Method for connecting nickel ferrite-based ceramic inert anode and metal conductive block

Vacuum diffusion welding technology uses transition alloy foil dielectric to connect the nickel ferrite-based ceramic inert anode and the metal conductive block, which solves the problem of difficulty in connecting the ceramic alloy and the metal conductive block, and achieves a high-strength, dense and corrosion-resistant joint, suitable for Stable operation under aluminum electrolysis conditions.

WO2024199041A1PCT designated stage expired Publication Date: 2024-10-03ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/082743
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

In the aluminum electrolysis process, it is difficult to connect the ceramic alloy inert anode to the metal conductive block, mainly due to differences in their physical and chemical properties, which lead to different melting points, difficulty in element diffusion, disparity in thermal expansion coefficients, and easy cracks in the joints, making it difficult to achieve a stable welding connection. .

Method used

Transition alloy foil is used as a medium to connect the nickel ferrite-based ceramic inert anode and the metal conductive block through vacuum diffusion welding. The low melting point alloy foil is used to form an instant liquid film, which promotes element diffusion and forms a metallurgical grade bond, reducing thermal stress. and the generation of brittle phases.

Benefits of technology

It achieves high-strength, dense, hole-free and crack-free connection joints with fast connection speed and high efficiency. It is suitable for various shapes and structures. It has high conductivity and corrosion resistance and is suitable for long-term use under aluminum electrolysis conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082743_03102024_PF_FP_ABST
    Figure CN2024082743_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to a method for connecting a nickel ferrite-based ceramic inert anode and a metal conductive block, comprising the following steps: providing a nickel ferrite-based ceramic inert anode (1) and a metal conductive block (3), and treating surfaces of the nickel ferrite-based ceramic inert anode (1) and the metal conductive block (3) to form surfaces to be connected; providing a transition alloy foil (2), and respectively attaching the surfaces to be connected of the nickel ferrite-based ceramic inert anode (1) and the metal conductive block (3) to two surfaces of the transition alloy foil (2) to form a prefabricated connector; and carrying out vacuum diffusion welding on the prefabricated connector.
Need to check novelty before this filing date? Find Prior Art

Description

A method for connecting a nickel ferrite-based ceramic inert anode and a metal conductive block

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application No. 202310298466.3 filed on March 24, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present disclosure relates to the field of aluminum electrolysis, and in particular to an aluminum electrolysis cell. Background Art

[0004] The current Hall-Herout aluminum electrolytic cell uses consumable carbon anodes, which not only consume a large amount of high-quality carbon materials and emit a large amount of greenhouse gas CO2 and carcinogenic fluorocarbons, but also require continuous replenishment of anode paste or replacement of anode carbon blocks during the aluminum electrolysis process, resulting in unstable electrolytic production and increased labor intensity.

[0005] Inert anodes and the corresponding electrolysis process have become the focus of attention and research hotspot in the international aluminum industry and materials industry because they can solve the above problems and reduce the production cost of aluminum ingots by nearly 30%. The use of inert anodes in the aluminum electrolysis process has the following advantages: (1) The electrodes are almost not consumed during the electrolysis process, and no additional carbon processing plant is required, which reduces production costs; (2) The electrodes are not consumed, the electrode spacing is stable, easy to control, the number of anode replacements is small, and labor intensity is reduced; (3) A higher anode current density can be used to increase the production capacity of the electrolytic cell; (4) The anode product is oxygen, which avoids environmental pollution. Oxygen can also be used as a by-product. It is estimated that the recovered oxygen may be 3% of the value of the original aluminum product. This series of advantages of inert anodes makes the development of suitable inert anodes an important part of improving traditional aluminum production methods. However, in the environment of aluminum electrolysis, inert anodes must be able to withstand the corrosion of electrolytes and have low solubility; be able to withstand the erosion of oxygen; have good conductivity (resistivity ≤ carbon anode); have high mechanical strength, strong thermal shock resistance, and are not easy to brittle; are easy to process and shape, and easy to connect with metal conductors; and the raw materials are easy to obtain and inexpensive. According to current research, ceramic alloy materials have the excellent electrical conductivity and processability of metal materials and the good resistance to molten salt corrosion of ceramic materials, making them the most promising inert anode materials to replace carbon anodes.

[0006] Inert anodes require a metal conductive block to provide current in order to work. However, ceramic alloy materials and metal conductive blocks have significant differences in physical and chemical properties, resulting in the following difficulties in welding: (1) Their different crystal structures lead to different melting points; (2) The strong bond energy of ceramic crystals makes it extremely difficult for elements to diffuse; (3) Their thermal expansion coefficients differ greatly, resulting in large thermal stress in the joint, which easily causes cracks on the ceramic side; (4) Brittle phases are generated on the bonding surface, which weakens the ceramic performance. Therefore, it is difficult to achieve connection using conventional fusion welding methods.

[0007] Summary of the Invention

[0008] The technical problem of difficulty in connecting an inert anode to a metal conductive block is solved by utilizing one or more embodiments of the present disclosure.

[0009] An embodiment of the present disclosure provides a method for connecting a nickel ferrite-based ceramic inert anode and a metal conductive block. The method comprises the following steps: providing a nickel ferrite-based ceramic inert anode and a metal conductive block, treating the surfaces of the nickel ferrite-based ceramic inert anode and the metal conductive block to form surfaces to be connected; providing a transition alloy foil, and laminating the surfaces to be connected of the nickel ferrite-based ceramic inert anode and the metal conductive block to two sides of the transition alloy foil, respectively, to form a prefabricated connector; and performing vacuum diffusion welding on the prefabricated connector. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present disclosure and, together with the description, serve to explain the principles of the present disclosure.

[0011] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure or related technologies, the following briefly introduces the drawings required for use in the embodiments or related technical descriptions. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0012] FIG1 is a schematic structural diagram of a prefabricated connector provided in Example 1 of the present disclosure;

[0013] FIG2 is a schematic structural diagram of a prefabricated connector provided in Example 2 of the present disclosure;

[0014] FIG3 is a schematic structural diagram of a prefabricated connector provided in Example 3 of the present disclosure. DETAILED DESCRIPTION

[0015] To make the objectives, technical solutions, and advantages of the embodiments of the present disclosure more clear, the technical solutions in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present disclosure without making any creative efforts shall fall within the scope of protection of the present disclosure.

[0016] Unless otherwise specified, the terms used herein should be understood as having the same meaning as commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs. In the event of any conflict, the present specification shall take precedence.

[0017] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present disclosure can be purchased from the market or prepared by existing methods.

[0018] Currently, there is a technical problem in the field of aluminum electrolysis that it is difficult to connect the inert anode to the metal conductive block.

[0019] The technical solutions provided by the embodiments of the present disclosure are intended to solve the above technical problems, and the overall idea is as follows:

[0020] The present disclosure provides a method for connecting a nickel ferrite-based ceramic inert anode to a metal conductive block. As shown in FIG1 to FIG3 , the method for connecting the nickel ferrite-based ceramic inert anode 1 to the metal conductive block 3 includes the following steps:

[0021] S1: providing a nickel ferrite-based ceramic inert anode 1 and a metal conductive block 3, and treating the surfaces of the nickel ferrite-based ceramic inert anode 1 and the metal conductive block 3 to form surfaces to be connected;

[0022] S2: providing a transition alloy foil 2, and laminating the surfaces to be connected of the nickel ferrite-based ceramic inert anode 1 and the metal conductive block 2 to the two sides of the transition alloy foil 2 to form a prefabricated connection body; and

[0023] S3: performing vacuum diffusion welding on the prefabricated connection body.

[0024] Those skilled in the art will appreciate that vacuum diffusion welding can be performed in a vacuum diffusion welding furnace. The melting point of the transition alloy foil 2 is lower than that of the metal conductive block 3 and the nickel ferrite-based ceramic inert anode 1, which is a general requirement for vacuum diffusion welding. By selecting a transition alloy foil 2 with a lower melting point as the interlayer, when heated to the joining temperature, the interlayer melts, forming a transient liquid film on the joining surfaces. During the insulation process, as the low-melting-point components diffuse into the metal conductive block 3 and the nickel ferrite-based ceramic inert anode 1, the thickness of the liquid film decreases until it disappears. After a certain period of insulation, the composition becomes homogenized, and the formation of a liquid phase sandwiches the transition alloy foil 2 between the joined surfaces.

[0025] As the melting-point-lowering elements in the liquid phase diffuse into the metal conductive block 3 and the nickel ferrite-based ceramic inert anode 1, some of these elements dissolve into the liquid phase, gradually raising the melting point of the liquid phase and causing it to solidify. The solidification interface advances from both sides toward the center. As the holding time increases, the liquid phase in the joint gradually decreases, ultimately forming a joint.

[0026] Transition alloy foil 2 can make the concentration gradient of liquid surface larger, promote the diffusion of elements, accelerate the disappearance of diffusion voids. Transition alloy foil 2 can also alleviate the residual stress caused by the different thermal expansion coefficients of ceramics and metals and control interface reaction, inhibit or change interface reaction products, and improve joint quality. Transition alloy foil 2 can select a combination of adhesive alloy material and reactive alloy material. Transition alloy foil 2 with suitable components can reduce diffusion welding connection temperature, time, and pressure, and improve joint performance. Adhesive alloy material is selected to be unreactive with ceramic material, but two ceramic components can diffuse with each other to form a diffusion layer. Reactive alloy material can interact with ceramic to form reaction products, and the generated reaction products are used to firmly connect ceramic and metal.

[0027] The present disclosure uses a transition alloy foil 2 as a welding medium and adopts a vacuum diffusion welding method to connect a nickel ferrite-based ceramic inert anode 1 and a metal conductive block 3 through a transient liquid phase diffusion connection method. Under the operating conditions of vacuum diffusion welding, the transition alloy foil 2 forms a transient liquid film on the bonding surface. As the components in the liquid phase diffuse with the base material, the thickness of the liquid film decreases and disappears, eventually forming a metallurgical-grade bond. The connection joint formed by this bonding method is uniform and dense, without the generation of holes and cracks, and the connection strength is ≥150MPa.

[0028] In addition, the connection speed disclosed herein is fast and the connection efficiency is high. The diffusion connection between the nickel ferrite-based ceramic inert anode 1 and the metal conductive block 3 can be completed in only 20 minutes. The connection accuracy is high and the material deformation is small. It is suitable for connecting nickel ferrite-based ceramic inert anode 1 structures of various shapes and can also be used for connecting large-sized planar nickel ferrite-based ceramic inert anode 1 structures, and has a wide applicability. The operation is simple, and the obtained connection joint has high strength, strong corrosion resistance, and good electrical conductivity. Under the conditions of aluminum electrolysis, it will not crack or fall off during long-term use.

[0029] In some embodiments of the present disclosure, the arithmetic mean deviation of the surface profile of the surface to be connected is 0.6 to 2.5×10 -4 cm.

[0030] Surface roughness has a significant impact on diffusion welding. Lower surface roughness can make parts bond more tightly under the influence of temperature and pressure, resulting in more complete diffusion and more reliable welding quality.

[0031] In some embodiments of the present disclosure, processing the surfaces of the nickel ferrite-based ceramic and the metal conductive block to form surfaces to be connected comprises the following steps:

[0032] S11: Cleaning the surfaces of the nickel ferrite-based ceramic inert anode 1 and the metal conductive block 3;

[0033] S12: Use 120#, 220#, 500#, 1000#, 1500#, 2000#, and 2500# sandpaper to polish the cleaned surface in sequence.

[0034] The purpose of sandpaper polishing the cleaned surface is to control the arithmetic mean deviation of the surface profile of the surface to be connected to 0.6~2.5×10 -4 cm.

[0035] In some embodiments of the present disclosure, the material of the transition alloy foil 2 includes Fe-Ni alloy.

[0036] In some embodiments of the present disclosure, the material of the transition alloy foil 2 further includes at least one of B, Si, V and Co.

[0037] In some embodiments of the present disclosure, the transition alloy foil 2 includes, in terms of mass percentage, the following:

[0038] In some embodiments of the present disclosure, the thickness of the transition alloy foil 2 is 5 μm-500 μm.

[0039] In some embodiments of the present disclosure, the vacuum diffusion welding:

[0040] The diffusion temperature is 950-1200°C; and / or,

[0041] The heating rate is 10-30°C / min; and / or,

[0042] The holding time is 2-20 minutes; and / or,

[0043] The pressure is 5-30 MPa; and / or,

[0044] The cooling rate is 4-8℃ / min.

[0045] The higher the temperature, the greater the diffusion coefficient, the faster the diffusion rate, and the lower the pressure required to achieve close contact between the connecting surfaces. However, excessively high temperatures can easily cause the metal conductive block 3 to melt or soften, affecting not only the material composition and surface state but also the phase transition of the intermediate layer. Therefore, the diffusion temperature is selected to be 0.6-0.8Tm, generally between 950-1200°C. Tm is the melting point of the metal conductive block.

[0046] The greater the applied pressure, the larger the close contact area, which is conducive to obtaining a good contact surface. At the same time, it can effectively fill the holes generated by the ceramic material of the nickel ferrite-based ceramic inert anode 1 at the connection interface to prevent the generation of diffusion holes. However, excessive pressure will cause macroscopic plastic deformation of the metal conductive block 3, so the diffusion pressure is 5-30MPa.

[0047] The depth of the diffusion layer is proportional to the square root of the diffusion time. The strength, plasticity, elongation and impact toughness of the diffusion joint increase to a certain extent and then tend to be stable with the holding time. Excessive high temperature and high pressure for too long will not have any effect on further improving the quality of the joint.

[0048] Due to the large difference in thermal expansion coefficients between the ceramic material of the nickel ferrite-based ceramic inert anode 1 and the metal material of the metal conductive block 3, after instantaneous diffusion bonding, the rapid cooling rate will cause a large internal stress in the joint, which in turn leads to the initiation of microcracks. After the insulation is completed, the cooling rate is controlled. When the joint is cooled at a cooling rate of 4-8°C / min, the internal stress in the joint can be effectively reduced, which is conducive to ensuring the joint performance.

[0049] The specific operation method of vacuum diffusion welding is a conventional technical means in the field. As an example, in some embodiments of the present disclosure, the specific operation method of vacuum diffusion welding is as follows:

[0050] Place the prefabricated connection body consisting of NiFe2O4-based ceramic inert anode, transition alloy foil 2, and metal conductive block 3 in a vacuum diffusion furnace, and start the mechanical pump and Roots pump respectively to effectively remove the air in the furnace. When the vacuum degree reaches 10 -3When the pressure reaches 0.1-0.9 Pa, high-purity argon or high-purity nitrogen is filled in, and the temperature is increased to 0.1-0.9 Pa. The heating rate is 10-30 ° C / min, and the temperature is heated to 950 ° C -1200 ° C. A pressure of 5-30 MPa is applied. Under this condition, the temperature is kept for 2-20 minutes, and then the temperature is cooled to 400 ° C at a rate of 4-8 ° C / min, and then the furnace is cooled to room temperature.

[0051] In some embodiments of the present disclosure, the nickel ferrite-based ceramic inert anode 1 is a sintered NiFe2O4-X ceramic inert anode or a NiFe2O4-XY metal ceramic inert anode.

[0052] In some embodiments of the present disclosure, in the NiFe2O4-X ceramic inert anode or the NiFe2O4-XY ceramic inert anode, X is a composite ceramic phase including at least one of ZnO, CuO, Cr2O3, MgO, Y2O3 and TiN.

[0053] Y is a composite metal phase including at least one of Cu, Ni, Fe, Co, Cr, Al, Mn and rare earth.

[0054] X is a composite ceramic phase, which can improve the sintering performance or densification performance of the inert anode.

[0055] Y is a composite metal phase, which can improve the corrosion resistance of the inert anode.

[0056] The present disclosure will be further described below with reference to specific examples. It should be understood that these examples are intended to illustrate the present disclosure only and are not intended to limit the scope of the present disclosure. Experimental methods in the following examples where specific conditions are not specified are generally measured in accordance with national standards. If no corresponding national standards are available, the methods were performed in accordance with commonly used international standards, conventional conditions, or conditions recommended by the manufacturer.

[0057] Example 1

[0058] The prepared NiO, Fe2O3, ZnO, Cu and Fe powders are pressed into a ceramic inert anode green body by isostatic pressing at 130 MPa, and then the ceramic inert anode green body is sintered at 1000°C in a nitrogen atmosphere to produce a nickel ferrite-based ceramic inert anode 1, wherein the oxygen content in the nitrogen atmosphere is controlled to be no more than 200 ppm; and then the metal conductive block 3 is precisely machined by mechanical processing so that its size meets the connection requirements.

[0059] Use compressed air to blow out foreign matter adhering to the surface to be connected. Then, polish it with 120#, 220#, 500#, 1000#, 1500#, 2000#, and 2500# sandpaper in sequence. Repeatedly clean the surface to be connected with alcohol to ensure that the surface to be connected between the nickel ferrite-based ceramic inert anode 1 and the metal conductive block 3 is clean and tidy. The arithmetic mean deviation of the surface profile is 1.5×10 -4 cm.

[0060] Please refer to Figure 1. The size of one end of the nickel ferrite-based ceramic inert anode 1 is smaller than the other end. The outline of one end of the processed metal conductive block 3 is completely consistent with the outline of one end of the nickel ferrite-based ceramic inert anode 1. The transition alloy foil 2 is applied to the surface to be connected between the NiFe2O4-based ceramic inert anode 1 and the metal conductive block 3 to form a prefabricated connector. The composition of the transition alloy foil 2 is Ni30%, Cr6%, B1%, Si1%, Co0.5%, V0.5%, and Fe is the balance. The thickness is 20μm. The prefabricated connector consisting of the NiFe2O4-based ceramic inert anode 1, the transition alloy foil 2, and the metal conductive block 3 is placed in a vacuum diffusion furnace. The mechanical pump and the Roots pump are turned on respectively to effectively remove the air in the furnace. When the vacuum degree reaches 10 -3 When the temperature is 1000 pa, high-purity argon or high-purity nitrogen is filled to 0.3 Pa, the heating rate is 12 ° C / min, heated to 1020 ° C, and a pressure of 6 MPa is applied. Under this condition, it is kept warm for 5 minutes, and then cooled to 400 ° C at a rate of 6 ° C / min, and then the furnace is cooled to room temperature. The connected nickel ferrite-based ceramic inert anode 1 is reassembled with a metal conductive block 3 of a certain length by threaded connection or welding to complete the overall connection of the inert anode. This structure is electrolytic at a temperature of 800 ° C and a current density of 10A / cm 2 It can operate stably for a long time under the following conditions.

[0061] Example 2

[0062] The prepared NiO, Fe2O3, MgO, Cu, Fe and Ni powders are pressed into a ceramic inert anode green body by isostatic pressing at 130 MPa. The ceramic inert anode green body is then sintered at 1000°C in a nitrogen atmosphere to produce a nickel ferrite-based ceramic inert anode 1, wherein the oxygen content in the nitrogen atmosphere is controlled to be no higher than 200 ppm. The metal conductive block 3 is then precisely machined to meet the connection requirements. Compressed air is used to blow away foreign matter adhering to the surface to be connected. The surface is then polished using 120#, 220#, 500#, 1000#, 1500#, 2000# and 2500# sandpaper in sequence. The surface to be connected is then repeatedly cleaned with alcohol to ensure that the surface to be connected between the nickel ferrite-based ceramic inert anode 1 and the metal conductive block 3 is clean and tidy, with an arithmetic mean deviation of the surface profile of 1.2×10 -4cm.

[0063] Please refer to Figure 2. One end of the nickel ferrite-based ceramic inert anode 1 has a groove, and the contour of one end of the processed metal conductive block 3 is completely consistent with the contour of the groove. The transition alloy foil 2 is applied to the surface to be connected between the NiFe2O4-based ceramic inert anode 1 and the metal conductive block 3 to form a prefabricated connector. The composition of the transition alloy foil 2 is Ni26%, Cr8%, B1.2%, Si1.5%, Co1.0%, V0.8%, and Fe is the balance. The thickness is 30μm. The prefabricated connector consisting of the NiFe2O4-based ceramic inert anode 1, the transition alloy foil 2, and the metal conductive block 3 is placed in a vacuum diffusion furnace. The mechanical pump and the Roots pump are turned on respectively to effectively remove the air in the furnace. When the vacuum degree reaches 10 -3 When the temperature is 0.5 pa, high-purity argon or high-purity nitrogen is filled to 0.3 pa, the heating rate is 10 ° C / min, heated to 1050 ° C, and a pressure of 8 MPa is applied. Under this condition, it is kept warm for 10 minutes, and then cooled to 400 ° C at a rate of 6 ° C / min, and then the furnace is cooled to room temperature. The connected nickel ferrite-based ceramic inert anode 1 is reassembled with a metal conductive block 3 of a certain length by threaded connection or welding to complete the overall connection of the inert anode. This structure is electrolytic at a temperature of 850 ° C and a current density of 10A / cm 2 It can operate stably for a long time under the following conditions.

[0064] Example 3

[0065] The prepared NiO, Fe2O3, Y2O3, Fe, Ni, and Co powders are pressed into a ceramic inert anode green body by isostatic pressing at 130 MPa. The ceramic inert anode green body is then sintered at 1000°C in a nitrogen atmosphere to produce a nickel ferrite-based ceramic inert anode 1, wherein the oxygen content in the nitrogen atmosphere is controlled to be no more than 200 ppm. The metal conductive block 3 is then precisely machined to meet the connection requirements. Compressed air is used to blow away foreign matter adhering to the surface to be connected. The surface is then polished using 120#, 220#, 500#, 1000#, 1500#, 2000#, and 2500# sandpaper in sequence. The surface to be connected is then repeatedly cleaned with alcohol to ensure that the surface to be connected between the nickel ferrite-based ceramic inert anode 1 and the metal conductive block 3 is clean and tidy, with an arithmetic mean deviation of the surface profile of 1.8×10 -4 cm.

[0066] Please refer to Figure 3. The size of one end of the nickel ferrite-based ceramic inert anode 1 is equal to the size of the other end. The outline of one end of the processed metal conductive block 3 is completely consistent with the outline of one end of the nickel ferrite-based ceramic inert anode 1. A transition alloy foil 2 is applied to the surface to be connected between the NiFe2O4-based ceramic inert anode and the metal conductive block 3 to form a prefabricated connector. The composition of the transition alloy foil 2 is Ni20%, Cr10%, B1.5%, Si2%, Co0.5%, V0.5%, and Fe is the balance. The thickness is 50μm. The prefabricated connector consisting of the NiFe2O4-based ceramic inert anode, the transition alloy foil 2, and the metal conductive block 3 is placed in a vacuum diffusion furnace. The mechanical pump and the Roots pump are turned on respectively to effectively remove the air in the furnace. When the vacuum degree reaches 10 -3 When the pressure reaches 0.5 Pa, high-purity argon or high-purity nitrogen is filled to 0.5 Pa, the heating rate is 12 ° C / min, heated to 1100 ° C, and a pressure of 10 MPa is applied. Under this condition, it is kept warm for 15 minutes, and then cooled to 400 ° C at a rate of 6 ° C / min, and then the furnace is cooled to room temperature. The connected nickel ferrite-based ceramic inert anode 1 is reassembled with a metal conductive block 3 of a certain length by threaded connection or welding to complete the overall connection of the inert anode. This structure is electrolytic at a temperature of 800 ° C and a current density of 10A / cm 2 It can operate stably for a long time under the following conditions.

[0067] Various embodiments of the present disclosure may be presented in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of the present disclosure; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numbers within the range. For example, the description of a range from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0068] In this disclosure, unless otherwise stated, directional terms such as "upper" and "lower" refer specifically to the directions of the drawings in the accompanying drawings. In addition, in the description of this disclosure, the terms "include", "comprise", etc. mean "including but not limited to". Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the phrase "include..." do not exclude the presence of other identical elements in the process, method, article or device comprising the elements. In this document, relational terms such as "first" and "second" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. In this document, "and / or" describes the association relationship of associated objects, indicating that three relationships can exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. For the association relationship of more than three associated objects described with "and / or", it means that any one of these three associated objects can exist alone, or any at least two of them exist at the same time. For example, for A, and / or B, and / or C, it can be represented that any one of A, B, and C exists alone, or any two of them exist at the same time, or three of them exist at the same time. In this article, "at least one" refers to one or more, and "multiple" refers to two or more. "At least one", "the following at least one (individual)" or similar expressions refer to any combination of these items, including any combination of single item (individual) or plural items (individual). For example, "at least one (individual) of a, b, or c", or "at least one (individual) of a, b, and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc or abc, where a, b, c can be single or multiple, respectively.

[0069] The foregoing description is intended only to provide specific embodiments of the present disclosure, intended to enable those skilled in the art to understand and implement the present disclosure. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present disclosure. Therefore, the present disclosure is not to be limited to the embodiments shown herein, but is to be construed in the broadest manner consistent with the principles and novel features claimed herein.

Claims

1. A method for connecting a nickel ferrite-based ceramic inert anode to a metal conductive block, comprising the following steps: Providing a nickel ferrite-based ceramic inert anode and a metal conductive block, and treating the surfaces of the nickel ferrite-based ceramic inert anode and the metal conductive block to form a surface to be connected; Providing a transition alloy foil, laminating the nickel ferrite-based ceramic inert anode and the metal conductive block to be connected to the two sides of the transition alloy foil to form a prefabricated connection body ; as well as, Performing vacuum diffusion welding on the prefabricated connector; Measured in terms of mass percentage of the transition alloy foil, the transition alloy foil comprises: B:0.01%~2%, Si: 0.05-5%, V:0.01%~2%, Co: 0.1-5%, Ni: 20-30%, The balance is Fe; The diffusion temperature of the vacuum diffusion welding is 950-1200° C., the heating rate is 10-30° C. / min, the heat preservation time is 2-20 min, the pressure is 5-30 MPa, and the cooling rate is 4-8° C. / min.

2. The method for connecting the nickel ferrite-based ceramic inert anode and the metal conductive block according to claim 1, in, The arithmetic mean deviation of the surface profile of the surface to be connected is 0.6 to 2.5×10 -4 cm.

3. The method for connecting the nickel ferrite-based ceramic inert anode and the metal conductive block according to claim 2, in, The surfaces of the nickel ferrite-based ceramic inert anode and the metal conductive block are processed to form surfaces to be connected, comprising the following steps: Cleaning the surfaces of the nickel ferrite-based ceramic inert anode and the metal conductive block; Use 120#, 220#, 500#, 1000#, 1500#, 2000#, and 2500# sandpaper to polish the cleaned surface in turn.

4. The method for connecting the nickel ferrite-based ceramic inert anode and the metal conductive block according to claim 1, in, The thickness of the transition alloy foil is 5 μm-500 μm.

5. The method for connecting the nickel ferrite-based ceramic inert anode and the metal conductive block according to claim 1, in, The nickel ferrite-based ceramic inert anode is a sintered NiFe 2 O 4 -X ceramic inert anode or NiFe 2 O 4 -One of the XY metal ceramic inert anodes.

6. The method for connecting the nickel ferrite-based ceramic inert anode and the metal conductive block according to claim 5, in, The NiFe 2 O 4 -X ceramic inert anode or NiFe 2 O 4 -XY ceramic inert anode, X is a composite ceramic phase, including ZnO, CuO, Cr 2 O 3 ,MgO,Y 2 O 3 and at least one of TiN, Y is a composite metal phase, including at least one of Cu, Ni, Fe, Co, Cr, Al, Mn and rare earth.

Citation Information

Patent Citations

  • Method for connecting ceramic-base inert anode used for aluminum electrolysis and metal conducting bar

    CN101168846A

  • Metal and ceramic welding device and method

    CN107520556A

  • Method for connecting metal ceramic inert anode for aluminum electrolysis with metal conducting rod

    CN108330508A

  • Metal ceramic-based inert anode and conductive rod connecting structure for aluminum electrolysis and preparation method thereof

    CN108396335A

  • Method for connecting nickel ferrite-based ceramic inert anode and metal conductive block

    CN116396094A