Hollow silica particles

The development of hollow silica particles with specific multimodal particle size distributions addresses the issues of viscosity increase and strength in resin kneading, achieving improved operability and functionality by dispersing pressure and maintaining the hollow structure, resulting in reduced dielectric properties.

WO2024202625A1PCT designated stage expired Publication Date: 2024-10-03TOKUYAMA CORP

Patent Information

Application Number
PCT/JP2024/004935
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-14
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Hollow silica particles with uniform or multimodal particle size distributions face challenges in increasing viscosity and operability when kneaded into resin, making it difficult to maintain strength and functionality, especially in fine spaces.

Method used

Developing hollow silica particles with a multimodal particle size distribution having peaks between 0.1 μm and 5.0 μm, with 60% or more of the particles in the 0.1 μm to 0.5 μm range and a maximum particle diameter of 10 μm or less, which helps in dispersing pressure during kneading and suppressing viscosity increase while maintaining strength.

Benefits of technology

The approach results in hollow silica particles that minimize viscosity increase, enhance resin composition strength, and maintain the hollow structure, allowing for better operability and functionality, with reduced dielectric constant and dielectric loss tangent compared to solid silica particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-M000001
    Figure JPOXMLDOC01-APPB-M000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

One embodiment of the present invention provides hollow silica particles that suppress an increase in viscosity after kneading into a resin, have high strength, and are capable of achieving both operability and functionality. The hollow silica particles according to one embodiment of the present invention exhibit one or more peaks in the range of 0.1-0.5 μm and one or more peaks in the range of more than 0.5 μm and 5.0 μm or less in a particle size distribution in terms of volume distribution measured by a laser diffraction scattering method, wherein particles associated with the peak(s) in the range of 0.1-0.5 μm in terms of volume distribution are 60% by volume or more, the maximum particle diameter (D100) of the hollow silica particles is 10 μm or less, and the apparent density A of the particles before kneading into the resin and the apparent density B of the particles after kneading into the resin satisfy 0.8 < (A / B).
Need to check novelty before this filing date? Find Prior Art

Description

Hollow Silica Particles

[0001] The present invention relates to fine hollow silica particles that exhibit a small increase in viscosity when kneaded into a resin and have high strength.

[0002] Hollow silica particles have a lower specific gravity than solid silica particles, and due to their hollow shape, they have properties such as a low dielectric constant, a low dielectric dissipation factor, and a low thermoelectric constant. Therefore, by blending hollow silica particles with resins, they can reduce the weight of the resin, lower the dielectric constant, lower the dielectric dissipation factor, and improve thermal insulation, and are used in a wide range of applications. Specifically, hollow silica particles with a uniform particle size distribution that improves packing ability (see, for example, Patent Document 1) and hollow particles with a multimodal particle size distribution with two or more peaks that achieve adhesion and strength (see, for example, Patent Document 2) have been reported.

[0003] Japanese Patent Publication No. 2009-203115 Japanese Patent Publication No. 2019-172474

[0004] The hollow silica particles with a uniform particle size distribution described in Patent Document 1 increase the viscosity of the resin composition when kneaded into a resin, leaving issues with operability. Furthermore, the multimodal hollow silica particles described in Patent Document 2 have a large particle diameter, which makes it difficult to fill the fine spaces with resin when kneaded into a resin, limiting their usable applications. Furthermore, in order for hollow silica particles to exhibit their functionality after kneading into a resin, it is generally necessary to achieve both particle strength and particle porosity. However, minute hollow silica particles have a small particle diameter relative to their shell thickness, and changing the shell thickness to improve particle strength has a significant impact on porosity. Therefore, it is necessary to maintain the hollow structure of minute hollow silica particles without changing the shell thickness. Based on the above background, an object of the present invention is to provide hollow silica particles that suppress an increase in viscosity after kneading into a resin, have high strength, and are capable of achieving both operability and functionality.

[0005] The present inventors have conducted extensive research to solve the above problems and have found that by producing multimodal hollow silica particles having a maximum particle size of a certain level or less, it is possible to suppress an increase in viscosity of a resin composition after kneading with a resin, and to obtain hollow silica particles with high strength.

[0006] That is, the hollow silica particles according to one embodiment of the present invention are hollow silica particles having, in a particle size distribution converted into a volume distribution as measured by a laser diffraction scattering method, one or more peaks in the range of 0.1 μm or more and one or more peaks in the range of more than 0.5 μm and 5.0 μm or less, wherein the particles on the peak side of 0.1 μm or more and 0.5 μm or less in the volume distribution converted into a volume distribution account for 60% or more by volume, the maximum particle size (D100) of the hollow silica particles is 10 μm or less, and the apparent density A of the hollow silica particles before being kneaded with a resin and the apparent density B of the hollow silica particles after being kneaded with a resin satisfy the relationship 0.8<(A / B).

[0007] According to the present invention, it is possible to provide hollow silica particles that are suppressed from increasing in viscosity after being kneaded with a resin, have high strength, and are capable of achieving both ease of handling and functionality.

[0008] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.

[0009] The hollow silica particles of the present invention have, in a particle size distribution converted into a volume distribution as measured by a laser diffraction scattering method, one or more peaks in the range of 0.1 μm or more and 0.5 μm or less, and one or more peaks in the range of more than 0.5 μm and 5.0 μm or less, in which the particles on the peak side of 0.1 μm or more and 0.5 μm or less in the volume distribution converted into a volume distribution account for 60% or more by volume, the maximum particle size (D100) of the hollow silica particles is 10 μm or less, and the apparent density A of the hollow silica particles before kneading with a resin and the apparent density B of the hollow silica particles after kneading with a resin satisfy the relationship 0.8<(A / B).

[0010] In the particle size distribution converted to volume distribution, the peak in the range of 0.1 μm or more and 0.5 μm or less is preferably located at 0.2 to 0.48 μm, more preferably 0.3 to 0.45 μm. Furthermore, the peak in the range of more than 0.5 μm and less than 5.0 μm is preferably located at 0.8 to 4 μm, more preferably 1 to 3 μm. Hollow silica particles having a multimodal particle size distribution with such peaks exhibit a small increase in viscosity when kneaded with a resin, and the difference in apparent density between the hollow silica particles after kneading with a resin and the hollow silica particles before kneading with a resin is small. The reason for this is unclear, but is presumed to be as follows: The presence of a peak in the range of 0.1 μm or more and 0.5 μm or less distributes the pressure during kneading with a resin, improving the strength of the hollow silica particles as a whole. Furthermore, the presence of a peak in the range of more than 0.5 μm and less than 5.0 μm suppresses the increase in viscosity of the hollow silica particles as a whole. For these reasons, the viscosity increase of the entire resin composition can be suppressed and the strength can be improved. Note that if the peak is 0.1 μm or less, the viscosity of the resin composition will increase significantly after kneading with the resin, and the porosity inside the hollow silica particles will decrease, which is not preferable. On the other hand, if the peak is in the range of more than 5 μm, it will be difficult for the resin composition to penetrate into fine gaps, which is not preferable.

[0011] The particle size distribution of the hollow silica particles of the present invention is such that, in the particle size distribution converted to a volume distribution measured by a laser diffraction scattering method, 60% or more by volume of particles are on the peak side in the range of 0.1 μm to 0.5 μm. The particle size distribution is measured by measuring the volume frequency of the detected particles for each particle size. Therefore, when a particle size is selected, the volume frequency at the selected particle size is compared with the volume frequencies of particle sizes measured before and after it. If the volume frequency at the selected particle size is greater than the volume frequencies of particle sizes measured before and after it, it can be determined that the selected particle size has a peak. This allows the peak positions of the measured particle size distribution to be determined, identifying the position of the largest peak in the range of 0.1 μm to 0.5 μm and the position of the smallest peak in the range of more than 0.5 μm to 5.0 μm. The particle size with the smallest volume frequency between the identified peaks is then set as the boundary value. The particles on the peak side of the range of 0.1 μm or more and 0.5 μm or less refer to the cumulative volume frequency of particle diameters in the range of 0 μm to the boundary value or less. If the particles on the peak side of the range of 0.1 μm or more and 0.5 μm or less are less than 60% by volume, it becomes difficult for the resin composition to penetrate into fine gaps, which is undesirable. Furthermore, by reducing this value to a certain extent, the functionality of the multi-modal particle size distribution can be further improved, and the viscosity after kneading into the resin can be further improved. From the viewpoint of the above balance, 60 to 95% by volume is preferable, 65 to 90% by volume is more preferable, and 70 to 85% is even more preferable.

[0012] The maximum particle diameter (D100) of the hollow silica particles of the present invention is 10 μm or less, preferably 9 μm or less, from the viewpoint of filling properties when the resin composition is penetrated into fine gaps. The maximum particle diameter (D100) of the hollow silica particles can be measured, for example, by the method described in the Examples.

[0013] The hollow silica particles of the present invention preferably have their shells not cracked or their pores not penetrated by resin even after being kneaded with resin, that is, can maintain their hollow shape.Specifically, the apparent density (A) of the hollow silica particles before being kneaded with resin is compared with the apparent density (B) of the hollow silica particles converted from the apparent density of the composition after being kneaded with resin, and the density difference (A / B) is greater than 0.8, that is, 0.8<(A / B).The more hollow silica particles that can maintain their hollow shape exist, the more the properties derived from the hollow shape are expressed, so 0.85<(A / B) is preferred, and 0.9<(A / B) is more preferred.

[0014] Due to their characteristics, the hollow silica particles of the present invention have a reduced dielectric constant and dielectric loss tangent compared to solid silica particles. The dielectric constant of the hollow silica particles is preferably 2.0 or less, more preferably 1.8 or less, and more preferably 1.7 or less at a frequency of 10 GHz. The dielectric loss tangent of the hollow silica particles is preferably 0.003 or less, more preferably 0.002 or less, and even more preferably 0.001 or less at a frequency of 10 GHz. The dielectric constant and dielectric loss tangent can be measured using a cavity resonator method or the like.

[0015] The hollow silica particles of the present invention have excellent strength due to their characteristics. The particle strength of the hollow silica particles is preferably 50 MPa or more, more preferably 55 MPa or more. The particle strength can be measured, for example, by the method described in the Examples.

[0016] The hollow silica particles of the present invention are not particularly limited as long as they satisfy the above-mentioned properties, and can be produced, for example, by a sol-gel method.

[0017] The hollow silica particles of the present invention have a multimodal particle size distribution, which can be achieved by mixing separately produced hollow silica particles, or by producing hollow silica particles having a multimodal particle size distribution at once. The produced particles may also be classified to adjust the particle size distribution.

[0018] The hollow silica particles of the present invention are particles having voids inside the particles and a shell portion separating the voids from the outside, and are different from porous silica.

[0019] As can be understood from the above description, the present invention encompasses the following aspects [1] to [3]. Aspect [1]: Hollow silica particles having, in a particle size distribution calculated as a volume distribution as measured by a laser diffraction scattering method, one or more peaks in the range of 0.1 μm to 0.5 μm and one or more peaks in the range of more than 0.5 μm to 5.0 μm, wherein 60 volume % or more of the particles are on the side of the peak at 0.1 μm to 0.5 μm in terms of the volume distribution, the maximum particle size (D100) of the hollow silica particles is 10 μm or less, and the apparent density A of the hollow silica particles before being kneaded with a resin and the apparent density B of the hollow silica particles after being kneaded with a resin satisfy the ratio 0.8<(A / B). Aspect [2]: Hollow silica particles according to aspect [1], having a dielectric constant of 2.0 or less and a dielectric loss tangent of 0.003 or less. Aspect [3]: The hollow silica particles according to aspect [1] or [2], having a particle strength of 50 MPa or more.

[0020] <Production of Hollow Silica Particles Having One or More Peaks in the 0.1 to 0.5 μm Range> (1) Hollow Silica Particles A1 100 g of methanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Wako First Grade), 1.7 g of dodecyltrimethylammonium chloride (manufactured by Tokyo Chemical Industry Co., Ltd.), and 1 g of dodecane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed in a 500 mL flask and stirred to prepare Solution A. 300 g of water and 0.825 g of a 25% aqueous tetramethylammonium hydroxide solution (manufactured by Wako Pure Chemical Industries, Ltd.) were placed in a 500 mL flask and stirred to prepare Solution B. Solution B was added to the resulting Solution A while stirring at 25°C, followed by the addition of 1.7 g of tetramethoxysilane (manufactured by Tama Chemical Industries, Ltd.), and the mixture was stirred at 25°C for 5 hours. The resulting hollow silica particle precursor dispersion was filtered through a 5C filter paper and washed three times with water to recover hollow silica particle precursors. The recovered hollow silica particle precursor was dried at 100°C for 12 hours in a constant temperature air-blowing dryer (Convection Oven, manufactured by Sanyo) to obtain a white powder of hollow silica particle precursor. The obtained white powder was heated to 1000°C at a rate of 1°C / min in an electric furnace (FO810, manufactured by Yamato Scientific) and calcined at 1000°C for 10 hours to obtain hollow silica particles A1 with a particle size distribution peak position of 0.4 µm.

[0021] (2) Hollow Silica Particles A2 100 g of methanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Wako First Grade), 0.9 g of dodecyltrimethylammonium chloride (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.5 g of dodecane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to a 500 mL flask and stirred to prepare Solution A. 300 g of water and 0.413 g of a 25% aqueous tetramethylammonium hydroxide solution (manufactured by Wako Pure Chemical Industries, Ltd.) were added to a 500 mL flask and stirred to prepare Solution B. Solution B was added to the obtained Solution A while stirring at 25 ° C., and then 0.9 g of tetramethoxysilane (manufactured by Tama Chemical Industries, Ltd.) was added and stirred at 25 ° C. for 5 hours. The obtained hollow silica particle precursor dispersion was filtered through 5C filter paper and washed three times with water to recover hollow silica particle precursors. The recovered hollow silica particle precursor was dried at 100°C for 12 hours in a constant temperature air-blowing dryer (Convection Oven, manufactured by Sanyo) to obtain a white powder of hollow silica particle precursor. The obtained white powder was heated to 1000°C at a rate of 1°C / min in an electric furnace (FO810, manufactured by Yamato Scientific) and calcined at 1000°C for 10 hours to obtain hollow silica particles A2 with a particle size distribution peak position of 0.2 µm.

[0022] (3) Hollow Silica Particles A3 100 g of methanol (manufactured by Fujifilm Wako Pure Chemical Industries, Wako First Grade), 1.4 g of dodecyltrimethylammonium chloride (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.8 g of dodecane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to a 500 mL flask and stirred to prepare Solution A. 300 g of water and 0.620 g of a 25% aqueous tetramethylammonium hydroxide solution (manufactured by Wako Pure Chemical Industries, Ltd.) were added to a 500 mL flask and stirred to prepare Solution B. Solution B was added to the obtained Solution A while stirring at 25 ° C., and then 1.4 g of tetramethoxysilane (manufactured by Tama Chemical Industries, Ltd.) was added and stirred at 25 ° C. for 5 hours. The obtained hollow silica particle precursor dispersion was filtered through 5C filter paper and washed three times with water to recover hollow silica particle precursors. The recovered hollow silica particle precursor was dried at 100°C for 12 hours in a constant temperature air-blowing dryer (Convection Oven, manufactured by Sanyo) to obtain a white powder of hollow silica particle precursor. The obtained white powder was heated to 1000°C at a rate of 1°C / min in an electric furnace (FO810, manufactured by Yamato Scientific) and calcined at 1000°C for 10 hours to obtain hollow silica particles A3 with a particle size distribution peak position of 0.3 µm.

[0023] <Preparation of Hollow Silica Particles Having One or More Peaks in the 0.5-5 μm Range> (1) Hollow Silica Particles B1: 1.3 g of hydroxypropyl cellulose (Sigma-Aldrich, average molecular weight approximately 370,000) was added to 86 g of 1-octanol (Junsei Chemical, special grade reagent) in a 200 ml flask, and the mixture was heated to 80°C and stirred for 4 hours. The mixture was then cooled to 40°C, and 2.7 g of sorbitan monooleate (Sigma-Aldrich, Span 80) was added to prepare Solution A. Additionally, 0.6 g of polyethylene glycol (Junsei Chemical, polyethylene glycol 20000) and 0.5 g of polyethylene glycol sorbitan monolaurate (Sigma-Aldrich, Tween 20) were added to 8.1 g of water in a 20 mL snap cup, and the mixture was stirred for 20 minutes. 0.8 g of 25% aqueous ammonia (Fujifilm Wako Pure Chemical Industries, Wako Grade 1) was then added to prepare Solution B. Thereafter, while stirring Solution A at a liquid temperature of 40°C, Solution B was added, and stirring was continued for 1 hour to prepare Solution C. Furthermore, while stirring Solution C, 20 g of tetraethoxysilane (Fujifilm Wako Pure Chemical Industries, Wako Special Grade tetraethyl orthosilicate) was added, and stirring was continued for 14 hours to obtain a hollow silica particle precursor dispersion. The hollow silica precursor dispersion was filtered through 5C filter paper and washed three times with ethanol (Fujifilm Wako Pure Chemical Industries, Wako Grade 1), to recover the hollow silica particle precursor. The recovered hollow silica particle precursor was dried at 130°C for 12 hours in a constant temperature air-blowing dryer (Sanyo, Convection Oven) to obtain a white powder of hollow silica particle precursor. The obtained white powder was heated to 1000°C at a rate of 100°C / hour in an electric furnace (Yamato Scientific, FO810) and calcined at 1000°C for 10 hours to obtain hollow silica B1 having a particle size distribution peak position of 1.7 µm.

[0024] (2) Hollow Silica Particles B2: 1.3 g of hydroxypropyl cellulose (Sigma-Aldrich, average molecular weight approximately 370,000) was added to a 200 ml flask and 86 g of 1-octanol (Junsei Chemical, special grade reagent). The mixture was heated to 80°C and stirred for 4 hours. The mixture was then cooled to 40°C, and 1.5 g of sorbitan monooleate (Sigma-Aldrich, Span 80) was added to prepare Solution A. Additionally, 0.6 g of polyethylene glycol (Junsei Chemical, polyethylene glycol 20000) and 0.3 g of polyethylene glycol sorbitan monolaurate (Sigma-Aldrich, Tween 20) were added to a 20 mL snap cup and stirred for 20 minutes. 0.8 g of 25% aqueous ammonia (Fujifilm Wako Pure Chemical Industries, Wako Grade 1) was then added to prepare Solution B. Thereafter, while stirring Solution A at a liquid temperature of 40°C, Solution B was added, and stirring was continued for 1 hour to prepare Solution C. Furthermore, while stirring Solution C, 20 g of tetraethoxysilane (Fujifilm Wako Pure Chemical Industries, Wako Special Grade tetraethyl orthosilicate) was added, and stirring was continued for 14 hours to obtain a hollow silica particle precursor dispersion. The hollow silica precursor dispersion was filtered through 5C filter paper and washed three times with ethanol (Fujifilm Wako Pure Chemical Industries, Wako Grade 1), to recover the hollow silica particle precursor. The recovered hollow silica particle precursor was dried at 130°C for 12 hours in a constant temperature air-blowing dryer (Sanyo, Convection Oven) to obtain a white powder of hollow silica particle precursor. The obtained white powder was heated to 1000°C at a rate of 100°C / hour in an electric furnace (Yamato Scientific, FO810) and calcined at 1000°C for 10 hours to obtain hollow silica B2 having a particle size distribution peak position of 3.0 μm.

[0025] (3) Hollow Silica Particles B3: 1.3 g of hydroxypropyl cellulose (Sigma-Aldrich, average molecular weight approximately 370,000) was added to a 200 ml flask and 86 g of 1-octanol (Junsei Chemical, special grade reagent). The mixture was heated to 80°C and stirred for 4 hours. The mixture was then cooled to 40°C, and 1.0 g of sorbitan monooleate (Sigma-Aldrich, Span 80) was added to prepare Solution A. Additionally, 0.6 g of polyethylene glycol (Junsei Chemical, polyethylene glycol 20000) and 0.2 g of polyethylene glycol sorbitan monolaurate (Sigma-Aldrich, Tween 20) were added to a 20 mL snap cup and stirred for 20 minutes. 0.8 g of 25% aqueous ammonia (Fujifilm Wako Pure Chemical Industries, Wako Grade 1) was then added to prepare Solution B. Thereafter, while stirring Solution A at a liquid temperature of 40°C, Solution B was added, and stirring was continued for 1 hour to prepare Solution C. Furthermore, while stirring Solution C, 20 g of tetraethoxysilane (Fujifilm Wako Pure Chemical Industries, Wako Special Grade tetraethyl orthosilicate) was added, and stirring was continued for 14 hours to obtain a hollow silica particle precursor dispersion. The hollow silica precursor dispersion was filtered through 5C filter paper and washed three times with ethanol (Fujifilm Wako Pure Chemical Industries, Wako Grade 1), to recover the hollow silica particle precursor. The recovered hollow silica particle precursor was dried at 130°C for 12 hours in a constant temperature air-blowing dryer (Sanyo, Convection Oven) to obtain a white powder of hollow silica particle precursor. The obtained white powder was heated to 1000°C at a rate of 100°C / hour in an electric furnace (Yamato Scientific, FO810) and calcined at 1000°C for 10 hours to obtain hollow silica B3 having a particle size distribution peak position of 4.6 µm.

[0026] The methods for evaluating the properties of the hollow silica particles are as follows.

[0027] (1) Volumetric Particle Size Distribution by Laser Diffraction Scattering Method 0.1 g of hollow silica particles was weighed into a 50 mL glass bottle using an electronic balance, 40 mL of ethanol was added, and the mixture was dispersed using an ultrasonic homogenizer (Sonifier 250, manufactured by BRANSON) at 60 W for 2 minutes. The volumetric mode diameter (μm) and maximum particle diameter (D100) (μm) were then measured using a laser diffraction scattering particle size distribution analyzer (LS 13 320, manufactured by Beckman Coulter). The refractive index of the dispersion medium was 1.36, and the refractive index of the object to be measured was 1.45. The largest particle diameter among the particle diameters detected by the laser diffraction scattering particle size distribution analyzer used was used as the maximum particle diameter (D100).

[0028] (2) Apparent Density of Hollow Silica Particles Before Mixing with Resin Hollow silica particles dried under reduced pressure at 110°C for 24 hours were weighed to the nearest 0.001 g in a 10 ml sample container. Next, the sample container was placed in the measurement chamber of a dry automatic densitometer (Shimadzu Corporation, Dry AccuPyc1330), and the particle density was measured at a measurement temperature of 25°C while flowing nitrogen gas into the measurement chamber. When the mass of the powder used for measurement was input into the dry automatic densitometer, the particle density was expressed in g / cm to five decimal places. 3 Expressed in units of g / cm 3 The particle density was calculated by rounding off the particle density to one decimal place.

[0029] (3) Particle Strength Hollow silica particles were dispersed in ethanol to a concentration of 0.02% by mass, and one drop was placed on the lower pressure plate of a microcompression testing machine (Shimadzu Corporation, MZCT-W510-J) and allowed to dry. A load was applied to one particle on the lower pressure plate using an upper pressure indenter (flat indenter, made of diamond) with a diameter of 20 μm, and the amount of deformation of the particle was automatically measured. Measurement was made using the test force P (N) at which the particle broke and the measured particle diameter Z (mm). Five particles were randomly selected and measured using a microscope attached to the testing machine, and the particle strength (MPa) was calculated using the average value according to the following formula: Particle strength (MPa) = 2.8 × P ÷ π ÷ Z 2

[0030] The following analyses were carried out on resin compositions prepared by the methods described in the Examples. Since the resin and curing agent in the resin composition react after kneading to form a uniform resin, the resin and curing agent were kneaded at a composition ratio of 71:29, and the cured composition was measured, and the value was used. (4) Viscosity Measurement The viscosity was measured using 0.2 g of the resin composition with a rheometer (manufactured by Thermo Fisher Scientific, HAAKE MARS40). The measurement temperature was 25°C, and the sensor was C35 / 1 (cone-plate type, diameter 35 mm, angle 1°, material titanium). The viscosity was measured at a shear rate of 1 s -1 is the value at

[0031] (5) Measurement of Dielectric Constant and Dielectric Loss Tangent The resin composition was poured into a SUS mold with a thickness of 0.4 mm, a short side of 60 mm, and a long side of 70 mm, and heated at 80°C for 1 hour in a constant temperature incubator (Yamato Scientific, DNK302) and then heated at 120°C for 3 hours. The dielectric constant and dielectric loss tangent of the cured resin composition were measured using a network analyzer (Keysight Technologies, N5209A). The measurement was performed at a frequency of 10 GHz. The physical properties of the hollow silica particles were then converted using the Bruggeman equation shown below.

[0032]

[0033] In the formula, Φa represents the volume fraction of the resin and curing agent in the resin composition, Φb represents the volume fraction of the hollow silica particles in the resin composition, εa represents the dielectric constant of the resin and curing agent, εb represents the dielectric constant of the hollow silica particles, and εc represents the dielectric constant of the resin composition.

[0034] (6) Apparent Density of Hollow Silica Particles After Kneading with Resin The resin composition was poured into a Teflon (registered trademark) mold with a thickness of 5 mm, a short side of 10 mm, and a long side of 15 mm, and heated at 80°C for 1 hour in a constant temperature incubator (Yamato Scientific, DNK302), and then heated at 120°C for 3 hours. The density of the cured resin composition was measured using a high-precision electronic hydrometer (Alpha Mirage, SD-200L). The apparent density of the hollow silica particles after kneading with resin was calculated from the true densities of the epoxy resin and curing agent used and the composition ratio of the resin composition. The true densities of the resin and curing agent were 1.18 g / cm. 3 Apparent density of hollow silica particles after kneading with resin = composition ratio of hollow silica particles ÷ {(1 ÷ measured value) - (total composition ratio of resin and curing agent ÷ 1.18)}

[0035]

[0036]

[0037] (Examples 1 to 8, Comparative Examples 1 and 2) A total of 5.0 g of hollow silica particles A and hollow silica particles B, 10.7 g of bisphenol F epoxy resin (YDF-8170 manufactured by Nippon Steel Chemical & Material Co., Ltd.), and 4.3 g of curing agent (KAYAHARD A-A manufactured by Nippon Kayaku Co., Ltd.) were hand-kneaded in the proportions shown in Tables 1 and 2. The resin composition was then pre-kneaded using a planetary centrifugal mixer (THINKY, Awatori Rentaro AR-500) (kneading: 1000 rpm, 8 minutes, degassing: 2000 rpm, 2 minutes). The pre-kneaded resin composition was stored in a 25°C thermostatic water bath and then kneaded using a three-roll mill (IMEX, BR-150HCV, roll diameter φ63.5). The kneading conditions were a kneading temperature of 25°C, a roll distance of 20 μm, and 8 kneading passes. The resulting resin composition was degassed for 30 minutes under reduced pressure using a vacuum pump (TSW-150 manufactured by Sato Vacuum Co., Ltd.). The results are shown in Tables 1 and 2.

[0038] From Tables 1 and 2, it can be seen that the resin compositions of Examples 1 to 8 containing the hollow silica particles of the present invention have low viscosity and high strength, and therefore have small density differences and low values ​​of dielectric constant and dielectric loss tangent. In Comparative Example 1, the viscosity of the resin composition was too high, making it impossible to measure the viscosity.

Claims

1. Hollow silica particles having at least one peak in the range of 0.1 μm or more and at most 0.5 μm or less, and at least one peak in the range of more than 0.5 μm and at most 5.0 μm, in a particle size distribution converted into volume distribution measured by a laser diffraction scattering method, wherein at least 60 volume % of the particles are on the peak side of 0.1 μm or more and at most 0.5 μm or less in a volume distribution converted into volume distribution, the maximum particle diameter (D100) of the hollow silica particles is 10 μm or less, and the apparent density A of the hollow silica particles before being kneaded with a resin and the apparent density B of the hollow silica particles after being kneaded with a resin are 0.8<(A / B).

2. The hollow silica particles according to claim 1, which have a dielectric constant of 2.0 or less and a dielectric loss tangent of 0.003 or less.

3. The hollow silica particles according to claim 1 or 2, having a particle strength of 50 MPa or more.

Citation Information

Patent Citations

  • Hollow silica particle and its manufacturing method

    JP2009203115A

  • Hollow particle and filler material for heat insulation coating

    JP2017031235A

  • Hollow particle and manufacturing method therefor

    JP2017109898A

  • Hollow particles

    JP2019172474A

  • Composition for optical films, base having optical film, molded body and method for producing molded body

    WO2017022175A1

Cited By

  • Hollow particle, resin composition, and circuit board

    WO2026203929A1