Paving material composition and structure
The composition of epoxy resin, polyamine compound, and aggregate in the paving material addresses the challenges of water permeability, weather resistance, and strength retention in humid environments, achieving superior performance in landscape paving applications.
Patent Information
- Application Number
- PCT/JP2024/004213
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-02-07
- Publication Date
- 2024-10-03
AI Technical Summary
Existing landscape paving materials lack high water permeability, weather resistance, and strength retention in humid environments, with complex processes and reduced strength when exposed to rain or moisture.
A paving material composition comprising an epoxy resin, a polyamine compound represented by a specific general formula as an epoxy resin curing agent, and aggregate, with a mass ratio of epoxy resin to aggregate between 0.005 and 0.5, and a particle size of aggregate between 0.002 and 50 mm, which forms a structure with high water permeability, weather resistance, and strength retention.
The composition achieves high water permeability, weather resistance, and strength retention, with excellent strength retention even in humid environments, as demonstrated by increased maximum bending stress and retention rate after water immersion.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Paving composition and structure
[0001] The present invention relates to paving compositions and structures.
[0002] Natural stone is used as aggregate in landscape paving materials. By using natural stone, it is possible to obtain paving materials that blend more closely with the landscape of parks, tourist spots, etc. than asphalt and concrete. In addition to the strength of the resulting structure, landscape paving materials are generally desired to have high water permeability. Furthermore, high weather resistance is particularly desirable for landscape paving materials.
[0003] A paving material composition with excellent weather resistance that uses an epoxy resin as a binder resin is known. For example, Patent Document 1 discloses that a paving material kneaded with a weather-resistant epoxy fiberized resin as a binder for aggregate, the weather-resistant epoxy fiberized resin being mainly composed of a mixture of an alicyclic epoxy resin in which an aromatic benzene ring is substituted by a reduction reaction and fibers having a fiber diameter and fiber length of a predetermined value or less, is strong, permeable, and has excellent weather resistance.
[0004] Japanese Patent Application Laid-Open No. 2002-294616
[0005] However, the technology disclosed in Patent Document 1 involves kneading an epoxy resin binder resin with fibers to form fibers, which results in a complicated process for obtaining a structure. Furthermore, since landscape paving materials are typically used outdoors, it is important that they not only have high initial strength but also maintain their strength even after exposure to rain. The objective of the present invention is to provide a paving composition that can be used to obtain a structure with high water permeability, weather resistance, and strength, and excellent strength retention even in a humid environment.
[0006] The present inventors have found that the above-mentioned problems can be solved by a paving material composition containing an epoxy resin, a specific epoxy resin curing agent, and an aggregate. That is, the present invention relates to the following: [1] A paving material composition containing an epoxy resin, an epoxy resin curing agent containing 50 mass % or more of a polyamine compound represented by the following general formula (1) or a modified product thereof (A), and an aggregate. 2 N-CH 2 -X-CH 2 -NH 2(1) (In formula (1), X is a cyclohexylene group.) [2] The paving composition according to the above item [1], wherein the modified polyamine compound is at least one selected from the group consisting of the following (I) to (IV): (I) a Mannich reaction product of a polyamine compound represented by the above general formula (1), a phenol compound, and an aldehyde compound (II) a reaction product of a polyamine compound represented by the above general formula (1) with an unsaturated hydrocarbon compound (III) a reaction product of a polyamine compound represented by the above general formula (1) with an epoxy compound having at least one epoxy group (IV) a reaction product of a polyamine compound represented by the above general formula (1) with an unsaturated carboxylic acid or a derivative thereof [3] The paving composition according to the above item [1] or [2], wherein the mass ratio of the epoxy resin to the aggregate [epoxy resin / aggregate] is in the range of 0.005 to 0.5. [4] The paving material composition according to any one of [1] to [3] above, wherein the particle size of the aggregate is 0.002 to 50 mm. [5] A structure comprising a cured product of the paving material composition according to any one of [1] to [4] above.
[0007] According to the present invention, it is possible to provide a paving material composition that can provide a structure having high water permeability, weather resistance, and strength, and excellent strength retention even in a wet environment.
[0008] [Definition] In this specification, the term "paving composition" refers to a composition containing paving aggregate and used to form paving materials. The paving composition of the present invention does not include primer compositions and the like used in paving materials.
[0009] In this specification, the strength of a structure obtained by curing a paving material composition can be evaluated by the method described in the Examples, using the maximum bending stress as an index. Hereinafter, unless otherwise specified, "strength of a structure" refers to the initial strength of the structure, and a high initial strength of a structure means that the maximum bending stress value before the structure is submerged in water is high. Furthermore, the strength retention rate of a structure in a wet environment is a value obtained by the ratio of the initial maximum bending stress (before submersion) of the obtained structure to the maximum bending stress after submersion for a predetermined period of time, and can be calculated specifically by the method described in the Examples.
[0010] [Paving Material Composition] The paving material composition of the present invention (hereinafter also referred to simply as "the composition (of the present invention)") contains an epoxy resin, an epoxy resin curing agent containing 50 mass % or more of a polyamine compound represented by the following general formula (1) or a modified product thereof (A), and an aggregate. 2 N-CH 2 -X-CH 2 -NH 2 (1) (In formula (1), X is a cyclohexylene group.) By having the above-mentioned structure, the composition of the present invention can form a structure that has high water permeability, weather resistance, and strength, and that has excellent strength retention even in a humid environment.
[0011] The reasons why the composition of the present invention exhibits the above-mentioned effects are unclear, but are thought to be as follows. The polyamine compound represented by the general formula (1) is an aliphatic cyclic polyamine, which has moderate hydrophilicity but is more hydrophobic than aliphatic chain polyamines. Furthermore, when the polyamine compound represented by the general formula (1) is used as an epoxy resin curing agent, a cured product with a high glass transition temperature (Tg) is obtained. Due to these properties, it is believed that cured products of the composition of the present invention, which uses an epoxy resin curing agent containing a predetermined amount or more of this polyamine compound or its modified form, have high water permeability, high strength, and high strength retention in humid environments. Furthermore, because the polyamine compound represented by the general formula (1) does not contain an aromatic ring and has a low proportion of nitrogen atoms in the molecule, it is believed that cured products of the composition of the present invention exhibit high weather resistance. The following describes each component used in the composition of the present invention.
[0012] <Epoxy Resin> The epoxy resin is not particularly limited as long as it is a resin having two or more glycidyl groups capable of reacting with active hydrogen in an epoxy resin curing agent described below, and may be any of a saturated or unsaturated aliphatic compound, alicyclic compound, aromatic compound, and heterocyclic compound. From the viewpoint of improving the strength of the structure obtained by curing the paving material composition and the strength retention rate in a humid environment, the epoxy resin is preferably an epoxy resin containing an aromatic ring or alicyclic structure in the molecule. Specific examples of the epoxy resin include at least one resin selected from the group consisting of epoxy resins having a glycidylamino group derived from meta-xylylenediamine, epoxy resins having a glycidylamino group derived from para-xylylenediamine, epoxy resins having a glycidylamino group derived from 1,3-bis(aminomethyl)cyclohexane, epoxy resins having a glycidylamino group derived from 1,4-bis(aminomethyl)cyclohexane, epoxy resins having a glycidylamino group derived from diaminodiphenylmethane, epoxy resins having a glycidylamino group and / or a glycidyloxy group derived from para-aminophenol, epoxy resins having a glycidyloxy group derived from bisphenol A, epoxy resins having a glycidyloxy group derived from bisphenol F, epoxy resins having a glycidyloxy group derived from hydrogenated bisphenol A, epoxy resins having a glycidyloxy group derived from hydrogenated bisphenol F, epoxy resins having a glycidyloxy group derived from phenol novolac, and epoxy resins having a glycidyloxy group derived from resorcinol. The above epoxy resins may be used in combination of two or more kinds.
[0013] Among the above, from the viewpoints of improving the strength of the structure obtained by curing the paving material composition and the strength retention rate in a humid environment, the epoxy resin is preferably one whose main component is at least one selected from the group consisting of epoxy resins having a glycidylamino group derived from meta-xylylenediamine, epoxy resins having a glycidylamino group derived from para-xylylenediamine, epoxy resins having a glycidyloxy group derived from bisphenol A, epoxy resins having a glycidyloxy group derived from bisphenol F, epoxy resins having a glycidyloxy group derived from hydrogenated bisphenol A, and epoxy resins having a glycidyloxy group derived from hydrogenated bisphenol F. From the viewpoints of improving the strength of the structure obtained by curing the paving material composition, the strength retention rate in a humid environment, availability, and economy, more preferred is one whose main component is an epoxy resin having a glycidyloxy group derived from bisphenol A. The term "main component" as used herein means that other components may be contained within a range that does not deviate from the spirit of the present invention, and preferably means 50 to 100% by mass, more preferably 70 to 100% by mass, and even more preferably 90 to 100% by mass of the total.
[0014] The epoxy resin may be either a solid epoxy resin or a liquid epoxy resin, but from the viewpoint of improving the strength of the resulting structure and the strength retention rate in a humid environment, a liquid epoxy resin is more preferable. In the present invention, "solid epoxy resin" means an epoxy resin that is solid at room temperature (25°C), and "liquid epoxy resin" means an epoxy resin that is liquid at room temperature (25°C).
[0015] From the viewpoint of improving handleability, the epoxy resin may contain a reactive diluent in addition to the epoxy resin that may be contained as a main component. Examples of the reactive diluent include low-molecular-weight compounds having at least one epoxy group, such as aromatic monoglycidyl ethers such as phenyl glycidyl ether and cresyl glycidyl ether; alkyl monoglycidyl ethers such as butyl glycidyl ether, hexyl glycidyl ether, octyl glycidyl ether, decyl glycidyl ether, lauryl glycidyl ether, and tetradecyl glycidyl ether; and diglycidyl ethers of aliphatic diols such as 1,3-propanediol diglycidyl ether, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, and 1,6-hexanediol diglycidyl ether. The reactive diluents may be used alone or in combination of two or more.
[0016] The epoxy equivalent of the epoxy resin is preferably 80 g / equivalent or more, more preferably 100 g / equivalent or more, even more preferably 120 g / equivalent or more, and even more preferably 150 g / equivalent or more, from the viewpoint of improving the strength of the structure obtained by curing the paving material composition and the strength retention rate in a humid environment; and from the viewpoint of handleability, it is preferably 1,000 g / equivalent or less, more preferably 800 g / equivalent or less, even more preferably 500 g / equivalent or less, even more preferably 300 g / equivalent or less, and even more preferably 200 g / equivalent or less.
[0017] Commercially available epoxy resins may also be used. Examples of commercially available epoxy resins include "jER825", "jER827", "jER828", "jER801N", "jER801PN", "jER802", "jER811", "jER813", "jER819", "jER806", "jER806H", and "jER807" manufactured by Mitsubishi Chemical Corporation.
[0018] <Epoxy Resin Curing Agent> The epoxy resin curing agent contains 50% by mass or more of a polyamine compound represented by the following general formula (1) or a modified product thereof (A). When an epoxy resin curing agent containing 50% by mass or more of component (A) is used, a structure having high water permeability, weather resistance, and strength and excellent strength retention even in a humid environment can be formed. 2 N-CH 2 -X-CH 2 -NH 2 (1) (In formula (1), X is a cyclohexylene group.)
[0019] In the formula (1), X represents a 1,2-cyclohexylene group, a 1,3-cyclohexylene group, or a 1,4-cyclohexylene group, and is preferably a 1,3-cyclohexylene group or a 1,4-cyclohexylene group, more preferably a 1,3-cyclohexylene group, from the viewpoint of improving the water permeability, weather resistance, strength, and strength retention rate in humid environments of the structure obtained by curing the paving material composition. That is, the polyamine compound represented by the general formula (1) is one or more bis(aminomethyl)cyclohexanes selected from the group consisting of 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, and 1,4-bis(aminomethyl)cyclohexane, and is preferably one or more bis(aminomethyl)cyclohexanes selected from the group consisting of 1,3-bis(aminomethyl)cyclohexane and 1,4-bis(aminomethyl)cyclohexane, with 1,3-bis(aminomethyl)cyclohexane being more preferred.
[0020] The modified polyamine compound represented by the general formula (1) is preferably at least one selected from the group consisting of the following (I) to (IV): (I) a Mannich reaction product of a polyamine compound represented by the general formula (1), a phenol compound, and an aldehyde compound; (II) a reaction product of a polyamine compound represented by the general formula (1) with an unsaturated hydrocarbon compound; (III) a reaction product of a polyamine compound represented by the general formula (1) with an epoxy compound having at least one epoxy group; and (IV) a reaction product of a polyamine compound represented by the general formula (1) with an unsaturated carboxylic acid or a derivative thereof.
[0021] ((I) Mannich reaction product of a polyamine compound, a phenol compound, and an aldehyde compound represented by the general formula (1)) The modified product (I) is a Mannich reaction product of a polyamine compound, a phenol compound, and an aldehyde compound represented by the general formula (1). Examples of phenolic compounds used in the modified product (I) include naturally occurring phenolic compounds such as phenol, alkylphenols, alkenylphenols, terpene phenols, and cardanol. From the viewpoint of improving the water permeability, weather resistance, strength, and strength retention rate in humid environments of a structure obtained by curing the paving material composition, the number of carbon atoms in the alkyl group of the alkylphenol is preferably 1 to 24, more preferably 1 to 18, and the number of carbon atoms in the alkenyl group of the alkenylphenol is preferably 2 to 24, more preferably 2 to 18. Specific examples of the phenol compound include phenol, cresol, ethylphenol (e.g., p-ethylphenol), isopropylphenol (e.g., o-isopropylphenol, p-isopropylphenol), butylphenol (e.g., p-tert-butylphenol, p-sec-butylphenol, o-tert-butylphenol, o-sec-butylphenol), amylphenol (e.g., p-tert-amylphenol, o-tert-amylphenol), p-octylphenol, nonylphenol, p-cumylphenol, decylphenol, undecylphenol, p-dodecylphenol, tridecylphenol, tetradecylphenol, pentadecylphenol, pentadecenylphenol, pentadecadienylphenol, pentadecatrienylphenol, hexadecylphenol, heptadecylphenol, octadecylphenol, octadecenylphenol, terpene phenol, and cardanol. These may be used alone or in combination of two or more.Among the above, from the viewpoint of reactivity with the polyamine compound represented by the general formula (1), and from the viewpoint of improving the water permeability, weather resistance, strength, and strength retention rate in a humid environment of the structure obtained by curing the paving material composition, the phenol compound used in the modified product (I) is preferably at least one selected from the group consisting of phenol, cresol, p-tert-butylphenol, nonylphenol, and cardanol, and more preferably phenol.
[0022] Examples of the aldehyde compound used in the modified product (I) include formaldehyde; formaldehyde-releasing compounds such as trioxane and paraformaldehyde; and other aldehydes such as benzaldehyde. Among these, at least one selected from the group consisting of formaldehyde and formaldehyde-releasing compounds is preferred. Among these, from the viewpoint of workability in the Mannich reaction, it is more preferred to use an aqueous formaldehyde solution.
[0023] The method for producing the modified product (I) is not particularly limited, and known methods can be used. For example, an aldehyde compound or a solution thereof is added dropwise to a mixture of the polyamine compound and the phenol compound, preferably at 80°C or below, more preferably 60°C or below. After the addition is complete, the temperature is raised to 80 to 180°C, more preferably 90 to 150°C, and the reaction is continued for 1 to 10 hours while removing the distillate from the reaction system. The amounts of the polyamine compound, phenol compound, and aldehyde compound used in the Mannich reaction are not particularly limited, as long as the resulting modified product (I) contains an amino group having an active hydrogen. However, from the viewpoints of reactivity with the polyamine compound represented by the general formula (1) and the water permeability, weather resistance, strength, and strength retention in humid environments of the structure obtained by curing the paving material composition, the following ranges are preferred. The aldehyde compound is preferably used in an amount of 0.3 to 2 moles, more preferably 0.5 to 1.5 moles, per mole of the polyamine compound. The phenol compound is used in an amount of preferably 0.3 to 2 moles, more preferably 0.5 to 1.5 moles, per mole of the polyamine compound.
[0024] ((II) Reaction Product of Polyamine Compound Represented by General Formula (1) and Unsaturated Hydrocarbon Compound) The modified product (II) is a reaction product of a polyamine compound represented by General Formula (1) and an unsaturated hydrocarbon compound. The unsaturated hydrocarbon compound used in the modified product (II) is preferably an unsaturated hydrocarbon compound having 2 to 10 carbon atoms, from the viewpoints of reactivity with the polyamine compound represented by General Formula (1) and improving the water permeability, weather resistance, strength, and strength retention rate in humid environments of the structure obtained by curing the paving material composition. Examples of the unsaturated hydrocarbon compound include unsaturated aliphatic hydrocarbon compounds having 2 to 10 carbon atoms and aromatic hydrocarbon compounds having 2 to 10 carbon atoms and having an ethylenically unsaturated bond, such as at least one selected from the group consisting of ethylene, propylene, butene, pentene, hexene, heptene, octene, nonene, decene, isobutylene, 2-pentene, 3-methyl-1-butene, 2-methyl-2-butene, 2,3-dimethyl-2-butene, cyclohexene, cyclohexadiene, styrene, and divinylbenzene. Among these, aromatic hydrocarbon compounds having an ethylenically unsaturated bond, such as styrene and divinylbenzene, are preferred, with styrene being more preferred, from the viewpoint of reactivity with the polyamine compound represented by general formula (1) and from the viewpoint of improving the water permeability, weather resistance, strength, and strength retention in humid environments of the structure obtained by curing the paving material composition.
[0025] The method for producing the modified product (II) is not particularly limited, and known methods can be used. For example, it can be obtained by subjecting the polyamine compound and an unsaturated hydrocarbon compound to an addition reaction under heating. The amount of the unsaturated hydrocarbon compound used in the addition reaction is not particularly limited as long as the resulting modified product (II) contains an amino group having an active hydrogen. The amount is preferably 0.1 to 5.0 mol, more preferably 0.4 to 3.0 mol, even more preferably 0.5 to 1.5 mol, and even more preferably 0.8 to 1.2 mol per mol of the polyamine compound.
[0026] ((III) Reaction Product of Polyamine Compound Represented by General Formula (1) and Epoxy Compound Having at Least One Epoxy Group) The modified product (III) is a reaction product of a polyamine compound represented by General Formula (1) and an epoxy compound having at least one epoxy group. Examples of epoxy compounds used in the modified product (III) include epichlorohydrin, butyl glycidyl ether, neopentyl glycol diglycidyl ether, 1,3-propanediol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, biphenol diglycidyl ether, dihydroxynaphthalene diglycidyl ether, dihydroxyanthracene diglycidyl ether, triglycidyl isocyanurate, tetraglycidyl glycoluril, a polyfunctional epoxy resin having a glycidylamino group derived from metaxylylenediamine, and a polyfunctional epoxy resin derived from 1,3-bis(aminomethyl)cyclohexane. Examples of suitable epoxy resins include polyfunctional epoxy resins having glycidylamino groups derived from diaminodiphenylmethane, polyfunctional epoxy resins having glycidylamino groups and glycidyloxy groups derived from paraaminophenol, polyfunctional epoxy resins having glycidyloxy groups derived from bisphenol A, polyfunctional epoxy resins having glycidyloxy groups derived from bisphenol F, polyfunctional epoxy resins having glycidyloxy groups derived from phenol novolac, and polyfunctional epoxy resins having glycidyloxy groups derived from resorcinol, and one or more of these may be used.
[0027] The method for producing the modified product (III) is not particularly limited, and known methods can be used. For example, it can be obtained by subjecting the polyamine compound and the epoxy compound to an addition reaction under heating. The amounts of the polyamine compound and the epoxy compound used in the addition reaction are not particularly limited as long as the ratio is such that the resulting modified product (III) contains an amino group having active hydrogen. However, it is preferable to use an excess amount of the polyamine compound relative to the epoxy equivalent of the epoxy compound. Specifically, the polyamine compound and the epoxy compound are reacted in a ratio such that the number of active hydrogen atoms in the polyamine compound / the number of epoxy groups in the epoxy compound is preferably 4 to 50, more preferably 8 to 20.
[0028] (IV) Reaction product of polyamine compound represented by the general formula (1) and unsaturated carboxylic acid or its derivative) The modified product (IV) is a reaction product of polyamine compound represented by the general formula (1) and unsaturated carboxylic acid or its derivative. Examples of the unsaturated carboxylic acid or a derivative thereof used in the modified product (IV) include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, α-ethylacrylic acid, α-propylacrylic acid, α-isopropylacrylic acid, α-n-butylacrylic acid, α-t-butylacrylic acid, α-pentylacrylic acid, α-phenylacrylic acid, α-benzylacrylic acid, crotonic acid, 2-pentenoic acid, 2-hexenoic acid, 4-methyl-2-pentenoic acid, 2-heptenoic acid, 4-methyl-2-hexenoic acid, 5-methyl-2-hexenoic acid, 4,4-dimethyl-2-pentenoic acid, 4-phenyl-2-butenoic acid, cinnamic acid, o-methylcinnamic acid, m-methylcinnamic acid, p-methylcinnamic acid, and 2-octenoic acid, as well as esters, amides, acid anhydrides, and acid chlorides thereof. Among the above, the unsaturated carboxylic acid or derivative thereof is preferably at least one selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid, and derivatives thereof, more preferably at least one selected from the group consisting of acrylic acid, methacrylic acid, crotonic acid, and alkyl esters thereof, still more preferably at least one selected from the group consisting of acrylic acid, methacrylic acid, and alkyl esters thereof, even more preferably alkyl esters of acrylic acid, and even more preferably methyl acrylate.
[0029] The method for producing the modified product (IV) is not particularly limited, and known methods can be used. For example, the modified product (IV) can be obtained by reacting the polyamine compound with an unsaturated carboxylic acid or a derivative thereof under heating. The reaction molar ratio of the polyamine compound to the unsaturated carboxylic acid or a derivative thereof (polyamine compound / unsaturated carboxylic acid or a derivative thereof) is not particularly limited as long as the resulting modified product (IV) contains an amino group having an active hydrogen, but is preferably in the range of 0.3 to 1.0, more preferably 0.6 to 1.0.
[0030] The polyamine compounds and modified products thereof can be used alone or in combination of two or more. Among the above, component (A) is at least one selected from the group consisting of 1,3-bis(aminomethyl)cyclohexane and 1,4-bis(aminomethyl)cyclohexane, and more preferably 1,3-bis(aminomethyl)cyclohexane.
[0031] The active hydrogen equivalent weight (AHEW) of component (A) is preferably 130 or less, more preferably 120 or less, and even more preferably 110 or less. When the AHEW of component (A) is 130 or less, good curing performance is exhibited even when the amount blended into the paving material composition is small. Furthermore, the AHEW of component (A) is a value equal to or greater than the AHEW of bis(aminomethyl)cyclohexane, and is therefore 35.6 or more. The AHEW of component (A) can be determined, for example, by titration.
[0032] The content of component (A) in the epoxy resin curing agent is 50% by mass or more, preferably 70% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, and still more preferably 95% by mass or more, and 100% by mass or less, from the viewpoint of improving the water permeability, weather resistance, strength, and strength retention rate in a humid environment of the structure obtained by curing the paving material composition.
[0033] (Other Curing Agent Components) The epoxy resin curing agent may further contain other curing agent components other than component (A). Examples of the "other curing agent components" include polyamine compounds other than component (A) or modified products thereof. Examples of the polyamine compounds include linear aliphatic polyamine compounds such as ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, hexamethylenediamine, 2-methylpentamethylenediamine, and trimethylhexamethylenediamine; aliphatic polyamine compounds having an aromatic ring such as orthoxylenediamine, metaxylylenediamine, and paraxylylenediamine; menthanediamine, isophoronediamine, norbornanediamine, tricyclodecanediamine, adamantanediamine, diaminocyclohexane, 1,4-diamino-2-methylcyclohexane, 1,4-diamino-3,6-diethylcyclohexane, and diaminodiethylmethylcyclohexane. Examples of suitable polyamine compounds include polyamine compounds having an alicyclic structure such as cyclohexane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane (bis(4-amino-3-methylcyclohexyl)methane), 3,3',5,5'-tetramethyl-4,4'-diaminodicyclohexylmethane, and 4,4'-diaminodicyclohexylmethane; aromatic polyamine compounds such as phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone, diethyltoluenediamine, and 2,2'-diethyl-4,4'-methylenedianiline; polyamine compounds having a heterocyclic structure such as N-aminomethylpiperazine, N-aminoethylpiperazine, and N,N'-bis(aminoethyl)piperazine; and polyether polyamine compounds. Modified versions of the polyamine compounds include Mannich-modified versions, epoxy-modified versions, Michael adducts, Michael addition / polycondensation products, styrene-modified versions, and polyamide-modified versions of the above compounds. These may be used alone or in combination of two or more.
[0034] However, from the viewpoint of more effectively obtaining the effects of the present invention, the content of curing agent components other than component (A) in the epoxy resin curing agent is 50% by mass or less, preferably 30% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, still more preferably 5% by mass or less, and may be 0% by mass.
[0035] From the viewpoint of exhibiting high curing properties even when incorporated in a small amount into a paving material composition, the active hydrogen equivalent weight (AHEW) of the epoxy resin curing agent is preferably 150 or less, more preferably 140 or less, even more preferably 130 or less, and even more preferably 120 or less. On the other hand, from the viewpoint of improving the water permeability, weather resistance, strength, and strength retention rate in humid environments of a structure obtained by curing the paving material composition, the AHEW of the curing agent is preferably 30 or more, more preferably 35 or more.
[0036] <Aggregate> The aggregate used in the present invention is preferably an inorganic granular aggregate for landscape paving. The aggregate may be either a natural aggregate or an artificial aggregate, but from the perspective of use in landscape paving, natural aggregates such as natural stone are preferred. Specific examples of aggregates include pebbles, river gravel, crushed stone, silica stone, river sand, crushed sand, silica sand, slag, glass beads, crushed glass pieces, crushed pottery pieces, ceramic balls, processed industrial waste products, and powders or fine particles of alumina, clay, talc, glass, mica, calcium carbonate, barium sulfate, aluminum oxide, and aluminum hydroxide. One or more of these may be used. Among the above, from the perspective of use in landscape paving and from the perspective of improving the water permeability, weather resistance, strength, and strength retention rate in humid environments of the structure obtained by curing the paving composition, at least one selected from the group consisting of pebbles and silica sand is preferred. Pebbles are more preferred from the perspective of improving the water permeability of the structure obtained by curing the paving composition.
[0037] The particle size of the aggregate is not particularly limited, but is preferably 0.002 to 50 mm, more preferably 0.1 to 30 mm, even more preferably 0.5 to 20 mm, and even more preferably 0.5 to 10 mm. If the particle size of the aggregate is 0.002 mm or more, the resulting structure will have good permeability, strength, and improved strength retention in a wet environment. If the particle size is 50 mm or less, the resulting structure will have good strength and improved strength retention in a wet environment. The particle size of the aggregate can be determined by a method in accordance with JIS A1204:2020 "Soil Grain Size Testing Method."
[0038] The particle size classification of silica sand is classified into No. 3 to No. 8 in JIS G 5901:2016. When the aggregate is silica sand, the particle size classification of the silica sand is preferably silica sand No. 3 to No. 7, more preferably silica sand No. 3 to No. 5, and even more preferably silica sand No. 3 to No. 4, from the viewpoint of improving the water permeability, weather resistance, strength, and strength retention rate in a humid environment of a structure obtained by curing the paving material composition.
[0039] The particle shape of the aggregate is not particularly limited and may be either spherical or non-spherical. Spherical includes nearly spherical shapes such as elliptical cross sections. Non-spherical particle shapes include plate-like, scale-like, chain-like, columnar, and fragment-like shapes.
[0040] The moisture content of the aggregate is not particularly limited, but from the viewpoint of improving the strength of the resulting structure and strength retention in a humid environment, it is preferably 30% by mass or less, more preferably 25% by mass or less, even more preferably 20% by mass or less, even more preferably 10% by mass or less, even more preferably 5.0% by mass or less, and even more preferably 3.0% by mass or less. The lower limit may be 0% by mass, and is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more. The moisture content of the aggregate referred to here means the moisture content of the aggregate when blended into the composition of the present invention. Specifically, the moisture content of the aggregate can be measured by the method described in the Examples.
[0041] <Other Components> The paving material composition may further contain other components such as known modifying components such as plasticizers, flow-adjusting components such as thixotropic agents, leveling agents, tackifiers, and curing accelerators, within the scope of the present invention.
[0042] <Contents> The contents or content ratios of each component in the paving material composition are preferably within the following ranges: The ratio of the epoxy resin to the epoxy resin curing agent contained in the paving material composition is, from the viewpoints of curability and improving the water permeability, weather resistance, strength, and strength retention rate in humid environments of the resulting structure, such that the ratio of the number of active hydrogens in the epoxy resin curing agent to the number of epoxy groups in the epoxy resin [number of active hydrogens / number of epoxy groups] is preferably 1 / 0.8 to 1 / 1.2, more preferably 1 / 0.9 to 1 / 1.1, and even more preferably 1 / 1.
[0043] The mass ratio of the epoxy resin to the aggregate contained in the paving material composition [epoxy resin / aggregate] is preferably in the range of 0.005 to 0.5, more preferably 0.01 to 0.3, even more preferably 0.01 to 0.2, and even more preferably 0.01 to 0.1. If the [epoxy resin / aggregate] is 0.005 or higher, it is easy to suppress aggregate shedding in the resulting structure, and if it is 0.5 or lower, the water permeability, strength, and strength retention rate in humid environments of the resulting structure are further improved. Note that when the aggregate used is a wet aggregate, it is preferable that the mass ratio of the epoxy resin to the dry mass of the aggregate be in the above range.
[0044] The content of the epoxy resin in the paving material composition is preferably 0.1 to 30% by mass, more preferably 0.2 to 25% by mass, even more preferably 0.5 to 20% by mass, still more preferably 1.0 to 15% by mass, and even more preferably 1.0 to 10% by mass, from the viewpoints of curability, water permeability, weather resistance, strength, and improving strength retention in a humid environment of the resulting structure.
[0045] The content of the epoxy resin curing agent in the paving material composition is preferably 0.01 to 15% by mass, more preferably 0.05 to 10% by mass, and even more preferably 0.1 to 5.0% by mass, from the viewpoints of curability, water permeability, weather resistance, strength, and improvement of strength retention in a humid environment of the resulting structure.
[0046] The content of aggregate in the paving material composition is preferably 50 to 99.5% by mass, more preferably 55 to 99% by mass, even more preferably 60 to 99% by mass, even more preferably 70 to 99% by mass, even more preferably 80 to 99% by mass, even more preferably 85 to 99% by mass, and even more preferably 87 to 99% by mass, from the viewpoints of hardening property, water permeability, weather resistance, strength, and strength retention in wet environments of the resulting structure. In this specification, "aggregate content" means the content based on the dry mass of the aggregate, even when wet aggregate is used.
[0047] The total content of epoxy resin, epoxy resin curing agent, and aggregate in the paving material composition is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, still more preferably 90% by mass or more, and still more preferably 95% by mass or more, but not more than 100% by mass, from the viewpoint of improving the water permeability, weather resistance, strength, and strength retention rate in a humid environment of the resulting structure.
[0048] The water content in the paving material composition is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less, from the viewpoint of improving the strength of the resulting structure and the strength retention rate in a wet environment. However, the water content is the amount of water intentionally blended, and does not exclude, for example, the inclusion of water already contained in each blending component.
[0049] The content of organic solvents in the paving material composition is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less, from the viewpoint of improving the strength of the resulting structure and the strength retention rate in a wet environment, with the lower limit being 0% by mass.
[0050] The method for producing the epoxy resin composition of the present invention is not particularly limited, and the composition can be produced by mixing the epoxy resin, the epoxy resin curing agent, the aggregate, and, if necessary, other components using a known method and apparatus.
[0051] [Structure] The structure of the present invention includes a cured product of the paving composition of the present invention described above. The paving composition can be cured by a known method. The curing conditions for the paving composition are appropriately selected depending on the use environment, the shape of the structure, etc., and are not particularly limited, but it can be cured under room temperature conditions in the atmosphere. The structure of the present invention is suitable for use as a paving material, particularly a landscape paving material.
[0052] <Structure Properties> The paving composition of the present invention can provide a structure with high strength and strength retention in a humid environment. For example, a 16 cm x 16 cm x 4 cm flat plate-shaped structure obtained by curing the paving composition of the present invention has a maximum bending stress measured by a bending test at a test speed of 1 mm / min according to JIS R 5201:2015 of preferably 2.0 MPa or more, more preferably 2.5 MPa or more, and even more preferably 3.0 MPa or more. Furthermore, the maximum bending stress retention rate after immersion of the structure in water at 23 ° C for one week is preferably 90% or more, more preferably 95% or more. The maximum bending stress and its retention rate can be specifically determined by the method described in the examples.
[0053] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. Various measurements in the examples were carried out by the following methods.
[0054] (Moisture Content of Aggregate) 100 to 150 g of aggregate that had been stored under conditions of 23°C and 50% RH was weighed out and dried in a hot air dryer at 110°C. The weight was measured as appropriate, and when no change in weight was observed, it was assumed that the moisture had completely dried, and the moisture content of the aggregate was calculated using the following formula: Moisture content of aggregate (mass%) = [(mass (g) of aggregate before drying) - (mass (g) of aggregate after drying)] / (mass (g) of aggregate before drying) x 100
[0055] (Water Permeability) The paving composition obtained in each example was placed in an 11 cm x 11 cm x 2 cm mold and cured for one week in an atmosphere at 23 ° C and 50% RH. A 50 mL screw tube filled with water was placed upside down on the obtained flat-plate-shaped cured product, and the time until the water in the screw tube completely drained was measured. Here, the water drained relatively slowly in the first test, but with repeated tests, the time until the water completely drained gradually became faster and eventually reached a steady state. Therefore, this test was repeated using the same cured product, and the test was terminated when the water draining rate became constant. The time required for the water to completely drain when the water draining rate became constant is shown in Table 1. If the time until the water completely drained was less than 2 minutes, it was determined that the water permeability was good.
[0056] (Glass transition temperature (Tg)) The epoxy resins and epoxy resin curing agents shown in Table 1 were mixed so that the number of epoxy groups in the epoxy resins and the number of active hydrogens in the epoxy resin curing agents were equal in amount. The resulting mixture was cured and aged for 7 days under conditions of 23°C and 50% RH to prepare a sample. The sample was subjected to differential scanning calorimetry from 35 to 225°C at a heating rate of 10°C / min using a differential scanning calorimeter "TA DSC-25" (manufactured by Omron Corporation) to determine Tg.
[0057] (Weather Resistance (YI)) A weather resistance test was carried out in accordance with ISO 4982 Part 3 Method A. The epoxy resins and epoxy resin curing agents shown in Table 1 were mixed so that the number of epoxy groups in the epoxy resin and the number of active hydrogens in the epoxy resin curing agent were equal in amount. The resulting mixture was placed in a 5 cm x 5 cm x 2 mm mold and cured in an atmosphere at 23°C and 50% RH for one week. The YI value of the obtained flat-plate-shaped cured product (test piece) was measured in accordance with JIS K7373:2006 using a color difference meter ("COH400" manufactured by Nippon Denshoku Industries Co., Ltd.) (cumulative exposure of 0 kJ / m 2 Then, the test piece was placed in a UV tester "Suntest XXL+" (manufactured by Toyo Seiki Seisakusho Co., Ltd.), and exposed to ultraviolet light of 300 to 400 nm wavelength from a xenon lamp at an illuminance of 60 W / m 2After the cumulative exposure reached a predetermined amount, the test piece was removed and the YI value was measured in the same manner as above, and the results are shown in Table 1. The smaller the increase in the YI value, the better the weather resistance of the cured product. 2 If the YI value at this point is 15 or less, it can be determined that the weather resistance is good.
[0058] (Maximum bending stress) The paving material compositions listed in Tables 2 and 3 were placed in a 16 cm x 16 cm x 4 cm mold and cured in an atmosphere at 23°C and 50% RH for one week. The resulting cured products were subjected to a bending test (N = 3) at a test speed of 1 mm / min using a precision universal testing machine (Shimadzu Corporation's "Autograph AG-Xplus 100kN") in accordance with JIS R 5201:2015, to measure the maximum bending stress before immersion in water. The maximum bending stress was taken as the average value of three measurements. The above cured products were also immersed in water at 23°C for one week and subjected to a bending test in the same manner. The bending stress retention of the cured product after immersion in water was calculated according to the following formula: Bending stress retention (%) = (maximum bending stress of cured product after immersion in water) / (maximum bending stress of cured product before immersion in water) x 100
[0059] Examples 1 to 4, Comparative Examples 1 to 6 (Preparation and Evaluation of Paving Material Compositions and Cured Products (1) - Water Permeability and Weather Resistance) The epoxy resins, epoxy resin curing agents, and aggregates listed in Table 1 were each weighed and mixed, and then stirred by hand for 4 minutes under conditions of 23°C and 50% RH to prepare paving material compositions. The mixture was mixed so that the number of epoxy groups in the epoxy resin and the number of active hydrogens in the epoxy resin curing agent were equal. Using these compositions, water permeability was evaluated using the method described above. Furthermore, weather resistance was evaluated using the epoxy resins and epoxy resin curing agents listed in Table 1, using the method described above. The results are shown in Table 1.
[0060] Examples 2 and 4, Comparative Examples 7 to 16 (Preparation and Evaluation of Paving Material Compositions and Cured Products (2) - Strength of Cured Products Before and After Immersion in Water) The epoxy resins, epoxy resin curing agents, and aggregates listed in Tables 2 and 3 were weighed and mixed together, and then stirred by hand for 4 minutes at 23°C and 50% RH to prepare paving material compositions. The mixture was mixed so that the number of epoxy groups in the epoxy resin and the number of active hydrogens in the epoxy resin curing agent were equal. Using these compositions, cured products were prepared and their strength was evaluated (measurement of maximum bending stress and bending stress retention) using the method described above. The results are shown in Tables 2 and 3.
[0061]
[0062]
[0063]
[0064] The components used in Tables 1 to 3 are as follows: <Epoxy resin> jER828: Liquid epoxy resin having a glycidyloxy group derived from bisphenol A (manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 186 g / equivalent, solid content: 100% by mass) <Epoxy resin curing agent> 1,3-BAC: 1,3-bis(aminomethyl)cyclohexane, manufactured by Mitsubishi Gas Chemical Co., Ltd. MXDA: metaxylylenediamine, manufactured by Mitsubishi Gas Chemical Co., Ltd. IPDA: isophoronediamine DETA: diethylenetriamine TETA: triethylenetetramine <Aggregate> Silica sand No. 4: "Nikko Silica Sand No. 4" manufactured by JFE Mineral Corporation, particle size 0.6 to 1.2 mm, moisture content 0.2% by mass Gravel: "Gravel friendly to aquatic plants and fish" manufactured by Kamihata Fish Farming Co., Ltd., particle size 1 to 5 mm, moisture content 1.3% by mass
[0065] As shown in Table 1, the cured product of the paving composition of the present invention has high water permeability, and the cured product of the epoxy resin composition (epoxy resin + epoxy resin curing agent) used in the paving composition has high Tg and weather resistance. Furthermore, as shown in Tables 2 and 3, the cured product of the paving composition of the present invention has high initial strength (maximum bending stress before submersion) and bending stress retention after submersion, indicating high strength and excellent strength retention even in humid environments. In contrast, as shown in Table 1, compared to the Examples, the cured products of the paving compositions of Comparative Examples 1-2 and 5-6 had low water permeability, the cured products of the epoxy resin composition (epoxy resin + epoxy resin curing agent) used in the paving compositions of Comparative Examples 1-6 had low Tg, and the cured products of the epoxy resin composition used in the paving compositions of Comparative Examples 1-2 and 4-6 had poor weather resistance. Furthermore, as shown in Tables 2 and 3, compared to the Examples, the cured products of the paving compositions of Comparative Examples 7-16 had inferior early strength (maximum bending stress before submersion) or bending stress retention.
[0066] According to the present invention, it is possible to provide a paving material composition that can provide a structure having high water permeability, weather resistance, and strength, and excellent strength retention even in a wet environment.
Claims
1. A paving material composition comprising an epoxy resin, an epoxy resin curing agent containing 50% by mass or more of a polyamine compound represented by the following general formula (1) or a modified product thereof (A), and an aggregate. 2 N-CH 2 -X-CH 2 -NH 2 (1) (In formula (1), X is a cyclohexylene group.) 2. The paving material composition according to claim 1, wherein the modified polyamine compound is at least one selected from the group consisting of the following (I) to (IV): (I) a Mannich reaction product of the polyamine compound represented by the general formula (1), a phenol compound, and an aldehyde compound (II) a reaction product of the polyamine compound represented by the general formula (1) and an unsaturated hydrocarbon compound (III) a reaction product of the polyamine compound represented by the general formula (1) and an epoxy compound having at least one epoxy group (IV) a reaction product of the polyamine compound represented by the general formula (1) and an unsaturated carboxylic acid or a derivative thereof.
3. A paving material composition according to claim 1 or 2, wherein the mass ratio of said epoxy resin to said aggregate [epoxy resin / aggregate] is in the range of 0.005 to 0.
5.
4. A paving material composition according to any one of claims 1 to 3, wherein the aggregate has a particle size of 0.002 to 50 mm.
5. A structure comprising a cured product of the paving material composition according to any one of claims 1 to 4.
Citation Information
Patent Citations
Pavement material using attenuated resin as binder and pavement construction method using it
JP2002294616A
Cold-stirring cold-paving type epoxy modified asphalt material and preparation method thereof
CN106977966A
Water-resistant grouting material for treating bulge disease of steel bridge deck pavement as well as preparation method and usage method
CN107446119A
Pavement wearing layer with efficient snow melting and deicing functions and preparation method thereof
CN113861796A
Economical low-temperature-resistant high-flexibility epoxy resin material for epoxy asphalt and preparation method thereof
CN114891319A