Adhesive-attached metal substrate, and laminate
The adhesive-attached metal base material with a smooth copper foil and specific adhesive composition ensures strong adhesion and low dielectric properties, addressing transmission loss and peeling issues in high-frequency copper clad laminates.
Patent Information
- Application Number
- PCT/IB2024/052629
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-07
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-03
AI Technical Summary
High-frequency copper clad laminates face challenges in achieving low transmission loss due to the skin effect, which is exacerbated by the need for smooth metal foils that compromise adhesive strength between resin and metal layers, leading to potential circuit peeling issues.
An adhesive-attached metal base material with a copper foil surface roughness of 1.5 μm or less, utilizing a polyimide resin and maleimide compound adhesive composition with a radical initiator, and a specific thickness range for the adhesive resin layer, ensuring strong adhesion and low dielectric properties, is used in conjunction with prepregs to form a laminate.
The solution provides excellent transmission characteristics and sufficient adhesive strength, reducing transmission loss and preventing circuit peeling, while maintaining low dielectric properties even at high frequencies.
Smart Images

Figure IB2024052629_03102024_PF_FP_ABST
Abstract
Description
Adhesive-backed metal substrate and laminate
[0001] The present invention relates to adhesive-backed metal substrates and laminates.
[0002] Copper clad laminates (hereinafter, sometimes referred to as "CCL") used for transmitting high frequency signals are manufactured by laminating copper foil and a resin layer.
[0003] In recent years, with the increasing speed of transmission signals, further improvements in transmission characteristics are required of CCLs.
[0004] For example, Patent Document 1 discloses a laminate in which a resin substrate and a metal substrate are laminated via an adhesive layer. The adhesive layer of the laminate disclosed in Patent Document 1 is in a low frequency band relative to the 5G frequency band, but has a relative permittivity of 3.0 or less and a dielectric loss tangent of 0.02 or less at a frequency of 1 MHz.
[0005] Japanese Patent Application Publication No. 2021-003886
[0006] In high-frequency transmission, the current tends to flow only on the surface of the metal wiring as the frequency band increases. Therefore, if the surface shape is not smooth, transmission loss increases. This is a well-known phenomenon called the "skin effect." To reduce transmission loss due to the skin effect, for example, metal foils with small surface roughness tend to be used as metal substrates.
[0007] The lower the surface roughness of the metal foil, the less effective the anchoring effect becomes, and the lower the adhesion between the resin substrate and the metal foil becomes, which can lead to the problem of circuit peeling occurring on printed circuit boards.
[0008] The present invention has been made in view of the above circumstances, and aims to provide an adhesive-backed metal substrate and a laminate that have excellent transmission characteristics and can ensure sufficient adhesive strength between a resin substrate and a metal layer.
[0009] That is, the present invention employs the following configurations. [1] An adhesive-backed metal substrate comprising a metal layer and an adhesive resin layer formed from an adhesive resin composition, wherein the metal layer has a surface roughness Rzjis of 1.5 μm or less, the adhesive resin composition contains a polyimide resin (A), a maleimide compound (B), and a radical initiator, the mass ratio of the polyimide resin (A) to the maleimide compound (B) is 10:1 to 3:2, and the content of the radical initiator is 1 part by mass or more and less than 25 parts by mass per 100 parts by mass of the maleimide compound (B). [2] The adhesive-backed metal substrate according to [1], wherein the metal layer is a copper foil having a surface roughness Rzjis of less than 1.0 μm. [3] A laminate comprising the adhesive-backed metal substrate according to [1] or [2] on both sides of a prepreg, wherein the prepreg is laminated on the side opposite to the side where the adhesive resin layer of the adhesive-backed metal substrate contacts the metal layer, and the prepreg is one or more selected from the group consisting of modified polyimide resin prepreg, polyester resin prepreg, liquid crystal polymer prepreg, cyclic olefin resin prepreg, polyphenylene ether resin prepreg, polyphenylene sulfide resin prepreg, polyether ether ketone resin prepreg, bismaleimide resin prepreg, triazine resin prepreg, bismaleimide-triazine resin prepreg, benzocyclobutene resin prepreg, and low dielectric epoxy resin prepreg. [4] An adhesive-backed metal substrate comprising a metal layer and an adhesive resin layer formed from an adhesive resin composition, wherein the adhesive resin composition comprises a polyimide resin (A), a maleimide compound (B), and a radical initiator, the mass ratio of the polyimide resin (A) to the maleimide compound (B) is 10:1 to 3:2, the content of the radical initiator is 1 part by mass or more and less than 25 parts by mass per 100 parts by mass of the maleimide compound (B), and the adhesive resin layer has a thickness of 0.2 μm or more and 9 μm or less. [5] An adhesive-backed metal substrate according to [4], wherein the metal layer is a copper foil having a surface roughness Rzjis of 1.0 μm or less.[6] A laminate comprising the adhesive-backed metal substrate according to [4] or [5] on both sides of a prepreg, wherein the prepreg is laminated on the side opposite to the side where the adhesive resin layer of the adhesive-backed metal substrate contacts the metal layer, and the prepreg is one or more selected from the group consisting of modified polyimide resin prepreg, polyester resin prepreg, liquid crystal polymer prepreg, cyclic olefin resin prepreg, polyphenylene ether resin prepreg, polyphenylene sulfide resin prepreg, polyether ether ketone resin prepreg, bismaleimide resin prepreg, triazine resin prepreg, bismaleimide-triazine resin prepreg, benzocyclobutene resin prepreg, and low dielectric epoxy resin prepreg. [7] The laminate according to [6], wherein the adhesive resin layer has a thickness of 0.2 μm or more and 9 μm or less, the prepreg has a thickness of 50 μm or more and 1000 μm or less, and the metal layer has a thickness of 1 μm or more and 35 μm or less, and the following mathematical formula (1) is satisfied: 0.05≦(X / Y)×100≦7 (1) [In mathematical formula (1), X is the thickness (μm) of the adhesive resin layer, and Y is the thickness (μm) of the prepreg.]
[0010] According to the present invention, it is possible to provide an adhesive-backed metal substrate and a laminate that have excellent transmission characteristics and can ensure sufficient adhesive strength between the resin substrate and the metal layer.
[0011] 1 is a cross-sectional view of an example of an adhesive-backed metal substrate of the present embodiment. 2 is a cross-sectional view of an example of a laminate of the present embodiment. 3 is a diagram showing the results of measuring the transmission loss (dB / 100 mm) of the laminates of Example 21, Comparative Example 21, and Comparative Example 22.
[0012] <Adhesive-Backed Metal Substrate> The adhesive-backed metal substrate of the present invention includes the adhesive-backed metal substrate X according to the first embodiment and the adhesive-backed metal substrate Y according to the second embodiment.
[0013] <<Adhesive-Backed Metal Substrate X (First Embodiment)>> The adhesive-backed metal substrate X according to the first embodiment comprises a metal layer and an adhesive resin layer formed from an adhesive resin composition, wherein the metal layer has a surface roughness Rzjis of 1.5 μm or less, the adhesive resin composition contains a polyimide resin (A), a maleimide compound (B), and a radical initiator, the mass ratio of the polyimide resin (A) to the maleimide compound (B) is 10:1 to 3:2, and the content of the radical initiator is 1 part by mass or more and less than 25 parts by mass per 100 parts by mass of the maleimide compound (B).
[0014] 1 shows a schematic cross-sectional view of an adhesive-backed metal substrate 1 of this embodiment. The adhesive-backed metal substrate 1 comprises a metal layer 10 and an adhesive resin layer 11.
[0015] A rigid substrate for high-speed transmission can be manufactured by combining the adhesive-backed metal substrate 1 with any low-dielectric substrate and thermally laminating them. For example, a rigid substrate can be manufactured by using a prepreg made of polyphenylene ether resin as the low-dielectric substrate.
[0016] (Metal Layer 10) Any known conductive material that can be used for circuit boards can be used for the metal layer 10. Specifically, metal materials such as SUS, copper, aluminum, iron, steel, zinc, and nickel, and alloys of the above metal materials are included.
[0017] The metal layer 10 is preferably a metal foil having a surface roughness of 1.5 μm or less, more preferably a metal foil having a surface roughness of 1.4 μm or less, even more preferably a metal foil having a surface roughness of 1.3 μm or less, even more preferably a metal foil having a surface roughness of 1.0 μm or less, and particularly preferably a metal foil having a surface roughness of less than 1.0 μm. The metal layer 10 is preferably a copper foil having a surface roughness of 1.5 μm or less, more preferably a copper foil having a surface roughness of 1.4 μm or less, even more preferably a copper foil having a surface roughness of 1.3 μm or less, even more preferably a copper foil having a surface roughness of 1.0 μm or less, and particularly preferably a copper foil having a surface roughness of less than 1.0 μm.
[0018] The surface roughness in this specification refers to the ten-point average roughness (Rzjis). The surface roughness of a metal foil, such as a copper foil, can be measured using a surface roughness measuring instrument (model: SURFCOM 1900DX) manufactured by Tokyo Seimitsu Co., Ltd.
[0019] When the metal layer 10 is a copper foil, a rolled copper foil or an electrolytic copper foil can be used.
[0020] Furthermore, the material of the copper foil may be pure copper or a copper alloy in which a small amount of tin (Sn) or silver (Ag) is added to pure copper.
[0021] The thickness of the metal layer 10 is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. The thickness of the metal layer 10 is preferably 50 μm or less, more preferably 45 μm or less, and even more preferably 40 μm or less. The above upper and lower limit values for the thickness of the metal layer 10 can be combined arbitrarily. For example, the thickness of the metal layer 10 is 5 μm or more and 50 μm or less, 10 μm or more and 45 μm or less, or 15 μm or more and 40 μm or less.
[0022] (Adhesive Resin Layer 11) The adhesive resin layer 11 is formed from an adhesive resin composition described below. The adhesive-backed metal substrate 1 allows the metal layer 10 to be bonded to any low-dielectric substrate via the adhesive resin layer 11. The thickness of the adhesive resin layer 11 included in the adhesive-backed metal substrate 1 is preferably 0.2 μm or more, more preferably 0.5 μm or more, even more preferably 0.6 μm or more, even more preferably 0.7 μm or more, particularly preferably 1.0 μm or more, and most preferably 1.2 μm or more. The thickness of the adhesive resin layer 11 is preferably 9 μm or less, more preferably 8 μm or less, even more preferably 7 μm or less, even more preferably 5 μm or less, particularly preferably 4.8 μm or less, and most preferably 4.6 μm or less. The above upper and lower limits of the thickness of the adhesive resin layer 11 can be combined arbitrarily, and for example, the thickness of the adhesive resin layer 11 is 0.2 μm or more and 9 μm or less, 0.5 μm or more and 8 μm or less, or 0.7 μm or more and 7 μm or less.
[0023] When the thickness of the adhesive resin layer 11 is equal to or greater than the above-mentioned lower limit, the metal layer 10 and the low-dielectric substrate can be bonded together. When the thickness of the adhesive resin layer 11 is equal to or less than the above-mentioned upper limit, the adhesive resin layer 11 has a low residual solvent ratio, and delamination due to volatilized gases during the heating process is less likely to occur.
[0024] (Adhesive Resin Composition) Hereinafter, a description will be given of an adhesive resin composition for forming the adhesive resin layer 11. In this embodiment, by forming the adhesive resin layer 11 using a specific adhesive resin composition, it is possible to provide an adhesive-backed metal substrate and a laminate that can exhibit low dielectric properties in the high frequency region of 10 GHz, which is a frequency band of 6 GHz or higher assuming 5 G.
[0025] The specific adhesive resin composition described below contains a specific amount of a maleimide compound, which is one component of the precursor of the polyimide resin (A), and is therefore believed to result in an adhesive resin layer 11 that exhibits low dielectric properties in the high-frequency range. The maleimide groups of the maleimide compound maintain a cyclic structure even after crosslinking, and crosslinking between maleimide groups results in a symmetrical structure. In this case, molecular motion is likely to be suppressed, and the resulting adhesive resin layer 11 is believed to exhibit low dielectric properties in the high-frequency range.
[0026] The adhesive resin composition includes a polyimide resin (A), a maleimide compound (B), and a radical initiator. As the adhesive resin composition, the resin composition disclosed in WO 2022 / 004583 can be used. Specific examples are described below.
[0027] [Polyimide resin (A)] The polyimide resin (A) is an isocyanate-modified polyimide resin (A1) or a terminal-modified isocyanate-modified polyimide resin (A2). Hereinafter, the isocyanate-modified polyimide resin (A1) will be referred to as "polyimide resin (A1)," and the terminal-modified isocyanate-modified polyimide resin (A2) will be referred to as "polyimide resin (A2)."
[0028] Polyimide Resin (A1) The polyimide resin (A1) is obtained by reacting a diisocyanate compound (a) with an intermediate polyimide resin. Hereinafter, the diisocyanate compound (a) will be referred to as "component (a)."
[0029] The intermediate polyimide resin is a reaction product of an aliphatic diamino compound (b) (hereinafter referred to as "component (b)"), a tetrabasic acid dianhydride (c) (hereinafter referred to as "component (c)"), and an aromatic diamino compound (d) (hereinafter referred to as "component (d)").
[0030] The polyimide resin (A1) is a reaction product of either or both of an amino group and an acid anhydride group present at both ends of the intermediate polyimide resin with an isocyanate group present in the component (a).
[0031] The reaction between the intermediate polyimide resin and component (a) is a copolymerization reaction between an amino group or an acid anhydride group at the terminal of the intermediate polyimide resin and an isocyanate group in component (a). That is, the reaction between the amino group and the isocyanate group forms a urea bond, and the reaction between the acid anhydride and the isocyanate group forms an imide bond.
[0032] The amount of component (a) used in the copolymerization reaction of the intermediate polyimide resin with component (a) is preferably less than 1 equivalent of the isocyanate group of component (a) relative to 1 equivalent of the terminal functional group of the intermediate polyimide resin, more preferably 0.50 to 0.99 equivalents, and even more preferably 0.67 to 0.98 equivalents.
[0033] By using the component (a) in an amount within the above range relative to the intermediate polyimide resin, the polyimide resin (A1) can be sufficiently polymerized, and the residual proportion of unreacted raw materials can be reduced, improving the properties of the adhesive resin composition after curing, such as heat resistance and flexibility.
[0034] The terminal functional group equivalent of the intermediate polyimide resin referred to here means a value calculated from the amounts of each raw material used when synthesizing the intermediate polyimide resin.
[0035] The component (a) used in the synthesis of the polyimide resin (A1) can be any compound having two isocyanate groups in the molecule, and multiple diisocyanate compounds can be reacted simultaneously.
[0036] As the component (a), phenylene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, tridenediisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, allylene sulfone ether diisocyanate, allyl cyanide diisocyanate, N-acyl diisocyanate, trimethylhexamethylene diisocyanate, 1,3-bis(isocyanate methyl)cyclohexane or norbornane-diisocyanate methyl is preferred.Among them, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate or isophorone diisocyanate are more preferred, as they have an excellent balance of flexibility, adhesiveness, etc.
[0037] The reaction of the intermediate polyimide resin with the component (a) may be carried out by a known synthesis method. Specifically, the polyimide resin (A1) can be obtained by adding the component (a) to a solution of the intermediate polyimide resin obtained by the synthesis method described below, and heating and stirring the mixture at a temperature of 80° C. or higher and 150° C. or lower.
[0038] The reaction time for the synthesis reaction of the intermediate polyimide resin and the reaction of the intermediate polyimide resin with component (a) is greatly affected by the reaction temperature, but it is preferable to carry out the reaction until the increase in viscosity accompanying the progress of the reaction reaches equilibrium and the maximum molecular weight is obtained, which is usually several tens of minutes to 10 hours.
[0039] The intermediate polyimide resin solution obtained above can be poured into a poor solvent such as water, methanol, or hexane to separate the resulting polymer, and then a solid content of polyimide resin (A1) can be obtained by a reprecipitation method.
[0040] Polyimide Resin (A2) The polyimide resin (A2) has either or both of an amino group and an acid anhydride group at both ends, and therefore, the ends can be modified by reacting it with a compound having one functional group reactive with these functional groups to prepare a terminally modified isocyanate-modified polyimide resin, i.e., polyimide resin (A2).
[0041] Examples of compounds that can react with either or both of an amino group and an acid anhydride group include compounds having an acid anhydride group such as maleic anhydride, compounds having an alcoholic hydroxyl group such as hydroxyethyl acrylate, compounds having a phenolic hydroxyl group such as phenol, compounds having an isocyanate group such as 2-methacryloyloxyethyl isocyanate, and compounds having an epoxy group such as glycidyl methacrylate.
[0042] By modifying the terminals, both terminals of the isocyanate compound of the present invention can be converted to functional groups other than amino groups and acid anhydride groups (for example, when terminal modification is performed with hydroxyethyl acrylate, the terminals of the isocyanate-modified polyimide resin can be converted to acryloyl groups). Therefore, it is also possible to prepare a composition in which the isocyanate compound is combined with a compound that reacts with functional groups other than amino groups or acid anhydride groups.
[0043] Intermediate Polyimide Resin The intermediate polyimide resin is a reaction product of the above-mentioned components (b), (c), and (d). The reaction of components (b), (c), and (d) includes two steps: obtaining a polyamic acid through a copolymerization reaction between the amino groups in components (b) and (d) and the acid anhydride groups in component (c), and obtaining an intermediate polyimide resin through a dehydration cyclization reaction (imidization reaction) of the polyamic acid. These two steps may be performed separately, but it is more efficient to perform them continuously in one go.
[0044] When the number of moles of component (b) used in the copolymerization reaction is defined as MB, the number of moles of component (c) as MC, and the number of moles of component (d) as MD, if the relationship MB + MD > MC is satisfied, both terminals of the resulting intermediate polyimide resin will be amino groups, and if the relationship MB + MD < MC is satisfied, both terminals of the resulting intermediate polyimide resin will be acid anhydride groups.
[0045] Furthermore, when the relationship MB+MD=MC is satisfied, the resulting intermediate polyimide resin theoretically has an infinite molecular weight and has one amino group and one acid anhydride group at each end.
[0046] An example of the amount of component (b) used in the copolymerization reaction is preferably an amount in the range of 10% by mass or more and 50% by mass or less of the mass obtained by subtracting the mass of water generated in the dehydration cyclization reaction step during the synthesis of the intermediate polyimide resin from the sum of the masses of components (b), (c), and (d) used in the synthesis step of the intermediate polyimide resin and the mass of component (a) used in the synthesis step of the polyimide resin (A1) described above (this mass is substantially equal to the mass of the isocyanate-modified polyimide resin finally obtained).
[0047] If the amount of component (b) is below the above range, the proportion of aliphatic chains derived from component (b) in the intermediate polyimide resin will be too small, resulting in a high dielectric constant and dielectric loss tangent. If the amount of component (b) is above the above range, the proportion of aliphatic chains derived from component (b) in the intermediate polyimide resin will be too large, resulting in a low heat resistance of the cured product.
[0048] The component (b) used in the synthesis of the intermediate polyimide resin is not particularly limited as long as it is an aliphatic compound having two amino groups in one molecule, but an aliphatic diamino compound having 6 to 36 carbon atoms is preferred.
[0049] Specific examples of component (b) include hexamethylenediamine, 1,3-bis(aminomethyl)cyclohexane, C14 branched diamine, C18 branched diamine, dimer diamine, and diaminopolysiloxane, etc. These may be used alone or in combination of two or more.
[0050] The dimer diamine described as a specific example of component (b) in this specification is a compound in which the two carboxy groups of a dimer acid, which is a dimer of an unsaturated fatty acid such as oleic acid, have been substituted with primary amino groups (see, for example, JP-A-9-012712).
[0051] Specific examples of commercially available dimer diamines include PRIAMINE 1074 and PRIAMINE 1075 (both manufactured by Croda Japan Co., Ltd.) and VERSAMINE 551 (both manufactured by Cognis Japan Co., Ltd.) These may be used alone or in combination of two or more.
[0052] The component (c) used in the synthesis of the intermediate polyimide resin is not particularly limited as long as it has two acid anhydride groups in one molecule.
[0053] Specific examples of the component (c) include pyromellitic anhydride, ethylene glycol bis(anhydrotrimellitate), glycerin bis(anhydrotrimellitate) monoacetate, 1,2,3,4-butanetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylethertetracarboxylic dianhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3- Examples include methylcyclohexene-1,2-dicarboxylic anhydride, 3a,4,5,9b-tetrahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-1,3-dione, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, bicyclo(2,2,2)-oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic dianhydride, and 5,5′-((propane-2,2-diylbis(4,1-phenylene))bis(oxy))bis(isobenzofuran-1,3-dione).
[0054] Among these, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 3,3',4,4'-diphenylethertetracarboxylic dianhydride are preferred in terms of solvent solubility, adhesion to substrates, and photosensitivity. These may be used alone or in combination of two or more.
[0055] The component (c) used in the synthesis of the intermediate polyimide resin preferably contains at least one compound selected from the group consisting of the following chemical formulas (1) to (4).
[0056]
[0057] In the chemical formula (4), Y is C(CF3 ) 2 , S.O. 2 , CO, O, a direct bond, or a divalent linking group represented by the following chemical formula (5): The two linking moieties represented by chemical formula (5) are each a moiety that bonds to phthalic anhydride.
[0058]
[0059] The component (d) used in the synthesis of the intermediate polyimide resin is not particularly limited as long as it is an aromatic compound having two amino groups in one molecule.
[0060] Specific examples of the component (d) include m-phenylenediamine, p-phenylenediamine, m-tolylenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl thioether, 3,3'-dimethyl-4,4'-diaminodiphenyl thioether, 3,3'-diethoxy-4,4'-diaminodiphenyl thioether, and 3,3 4,4'-diaminodiphenylthioether, 4,4'-diaminobenzophenone, 3,3'-dimethyl-4,4'-diaminobenzophenone, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-dimethoxy-4,4'-diaminodiphenylthioether, 2,2'-bis(3-aminophenyl)propane, 2,2'-bis(4-aminophenyl)propane, 4,4'-diaminodi Phenyl sulfoxide, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, benzidine, 3,3'-dimethylbenzidine, 3,3'-dimethoxybenzidine, 3,3'-diaminobiphenyl, p-xylylenediamine, m-xylylenediamine, o-xylylenediamine, 2,2'-bis(3-aminophenoxyphenyl)propane, 2,2'-bis(4-aminophenoxyphenyl)propane, 1,3-bis(4- Examples of suitable bis(4-amino-3-methylphenyl)methane include 1,3'-bis(3-aminophenoxyphenyl)benzene, 1,3'-bis(3-aminophenoxyphenyl)propane, bis(4-amino-3-methylphenyl)methane, bis(4-amino-3,5-dimethylphenyl)methane, bis(4-amino-3-ethylphenyl)methane, bis(4-amino-3,5-diethylphenyl)methane, bis(4-amino-3-propylphenyl)methane, and bis(4-amino-3,5-dipropylphenyl)methane. These may be used alone or in combination of two or more.
[0061] The component (d) used in the synthesis of the intermediate polyimide resin preferably contains at least one compound selected from the group consisting of the following chemical formulas (6) and (8).
[0062]
[0063] In chemical formula (6), R 1 represents a methyl group or a trifluoromethyl group, and in the chemical formula (8), Z represents CH(CH 3 ), SO 2 , C.H. 2 , O-C 6 H 4 represents —O, O, a direct bond, or a divalent linking group represented by the above chemical formula (5); R 3 represents a hydrogen atom, a methyl group, an ethyl group, or a trifluoromethyl group. The two linking moieties represented by chemical formula (5) are each a moiety that binds to phthalic anhydride.
[0064] The intermediate polyimide resin can be synthesized by known methods. For example, a solvent, a dehydrating agent, and a catalyst are added to a mixture of components (b) to (d) used for synthesis, and the mixture is heated and stirred at 100 to 300°C under an inert gas atmosphere such as nitrogen. This causes an imidization reaction (a ring-closing reaction accompanied by dehydration) via polyamic acid, yielding an intermediate polyimide resin solution. During this process, water generated during imidization is distilled out of the system, and after the reaction is complete, the dehydrating agent and catalyst are also distilled out of the system, allowing for the production of a highly pure intermediate polyimide resin without the need for washing. Examples of dehydrating agents include toluene and xylene, and examples of catalysts include pyridine and triethylamine.
[0065] Examples of solvents that can be used in the synthesis of the intermediate polyimide resin include methyl ethyl ketone, methyl propyl ketone, methyl isopropyl ketone, methyl butyl ketone, methyl isobutyl ketone, methyl n-hexyl ketone, diethyl ketone, diisopropyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, methylcyclohexanone, acetylacetone, γ-butyrolactone, diacetone alcohol, cyclohexen-1-one, dipropyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, tetrahydropyran, ethyl isoamyl ether, ethyl t-butyl ether, ethyl benzyl ether, cresyl methyl ether, anisole, phenetole, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, and the like. Examples of suitable esters include, but are not limited to, propyl, butyl acetate, isobutyl acetate, amyl acetate, isoamyl acetate, 2-ethylhexyl acetate, cyclohexyl acetate, methylcyclohexyl acetate, benzyl acetate, methyl acetoacetate, ethyl acetoacetate, methyl propionate, ethyl propionate, butyl propionate, benzyl propionate, methyl butyrate, ethyl butyrate, isopropyl butyrate, butyl butyrate, isoamyl butyrate, methyl lactate, ethyl lactate, butyl lactate, ethyl isovalerate, isoamyl isovalerate, diethyl oxalate, dibutyl oxalate, methyl benzoate, ethyl benzoate, propyl benzoate, methyl salicylate, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide. These may be used alone or in combination of two or more.
[0066] [Maleimide Compound (B)] The maleimide compound (B) is not particularly limited as long as it is a compound having one or more maleimide groups in one molecule, but a compound having two or more maleimide groups in one molecule is preferred, and examples thereof include polyfunctional maleimide compounds obtained by reacting 3,4,4′-triaminodiphenylmethane, triaminophenol, or the like with maleic anhydride, maleimide compounds obtained by reacting tris-(4-aminophenyl)-phosphate, tris(4-aminophenyl)-phosphate, or tris(4-aminophenyl)-thiophosphate with maleic anhydride, trismaleimide compounds such as tris(4-maleimidephenyl)methane, bis(3,4-dimaleimidephenyl)methane, tetrahydrofuran ... Examples of such maleimide compounds include maleimide compounds such as maleimide obtained by reacting maleimide with maleic anhydride, tetramaleimide benzophenone, tetramaleimide naphthalene, and triethylenetetramine with maleic anhydride, phenol novolac-type maleimide resins, isopropylidenebis(phenoxyphenylmaleimide)phenylmaleimide aralkyl resins, and biphenylene-type phenylmaleimide aralkyl resins. Commercially available products include MIR-3000 and MIR-5000 (all manufactured by Nippon Kayaku Co., Ltd.), BMI-70 and BMI-80 (all manufactured by K.I. Kasei Co., Ltd.), BMI-1000, BMI-2000 and BMI-3000 (all manufactured by Daiwa Kasei Kogyo Co., Ltd.), etc.
[0067] Since maleimide compounds undergo self-crosslinking between maleimide groups due to the action of a radical initiator, a resin composition using an isocyanate-modified polyimide resin having amino groups at its terminals, a maleimide compound, and a radical initiator undergoes self-crosslinking of the maleimide groups upon heating, and becomes a cured product in which the polyimide resin and the maleimide resin are copolymerized.
[0068] [Radical initiator] Radical initiators that can be used for self-crosslinking between maleimide groups include peroxides such as dicumyl peroxide and dibutyl peroxide, and azo compounds such as 2,2'-azobis(isobutyronitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile).
[0069] The mass ratio of the polyimide resin (A) to the maleimide compound (B) in the adhesive resin composition used in this embodiment is 10:1 to 3:2, preferably 7:1 to 5:2. When the mass ratio of the polyimide resin (A) to the maleimide compound (B) is within the above range, an adhesive-attached metal substrate or laminate exhibits low dielectric properties in the high-frequency range. Furthermore, the adhesive easily adheres to metal foils with a low surface roughness of 1.5 μm or less, and exhibits high adhesive strength.
[0070] The content of the radical initiator in the adhesive resin composition used in this embodiment is 1 part by mass or more but less than 25 parts by mass, and preferably 5 parts by mass or more and 20 parts by mass or less, per 100 parts by mass of the maleimide compound (B). When the content of the radical initiator satisfies the above range, an adhesive-attached metal substrate or laminate can be obtained that can ensure sufficient adhesive strength between the resin film and the metal layer. In particular, it is easy to adhere even to metal foil with a low surface roughness of 1.5 μm or less, and is likely to exhibit high adhesive strength.
[0071] The adhesive resin composition used in this embodiment may contain an organic solvent. Specific examples of the organic solvent include amide-based solvents such as γ-butyrolactones, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and N,N-dimethylimidazolidinone, sulfones such as tetramethylene sulfone, ether-based solvents such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether monoacetate, and propylene glycol monobutyl ether, ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone, and aromatic solvents such as toluene and xylene.
[0072] The organic solvent is used in such a proportion that the solids concentration in the adhesive resin composition excluding the organic solvent is usually 5% by mass or more and 80% by mass or less, and preferably 10% by mass or more and 70% by mass or less.
[0073] The adhesive resin composition can be produced by adding a base agent containing a polyimide resin (A) and a maleimide compound (B) to an organic solvent, and further adding a radical initiator.
[0074] <Laminate> The laminate of this embodiment comprises an adhesive-backed metal substrate of this embodiment on both sides of a prepreg. Figure 2 shows a schematic cross-sectional view of a laminate 2 of this embodiment. The laminate 2 comprises an adhesive-backed metal substrate 1 on both sides of a prepreg 12. The prepreg 12 is laminated on the surface 11a opposite to the surface where the adhesive resin layer 11 of the adhesive-backed metal substrate 1 contacts the metal layer 10. That is, the laminate 2 comprises the metal layer 10 / adhesive resin layer 11 / prepreg 12 / adhesive resin layer 11 / metal layer 10 laminated in this order.
[0075] (Prepreg) The prepreg 12 is preferably at least one selected from the group consisting of modified polyimide resin prepreg, polyester resin prepreg, liquid crystal polymer prepreg, cyclic olefin resin prepreg, polyphenylene ether resin prepreg, polyphenylene sulfide resin prepreg, polyether ether ketone resin prepreg, bismaleimide resin prepreg, triazine resin prepreg, bismaleimide-triazine resin prepreg, benzocyclobutene resin prepreg, and low dielectric epoxy resin prepreg.
[0076] In addition, in the laminate 2 including the adhesive-backed metal substrate X according to the first embodiment, it is preferable that the thickness of the adhesive resin layer 11 is 0.2 μm or more and 9 μm or less, and the thickness of the metal layer 10 is 5 μm or more and 50 μm or less.
[0077] An example of the laminate 2 is a copper clad laminate.
[0078] <<Adhesive-backed metal substrate Y (second embodiment)>> The adhesive-backed metal substrate X according to the first embodiment described above has a surface roughness Rzjis of 1.5 μm or less of the metal layer provided on the adhesive-backed metal substrate, but the adhesive-backed metal substrate Y according to the second embodiment is characterized in that the thickness of the adhesive resin layer provided on the adhesive-backed metal substrate is 0.2 μm or more and 9 μm or less.
[0079] Specifically, the adhesive-backed metal substrate Y according to the second embodiment comprises a metal layer and an adhesive resin layer formed from an adhesive resin composition, the adhesive resin composition containing a polyimide resin (A), a maleimide compound (B), and a radical initiator, the mass ratio of the polyimide resin (A) to the maleimide compound (B) is 10:1 to 3:2, the content of the radical initiator is 1 part by mass or more and less than 25 parts by mass per 100 parts by mass of the maleimide compound (B), and the thickness of the adhesive resin layer is 0.2 μm or more and 9 μm or less.
[0080] As explained above, the adhesive-backed metal substrate Y according to the second embodiment is the same as the adhesive-backed metal substrate X according to the first embodiment except that the thickness of the adhesive resin layer is within a specific range, and detailed explanation thereof will be omitted. However, in the laminate 2 including the adhesive-backed metal substrate Y according to the second embodiment, it is preferable that the thickness of the adhesive resin layer 11 is 0.2 μm or more and 9 μm or less, the thickness of the metal layer 10 is 1 μm or more and 35 μm or less, and the thickness of the prepreg is 50 μm or more and 1000 μm or less.
[0081] Furthermore, the laminate 2 including the adhesive-backed metal substrate Y according to the second embodiment preferably satisfies the following formula (1): 0.01≦(X / Y)×100≦7 (1) (In formula (1), X is the thickness (μm) of the adhesive resin layer, and Y is the thickness (μm) of the prepreg.)
[0082] The above formula (1) is preferably any one of the following formulas (1)-1 to (1)-3: 0.05≦(X / Y)×100≦7 (1)-1 0.2≦(X / Y)×100≦6.5 (1)-2 0.4≦(X / Y)×100≦6 (1)-3
[0083] The present invention will be explained in more detail below using examples, but the present invention is not limited to these examples.
[0084] <<Adhesive-Coated Metal Substrate X and Laminate Thereof>> <Preparation of Adhesive Resin Composition> A polyimide resin (A) and a maleimide compound (B) were mixed at a mass ratio of 4:1 to form a base material, and the base material was dissolved in anisole. Next, 17 parts by mass of dicumyl peroxide (manufactured by Sigma-Aldrich) was added to 100 parts by mass of the maleimide compound (B), and the mixture was diluted with an organic solvent (anisole:toluene=9:1) to prepare adhesive resin composition 1 having a solids concentration of 11% by mass.
[0085] <Production of adhesive-backed metal substrate X> (Example 1) The adhesive resin composition 1 obtained was applied as a metal layer to an electrolytic copper foil (CF-T9DA-SV, manufactured by Fukuda Metal Foil & Powder Co., Ltd.) having a surface roughness Rzjis of 0.85 μm and a thickness of 18 μm using a bar coater so that the adhesive resin layer would have a thickness of 6 μm after drying, and the resultant was dried at 140° C. for 1 minute until the residual solvent content was 1%, thereby producing the adhesive-backed metal substrate of Example 1.
[0086] Comparative Example 1 An adhesive-backed metal substrate of Comparative Example 1 was produced in the same manner as in Example 1, except that the metal layer was changed to an electrolytic copper foil (CF-T4X-SV-9, manufactured by Fukuda Metal Foil & Powder Co., Ltd.) having a surface roughness Rzjis of 1.6 μm and a thickness of 9 μm.
[0087] Reference Example 1 An electrolytic copper foil (CF-T4X-SV-18, manufactured by Fukuda Metal Foil & Powder Co., Ltd.) having a surface roughness Rzjis of 1.0 μm and a thickness of 18 μm was used as Reference Example 1.
[0088] Reference Example 2 An electrolytic copper foil (CF-T9DA-SV, manufactured by Fukuda Metal Foil & Powder Co., Ltd.) having a surface roughness Rzjis of 0.85 μm and a thickness of 18 μm was used as Reference Example 2.
[0089] Reference Example 3 An electrolytic copper foil (HS1-VSP, manufactured by Mitsui Mining & Smelting Co., Ltd.) having a surface roughness Rzjis of 1.5 μm and a thickness of 18 μm was used as Reference Example 3.
[0090] <Production of Laminate> (Types of Prepregs) Five types of polyphenylene ether resin prepregs and two types of bismaleimide-triazine resin prepregs were used. Hereinafter, polyphenylene ether resin prepregs will be referred to as "PPE-based prepregs" and bismaleimide-triazine resin prepregs will be referred to as "BT-based prepregs."
[0091] (PPE-based prepregs) PPE-based prepreg 1 (PPE1): Meteorwave (registered trademark) 4000 manufactured by AGC Inc., thickness: 110.3 μm PPE-based prepreg 2 (PPE2): MEGTRON (registered trademark) 4 manufactured by Panasonic Industries Co., Ltd., thickness: 100.5 μm PPE-based prepreg 3 (PPE3): MEGTRON (registered trademark) 6 manufactured by Panasonic Industries Co., Ltd., thickness: 130.3 μm PPE-based prepreg 4 (PPE4): MEGTRON (registered trademark) 7 manufactured by Panasonic Industries Co., Ltd., thickness: 140.5 μm PPE-based prepreg 5 (PPE5): Commercially available prepreg with a relative permittivity of 3.6 and a dielectric dissipation factor of 0.0041 at 10 GHz, thickness: 100 μm
[0092] (BT-based prepreg) BT-based prepreg 1 (BT1): manufactured by AGC Inc., N5000, thickness: 30 μm BT-based prepreg 2 (BT2): manufactured by Mitsubishi Gas Chemical Company, Inc., GHPL-970LF, thickness: 45 μm
[0093] The adhesive-backed metal substrates of Example 1 and Comparative Example 1 were laminated on both sides of each prepreg in the following order: copper foil (metal layer) / adhesive resin layer / prepreg / adhesive resin layer / copper foil (metal layer). When the metal substrates of Reference Examples 1 and 2 were used, the layers were laminated in the following order: copper foil (metal layer) / prepreg / copper foil (metal layer). The lamination conditions varied depending on the type of prepreg, and lamination was performed under the conditions shown in Table 1 below.
[0094]
[0095] In this way, laminates 1A to 1D, 2A to 2D, 3A to 3D, 4A to 4D, 5A, 5D, 6A to 6D, and 7A to 7D were produced.
[0096] <Adhesive Strength Measurement> The adhesive strength between the copper foil (metal layer) and the prepreg of the resulting laminate was measured. The resulting laminate was cut to a width of 10 mm to create a test piece, and the prepreg side was attached to a ring core with a diameter of 11 cm. A 90° peel test was performed by pulling the copper foil (metal layer) at a rate of 50 mm / min. In this measurement, an adhesive strength of 0.60 N / mm or more (3.4 lbs / inch or more) was evaluated as "sufficient adhesive strength." The adhesive strengths of the produced laminates are listed in Table 2. Note that, as an index of adhesive strength between the prepreg and the metal layer, an adhesive strength of 0.60 N / mm or more (3.4 lbs / inch or more) is required to prevent peeling of the metal layer during the manufacturing process. Therefore, an adhesive strength of 0.60 N / mm or more (3.4 lbs / inch or more) was considered a pass value.
[0097] <Soldering heat resistance> The produced laminate was left in a thermostatic chamber at a temperature of 23°C and a humidity of 50% for 24 hours, and then floated in a solder bath at 288°C. The time until deformation or bubbling occurred was measured to evaluate heat resistance. The results are shown in Table 2. A laminate that did not undergo deformation or bubbling for 300 seconds was evaluated as passing.
[0098] <Measurement of Dielectric Properties> The copper foil (metal layer) was removed from the obtained laminate by etching, and test pieces (50 mm wide, 100 mm long) were prepared in which the adhesive resin layer / prepreg / adhesive resin layer were laminated in this order. The test pieces were dried at 135°C for 1 hour and used as "dried" test pieces. Furthermore, the test pieces were left to stand for 24 hours after drying under conditions of 23°C and 50% humidity and used as "humidity-conditioned" test pieces, and the dielectric properties of each were measured.
[0099] The dielectric properties were measured by using a resonator manufactured by QWED Inc., and the relative permittivity and dielectric loss tangent were measured at a frequency of 10 GHz by the split post dielectric resonator method.
[0100] Table 2 shows the type of adhesive-backed metal substrate, type of prepreg, adhesive strength, solder heat resistance, and dielectric properties for laminates 1A to 1D, 2A to 2D, 3A to 3D, 4A to 4D, 5A to 5D, 6A to 6D, and 7A to 7D.
[0101]
[0102] As shown in Table 2, when comparing Reference Examples 1 and 2 with Example 1 for each laminate, Example 1 had higher adhesive strength than Reference Examples 1 and 2. Furthermore, when comparing Example 1 with Comparative Example 1 for each laminate, Example 1 had better adhesive strength and transmission characteristics than Comparative Example 1.
[0103] <<Adhesive-Coated Metal Substrate Y and Laminate Thereof>> <Preparation of Adhesive Resin Composition> A polyimide resin (A) and a maleimide compound (B) were mixed at a mass ratio of 4:1 to form a base material, which was then dissolved in anisole. Next, 17 parts by mass of dicumyl peroxide (manufactured by Sigma-Aldrich) was added to 100 parts by mass of the maleimide compound (B), and the mixture was diluted with an organic solvent (anisole:toluene = 9:1) to prepare adhesive resin composition 2 with an adjusted solid content. The solid content was adjusted to the following concentrations depending on the thickness of the adhesive resin layer. ・Adhesive resin layer thickness of 1 to 6 μm: The solid content was adjusted to 11% by mass and applied using a bar coater. ・Adhesive resin layer thickness of more than 10 μm: The solid content was adjusted to 11% by mass and applied using an applicator. ・Adhesive resin layer thickness of less than 0.1 μm: The solid content was adjusted to 1% by mass and applied using a bar coater.
[0104] <Production of adhesive-backed metal substrate Y> (Example 11) The adhesive resin composition 2 obtained was applied as a metal layer to an electrolytic copper foil (CF-T9DA-SV, manufactured by Fukuda Metal Foil & Powder Co., Ltd.) having a surface roughness Rzjis of 0.85 μm and a thickness of 18 μm, using an applicator or a bar coater, so that the adhesive resin layer would have a thickness of 6 μm after drying, and then dried at 140° C. for 1 minute until the residual solvent content was 1%, thereby producing the adhesive-backed metal substrate of Example 11.
[0105] (Examples 12 to 16, Comparative Examples 11 to 12) Adhesive-backed metal substrates of Examples 12 to 16 and Comparative Examples 11 and 12 were produced in the same manner as in Example 11, except that the thickness of the adhesive resin layer was changed to the thickness shown in Table 3 below.
[0106]
[0107] <Evaluation of Processability> The processability was evaluated by evaluating the residual solvent rate and the processing speed.
[0108] (Residual Solvent Ratio) Adhesive resin layers of the same thickness as those in Examples 11 and 13 and Comparative Example 11 were formed on polyimide sheets and dried at 120°C for 10 minutes, after which the residual organic solvent ratio was measured. TG / DTA was used for the measurement. The results are shown in Table 3. As shown in Table 3, Comparative Example 11, in which the adhesive resin layer was 10.0 μm thick, had a high residual solvent ratio of 0.85%. If the residual solvent ratio is high, gas will evaporate from the adhesive resin layer during the heating process, causing delamination. On the other hand, Examples 11 and 13, in which the adhesive resin layer was 6.0 μm or 3.0 μm thick, had a low residual solvent ratio, indicating a low possibility of delamination due to gas generation.
[0109] (Processing Speed) A coater test was conducted simulating an adhesive coating process in which copper foil was in a rolled state. The processing speed was measured under the same drying conditions (drying oven (8 zones, 1 m each) set at 70-140°C) to obtain the same residual solvent content (0.7% or less). Changing the drying conditions to a higher temperature or longer time to reduce the residual solvent content was not performed because this would hinder the curing reaction. Therefore, to reduce the residual solvent content of the adhesive resin layer to be formed, drying was performed at a slower processing speed. However, an excessively slow processing speed is not preferred because it reduces productivity. As shown in Table 4, when the adhesive resin layer thickness is 1.5-6 μm, processing is possible at a processing speed of approximately 3-5 m / min, allowing productivity to be maintained. On the other hand, when the adhesive resin layer thickness is 9 μm, the processing speed is 1 m / min, raising concerns about reduced productivity.
[0110]
[0111] Reference Example 11 An electrolytic copper foil (CF-T9DA-SV, manufactured by Fukuda Metal Foil & Powder Co., Ltd.) having a surface roughness Rzjis of 0.85 μm and a thickness of 18 μm was used as Reference Example 11.
[0112] Reference Example 12 An electrolytic copper foil (HS1-VSP, manufactured by Mitsui Mining & Smelting Co., Ltd.) having a surface roughness Rzjis of 1.5 μm and a thickness of 18 μm was used as Reference Example 12.
[0113] <Production of Laminate> (Types of Prepregs) Four types of polyphenylene ether resin prepregs were used. The polyphenylene ether resin prepregs are referred to as "PPE-based prepregs."
[0114] (PPE-based prepregs) PPE-based prepreg 11 (PPE11): Meteorwave (registered trademark) 4000 manufactured by AGC Inc., thickness: 110.3 μm PPE-based prepreg 12 (PPE12): MEGTRON (registered trademark) 6 manufactured by Panasonic Industries Co., Ltd., thickness: 130.3 μm PPE-based prepreg 13 (PPE13): MEGTRON (registered trademark) 7 manufactured by Panasonic Industries Co., Ltd., thickness: 140.5 μm PPE-based prepreg 14 (PPE14): Commercially available prepreg with a relative permittivity of 3.6 and a dielectric dissipation factor of 0.0041 at 10 GHz, thickness: 100 μm
[0115] The adhesive-backed metal substrates of Examples 11 to 16 and Comparative Examples 11 and 12 were laminated on both sides of each prepreg in the order copper foil (metal layer) / adhesive resin layer / prepreg / adhesive resin layer / copper foil (metal layer). When the metal substrate of Reference Example 11 was used, the layers were laminated in the order copper foil (metal layer) / prepreg / copper foil (metal layer). The lamination conditions varied depending on the type of prepreg, and lamination was performed under the conditions shown in Table 5 below.
[0116]
[0117] In this way, laminates 11A to 11I, 12A to 12I, and 13A to 13I were manufactured.
[0118] <Adhesive Strength Measurement> The adhesive strength between the copper foil (metal layer) and the prepreg of the resulting laminate was measured. The resulting laminate was cut to a width of 10 mm to prepare a test piece. The prepreg side was attached to a ring core with a diameter of 11 cm, and a 90° peel test was performed by pulling the copper foil (metal layer) at a rate of 50 mm / min. In this measurement, an adhesive strength of 0.60 N / mm or more (3.4 lbs / inch or more) was evaluated as "sufficient adhesive strength." The adhesive strength of the produced laminate is listed in Table 5. Note that, as an index of adhesive strength between the prepreg and the metal layer, an adhesive strength of 0.60 N / mm or more (3.4 lbs / inch or more) is required to prevent peeling of the metal layer during the manufacturing process. Therefore, an adhesive strength of 0.60 N / mm or more (3.4 lbs / inch or more) was considered a pass value.
[0119] <Soldering heat resistance> The manufactured laminate was left in a thermostatic chamber at a temperature of 23°C and a humidity of 50% for 24 hours, and then floated in a solder bath at 288°C. The time until deformation or bubbling occurred was measured to evaluate heat resistance. The results are shown in Tables 6 to 8. A sample that did not undergo deformation or bubbling for 300 seconds was evaluated as passing.
[0120] <Measurement of Dielectric Properties> The copper foil (metal layer) was removed from the obtained laminate by etching, and test pieces (50 mm wide, 100 mm long) were prepared in which the adhesive resin layer / prepreg / adhesive resin layer were laminated in this order. The test pieces were dried at 135°C for 1 hour and used as "dried" test pieces. Furthermore, the test pieces were left to stand for 24 hours after drying under conditions of 23°C and 50% humidity and used as "humidity-conditioned" test pieces, and the dielectric properties of each were measured.
[0121] The dielectric properties were measured by using a resonator manufactured by QWED Inc., and the relative permittivity and dielectric loss tangent were measured at a frequency of 10 GHz by the split post dielectric resonator method.
[0122] For laminates 11A to 11I, 12A to 12I, and 13A to 13I, the type of adhesive-backed metal substrate, the type of prepreg, adhesive strength, solder heat resistance, X / Y (X is the thickness (μm) of the adhesive resin layer, and Y is the thickness (μm) of the prepreg), and dielectric properties are shown in Tables 6 to 8.
[0123]
[0124]
[0125]
[0126] As shown in Tables 6 to 8, when comparing Reference Example 11 with each Example in each laminate, the Example had a higher adhesive strength than Reference Example 11. Furthermore, when comparing Example 11 with Comparative Example 11 in each laminate, the adhesive strength was equivalent. Since delamination was a concern in Comparative Example 11, in which the adhesive resin layer had a film thickness of 10.0 μm, based on the evaluation results of the processing speed, the advantage of setting the adhesive resin layer thickness to 0.2 μm or more and 9 μm or less was confirmed. Furthermore, when comparing Example 11 with Comparative Example 12 in each laminate, the adhesive strength of Comparative Example 12 was either NG or lower than that of the Examples.
[0127] Furthermore, in the laminate, when the dielectric properties of the prepreg are poorer than those of the adhesive resin layer, comparing the Examples and Comparative Example 11, it is expected that the transmission loss of Comparative Example 11 will be better than that of the Examples. However, when the dielectric properties of the prepreg are better than those of the adhesive resin layer, it is expected that the thicker adhesive resin layer will affect the transmission loss, and therefore, taking other performance properties into consideration, the thickness of the adhesive resin layer is preferably 9 μm or less.
[0128] Furthermore, when Example 11 and Reference Example 11 are compared, Reference Example 11 was evaluated as "NG" in adhesive strength, and the Example had a lower dielectric constant than Reference Example 11. Therefore, it was confirmed that the Example had better adhesive strength and transmission characteristics than Reference Example 11.
[0129] <Measurement of Transmission Characteristics> Laminates of Example 21, Comparative Example 21, and Comparative Example 22 shown in Table 9 below were produced.
[0130]
[0131] The transmission loss (dB / 100 mm) was measured for the laminates of Example 21, Comparative Example 21, and Comparative Example 22 using the following equipment. The results are shown in FIG.
[0132] [Equipment] KEISIGHT TECHNOLOGIES, Inc. 10MHz-67GHz: Network analyzer PNA series N5227B 55GHz-95GHz: Frequency extender for WR12 signal analyzer N9029AV12
[0133] As shown in Figure 3, Example 21 had lower transmission loss than Comparative Examples 21 and 22, even at high frequencies. Furthermore, as shown in Table 9, Example 21 also had high adhesive strength. On the other hand, Comparative Example 21 had a high surface roughness Rzjis of 1.5 µm, so although adhesive strength was exhibited, the transmission loss increased as the frequency increased. Comparative Example 22 had a surface roughness Rzjis of 0.85 µm, so although the transmission loss was lower than Comparative Example 21, the absence of an adhesive resin layer resulted in lower adhesive strength.
[0134] 1: adhesive-attached metal substrate, 2: laminate, 10: metal layer, 11: adhesive resin layer, 12: prepreg
Claims
An adhesive-coated metal substrate comprising a metal layer and an adhesive resin layer formed from an adhesive resin composition, The metal layer has a surface roughness Rzjis of 1.5 μm or less, The adhesive resin composition comprises a polyimide resin (A), a maleimide compound (B), and a radical initiator, a mass ratio of the polyimide resin (A) to the maleimide compound (B) is 10:1 to 3:2; The adhesive-attached metal substrate, wherein the content of the radical initiator is 1 part by mass or more and less than 25 parts by mass per 100 parts by mass of the maleimide compound (B). The adhesive-backed metal substrate according to claim 1 , wherein the metal layer is a copper foil having a surface roughness Rzjis of less than 1.0 μm. A laminate comprising the adhesive-backed metal substrate according to claim 1 or 2 on both sides of a prepreg, The prepreg is laminated on a surface of the adhesive-bonded metal substrate opposite to a surface in contact with the metal layer, The prepreg is at least one selected from the group consisting of modified polyimide resin prepregs, polyester resin prepregs, liquid crystal polymer prepregs, cyclic olefin resin prepregs, polyphenylene ether resin prepregs, polyphenylene sulfide resin prepregs, polyether ether ketone resin prepregs, bismaleimide resin prepregs, triazine resin prepregs, bismaleimide-triazine resin prepregs, benzocyclobutene resin prepregs, and low dielectric epoxy resin prepregs. An adhesive-coated metal substrate comprising a metal layer and an adhesive resin layer formed from an adhesive resin composition, The adhesive resin composition comprises a polyimide resin (A), a maleimide compound (B), and a radical initiator, a mass ratio of the polyimide resin (A) to the maleimide compound (B) is 10:1 to 3:2; the content of the radical initiator is 1 part by mass or more and less than 25 parts by mass with respect to 100 parts by mass of the maleimide compound (B), The adhesive-coated metal substrate, wherein the adhesive resin layer has a thickness of 0.2 μm or more and 9 μm or less.
5. The adhesive-backed metal substrate according to claim 4, wherein the metal layer is a copper foil having a surface roughness Rzjis of 1.0 μm or less. A laminate comprising the adhesive-backed metal substrate according to claim 4 or 5 on both sides of a prepreg, The prepreg is laminated on a surface of the adhesive-bonded metal substrate opposite to a surface in contact with the metal layer, The prepreg is at least one selected from the group consisting of modified polyimide resin prepregs, polyester resin prepregs, liquid crystal polymer prepregs, cyclic olefin resin prepregs, polyphenylene ether resin prepregs, polyphenylene sulfide resin prepregs, polyether ether ketone resin prepregs, bismaleimide resin prepregs, triazine resin prepregs, bismaleimide-triazine resin prepregs, benzocyclobutene resin prepregs, and low dielectric epoxy resin prepregs. The adhesive resin layer has a thickness of 0.2 μm or more and 9 μm or less, The thickness of the prepreg is 50 μm or more and 1000 μm or less, The thickness of the metal layer is 1 μm or more and 35 μm or less, The laminate according to claim 6 , which satisfies the following formula (1). 0.05≦(X / Y)×100≦7...(1) [In formula (1), X is the thickness (μm) of the adhesive resin layer, and Y is the thickness (μm) of the prepreg.]
Citation Information
Patent Citations
Polyamide resin originated from dimer diamine and optical material made of synthetic resin containing the polyamide
JP1997012712A
Low dielectric fire-resistant adhesive composition
JP2021003886A
Polyimide resin, resin composition containing the polyimide resin and cured product of the same
JP2023039241A
Polyimide resin composition and cured product of the same
JP2023068801A
Metal substrate with adhesive, and laminate
JP2023147328A