Blocked polyisocyanate composition, curing agent for aqueous coating, aqueous coating composition, and coating film
The block polyisocyanate composition with alkoxy polyethylene oxide and quaternary ammonium salt addresses the short pot life and temperature limitations of conventional polyisocyanate paints, achieving excellent low-temperature curability and workability in water-based paints, suitable for diverse painting applications.
Patent Information
- Application Number
- PCT/JP2024/002924
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-01-30
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional polyisocyanate-based paints have a short pot life due to rapid hardening and cannot be used in water-based systems, limiting their workability and application in water-based paints, especially at low temperatures, which is a challenge for reducing costs and carbon emissions in painting processes.
A block polyisocyanate composition with an alkoxy polyethylene oxide group and a quaternary ammonium salt as a blocking agent dissociation catalyst, allowing for low-temperature curability and extended pot life by controlling the reaction of isocyanate groups with polyols in water-based paints.
The block polyisocyanate composition enables the formation of a coating film with excellent low-temperature curability and improved workability, allowing for efficient application and curing at temperatures as low as 100°C or lower, enhancing the usability of water-based paints on various substrates, including plastics.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Blocked polyisocyanate composition, curing agent for water-based paint, water-based paint composition and coating film
[0001] The present disclosure relates to a blocked polyisocyanate composition, a curing agent for an aqueous coating material, an aqueous coating material composition, and a coating film.
[0002] Polyisocyanates have been known as components of compositions used in adhesives, paints, etc. For example, polyurethane resin paints, which combine polyols and polyisocyanates, are known to have excellent abrasion resistance, chemical resistance, and stain resistance.
[0003] Paints using polyisocyanate as a curing agent are generally two-component compositions containing a base component (e.g., polyol) and a polyisocyanate. In two-component compositions, the base component and the polyisocyanate are stored separately and mixed together before use. However, once mixed, the paint cures in a short time, resulting in a short usable time and problems with workability during application. Furthermore, because polyisocyanate readily reacts with water, it has been impossible to use polyisocyanate in water-based paints such as electrodeposition paints.
[0004] To address the above-mentioned problems, a method of inactivating polyisocyanate by reacting it with an active hydrogen group-containing compound called a blocking agent is known. The blocked polyisocyanate obtained by this method does not react with the base component (such as a polyol) at room temperature, but when heated, the blocking agent dissociates, regenerating the isocyanate group, which then reacts with the base component to form crosslinks. Therefore, blocked polyisocyanate has no limit on its pot life, and it can be prepared as a paint by mixing the base component and curing agent component in advance, making it possible to apply polyisocyanate to water-based paints.
[0005] Conventionally, as a catalyst for dissociating the blocking agent from the blocked polyisocyanate (blocking agent dissociation catalyst), a quaternary ammonium salt, a metal catalyst, or the like has been used (for example, Patent Documents 1 to 3).
[0006] JP-A-06-192364 JP-A-08-170048 Patent No. 5073978
[0007] In recent years, there has been a demand for coating films to be cured at lower temperatures than before, with the aim of reducing costs during baking and carbon dioxide emissions, and also to enable coating on plastic members. However, when the above-mentioned blocking agent dissociation catalysts are used, it is difficult to obtain sufficient low-temperature curing properties in aqueous coating compositions.
[0008] An object of one aspect of the present disclosure is to provide an aqueous coating composition that uses a blocked polyisocyanate composition and has excellent low-temperature curing properties.
[0009] The present disclosure provides at least the following [1] to
[10] .
[0010] [1] A blocked polyisocyanate composition comprising a blocked polyisocyanate and a blocking agent dissociation catalyst, wherein the blocked polyisocyanate has an alkoxypolyethylene oxide group containing an average of 14 to 50 ethylene oxide units, and the blocking agent dissociation catalyst comprises a quaternary ammonium salt.
[0011] [2] The blocked polyisocyanate composition according to [1], wherein the number of ethylene oxide units contained in the alkoxypolyethylene oxide group is 15 to 25 on average.
[0012] [3] The blocked polyisocyanate composition according to [1] or [2], wherein the content of the alkoxy polyethylene oxide group is 5 to 30 mass% based on the total amount of isocyanate compounds in the isocyanate composition obtained by dissociating the blocking agent from the blocked polyisocyanate.
[0013] [4] The blocked polyisocyanate composition according to [1] or [2], wherein the content of the alkoxy polyethylene oxide group is 5 to 25 mass% based on the total amount of isocyanate compounds in the isocyanate composition obtained by dissociating the blocking agent from the blocked polyisocyanate.
[0014] [5] The blocked polyisocyanate composition according to any one of [1] to [4], wherein the blocked polyisocyanate contains a structure derived from an aliphatic polyisocyanate having 4 to 6 carbon atoms or a derivative thereof.
[0015] [6] The blocked polyisocyanate composition according to any one of [1] to [5], wherein the quaternary ammonium salt contains a cationic group represented by the following formula (1):
[0016] [In formula (1), R 1 represents an alkyl group having 1 to 16 carbon atoms which may have a hydroxy group, an amino group or an alkoxy group as a substituent, and R 2 ~R 4 each independently represents an alkyl group having 1 to 8 carbon atoms.
[0017] [7] The blocked polyisocyanate composition according to any one of [1] to [6], wherein the blocked polyisocyanate has an isocyanate group blocked with an oxime-based blocking agent.
[0018] [8] A curing agent for aqueous coating materials, comprising the blocked polyisocyanate composition according to any one of [1] to [7].
[0019] [9] An aqueous coating composition comprising a compound having two or more isocyanate-reactive groups, a blocked polyisocyanate, a blocking agent dissociation catalyst, and water, wherein the blocked polyisocyanate has alkoxypolyethylene oxide groups containing an average of 14 to 50 ethylene oxide units, and the blocking agent dissociation catalyst contains a quaternary ammonium salt.
[0020]
[10] A coating film formed from the aqueous coating composition according to [9].
[0021] According to one aspect of the present disclosure, it is possible to provide an aqueous coating composition that is excellent in low-temperature curing properties by using a blocked polyisocyanate composition.
[0022] Illustrative embodiments of the present disclosure will be described below. However, the present disclosure is not limited to the following embodiments. In this specification, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. Furthermore, unless specifically stated otherwise, the units of the numerical values before and after "to" are the same. Furthermore, the upper and lower limit values individually stated can be combined in any combination. Furthermore, in this specification, room temperature means 5 to 35°C.
[0023] <Blocked Polyisocyanate Composition> One embodiment of the present disclosure is a blocked polyisocyanate composition containing a blocked polyisocyanate and a blocking agent dissociation catalyst, wherein the blocked polyisocyanate has alkoxypolyethylene oxide groups containing an average of 14 to 50 ethylene oxide units (hereinafter also referred to as "EO units"), and the blocking agent dissociation catalyst contains a quaternary ammonium salt. Hereinafter, the blocked polyisocyanate having the specific alkoxypolyethylene oxide groups will be referred to as "blocked polyisocyanate (A)."
[0024] The blocked polyisocyanate (A) may have hydrophilic properties due to the presence of the alkoxypolyethylene oxide group, and therefore, the blocked polyisocyanate (A) can also be referred to as an aqueous blocked polyisocyanate.
[0025] The above-described blocked polyisocyanate composition provides an aqueous coating composition with excellent low-temperature curing properties. "Excellent low-temperature curing properties" means that the composition is resistant to solvent (e.g., methyl ethyl ketone) dissolution and capable of forming a coating film with high hardness, even when cured at low temperatures (e.g., temperatures below 100°C). The reason for this effect is unclear, but it is thought to be due to the fact that the blocked polyisocyanate (A) contains alkoxypolyethylene oxide groups containing an average of 14 to 50 EO units, allowing the blocked polyisocyanate (A) and the quaternary ammonium salt to coexist in a well-dispersed state, facilitating the release of the blocking agent by the blocking agent release catalyst (quaternary ammonium salt). Furthermore, the number of EO units is not too high, which facilitates the formation of a densely structured film after curing.
[0026] (Blocked Polyisocyanate) The blocked polyisocyanate (A) is a compound that can be derived from a polyisocyanate that does not have an isocyanate group blocked with a blocking agent and an alkoxypolyethylene oxide group (hereinafter also referred to as a "non-aqueous unblocked polyisocyanate"). The blocked polyisocyanate (A) has, for example, a structure derived from a non-aqueous unblocked polyisocyanate, an alkoxypolyethylene oxide group containing an average of 14 to 50 EO units, and an isocyanate group blocked with a blocking agent (hereinafter also referred to as a "blocked isocyanate group").
[0027] [Non-aqueous Unblocked Polyisocyanate] Non-aqueous unblocked polyisocyanates are compounds that have multiple isocyanate groups (free isocyanate groups) and do not have isocyanate groups blocked with a blocking agent or alkoxypolyethylene oxide groups. Examples of non-aqueous unblocked polyisocyanates include aromatic polyisocyanates, aliphatic polyisocyanates, alicyclic polyisocyanates, and polyisocyanate derivatives thereof. Examples of derivatives include isocyanurates, allophanates, biurets, etc. The derivative may be an isocyanate group-containing prepolymer obtained by reacting the above polyisocyanate with a polyol, or a derivative of the prepolymer (e.g., an isocyanurate, allophanate, biuret, etc.). As the polyol, for example, a diol having 2 to 9 carbon atoms is used. Examples of such diols include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, and 2-ethyl-1,3-hexanediol.
[0028] The non-aqueous unblocked polyisocyanate does not need to have an aromatic ring, from the viewpoint of improving the yellowing resistance of the cured coating film. That is, the non-aqueous unblocked polyisocyanate may be a non-aromatic polyisocyanate. Examples of non-aromatic polyisocyanates include aliphatic polyisocyanates such as hexamethylene diisocyanate, tetramethylene diisocyanate, 2-methyl-pentane-1,5-diisocyanate, 3-methyl-pentane-1,5-diisocyanate, lysine triisocyanate, and trioxyethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate, cyclohexyl diisocyanate, hydrogenated diphenylmethane diisocyanate, norbornane diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated xylene diisocyanate, and hydrogenated tetramethylxylene diisocyanate, and derivatives thereof.
[0029] The nonaqueous unblocked polyisocyanate may contain an aliphatic polyisocyanate having 4 to 6 carbon atoms or a derivative thereof from the viewpoint of further improving curability, and may contain hexamethylene diisocyanate or a derivative thereof from the viewpoint of further improving curability. In other words, the blocked polyisocyanate (A) may have a structure derived from an aliphatic polyisocyanate having 4 to 6 carbon atoms or a derivative thereof, or may have a structure derived from hexamethylene diisocyanate or a derivative thereof. As the derivative of hexamethylene diisocyanate, at least one selected from the group consisting of an isocyanurate, an allophanate, and a biuret may be used. In particular, when an isocyanurate is used, the coating hardness can be further improved. The isocyanate compound may be an isocyanurate compound of hexamethylene diisocyanate, or may be an isocyanate compound of an isocyanate group-containing prepolymer obtained by reacting hexamethylene diisocyanate with a polyol (for example, the above-mentioned diol).
[0030] When a non-aqueous unblocked polyisocyanate containing an isocyanurate compound is used, from the viewpoint of further improving the coating hardness, the content of the isocyanurate trimer (isocyanurate trimer content) based on the total mass of the non-aqueous unblocked polyisocyanate may be 50 mass% or more, and the content of the isocyanurate groups (isocyanurate group content) relative to the total (100 mol%) of the isocyanurate groups and allophanate groups in the non-aqueous unblocked polyisocyanate may be more than 80 mol%. The upper limit of the isocyanurate trimer content may be 80 mass%, and the upper limit of the isocyanurate group content may be 99 mol%.
[0031] [Alkoxypolyethyleneoxide Group] The alkoxypolyethyleneoxide group is a group represented by the formula: -(OCH 2 CH 2 ) n OR, where n represents the number of EO units (hereinafter also referred to as "the number of EO units"), and R represents an alkyl group.
[0032] The alkoxypolyethylene oxide groups contain an average of 14 to 50 EO units. "An average of 14 to 50" means that, when the blocked polyisocyanate (A) contains a plurality of alkoxypolyethylene oxide groups, the average value calculated by dividing the total number of EO units contained in those groups by the total number of alkoxypolyethylene oxide groups (total number of EO units / total number of alkoxypolyethylene oxide groups) is 14 to 50. In calculating the average number of EO units, any decimal point is rounded off.
[0033] From the viewpoint of making it easier to obtain an aqueous coating composition with excellent low-temperature curing properties, the average number of EO units contained in the alkoxypolyethylene oxide group may be 14 to 45, or 15 to 30, or 15 to 25. The average number of EO units contained in the alkoxypolyethylene oxide group may be 20 or more, 30 or more, or 40 or more.
[0034] The alkyl group (R) contained in the alkoxypolyethylene oxide group may be linear, branched, or cyclic. The number of carbon atoms in the alkyl group (R) is, for example, 1 to 18, and may be 1 to 12, 1 to 6, or 1 to 2. Specific examples of the alkyl group (R) include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, 2-ethylhexyl, 2-propylheptyl, nonyl, decyl, isodecyl, dodecyl, hexadecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, and octadecyl groups. Among these, when the alkyl group (R) is a methyl or ethyl group, the low-temperature curing properties of the aqueous coating composition tend to be further improved.
[0035] The alkoxypolyethylene oxide group is a polyethylene glycol monoalkyl ether (H(OCH 2 CH 2 ) n OR) and an isocyanate group (—NHCO(OCH 2 CH 2 ) n OR).
[0036] The polyethylene glycol monoalkyl ether has a number average molecular weight such that the average number of EO units falls within the above range. The number average molecular weight of the polyethylene glycol monoalkyl ether may be, for example, 200 to 10,000, 200 to 2,000, or 200 to 1,000. The lower limit of the number average molecular weight of the polyethylene glycol monoalkyl ether may be 400 or 600. The number average molecular weight is measured using gel permeation chromatography (GPC) and means a value determined using polystyrene as a standard substance.
[0037] From the viewpoint of easily obtaining an aqueous coating composition having excellent low-temperature curing properties, the content of alkoxypolyethylene oxide groups may be 5% by mass or more, 10% by mass or more, 15% by mass or more, or 20% by mass or more, based on the total amount of isocyanate compounds in the isocyanate composition obtained by dissociating the blocking agent from the blocked polyisocyanate (A). From the viewpoint of easily obtaining an aqueous coating composition having excellent low-temperature curing properties, the content of alkoxypolyethylene oxide groups may be 30% by mass or less, 25% by mass or less, or 20% by mass or less, based on the total amount of isocyanate compounds in the isocyanate composition obtained by dissociating the blocking agent from the blocked polyisocyanate (A). From these viewpoints, the content of alkoxypolyethylene oxide groups may be 5 to 30% by mass, 5 to 25% by mass, or 5 to 20% by mass, based on the total amount of isocyanate compounds in the isocyanate composition obtained by dissociating the blocking agent from the blocked polyisocyanate (A). In this specification, the term "isocyanate compound" means a compound having an isocyanate group.
[0038] The content of alkoxypolyethylene oxide groups based on the total mass of hydrophilic groups in the blocked polyisocyanate (A) may be 90 mass% or more, or may be 95 mass% or more, from the viewpoint of achieving better low-temperature curing properties. The blocked polyisocyanate (A) may not have hydrophilic groups other than alkoxypolyethylene oxide groups.
[0039] [Blocked Isocyanate Group] The blocked isocyanate group is an isocyanate group blocked with a blocking agent, and has a structure derived from the blocking agent.
[0040] Examples of the blocking agent include alcohol-based blocking agents such as methanol, ethanol, n-butanol, isobutanol, 2-ethylhexanol, butyl cellosolve, propylene glycol monomethyl ether, ethylene glycol, and benzyl alcohol; phenol-based blocking agents such as phenol, cresol, ethylphenol, butylphenol, and 2-hydroxypyridine; lactam-based blocking agents such as ε-caprolactam, δ-valerolactam, and γ-butyrolactam; and blockers such as formaldoxime, acetaldoxime, acetoneoxime, methyl ethyl ketoxime, methyl isobutyl ketoxime, and cyclohexanone oxime. Examples of suitable blocking agents include oxime-based blocking agents, imidazole-based blocking agents such as imidazole, 2-methylimidazole, 4-methylimidazole, 2,4-dimethylimidazole, 2-ethylimidazole, 2-propylimidazole, 2-isopropylimidazole, 4-methyl-2-propylimidazole, 2-phenylimidazole, 4-phenylimidazole, 5-phenylimidazole, 2-methyl-4-phenylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, and 2-heptadecylimidazole, and amine-based blocking agents such as diphenylamine, diisopropylamine, and isopropylethylamine. Among these, oxime-based blocking agents may be used from the viewpoint of improving storage stability, and methyl ethyl ketoxime may be used from the viewpoint of further improving storage stability.
[0041] The blocked polyisocyanate (A) may have free isocyanate groups, or from the viewpoint of improving storage stability, it may not have free isocyanate groups. For example, all of the available isocyanate groups in the blocked polyisocyanate (A) may be blocked isocyanate groups. Here, the term "available isocyanate groups" refers to both free isocyanate groups and blocked isocyanate groups.
[0042] The blocked polyisocyanate (A) can be obtained, for example, by reacting the nonaqueous unblocked polyisocyanate, the poly(oxyethylene) glycol monoalkyl ether, and the blocking agent. That is, the blocked polyisocyanate (A) can be a reaction product of the nonaqueous unblocked polyisocyanate, the poly(oxyethylene) glycol monoalkyl ether, and the blocking agent. The nonaqueous unblocked polyisocyanate, the poly(oxyethylene) glycol monoalkyl ether, and the blocking agent may each be used alone or in combination of two or more. However, when an aromatic polyisocyanate is not used as the nonaqueous unblocked polyisocyanate, the yellowing resistance of the cured coating film can be improved.
[0043] The order in which the nonaqueous unblocked polyisocyanate, the poly(oxyethylene) glycol monoalkyl ether, and the blocking agent are reacted is not particularly limited. For example, the nonaqueous unblocked polyisocyanate may be reacted with the poly(oxyethylene) glycol monoalkyl ether to obtain an isocyanate-terminated precursor, and then the obtained isocyanate-terminated precursor may be reacted with the blocking agent.
[0044] The reaction between the nonaqueous unblocked polyisocyanate and the poly(oxyethylene) glycol monoalkyl ether may be carried out, for example, in the presence of a solvent. Examples of the solvent that can be used include aromatic solvents such as toluene and xylene; ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ester solvents such as ethyl acetate and butyl acetate; and glycol ether solvents such as ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and diethylene glycol diethyl ether. The reaction temperature may be, for example, 20 to 200°C. The reaction time may be, for example, 1 to 10 hours. The amounts of the polyisocyanate and poly(oxyethylene) glycol monoalkyl ether used may be adjusted so that the content of alkoxypolyethylene oxide groups falls within the above range. While the reaction proceeds without a catalyst, the reaction can also be accelerated by using a known urethane reaction catalyst.
[0045] The reaction between the isocyanate-terminated precursor and the blocking agent can be carried out under reaction conditions for a typical blocking reaction. The reaction between the isocyanate-terminated precursor and the blocking agent can be carried out at room temperature or with heating. Regardless of whether heating is performed or not, the temperature of the reaction solution can be, for example, 20 to 200°C.
[0046] The method for producing the blocked polyisocyanate (A) is not limited to the above. For example, when a nonaqueous unblocked polyisocyanate, a poly(oxyethylene) glycol monoalkyl ether, and a blocking agent are reacted and the resulting reaction product has free isocyanate groups, the blocked polyisocyanate (A) can also be obtained by reacting the free isocyanate groups of the reaction product with a modifying agent such as an active hydrogen group-containing compound.
[0047] Alternatively, an unblocked polyisocyanate having an alkoxypolyethylene oxide group may be used in place of the nonaqueous unblocked polyisocyanate. In this case, the blocked polyisocyanate (A) can be obtained by reacting the unblocked polyisocyanate having an alkoxypolyethylene oxide group with a blocking agent.
[0048] Alternatively, the blocked polyisocyanate (A) can be obtained by using a blocked polyisocyanate having no alkoxypolyethylene oxide groups (non-aqueous blocked polyisocyanate) instead of the non-aqueous unblocked polyisocyanate. For example, the blocked polyisocyanate (A) can be obtained by reacting a blocked polyisocyanate having no alkoxypolyethylene oxide groups with the poly(oxyethylene) glycol monoalkyl ether.
[0049] The blocked polyisocyanate (A) may be used alone or in combination of two or more types. For example, two or more types of blocked polyisocyanates (A) derived from different types of non-aqueous unblocked polyisocyanates may be used in combination.
[0050] The content of the block polyisocyanate (A) may be 40% by mass or more, 60% by mass or more, or 80% by mass or more, based on the total solid content of the block polyisocyanate composition, from the viewpoint of easily obtaining an aqueous coating composition having excellent low-temperature curing properties. The content of the block polyisocyanate (A) may be less than 100% by mass, or 95% by mass or less, or 90% by mass or less, based on the total solid content of the block polyisocyanate composition, from the viewpoint of improving the storage stability of the coating. From these viewpoints, the content of the block polyisocyanate (A) may be, for example, 40% by mass or more and less than 100% by mass, based on the total solid content of the block polyisocyanate composition. Note that, when the block polyisocyanate composition contains a solvent, the total solid content of the block polyisocyanate composition refers to the amount obtained by subtracting the amount of the solvent from the total amount of the block polyisocyanate composition. When the block polyisocyanate composition does not contain a solvent, the total solid content of the block polyisocyanate composition refers to the total amount of the block polyisocyanate composition.
[0051] (Blocking Agent Dissociation Catalyst) The blocking agent dissociation catalyst contains a quaternary ammonium salt. As the quaternary ammonium salt, any quaternary ammonium salt known as a blocking agent dissociation catalyst can be used without particular limitation. In particular, when a quaternary ammonium salt containing a cationic group represented by the following formula (1) is used, an aqueous coating composition with excellent low-temperature curing properties is likely to be obtained.
[0052] In formula (1), R 1 represents an alkyl group having 1 to 16 carbon atoms or an aryl group having 6 to 16 carbon atoms, which may have a hydroxy group, an amino group, or an alkoxy group as a substituent, and R 2 ~R 4 are each independently an alkyl group having 1 to 8 carbon atoms.
[0053] R 1 The number of carbon atoms in the alkyl group represented by R may be 1 to 10, or may be 6 to 8. 1 Specific examples of the alkyl group represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, a 2-ethylhexyl group, a 2-propylheptyl group, a nonyl group, a decyl group, an isodecyl group, a dodecyl group, and a hexadecyl group. These groups may be substituted with one or more hydroxy groups, one or more amino groups, or one or more alkoxy groups. The number of carbon atoms in the alkoxy group may be, for example, 1 to 8, 1 to 6, 1 to 4, or 1 to 2. Examples of the alkoxy group include a methoxy group, an ethoxy group, a butoxy group, a propyloxy group, a pentyloxy group, and a hexyloxy group.
[0054] R 1 Examples of the aryl group represented by the formula (I) include a phenyl group, a naphthyl group, an anthryl group, a tolyl group, a xylyl group, a cumenyl group, a vinylphenyl group, a biphenylyl group, and a phenanthryl group.
[0055] R 1From the viewpoint of easily obtaining an aqueous coating composition with excellent low-temperature curing properties, R may be an alkyl group having 1 to 16 carbon atoms which may have a hydroxy group, an amino group or an alkoxy group as a substituent, or may be an alkyl group or a hydroxyalkyl group which has no substituent. 1 When R is a hydroxyalkyl group having no substituent, an aqueous coating composition having even better low-temperature curing properties is more likely to be obtained, 1 When R is an alkyl group having no substituent, it is easy to obtain an aqueous coating composition having particularly excellent low-temperature curing properties. The number of carbon atoms in the alkyl group having no substituent may be 1 to 10, or may be 6 to 8. In particular, when the alkyl group has 8 carbon atoms, the low-temperature curing properties of the aqueous coating composition tend to be further improved, and 1 When is an n-octyl group, the low-temperature curing properties of the aqueous coating composition tend to be further improved.
[0056] R 2 ~R 4 The number of carbon atoms in the alkyl group represented by R may be 1 to 4, or may be 1 to 2. 2 ~R 4 Specific examples of the alkyl group represented by R include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, and a 2-ethylhexyl group. 2 ~R 4 may all be methyl groups.
[0057] From the viewpoint of facilitating the production of an aqueous coating composition with even more excellent low-temperature curing properties, the quaternary ammonium salt may have a structure represented by the following formula (2) or (3). In particular, when the quaternary ammonium salt has a structure represented by the following formula (2), an aqueous coating composition with particularly excellent low-temperature curing properties is more likely to be produced.
[0058]
[0059]
[0060] The anion group of the quaternary ammonium salt may be, for example, an organic acid group or an inorganic acid group. Examples of the organic acid group include a fatty acid group and a monoalkyl carbonate group. Examples of the inorganic acid group include a halogen group (e.g., a fluoro group, a chloro group, a bromo group, etc.), a hydroxyl group, a bicarbonate group, and a carbonate group.
[0061] The number of carbon atoms in the fatty acid group (aliphatic monocarboxylic acid group) may be, for example, 1 to 12, 1 to 7, or 1 to 3. Specific examples of the fatty acid group include a formic acid group, an acetic acid group, octylic acid, lauric acid, cyclohexanecarboxylic acid, and pivalic acid.
[0062] The number of carbon atoms in the alkyl group in the monoalkyl carbonate group may be, for example, 1 to 8, 1 to 4, or 1 to 2. Specific examples of the monoalkyl carbonate group include a methyl carbonate group, an ethyl carbonate group, a propyl carbonate group, and a butyl carbonate group.
[0063] The anionic group of the quaternary ammonium salt may be a fatty acid group having 1 to 12 carbon atoms, a monoalkyl carbonate group having an alkyl group having 1 to 8 carbon atoms, or a hydroxyl group, from the viewpoint of easily obtaining an aqueous coating composition having even better low-temperature curing properties. The anionic group of the quaternary ammonium salt may be a fatty acid group having 1 to 7 carbon atoms, or a monoalkyl carbonate group having an alkyl group having 1 to 4 carbon atoms, from the viewpoint of easily obtaining an aqueous coating composition having even better low-temperature curing properties. In particular, when the anionic group of the quaternary ammonium salt is a monoalkyl carbonate group having an alkyl group having 1 to 2 carbon atoms, an aqueous coating composition having particularly excellent low-temperature curing properties is more likely to be obtained.
[0064] From the above viewpoint, the quaternary ammonium salt may be composed of a combination of a cationic group represented by any one of the above formulas (1) to (3) and a fatty acid group having 1 to 12 carbon atoms, a monoalkyl carbonate group having an alkyl group having 1 to 8 carbon atoms, or a hydroxyl group.
[0065] Specific examples of quaternary ammonium salts include trimethyl n-octylammonium hydrogen carbonate, trimethyl n-octylammonium methyl carbonate, trimethyl n-octylammonium carbonate, tetramethylammonium acetate, hexadecyltrimethylammonium hydroxide, trimethyl(2-hydroxypropyl)ammonium 2-ethylhexanoate, tetramethylammonium hydrogen carbonate, tetraethylammonium hydrogen carbonate, tetra n-propylammonium hydrogen carbonate, tetra n-butylammonium hydrogen carbonate, triethylmonomethylammonium hydrogen carbonate, tri n-propylmonomethylammonium hydrogen carbonate, tri n-butylmonomethylammonium hydrogen carbonate, tri n-butylmonoethylammonium hydrogen carbonate, tetramethylammonium monomethyl carbonate, tetraethylammonium monoethyl carbonate, tetra n-butylammonium monobutyl carbonate, triethylmonomethylammonium monomethyl carbonate, tri n-propylmonomethylammonium monomethyl carbonate, tri n-butylmonomethylammonium monomethyl carbonate, tri n-butylmonoethylammonium monoethyl carbonate, tetramethylammonium carbonate, and tetra n-butylammonium carbonate. The quaternary ammonium salts may be used singly or in combination of two or more.
[0066] The blocked polyisocyanate composition may contain a blocking agent dissociation catalyst other than a quaternary ammonium salt. The proportion of the quaternary ammonium salt in the total blocking agent dissociation catalyst in the blocked polyisocyanate composition may be 0.0001 to 100 mass%, 0.001 to 100 mass%, or 0.01 to 100 mass%.
[0067] From the viewpoint of improving low-temperature curing properties, the content of the blocking agent dissociating catalyst may be 0.0001 parts by mass or more, 0.001 parts by mass or more, 0.01 parts by mass or more, 0.1 parts by mass or more, 1 part by mass or more, 5 parts by mass or more, or 10 parts by mass or more, relative to 100 parts by mass of the blocked polyisocyanate (A). From the viewpoint of improving the storage stability of the coating material, the content of the blocking agent dissociating catalyst may be 40 parts by mass or less, 30 parts by mass or less, or 20 parts by mass or less, relative to 100 parts by mass of the blocked polyisocyanate (A). From these viewpoints, the content of the blocking agent dissociating catalyst may be, for example, 0.0001 to 40 parts by mass, relative to 100 parts by mass of the blocked polyisocyanate (A).
[0068] (Other Components) The blocked polyisocyanate composition may contain a solvent. The solvent may be a hydrophilic solvent. Examples of the solvent include water, ethylene glycol, propylene glycol, 1,4-butanediol, methyl ethyl ketone, acetone, ethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol dimethyl ether, N-methylpyrrolidone, ethylene glycol monoethyl ether acetate, and diethylene glycol diethyl ether. These solvents may be used alone or in combination of two or more.
[0069] The content of the solvent may be 0 to 90% by mass, 5 to 80% by mass, or 10 to 70% by mass, based on the total mass of the blocked polyisocyanate composition.
[0070] The blocked polyisocyanate composition may contain unblocked polyisocyanate (e.g., polyisocyanate remaining as an unreacted product) and may contain unreacted blocking agent. The content of unblocked polyisocyanate contained in the blocked polyisocyanate composition may be 5% by mass or less, or even 0% by mass, based on the total solid content of the blocked polyisocyanate composition. The content of unreacted blocking agent contained in the blocked polyisocyanate composition may be 5% by mass or less, or even 0% by mass, based on the total solid content of the blocked polyisocyanate composition.
[0071] The blocked polyisocyanate composition may further contain additives such as pigments, dispersion stabilizers, viscosity modifiers, leveling agents, antigelling agents, light stabilizers, antioxidants, ultraviolet absorbers, heat resistance improvers, inorganic and organic fillers, plasticizers, lubricants, antistatic agents, reinforcing materials, and catalysts.
[0072] The effective isocyanate group content (hereinafter referred to as "effective NCO content") of the blocked polyisocyanate composition may be 4 to 28% by mass, 5 to 22% by mass, or 6 to 16% by mass, from the viewpoint of further enhancing the curability of the coating material. Here, the effective NCO content refers to the isocyanate groups present in the blocked polyisocyanate composition that can participate in a crosslinking reaction, expressed in mass %. The effective NCO content can also be expressed as the content (free NCO content) of free isocyanate groups in a polyisocyanate composition obtained by dissociating a blocking agent from a blocked isocyanate, relative to the total mass of the blocked polyisocyanate composition. The free NCO content can be determined by reacting the isocyanate groups in a measurement sample (a polyisocyanate composition obtained by dissociating a blocking agent from a blocked isocyanate) with an excess of a secondary amine, followed by back titration of the unreacted secondary amine with hydrochloric acid.
[0073] The blocked polyisocyanate composition described above can be obtained by mixing the blocked polyisocyanate (A), the blocking agent dissociation catalyst, and the other components that may be included. The blocked polyisocyanate composition may be used as a curing agent component of an aqueous coating composition. That is, another embodiment of the present disclosure is a curing agent for aqueous coatings, comprising the blocked polyisocyanate composition.
[0074] (Aqueous Coating Composition) Another embodiment of the present disclosure is an aqueous coating composition comprising a compound having two or more isocyanate-reactive groups (hereinafter referred to as an "isocyanate-reactive compound"), the above-mentioned blocked polyisocyanate (A), a quaternary ammonium salt serving as a blocking agent dissociation catalyst, and water. Details of the blocked polyisocyanate (A) and the quaternary ammonium salt are the same as those of the blocked polyisocyanate (A) and the quaternary ammonium salt contained in the blocked polyisocyanate composition of the above-mentioned embodiment.
[0075] The aqueous coating composition contains the blocked polyisocyanate (A) and a quaternary ammonium salt, and therefore has excellent low-temperature curing properties.
[0076] The isocyanate-reactive compound has two or more isocyanate-reactive groups (e.g., active hydrogen groups). Examples of the isocyanate-reactive group include a hydroxy group and an amino group. From the viewpoint of further improving low-temperature curing properties, the isocyanate-reactive compound may have 4 to 70 isocyanate-reactive groups (e.g., active hydrogen groups).
[0077] Examples of isocyanate-reactive compounds include polyols, polyamines, and amino alcohols. Among these, the effects of the present disclosure are more easily achieved when polyols are used. Examples of polyols include acrylic polyols, polyester polyols, polyether polyols, epoxy polyols, polycarbonate polyols, and polylactone polyols. The hydroxyl value of the polyol may be, for example, 10 to 300 mg KOH / g per solid content.
[0078] The number average molecular weight of the isocyanate-reactive compound is, for example, 1,000 to 100,000, and from the viewpoint of further improving low-temperature curing properties, it may be 5,000 to 50,000. The number average molecular weight is measured using gel permeation chromatography (GPC) and means a value determined using polystyrene as a standard substance.
[0079] The isocyanate-reactive compound may be used in a state of being emulsified, dispersed, or dissolved in water. In other words, the aqueous coating composition may contain an isocyanate-reactive compound-containing liquid (solution, dispersion, emulsion, or suspension) obtained by emulsifying, dispersing, or dissolving the isocyanate-reactive compound in water. The isocyanate-reactive compound-containing liquid may contain a neutralizing agent. Examples of the neutralizing agent include ammonia and water-soluble amino compounds (tertiary amines such as triethylamine and 2-(dimethylamino)ethanol).
[0080] The equivalent ratio of the isocyanate-reactive groups to the available isocyanate groups contained in the aqueous coating composition ([isocyanate-reactive groups] / [available isocyanate groups]) is determined based on the required physical properties of the coating film. The equivalent ratio is not particularly limited, but is usually in the range of 0.2 to 2.
[0081] The aqueous coating composition may contain other components that can be contained in the above-mentioned blocked polyisocyanate composition.
[0082] The aqueous coating composition may be a one-component composition in which all of the constituent components are contained in one component, or a multi-component composition in which the constituent components are present in multiple components. The multi-component aqueous coating composition may comprise a first component (main component) containing an isocyanate-reactive compound and a second component (curing agent) containing a blocked polyisocyanate. In this case, the other constituent components (blocking agent dissociation catalyst and other components) may be contained in the first component, the second component, or a component different from the first and second components.
[0083] The aqueous coating composition can be used as an automotive topcoat paint, a chipping-resistant paint, an electrodeposition paint, a paint for automotive parts, a paint for automotive repair, pre-coated metals and rust-proof steel sheets for metal products such as home appliances and office equipment, a paint for building materials, a paint for plastics, an adhesive, an adhesion promoter, a sealant, etc.
[0084] <Coating Film> Another embodiment of the present disclosure is a coating film formed from the aqueous coating composition of the above embodiment.
[0085] The coating film includes a cured product of the aqueous coating composition of the above embodiment. The coating film can be formed by applying the aqueous coating composition to a substrate using a known method and curing the coating film (uncured coating film) made of the aqueous coating composition. Known methods include, for example, roll coating, curtain flow coating, spray coating, electrostatic coating, bell coating, and electrodeposition coating. The amount of the aqueous coating composition applied, the thickness of the coating film, etc. may be determined appropriately depending on the material of the surface to be coated, etc.
[0086] Curing of a coating film made from the aqueous coating composition may be carried out by heating the coating film. The heating temperature (baking temperature) may be, for example, 200°C or lower. The heating time (baking time) may be, for example, 10 to 180 minutes. With the aqueous coating composition of this embodiment, a good cured coating film can be obtained even when baking is carried out at a low temperature of 100°C or lower.
[0087] The present disclosure will be described in more detail below using examples and comparative examples, but the present disclosure is not limited to the following examples.
[0088] <Production Example 1> (Preparation of Polyisocyanate A-1) 995 g of HDI, 5.0 g of 1,3-butanediol (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.3 g of phenol (manufactured by Tokyo Chemical Industry Co., Ltd.) were charged into a four-necked flask equipped with a stirrer, thermometer, heating device, nitrogen seal tube, and condenser, and a urethane-forming reaction was carried out at 80°C for 2 hours under a nitrogen stream. Thereafter, 0.04 g of potassium 2-ethylhexanoate (manufactured by Tokyo Chemical Industry Co., Ltd.), an isocyanuration catalyst, was added, and the isocyanuration reaction was carried out at 70°C for 2 hours. After the NCO content reached 40.0% by mass, 0.15 g of JP-508 (manufactured by Johoku Chemical Industry Co., Ltd.) was added to carry out a termination reaction, and the reaction solution was cooled to room temperature. This reaction solution was subjected to thin-film distillation at a temperature of 130°C and a pressure of 0.04 kPa to remove unreacted HDI, thereby obtaining purified polyisocyanate A-1. The NCO content of Polyisocyanate A-1 was 21.8% by mass, and the viscosity at 25°C was about 2,500 mPa·s.
[0089] ( 1 H-NMR: Measurement of isocyanurate group content) Polyisocyanate A-1 1 H-NMR measurement was carried out to determine the isocyanurate group content (the content of isocyanurate groups relative to the total (100 mol%) of isocyanurate groups and allophanate groups). Specifically, the isocyanurate group content was calculated from the area of the signal of the hydrogen atom of the methylene group adjacent to the nitrogen atom of the isocyanurate group at around 3.7 ppm and the signal of the hydrogen atom bonded to the nitrogen atom of the allophanate group at around 8.5 ppm. The isocyanurate group content was 89 mol%. 1 H-NMR measurement was carried out under the following measurement conditions: [Measurement conditions] (1) Measurement equipment: ECX400M (manufactured by JEOL Ltd.) 1 H-NMR) (2) Measurement temperature: 23°C (3) Sample concentration: 0.1 g / 1 ml (4) Number of accumulations: 16 (5) Relaxation time: 5 seconds (6) Solvent: deuterium dimethyl sulfoxide (7) Chemical shift reference: hydrogen atom signal of methyl group in deuterium dimethyl sulfoxide (2.5 ppm)
[0090] (GPC: Measurement of Isocyanurate Trimer Content) Polyisocyanate A-1 was analyzed by GPC (gel permeation chromatography) to determine the isocyanurate trimer content. In GPC, the isocyanurate trimer peak was detected as a single peak with a peak start time of 20.5 minutes, a peak end time of 23.0 minutes, and a peak top time of 21.2 minutes. The isocyanurate trimer content determined from the peak area of the isocyanurate trimer was 52% by mass. The GPC measurement was performed under the following measurement conditions. [Measurement conditions] (1) Measuring instrument: HLC-8220 (manufactured by Tosoh Corporation) (2) Column: TSKgel (manufactured by Tosoh Corporation) ・G3000H-XL ・G2500H-XL ・G2000H-XL ・G1000H-XL One of each of the above connected in series (3) Carrier: THF (tetrahydrofuran) (4) Detector: RI (refractive index) detector (5) Temperature: 40°C (6) Flow rate: 1.000 ml / min (7) Calibration curve: Standard polystyrene (manufactured by Tosoh Corporation) ・F-80 (molecular weight: 7.06 × 105, molecular weight distribution: 1.05) ・F-20 (molecular weight: 1.90 × 105, molecular weight distribution: 1.05) ・F-10 (molecular weight: 9.64 × 104, molecular weight distribution: 1.01) ・F-2 (molecular weight: 1.81×104, molecular weight distribution: 1.01) ・F-1 (molecular weight: 1.02×104, molecular weight distribution: 1.02) ・A-5000 (molecular weight: 5.97×103, molecular weight distribution: 1.02) ・A-2500 (molecular weight: 2.63×103, molecular weight distribution: 1.05) - A-500 (molecular weight: 5.0 x 102, molecular weight distribution: 1.14) (8) Sample solution concentration: 0.5% THF solution.
[0091] Example 1 Preparation of Blocked Polyisocyanate Composition 312 g of Polyisocyanate A-1, 78 g of MPG-081 (trade name, manufactured by Nippon Nyukazai Co., Ltd., polyethylene glycol monomethyl ether, average number of EO units=15, number average molecular weight=690), and 336 g of diethyldiglycol (trade name, manufactured by Nippon Nyukazai Co., Ltd., diethylene glycol diethyl ether, trade name, "DEDG" in Table 1) were placed in a four-neck flask equipped with a stirrer, a thermometer, a heating device, a nitrogen seal tube, and a cooling tube. The atmosphere in the flask was replaced with nitrogen, and the mixture was heated to 80°C with stirring and reacted at the same temperature for 4 hours to obtain an isocyanate-terminated precursor having alkoxypolyethylene oxide groups (average number of EO units=15) as hydrophilic groups. Subsequently, 131 g of methyl ethyl ketoxime (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., "MEKO" in Table 1) was charged so that the temperature did not exceed 80°C, and the mixture was reacted at 70°C for 2 hours. When the peak of the NCO group (near 2270 cm-1) disappeared in the infrared absorption spectrum (IR measurement), the mixture was cooled to room temperature, and 142 g of trimethylmono-n-octylammonium monomethyl carbonate solution (manufactured by Tosoh Corporation, solids concentration 55% by mass, "TMOA-MC" in Table 1) was added and stirred for 30 minutes to obtain a composition containing a blocked polyisocyanate (blocked polyisocyanate composition (BI-1)).
[0092] Examples 2 and 3 Blocked polyisocyanate compositions BI-2 to BI-3 were obtained in the same manner as in Example 1, except that MPEG-1000 (manufactured by Tokyo Chemical Industry Co., Ltd., polyethylene glycol monomethyl ether, average number of EO units=22, number average molecular weight=1000) was used instead of MPG-081 and the blending amounts of the materials were changed to the amounts shown in Table 1.
[0093] Example 4 A blocked polyisocyanate composition BI-4 was obtained in the same manner as in Example 1, except that MPEG-2000 (manufactured by Tokyo Chemical Industry Co., Ltd., polyethylene glycol monomethyl ether, average number of EO units=45, number average molecular weight=2000) was used instead of MPG-081 and the blending amounts of the materials were changed to those shown in Table 1.
[0094] Example 5 A blocked polyisocyanate composition BI-5 was obtained in the same manner as in Example 1, except that 3,5-dimethylpyrazole (manufactured by Tokyo Chemical Industry Co., Ltd., “3,5-DMP” in Table 1) was used instead of methyl ethyl ketoxime and the blending amounts of the materials were changed to those shown in Table 1.
[0095] Example 6 A blocked polyisocyanate composition BI-6 was obtained in the same manner as in Example 1, except that a tetramethylammonium acetate solution (manufactured by Tokyo Chemical Industry Co., Ltd., solids concentration 25 mass%, “TMA-Ac” in Table 1) was used instead of the trimethylmono-n-octylammonium monomethyl carbonate solution, and the blending amounts of the materials were changed to the amounts shown in Table 1.
[0096] Example 7 A blocked polyisocyanate composition BI-7 was obtained in the same manner as in Example 1, except that a hexadecyltrimethylammonium hydroxide solution (manufactured by Tokyo Chemical Industry Co., Ltd., solids concentration 25 mass%, “HDTMA-H” in Table 1) was used instead of the trimethylmono-n-octylammonium monomethyl carbonate solution, and the blending amounts of the materials were changed to the amounts shown in Table 1.
[0097] Example 8 A blocked polyisocyanate composition BI-8 was obtained in the same manner as in Example 2, except that DABCOTMR (trade name, manufactured by Sankyo Air Products Co., Ltd., solids concentration 75 mass %) was used instead of the trimethylmono-n-octylammonium monomethyl carbonate solution and the blending amounts of the materials were changed to those shown in Table 1.
[0098] Example 9 A blocked polyisocyanate composition BI-9 was obtained in the same manner as in Example 1, except that the blending amounts of the materials were changed to those shown in Table 1.
[0099] Comparative Example 1 A blocked polyisocyanate composition BI-10 was obtained in the same manner as in Example 1, except that the addition of the trimethylmono-n-octylammonium monomethyl carbonate solution and the subsequent stirring were not performed, and the blending amounts of the materials were changed to the amounts shown in Table 2.
[0100] Comparative Example 2 A blocked polyisocyanate composition BI-11 was obtained in the same manner as in Example 1, except that dioctyltin dilaurate (manufactured by Kishida Chemical Co., Ltd., "DOTDL" in Table 2) was used instead of the trimethylmono-n-octylammonium monomethyl carbonate solution and the blending amounts of the materials were changed to those shown in Table 2.
[0101] Comparative Example 3 A blocked polyisocyanate composition BI-12 was obtained in the same manner as in Example 1, except that MPEG-550 (manufactured by Tokyo Chemical Industry Co., Ltd., polyethylene glycol monomethyl ether, average number of EO units=12, number average molecular weight=550) was used instead of MPG-081 and the blending amounts of the materials were changed to the amounts shown in Table 2.
[0102] Comparative Example 4 A blocked polyisocyanate composition BI-13 was obtained in the same manner as in Comparative Example 3, except that the blending amounts of the materials were changed to the amounts shown in Table 2.
[0103] Comparative Example 5 A blocked polyisocyanate composition BI-14 was obtained in the same manner as in Example 1, except that MPEG-4000 (manufactured by Tokyo Chemical Industry Co., Ltd., polyethylene glycol monomethyl ether, average number of EO units=90, number average molecular weight=4000) was used instead of MPG-081 and the blending amounts of the materials were changed to the amounts shown in Table 2.
[0104] Comparative Example 6 A blocked polyisocyanate composition BI-15 was obtained in the same manner as in Example 1, except that PEG-1000 (manufactured by Tokyo Chemical Industry Co., Ltd., polyethylene glycol, average number of EO units=22, number average molecular weight=1000) was used instead of MPG-081 and the blending amounts of the materials were changed to the amounts shown in Table 2.
[0105] Comparative Example 7 A blocked polyisocyanate composition BI-16 was obtained in the same manner as in Comparative Example 6, except that the blending amounts of the materials were changed to the amounts shown in Table 2.
[0106] Comparative Example 8: A four-neck flask equipped with a stirrer, thermometer, heating device, nitrogen seal tube, and condenser was charged with 379 g of polyisocyanate A-1, 20 g of 12-hydroxystearic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 377 g of diethyl diglycol. The atmosphere in the flask was replaced with nitrogen, and the mixture was heated to 80°C with stirring and reacted at the same temperature for 4 hours to obtain an isocyanate group-terminated precursor. Subsequently, 160 g of methyl ethyl ketoxime was charged so that the temperature did not exceed 80°C, and the mixture was reacted at 70°C for 2 hours. When the NCO group peak (near 2270 cm-1) disappeared in the infrared absorption spectrum (IR measurement), the mixture was cooled to room temperature, and 13 g of 2-(dimethylamino)ethanol (manufactured by Tokyo Chemical Industry Co., Ltd.) was charged and stirred for 30 minutes. 51 g of trimethyl mono-n-octylammonium monomethyl carbonate solution was added and stirred for 30 minutes to obtain blocked polyisocyanate BI-17.
[0107] Comparative Example 9 A blocked polyisocyanate composition BI-18 was obtained in the same manner as in Comparative Example 8, except that the blending amounts of the materials were changed to the amounts shown in Table 2.
[0108]
[0109]
[0110] The hydrophilic group introduction rate in Tables 1 and 2 is the introduction rate of the hydrophilic group (alkoxypolyethylene oxide group) in the isocyanate group-terminated precursor, and is equal to the content of the alkoxypolyethylene oxide group, based on the total amount of isocyanate compounds, in the isocyanate composition obtained by dissociating the blocking agent from the blocked polyisocyanate in the blocked polyisocyanate composition.
[0111] The effective NCO content in Tables 1 and 2 is the content of effective isocyanate groups in the blocked polyisocyanate composition, and was determined by adding an excess amount of secondary amine relative to the isocyanate groups to the blocked polyisocyanate composition, heating the composition at a temperature equal to or higher than the dissociation temperature of the oxime-based blocking agent (e.g., 160°C) for a period of time sufficient for the blocking agent to dissociate (e.g., 1 hour), and allowing the free isocyanate groups to react with the secondary amine, followed by back-titrating the unreacted secondary amine with hydrochloric acid.
[0112] The catalyst amount in Tables 1 and 2 is the amount (unit: parts by mass) of the blocking agent dissociation catalyst contained in the composition when the amount of the blocked polyisocyanate contained in the composition is taken as 100 parts by mass.
[0113] <Evaluation> (Preparation of Aqueous Coating Compositions) The blocked polyisocyanate compositions of Examples 1 to 9 and Comparative Examples 1 to 9 were used to prepare aqueous coating compositions of Examples 1 to 9 and Comparative Examples 1 to 9, respectively. Specifically, the main agent, Burnock WE-301 (trade name, manufactured by DIC Corporation, acrylic emulsion, solids concentration 45% by mass, hydroxyl value 36 mg KOH / g, number average molecular weight: 30,000), the curing agent, the blocked polyisocyanate composition, and water were mixed, and the mixture was stirred at high speed at 2,000 rpm for 2 minutes using a homomixer to prepare the aqueous coating compositions. The amounts (units: g) of the main agent (Burnoc WE-301), curing agent (blocked polyisocyanate composition), and water used were as shown in Tables 3 and 4. The amount of the main agent shown in the tables is the total mass including the solvent.
[0114] (Evaluation of low-temperature curing properties) [Gel fraction measurement] The aqueous coating composition prepared above was applied to release paper so that the thickness before drying was 200 μm. The resulting coating film was left to stand at room temperature for 60 minutes, and then baked by heating in a thermostatic chamber at 100°C for 20 minutes. The baked coating film (cured coating film) was immersed in methyl ethyl ketone at room temperature for 24 hours, and the gel fraction was determined. The gel fraction was calculated using the following formula. The results are shown in Tables 3 and 4. Gel fraction (unit: mass %) = mass of coating film after immersion (mass of undissolved portion) / mass of coating film before immersion × 100
[0115] [Martens Hardness Measurement] The aqueous coating composition prepared above was applied to a color steel plate (white) so that the thickness before drying was 100 μm (wet). The resulting coating film was left to stand at room temperature for 60 minutes, and then baked by heating in a thermostatic chamber at 100°C for 20 minutes. The indentation strength of the baked coating film (cured coating film) was measured in accordance with ISO 14577 under the following conditions. The results are shown in Tables 3 and 4. [Conditions] Testing equipment: Fischerscope HM2000 (manufactured by Fischer Instruments) Indenter: Vickers diamond Test load: 5 mN Test temperature: 25°C
[0116] The gel fraction measured above is 70% by mass or more, and the Martens hardness is 60 N / mm 2 When the value was equal to or greater than this, the composition was evaluated as having excellent low-temperature curing properties.
[0117] (Storage Stability Evaluation) The aqueous coating composition was allowed to stand at 25°C for 6 hours, and the dispersion state before and after standing was visually observed to evaluate storage stability. If the aqueous coating composition was liquid and no precipitation occurred after standing, it was evaluated as having sufficient storage stability (A). If the aqueous coating composition solidified or precipitation occurred after standing, it was evaluated as having poor storage stability (B). In addition, if the aqueous coating composition solidified or precipitation occurred in the initial state before standing, it was also evaluated as having poor storage stability. The evaluation results are shown in Tables 3 and 4.
[0118]
[0119]
Claims
1. A blocked polyisocyanate composition comprising a blocked polyisocyanate and a blocking agent dissociation catalyst, wherein the blocked polyisocyanate has an alkoxypolyethylene oxide group containing an average of 14 to 50 ethylene oxide units, and the blocking agent dissociation catalyst contains a quaternary ammonium salt.
2. The blocked polyisocyanate composition according to claim 1, wherein the number of ethylene oxide units contained in the alkoxypolyethylene oxide group is 15 to 25 on average.
3. The blocked polyisocyanate composition according to claim 1, wherein the content of the alkoxy polyethylene oxide group is 5 to 30 mass % based on the total amount of isocyanate compounds in the isocyanate composition obtained by dissociating the blocking agent from the blocked polyisocyanate.
4. The blocked polyisocyanate composition according to claim 1, wherein the content of the alkoxy polyethylene oxide group is 5 to 25 mass% based on the total amount of isocyanate compounds in the isocyanate composition obtained by dissociating the blocking agent from the blocked polyisocyanate.
5. The blocked polyisocyanate composition according to claim 1, wherein the blocked polyisocyanate contains a structure derived from an aliphatic polyisocyanate having 4 to 6 carbon atoms or a derivative thereof.
6. The blocked polyisocyanate composition according to claim 1, wherein the quaternary ammonium salt contains a cationic group represented by the following formula (1): [In formula (1), R 1 represents an alkyl group having 1 to 16 carbon atoms which may have a hydroxy group, an amino group or an alkoxy group as a substituent; R 2 ~R 4 each independently represents an alkyl group having 1 to 8 carbon atoms.
7. The blocked polyisocyanate composition according to claim 1, wherein the blocked polyisocyanate has an isocyanate group blocked with an oxime-based blocking agent.
8. A curing agent for water-based paints, comprising the blocked polyisocyanate composition according to any one of claims 1 to 7.
9. An aqueous coating composition comprising a compound having two or more isocyanate-reactive groups, a blocked polyisocyanate, a blocking agent dissociation catalyst, and water, wherein the blocked polyisocyanate has alkoxypolyethylene oxide groups containing an average of 14 to 50 ethylene oxide units, and the blocking agent dissociation catalyst contains a quaternary ammonium salt.
10. A coating film formed from the aqueous coating composition according to claim 9.
Citation Information
Patent Citations
One-component container sealing material and container sealing component using the same
JP5073978B2
Blocking agent dissociation catalyst containing quaternary ammonium salt and usage of the same
JP2013091767A
Block polyisocyanate composition, hydrophilic polyisocyanate composition, resin composition, resin film and laminate
JP2021101007A
Block polyisocyanate composition, one-component coating composition, coating film, and coated article
WO2021020534A1
Cited By
Blocked-polyisocyanate composition, coating composition, curing agent for aqueous coating material, aqueous coating composition, and coating film
WO2025204707A1