations of the nitrogen source powder and the carbon source powder used. The nitrogen source and carbon source used in this embodiment are melamine and cellulose, respectively; the rest are the same as in embodiment 1.
[0105] (2) Preparation of lithium iron phosphate positive electrode
[0106] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0107] (3) Battery preparation
[0108] The preparation of the battery in this example is the same as that in Example 1.
[0109] Example 10
[0110] (1) Preparation of nitrogen-doped carbon nanotubes
[0111] The difference between the preparation of nitrogen-doped carbon nanotubes in this embodiment and that in Example 1 lies in the different combinations of nitrogen source powder and carbon source powder used. The nitrogen source and carbon source used in this embodiment are melamine and camphor, respectively; the rest are the same as in Example 1.
[0112] (2) Preparation of lithium iron phosphate positive electrode
[0113] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0114] (3) Battery preparation
[0115] The preparation of the battery in this example is the same as that in Example 1.
[0116] Example 11
[0117] (1) Preparation of nitrogen-doped carbon nanotubes
[0118] The difference between the preparation of nitrogen-doped carbon nanotubes in this embodiment and that in embodiment 1 lies in the different material combinations of the nitrogen source powder and the carbon source powder used. The nitrogen source and carbon source used in this embodiment are ammonium carbonate and cellulose, respectively; the rest are the same as in embodiment 1.
[0119] (2) Preparation of lithium iron phosphate positive electrode
[0120] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0121] (3) Battery preparation
[0122] The preparation of the battery in this example is the same as that in Example 1.
[0123] Example 12
[0124] (1) Preparation of nitrogen-doped carbon nanotubes
[0125] The difference between the preparation of nitrogen-doped carbon nanotubes in this embodiment and that in Example 1 lies in the different combinations of nitrogen source powder and carbon source powder used. The nitrogen source and carbon source used in this embodiment are ammonium carbonate and camphor, respectively; the rest are the same as in Example 1.
[0126] (2) Preparation of lithium iron phosphate positive electrode
[0127] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0128] (3) Battery preparation
[0129] The preparation of the battery in this example is the same as that in Example 1.
[0130] Example 13
[0131] (1) Preparation of nitrogen-doped carbon nanotubes
[0132] The preparation of the nitrogen-doped carbon nanotubes of this embodiment is the same as that of Example 1.
[0133] (2) Preparation of lithium iron phosphate positive electrode
[0134] In the preparation example of the lithium iron phosphate positive electrode sheet, the mass ratio of the lithium iron phosphate active material, carbon black, nitrogen-doped carbon nanotubes, and PVDF (polytetrafluoroethylene) is 95:2.7:0.5:1.8. In the obtained lithium iron phosphate positive electrode sheet, the mass fraction of the nitrogen-doped carbon nanotube conductive agent in the positive electrode active material layer is 0.5wt%; the rest is consistent with Example 1.
[0135] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0136] (3) Battery preparation
[0137] The preparation of the battery in this example is the same as that in Example 1.
[0138] Example 14
[0139] (1) Preparation of nitrogen-doped carbon nanotubes
[0140] The preparation of the nitrogen-doped carbon nanotubes of this embodiment is the same as that of Example 1.
[0141] (2) Preparation of lithium iron phosphate positive electrode
[0142] In the preparation example of the lithium iron phosphate positive electrode sheet, the mass ratio of the lithium iron phosphate active material, carbon black, nitrogen-doped carbon nanotubes, and PVDF (polytetrafluoroethylene) is 95:2.2:1.0:1.8. In the obtained lithium iron phosphate positive electrode sheet, the mass fraction of the nitrogen-doped carbon nanotube conductive agent in the positive electrode active material layer is 1wt%; the rest is consistent with Example 1.
[0143] The preparation of the lithium iron phosphate positive electrode sheet in this embodiment is the same as that in Example 1.
[0144] (3) Battery preparation
[0145] The preparation of the battery in this example is the same as that in Example 1.
[0146] Comparative Example 1
[0147] (1) Preparation of nitrogen-doped carbon nanotubes
[0148] The difference between the preparation of nitrogen-doped carbon nanotubes in the comparative example and Example 1 is that the nitrogen doping amount in the nitrogen-doped carbon nanotubes is 0.5 wt % by controlling the feed ratio of nitrogen source powder to carbon source powder in S2; the rest is the same as Example 1.
[0149] (2) Preparation of lithium iron phosphate positive electrode
[0150] The preparation of the lithium iron phosphate positive electrode sheet in this comparative example is the same as that in Example 1.
[0151] (3) Battery preparation
[0152] The preparation of the battery in this comparative example is consistent with that in Example 1.
[0153] Comparative Example 2
[0154] (1) Preparation of nitrogen-doped carbon nanotubes
[0155] The difference between the preparation of nitrogen-doped carbon nanotubes in this comparative example and Example 1 is that the nitrogen doping amount in the nitrogen-doped carbon nanotubes is 1.8 wt % by controlling the feed ratio of nitrogen source powder to carbon source powder; the rest is the same as Example 1.
[0156] (2) Preparation of lithium iron phosphate positive electrode
[0157] The preparation of the lithium iron phosphate positive electrode sheet in this comparative example is the same as that in Example 1.
[0158] (3) Battery preparation
[0159] The preparation of the battery in this comparative example is consistent with that in Example 1.
[0160] Comparative Example 3
[0161] This comparative example differs from Example 1 in that nitrogen-doped carbon nanotubes are not prepared in this example, and nitrogen-doped carbon nanotubes are not used in the preparation of the lithium iron phosphate positive electrode sheet. The raw material ratios in the positive electrode slurry in this comparative example are as follows: lithium iron phosphate active material: carbon black: PVDF (polytetrafluoroethylene) = 95:3.2:1.8, calculated by mass ratio. The remaining ratios are consistent with Example 1. The battery in this comparative example is prepared in the same manner as in Example 1.
[0162] Comparative Example 4
[0163] (1) Preparation of carbon nanotubes
[0164] The carbon nanotubes prepared in this comparative example are different from those in Example 1 in that no nitrogen source is added to S2, and the obtained carbon nanotubes are nitrogen-undoped carbon nanotubes. The nitrogen-doped carbon nanotubes in Example 1 are replaced by nitrogen-undoped carbon nanotubes, and the rest are the same as in Example 1.
[0165] (2) Preparation of lithium iron phosphate positive electrode
[0166] The preparation of the lithium iron phosphate positive electrode sheet in this comparative example is the same as that in Example 1.
[0167] (3) Battery preparation
[0168] The preparation of the battery in this comparative example is consistent with that in Example 1.
[0169] Test Case
[0170] 1. Experimental Construction Method
[0171] The resistivity of the lithium iron phosphate positive electrode sheets in Examples 1 to 14 and Comparative Examples 1 to 4 was tested, and the electrochemical performance tests such as initial DC impedance, low-temperature discharge capacity, low-rate capacity retention, and high-rate capacity retention of the batteries in Examples 1 to 14 and Comparative Examples 1 to 4 were performed.
[0172] The resistivity test method is: take a certain number of electrodes and use the two-probe method to directly test the overall resistivity of the electrodes.
[0173] The test method for initial DC resistance is as follows: at 25°C, charge and discharge at a rate of 1C for 5 cycles, mark the capacity of the last cycle as the nominal capacity, adjust the SOC to 50% with the actual capacity, leave it for one hour, and discharge at a certain rate within a certain period of time to obtain the initial DCR.
[0174] The low-temperature discharge capacity test method is: charge and discharge at a rate of 1C for 5 cycles at room temperature, mark the last cycle as the nominal capacity, adjust the incubator temperature to -10°C, and monitor the discharge capacity of each battery.
[0175] The test method for low-rate capacity retention is: at 25°C, cycle the battery for 5 cycles at 1C capacity, record the last cycle as the nominal capacity, and then cycle at 1C / 1C, and record the discharge capacity of each cycle / nominal capacity as the capacity retention rate.
[0176] The test method for high-rate capacity retention is: cycle the battery at 3C capacity for 5 cycles at 25°C, recording the last cycle as the nominal capacity. Then cycle at 3C / 3C, and record the discharge capacity of each cycle divided by the nominal capacity as the capacity retention rate.
[0177] 2. Experimental Results
[0178] The test results of the resistivity of the lithium iron phosphate positive electrode sheets and the electrochemical performance of the corresponding batteries in Examples 1 to 14 and Comparative Examples 1 to 4 are shown in Table 1.
[0179] Table 1: Test results of the resistivity of the lithium iron phosphate positive electrode sheets and the electrochemical performance of the corresponding batteries in Examples 1 to 14 and Comparative Examples 1 to 4
[0180] Resistivity (Ω·cm2) Initial DC impedance (mΩ) -10℃ Discharge capacity percentage (%) Capacity retention rate after 1000 cycles (%) (1C, low rate) Capacity retention rate after 1000 cycles (%) (3C, high rate) Example 1 4.0×10-21 1587.2591.0592.82 Example 2 6.0×10-21 2585.8890.0391.26 Example 3 4.5×10-21 1886.9590.8791.99Example 45.8×10-212485.7890.1291.32Example 54.4×10-211686.9690.7992.21Example 66.5×10-212884.6589.6790.13Example 74.4×10-211786.8990.8592.17Example 84.1×10-211587.0 990.8892.67Example 94.3×10-211686.9690.7892.19Example 104.3×10-211686.8890.6992.05Example 114.5×10-211886.9490.8092.20Example 124.5×10-211886.8790.7992.17Example 136.5×10-212885.238 9.5390.87 Example 143.0×10-2108888.5690.8591.98 Comparative Example 16.8×10-212885.5589.9587.98 Comparative Example 25.0×10-211986.8990.5888.81 Comparative Example 39×10-215082.1287.2588.82 Comparative Example 47×10-213085.1289.0590.62
[0181] It can be seen from the test results in Table 1 that the lithium iron phosphate positive electrode sheet modified with nitrogen-doped carbon nanotubes prepared by the present application has a lower resistivity and initial DC impedance, which is conducive to the battery releasing more capacity at low temperatures and has a better high-rate cycle capacity retention rate.
[0182] Further, comparing Examples 1 to 3 and Comparative Examples 1 to 2, the nitrogen content in the nitrogen-doped carbon nanotubes in Comparative Examples 1 to 2 is too little and too much. Too little nitrogen has a poor modification effect on the carbon nanotubes, and too much nitrogen is not conducive to the nitrogen atoms and the carbon nanotubes forming a more stable lattice structure. Therefore, the nitrogen-doped carbon nanotubes obtained in Comparative Examples 1 and 2 have poor modification effects on the lithium iron phosphate positive electrode sheet, which is reflected in a slightly poor cycle capacity retention rate at high rates; while in Examples 1 to 3, the battery in Example 1 has the best cycle performance, and it is apparent that when the nitrogen doping amount in the carbon nanotubes is 1.2wt%, the nitrogen-doped carbon nanotubes have the best modification effect on the lithium iron phosphate positive electrode sheet. This may be because at this nitrogen doping amount, the network structure formed by the nitrogen-doped carbon nanotubes and the lithium iron phosphate active material is the most stable, thereby enhancing the cycle performance of the battery.
[0183] Comparing Examples 1 and 4 to 7, it can be seen that the aspect ratio of nitrogen-doped carbon nanotubes also has a certain influence on their performance. The use of nitrogen-doped carbon nanotubes with an aspect ratio of 1000:1 in Example 1 is more conducive to reducing the resistivity and initial DC impedance of the lithium iron phosphate positive electrode sheet, and has a higher low-temperature discharge capacity and better cycle performance.
[0184] By comparing Examples 1 and 8 to 12, it can be seen that the nitrogen source powder and the carbon source powder also have a certain influence on the performance of the nitrogen-doped carbon nanotubes finally formed. The nitrogen-doped carbon nanotubes obtained by using melamine and graphite in combination have the best effect on improving the conductivity and cycle performance of the lithium iron phosphate positive electrode.
[0185] Comparing Examples 1 and 13-14, it can be seen that when the proportion of nitrogen-doped carbon nanotubes in the lithium iron phosphate positive electrode sheet is in the range of 0.8-1.5wt%, the conductivity, low-temperature discharge capacity and cycle performance of the obtained lithium iron phosphate positive electrode sheet are all better.
[0186] The lithium iron phosphate positive electrode sheet in Comparative Example 3 does not contain nitrogen-doped carbon nanotubes, and the carbon nanotubes used in Comparative Example 4 are not doped with nitrogen. The resistivity and initial DC impedance of the lithium iron phosphate positive electrode sheets in these two examples are significantly larger, and the corresponding low-temperature discharge capacity is lower, indicating that the presence or absence of carbon nanotubes and whether the carbon nanotubes are doped with nitrogen have a great influence on the conductivity and cycle performance of the lithium iron phosphate positive electrode sheet.
Claims
1. A lithium iron phosphate conductive agent, wherein the lithium iron phosphate conductive agent is nitrogen-doped carbon nanotubes, in which the nitrogen element accounts for 0.8-1.5wt% of the total mass of the nitrogen-doped carbon nanotubes.
2. The lithium iron phosphate conductive agent according to claim 1, wherein: The pore diameter of the nitrogen-doped carbon nanotube is 5-10 nm, and the aspect ratio is 800-1100:
1.
3. A method for preparing the lithium iron phosphate conductive agent as claimed in claim 1, which is prepared according to the following steps: S1. Using a silicon wafer as a substrate, a 0.5-1.5 nm gold thin film layer is deposited on the substrate by thermal evaporation to obtain a silicon wafer containing a gold thin film layer, and the current during gold plating is 120-150A; S2. S2.
1. Use ethanol to clean the gold-containing thin film silicon wafer, blow dry with gas, and place the nitrogen source powder, carbon source powder, and the gold-containing thin film silicon wafer in the reaction chamber in sequence, the nitrogen source powder is close to one end of the gas inlet, the distance between the nitrogen source powder and the carbon source powder is 10~12cm, and the distance between the carbon source powder and the gold-containing thin film silicon wafer is 10~12cm; S2.
2. The reaction chamber is evacuated for 5 to 10 minutes, and the vacuum degree of the reaction chamber is maintained at 0.05 to 0.2 Pa; S2.
3. Under heating and high pressure conditions, an inert gas and nitrogen are introduced. Under heating and high pressure conditions, the gold thin film layer on the gold-containing thin film layer silicon wafer forms alloy droplets as a catalyst, and the nitrogen source powder and the carbon source powder undergo a gas-liquid-solid reaction to precipitate nitrogen-doped carbon nanotubes on the silicon substrate; S3. After the reaction chamber is cooled to room temperature, the silicon wafer containing the reactants is taken out, the reactants are scraped off the silicon wafer, and a suspension is obtained after acid soaking and alkali neutralization. The suspension is filtered, washed, and dried to obtain the nitrogen-doped carbon nanotubes.
4. The method of claim 3, wherein: In S2.3, the conditions of the high pressure heating are a heating temperature of 750-850° C., a pressure of 400-600 mbar, and a reaction time of 30-40 minutes.
5. The method of claim 3, wherein: In the nitrogen source powder, the nitrogen source includes at least one of melamine and ammonium carbonate.
6. The method of claim 3, wherein: In the carbon source powder, the carbon source includes at least one of graphite, cellulose and camphor.
7. The method of claim 3, wherein: The nitrogen source is melamine, and the carbon source is graphite.
8. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode active material and the lithium iron phosphate conductive agent as claimed in claim 1; and the positive electrode active material comprises lithium iron phosphate.
9. The positive electrode sheet according to claim 8, wherein: The lithium iron phosphate conductive agent accounts for 2-4 wt % of the total mass of the positive electrode active material layer.
10. A battery comprising the positive electrode sheet, the negative electrode sheet, the separator and the electrolyte according to any one of claims 8 to 9.
Citation Information
Patent Citations
Flexible oriented nitrogen-doped carbon nanotube thin film and preparation method and application therefor
CN105552381A
Lithium ion battery electrode and preparation method thereof
CN108511692A
Preparation method of nitrogen-doped carbon nanotube conductive paste for lithium ion battery
CN115020029A
Lithium iron phosphate conductive agent and lithium iron phosphate positive plate and battery using same
CN116344817A
Positive electrode and method for making the same, and battery using the same
US20200067073A1