Magnetic material and magnet, and method for manufacturing rapidly-solidified alloy, magnetic material and magnet

By adding specific metal elements and Carbon to Sm-Fe-N magnetic materials, the formation of undesirable phases is suppressed, leading to enhanced magnetic properties and squareness ratio, addressing the degradation issues in Sm-Fe-N magnetic materials and enabling their use in advanced electromagnetic devices.

WO2024202236A1PCT designated stage expired Publication Date: 2024-10-03MURATA MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/042387
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2023-11-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Sm-Fe-N magnetic materials face challenges in maintaining good magnetic properties, particularly squareness ratio, due to the precipitation of unwanted phases such as Fe-Zr or Fe-M2, which degrade their performance.

Method used

Incorporating specific combinations of metal elements like Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W, along with Carbon (C), to promote the precipitation of a non-magnetic M1-M2-C phase, suppressing the formation of detrimental Fe-M1 or Fe-M2 phases and enhancing the magnetic properties.

Benefits of technology

The approach results in Sm-Fe-N magnetic materials with improved magnetic properties and squareness ratio, suitable for various electromagnetic applications, including miniaturization and high-temperature reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023042387_03102024_PF_FP_ABST
    Figure JP2023042387_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present disclosure is to provide an Sm-Fe-N magnetic material having good magnetic characteristics. An Sm-Fe-N magnetic material according to the present disclosure comprises: M1 which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo and W; M2 which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo and W and is different from the M1; and C.
Need to check novelty before this filing date? Find Prior Art

Description

Magnetic material and magnet, and method for manufacturing rapidly solidified alloy, magnetic material and magnet

[0001] The present disclosure relates to magnetic materials and magnets and methods of manufacturing rapidly solidified alloys, magnetic materials, and magnets.

[0002] Rare earth magnets have high magnetic flux density and can be made into extremely powerful permanent magnets, and are used in a variety of applications. Sm—Fe—N magnets are known as one type of rare earth magnet. Sm—Fe—N magnets are typically produced by nitriding Sm—Fe polycrystals. When N atoms dissolve in the crystal lattice of Sm—Fe polycrystals, the lattice becomes distorted, resulting in the development of uniaxial magnetic anisotropy, and the resulting Sm—Fe—N magnetic material is thought to be able to function as a hard magnetic material.

[0003] As such an Sm-Fe-N magnetic material, Patent Document 1 discloses that a flake-shaped isotropic Sm-Fe-N powder magnet material is produced by nitriding a powder of a magnet alloy obtained by a roll quenching method, and the content of the powder is, in atomic %, Sm x Fe 100-x-v N v , Sm x Fe 100-x-y-v M 1 y N v Or, Sm x Fe 100-x-z-v M 2 z N v (In the formula, M 1 is Hf or Zr. M 2 is one or more elements selected from Si, Nb, Ti, Ga, Al, Ta, and C. 7≦x≦12, 0.5≦v≦20, 0.1≦y≦1.5, and 0.1≦z≦1.0), has a TbCu type crystal structure, and has a flake thickness of 10 to 30 μm.

[0004] Patent Document 2 describes a Sm—Fe—N based magnetic material whose composition expressed in atomic percent is Sm x R a Fe100-xy-z-aM y N z(wherein R is at least one of Zr and Hf, M is at least one of Co, Ti, Nb, Cr, V, Mo, Si, Ga, Ni, Mn, and Al, x+a is 7% to 10%, a is 0% to 1.5%, y is 0% to 5%, and z is 10% to 14%).

[0005] JP 2002-57017 A JP 2018-157197 A

[0006] Patent Document 1 describes the use of one type of metal element in addition to Sm, Fe, and N in an Sm—Fe—N based magnetic material, and Patent Document 2 describes the use of two types of metal elements in addition to Sm, Fe, and N in an Sm—Fe—N based magnetic material. As a result of investigations by the present inventors, it was found that, while the addition of a metal element in addition to Sm and Fe can improve the magnetic properties, a heterogeneous phase consisting of Fe and the added element also newly precipitates, and this heterogeneous phase may degrade the magnetic properties of the resulting Sm—Fe—N based magnetic material.

[0007] The present disclosure aims to provide an Sm—Fe—N based magnetic material having good magnetic properties, particularly squareness ratio, and a method for producing the same. The present disclosure also aims to provide a magnet including the Sm—Fe—N based magnetic material and a method for producing the same.

[0008] The Sm—Fe—N based magnetic material of the present disclosure includes: M1, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W; M2, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W and is different from M1; and C.

[0009] The present disclosure can provide an Sm—Fe—N based magnetic material with good magnetic properties, particularly squareness ratio, and a method for producing the same. The present disclosure can also provide a magnet including the Sm—Fe—N based magnetic material and a method for producing the same.

[0010] 1 shows the results of STEM-EDX analysis of the Sm—Fe—N magnetic material obtained in Example 1, where DF-I is a dark-field image, and Fe, Zr, Nb, and C are mapping images (element distribution images) showing the concentration distribution of each element. 1 shows the results of STEM-EDX analysis of the Sm—Fe—N magnetic material obtained in Comparative Example 1, where DF-I is a dark-field image, and Fe, Zr, and C are mapping images (element distribution images) showing the concentration distribution of each element. 1 shows the results of STEM-EDX analysis of the Sm—Fe—N magnetic material obtained in Comparative Example 2, where DF-I is a dark-field image, and Fe, Nb, and C are mapping images (element distribution images) showing the concentration distribution of each element. 1 is a schematic diagram showing the concentration distributions of Fe, M1, M2, and C in the Sm—Fe—N magnetic material in one aspect of embodiment 1.

[0011] (Embodiment 1: Sm—Fe—N-based magnetic material) Hereinafter, a Sm—Fe—N-based magnetic material according to one embodiment of the present disclosure will be described in detail, but the present disclosure is not limited to this embodiment.

[0012] The Sm—Fe—N based magnetic material of the present disclosure includes: M1, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W; M2, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W and is different from M1; and C.

[0013] The Sm—Fe—N magnetic material of the present disclosure has the above-described structure, and therefore has excellent magnetic properties, particularly excellent squareness ratio. Although not limited to a specific theory, the reason why the Sm—Fe—N magnetic material of the present disclosure exhibits the above-described effects is thought to be as follows.

[0014] That is, it is believed that adding a metal element, such as Zr, to an Sm—Fe—N magnetic material can promote amorphization during the manufacturing process of the Sm—Fe—N magnetic material, and that in the final Sm—Fe—N magnetic material, the main phase precipitates finely and uniformly, improving the magnetic properties. However, it is believed that adding a metal element such as Zr precipitates, for example, a heterogeneous phase of Fe—Zr, which reduces the magnetic properties, particularly the squareness ratio. In such cases, a method has been investigated in which the Fe—Zr heterogeneous phase is made less likely to be precipitated by further adding C to precipitate a nonmagnetic phase of Zr—C, but it has not been possible to sufficiently reduce the Fe—Zr heterogeneous phase.

[0015] In contrast, when M1, M2 and C are further added, it is believed that the main phase precipitates finely and uniformly, and the non-magnetic M1-M2-C phase precipitates preferentially. As a result, it is believed that the precipitation of the Fe-M1 and Fe-M2 phases is suppressed, and a Sm-Fe-N magnetic material with good magnetic properties, particularly good squareness ratio, can be obtained.

[0016] The Sm—Fe—N magnetic material includes M1, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W, and M2, which is one element different from M1 and is selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W. These elements are metal elements of Groups 4 to 6, and all are transition metal elements. For unknown reasons, the inclusion of both M1 and M2 allows the precipitation of an M1-M2-C phase, suppressing the precipitation of a heterogeneous phase of Fe-M1 or Fe-M2, resulting in an Sm—Fe—N magnetic material with good magnetic properties, particularly squareness ratio.

[0017] In a preferred embodiment, M1 is an element selected from Zr, Ti, Hf, V, Nb, and Ta, and M2 is an element selected from Zr, Ti, Hf, V, Nb, and Ta, and may be an atom different from M1.

[0018] In a more preferred embodiment, M1 is one element selected from Zr, Hf, V, Nb, and Ta, and M2 is one element selected from Zr, Hf, V, Nb, and Ta, and is different from M1.

[0019] The ratio of the content of M1 to the content of M2 (M1:M2) may be, on an atomic percent basis, preferably 2:8 to 8:2, more preferably 3:7 to 7:3, and even more preferably 4:6 to 6:4. When the content ratio of M1 to M2 is within this range, precipitation of the Fe-M1-M2 phase can be promoted, and the squareness ratio of the Sm-Fe-N magnetic material can be improved.

[0020] The total content of M1 and M2 in the Sm—Fe—N magnetic material is preferably 1.6 atomic % to 5.0 atomic %, more preferably 1.8 atomic % to 4.0 atomic %, and even more preferably 2.0 atomic % to 3.5 atomic %, based on 100 atomic % of the total elements contained in the Sm—Fe—N magnetic material. When the total content of M1 and M2 is within this range, the squareness ratio of the Sm—Fe—N magnetic material can be improved.

[0021] The Sm—Fe—N based magnetic material contains C. By containing C, a nonmagnetic M1-M2-C phase is precipitated, and the magnetic properties, particularly the squareness ratio, of the Sm—Fe—N based magnetic material can be improved.

[0022] In the Sm—Fe—N magnetic material, the C content is preferably more than 0 atomic % and not more than 2.5 atomic %, more preferably 0.1 atomic % to 2.3 atomic %, and even more preferably 0.1 atomic % to 2.2 atomic %, based on the total of 100 atomic % of the elements contained in the Sm—Fe—N magnetic material. When the C content in the Sm—Fe—N magnetic material is within the above range, the squareness ratio of the Sm—Fe—N magnetic material can be improved.

[0023] In the Sm—Fe—N magnetic material, the Sm content is preferably 7.0 atomic % or more and 11.0 atomic % or less, more preferably 7.5 atomic % or more and 10.5 atomic % or less, and more preferably 7.5 atomic % or more and 10.0 atomic % or less, based on a total of 100 atomic % of the elements contained in the Sm—Fe—N magnetic material. When the Sm content in the Sm—Fe—N magnetic powder is within this range, the squareness ratio of the Sm—Fe—N magnetic material can be further improved.

[0024] In the Sm—Fe—N magnetic material, the Fe content is preferably 69.5 atomic % or more and 82.0 atomic % or less, more preferably 70.0 atomic % or more and 80.0 atomic % or less, and even more preferably 71.0 atomic % or more and 78.0 atomic % or less, based on a total of 100 atomic % of the elements contained in the Sm—Fe—N magnetic material. When the Fe content in the Sm—Fe—N magnetic powder is within this range, the squareness ratio of the Sm—Fe—N magnetic material can be improved.

[0025] In the Sm—Fe—N magnetic material, the ratio of the Fe content to the Sm content (Fe content / Sm content), on an atomic basis, is preferably 5 or more and 10 or less, more preferably 7 or more and 9.5 or less, and even more preferably 8 or more and 9 or less. When the ratio of the Fe content to the Sm content in the Sm—Fe—N magnetic material is within this range, the squareness ratio of the Sm—Fe—N magnetic material can be improved.

[0026] In the Sm—Fe—N magnetic material, the total content of Sm and Fe is preferably 66.5 atomic % or more and 96.5 atomic % or less, more preferably 68.5 atomic % or more and 90.0 atomic % or less, and even more preferably 70.0 atomic % or more and 86.0 atomic % or less, based on 100 atomic % of the total Sm—Fe—N magnetic powder. When the total content of Sm and Fe in the Sm—Fe—N magnetic material is within this range, the squareness ratio of the Sm—Fe—N magnetic material can be improved.

[0027] In the Sm—Fe—N magnetic material, the N content is preferably 12.0 atomic % or more and 18.0 atomic % or less, more preferably 12.5 atomic % or more and 17.0 atomic % or less, and more preferably 13.0 atomic % or more and 16.5 atomic % or less, based on a total of 100 atomic % of the ratio of the Fe content to the Sm content. When the N content in the Sm—Fe—N magnetic material is within this range, the squareness ratio of the Sm—Fe—N magnetic material can be improved.

[0028] The Sm—Fe—N magnetic material may further contain Co. In the Sm—Fe—N magnetic powder, the Co content is preferably 0.0 atomic % or more and 5.0 atomic % or less, and in one embodiment, more preferably 1.0 atomic % or more and 5.0 atomic % or less, and even more preferably 1.5 atomic % or more and 5.0 atomic % or less, based on 100 atomic % of the total of the elements contained in the main phase. When the Co content in the Sm—Fe—N magnetic material is within the above range, the squareness ratio of the Sm—Fe—N magnetic material can be improved.

[0029] In another aspect, the Co content in the Sm—Fe—N magnetic material is more preferably 0.0 atomic % or more and 5 atomic % or less, more preferably 0.0 atomic % or more and 2.0 atomic % or less. When the Co content in the Sm—Fe—N magnetic material is in the above range, the squareness ratio of the Sm—Fe—N magnetic material can be improved.

[0030] The Sm—Fe—N magnetic material may contain Al, Si, Mn, and O as inevitable impurities. When the Sm—Fe—N magnetic material contains Al, the Al content may be, for example, 10.0 atomic % or less, or even 5.0 atomic % or less, based on 100 atomic % of the total elements contained in the Sm—Fe—N magnetic material. When the Sm—Fe—N magnetic material contains Si, the Si content may be, for example, 10.0 atomic % or less, or even 5.0 atomic % or less, based on 100 atomic % of the total elements contained in the Sm—Fe—N magnetic material. When the Sm—Fe—N magnetic material contains Mn, the Mn content may be, for example, 10.0 atomic % or less, or even 5.0 atomic % or less, based on 100 atomic % of the total elements contained in the Sm—Fe—N magnetic material. When the Sm—Fe—N based magnetic material contains O, the O content may be, for example, 10.0 atomic % or less, or even 5.0 atomic % or less, based on a total of 100 atomic % of the elements contained in the Sm—Fe—N based magnetic material.

[0031] The total content of each element in the Sm—Fe—N magnetic material does not exceed 100 atomic %. The total content of all elements that can be contained in the Sm—Fe—N magnetic material theoretically becomes 100 atomic %.

[0032] In the present disclosure, the types and contents of elements, excluding C, N, and O, that may be contained in the Sm—Fe—N-based magnetic material can be measured by X-ray fluorescence analysis (XRF) or inductively coupled plasma atomic emission spectrometry (ICP-AES), preferably by X-ray fluorescence analysis (XFR). Furthermore, C can be measured by oxygen flow combustion-infrared absorption spectrometry, and N and O can be measured by inert gas fusion-thermal conductivity spectrometry (TCD).

[0033] (Main Phase) The main phase is composed of Sm—Fe—N crystal grains. The Sm—Fe—N crystal grains have a structure in which N atoms are dissolved in the crystal lattice of Sm—Fe crystals. The main phase is a region in the Sm—Fe—N magnetic material that can contribute to the exertion of magnetism, and the solid solution of N atoms applies distortion to the crystal lattice, resulting in the development of uniaxial magnetic anisotropy and enabling the material to function as a hard magnetic material.

[0034] The main phase is Th 2 Zn 17 Sm—Fe—N crystals and TbCu crystals showing the type structure 7 It is preferable that the alloy contains one or more types of crystals selected from Sm--Fe--N type crystals exhibiting a type structure.

[0035] The main phase contains at least Sm, Fe, and N.

[0036] The main phase also contains M1, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W; M2, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W and is different from M1; and C.

[0037] The main phase may further contain Co.

[0038] The crystallite diameter of the Sm—Fe—N crystal grains contained in the main phase is preferably 10 nm or more and 1 μm or less, more preferably 15 nm or more and 400 nm or less, and even more preferably 20 nm or more and 200 nm or less. When the crystallite diameter of the Sm—Fe—N crystal grains is within the above range, the squareness ratio of the Sm—Fe—N magnetic material can be improved. The Sm—Fe—N crystal grains typically exist as single crystals. In the present disclosure, the crystallite diameter can be measured directly from images obtained by a transmission electron microscope (TEM) or a scanning transmission electron microscope (STEM).

[0039] (Grain boundary phase) The grain boundary phase exists between the plurality of Sm—Fe—N crystal grains that constitute the main phase. The grain boundary phase can typically be a layer that covers the Sm—Fe—N crystal grains, and can exist as a continuous layer that separates the plurality of Sm—Fe—N crystal grains, for example. The grain boundary phase can typically be a non-magnetic phase. When the grain boundary phase is a non-magnetic phase, the magnetic domains of the main phase are separated by the grain boundary phase, which suppresses magnetic field reversal and increases remanent magnetization, thereby increasing the squareness ratio.

[0040] The grain boundary phase may further contain one or more elements selected from Sm, Fe, Co, Ti, V, Mn, Zr, Nb, Hf, Ta, Si, B and C.

[0041] In one embodiment, the grain boundary phase may be a region in which a measured value of 2 nm or more continuously indicates a higher N content than the Sm—Fe—N-based crystalline grain phase in STEM-EDX analysis. In this embodiment, the thickness of the grain boundary phase is preferably 2 nm or more and 8 nm or less, and more preferably 4 nm or more and 6 nm or less. When the width of the grain boundary phase is within this range, the squareness ratio of the Sm—Fe—N-based crystalline material can be improved.

[0042] (M1-M2-C Phase) The Sm—Fe—N based magnetic material of the present disclosure preferably contains an M1-M2-C phase. By containing the M1-M2-C phase, precipitation of Fe-M1 and Fe-M2 phases can be suppressed, resulting in an Sm—Fe—N based magnetic material with good magnetic properties, particularly squareness ratio.

[0043] 4, when the distribution concentrations of Fe, M1, M2, and C are compared in the region where the M1-M2-C phase exists, the regions other than region 1 where the distribution concentration of Fe is high are identical in shape to region 2 where the distribution concentration of M1 is high, region 3 where the distribution concentration of M2 is high, and region 4 where the distribution concentration of C is high. From this, it can be said that the M1-M2-C phase exists in the region where region 2, region 3, and region 4 overlap.

[0044] The presence of the M1-M2-C phase in the Sm—Fe—N based magnetic material of the present disclosure can be confirmed by energy dispersive X-ray analysis using a scanning transmission electron microscope (STEM-EDX). For example, the Sm—Fe—N based magnetic material is observed with a scanning transmission electron microscope (STEM) to determine whether a field of view (e.g., 522 × 522 nm) including multiple main phases and grain boundary phases is present. 2 ) element distribution images of Fe, M1, M2, and C are obtained by energy dispersive X-ray analysis (EDX), and the distribution of each element is compared. The presence of regions with low Fe distribution density and high M1, M2, and C distribution densities confirms the presence of the M1-M2-C phase. A sample for STEM-EDX analysis of an Sm—Fe—N based magnetic material may be processed, for example, using a focused ion beam (FIB) device.

[0045] The M1-M2-C phase may be distributed throughout the Sm—Fe—N based magnetic material, and may be present, for example, in the main phase (i.e., in the region surrounded by the main phase), in the grain boundary phase (i.e., in the region surrounded by the grain boundary phase), or between the main phase and the grain boundary phase.

[0046] The major axis of the M1-M2-C phase may be preferably 1 nm or more and 30 nm or less, more preferably 3 nm or more and 25 nm or less, and even more preferably 5 nm or more and 25 nm or less, but is not limited thereto.

[0047] In the Sm—Fe—N based magnetic material of the present disclosure, the major axis of the M1-M2-C phase can be confirmed by energy dispersive X-ray analysis using a scanning transmission electron microscope (STEM-EDX). For example, the Sm—Fe—N based magnetic material is observed with a scanning transmission electron microscope (STEM), and a field of view (e.g., 522 × 522 nm) including multiple main phases and grain boundary phases is observed.2 In the above, element distribution images of Fe, M1, M2, and C are obtained by energy dispersive X-ray analysis (EDX), the major axis of regions with low Fe distribution density is measured at 10 or more locations, and the average value thereof may be used as the major axis of the M1-M2-C phase.

[0048] In addition, in the present disclosure, the major axis of a certain region means the length of the longest line segment that passes through the region and is separated by the boundary of the region.

[0049] The Sm—Fe—N based magnetic material of the present disclosure may contain other heterophases in addition to the main phase, grain boundary phase, and M1-M2-C phase. The Sm—Fe—N based magnetic material may be a material containing the main phase and grain boundary phase, and in a preferred embodiment, a material containing the main phase, grain boundary phase, and M1-M2 phase, preferably a material containing the main phase, grain boundary phase, and M1-M2-C phase, and a heterophase that may be included in some cases (which may typically be different from the Fe-M1 phase and Fe-M2 phase), and more preferably a material consisting of the main phase, grain boundary phase, and M1-M2-C phase, and a heterophase that may be included in some cases.

[0050] The Sm—Fe—N based magnetic material of the present disclosure may be in the form of magnetic powder, a magnet, or the like.

[0051] (Sm—Fe—N based magnetic powder) The Sm—Fe—N based magnetic material can be in the form of magnetic powder (i.e., powder). Hereinafter, the Sm—Fe—N based magnetic material in the form of powder will also be referred to as “Sm—Fe—N based magnetic powder.”

[0052] The Sm—Fe—N based magnetic powder contains the main phase and the grain boundary phase, and in a preferred embodiment is a material containing the main phase, grain boundary phase, and M1-M2 phase, preferably a powder material containing the main phase, grain boundary phase, and M1-M2-C phase, and optionally a heterogeneous phase, and more preferably a material consisting of the main phase, grain boundary phase, and M1-M2-C phase, and optionally a heterogeneous phase. The Sm—Fe—N based magnetic powder contains Sm, Fe, and N.

[0053] The average particle size of the Sm-Fe-N magnetic powder is preferably 10 μm or more and 300 μm or less, more preferably 10 μm or more and 50 μm or less, and even more preferably 20 μm or more and 40 μm or less.

[0054] The average particle size of the Sm-Fe-N magnetic powder can be measured by a laser diffraction particle size distribution measurement method.

[0055] (Sm—Fe—N based magnet) The Sm—Fe—N based magnetic material can be in the form of a magnet (i.e., bulk). Hereinafter, the Sm—Fe—N based magnetic material in bulk form will also be referred to as an “Sm—Fe—N based magnet.”

[0056] In one embodiment, the Sm—Fe—N magnet preferably includes the Sm—Fe—N magnetic powder and a binder. The binder can act as a binder for the Sm—Fe—N magnetic powder and can typically include resin (plastic), rubber, or a metal such as Zn.

[0057] In this embodiment, the content of Sm—Fe—N magnetic powder contained in the Sm—Fe—N magnet may be preferably 90% by mass or more and 99.5% by mass or less, and more preferably 95% by mass or more and 99% by mass or less.

[0058] In this embodiment, examples of the resin include thermosetting resins such as epoxy resins, phenolic resins, allyl resins, and unsaturated polyester resins; and thermoplastic resins such as polyamide resins, polyphenylene sulfide resins, polyether ketone resins, polyether ether ketone resins, and polyester resins.

[0059] In this embodiment, the Sm--Fe--N magnet may contain other additives in addition to the Sm--Fe--N magnetic powder and resin.

[0060] In another aspect, the Sm—Fe—N based magnet may be a bulk magnetic material preferably including the main phase, the grain boundary phase, and optionally a heterogeneous phase, and more preferably a bulk magnetic material consisting of the main phase, the grain boundary phase, and optionally a heterogeneous phase.

[0061] (Embodiment 2: Manufacturing Method of Sm—Fe-Based Alloy) A manufacturing method of an Sm—Fe-based alloy according to the present disclosure includes melting, rapidly cooling, and solidifying a raw material (hereinafter also simply referred to as a “metal raw material”) containing Sm; Fe; M1, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W; M2, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W and is different from M1; and C.

[0062] According to the manufacturing method of the present disclosure, it is possible to manufacture an Sm—Fe-based alloy in which Sm, M1, M2 and C are uniformly distributed, and to provide a raw material for the Sm—Fe—N-based magnetic material.

[0063] The types and proportions of elements contained in the metal raw materials are the same as those of elements constituting the Sm--Fe--N based magnetic material.

[0064] By melting the metal raw materials, each element can be uniformly distributed in the melt. The temperature when melting the metal is preferably, for example, 1,200°C or higher and 1,700°C or lower. The atmosphere when melting the metal is preferably, for example, an inert atmosphere not containing nitrogen, such as an Ar atmosphere or a He atmosphere. Such melting is not particularly limited, but is preferably performed by high-frequency melting. The metal raw materials may be mixed before being melted.

[0065] By rapidly cooling the melt, the melt can be cooled below its freezing point without crystallization while maintaining its compositional uniformity, thereby obtaining a Sm—Fe alloy, which typically contains an amorphous phase.

[0066] The quenching is not particularly limited, but is preferably carried out by roll quenching. In roll quenching, the molten material is quenched by spraying it onto a rotating metal roll. The conditions for roll quenching are not particularly limited. As the metal roll, it is preferable to use a roll made of, for example, molybdenum, copper, or an alloy material containing these as the main component. The peripheral speed of the roll can be, for example, preferably 30 m / s or more and 100 m / s or less, more preferably 50 m / s or more and 90 m / s or less.

[0067] (Embodiment 3: Method for manufacturing Sm—Fe—N based magnetic material) The method for manufacturing an Sm—Fe—N based magnetic material of the present disclosure includes: (a) crystallizing an Sm—Fe based alloy to obtain an Sm—Fe based crystalline material; and (b) nitriding the Sm—Fe based crystalline material to obtain an Sm—Fe—N based magnetic material, and may further include (c) heat treating the Sm—Fe—N based magnetic material.

[0068] According to the manufacturing method of the present disclosure, it is possible to provide an Sm—Fe—N based magnetic material having good magnetic properties, particularly good squareness ratio.

[0069] (a) Preparation of Sm—Fe-based crystalline material By subjecting the Sm—Fe-based alloy to a crystallization treatment, Sm—Fe-based crystals are precipitated, and an Sm—Fe-based crystalline material is obtained. The crystallization treatment can be typically carried out by heating.

[0070] The temperature when heating the Sm—Fe-based alloy may be, for example, preferably 690° C. or higher and 800° C. or lower, more preferably 725° C. or higher and 785° C. or lower. The heating time when heating the Sm—Fe-based alloy may be, for example, 5 minutes or higher and 60 minutes or lower, preferably 5 minutes or higher and 30 minutes or lower. The atmosphere when heating the Sm—Fe-based non-alloy may be, for example, an inert atmosphere not containing nitrogen, such as an Ar atmosphere or a He atmosphere. Heating the Sm—Fe-based alloy under such conditions makes it easier to generate Sm—Fe-based crystals more uniformly.

[0071] The Sm—Fe-based crystalline material may be further pulverized. By pulverization, a powdered Sm—Fe-based crystalline material is obtained. The pulverization method is not particularly limited, but it can be performed using, for example, a crusher, a stamp mill, a ball mill, or the like. By such pulverization, the Sm—Fe-based crystalline material is pulverized to, for example, 10 to 300 μm, preferably 10 to 150 μm, and more preferably 30 to 80 μm.

[0072] (b) Nitriding of Sm-Fe-based crystalline material By nitriding an Sm-Fe-based crystalline material, N atoms are incorporated into the Sm-Fe-based crystalline material, and an Sm-Fe-N-based magnetic material is obtained.

[0073] The nitriding treatment can be typically carried out by heat treatment in a nitrogen atmosphere, an ammonia atmosphere, a hydrogen atmosphere, or a mixture thereof.

[0074] When nitrogen gas is used in the nitriding treatment, the partial pressure of nitrogen is 10 kPa or more and 100 kPa or less, preferably 50 kPa or more and 100 kPa or less. By using such a nitrogen partial pressure, the nitriding reaction proceeds sufficiently.

[0075] In the above nitriding treatment, when a mixed gas of ammonia and hydrogen is used, the partial pressure of ammonia is 20 kPa or more and 40 kPa or less, preferably 25 kPa or more and 33 kPa or less, when the total pressure of the mixed gas is 0.1 MPa. By using such a partial pressure of ammonia, the nitriding reaction proceeds sufficiently.

[0076] In the nitriding treatment, the heating temperature is preferably 350° C. or higher and 500° C. or lower, more preferably 400° C. or higher and 500° C. or lower. By using this heating temperature, it is possible to prevent decomposition into SmN and Fe, which may occur when the nitriding reaction is carried out at a higher temperature, and it is possible to allow the reaction to proceed more sufficiently compared to when the nitriding reaction is carried out at a lower temperature.

[0077] The nitriding treatment can typically be carried out under atmospheric pressure, for example, preferably under a pressure of 900 hPa or more and 1,100 hPa or less, more preferably 950 hPa or more and 1,050 hPa or less.

[0078] When nitrogen gas is used in the nitriding treatment, the heating time is preferably 2 to 30 hours, more preferably 8 to 25 hours. This heating time can prevent grain growth and decomposition into SmN and Fe, which may occur with a longer heating time, and allows the reaction to proceed more efficiently than with a shorter heating time. By adjusting this heating time, the amount of nitrogen incorporated into the Sm—Fe crystalline material can be adjusted.

[0079] When a mixed gas of ammonia and hydrogen is used in the nitriding treatment, the heating time is preferably 10 to 90 minutes, more preferably 20 to 60 minutes. This heating time can prevent grain growth and decomposition into SmN and Fe, which may occur with a longer heating time, and allows the reaction to proceed more fully than with a shorter heating time. By adjusting this heating time, the amount of nitrogen incorporated into the Sm—Fe crystalline material can be adjusted.

[0080] (c) Heat Treatment of Sm—Fe—N-Based Magnetic Material After obtaining an Sm—Fe—N-based magnetic material by nitriding, the material may be further heated. Typically, the Sm—Fe—N-based magnetic material is further heat-treated at 400° C. or higher and 500° C. or lower in an atmosphere in which the concentrations of N atoms and O atoms are each 100 ppm or lower, thereby allowing the N atoms to diffuse into the main phase, resulting in an Sm—Fe—N-based magnetic material with an increased N atom content in the main phase. Hereinafter, the heat treatment of the Sm—Fe—N-based magnetic material is also referred to as "continuous heat treatment."

[0081] It is preferable that the step of cooling the Sm-Fe-N based magnetic material is not included between the nitriding treatment and the continuous heat treatment, and it is preferable that the continuous heat treatment is carried out directly following the nitriding treatment.

[0082] In the continuous heat treatment, the atmosphere in which the N atom concentration and the O atom concentration are each 100 ppm or less is H 2 Gas atmosphere; Ar atmosphere; He atmosphere; and H 2 An example of the atmosphere is a mixture of a gas and Ar or He.

[0083] In the continuous heat treatment, the heating temperature is preferably 350° C. or higher and 500° C. or lower, more preferably 400° C. or higher and 500° C. or lower. By using this heating temperature, it is possible to prevent decomposition into SmN and Fe, which may occur when heat treatment is performed at a higher temperature, and it is possible to sufficiently promote the solid solution of N atoms into the main phase, compared to when heat treatment is performed at a lower temperature.

[0084] The continuous heat treatment can typically be carried out under atmospheric pressure, for example, preferably under a pressure of 900 hPa or more and 1,100 hPa or less, more preferably 950 hPa or more and 1,050 hPa or less.

[0085] In the continuous heat treatment, the heating time is preferably 30 to 600 minutes, more preferably 30 to 240 minutes. By using this heating time, it is possible to prevent grain growth and decomposition into SmN and Fe, which may occur when the heating time is longer, and it is possible to more sufficiently promote the solid solution of N atoms into the main phase than when the heating time is shorter.

[0086] After the continuous heat treatment, the product may be naturally cooled.

[0087] The above-described (a) preparation of the Sm—Fe—N crystalline material, (b) nitriding of the Sm—Fe crystalline material, and (c) heat treatment of the Sm—Fe—N magnetic material, if necessary, typically results in the production of a powdered Sm—Fe—N magnetic material (i.e., Sm—Fe—N magnetic powder).

[0088] In one embodiment, the Sm—Fe—N magnet can be produced by a manufacturing method including mixing Sm—Fe—N magnetic powder and binder raw materials to obtain a mixture, and molding the mixture to obtain the Sm—Fe—N magnet. Methods for molding the mixture include compression molding, injection molding, and the like. For example, molding can be performed by heating and melting the resin raw materials in the mixture or dissolving them in a solvent to form a liquid, and then subjecting the liquid mixture to compression molding or injection molding. The liquid mixture can be hardened by cooling, crosslinking the binder raw materials, removing the solvent, or the like. Alternatively, the Sm—Fe—N magnet can be produced by sintering the Sm—Fe—N magnetic powder.

[0089] The Sm—Fe—N magnetic material of the present disclosure has good magnetic properties, particularly a squareness ratio, and can be suitably used in various electromagnetic devices such as electromagnetic actuators (motors). In particular, the Sm—Fe—N magnetic material of the present disclosure has a good squareness ratio, which can suppress demagnetization, and is expected to contribute to the miniaturization and high output of such electromagnetic devices. In addition, because demagnetization is suppressed in the Sm—Fe—N magnetic material of the present disclosure, it can be suitably used in applications requiring reliability in high-temperature environments, such as automotive applications.

[0090] The present invention will be explained in more detail with reference to the following examples, but the present invention is not limited to these examples.

[0091] (Examples 1 to 10, Comparative Examples 1 to 5) Elements having the compositions shown in Table 1 were charged and subjected to high-frequency melting to prepare master alloys. The obtained master alloys were melted in an Ar atmosphere and sprayed onto a Mo roll rotating at a peripheral speed of 70 m / s to obtain quenched ribbons (Sm—Fe-based amorphous material). The quenched ribbons were heat-treated in an Ar gas atmosphere at a treatment temperature of 755°C to obtain Sm—Fe-based crystalline material, which was then pulverized until it passed through a 150 μm mesh. The compositions shown in Table 1 are based on atomic percent.

[0092] The heat-treated powder (powdered Sm—Fe alloy) was then nitrided in an atmosphere at a temperature for a time shown in Table 1 to obtain an Sm—Fe—N magnetic material. After the nitriding treatment, a continuous heat treatment was carried out in the atmosphere, at the temperature, and for the time shown in Table 1.

[0093]

[0094] (STEM-EDX analysis) The materials obtained in the above examples and comparative examples were processed using a focused ion beam (FIB) and an Ar milling device, and observation images (dark-field images) were obtained using a transmission electron microscope (acceleration voltage 200 kV) manufactured by JEOL Ltd., and element distribution maps were obtained using energy dispersive X-ray analysis (EDX). The field of view length of each image was 522 nm × 522 nm, and the number of pixels when collecting EDX data was 512 × 512 px.

[0095] Fig. 1 shows the analysis results of the Sm—Fe—N magnetic material obtained in Example 1, Fig. 2 shows the analysis results of the material obtained in Comparative Example 1, and Fig. 3 shows the analysis results of the material obtained in Comparative Example 2. In Figs. 1, 2, and 3, the images indicated by DF-I are dark-field images obtained by STEM, and the images indicated by Fe, Zr, Nb, and C are element distribution images of each element.

[0096] In the material of Comparative Example 1 shown in Figure 2, when the STEM dark-field image was compared with the element distribution image of each element, it was confirmed that there were regions where the distribution concentration of Fe was low and the distribution concentrations of Zr and C were high (regions indicated by white arrows in Figure 2). This confirmed that a non-magnetic Zr-C phase had precipitated in the material of Comparative Example 1. However, it was confirmed that the distribution concentration of Fe was high in the material of Comparative Example 1, and there were also regions where Fe was present (regions surrounded by white circles in Figure 2). This confirmed that a heterogeneous phase, the Fe-Zr phase, had also precipitated in the material of Comparative Example 1.

[0097] In the material of Comparative Example 2 shown in Figure 3, when the STEM dark-field image and the element distribution image of each element were compared, it was confirmed that there were regions where the distribution concentration of Fe was low and the distribution concentrations of Nb and C were high (regions indicated by white arrows in Figure 3). This confirmed that the material of Comparative Example 2 had precipitated a non-magnetic Nb-C phase. However, it was also confirmed that the material of Comparative Example 2 had a high distribution concentration of Nb and also had regions where Fe was present (regions surrounded by white circles in Figure 3). This confirmed that the material of Comparative Example 2 also had precipitated a heterogeneous Fe-Nb phase.

[0098] In contrast, in the material of Example 1 shown in Figure 1, comparison of the STEM dark-field image with the element distribution image of each element confirmed the presence of regions where the distribution concentration of Fe is low and the distribution concentrations of Zr, Nb, and C are high. This confirmed that a non-magnetic Zr-Nb-C phase was precipitated in the Sm-Fe-N magnetic material of Example 1. Furthermore, the presence of an Fe-Zr phase or an Fe-Nb phase was not confirmed in the Sm-Fe-N magnetic material of Example 1.

[0099] (Magnetic Measurement) Magnetic measurements were performed using a VSM (vibrating sample magnetometer). The demagnetizing field Hk is the magnitude of the magnetic field when the magnetic flux density is 90% of the residual magnetic flux density, and the squareness ratio (Hk / Hcj) is the ratio obtained by dividing this by the magnitude of the coercive force Hcj. The higher the squareness ratio, the better the performance of the magnetic material is expected to be.

[0100]

[0101] Compared with the materials of the comparative examples, the Sm—Fe—N magnetic materials of the examples were confirmed to have a squareness ratio (Hk / Hcj) of 0.12 or more, indicating a favorable squareness ratio. This is believed to be because, in the Sm—Fe—N magnetic materials of the examples, the nonmagnetic M1-M2-C phase precipitates, suppressing the precipitation of heterogeneous phases such as the Fe-M1 phase and the Fe-M2 phase.

[0102] Furthermore, it was confirmed that the Sm—Fe—N-based materials of Examples 1 to 6, 8, and 10 in particular had an M1 to M2 content ratio of 5:5 on an atomic percent basis, and an even better squareness ratio of 0.21 to 0.28.

[0103] On the other hand, the materials of Comparative Examples 1 to 5 contained one type each of Zr, Nb, Hf, Ta, or V, and did not have a fully satisfactory squareness ratio (Hk / Hcj). This is thought to be because, in the materials of Comparative Examples 1 to 5, where the metal contained in each is M, the nonmagnetic M-C phase precipitated, but the precipitation of the heterophase Fe-M phase was not sufficiently suppressed.

[0104] Thus, even though the constituent elements and compositions contained in the materials are similar between the examples and the comparative examples, there can be large differences in magnetic properties, particularly squareness ratio.

[0105] The present disclosure provides the following aspects: [1] An Sm—Fe—N based magnetic material comprising: M1, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W; M2, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W and is different from M1; and C. [2] The Sm—Fe—N based magnetic material according to [1], wherein M1 is one element selected from Zr, Ti, Hf, V, Nb, and Ta, and M2 is one element selected from Zr, Ti, Hf, V, Nb, and Ta and is different from M1. [3] The Sm—Fe—N based magnetic material according to [1] or [2], wherein the ratio of the content of M1 to the content of M2 is 2:8 to 8:2 on an atomic percent basis. [4] The Sm—Fe—N based magnetic material according to any one of [1] to [3], which contains an M1-M2-C phase. [5] The Sm—Fe—N based magnetic material according to any one of [1] to [4], wherein the major axis of the M1-M2-C phase is 30 nm or less. [6] The Sm—Fe—N based magnetic material according to any one of [1] to [5], wherein the Sm content is 7.0 atomic % or more and 11.0 atomic % or less, the Fe content is 69.5 atomic % or more and 82.0 atomic % or less, the Co content is 0 atomic % or more and 5 atomic % or less, the N content is 11.0 atomic % or more and 19.5 atomic % or less, the total content of M1 and M2 is 1.6 atomic % or more and 5.0 atomic % or less, and the C content is more than 0 atomic % and 2.5 atomic % or less. [7] The Sm—Fe—N based magnetic material according to any one of [1] to [6], in the form of magnetic powder or a magnet. [8] An Sm—Fe—N based magnet comprising the Sm—Fe—N based magnetic material according to any one of [1] to [7], and a binder. [9] A method for producing a Sm—Fe-based alloy, comprising melting a raw material containing Sm; Fe; M1, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W; M2, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W and is different from M1; and C, followed by rapid cooling and solidification to obtain a Sm—Fe-based alloy.

[10] A method for producing an Sm—Fe—N based magnetic material, comprising: crystallizing the Sm—Fe based alloy produced by the production method according to [9] to obtain an Sm—Fe based crystalline material; and nitriding the Sm—Fe based crystalline material to obtain an Sm—Fe—N based magnetic material.

[11] A method for producing a Sm—Fe—N system magnet, comprising: melting and rapidly cooling raw materials containing Sm; Fe; M1, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W; M2, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W and is different from M1; and C, to obtain a Sm—Fe system rapidly solidified alloy; crystallizing the Sm—Fe system rapidly solidified alloy to obtain a Sm—Fe system crystalline material; nitriding the Sm—Fe system crystalline material to obtain a Sm—Fe—N system magnetic powder; mixing the Sm—Fe—N system magnetic powder with a binder raw material to obtain a mixture; and molding the mixture to obtain a Sm—Fe—N system magnet.

[0106] The Sm—Fe—N based magnetic material of the present disclosure has good magnetic properties, particularly good squareness ratio, and can be suitably used in a variety of applications.

[0107] 1 Region with high Fe distribution concentration 2 Region with high M1 distribution concentration 3 Region with high M2 distribution concentration 4 Region with high C distribution concentration

Claims

1. A Sm-Fe-N magnetic material comprising: M1, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W; M2, which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W and is different from M1; and C.

2. The Sm-Fe-N magnetic material according to claim 1, wherein M1 is one element selected from Zr, Ti, Hf, V, Nb and Ta, and M2 is one element selected from Zr, Ti, Hf, V, Nb and Ta, and is different from M1.

3. The Sm-Fe-N magnetic material according to claim 1 or 2, wherein the ratio of the content of M1 to the content of M2 is 2:8 to 8:2 on an atomic percent basis.

4. The Sm-Fe-N magnetic material according to any one of claims 1 to 3, which contains an M1-M2-C phase.

5. The Sm-Fe-N magnetic material according to any one of claims 1 to 4, wherein the major axis of the M1-M2-C phase is 30 nm or less.

6. A Sm-Fe-N magnetic material according to any one of claims 1 to 5, wherein the Sm content is 7.0 atomic % or more and 11.0 atomic % or less, the Fe content is 69.5 atomic % or more and 82.0 atomic % or less, the Co content is 0 atomic % or more and 5 atomic % or less, the N content is 11.0 atomic % or more and 19.5 atomic % or less, the total content of M1 and M2 is 1.6 atomic % or more and 5.0 atomic % or less, and the C content is more than 0 atomic % and 2.5 atomic % or less.

7. The Sm-Fe-N magnetic material according to any one of claims 1 to 6, which is in the form of magnetic powder or a magnet.

8. A Sm-Fe-N magnet comprising the Sm-Fe-N magnetic material according to any one of claims 1 to 7 and a binder.

9. A method for producing a Sm-Fe alloy, comprising melting raw materials containing Sm; Fe; M1 which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W; M2 which is one element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W and is different from M1; and C, followed by rapid cooling and solidification to obtain a Sm-Fe alloy.

10. A method for producing a Sm-Fe-N based magnetic material, comprising: crystallizing the Sm-Fe based alloy produced by the method according to claim 9 to obtain a Sm-Fe based crystalline material; and nitriding the Sm-Fe based crystalline material to obtain a Sm-Fe-N based magnetic material.

11. A method for producing a Sm-Fe-N system magnet, comprising: melting and rapidly cooling raw materials containing Sm; Fe; M1 which is an element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W; M2 which is an element selected from Zr, Ti, Hf, V, Nb, Ta, Cr, Mo, and W and is different from M1; and C to obtain a Sm-Fe system rapidly solidified alloy; crystallizing the Sm-Fe system rapidly solidified alloy to obtain a Sm-Fe system crystalline material; nitriding the Sm-Fe system crystalline material to obtain a Sm-Fe-N system magnetic powder; mixing the Sm-Fe-N system magnetic powder with a binder raw material to obtain a mixture; and molding the mixture to obtain a Sm-Fe-N system magnet.

Citation Information

Patent Citations

  • Magnetic material

    JP1994172936A

  • Iron-rare earth permanent magnet material and its manufacture

    JP1994283316A

  • Permanent magnet

    JP2001189206A

  • Rare earth permanent magnet powder, an adhesive magnetic material containing the same, and an element using the adhesive magnetic material

    JP2016526298A