Piezoelectric multilayer body, method for producing piezoelectric multilayer body, and piezoelectric element
A two-stage film formation process for KNN films achieves spontaneous polarization, low dielectric constant, and reduced film stress, addressing the challenges of high film stress and structural deformation in piezoelectric elements, enabling reliable and sensitive piezoelectric element performance.
Patent Information
- Application Number
- PCT/JP2023/045473
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2023-12-19
- Publication Date
- 2024-10-03
AI Technical Summary
Piezoelectric films with potassium, sodium, niobium, and oxygen (KNN) face challenges in achieving spontaneous polarization, low dielectric constant, and low film stress simultaneously, leading to high film stress and structural deformation issues in piezoelectric elements.
A method involving a two-stage film formation process where the first KNN film is formed at a temperature for high (001) orientation and low stress, followed by a second KNN film formation at a temperature for spontaneous polarization, resulting in a KNN film with a dielectric constant of 490 or less and film stress of 150 MPa or less.
The approach enables the production of a KNN film that is spontaneously polarized, has a low dielectric constant, and low film stress, eliminating the need for polarization treatment and ensuring reliable operation of piezoelectric elements with improved sensitivity and durability.
Smart Images

Figure JP2023045473_03102024_PF_FP_ABST
Abstract
Description
Piezoelectric laminate, method for manufacturing piezoelectric laminate, and piezoelectric element
[0001] The present disclosure relates to a piezoelectric laminate, a method for manufacturing a piezoelectric laminate, and a piezoelectric element.
[0002] Piezoelectric materials are widely used in functional electronic components such as sensors and actuators. KNN-based ferroelectric materials containing potassium, sodium, niobium, and oxygen are used as one of the materials for piezoelectric materials, and a laminate having a piezoelectric film (KNN film) formed using such a piezoelectric material has been proposed. For example, Patent Document 1 discloses a KNN film, which is a spontaneous polarization film that can obtain sufficient piezoelectric displacement without polarization treatment, i.e., a hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under predetermined conditions to the KNN film, in which the coercive electric field E C + and the coercive field E on the negative field side C - Patent Document 1 discloses a KNN film having a median coercive electric field between the film and the dielectric constant of the KNN film of 10.8 kV / cm or more. Patent Document 1 also discloses that the dielectric constant of the KNN film can be reduced by generating spontaneous polarization in the KNN film.
[0003] Furthermore, the piezoelectric film is required to have a small film stress (internal stress). For example, Patent Document 2 discloses a technique in which a lower electrode film, which is the base of the KNN film, is made of platinum (Pt), and the grain size of the crystal grains constituting the lower electrode film is controlled to be uniform, thereby reducing the surface unevenness of the lower electrode film, thereby alleviating the stress at the interface with the KNN film and reducing the film stress of the KNN film to 1.6 GPa or less. Patent Document 2 also discloses a technique in which the film stress of the KNN film is controlled (reduced) to 1.6 GPa or less by performing a heat treatment after the KNN film is formed.
[0004] JP 2014-207429 A JP 2011-029591 A
[0005] The KNN film obtained by the technique of the above-mentioned Patent Document 1 is a spontaneous polarization film that can obtain sufficient piezoelectric displacement without polarization treatment and has a low relative dielectric constant, but has a large film stress. On the other hand, the KNN film obtained by the technique of the above-mentioned Patent Document 2 is a film with low film stress, but is not a spontaneous polarization film.
[0006] An object of the present disclosure is to provide a piezoelectric laminate having a piezoelectric film that is a spontaneous polarization film, has a relative dielectric constant of 490 or less, and has a film stress of 150 MPa or less, and contains potassium, sodium, niobium, and oxygen.
[0007] According to one aspect of the present disclosure, there is provided a piezoelectric device comprising: a substrate; a lower electrode film formed on the substrate; and a piezoelectric film formed on the lower electrode film and composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, wherein a coercive field E C + and the coercive field E on the negative field side C - and a median value of the coercive electric field between the piezoelectric film and the piezoelectric layer is a positive value; the dielectric constant of the piezoelectric film is 490 or less; and the film stress of the piezoelectric film is 150 MPa or less.
[0008] According to another aspect of the present disclosure, there is provided a method for manufacturing a piezoelectric stack, comprising: a step of depositing a lower electrode film on a substrate; and a step of depositing a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film, wherein in the step of depositing the piezoelectric film, first, a first piezoelectric film, which is a part of the piezoelectric film, is deposited at a first temperature at which a (001) orientation rate is 95% or more and a film stress is 100 MPa or less, and then a second piezoelectric film, which is another part of the piezoelectric film, is deposited on the first piezoelectric film at a second temperature at which the second piezoelectric film becomes a spontaneous polarization film.
[0009] According to the present disclosure, it is possible to provide a piezoelectric laminate having a piezoelectric film that is a spontaneous polarization film, has a relative dielectric constant of 490 or less, and a film stress of 150 MPa or less, and contains potassium, sodium, niobium, and oxygen.
[0010] FIG. 1 is a diagram showing an example of the cross-sectional structure of a piezoelectric laminate according to an embodiment of the present disclosure. FIG. 2 is a diagram showing an example of the structure of a simplified piezoelectric element according to an embodiment of the present disclosure. FIG. 3 is a diagram showing an example of a schematic configuration of a piezoelectric element according to an embodiment of the present disclosure. FIG. 4 is a diagram showing an example of a schematic configuration of a piezoelectric device module according to an embodiment of the present disclosure. FIG. 5 is a diagram showing the polarization value-electric field hysteresis curve (P-E hysteresis curve) of Sample 3. FIG. 6 is a diagram showing the P-E hysteresis curve of Sample 9. FIG. 7(a) is a diagram showing an example of the schematic configuration of a simple unimorph cantilever fabricated using each sample, and FIG. 7(b) is a diagram explaining a method for measuring the amount of piezoelectric displacement. FIG. 1(a) to (e) are graphs showing evaluation results regarding the necessity of polarization treatment using a simplified piezoelectric element fabricated from Sample 3. FIG. 1(a) to (e) are graphs showing evaluation results regarding the necessity of polarization treatment using a simplified piezoelectric element fabricated from Sample 9. FIG. 1(a) and (b) are graphs showing evaluation results regarding the temperature resistance of spontaneous polarization using a simplified piezoelectric element fabricated from Sample 1. 10A and 10B are graphs showing the evaluation results of the temperature resistance of spontaneous polarization using a simplified piezoelectric element made from Sample 2.
[0011] <Discovery Obtained by the Inventors> In the above-mentioned Patent Document 1, when a KNN film is formed on a substrate such as a silicon (Si) substrate by sputtering, the KNN film is formed at a low temperature, thereby realizing a spontaneous polarization film (hereinafter also referred to as a "spontaneous polarization KNN film"). A spontaneous polarization KNN film has the advantage of not requiring the polarization process required for piezoelectric operation of the KNN film as a piezoelectric film. A laminate including a spontaneous polarization KNN film is particularly advantageous when applied to sensors. However, the spontaneous polarization KNN film realized in Patent Document 1 has a large film stress. Note that when the temperature during sputtering film formation is low, the film stress generated in the KNN film tends to be compressive stress, while when the temperature during sputtering film formation is high, the film stress generated in the KNN film tends to be tensile stress. If the film stress of the KNN film is large, for example, if the film stress of the KNN film exceeds 150 MPa, significant structural deformation occurs when fabricating piezoelectric elements with membrane structures, cantilever structures, or the like. As a result, the fabricated piezoelectric elements do not function properly. Furthermore, the manufacturing yield of piezoelectric elements and piezoelectric device modules decreases. For this reason, there is a demand to keep the film stress of the KNN film low, for example, to 150 MPa or less.
[0012] The present inventors conducted extensive research to develop a KNN film that possesses all three previously unrealized characteristics: a spontaneous polarization film, a low dielectric constant, and low film stress. As a result, they obtained the following five findings. (First finding) The film stress of a KNN film obtained by sputtering deposition is significantly dependent on the conditions at the initial stage of deposition of the KNN film. (Second finding) By first depositing a KNN film as a first layer (initial layer) under temperature conditions that reduce film stress (at the initial stage of deposition), and then depositing a KNN film as a second layer on the first layer under temperature conditions that reduce film stress, the film stress of the entire KNN film (the laminate of the first and second layers) is significantly reduced, even when the KNN film (second layer) is deposited at a low temperature that would normally result in a large film stress. (Third Finding) To reproducibly obtain a KNN film with a low dielectric constant, the (001) orientation rate of the KNN film must be high. To obtain a KNN film with a high (001) orientation rate, the deposition temperature of the KNN film must typically be within a predetermined range. By depositing a KNN film as the first layer under temperature conditions that increase the (001) orientation rate in the initial deposition phase, and then depositing a KNN film as the second layer on the first layer under temperature conditions that cause the KNN film to become a spontaneous polarization film, a KNN film with a high (001) orientation rate can be obtained even when the KNN film (second layer) is deposited at a low temperature that would normally decrease the (001) orientation rate. The (001) orientation rate of the KNN film refers to the orientation rate of the (001) plane of the crystals that make up the KNN film, and will be described in detail below. (Fourth finding) For example, to reproducibly obtain a KNN film having a dielectric constant of 490 or less, the (001) orientation rate of the KNN film must be 90% or more. By depositing a KNN film as the first layer under conditions that result in a (001) orientation rate of 95% or more at the initial stage of deposition, a KNN film with a (001) orientation rate of 90% or more can be obtained even when the KNN film as the second layer is subsequently deposited at a low temperature. (Fifth finding) By depositing a KNN film as the first layer under conditions that result in a small film stress and a high (001) orientation rate at the initial stage of deposition, and then depositing the KNN film as the second layer on the first layer under temperature conditions that result in the KNN film becoming a spontaneous polarization film, a KNN film with a low dielectric constant and a small film stress, i.e., a KNN film having all three of the above characteristics, can be realized.
[0013] Based on the above five findings, the inventors have found that by depositing a KNN film as a first layer under temperature conditions in which the film stress is 100 MPa or less and the (001) orientation rate is 95% or more in the early stages of film deposition, and then depositing a KNN film as a second layer under temperature conditions in which the KNN film becomes a spontaneous polarization film, a KNN film that is a spontaneous polarization film, has a film stress of 150 MPa or less, and a relative dielectric constant of 490 or less can be obtained.
[0014] The present disclosure has been made based on the above-mentioned problems and findings obtained by the present inventors.
[0015] <One Aspect of the Present Disclosure> Hereinafter, one aspect of the present disclosure will be described with reference to the drawings.
[0016] (1) Configuration of Piezoelectric Laminate As shown in FIG. 1 , a laminate (laminated substrate) 10 (hereinafter also referred to as piezoelectric laminate 10) having a piezoelectric film according to this embodiment includes a substrate 1, a lower electrode film 2 formed on the substrate 1, a piezoelectric film (piezoelectric thin film) 3 formed on the lower electrode film 2, and an upper electrode film 4 formed on the piezoelectric film 3.
[0017] The substrate 1 is a substrate having a surface oxide film (SiO 2 A single crystal silicon (Si) substrate 1a on which a surface oxide film 1b is formed, i.e., a Si substrate having a surface oxide film, can be suitably used. 2 It is also possible to use a Si substrate 1a having an insulating film formed of an insulating material other than the above. Also, as the substrate 1, a Si substrate 1a having an exposed Si(100) face or Si(111) face on the surface, that is, a Si substrate having no surface oxide film 1b or insulating film, can be used. Also, as the substrate 1, an SOI (Silicon On Insulator) substrate, a quartz glass (SiO 2 The thickness of the single crystal Si substrate 1a can be, for example, 300 μm to 1000 μm, and the thickness of the surface oxide film 1b can be, for example, 1 nm to 4000 nm.
[0018] The lower electrode film 2 can be formed using, for example, platinum (Pt). The lower electrode film 2 is a polycrystalline film. Hereinafter, a polycrystalline film formed using Pt will also be referred to as a Pt film. It is preferable that the (111) plane of the Pt film is parallel to the main surface of the substrate 1 (including cases where the (111) plane is inclined at an angle of ±5° or less with respect to the main surface of the substrate 1), i.e., the Pt film is oriented in the (111) plane. Orientation of the Pt film in the (111) plane means that no peaks other than those attributable to the (111) plane are observed in the X-ray diffraction pattern obtained by X-ray diffraction (XRD) measured on the surface of the piezoelectric film 3. Thus, the main surface of the lower electrode film 2 (the surface underlying the piezoelectric film 3) is preferably composed of the Pt (111) plane. The lower electrode film 2 can be formed by a method such as sputtering or vapor deposition. The material of the lower electrode film 2 may be, in addition to Pt, various metals such as gold (Au), ruthenium (Ru), or iridium (Ir), alloys containing these as main components, or strontium ruthenate (SrRuO 3 , abbreviated as SRO) or lanthanum nickelate (LaNiO 3 The lower electrode film 2 may also be formed using a metal oxide such as SiO2 (abbreviated as LNO). When the lower electrode film 2 is formed using a metal oxide, the crystals constituting the lower electrode film 2 preferably have a (001) plane orientation preferentially relative to the surface of the substrate 1. The lower electrode film 2 may be a single layer film formed using the above-mentioned metals, an alloy mainly composed of the above-mentioned metals, or a metal oxide. The lower electrode film 2 may be a laminate of a Pt film and a film mainly composed of SRO provided on the Pt film, or a laminate of a Pt film and a film mainly composed of LNO provided on the Pt film. The thickness of the lower electrode film 2 (when the lower electrode film 2 is a laminate, the total thickness of each layer) may be, for example, 100 nm to 400 nm.
[0019] An adhesion layer 6 may be provided between the substrate 1 and the lower electrode film 2 to enhance adhesion therebetween. The adhesion layer 6 may be, for example, a layer containing zinc (Zn) and oxygen (O) as main components (hereinafter also referred to as a "ZnO layer"). The ZnO layer may be formed using, for example, zinc oxide. The composition ratio of Zn and O constituting the ZnO layer preferably satisfies the relationship Zn:O = 1:1, but is not limited thereto and may vary somewhat. The ZnO layer is a polycrystalline layer. It is preferable that the (0001) plane of the ZnO layer is parallel to the major surface of the substrate 1 (including the case where the (0001) plane is inclined at an angle of ±5° or less with respect to the major surface of the substrate 1), i.e., the ZnO layer is oriented in the (0001) plane direction. The ZnO layer being oriented in the (0001) plane direction means that the intensity of the peak due to the (0002) plane is high in the X-ray diffraction pattern obtained by XRD measured on the surface of the piezoelectric film 3. As such, the main surface of the ZnO layer (the surface that serves as the base of the lower electrode film 2) is preferably configured as the ZnO (0001) plane. The ZnO layer can be formed by a method such as sputtering or vapor deposition. The thickness of the ZnO layer can be, for example, 1 nm or more and 200 nm or less, preferably 10 nm or more and 50 nm or less. The adhesion layer 6 can be formed of, for example, titanium (Ti), tantalum (Ta), titanium oxide (TiO 2 ), nickel (Ni), ruthenium oxide (RuO 2 ), iridium oxide (IrO 2 ) or the like as a main component may be provided. Such an adhesion layer 6 can also be formed by a method such as sputtering or vapor deposition, and the thickness of the adhesion layer 6 can be, for example, 1 nm to 200 nm, preferably 10 nm to 50 nm. In this specification, the adhesion layer 6 provided between the substrate 1 and the lower electrode film 2 is sometimes referred to as a lower adhesion layer 6.
[0020] The piezoelectric film 3 is a film formed of, for example, an alkali niobium oxide containing potassium (K), sodium (Na), niobium (Nb), and oxygen (O). That is, the piezoelectric film 3 is a film whose main component is an alkali niobium oxide containing K, Na, Nb, and O. The piezoelectric film 3 is a film formed of, for example, an alkali niobium oxide containing potassium (K), sodium (Na), niobium (Nb), and oxygen (O).1-x Na x ) NbO 3 The piezoelectric film 3 can be formed using an alkali niobium oxide represented by the formula (I), i.e., potassium sodium niobate (KNN). The coefficient x [= Na / (K+Na)] in the above composition formula can be within the range of 0<x<1, preferably 0.4≦x≦0.8. The piezoelectric film 3 is a KNN polycrystalline film (hereinafter also referred to as the KNN film 3). The crystal structure of KNN is a perovskite structure. That is, the KNN film 3 has a perovskite structure. Preferably, more than half of the crystals constituting the KNN film 3 have a columnar structure. In this specification, the crystal system of KNN is considered to be a tetragonal system. The KNN film 3 can be formed by a sputtering method. The thickness of the KNN film 3 can be, for example, 0.5 μm to 5 μm, preferably 1 μm to 3 μm.
[0021] The crystals constituting the KNN film 3 are preferentially oriented in the (001) plane with respect to the main surface of the substrate 1 (for example, the Si substrate 1a when the substrate 1 is a Si substrate 1a having a surface oxide film 1b or an insulating film, etc.). That is, the main surface of the KNN film 3 (the surface underlying the upper electrode film 4) is mainly composed of the KNN (001) plane. For example, by directly depositing the KNN film 3 on a Pt film (lower electrode film 2) whose main surface is mainly composed of the Pt (111) plane, a KNN film 3 whose main surface is mainly composed of the KNN (001) plane can be obtained. In this specification, the crystals constituting the KNN film 3 being oriented in the (001) plane means that the (001) plane of the crystals constituting the KNN film 3 is parallel or approximately parallel to the main surface of the substrate 1. Furthermore, the crystals constituting the KNN film 3 being preferentially oriented in the (001) plane direction means that there are many crystals whose (001) plane is parallel or approximately parallel to the main surface of the substrate 1 .
[0022] The alkali niobium oxide constituting the KNN film 3 may be selected from the group consisting of lithium (Li), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), bismuth (Bi), antimony (Sb), vanadium (V), indium (In), tantalum (Ta), molybdenum (Mo), tungsten (W), chromium (Cr), Ti, zirconium (Zr), hafnium (Hf), scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), The alkali niobium oxide may further contain at least one element (dopant) selected from the group consisting of samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), copper (Cu), zinc (Zn), silver (Ag), manganese (Mn), iron (Fe), cobalt (Co), Ni, aluminum (Al), Si, germanium (Ge), tin (Sn), and gallium (Ga). The concentration of these elements in the alkali niobium oxide can be, for example, 5 at % or less (when a plurality of the above elements is contained, the total concentration can be 5 at % or less).
[0023] As will be described in detail later, in this embodiment, first, a first KNN film 3a (first piezoelectric film, hereinafter also referred to as "KNN film 3a"), which is a part of the KNN film 3, is deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second KNN film 3b (second piezoelectric film, hereinafter also referred to as "KNN film 3b"), which is the other part of the KNN film 3, is deposited on the KNN film 3a at a second temperature at which the KNN film 3b becomes a spontaneous polarization film. As a result, the KNN film 3 in this embodiment (i.e., a laminate of the KNN film 3a and the KNN film 3b) has all of Features 1 to 3, which will be described later. Furthermore, the KNN film 3 in this embodiment may further have Feature 4, which will be described later.
[0024] The following describes features 1 to 4 that the KNN film 3 of this embodiment may have.
[0025] (Feature 1) The KNN film 3 has a coercive electric field E on the positive electric field side in a hysteresis curve (P-E hysteresis curve) showing the correlation between the polarization amount (P) of the KNN film 3 and the applied electric field (E) obtained by applying an electric field to the KNN film 3 under predetermined conditions. C + and the coercive field E on the negative field side C - The median value of the coercive field between the
[0026] The P-E hysteresis curve in this embodiment is prepared by, for example, forming an upper electrode film 4 on a 2 μm-thick KNN film 3, grounding the lower electrode film 2, applying a triangular or sinusoidal (sine wave) electric field of −150 kV / cm to +150 kV / cm (i.e., a triangular or sinusoidal voltage of −30 V to +30 V) at a frequency of 1 kHz to the KNN film 3 via the upper electrode film 4, measuring the polarization of the KNN film 3, and plotting the obtained polarization. The “coercive field” is defined as the electric field at which the polarization is 0 μC / cm. 2 The two electric field values at which the coercive electric field E C + " means that the polarization is 0 μC / cm 2 The "coercive electric field E C - " means that the polarization is 0 μC / cm 2 The "median value of the coercive field" is the electric field value on the negative electric field side when C + -E C - ) / 2.
[0027] As described above, the KNN film 3 in this embodiment is characterized in that the median value of the coercive field is a positive value in the P-E hysteresis curve. The KNN film 3 having this characteristic is a spontaneous polarization film (spontaneous polarization KNN film) in which the polarization direction is aligned in a fixed direction (e.g., upward).
[0028] The term "spontaneous polarization film" as used herein refers to a KNN film 3 whose polarization direction is spontaneously aligned in a fixed direction (without ever applying an electric field (voltage) via the lower electrode film 2 and the upper electrode film 4 after film formation). Furthermore, "upward" in this specification refers to the direction from the lower electrode film 2 side toward the upper electrode film 4 side. Furthermore, "polarization direction aligned in a fixed direction" means that the majority (more than half) of the crystals constituting the KNN film 3 are polarized in a fixed direction. For example, "polarization direction aligned upward" means that the polarization direction of the majority of the crystals constituting the KNN film 3 is upward.
[0029] In addition, in the case of a KNN film that is not a spontaneous polarization film, the P-E hysteresis curve is generally a graph symmetrical about the origin, and the coercive field E C + Absolute value of and coercive field E C - The absolute values of are almost the same. When a piezoelectric element 20 (described later) such as a sensor device is manufactured using a piezoelectric laminate having such a KNN film, a polarization process must be performed during the manufacturing process. The "polarization process" refers to a process in which a large electric field is applied to the KNN film 3 (under heating, if necessary) to align the polarization direction of the KNN film 3 in a certain direction (the direction of the applied electric field).
[0030] Since the KNN film 3 is a spontaneous polarization film, polarization processing is not required when the piezoelectric stack 10 having the KNN film 3 of this embodiment is used to fabricate the piezoelectric element 20 described below.
[0031] The median value of the coercive field is preferably 10 kV / cm or more. This allows a larger number of crystals constituting the KNN film 3 to be polarized in a certain direction (e.g., upward). As a result, the direction of spontaneous polarization (i.e., the polarization direction of the KNN film 3) generated in the KNN film 3 can be stabilized, and a KNN film 3 that does not require polarization treatment can be reliably obtained.
[0032] The median value of the coercive electric field is preferably 100 kV / cm or less, more preferably 70 kV / cm or less, so that a decrease in the piezoelectric properties (for example, the piezoelectric constant) of the KNN film 3 can be avoided.
[0033] The polarization characteristics of the KNN film 3 are maintained (not lost) even when the KNN film 3 is exposed to high temperatures, for example, when the KNN film 3 is subjected to a thermal history of 400° C. or higher. For example, even when the KNN film 3 is exposed to high temperatures after deposition, during deposition of the upper electrode film 4, annealing, deposition of the insulating film 8 and metal wirings 9 a, 9 b (described later) (for example, deposition of the insulating film 8 by plasma CVD or ALD, patterning), mounting (for example, wire bonding, die bonding, solder reflow), etc., the spontaneous polarization generated in the KNN film 3 is maintained. The inventors have confirmed that the polarization characteristics of the KNN film 3 are maintained without degradation even when the KNN film 3 is subjected to a thermal history of 500° C. Furthermore, the inventors have confirmed that when the KNN film 3 is subjected to a thermal history of about 600°C, the polarization characteristics of the KNN film 3 deteriorate somewhat, but the spontaneous polarization generated in the KNN film 3 is maintained. This makes it possible to suitably apply the piezoelectric element 20 (piezoelectric device module 30) described below, which is obtained by processing the piezoelectric stack 10 having the KNN film 3, to sensor applications. Furthermore, degradation of the performance of a sensor fabricated using the piezoelectric element 20 can be avoided.
[0034] (Feature 2) The KNN film 3 further has the feature that "the relative dielectric constant is 490 or less."
[0035] Since the dielectric constant of the KNN film 3 is 490 or less, a highly sensitive sensor can be obtained when the piezoelectric element 20 (piezoelectric device module 30) described below obtained by processing the piezoelectric laminate 10 is used for a sensor. Note that the lower the dielectric constant of the KNN film 3, the higher the sensitivity of the sensor produced by processing the piezoelectric laminate 10.
[0036] In order to reproducibly (reliably) exhibit this characteristic, the (001) orientation rate of the KNN film 3 must be 90% or more. The (001) orientation rate of the KNN film 3 refers to the orientation rate of the crystals constituting the KNN film 3 in the (001) plane orientation. "The (001) orientation rate of the KNN film 3 is 90% or more" means that, for example, 90% or more of the crystals constituting the KNN film 3 are oriented in the (001) plane orientation with respect to the main surface of the substrate 1. Note that the "orientation rate" in this specification is a value calculated by the following formula (1) based on the peak intensity of the X-ray diffraction pattern (2θ / θ) obtained by performing XRD measurement on the KNN film 3.
[0037] Orientation rate (%)={(001) peak intensity / ((001) peak intensity+(110) peak intensity)}×100 (1)
[0038] The "(001) peak intensity" in the above formula (1) refers to the intensity of a diffraction peak due to crystals oriented in the (001) plane direction (i.e., crystals whose (001) plane is parallel to the main surface of the substrate 1) among the crystals constituting the KNN film 3 in an X-ray diffraction pattern obtained by performing XRD measurement on the KNN film 3, and is the intensity of a peak appearing within a 2θ range of 20° to 23°. When multiple peaks appear within a 2θ range of 20° to 23°, it is the intensity of the highest peak. Furthermore, the "(110) peak intensity" in the above formula (1) refers to the intensity of a diffraction peak due to crystals oriented in the (110) plane direction (i.e., crystals whose (110) plane is parallel to the main surface of the substrate 1) among the crystals constituting the KNN film 3 in an X-ray diffraction pattern obtained by performing XRD measurement on the KNN film 3, and is the intensity of a peak appearing within a 2θ range of 30° to 33°. When multiple peaks appear within the 2θ range of 30° to 33°, the intensity is that of the highest peak.
[0039] (Feature 3) The KNN film 3 further has the feature that "the film stress is 150 MPa or less."
[0040] By keeping the film stress of the KNN film 3 at 150 MPa or less, it is possible to suppress large structural deformation when processing the piezoelectric stack 10 to fabricate piezoelectric elements 20 having a membrane structure, a cantilever structure, or the like, as described below. This allows the piezoelectric elements 20 (piezoelectric device modules 30) obtained by processing the piezoelectric stack 10, as described below, to operate normally.
[0041] (Feature 4) The KNN film 3 may further have the feature that "when a negative (AC) voltage is continuously applied to the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film 2 and the upper electrode film 4 (i.e., in the KNN film 3), the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 decreases to 80% or less of its initial value exceeds 10 million."
[0042] For example, in the case of a piezoelectric laminate 10 having a KNN film 3 with a thickness of 2 μm, when a unipolar triangular or sinusoidal AC voltage having an amplitude in the range of 0 V to −60 V is continuously applied to the upper electrode film 4 (via the KNN film 3) at a frequency of 300 Hz with the lower electrode film 2 grounded so that the direction of the electric field applied to the KNN film 3 does not reverse (so that the direction of the electric field is in one direction), the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 decreases to 80% or less of its initial value exceeds 10 million.
[0043] In this specification, the term "unipolar electric field" refers to an electric field that is unidirectional even if the magnitude of the voltage applied to the KNN film 3 via the upper electrode film 4 periodically fluctuates within a range of, for example, 0 V to -60 V. In addition, in this specification, the "number of voltage application cycles until the piezoelectric displacement of the KNN film 3 falls to 80% or less of its initial value when a negative voltage is continuously applied to the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film 3" is also referred to as the "number of application cycles."
[0044] When an AC voltage is applied to the KNN film 3 via the upper electrode film 4, the KNN film 3 deforms. The higher the applied voltage, the greater the deformation of the KNN film 3. The KNN film 3 in this embodiment can have the characteristic that the amount of piezoelectric displacement is unlikely to decrease even when it is repeatedly deformed by applying a large AC voltage continuously, i.e., has the characteristic of excellent AC stress resistance.
[0045] In the piezoelectric laminate 10 obtained by the above-described novel method, a KNN film 3a having a high (001) orientation rate and low film stress, for example, a KNN film 3a having a (001) orientation rate of 95% or more and a film stress of 100 MPa or less, is interposed between the bottom electrode film 2 and the KNN film 3b. This allows the KNN film 3 (a laminate of the KNN film 3a and the KNN film 3b) in this embodiment to have superior AC stress resistance compared to a laminate without the KNN film 3a. This is believed to be because the interposition of the KNN film 3a significantly improves the adhesion between the bottom electrode film 2 and the KNN film 3. The fact that the interposition of the KNN film 3a can increase the number of application cycles to more than 10 million, i.e., improves the AC stress resistance of the KNN film 3, is a novel finding first discovered as a result of extensive research by the present inventors.
[0046] The excellent AC stress resistance of the KNN film 3 makes it possible to improve the reliability of the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10, which will be described later.
[0047] The inventors have confirmed that in a piezoelectric laminate 10 having a KNN film 3a with a (001) orientation rate of 95% or more and a film stress of 100 MPa or less interposed between a lower electrode film 2 and a KNN film 3b, when a negative voltage is continuously applied to the KNN film 3 via the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film 3, the piezoelectric displacement of the KNN film 3 can be maintained at 80% or more of its initial value even after the number of application cycles exceeds 10 million, and even reaches 50 million or more.
[0048] On the other hand, when the KNN film 3a is not interposed, that is, when the KNN film 3 is not configured as a laminate of the KNN film 3a and the KNN film 3b, if a large AC voltage is continuously applied to the KNN film 3 via the upper electrode film 4 and the KNN film 3 is continuously deformed, the KNN film 3 will gradually peel off from the lower electrode film 2. As a result, the amount of piezoelectric displacement of the KNN film 3 will be easily reduced.
[0049] The inventors have confirmed that in a piezoelectric laminate in which the KNN film 3a is not interposed between the lower electrode film 2 and the KNN film 3b, when a negative voltage is continuously applied to the KNN film via the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film, the piezoelectric displacement of the KNN film falls to less than 80% of its initial value before the number of application cycles reaches 10 million.
[0050] As described above, the KNN film 3 in this embodiment can have all of the above-mentioned features 1 to 3, and preferably all of the above-mentioned features 1 to 4. When the KNN film 3 has all of the above-mentioned features 1 to 3, it becomes possible to suitably apply the piezoelectric element 20 (piezoelectric device module 30) described below, which is obtained by processing the piezoelectric stack 10 having the KNN film 3, to sensor applications. Furthermore, when the KNN film 3 has all of the above-mentioned features 1 to 4, it becomes possible to even more suitably apply the piezoelectric element 20 (piezoelectric device module 30) described below to sensor applications.
[0051] In this embodiment, when depositing the KNN film 3, the KNN film 3a is first deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is deposited on the KNN film 3a at a second temperature at which the KNN film 3b becomes a spontaneous polarization film. Therefore, the KNN film 3 in this embodiment has a laminated structure of the KNN film 3a as a first layer (initial layer) deposited at the first temperature and the KNN film 3b as a second layer deposited at the second temperature.
[0052] The KNN film 3a deposited at the first temperature does not exhibit spontaneous polarization. In other words, the KNN film 3a is not a spontaneous polarization film. Therefore, as the ratio of the thickness of the KNN film 3a to the total thickness of the KNN film 3 (the total thickness of the KNN film 3a and the KNN film 3b) increases, the aforementioned feature 1 tends to be less likely to be realized. In other words, it tends to be less likely to generate spontaneous polarization in the KNN film 3. Therefore, it is preferable to minimize the thickness of the KNN film 3a so as to reduce the film stress of the KNN film 3 and keep the overall film stress of the KNN film 3 at 150 MPa or less. While the thickness of the KNN film 3a is not strictly limited, it is preferable that it be 20% or less of the total thickness of the KNN film 3. This ensures that the KNN film 3 having the aforementioned feature 1, i.e., the KNN film 3 being a spontaneous polarization film, can be obtained.
[0053] The upper electrode film 4 is mainly composed of various metals such as Pt, Au, Al, Cu, etc., or alloys thereof. The upper electrode film 4 can be formed by a method such as sputtering, vapor deposition, plating, or metal paste. The upper electrode film 4 does not have a significant effect on the crystal structure of the KNN film 3, unlike the lower electrode film 2. Therefore, the material, crystal structure, and film formation method of the upper electrode film 4 are not particularly limited. Note that, for example, RuO may be interposed between the KNN film 3 and the upper electrode film 4 to enhance their adhesion. 2 , IrO 2 , Ti, Ta, TiO 2 An adhesion layer 7 containing, as a main component, Ni or the like may be provided. The thickness of the upper electrode film 4 may be, for example, 50 nm to 5000 nm, preferably 50 nm to 300 nm, and when the adhesion layer 7 is provided, the thickness of the adhesion layer 7 may be, for example, 1 nm to 200 nm, preferably 5 nm to 50 nm. In this specification, the adhesion layer 7 provided between the KNN film 3 and the upper electrode film 4 may also be referred to as the upper adhesion layer 7.
[0054] (2) Methods of Manufacturing the Piezoelectric Laminate, Piezoelectric Element, and Piezoelectric Device Module Methods of manufacturing the above-described piezoelectric laminate 10, piezoelectric element, and piezoelectric device module will now be described.
[0055] (Deposition of Lower Adhesion Layer and Lower Electrode Film) First, a substrate 1 is prepared, and a lower adhesion layer 6 (e.g., a ZnO layer) and a lower electrode film 2 (e.g., a Pt film) are deposited in this order by, for example, sputtering on one of the main surfaces of the substrate 1. Note that a substrate 1 may be prepared on which the lower adhesion layer 6 and the lower electrode film 2 have already been deposited on one of the main surfaces.
[0056] The conditions for depositing the ZnO layer as the lower adhesive layer 6 are exemplified below. The deposition time for the lower adhesive layer 6 is adjusted appropriately depending on the target thickness of the lower adhesive layer 6. Target: ZnO sintered body Temperature (substrate temperature): 200°C or higher and 700°C or lower, preferably 300°C or higher and 700°C or lower, more preferably 500°C or higher and 700°C or lower Discharge power density: 2 W / cm 2 More than 6W / cm 2 Preferably less than 3 W / cm 2 More than 5W / cm 2 The following atmosphere: argon (Ar) gas and oxygen (O 2 ) gas (hereinafter referred to as "Ar / O 2 (also called "mixed gas atmosphere") O 2 The ratio of the partial pressure of Ar gas to the partial pressure of O 2 Gas partial pressure): 5 / 1 to 30 / 1, preferably 7 / 1 to 20 / 1, more preferably 10 / 1 to 15 / 1 Atmospheric pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 1 nm or more and 200 nm or less, preferably 10 nm or more and 50 nm or less
[0057] In this specification, when a numerical range is expressed, such as "5 / 1 to 30 / 1," it means that the lower limit and the upper limit are included in the range. The same applies to other numerical ranges.
[0058] The conditions for forming a Ti layer or the like as the lower adhesion layer 6 are exemplified as follows: Target: Ti plate or the like Temperature (substrate temperature): 100°C or higher and 500°C or lower, preferably 200°C or higher and 400°C or lower Atmosphere: Ar gas atmosphere Atmosphere pressure: 0.1 Pa or higher and 0.5 Pa or lower, preferably 0.2 Pa or higher and 0.4 Pa or lower Other conditions can be the same as those for forming a ZnO layer.
[0059] The conditions for depositing a Pt film as the lower electrode film 2 are exemplified below. The deposition time for the lower electrode film 2 is adjusted appropriately depending on the target thickness of the lower electrode film 2. Target: Pt plate Temperature (substrate temperature): 200°C or higher and 600°C or lower, preferably 300°C or higher and 500°C or lower Discharge power density: 1 W / cm 2 More than 5W / cm 2 Preferably 2 W / cm or less 2 More than 4W / cm 2 Atmosphere: Ar gas atmosphere Atmosphere pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 100 nm or more and 400 nm or less
[0060] (Deposition of KNN film) After the deposition of the lower adhesive layer 6 and the lower electrode film 2 is completed, the KNN film 3 is deposited on the lower electrode film 2 by a sputtering method such as RF magnetron sputtering. The composition of the KNN film 3 can be adjusted by controlling the composition of the target used during sputter deposition, for example. 2 CO 3 Powder, Na 2 CO 3 powder, Nb 2 O 5 The target can be prepared by mixing powders and firing them. 2 CO 3 Powder, Na 2 CO 3 powder, Nb 2 O 5 This can be controlled by adjusting the mixing ratio of the powders, etc. When depositing the KNN film 3 containing the above elements such as Cu and Mn, a target may be used in which Cu powder (or CuO powder), Mn powder (or MnO powder), etc. are mixed in a predetermined ratio in addition to the above powders.
[0061] The KNN film 3 is formed in two stages by changing the temperature conditions. Specifically, first (at the beginning of the film formation), the KNN film 3a is formed at a first temperature, and then the KNN film 3b is formed at a second temperature.
[0062] The first temperature is a temperature at which the (001) orientation rate of the KNN film 3a becomes 95% or more and the film stress becomes 100 MPa or less. For example, the first temperature is a temperature at which the (001) orientation rate of the KNN film 3a becomes 95% or more when the KNN film 3a is formed to a thickness of 2 μm (±10%) at the first temperature. Furthermore, the first temperature is a temperature at which the film stress of the KNN film 3a becomes 100 MPa or less when the KNN film 3a is formed to a thickness of 2 μm (±10%) at the first temperature.
[0063] The second temperature is the temperature at which the KNN film 3b becomes a spontaneous polarization film, i.e., the temperature at which the median value of the coercive field of the P-E hysteresis curve becomes a positive value. For example, the second temperature is the temperature at which the KNN film 3b becomes a spontaneous polarization film when the KNN film 3b is deposited to a thickness of 2 μm (±10%) at the second temperature.
[0064] Although the first and second temperatures depend somewhat on the sputtering deposition apparatus and deposition conditions, in the sputtering deposition of the KNN film 3 in this embodiment, the second temperature is usually lower than the first temperature (first temperature > second temperature). For example, the first temperature can be in the range of 550°C to 600°C, and the second temperature can be in the range of 400°C to 500°C.
[0065] The conditions other than the temperature when depositing the KNN film 3 (KNN film 3a, KNN film 3b) are, for both the deposition at the first temperature and the deposition at the second temperature, as follows: Discharge power density: 2.7 W / cm 2 More than 4.1W / cm 2 Preferably 2.8 W / cm or less 2 More than 3.8W / cm 2 Atmosphere: an atmosphere containing at least Ar gas, preferably Ar / O 2 Mixed gas atmosphere: Atmospheric pressure: 0.03 Pa or more and 0.5 Pa or less, preferably 0.04 Pa or more and 0.4 Pa or less O relative to Ar gas 2 Ratio of partial pressures of gases (O 2 Gas partial pressure / Ar gas partial pressure): 0 to 1 / 20, preferably 0 to 1 / 30 Film formation rate: 0.5 μm / hr to 4 μm / hr, preferably 0.5 μm / hr to 2 μm / hr Total thickness of KNN film: 0.5 μm to 5 μm, preferably 1 μm to 3 μm
[0066] In addition, "O 2 The "gas partial pressure / Ar gas partial pressure is 0 (zero)" means that 2 This refers to a state where the gas partial pressure is 0, i.e., an atmosphere of only Ar gas. The "total thickness of the KNN film" refers to the total thickness of the KNN film 3a deposited at the first temperature and the KNN film 3b deposited at the second temperature. The deposition times for the KNN films 3a and 3b are adjusted appropriately depending on the target thicknesses of the KNN films 3a and 3b. As described above, the thickness of the KNN film 3a is preferably set to the minimum necessary to reduce the film stress in the KNN film 3b during deposition at the second temperature and to keep the film stress of the entire KNN film 3 at 150 MPa or less. Therefore, the deposition time for the KNN film 3a (deposition time at the first temperature) is preferably adjusted so that the thickness of the KNN film 3a is 20% or less of the total thickness of the KNN film 3, for example.
[0067] As described above, first, the KNN film 3a is deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is deposited on the KNN film 3a at a second temperature at which the KNN film 3b becomes a spontaneous polarization film. Even if the second temperature is low enough to reduce the (001) orientation rate or to generate a large film stress in the KNN film 3b, the (001) orientation rate of the entire KNN film 3 after the KNN film 3b is deposited can be 90% or more, and the film stress of the entire KNN film 3 can be significantly reduced. As a result, the dielectric constant of the entire KNN film 3 can be reproducibly reduced to 490 or less, and the film stress of the entire KNN film 3 can be reduced to 150 MPa or less, while the KNN film 3 becomes a spontaneous polarization film. That is, by forming the KNN film 3 (KNN film 3a and KNN film 3b) in two stages while changing the temperature under the above-mentioned conditions, it is possible to obtain a KNN film 3 having all of the above-mentioned features 1 to 3. Furthermore, by forming the KNN film 3 in two stages while changing the temperature under the above-mentioned conditions, i.e., by providing a KNN film 3a having a high (001) orientation rate and small film stress, it is also possible to obtain a KNN film 3 having all of the above-mentioned features 1 to 4.
[0068] (Deposition of Upper Adhesion Layer and Upper Electrode Film) After the deposition of the KNN film 3 is completed, the upper adhesion layer 7 (for example, RuO2 layer) and the upper electrode film 4 (for example, a Pt film) are deposited in this order.
[0069] RuO as the upper adhesive layer 7 2 The conditions for forming the upper adhesive layer 7 are exemplified as follows. The deposition time for the upper adhesive layer 7 is adjusted appropriately depending on the target thickness of the upper adhesive layer 7. Target: Ru plate or the like Temperature (substrate temperature): Room temperature (25°C) or higher and 500°C or lower Discharge power density: 0.3 W / cm 2 More than 2W / cm 2 or less, preferably 0.5 W / cm 2 1W / cm or more 2 Atmosphere: Ar / O 2 Mixed gas atmosphere O 2 The ratio of the partial pressure of Ar gas to the partial pressure of O 2 Gas partial pressure): 3 / 5 to 1 / 1, preferably 3 / 4 to 1 / 1 Atmospheric pressure: 0.1 Pa or more and 1.0 Pa or less, preferably 0.2 Pa or more and 0.7 Pa or less Thickness: 1 nm or more and 200 nm or less, preferably 5 nm or more and 50 nm or less
[0070] The conditions for depositing a Pt film or the like as the upper electrode film 4 are exemplified below. The deposition time for the upper electrode film 4 is adjusted appropriately depending on the target thickness of the upper electrode film 4. Target: Pt plate or the like Temperature (substrate temperature): Room temperature (25°C) or higher and 500°C or lower Discharge power density: 1 W / cm 2 More than 5W / cm 2 Preferably 2 W / cm or less 2 More than 4W / cm 2 Atmosphere: Ar gas atmosphere Atmosphere pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 50 nm or more and 5000 nm or less, preferably 50 nm or more and 300 nm or less
[0071] As described above, by sequentially depositing the lower adhesive layer 6, the lower electrode film 2, the KNN film 3 (KNN films 3a and 3b), the upper adhesive layer 7, and the upper electrode film 4, a piezoelectric laminate 10 as shown in FIG. 1 is obtained.
[0072] (Fabrication of Piezoelectric Element) After fabricating the piezoelectric laminate 10 as shown in FIG. 1, the piezoelectric laminate 10 is processed to form an element having a KNN film 3 (also referred to as a piezoelectric element 20).
[0073] Specifically, first, the upper electrode film 4 (including the upper adhesive layer 7) and the KNN film 3 are individually patterned by dry etching using, for example, Ar gas or a reactive gas. In the patterning, the upper electrode film 4 (including the upper adhesive layer 7) and the KNN film 3 are each formed into a predetermined shape, and a portion of the lower electrode film 2 is exposed. In the patterning, a photoresist can be used as an etching mask. FIG. 2 shows the piezoelectric stack 10 after patterning, i.e., the piezoelectric element 20. The piezoelectric element 20 shown in FIG. 2 is also referred to as a simple piezoelectric element.
[0074] 2, the lower electrode film 2 and the lower adhesive layer 6 are patterned by dry etching using, for example, Ar gas or a reactive gas, to form the lower electrode film 2 and the lower adhesive layer 6 into predetermined shapes. In this patterning, a photoresist can be used as an etching mask.
[0075] After completing the patterning of the lower electrode film 2 and the lower adhesive layer 6, the insulating film 8 and the metal wirings 9a and 9b are provided. Specifically, first, a layer made of an insulating material is provided from the upper electrode film 4 to the substrate 1 so as to cover the side surface of the KNN film 3, and then a layer of Ar gas or CF 4 The insulating layer is patterned by dry etching using a reactive gas such as silicon dioxide (SiO 2 ) or wet etching to form an insulating film 8. 2 ), aluminum oxide (Al 2 O 3 ), tantalum oxide (Ta 2 O 5 The insulating film 8 may be a single layer film or a laminated film having multiple layers stacked on top of each other. The insulating film 8 may be formed by a method such as a CVD method or a sputtering method.
[0076] After providing the insulating film 8, a layer (metal wiring layer) made of a material containing metal is provided. Then, the metal wiring layer is patterned by dry etching using Ar gas or a reactive gas, or wet etching, to form metal wirings 9a and 9b. The metal wiring 9a is formed (patterned) so as to be connected to (contact) the lower electrode film 2 but not to (contact) the upper electrode film 4, while the metal wiring 9b is formed so as to be connected to the upper electrode film 4 but not to (contact) the lower electrode film 2. The metal wirings 9a and 9b can be formed using various metals, such as Au, Al, Ti, and Cr, or alloys containing these metals as their main components. The metal wirings 9a and 9b can be single-layer films or laminates of multiple layers. The metal wirings 9a and 9b (metal wiring layer) can be provided by methods such as sputtering, vapor deposition, plating, and metal paste deposition.
[0077] Further, by Deep-RIE or wet etching, a part of the substrate 1 is removed from the back surface side of the substrate 1 (one of the two main surfaces of the substrate 1 opposite to the surface on which the lower electrode film 2 and the like are formed), thereby obtaining a piezoelectric element 20 having a membrane structure, a cantilever structure, or the like, for example, a membrane-type MEMS piezoelectric element 20 as shown in FIG.
[0078] The etching conditions for pattern processing when forming the insulating film 8 and the metal wiring 9a, 9b, and the etching conditions for the substrate 1 when processing the piezoelectric stack 10 into the piezoelectric element 20 can be general etching conditions used in semiconductor device manufacturing processes, as long as the conditions do not deteriorate the insulating properties of the KNN film 3.
[0079] (Fabrication of Piezoelectric Device Module) By connecting a voltage detection means 11a to the obtained piezoelectric element 20, a device module 30 having a KNN film 3 (hereinafter also referred to as piezoelectric device module 30) is obtained. FIG. 4 shows a schematic configuration diagram of the piezoelectric device module 30 according to this embodiment. The piezoelectric device module 30 includes at least the piezoelectric element 20 and a voltage detection means 11a connected to the piezoelectric element 20. The voltage detection means 11a is a means for detecting a voltage generated between the lower electrode film 2 and the upper electrode film 4 (between the electrodes). Various known means can be used as the voltage detection means 11a.
[0080] By connecting the voltage detection means 11a between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20, the piezoelectric device module 30 can function as a sensor. When the KNN film 3 deforms in response to a change in some physical quantity, a voltage is generated between the lower electrode film 2 and the upper electrode film 4 due to the deformation. By detecting this voltage with the voltage detection means 11a, it is possible to measure the magnitude of the physical quantity applied to the KNN film 3. In this case, the piezoelectric device module 30 can be used, for example, as an angular velocity sensor, an ultrasonic sensor, a pressure sensor, an acceleration sensor, etc.
[0081] (3) Effects According to this aspect, one or more of the following effects can be obtained.
[0082] (a) The KNN film 3 has all three characteristics: a positive median value of the coercive field in the P-E hysteresis curve (characteristic 1 described above), a dielectric constant of 490 or less (characteristic 2 described above), and a film stress of 150 MPa or less (characteristic 3 described above). That is, the KNN film 3 is a spontaneous polarization film, but has a small film stress and a low dielectric constant.
[0083] Because the KNN film 3 is a spontaneous polarization film, when the piezoelectric stack 10 is processed to produce the piezoelectric element 20 (piezoelectric device module 30), there is no need to perform a polarization process on the KNN film 3. Since the polarization process is not required, the manufacturing process of the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric stack 10 can be simplified.
[0084] Since the relative dielectric constant of the KNN film 3 is 490 or less, when the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 is used for a sensor, a highly sensitive sensor can be obtained.
[0085] By setting the film stress of the KNN film 3 to 150 MPa or less, it is possible to suppress large structural deformation when processing the piezoelectric stack 10 to fabricate the piezoelectric element 20 (piezoelectric device module 30) having a membrane structure, a cantilever structure, or the like. This allows the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric stack 10 to function normally. For example, it becomes possible for the piezoelectric element 20 (piezoelectric device module 30) to function reliably as a sensor.
[0086] In this way, since the KNN film 3 has all of the above-mentioned features 1 to 3, the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 can be suitably applied to sensor applications.
[0087] (b) By interposing the KNN film 3a having a high (001) orientation rate and low film stress between the lower electrode film 2 and the KNN film 3b, the KNN film 3 can further have the above-mentioned feature of being able to withstand more than 10 million application cycles (the above-mentioned feature 4) in addition to the above-mentioned features 1 to 3. That is, the KNN film 3 can be a film that has low film stress, a low dielectric constant, and excellent AC stress resistance, even though it is a spontaneous polarization film.
[0088] Since the KNN film 3 has excellent AC stress resistance, i.e., the piezoelectric displacement amount is less likely to decrease even if the KNN film 3 is repeatedly deformed significantly, it is possible to improve the reliability of the piezoelectric element 20 (piezoelectric device module 30).
[0089] In this way, since the KNN film 3 has all of the above-mentioned features 1 to 4, the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 can be more suitably applied to sensor applications.
[0090] (c) The polarization characteristics of the KNN film 3 in this embodiment are maintained even when the KNN film 3 is exposed to high temperatures. For example, even if the KNN film 3 is exposed to high temperatures after deposition of the KNN film 3 during deposition of the upper electrode film 4, annealing, formation of the insulating film 8 and metal wiring 9a, 9b, mounting, etc., the spontaneous polarization generated in the KNN film 3 is maintained. This makes it possible to more suitably apply the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric stack 10 to sensor applications. Furthermore, degradation of the performance of a sensor fabricated using the piezoelectric element 20 (piezoelectric device module 30) can be avoided.
[0091] (d) By setting the median value of the coercive field to 10 kV / cm or more, it is possible to stabilize the direction of spontaneous polarization generated in the KNN film 3, and to reliably obtain a KNN film 3 that does not require polarization treatment. Furthermore, by setting the median value of the coercive field to 10 kV / cm or more, it is possible to maintain the initial polarization direction (spontaneously polarized direction) even if a reverse electric field (an electric field in a direction that reverses the polarization direction that is aligned in a certain direction) is mistakenly applied to the KNN film 3 during the fabrication of the piezoelectric stack 10, the piezoelectric element 20, and the piezoelectric device module 30, or during the use of the piezoelectric element 20 (piezoelectric device module 30).
[0092] (e) When depositing the KNN film 3, first, the KNN film 3a is deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is deposited on the KNN film 3a at a second temperature at which the KNN film 3b becomes a spontaneous polarization film, thereby making it possible to obtain a KNN film 3 having all of the above-mentioned features 1 to 3, and preferably all of the above-mentioned features 1 to 4.
[0093] <Other Aspects> One aspect of the present disclosure has been specifically described above. However, the present disclosure is not limited to the above aspect and can be modified in various ways without departing from the spirit of the present disclosure. Furthermore, these aspects can be combined in any way.
[0094] In the above embodiment, the piezoelectric device module 30 functions as a sensor, but this is not limiting. That is, the piezoelectric device module 30 may also function as an actuator. In this case, the piezoelectric device module 30 includes at least a piezoelectric element 20 obtained by molding the piezoelectric stack 10 into a predetermined shape and a voltage application means 11b (see FIG. 4 ) connected to the piezoelectric element 20. The voltage application means 11b is a means for applying a voltage between the lower electrode film 2 and the upper electrode film 4 (between the electrodes). Various known means can be used as the voltage application means 11b. By connecting the voltage application means 11b between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20, the piezoelectric device module 30 can function as an actuator. By applying a voltage between the lower electrode film 2 and the upper electrode film 4 using the voltage application means 11b, the KNN film 3 can be deformed. This deformation can actuate various components connected to the piezoelectric device module 30. In this case, examples of applications of the piezoelectric device module 30 include a head for an inkjet printer, a MEMS mirror for an optical scanner, and a vibrator for an ultrasonic generator.
[0095] Furthermore, for example, when the above-mentioned piezoelectric laminate 10 is molded into the piezoelectric element 20, the substrate 1 from the piezoelectric laminate 10 may be replaced with another substrate, as long as the piezoelectric device module 30 made using the piezoelectric laminate 10 (piezoelectric element 20) can be applied to a desired application such as a sensor.
[0096] The following describes experimental results that support the effects of the above-described embodiment.
[0097] [Experiment 1] An experiment was conducted to confirm the temperatures that can be applied to the first temperature and the second temperature when depositing a KNN film.
[0098] (Fabrication of Samples A to G) A Si substrate with a surface oriented in the (100) plane, a thickness of 610 μm, and a diameter of 6 inches (also referred to as "φ6 inches"), on which a thermally oxidized film (200 nm thick) was formed, was prepared. Then, on the thermally oxidized film of this Si substrate, a ZnO layer (25 nm thick) was formed as a lower adhesive layer, a Pt film (preferentially oriented in the (111) plane with respect to the surface of the substrate, 200 nm thick) was formed as a lower electrode film, a KNN film (2 μm thick) was formed as a piezoelectric film, and a RuO 2 A KNN layer (10 nm thick) as a lower adhesive layer, and a Pt film (100 nm thick) as an upper electrode film were deposited in this order to fabricate samples A to G, which were piezoelectric laminates. In samples A to G, the lower adhesive layer, lower electrode film, KNN film, upper adhesive layer, and upper electrode film were all deposited by RF magnetron sputtering.
[0099] The conditions for depositing the ZnO layer as the lower adhesive layer were as follows: Target: ZnO sintered body Substrate temperature: 500° C. Discharge power density: 4 W / cm 2 Atmosphere: Ar / O 2 Mixed gas atmosphere Ambient pressure: 0.3 Pa Ar gas partial pressure / O 2 Gas partial pressure: 10 / 1 Film formation time: 3 minutes (thickness 25 nm)
[0100] The conditions for depositing a Pt film as the lower electrode film were as follows: Target: Pt plate Substrate temperature: 500° C. Discharge power density: 2 W / cm 2 Atmosphere: Ar gas atmosphere Atmosphere pressure: 0.3 Pa Film formation time: 14 minutes (thickness 200 nm)
[0101] The conditions for forming the KNN film were as follows: Target: KNN sintered body Discharge power density: 3 W / cm 2 Atmosphere: Ar / O 2 Mixed gas atmosphere Ambient pressure: 0.1 Pa O 2 Gas partial pressure / Ar gas partial pressure: 1 / 20 Film formation temperature: a predetermined temperature in the range of 300°C to 650°C Film formation time: 60 minutes (thickness 2000 nm (2 μm))
[0102] RuO as an upper adhesion layer 2The conditions for depositing the layer were as follows: Target: Ru plate Substrate temperature: room temperature (25° C.) Discharge power density: 0.5 W / cm 2 Atmosphere: Ar / O 2 Mixed gas atmosphere Ambient pressure: 0.3 Pa Ar gas partial pressure / O 2 Gas partial pressure: 1 / 1 Film formation time: 6 minutes (thickness 10 nm)
[0103] The conditions for depositing a Pt film as the upper electrode film were as follows: Target: Pt plate Substrate temperature: room temperature (25° C.) Discharge power density: 2 W / cm 2 Atmosphere: Ar gas atmosphere Atmosphere pressure: 0.3 Pa Film formation time: 7 minutes (thickness 100 nm)
[0104] Samples A to G were fabricated under the same conditions as described above, except for the deposition temperature of the KNN film. The deposition temperatures of the KNN films of Samples A to G are as shown in Table 1 below.
[0105] <Evaluation> Samples A to G were evaluated for the (001) orientation rate of the KNN film, the film stress of the KNN film, and the median value of the coercive electric field.
[0106] (Evaluation of (001) Orientation Ratio) The (001) orientation ratio of the KNN film was evaluated by calculating using the above formula (1) based on the peak intensity of the X-ray diffraction pattern (2θ / θ) obtained by performing XRD measurement on the KNN film. The XRD measurement was performed after the KNN film was formed and before the upper adhesive layer and the upper electrode film were formed. The calculation results of the (001) orientation ratio are shown in Table 1 below. In Table 1, "orientation ratio" means the (001) orientation ratio of the KNN film.
[0107] (Evaluation of Film Stress) The stress of the thin film on the substrate can be calculated by measuring the amount of warpage of the substrate caused by the thin film, specifically, the radius of curvature of the warpage of the substrate, as shown in the following formula (2). Therefore, in this evaluation, the radius of curvature R of the warpage of the substrate (Si substrate) of each sample was measured after the lower adhesive layer, the lower electrode film, and the KNN film were formed, and before the upper adhesive layer and the upper electrode film were formed. Then, the film stress of the KNN film of each sample was calculated using the following formula (2). In this evaluation, the radius of curvature R of the Si substrate was calculated from the warpage shape measured by a laser displacement meter of the Si substrate after the lower adhesive layer, the lower electrode film, and the KNN film were formed.
[0108]
[0109] In the above formula (2), σ is the stress of the thin film (KNN film), E s / (1-ν s ) is the biaxial elastic modulus of the substrate (Pa), h is the thickness of the substrate (m), R is the radius of curvature of the warp of the substrate (m), and t is the thickness of the KNN film (m). In samples A to G, a Si substrate was used as the substrate, so the biaxial elastic modulus value was set to 30.3. The film stress (σ) of the KNN film was calculated assuming that the Si substrate was sufficiently flat. In samples A to G, a lower adhesive layer (ZnO layer) and a lower electrode film (Pt film) were formed, but the thickness of the lower adhesive layer (25 nm) and the thickness of the lower electrode film (200 nm) were sufficiently smaller than the thickness of the KNN film (2 μm). Therefore, the influence of the lower adhesive layer and the lower electrode film was ignored when calculating the film stress of the KNN film.
[0110] The calculation results of the film stress of the KNN films of samples A to G are shown in Table 1 below. In Table 1, "compressive" means that the film stress is compressive stress, and "tensile" means that the film stress is tensile stress.
[0111] (Evaluation of Median Coercive Field) The median coercive field was evaluated as follows. First, the piezoelectric laminates of Samples A to G were fabricated, and then the upper electrode film (including the upper adhesive layer) and the KNN film were individually patterned by dry etching using Ar gas. In the patterning, a photoresist was used as an etching mask to shape the upper electrode film to a size of φ0.5 mm, while partially exposing the lower electrode film, to fabricate simplified piezoelectric elements as shown in FIG. 2 . P-E hysteresis curves were created for each simplified piezoelectric element fabricated from Samples A to G. Specifically, with the lower electrode film grounded, a triangular or sine wave electric field of −150 kV / cm to +150 kV / cm was applied to the KNN film via the upper electrode film at a frequency of 1 kHz, and the polarization of the KNN film was measured. The resulting polarization versus the applied electric field was plotted to create a P-E hysteresis curve. The P-E hysteresis curves were prepared using an apparatus (DBLI) manufactured by Aguzact. The coercive electric field E C + and coercive electric field E C - and obtain the value of the coercive field E C + and coercive electric field E C - From the value of C + -E C - ) / 2) was calculated. The results of calculating the median values of the coercive electric fields of samples A to G are shown in Table 1 below. Note that the "median value" in Table 1 refers to the median value of the coercive electric field.
[0112]
[0113] In Sample A, the crystal structure of the KNN film did not become a perovskite structure. Therefore, in the X-ray diffraction pattern obtained by XRD measurement, no peak was observed within the 2θ range of at least 20° to 23°, and as a result, the (001) orientation rate could not be calculated. Furthermore, because the crystal structure of the KNN film did not become a perovskite structure, the KNN film had low withstand voltage characteristics. When preparing a P-E hysteresis curve, it was not possible to apply a triangular or sine wave electric field of -150 kV / cm to +150 kV / cm at a frequency of 1 kHz to the KNN film via the upper electrode film. Therefore, it was not possible to prepare a P-E hysteresis curve, and as a result, it was not possible to measure the median coercive field. From these findings, it can be confirmed that the film formation temperature of Sample A is not applicable to either the first or second temperature.
[0114] In samples B to D, the film stress exceeds 100 MPa. This confirms that the film deposition temperatures of samples B to D are not applicable to the first temperature. On the other hand, in samples B to D, the median coercive electric field is 10 kV / cm or more. This confirms that the film deposition temperatures of samples B to D, that is, the temperature range of 400°C to 500°C, are temperatures at which the KNN film becomes a spontaneous polarization film and are applicable to the second temperature.
[0115] In samples E and F, the (001) orientation rate is 95% or more, and the film stress is 100 MPa or less. This confirms that the film formation temperatures of samples E and F, i.e., the temperature range of 550°C or more and 600°C or less, are applicable to the first temperature. On the other hand, in samples E and F, the median value of the coercive field is 0 kV / cm. In other words, the KNN films of samples E and F are not spontaneous polarization films. This confirms that the film formation temperatures of samples E and F are not applicable to the second temperature.
[0116] In sample G, the (001) orientation rate is less than 95% and the film stress is more than 100 MPa. In addition, in sample G, the median value of the coercive field is 0 kV / cm. From these results, it can be confirmed that the film formation temperature of sample G cannot be applied to either the first temperature or the second temperature.
[0117] [Experiment 2] An experiment was conducted to confirm the effect of forming a KNN film in two stages by changing the temperature.
[0118] (Fabrication of Samples 1 to 16) A Si substrate with a surface oriented in the (100) plane, a thickness of 610 μm, a diameter of 6 inches, and a thermally oxidized film (200 nm thick) formed on the surface was prepared. Then, on the thermally oxidized film of this Si substrate, a ZnO layer (25 nm thick) was formed as a lower adhesive layer, a Pt film (preferentially oriented in the (111) plane with respect to the surface of the substrate, 200 nm thick) was formed as a lower electrode film, a KNN film (2 μm thick) was formed as a piezoelectric film, and a RuO 2 A KNN layer (10 nm thick) as a lower electrode film, and a Pt film (100 nm thick) as a lower electrode film were deposited in this order to fabricate piezoelectric laminates Samples 1 to 16. The lower adhesive layer, lower electrode film, KNN film, upper adhesive layer, and upper electrode film were all deposited by RF magnetron sputtering.
[0119] For Samples 1 to 14, the KNN films were deposited in two stages under different temperature conditions. Specifically, a first KNN film was first deposited at a first temperature, and then a second KNN film was deposited on the first KNN film at a second temperature different from the first temperature. The first and second temperatures used to deposit the KNN films for Samples 1 to 14 were as shown in Table 2 below. The deposition time at the first temperature was 6 minutes (thickness: 200 nm), and the deposition time at the second temperature was 54 minutes (thickness: 1800 nm). For Samples 15 and 16, the KNN films were deposited at a predetermined temperature without changing the temperature conditions. The temperature used to deposit the KNN films for Samples 15 and 16 was as shown in the "Second Temperature" column in Table 2 below, and the deposition time was 60 minutes (thickness: 2000 nm). The conditions other than the deposition temperature and deposition time when depositing the KNN film, and the deposition conditions for each film (each layer) other than the KNN film, were the same as those in the above-mentioned Experiment 1. Moreover, Samples 1 to 16 were each produced under the same conditions as those described above, except for the deposition temperature (first temperature, second temperature) of the KNN film.
[0120] <Evaluation> Samples 1 to 16 were evaluated for the median coercive field, the relative dielectric constant of the KNN film, the film stress of the KNN film, and the AC stress resistance. Furthermore, using simple piezoelectric elements fabricated from samples 3 and 9, an evaluation was conducted regarding the necessity of polarization treatment. Furthermore, using simple piezoelectric elements fabricated from samples 1, 2, and 8, an evaluation was conducted regarding the temperature resistance of spontaneous polarization generated in the KNN film. Furthermore, using simple piezoelectric elements fabricated from samples 3 and 9, an evaluation was conducted regarding the heat resistance performance of the piezoelectric elements.
[0121] (Evaluation of Median Value of Coercive Electric Field) Using Samples 1 to 16, simplified piezoelectric elements as shown in FIG. 2 were fabricated using the same method as described in the evaluation of the median value of the coercive electric field in Experiment 1 above. Then, P-E hysteresis curves were fabricated using each of the simplified piezoelectric elements fabricated from Samples 1 to 16. The P-E hysteresis curves were fabricated using the same conditions, method, and equipment as described in the evaluation of the median value of the coercive electric field in Experiment 1 above. The P-E hysteresis curves of Samples 3 and 9 are shown in FIGS. 5 and 6, respectively. Furthermore, the coercive electric field E C + and coercive electric field E C - The values of the coercive electric fields were obtained and the median values of the coercive electric fields were calculated. The calculation results of the median values of the coercive electric fields of Samples 1 to 16 are shown in Table 2 below. Note that the "median value" in Table 2 means the median value of the coercive electric field.
[0122] (Evaluation of relative permittivity) Using Samples 1 to 16, simple piezoelectric elements as shown in FIG. 2 were fabricated using the same method as described in the evaluation of the median value of the coercive electric field in Experiment 1 above. Then, using each of the simple piezoelectric elements fabricated from Samples 1 to 16, the lower electrode film and the upper electrode film were connected to an LCR meter, and the capacitance was measured under conditions of ±1 V and 1 kHz. The measured capacitance, the area of the upper electrode film (0.625 mm 2 The dielectric constant of the KNN film of each sample was calculated using the values of the thickness (2 μm) of the KNN film, and the dielectric constant of the KNN film of each sample. The dielectric constants of Samples 1 to 16 are shown in Table 2 below.
[0123] (Evaluation of Film Stress) For each of Samples 1 to 16, the film stress of the KNN film was evaluated using the same method as described for evaluating the film stress in Experiment 1 above. A lower adhesive layer and a lower electrode film were also formed in Samples 1 to 16, but as with Samples A to G, the thicknesses of the lower adhesive layer and the lower electrode film were sufficiently smaller than the thickness of the KNN film. Therefore, the influence of the lower adhesive layer and the lower electrode film was ignored when calculating the film stress of the KNN film. The calculation results of the film stress of the KNN film for Samples 1 to 16 are shown in Table 2 below. The terms "compression" and "tension" in Table 2 have the same meanings as "compression" and "tension" in Table 1.
[0124] (Evaluation of AC Stress Resistance) The AC stress resistance was evaluated by measuring the AC stress lifetime. The AC stress lifetime was evaluated as follows. First, small strips measuring 20 mm in length and 2.5 mm in width were cut out from each of Samples 1 to 16. Then, as shown in FIG. 7( a), one end in the longitudinal direction of each of the small pieces obtained from Samples 1 to 16 was fixed with a clamp, and a voltage application means (not shown) was connected between the lower electrode film and the upper electrode film to fabricate a simple unimorph cantilever. Then, using a voltage application means, a negative voltage was continuously applied to the KNN film via the upper electrode film so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and the upper electrode film (i.e., the KNN film). Specifically, with the lower electrode film grounded, a unipolar sine wave AC voltage ranging from 0 V to −60 V was continuously applied to the KNN film via the upper electrode film at a frequency of 300 Hz, continuously deforming each small piece of KNN film (2 μm thick). The deformation of the KNN film caused the entire cantilever to bend and stretch (vibrate), causing the tip of the cantilever to continuously reciprocate up and down. The displacement Δ (piezoelectric displacement) of the cantilever tip at this time was measured by irradiating the cantilever tip with laser light L from a laser Doppler displacement meter, as shown in Figure 7(b). In this evaluation, the displacement Δ was measured every 1 million application cycles. The number of application cycles at which the displacement Δ became 80% or less of the initial value was defined as the AC stress life. If the displacement Δ remained 80% or more of the initial value even after the number of application cycles reached 50 million, the measurement was stopped and the measurement result of the AC stress life was defined as more than 50 million cycles (>50 million cycles). The measurement results are shown in Table 2 below.
[0125] In addition, in Figures 7(a) and 7(b), for ease of understanding, the lower adhesive layer and the upper adhesive layer are omitted, and the stack of the first KNN film and the second KNN film is illustrated as a KNN film.
[0126]
[0127] In Samples 1 to 6, the median value of the coercive field is a positive value, the relative dielectric constant is 490 or less, and the film stress is 150 MPa or less. That is, Samples 1 to 6 show that when depositing a KNN film, first, a first KNN film is deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second KNN film is deposited on the first KNN film at a second temperature at which the second KNN film becomes a spontaneous polarization film, thereby obtaining a KNN film having all three characteristics: a positive median value of the coercive field (Feature 1 described above), a relative dielectric constant is 490 or less (Feature 2 described above), and a film stress is 150 MPa or less (Feature 3 described above).
[0128] For Sample 7, in which the second temperature was set to 300°C, it was not possible to calculate the (001) orientation ratio or measure the median coercive field. This is believed to be because the crystal structure of the second KNN film did not become a perovskite structure. For Samples 8 to 10, the median coercive field was zero. This is believed to be because the second temperature for Samples 8 to 10 was above 500°C (600°C, 650°C). This confirms that if the second temperature is not a temperature at which the second KNN film becomes a spontaneous polarization film, a KNN film that is a spontaneous polarization film, i.e., a KNN film having the above-mentioned feature 1, cannot be obtained. For Samples 11 and 12, the relative dielectric constant was above 490 and the film stress was above 150 MPa. This is believed to be because the first temperature for Samples 11 and 12 was above 600°C (650°C). Furthermore, for Samples 13 and 14, the film stress was above 150 MPa. This is thought to be because the first temperature was less than 550° C. (500° C.) in Samples 13 and 14. Samples 11 to 14 confirm that unless the first temperature is a temperature at which the (001) orientation rate of the first KNN film is 95% or more and the film stress is 100 MPa or less, a KNN film having a relative dielectric constant of 490 or less and a film stress of 150 MPa or less, i.e., a KNN film having the above-mentioned features 2 and 3, cannot be obtained.
[0129] Furthermore, in Samples 1 to 6 and 8 to 10, the number of application cycles until the displacement Δ became 80% or less of the initial value exceeded 50 million, and they had excellent AC stress resistance. This is thought to be due to the presence of a first KNN film with a high (001) orientation rate and low film stress (for example, a first KNN film with a (001) orientation rate of 95% or more and a film stress of 100 MPa or less) between the bottom electrode film and the second KNN film.
[0130] In particular, Samples 1 to 6 have a positive median coercive field, a dielectric constant of 490 or less, a film stress of 150 MPa or less, and the number of application cycles described above exceeds 10 million (50 million or more). Thus, Samples 1 to 6 are confirmed to have, in addition to the above-mentioned Features 1 to 3, the additional feature of excellent AC stress resistance (Feature 4 described above). Samples 1 to 6 confirm that, when depositing a KNN film, a first KNN film is first deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second KNN film is deposited on the first KNN film at a second temperature that is a predetermined temperature higher than the first temperature, thereby obtaining a KNN film having all of the above-mentioned Features 1 to 4.
[0131] In contrast, in Sample 7, a large voltage sufficient to generate a unipolar AC electric field of 300 kV / cm could not be applied to the KNN film, and the number of application cycles could not be measured. This is thought to be because the crystal structure of the second KNN film did not become a perovskite structure, resulting in low voltage resistance of the KNN film. Furthermore, in Samples 11 to 16, the number of application cycles until the displacement Δ was 80% or less of the initial value was 10 million or less, resulting in low AC stress resistance. This is thought to be because in Samples 11 to 14, the first KNN film was not deposited at a temperature at which the (001) orientation ratio was 95% or more and the film stress was 100 MPa or less, i.e., the first KNN film had a low (001) orientation ratio and a large film stress. Furthermore, in samples 15 and 16, the KNN film is not constructed of a laminate of a first KNN film and a second KNN film. Specifically, this is thought to be because a KNN film with a high (001) orientation rate and low film stress (for example, a KNN film with a (001) orientation rate of 95% or more and a film stress of 100 MPa or less) is not interposed between the lower electrode film and the KNN film.
[0132] In the deposition of the KNN film, the deposition time at the first temperature was set to 6 minutes for Samples 1 to 14, but this is not limited to this. The inventors have confirmed that results similar to those described above can be obtained if the deposition time at the first temperature is in the range of 1 minute to 12 minutes. In the deposition of the KNN film, it has been confirmed that the deposition time at the first temperature, i.e., the optimal value for the thickness of the KNN film deposited at the first temperature, may have a certain degree of range.
[0133] (Regarding evaluation of film stress) In the above-mentioned Experiments 1 and 2, the film stress of the KNN film was calculated from the amount of warpage of the substrate (Si substrate), i.e., the radius of curvature of the warpage of the substrate, but this is not limiting. The film stress of the KNN film can also be determined in the state of a piezoelectric element (piezoelectric device module) in which a MEMS structure is fabricated by processing a piezoelectric laminate by comparing the MEMS simulation with the shape of the actual object.
[0134] (Evaluation of the necessity of polarization treatment) Using simple piezoelectric elements made from the piezoelectric laminates of sample 3, whose median coercive field is a positive value, and sample 9, whose median coercive field is zero (0), we confirmed whether the KNN films of samples 3 and 9 were spontaneous polarization films, that is, we evaluated whether polarization treatment was necessary.
[0135] In a piezoelectric film such as a KNN film, the polarization direction is aligned in a certain direction, and when an electric field is applied in that polarization direction, the film undergoes piezoelectric deformation. Therefore, by applying a low voltage (electric field) to a KNN film that has not been subjected to polarization treatment and checking whether the KNN film deforms, it is possible to determine whether the KNN film is a spontaneous polarization film, i.e., whether polarization treatment is necessary.
[0136] The necessity of polarization treatment was confirmed by carrying out the following measurements (a) to (e) in order. The graphs obtained from measurements (a) to (e) are shown in Figures 8(a) to 8(e) and Figures 9(a) to 9(e). Figures 8(a) to 8(e) are graphs for Sample 3, and Figures 9(a) to 9(e) are graphs for Sample 9.
[0137] <Measurement (a)> First, using the simplified piezoelectric elements fabricated from Samples 3 and 9, with the lower electrode film grounded, a sine wave voltage of -2 V to +2 V (a sine wave electric field of -10 kV / cm to +10 kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1 kHz, and the displacement of the KNN film (surface of the upper electrode film) was measured (Measurement (a)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The graphs obtained in Measurement (a) are shown in Figure 8(a) and Figure 9(a), respectively.
[0138] <Measurement (b)> After measurement (a) was completed, a sine wave voltage of 0 V to −30 V (a sine wave electric field of 0 kV / cm to −300 kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1 kHz with the lower electrode film grounded, and the displacement of the KNN film (surface of the upper electrode film) was measured (measurement (b)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The application of a voltage of −30 V in measurement (b) corresponds to the implementation of a process for aligning polarization in an upward direction (hereinafter also referred to as "upward polarization process"). The graphs obtained in measurement (b) are shown in Figures 8(b) and 9(b), respectively.
[0139] <Measurement (c)> After the measurement (b), a sine wave voltage of -2 V to +2 V (a sine wave electric field of -10 kV / cm to +10 kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1 kHz with the lower electrode film grounded again, and the displacement of the KNN film (surface of the upper electrode film) was measured (Measurement (c)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The graphs obtained in Measurement (c) are shown in Figure 8(c) and Figure 9(c), respectively.
[0140] <Measurement (d)> After measurement (c) was completed, a sine wave voltage of 0 V to +30 V (a sine wave electric field of 0 kV / cm to +300 kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1 kHz with the lower electrode film grounded, and the displacement of the KNN film (surface of the upper electrode film) was measured (measurement (d)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The application of a voltage of +30 V in measurement (d) corresponds to the implementation of a process for aligning polarization in a downward direction (hereinafter also referred to as "downward polarization process"). The graphs obtained in measurement (d) are shown in Figures 8(d) and 9(d), respectively.
[0141] <Measurement (e)> After the end of measurement (d), a sine wave voltage of -2 V to +2 V (a sine wave electric field of -10 kV / cm to +10 kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1 kHz with the lower electrode film grounded again, and the displacement of the KNN film (surface of the upper electrode film) was measured (measurement (e)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The graphs obtained in measurement (e) are shown in Figure 8(e) and Figure 9(e), respectively.
[0142] For the simplified piezoelectric element of Sample 3, a clear piezoelectric displacement can be seen in the graph shown in FIG. 8(a). It can also be seen that the piezoelectric displacement in the graph shown in FIG. 8(c) is similar to that in the graph shown in FIG. 8(a). From these results, it can be seen that the polarization direction of the KNN film of Sample 3 is aligned in the upward direction even in the initial state before polarization treatment. In other words, it can be seen that the KNN film of Sample 3 is a spontaneously polarized film. Furthermore, it can be seen that the piezoelectric displacement in the graph shown in FIG. 8(e) is similar to that in the graphs shown in FIGS. 8(a) and 8(c). This indicates that the initial polarization state (upward polarization) is maintained even after the treatment corresponding to the downward polarization treatment (Measurement (d)), which is the opposite direction to the treatment corresponding to the upward polarization treatment (Measurement (b)). From these results, it can be seen that the spontaneous polarization generated in the KNN film of Sample 3 is maintained even after the application of a large voltage (whether forward or reverse). That is, it is clear that the polarization process is not necessary for sample 3.
[0143] On the other hand, for the simplified piezoelectric element of Sample 9, no clear piezoelectric displacement was observed in the graph shown in Figure 9(a), but piezoelectric displacement was observed in the graph shown in Figure 9(c). This indicates that the upward polarization process (Measurement (b)) in Sample 9 caused the polarization direction of the KNN film to align in the upward (forward) direction. Furthermore, Figure 9(e) shows a piezoelectric displacement in the opposite direction to that shown in Figure 9(c). This indicates that the downward polarization process (Measurement (d)), which is the opposite direction to the upward polarization process (Measurement (b)), changed the polarization direction of the KNN film to align in the downward direction. These results indicate that the KNN film of Sample 9 does not exhibit spontaneous polarization, and that this KNN film has the property of aligning its polarization direction in the direction of applied voltage after a large voltage is applied (whether forward or reverse). Such a property of the KNN film of Sample 9 is a general property of a KNN film (piezoelectric film) that requires polarization treatment. In other words, it is clear that Sample 9 requires polarization treatment.
[0144] (Evaluation of Temperature Resistance of Spontaneous Polarization) Using simple piezoelectric elements fabricated from the piezoelectric laminates of Samples 1 and 2, the temperature resistance of the spontaneous polarization generated in the KNN film was evaluated.
[0145] First, using the simplified piezoelectric element fabricated from Sample 1, with the lower electrode film grounded, a sine wave voltage of −2 V to +2 V (a sine wave electric field of −10 kV / cm to +10 kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1 kHz, and the displacement of the KNN film (surface of the upper electrode film) was measured, and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in FIG. 10(a). The simplified piezoelectric element was then placed in an air atmosphere at 400°C for 2 hours. Thereafter, with the lower electrode film again grounded, a sine wave voltage of −2 V to +2 V (a sine wave electric field of −10 kV / cm to +10 kV / cm) was applied to the KNN film via the upper electrode film at a frequency of 1 kHz, and the displacement of the KNN film (surface of the upper electrode film) was measured, and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in FIG.
[0146] Furthermore, using a simplified piezoelectric element fabricated from Sample 2, a sine wave voltage of −2 V to +2 V (a sine wave electric field of −10 kV / cm to +10 kV / cm) was applied to the KNN film via the upper electrode film with a frequency of 1 kHz while the lower electrode film was grounded. The displacement of the KNN film (surface of the upper electrode film) was measured, and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in FIG. 11(a). The simplified piezoelectric element was then placed in an air atmosphere at 500°C for 2 hours. Thereafter, again, with the lower electrode film grounded, a sine wave voltage of −2 V to +2 V (a sine wave electric field of −10 kV / cm to +10 kV / cm) was applied to the KNN film via the upper electrode film with a frequency of 1 kHz while the lower electrode film was grounded. The displacement of the KNN film (surface of the upper electrode film) was measured, and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in FIG.
[0147] 10(a) and 10(b) show that the piezoelectric displacement of the KNN film is almost unchanged before and after exposure to an atmosphere at 400° C. Also, from FIGS. 11(a) and 11(b), it can be seen that the piezoelectric displacement of the KNN film is almost unchanged before and after exposure to an atmosphere at 500° C. These results demonstrate that the polarization characteristics of the KNN film, which is a spontaneous polarization film formed by the method of the present disclosure, are maintained even when the KNN film is subjected to a thermal history of 400° C. and even 500° C.
[0148] The KNN film of Sample 8 was also subjected to polarization treatment, and the temperature resistance of the polarization generated in the KNN film of Sample 8 was evaluated. Specifically, a simple piezoelectric element fabricated from Sample 8 was first prepared and subjected to downward polarization treatment (i.e., the above-described measurement (b)). Then, using the same method as Samples 1 and 2, the displacement of the KNN film was observed before and after exposure to a 400°C or 500°C atmosphere. As a result, it was confirmed that the piezoelectric displacement of the KNN film of Sample 8 changed before and after exposure to a 400°C or 500°C atmosphere. Specifically, while a clear piezoelectric displacement was observed in Sample 8 before exposure to a 400°C or 500°C atmosphere, no clear piezoelectric displacement was observed after exposure to a 400°C or 500°C atmosphere. In other words, it was confirmed that no polarization occurred in the KNN film of Sample 8 after exposure to a 400°C or 500°C atmosphere.
[0149] (Evaluation of Heat Resistance of Piezoelectric Elements) Using piezoelectric elements (membrane-type MEMS devices) fabricated from the piezoelectric laminates of Samples 3 and 9, the heat resistance of the piezoelectric elements was evaluated.
[0150] First, a piezoelectric element chip was fabricated as follows. The piezoelectric laminates of Samples 3 and 9 were prepared, and an insulating film was provided from the upper electrode film to the lower electrode film so as to cover part of the side surface of the KNN film of each sample. In this experiment, a 5 nm thick aluminum oxide (Al 2 O 3 ) layer and Al 2 O 3 A 500 nm thick silicon oxide (SiO 2 ) layer and a laminate of the CF 4The insulating film was patterned by dry etching using gas. Then, a laminate was formed as a metal wiring layer, consisting of a 10 nm thick Ti layer and a 300 nm thick Au layer provided on the Ti layer. The metal wiring layer was then patterned by wet etching to form metal wiring of a predetermined pattern. Furthermore, a portion of the Si substrate was removed from the back side of the Si substrate by deep-RIE etching to form a membrane structure. The piezoelectric laminate (each sample) was then divided into chips to produce multiple piezoelectric element chips as shown in FIG. 3.
[0151] Then, a polarization process was performed on the piezoelectric element chip fabricated using the piezoelectric laminate of Sample 9, in which spontaneous polarization was not generated, by applying a DC voltage of −30 V to the KNN film via the upper electrode film by probing. Note that the polarization process was not performed on the piezoelectric element chip fabricated using the piezoelectric laminate of Sample 3, in which spontaneous polarization was generated.
[0152] The obtained piezoelectric element chips were then mounted in packages (by bonding and wire bonding). In order to evaluate the heat resistance of the fabricated piezoelectric element chips, the heat treatment temperatures during package mounting (hereinafter also referred to as "PKG temperatures") were set to 200°C and 300°C.
[0153] In this piezoelectric element (membrane-type MEMS device), the membrane structure is deformed by the sound pressure of ultrasonic waves, generating a voltage from the KNN film. In other words, this piezoelectric element functions as an ultrasonic sensor. Ultrasonic waves were applied to each of the fabricated piezoelectric element chips to evaluate the sensitivity of the piezoelectric element to ultrasonic waves (i.e., sensor sensitivity, hereinafter also referred to as "ultrasonic sensitivity"). The evaluation results are shown in Table 3 below. In the "ultrasonic sensitivity" column in Table 3, "pass" means that the piezoelectric element operated normally after packaging, and "fail" means that the piezoelectric element did not operate normally after packaging.
[0154]
[0155] The piezoelectric element fabricated using the piezoelectric laminate of Sample 3 operated normally regardless of the package temperature.
[0156] On the other hand, the piezoelectric element fabricated using the piezoelectric laminate of Sample 9 and subjected to polarization treatment operated normally when the package temperature was 200°C, but not when the package temperature was 300°C. This indicates that the ultrasonic sensitivity of the piezoelectric element subjected to a thermal history of 300°C after polarization treatment deteriorates. This is presumably because the polarization direction of the KNN film, which was aligned by polarization treatment, becomes disturbed by exposure to high temperatures. This indicates that the piezoelectric element fabricated using the spontaneously polarized KNN film has higher heat resistance than the piezoelectric element subjected to polarization treatment. This indicates that the piezoelectric element has high heat resistance and is highly reliable.
[0157] <Preferred Aspects of the Present Disclosure> Preferred aspects of the present disclosure will be additionally described below.
[0158] (Supplementary Note 1) According to one aspect of the present disclosure, there is provided a piezoelectric device comprising: a substrate; a lower electrode film formed on the substrate; and a piezoelectric film formed on the lower electrode film and made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, wherein a coercive field E C + and the coercive field E on the negative field side C - and the median value of the coercive electric field between the piezoelectric film and the piezoelectric film is a positive value; the dielectric constant of the piezoelectric film is 490 or less; and the film stress of the piezoelectric film is 150 MPa or less.
[0159] (Supplementary Note 2) In the piezoelectric laminate according to Supplementary Note 1, preferably, in the hysteresis curve, the coercive electric field E when the thickness of the piezoelectric film is 2 μm C + and the coercive electric field E C - The median value of the coercive electric field between the electrodes is 10 kV / cm or more.
[0160] (Appendix 3) In the piezoelectric laminate according to Appendix 1 or 2, preferably, when a negative voltage is continuously applied to the upper electrode film so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and an upper electrode film provided on the piezoelectric film, the number of cycles of application of the voltage until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.
[0161] (Supplementary Note 4) In the piezoelectric stack according to any one of Supplementary Notes 1 to 3, preferably, the piezoelectric film contains, as a dopant, at least one element selected from copper and manganese at a concentration of 0.1 at % or more and 2.0 at % or less.
[0162] (Supplementary Note 5) In the piezoelectric laminate according to any one of Supplementary Notes 1 to 4, preferably, a layer containing zinc and oxygen is provided between the substrate and the piezoelectric film.
[0163] (Appendix 6) According to another aspect of the present disclosure, there is provided a method for manufacturing a piezoelectric stack, comprising: a step of depositing a lower electrode film on a substrate; and a step of depositing a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film, wherein in the step of depositing the piezoelectric film, first, a first piezoelectric film that is a part of the piezoelectric film is deposited at a first temperature at which a (001) orientation rate is 95% or more and a film stress is 100 MPa or less, and then a second piezoelectric film that is another part of the piezoelectric film is deposited on the first piezoelectric film at a second temperature at which the second piezoelectric film becomes a spontaneous polarization film.
[0164] (Supplementary Note 7) In the method according to Supplementary Note 6, preferably, the thickness of the first piezoelectric film is 20% or less of the total thickness of the piezoelectric film.
[0165] (Appendix 8) In the method according to appendix 6 or 7, preferably, the first temperature is a temperature at which, when the first piezoelectric film is deposited to a thickness of 2 μm at the first temperature, the (001) orientation rate of the first piezoelectric film is 95% or more.
[0166] (Appendix 9) In the method according to any one of Appendices 6 to 8, preferably, the first temperature is a temperature at which the film stress of the first piezoelectric film becomes 100 MPa or less when the first piezoelectric film is formed to a thickness of 2 μm at the first temperature.
[0167] (Appendix 10) The method according to any one of Appendices 6 to 9 preferably further comprises a step of providing a layer containing zinc and oxygen on the substrate before the step of depositing the piezoelectric film, and in the step of depositing the piezoelectric film, the piezoelectric film is deposited on the layer containing zinc and oxygen.
[0168] (Supplementary Note 11) According to yet another aspect of the present disclosure, there is provided a piezoelectric device comprising: a substrate; a lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; and an upper electrode film formed on the piezoelectric film, wherein a coercive field E on the positive electric field side is smaller than a coercive field E on the positive electric field side in a hysteresis curve obtained by applying an electric field to the piezoelectric film under predetermined conditions and showing a correlation between the amount of polarization and the applied electric field. C + and the coercive field E on the negative field side C - and the median value of the coercive electric field between the piezoelectric film and the piezoelectric element or the piezoelectric device module is a positive value; the relative dielectric constant of the piezoelectric film is 490 or less; and the film stress of the piezoelectric film is 150 MPa or less.
[0169] (Supplementary Note 12) According to yet another aspect of the present disclosure, there is provided a piezoelectric element or a piezoelectric device module utilizing the polarization characteristics of a piezoelectric film, wherein a coercive electric field E on the positive electric field side is smaller than a coercive electric field E on the positive electric field side in a hysteresis curve showing a correlation between the amount of polarization and the applied electric field obtained by applying an electric field under predetermined conditions. C + and the coercive field E on the negative field side C - The present invention provides a piezoelectric element or a piezoelectric device module that is equipped with a piezoelectric film having a positive median value of the coercive electric field between the piezoelectric film and the sensor, and that does not deteriorate in sensor sensitivity (maintains sensor sensitivity) even when subjected to a thermal history of 300°C.
[0170] (Supplementary Note 13) According to yet another aspect of the present disclosure, there is provided a piezoelectric film made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, wherein a coercive field E on the positive electric field side is smaller than a coercive field E on the positive electric field side in a hysteresis curve showing a correlation between the amount of polarization and the applied electric field obtained by applying an electric field under predetermined conditions to the piezoelectric film. C + and the coercive field E on the negative field side C - and a positive median value of the coercive electric field between the piezoelectric film and the dielectric constant of the piezoelectric film is 490 or less, and the film stress is 150 MPa or less.
[0171] (Supplementary Note 14) According to still another aspect of the present disclosure, in a hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under predetermined conditions, a coercive electric field E C + and the coercive field E on the negative field side C - and the median value of the coercive field between the film and the temperature is positive, and the polarization characteristics are maintained even when the film is subjected to a thermal history of 400° C. or higher.
[0172] (Appendix 15) The piezoelectric film, piezoelectric element, or piezoelectric device module according to any one of Appendices 11 to 14, preferably, when a negative voltage is continuously applied to the upper electrode film (an upper electrode film provided on the piezoelectric film) so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and the upper electrode film (in the piezoelectric film), the number of cycles of application of the voltage until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.
[0173] REFERENCE SIGNS LIST 1 substrate 2 lower electrode film 3 piezoelectric film 4 upper electrode film 6 lower adhesive layer 10 piezoelectric laminate 20 piezoelectric element 30 piezoelectric device module
Claims
1. A piezoelectric film comprising: a substrate; a lower electrode film formed on the substrate; and a piezoelectric film formed on the lower electrode film and made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; wherein a coercive electric field E on the positive electric field side is a hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under predetermined conditions to the piezoelectric film. C + and the coercive electric field E on the negative electric field side C - a median value of a coercive electric field between said piezoelectric film and said piezoelectric layer is a positive value; a relative dielectric constant of said piezoelectric film is 490 or less; and a film stress of said piezoelectric film is 150 MPa or less.
2. The piezoelectric stack described in claim 1, wherein when a negative AC voltage is continuously applied to the upper electrode film so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and an upper electrode film provided on the piezoelectric film, the number of cycles of voltage application until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.
3. The piezoelectric stack according to claim 1 or 2, wherein the piezoelectric film contains at least one element selected from copper and manganese as a dopant at a concentration of 0.1 at % or more and 2.0 at % or less.
4. A method for manufacturing a piezoelectric laminate, comprising: a step of depositing a lower electrode film on a substrate; and a step of depositing a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film, wherein in the step of depositing the piezoelectric film, first, a first piezoelectric film, which is a part of the piezoelectric film, is deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then, a second piezoelectric film, which is the other part of the piezoelectric film, is deposited on the first piezoelectric film at a second temperature at which the second piezoelectric film becomes a spontaneously polarized film.
5. A piezoelectric device comprising: a substrate; a lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; and an upper electrode film formed on the piezoelectric film; and a coercive electric field E on the positive electric field side in a hysteresis curve showing the correlation between the polarization amount and the applied electric field obtained by applying an electric field under predetermined conditions to the piezoelectric film. C + and the coercive electric field E on the negative electric field side C - a median value of a coercive electric field between said piezoelectric film and said piezoelectric element is a positive value; a relative dielectric constant of said piezoelectric film is 490 or less; and a film stress of said piezoelectric film is 150 MPa or less.
6. The piezoelectric element according to claim 5, wherein when a negative AC voltage is continuously applied to the upper electrode film so as to generate a unipolar electric field of 300 kV / cm between the lower electrode film and the upper electrode film, the number of cycles of voltage application until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.
Citation Information
Patent Citations
Piezoelectric thin film element and manufacturing method of piezoelectric thin film element, and piezoelectric thin film device
JP2011029591A
Piezoelectric thin-film device, piezoelectric sensor, and vibration power generator
JP2014207429A
Piezoelectric elements, piezoelectric actuators, hard disk drives, inkjet printers, and piezoelectric sensors
JP2015529963A
Piezoelectric thin film-attached laminate board, piezoelectric thin-film device and manufacturing method thereof
JP2017076730A