In-situ preparation and application of flame-retardant PDOL-based polymer solid electrolyte

The preparation of flame-retardant PDOL-based polymer solid electrolytes through in-situ polymerization method solves the energy density and safety problems of lithium-ion batteries, realizes stable cycle and flame retardant performance at high temperatures, and improves the interface contact and electrochemistry of solid-state batteries. performance.

CN118919833APending Publication Date: 2024-11-08HARBIN INST OF TECH
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202410946677.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The energy density of traditional liquid lithium-ion batteries is limited and safety problems occur frequently. The poor solid-solid interface contact in solid-state batteries leads to low battery capacity and energy density and large interface impedance, and poor thermal stability of PDOL-based polymer solid electrolyte at high temperatures. And flammable.

Method used

The in-situ polymerization method is used to prepare flame retardant PDOL-based polymer solid electrolyte. By combining components A, B, C, D, E, and F, an electrolyte with high thermal stability and flame retardant properties is formed, and the electrolyte with high thermal stability and flame retardant properties is used in solid-state batteries. Assembly.

Benefits of technology

It improves the cycle stability and safety of solid-state batteries at high temperatures, inhibits the depolymerization of PDOL, provides good flame retardant effect and electrochemical stability window, and improves the interface contact between the electrode and the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919833A_ABST
    Figure CN118919833A_ABST
Patent Text Reader

Abstract

The invention discloses in-situ preparation and application of a flame-retardant PDOL-based polymer solid-state electrolyte, and relates to a preparation method of a thermally stable flame-retardant PDOL-based polymer solid-state electrolyte and application of the flame-retardant PDOL-based polymer solid-state electrolyte in a solid-state battery, and the PDOL-based solid-state battery can be used under a high-temperature condition. The invention aims to solve the problems of poor safety and high-temperature cycle performance of the solid-state battery caused by depolymerization and flammability of the existing PDOL polymer solid-state electrolyte at high temperature. The invention relates to in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte. The flame-retardant PDOL-based polymer solid electrolyte is composed of 1, 3-dioxolane, a trifunctional aziridine cross-linking agent, cross-linking agents such as tetraethylene glycol diglycidyl ether, a flame-retardant initiator, a lithium salt, a plasticizer and an additive. The obtained PDOL-based solid electrolyte has relatively good thermal stability and flame-retardant property, and the assembled solid-state battery can stably circulate at high temperature. The obtained solid electrolyte can be used in a lithium iron phosphate and nickel-cobalt-manganese ternary positive electrode solid-state battery, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid-state batteries and relates to an in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte. Background Art

[0002] Lithium-ion batteries are widely used in various fields due to their superior performance. However, the energy density of the electrode materials of traditional liquid lithium-ion batteries is limited, which makes it difficult to meet the growing energy demand; and in recent years, traditional liquid lithium-ion batteries have frequent safety issues, so improving the energy density and safety of batteries has become an urgent problem to be solved in the field of lithium-ion batteries. Solid-state batteries that use solid electrolytes instead of liquid electrolytes can be compatible with positive and negative electrodes with high specific capacity, and can simultaneously improve the energy density and safety of the battery cell. However, the poor solid-solid interface contact in solid-state batteries can lead to problems such as low battery capacity and energy density, and large interface impedance. The use of in-situ polymerization technology to prepare solid-state batteries can improve interface contact, increase compatibility, and reduce interface impedance.

[0003] Poly (1,3-dioxolane) (PDOL) has been widely studied because of its good compatibility with lithium metal and high conductivity. However, PDOL has poor thermal stability and will depolymerize into DOL monomer at 60°C. In addition, traditional PDOL electrolytes will burn rapidly when exposed to external fire sources. Therefore, the difficulty of PDOL-based polymer solid electrolytes lies in improving their high-temperature stability while making the electrolytes have better flame retardancy.

[0004] In the prior art, CN 118231756A discloses a flame-retardant gel polymer electrolyte, a preparation method and its application in a high energy density battery system, which obtains flame-retardant properties by polymerizing VC; CN117810527A discloses a flame-retardant electrolyte and its preparation method and application, which obtains flame-retardant properties by adding flame-retardant fillers to the system. However, the flame-retardant polymer electrolyte studied in the prior art does not contain a PDOL system, and PDOL will depolymerize into liquid DOL monomers at high temperatures, so that the system needs to obtain better flame-retardant properties than other common polymer electrolyte systems, otherwise it will bring more serious safety problems than other common polymer solid-state batteries at high temperatures. Summary of the invention

[0005] The present invention is to assemble a solid-state battery through an in-situ polymerization method. The core is to prepare a flame-retardant PDOL-based polymer solid electrolyte with high thermal stability, thereby achieving stable circulation and good flame-retardant properties of the solid-state battery at high temperature, and providing an in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte.

[0006] The invention discloses an in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte, characterized in that the flame-retardant solid electrolyte is composed of component A, component B, component C, component D, component E and component F.

[0007] The component A is 1,3-dioxolane;

[0008] The component B is at least one of a trifunctional aziridine crosslinker, tris(2-methylaziridine)phosphine oxide, triglycidyl isocyanurate, trimethylolpropane triglycidyl ether, glycerol triglycidyl ether, triglycidyl p-aminophenol, 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, ethylene glycol diglycidyl ether, tetraethylene glycol diglycidyl ether, pentaerythritol glycidyl ether, resorcinol diglycidyl ether, bisphenol A diglycidyl ether or neopentyl glycol diglycidyl ether;

[0009] The component C is at least one of trispentafluorophenylborane or tris(hexafluoroisopropyl) borate;

[0010] The component D is at least one of lithium perchlorate, lithium bis(oxalatoborate), lithium bis(trifluoromethanesulfonyl)amide or lithium bis(fluorosulfonyl)amide;

[0011] The component E is at least one of ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, propylene carbonate or ethylene glycol dimethyl ether;

[0012] The component F is lithium difluorophosphate and N,N-dimethyltrifluoroacetamide.

[0013] The in-situ preparation of the flame-retardant PDOL-based polymer solid electrolyte and the assembly of the solid-state battery of the present invention are carried out according to the following steps:

[0014] 1. Preparation of a component A-component B-component D-component F mixed solution: Component A, component B, component D and component F are mixed, and stirred for 5 to 600 minutes at room temperature and in air-tight conditions to obtain a component A-component B-component D-component F mixed solution;

[0015] 2. Preparation of a component C-component E mixed solution: Mix component C and component E, and stir for 30 min to 600 min at 40° C. in an air-tight condition to obtain a component C-component E mixed solution;

[0016] 3. Preparation method of flame-retardant PDOL-based polymer solid electrolyte: slowly drop the component C-component E mixed solution prepared in step 2 into the component A-component B-component D-component F mixed solution prepared in step 1 while stirring, stir for 5min to 600min at room temperature in an air-tight condition, and after mixing evenly, obtain a precursor solution of the polymer solid electrolyte. The precursor solution is allowed to stand at 40°C to 60°C for 24h to 100h to obtain a flame-retardant PDOL-based polymer solid electrolyte.

[0017] 4. Application of flame-retardant PDOL-based polymer solid electrolyte in solid-state batteries: Assemble the battery using the positive electrode, diaphragm and negative electrode in a glove box, inject the solid electrolyte precursor prepared in step 3 into the battery, soak it on the diaphragm, and then use a battery packaging machine to package it. Let it stand at 40℃~60℃ for 24h~100h, and obtain a solid-state battery by in-situ polymerization, wherein the amount of solid electrolyte precursor used is 2g / Ah~15g / Ah.

[0018] Beneficial effects of the present invention:

[0019] The present invention introduces an in-situ preparation of a flame-retardant PDOL-based polymer solid electrolyte, thereby obtaining a flame-retardant PDOL-based polymer solid electrolyte with high thermal stability, thereby improving the cycle stability and safety of solid batteries under high temperature conditions. The present invention involves mild chemical reaction conditions, simple methods, and no side reactions.

[0020] The solid electrolyte prepared by this method has the following effects: (1) The PDOL cross-linked skeleton in the solid electrolyte inhibits the depolymerization of PDOL, making it have better thermal stability. (2) The high fluorine content initiator in the solid electrolyte makes the electrolyte have a good flame retardant effect, improving the safety of the battery. (3) The polymer solid electrolyte prepared by in situ polymerization is viscous, which is beneficial to improve the interface contact between the solid electrolyte and the electrode. (4) The cross-linked structure in the solid electrolyte and the addition of additives improve the electrochemical stability window of the electrolyte, making it compatible with high-voltage positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a flame retardant performance test diagram of the solid electrolyte in Experiment 2;

[0022] Figure 2 This is the cycle performance curve of the lithium iron phosphate solid-state battery in test 3 at 80°C; DETAILED DESCRIPTION

[0023] The present invention will be further described below with reference to embodiments and drawings, but the present invention is not limited to these embodiments.

[0024] Specific implementation method 1: A flame-retardant PDOL-based polymer solid electrolyte of the present invention is specifically composed of component A, component B, component C, component D, component E and component F.

[0025] The component A is 1,3-dioxolane;

[0026] The component B is at least one of a trifunctional aziridine crosslinker, tris(2-methylaziridine)phosphine oxide, triglycidyl isocyanurate, trimethylolpropane triglycidyl ether, glycerol triglycidyl ether, triglycidyl p-aminophenol, 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, ethylene glycol diglycidyl ether, tetraethylene glycol diglycidyl ether, pentaerythritol glycidyl ether, resorcinol diglycidyl ether, bisphenol A diglycidyl ether or neopentyl glycol diglycidyl ether;

[0027] The component C is at least one of trispentafluorophenylborane or tris(hexafluoroisopropyl) borate;

[0028] The component D is at least one of lithium perchlorate, lithium bis(oxalatoborate), lithium bis(trifluoromethanesulfonyl)amide or lithium bis(fluorosulfonyl)amide;

[0029] The component E is at least one of ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, propylene carbonate or ethylene glycol dimethyl ether;

[0030] The component F is lithium difluorophosphate and N,N-dimethyltrifluoroacetamide.

[0031] Specific implementation method 2: This implementation method is the in-situ preparation of the flame-retardant PDOL-based polymer solid electrolyte and the assembly of the solid-state battery of specific implementation method 1, which is specifically carried out according to the following steps:

[0032] 1. Preparation of a component A-component B-component D-component F mixed solution: Component A, component B, component D and component F are mixed, and stirred for 5 to 600 minutes at room temperature and in air-tight conditions to obtain a component A-component B-component D-component F mixed solution;

[0033] 2. Preparation of a component C-component E mixed solution: Mix component C and component E, and stir for 30 min to 600 min at 40° C. in an air-tight condition to obtain a component C-component E mixed solution;

[0034] 3. Preparation method of flame-retardant PDOL-based polymer solid electrolyte: slowly drop the component C-component E mixed solution prepared in step 2 into the component A-component B-component D-component F mixed solution prepared in step 1 while stirring, stir for 5min to 600min at room temperature in an air-tight condition, and after mixing evenly, obtain a precursor solution of the polymer solid electrolyte. The precursor solution is allowed to stand at 40°C to 60°C for 24h to 100h to obtain a flame-retardant PDOL-based polymer solid electrolyte.

[0035] 4. Application of flame-retardant PDOL-based polymer solid electrolyte in solid-state batteries: Assemble the battery using the positive electrode, diaphragm and negative electrode in a glove box, inject the solid electrolyte precursor prepared in step 3 into the battery, soak it on the diaphragm, and then use a battery packaging machine to package it. Let it stand at 40℃~60℃ for 24h~100h, and obtain a solid-state battery by in-situ polymerization, wherein the amount of solid electrolyte precursor used is 2g / Ah~15g / Ah.

[0036] Specific implementation method 3: This implementation method is different from specific implementation method 2 in that the volume ratio of component A to component B is (9.5:0.5-1:9). Other aspects are the same as specific implementation method 2.

[0037] Specific embodiment 4: This embodiment differs from specific embodiment 2 in that the molar concentration of component C in the precursor solution is (0.02 mol / L to 0.5 mol / L). Other aspects are the same as those of specific embodiment 2.

[0038] Specific embodiment 5: This embodiment is different from specific embodiment 2 in that the molar concentration of component D in the precursor solution is (0.5 mol / L to 2.5 mol / L). Other aspects are the same as those of specific embodiment 2.

[0039] Specific embodiment 6: This embodiment is different from the specific embodiment 2 in that the volume percentage of the component E in the precursor solution is (5% to 50%). Other aspects are the same as the specific embodiment 2.

[0040] Specific embodiment 7: This embodiment differs from specific embodiment 2 in that the mass percentages of the component F in the precursor solution are (0.5% to 5%) and (0.5% to 10%) respectively. The rest is the same as specific embodiment 2.

[0041] Specific embodiment 8: This embodiment differs from specific embodiment 2 in that the separator used is a PE separator, a cellulose separator, a glass fiber separator, a polyimide separator, a polyacrylonitrile separator or a PE / PP / PE composite separator. The rest is the same as specific embodiment 2.

[0042] The present invention is verified by the following tests:

[0043] Experiment 1: This experiment is a method for preparing a precursor solution of a polymer solid electrolyte, which is specifically carried out in the following steps:

[0044] 1. Preparation of precursor solution of polymer solid electrolyte: 1,3-dioxolane, triglycidyl p-aminophenol, lithium bis(trifluoromethylsulfonyl)amide, lithium difluorophosphate and N,N-dimethyltrifluoroacetamide were mixed, and stirred for 30 minutes at room temperature and in air-tight conditions to obtain precursor solution 1. Tri(hexafluoroisopropyl) borate and ethylene carbonate were mixed, and stirred for 30 minutes at 40°C and in air-tight conditions to obtain precursor solution 2. Precursor solution 2 was slowly dripped into precursor solution 1 while it was being stirred, and stirred for 10 minutes at room temperature and in air-tight conditions. After mixing evenly, a precursor solution of polymer solid electrolyte was obtained:

[0045] The volume ratio of 1,3-dioxolane to triglycidyl p-aminophenol is 8:2;

[0046] The molar concentration of tris(hexafluoroisopropyl) borate in the precursor solution is 0.3 mol / L;

[0047] The molar concentration of the lithium bis(trifluoromethanesulfonic acid) amide in the precursor solution is 2 mol / L;

[0048] The volume percentage of the ethylene carbonate in the precursor solution is 10%;

[0049] The mass percentages of the lithium difluorophosphate and N,N-dimethyltrifluoroacetamide in the precursor solution are 0.5% and 3% respectively.

[0050] Experiment 2: Use the precursor solution of the polymer solid electrolyte obtained in Experiment 1 to prepare a solid electrolyte and conduct a flame retardant performance test:

[0051] The polymer solid electrolyte precursor solution was allowed to stand at 60° C. for 24 hours to obtain a polymer solid electrolyte, and an ignition experiment was performed on it to verify its flame retardant properties.

[0052] Figure 1 This is the flame retardant performance diagram in Experiment 2. As shown in the figure, the prepared polymer solid electrolyte has good flame retardant properties.

[0053] Experiment 3: Use the precursor solution of the polymer solid electrolyte obtained in Experiment 1 to assemble an in-situ solid-state lithium iron phosphate battery and conduct a test:

[0054] 1. Solid-state lithium iron phosphate battery assembly:

[0055] Lithium iron phosphate, conductive carbon material and adhesive were mixed in a mass ratio of 8:1:1, and added to N-methylpyrrolidone to form a uniform slurry. The slurry was applied to the current collector aluminum foil and dried in a vacuum oven at 100°C for 12 hours. The dried aluminum foil was then cut into discs and assembled with the diaphragm and lithium sheet. The polymer solid electrolyte precursor was then injected and packaged using a battery packaging machine. After standing at 60°C for 24 hours, a solid-state lithium iron phosphate battery was obtained for testing.

[0056] 2. Electrochemical performance test:

[0057] The constant current charge and discharge tester produced by Xinwei Company was used to carry out charge and discharge tests to measure the cycle performance curve of the solid-state lithium iron phosphate battery. The charge and discharge voltage range was 2.5V to 3.8V.

[0058] Figure 2 To test the cycle performance curve of the three phosphoric acid batteries, as shown in the figure, the assembled lithium iron phosphate battery can be charged and discharged 100 times at 80°C.

[0059] The above data fully demonstrate that the solid electrolyte prepared in the present invention can be applied to high-temperature solid-state batteries, and the obtained solid-state batteries have good flame retardant properties and high-temperature cycle performance.

[0060] It should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte, characterized in that The flame retardant solid electrolyte is composed of component A, component B, component C, component D, component E and component F; The component A is 1,3-dioxolane; The component B is at least one of a trifunctional aziridine crosslinker, tris(2-methylaziridine)phosphine oxide, triglycidyl isocyanurate, trimethylolpropane triglycidyl ether, glycerol triglycidyl ether, triglycidyl p-aminophenol, 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, ethylene glycol diglycidyl ether, tetraethylene glycol diglycidyl ether, pentaerythritol glycidyl ether, resorcinol diglycidyl ether, bisphenol A diglycidyl ether or neopentyl glycol diglycidyl ether; The component C is at least one of trispentafluorophenylborane or tris(hexafluoroisopropyl) borate; The component D is at least one of lithium perchlorate, lithium bis(oxalatoborate), lithium bis(trifluoromethanesulfonyl)amide or lithium bis(fluorosulfonyl)amide; The component E is at least one of ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, propylene carbonate or ethylene glycol dimethyl ether; The component F is lithium difluorophosphate and N,N-dimethyltrifluoroacetamide.

2. The in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte according to claim 1, characterized in that The preparation and application of a flame-retardant PDOL-based polymer solid electrolyte is carried out according to the following steps:

1. Preparation of a component A-component B-component D-component F mixed solution: Component A, component B, component D and component F are mixed, and stirred for 5 to 600 minutes at room temperature and in air-tight conditions to obtain a component A-component B-component D-component F mixed solution; 2. Preparation of a component C-component E mixed solution: Mix component C and component E, and stir for 30 min to 600 min at 40° C. in an air-tight condition to obtain a component C-component E mixed solution; 3. Preparation method of flame-retardant PDOL-based polymer solid electrolyte: slowly drop the component C-component E mixed solution prepared in step 2 into the component A-component B-component D-component F mixed solution prepared in step 1 while stirring, stir for 5min to 600min at room temperature in an air-tight condition, and after mixing evenly, obtain a precursor solution of the polymer solid electrolyte. The precursor solution is allowed to stand at 40°C to 60°C for 24h to 100h to obtain a flame-retardant PDOL-based polymer solid electrolyte.

4. Application of flame-retardant PDOL-based polymer solid electrolyte in solid-state batteries: Assemble the battery using the positive electrode, diaphragm and negative electrode in a glove box, inject the solid electrolyte precursor prepared in step 3 into the battery, soak it on the diaphragm, and then use a battery packaging machine to package it. Let it stand at 40℃~60℃ for 24h~100h, and obtain a solid-state battery by in-situ polymerization, wherein the amount of solid electrolyte precursor used is 2g / Ah~15g / Ah.

3. The in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte according to claim 2, characterized in that The volume ratio of the component A to the component B is (9.5:0.5-1:9).

4. The in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte according to claim 2, characterized in that The molar concentration of the component C in the precursor solution is (0.02 mol / L to 0.5 mol / L).

5. The in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte according to claim 2, characterized in that The molar concentration of the component D in the precursor solution is (0.5 mol / L to 2.5 mol / L).

6. The in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte according to claim 2, characterized in that The volume percentage of the component E in the precursor solution is (5% to 50%).

7. The in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte according to claim 2, characterized in that The mass percentages of the component F in the precursor solution are (0.5% to 5%) and (0.5% to 10%) respectively.

8. The in-situ preparation and application of a flame-retardant PDOL-based polymer solid electrolyte according to claim 2, characterized in that The diaphragm used is a PE diaphragm, a PP diaphragm, a cellulose diaphragm, a glass fiber diaphragm, a polyimide diaphragm, a polyacrylonitrile diaphragm or a PE / PP / PE composite diaphragm.

9. Application of the flame-retardant PDOL-based polymer solid electrolyte according to claim 2 in the field of solid-state batteries. 10 . The flame-retardant PDOL-based polymer solid electrolyte according to claim 2 has good flame-retardant effect. 11 . The flame-retardant PDOL-based polymer solid electrolyte solid-state battery according to claim 2 can be stably cycled at 30° C.-120° C.

Citation Information

Cited By

  • In-situ polymerization electrolyte preparation method

    CN119890432A

  • A method for the preparation of an in-situ polymerized electrolyte

    CN119890432B

  • Preparation method of intrinsic flame-retardant solid electrolyte, prepared solid electrolyte and application

    CN121790505A

  • Preparation method of flame-retardant solid electrolyte, prepared flame-retardant solid electrolyte and application

    CN121812726A

  • Preparation method of flame-retardant solid-state electrolyte, prepared flame-retardant solid-state electrolyte and application

    CN121812726B