Welding wire, gas-shielded arc welding method, and method for producing weld metal

The use of a welding wire with controlled Mn, Ti, and Al content, combined with a specific gas-shielded arc welding method, addresses the issue of lumpy slag and enhances electrodeposition coating properties, ensuring corrosion resistance in corrosive environments.

WO2024202654A1PCT designated stage expired Publication Date: 2024-10-03KOBE STEEL LTD

Patent Information

Application Number
PCT/JP2024/005291
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional gas-shielded arc welding methods often result in lumpy slag formation on weld beads, which can lead to poor electrodeposition coating and increased corrosion risk due to peeling of the coating film under impact, especially in corrosive environments like those encountered by automobile suspension parts.

Method used

A welding wire composition with specific ranges of Mn, Ti, and Al, along with a gas-shielded arc welding method that includes a shielding gas and a feed control method to suppress lumpy slag formation, ensuring excellent electrodeposition coating properties and bead appearance.

Benefits of technology

The solution effectively prevents lumpy slag formation and ensures a weld bead with excellent electrodeposition coating properties, maintaining the coating integrity even under impact, thereby reducing corrosion risks in corrosive environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024005291_03102024_PF_FP_ABST
    Figure JP2024005291_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a welding wire for gas-shielded arc welding that enables a welding bead with excellent electrodeposition properties to be obtained, that suppresses the production of clumped slag on the welding bead, and that enables an excellent bead appearance to be obtained. This welding wire for use in arc welding contains, in relation to the total mass of the welding wire, more than 1.80% by mass and less than 2.20% by mass of manganese, at least 0.05% by mass and no more than 0.23% by mass of titanium, and more than 0.10% by mass and no more than 0.25% by mass of aluminum. Silicon is no more than 0.45% by mass. If the aluminum and titanium content of the welding wire, in relation to the total mass of the welding wire in mass%, is represented as [Al] and [Ti], respectively, the value M1, calculated by Formula 1: [Al] + [Ti], is no more than 0.45, and the value M2, calculated by Formula 2: [Ti] / [Al], is at least 0.30 and no more than 2.50.
Need to check novelty before this filing date? Find Prior Art

Description

Welding wire, gas-shielded arc welding method, and method for producing weld metal

[0001] The present invention relates to a welding wire used in gas-shielded arc welding, a gas-shielded arc welding method using the welding wire, and a method for producing a weld metal using the gas-shielded arc welding method.

[0002] Automotive undercarriage parts are exposed to corrosive environments due to moisture from the road surface and salt damage from snow-melting agents, and therefore technologies to prevent corrosion are needed. A common method for protecting undercarriage parts from corrosive environments is to apply electrodeposition coating after arc welding. However, when electrodeposition coating is performed after welding, the electrodeposition coating film does not form on the welding slag (hereinafter simply referred to as "slag"), resulting in paint defects, which can lead to corrosion progression from these defects. While methods for suppressing paint defects, such as by thickening the electrodeposition coating film, can sometimes result in the coating film peeling off along with the slag due to impacts such as pebbles hitting the vehicle while driving, resulting in corrosion progression from the peeled areas. Thus, parts manufactured by conventional methods are susceptible to corrosion due to poor coating on the welding slag, or even if a coating film is formed, corrosion can occur due to slag peeling off during driving.

[0003] In response to the above-described problems, for example, Patent Document 1 proposes a gas-shielded arc welding wire that generates less spatter during welding, does not require a step such as slag removal after welding, has excellent electrodeposition paintability, and can obtain a weld with a good bead shape. The welding wire contains, per total mass of the wire, C: 0.01 mass% or more and 0.10 mass% or less, Si: 0.05 mass% or more and 0.55 mass% or less, Mn: 1.60 mass% or more and 2.40 mass% or less, Ti: 0.05 mass% or more and 0.25 mass% or less, Cu: 0.01 mass% or more and 0.30 mass% or less, S: 0.001 mass% or more and 0.020 mass% or less, N: 0.0045 mass% or more and 0.0150 mass% or less, O: 0.0010 mass% or more and 0.0050 mass% or less, Al: 0.10 mass% or less, P: 0.025 mass% or less, and the balance being Fe and unavoidable impurities, and the relationship is 0.1≦[Ti] / [Si]≦3.0. Patent Document 1 describes that when the above-mentioned gas-shielded arc welding wire is used, a thin slag can be uniformly formed in the weld, and excellent electrodeposition paintability can be obtained without the need to remove the slag after welding.

[0004] Patent Document 2 proposes a gas-shielded arc welding solid wire capable of forming a welded joint with excellent electrodeposition coatability and mechanical properties, and a method for manufacturing a welded joint. The solid wire contains, in mass % relative to the total mass of the wire, 0.05 to 0.20% C, 0.01 to 0.18% Si, 1.0 to 3.0% Mn, 0.06 to 0.25% Ti, 0.003 to 0.10% Al, 0 to 0.0100% B, more than 0 to 0.015% P, more than 0 to 0.015% S, and optional elements, with the balance consisting of iron and impurities, satisfying Si × Mn ≦ 0.30 and (Si + Mn / 5) / (Ti + Al) ≦ 3.0, and further having a Ceq of 0.40 to 0.90%. Patent Document 2 describes that use of the gas-shielded arc welding solid wire makes it possible to form a welded joint with excellent electrodeposition coatability and mechanical properties.

[0005] As described above, in the welding wires described in Patent Documents 1 and 2, the Si content is reduced to suppress the formation of Si- and Mn-based slag, which has extremely low electrical conductivity, making it possible to form an excellent electrodeposition coating film even when slag is generated on the weld bead.

[0006] Japanese Patent Publication No. 2021-74777 Japanese Patent Publication No. 2021-3732

[0007] However, the slag may aggregate depending on the elements added to the welding wire, and this aggregation may result in the formation of thick, lumpy slag. When this lumpy slag is formed, even if an electrodeposition coating film is formed on the slag, the slag may peel off or be crushed due to impacts that occur during travel, as described above, resulting in the peeling of the electrodeposition coating film.

[0008] Although Patent Document 1 describes the ability to form uniformly thin slag, even when using the above welding wire, it is difficult to form thin slag on all parts of the weld bead. For example, depending on the content of deoxidizing elements such as Ti, Si, and Mn contained in the welding wire, slag may aggregate in the molten pool or on the surface of the molten pool, resulting in the formation of lumpy slag. Patent Document 2 also fails to address the issue of lumpy slag. Since deoxidizing elements such as Ti, Si, and Mn are added to the welding wire, a significant amount of lumpy slag is likely to be formed. Therefore, the weld bead must have good electrodeposition coatability and an excellent bead appearance that prevents the formation of lumpy slag on the surface.

[0009] The present invention has been made in view of the above problems, and has an object to provide a welding wire for gas-shielded arc welding that can obtain a weld bead having excellent electrodeposition coatability, suppress the generation of lumpy slag on the weld bead, and obtain an excellent bead appearance, a gas-shielded arc welding method using the welding wire, and a method for producing a weld metal using the gas-shielded arc welding method.

[0010] The above object of the present invention is achieved by the following configuration [1] relating to a welding wire.

[0011] [1] A welding wire used for gas-shielded arc welding, containing, relative to the total mass of the welding wire: Mn: more than 1.80 mass% and less than 2.20 mass%, Ti: 0.05 mass% or more and 0.23 mass% or less, Al: more than 0.10 mass% and 0.25 mass% or less, and Si: 0.45 mass% or less, wherein, when the content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, and the content of Ti contained in the welding wire is expressed as [Ti] in mass% relative to the total mass of the welding wire, the value M1 calculated by the following (Equation 1) is 0.45 or less, and the value M2 calculated by the following (Equation 2) is 0.30 or more and 2.50 or less. M1 = [Al] + [Ti] (Equation 1) M2 = [Ti] / [Al] (Equation 2)

[0012] Furthermore, preferred embodiments of the present invention relating to the welding wire relate to the following [2] to [5].

[0013] [2] The welding wire according to [1], further comprising at least one selected from the group consisting of C: 0.30 mass% or less, Ni: 1.00 mass% or less, Cr: 1.00 mass% or less, Mo: 1.00 mass% or less, Cu: 1.00 mass% or less, Mg: 0.10 mass% or less, Zr: 0.10 mass% or less, Nb: 0.10 mass% or less, V: 0.10 mass% or less, B: 0.0050 mass% or less, Sn: 0.01 mass% or less, Sb: less than 0.01 mass%, P: 0.050 mass% or less, and S: 0.050 mass% or less, relative to the total mass of the welding wire, with the balance being Fe and inevitable impurities.

[0014] [3] A welding wire including a flux, comprising an alloy component and a compound included in the flux, wherein the alloy component contains, relative to a total mass of the welding wire, at least one selected from C: 0.30 mass% or less, Ni: 1.00 mass% or less, Cr: 1.00 mass% or less, Mo: 1.00 mass% or less, Cu: 1.00 mass% or less, Mg: 0.10 mass% or less, Zr: 0.10 mass% or less, Nb: 0.10 mass% or less, V: 0.10 mass% or less, B: 0.0050 mass% or less, Sn: 0.01 mass% or less, Sb: less than 0.01 mass%, P: 0.050 mass% or less, and S: 0.050 mass% or less, with the balance being Fe and inevitable impurities, The welding wire according to [1], characterized in that the compound is contained in an amount of more than 0 mass % and 5 mass % or less with respect to the total mass of the welding wire.

[0015] [4] The welding wire according to any one of [1] to [3], wherein the value M3 calculated by the following formula (3) is less than 0.25, where [Si] represents the content of Si contained in the welding wire in mass % relative to the total mass of the welding wire, and [Mn] represents the content of Mn contained in the welding wire in mass % relative to the total mass of the welding wire: M3 = [Si] / [Mn] (formula 3)

[0016] [5] The welding wire according to any one of [1] to [4], wherein the content of Mn contained in the welding wire is expressed as [Mn] in mass % relative to the total mass of the welding wire, and the value M4 calculated by the following (Equation 4) is 0.70 or more and 0.95 or less: M4 = [Mn] / ([Mn] + [Al] + [Ti]) (Equation 4)

[0017] The above object of the present invention is achieved by the gas-shielded arc welding method according to the following item [6].

[0018] [6] A gas-shielded arc welding method in which welding is performed while supplying a shielding gas using a welding wire, wherein the welding wire contains, relative to a total mass of the welding wire: Mn: more than 1.80 mass% and less than 2.20 mass%, Ti: 0.05 mass% or more and 0.23 mass% or less, Al: more than 0.10 mass% and 0.25 mass% or less, and Si: 0.45 mass% or less, wherein the content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, and the content of Ti contained in the welding wire is expressed as [Ti] in mass% relative to the total mass of the welding wire, a value M1 calculated by the following (Equation 1) is 0.45 or less, and a value M2 calculated by the following (Equation 2) is 0.30 or more and 2.50 or less. M1=[Al]+[Ti]...(Formula 1) M2=[Ti] / [Al]...(Formula 2)

[0019] Furthermore, preferred embodiments of the present invention relating to a gas-shielded arc welding method relate to the following [7] to [9].

[0020] [7] The shielding gas is Ar and CO 2 The gas-shielded arc welding method according to [6], characterized in that the gas contains at least one gas selected from the group consisting of:

[0021] [8] The gas-shielded arc welding method according to [6], characterized in that welding is performed using a feed control method in which the feeding of the welding wire is alternately switched between a forward feed period and a reverse feed period.

[0022] [9] The gas shielded arc welding method according to [8], characterized in that in the feed control method, a frequency when the forward feed period and the reverse feed period are defined as one cycle is set to a predetermined range, and the welding current supplied to the welding wire is switched between a current suppression period and a current non-suppression period based on information on at least one of a phase representing the feed speed of the welding wire and a phase representing a tip position of the welding wire.

[0023] The above object of the present invention relates to the following

[10] , which relates to a method for producing a weld metal.

[0024]

[10] A method for producing a weld metal, in which welding is performed using a welding wire while supplying a shielding gas to produce a weld metal, wherein the shielding gas is Ar and CO 2 and wherein the welding wire contains, relative to a total mass of the welding wire, Mn: more than 1.80 mass% and less than 2.20 mass%, Ti: 0.05 mass% or more and 0.23 mass% or less, Al: more than 0.10 mass% and 0.25 mass% or less, and Si: 0.45 mass% or less, wherein, when the content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, and the content of Ti contained in the welding wire is expressed as [Ti] in mass% relative to the total mass of the welding wire, a value M1 calculated by the following (Equation 1) is 0.45 or less, and a value M2 calculated by the following (Equation 2) is 0.30 or more and 2.50 or less. M1 = [Al] + [Ti] (Equation 1) M2 = [Ti] / [Al] (Equation 2)

[0025] According to the present invention, it is possible to provide a welding wire for gas-shielded arc welding that can obtain a weld bead having excellent electrodeposition coatability, can suppress the generation of lumpy slag on the weld bead, and can obtain an excellent bead appearance, a gas-shielded arc welding method using the welding wire, and a method for producing a weld metal using the gas-shielded arc welding method.

[0026] FIG. 1 is a waveform diagram illustrating the time change of the wire feed speed Fw, where the vertical axis represents the wire feed speed Fw and the horizontal axis represents time (phase). FIG. 2 is a waveform diagram illustrating the time change of the welding wire tip position (hereinafter also referred to as "wire tip position"), where the vertical axis represents time (phase). FIG. 3 is a diagram illustrating an example of control of the current setting signal, where the vertical axis represents the current detection signal Io and the horizontal axis represents time. FIG. 4 is a schematic diagram showing the welding posture during gas-shielded arc welding used in this example. FIG. 5 is a drawing-substitute photograph of the bead appearance after welding, after electrocoating, and after impact application for Invention Examples Nos. 1 to 4. FIG. 6 is a drawing-substitute photograph of the bead appearance after welding, after electrocoating, and after impact application for Invention Examples Nos. 5 to 8. FIG. 7 is a drawing-substitute photograph of the bead appearance after welding, after electrocoating, and after impact application for Comparative Example Nos. 1 to 8. Fig. 8 is a photograph, substitute for a drawing, of the bead appearance after welding, after electrodeposition coating, and after impact for Comparative Examples Nos. 5 to 7.

[0027] The inventors conducted extensive research to solve the above-mentioned problems and discovered the following: By specifying the combination of deoxidizing elements contained in the welding wire and their contents, it is possible to control the composition of oxides formed in or on the surface of the molten pool and further suppress the formation of non-conductive vitreous oxides. As a result, a weld bead with excellent electrodeposition paintability can be obtained. Furthermore, by dispersing the oxides, the formation of lumpy slag can be suppressed, and a weld metal with excellent bead appearance can be obtained.

[0028] Specifically, by limiting the Si content of the welding wire to 0.45 mass% or less with respect to the total mass of the wire, it is possible to suppress the generation of non-conductive vitreous oxides and ensure electrodeposition coatability. Also, by specifying the Mn, Ti, and Al contents in the welding wire such that Mn is more than 1.80 mass% and less than 2.20 mass%, Ti is 0.05 mass% or more and 0.23 mass% or less, and Al is more than 0.10 mass% and 0.25 mass% or less with respect to the total mass of the wire, and specifying the total amounts and ratios of Ti and Al, it is possible to generate oxides that are easily dispersed and suppress the formation of lumpy slag on the surface of the weld bead.

[0029] It is believed that lumpy slag is mainly generated by the aggregation of oxides in or on the molten pool. Generally, the poorer the wettability between the oxide and the molten metal, the more likely the oxide will aggregate and float to the surface of the molten pool. In other words, the poorer the wettability between the oxide and the molten metal, the more likely lumpy slag will form on the weld bead. For example, Al, an oxide of Al, 2 O 3 Generally, the inclusion of Al in welding wire is avoided due to poor wettability with molten steel. However, the present inventors discovered that by intentionally adding an appropriate amount of Al to the welding wire and also adding Mn and Ti, slag on the bead surface can be dispersed. This is presumably because the wettability between the molten metal and the complex oxides formed in or on the molten pool surface is good due to the elements contained in the wire.

[0030] [Welding Wire] Below, embodiments for carrying out the present invention will be described in detail in line with the above mechanism. The present invention is not limited to the embodiments described below, and can be modified as desired without departing from the spirit and scope of the present invention. Below, the reasons for adding and limiting the numerical values ​​of the alloying elements contained in the welding wire according to this embodiment will be described in detail. In the following description, the content of each element in the welding wire is defined as the content of the element contained as an alloying element relative to the total mass of the welding wire. As described above, in the present invention, in order to obtain a bead with excellent electrodeposition coatability, suppress the generation of lumpy slag on the bead surface, and have excellent bead appearance, it is necessary to define at least Si, Mn, Ti, and Al within the following ranges. However, other alloying elements may be added as desired depending on the base material used and the application. That is, elements other than Si, Mn, Ti, and Al do not need to be contained in the wire, and may be 0 mass %.

[0031] The welding wire may be a solid wire composed of alloying elements, or a flux-cored wire in which the flux is made only of metal powder (hereinafter also referred to as a metal-based flux-cored wire). Furthermore, the welding wire may be a flux-cored wire in which the flux contains even a small amount of compounds (mainly oxides, fluorides, etc.) (hereinafter also referred to as a slag-based flux-cored wire). In the metal-based flux-cored wire or slag-based flux-cored wire, the alloying elements described below may be contained in either the hoop or the flux.

[0032] (Si: 0.45 mass % or less (including 0 mass %)) Si is a deoxidizer, and when Si is contained in the welding wire, the effect of improving the mechanical performance of the weld metal can be obtained. The Si content can be adjusted appropriately depending on the required strength, but in this embodiment, as long as the strength can be ensured by other elements, the welding wire does not need to contain Si, and the Si content may be 0 mass %.

[0033] On the other hand, the oxide of Si, SiO 2Si is a non-conductive glassy oxide, and if it remains as slag on the weld bead, it becomes impossible to form an electrodeposition coating film. Therefore, from the viewpoint of electrodeposition coating properties, the Si content needs to be suppressed to 0.45 mass% or less with respect to the total mass of the welding wire. The lower the Si content, the better, and it is preferably 0.30 mass% or less, and more preferably 0.20 mass% or less.

[0034] (Mn: More than 1.80% by mass, Less than 2.20% by mass) Like Si, Mn is a deoxidizer. The inclusion of Mn in welding wire can enhance the mechanical properties of the weld metal. Furthermore, by combining Mn with Ti and Al, which will be described later, Mn can disperse slag formed on the bead. Furthermore, because MnO has relatively high electrical conductivity, the higher the Mn content in the welding wire, the better the electrodeposition paintability. If the Mn content in the welding wire is 1.80% by mass or less, the above-described effect cannot be achieved. Therefore, the Mn content in the welding wire is preferably more than 1.80% by mass and more preferably more than 1.90% by mass, based on the total mass of the welding wire. On the other hand, if the Mn content in the wire is 2.20% by mass or more, excessive deoxidation occurs, reducing the amount of oxygen in the molten pool. This increases the surface tension of the droplets, thereby impairing the bead shape. Therefore, the Mn content in the welding wire is preferably less than 2.20% by mass, based on the total mass of the wire, based on the total mass of the wire.

[0035] (Ti: 0.05% by mass or more, 0.23% by mass or less) Ti is a strong deoxidizing element that preferentially forms oxides through its deoxidizing action. Therefore, like Mn and Al, Ti is an element that significantly contributes to the composition of slag. As described above, by combining Ti with Mn and Al in the welding wire, the effect of dispersing slag generated on the bead can be obtained. If the Ti content in the welding wire is less than 0.05% by mass, the above effect cannot be obtained. Therefore, the Ti content in the welding wire is preferably 0.05% by mass or more, and more preferably 0.08% by mass or more, relative to the total mass of the welding wire. On the other hand, if Ti is excessively contained in the welding wire in an amount exceeding 0.23% by mass, the composition of the slag changes, and the desired slag dispersion effect cannot be obtained. Therefore, the Ti content in the welding wire is preferably 0.23% by mass or less, and more preferably 0.21% by mass or less, relative to the total mass of the wire.

[0036] (Al: More than 0.10 mass% and 0.25 mass% or less) Like Ti, Al is a strong deoxidizing element and preferentially forms oxides through its deoxidizing action. Therefore, like Mn and Ti, Al is an element that significantly contributes to the composition of slag. As described above, by combining Al with Mn and Ti in the welding wire, the effect of dispersing slag generated on the bead can be obtained. If the Al content in the welding wire is 0.10 mass% or less, the above effect cannot be obtained. Therefore, the Al content in the welding wire is preferably more than 0.10 mass% and 0.12 mass% or more, relative to the total mass of the welding wire. On the other hand, if Al is excessively contained in the welding wire at a content exceeding 0.25 mass%, the composition of the slag changes, and the desired slag dispersion effect cannot be obtained. Therefore, the Al content in the welding wire is preferably 0.25 mass% or less and 0.22 mass% or less, relative to the total mass of the wire.

[0037] (M1: 0.45 or less, M2: 0.30 to 2.50) As described above, in this embodiment, by specifying the total amount and ratio of Ti and Al, oxides that are easily dispersed are generated and the formation of lumpy slag on the surface of the weld bead is suppressed. If the total amount of Al and Ti, i.e., the value M1 calculated by the following (Equation 1), exceeds 0.45, the amount of slag itself increases and the slag composition changes, making it difficult to achieve the slag dispersion effect. Therefore, M1 is set to 0.45 or less, preferably 0.40 or less, more preferably 0.39 or less, and even more preferably 0.35 or less.

[0038] In this embodiment, the lower limits of the Al content and the Ti content are specified, and even if these are at the lower limit, the slag dispersion effect can be sufficiently obtained, so the lower limit of M1 is not particularly limited. However, to obtain a more effective slag dispersion effect, M1 is preferably 0.24 or more, more preferably 0.25 or more, and even more preferably 0.27 or more.

[0039] In this embodiment, it is important to specify the total content of Al and Ti, as well as the ratio of the Ti and Al contents, i.e., the value M2 calculated by the following (Equation 2). If M2 is less than 0.30, the slag dispersion effect cannot be sufficiently obtained. Therefore, M2 is set to 0.30 or more, and preferably 0.40 or more.

[0040] On the other hand, if M2 exceeds 2.50, the slag dispersion effect cannot be sufficiently obtained. Therefore, M2 is set to 2.50 or less, preferably 1.80 or less, and more preferably 1.30 or less.

[0041] In this way, it is believed that an optimal slag composition can be obtained by controlling the total content of Al and Ti and the Al content and Ti content in the wire within the range of their ratio, and as a result, an excellent slag dispersion effect can be obtained.

[0042] M1=[Al]+[Ti] (Formula 1) M2=[Ti] / [Al] (Formula 2) Here, [Al] is a value representing the content of Al contained in the welding wire, expressed as mass % with respect to the total mass of the welding wire, and [Ti] is a value representing the content of Ti contained in the welding wire, expressed as mass % with respect to the total mass of the welding wire.

[0043] As described above, the welding wire according to this embodiment has specified contents of Si, Mn, Ti, and Al, and the M1 and M2 are appropriately controlled, thereby achieving electrodeposition coatability on the weld bead and suppressing the generation of lumpy slag. Therefore, the contents of the following elements other than the above elements can be adjusted appropriately depending on the base material and the required properties, and may be 0 mass %. Below, the preferred content ranges of optional elements in the welding wire according to this embodiment and the reasons for limiting them will be described in detail. Note that when the welding wire according to this embodiment contains elements other than the above Si, Mn, Ti, and Al, it is sufficient that at least one of the following elements is contained within the ranges shown below, and the element to be contained can be selected depending on the required properties, etc.

[0044] (C: 0.30% by mass or less (including 0% by mass)) C has a deoxidizing effect, and when C is contained in the welding wire, the effect of improving the mechanical performance of the weld metal can be obtained. The C content can be adjusted appropriately depending on the required strength. In this embodiment, however, if strength can be ensured with other elements, the welding wire does not need to contain C, and C may be 0% by mass. However, if C is contained in the welding wire in an excessive amount, the deoxidizing effect becomes strong, and CO is generated near the arc, which may cause an explosion, resulting in the generation of spatter and an increase in the amount of fumes. Therefore, from the viewpoint of welding workability, the C content in the welding wire is preferably 0.30% by mass or less, more preferably 0.10% by mass or less, and even more preferably 0.08% by mass or less, relative to the total mass of the welding wire.

[0045] (Ni: 1.00 mass% or less (including 0 mass%)) When the welding wire contains Ni, the effect of improving the mechanical performance of the weld metal can be obtained. The Ni content can be adjusted appropriately depending on the required strength. In this embodiment, however, as long as strength can be ensured by other elements, the welding wire does not need to contain Ni, and the Ni content can be 0 mass%. Note that, when the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa class steel plates used in automobile suspension parts, the Ni content is preferably 1.00 mass% or less with respect to the total mass of the welding wire. By suppressing the Ni content as described above, a balance is achieved with other elements that improve mechanical performance, and excessive strength of the weld metal can be suppressed.

[0046] (Cr: 1.00 mass% or less (including 0 mass%)) When Cr is contained in the welding wire, the effect of improving the mechanical performance of the weld metal can be obtained. The Cr content can be adjusted appropriately depending on the required strength. In this embodiment, however, as long as strength can be ensured by other elements, the welding wire does not need to contain Cr, and 0 mass% of Cr may be contained. Note that, when the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa class steel plates used in automobile suspension parts, the Cr content is preferably 1.00 mass% or less with respect to the total mass of the welding wire. By suppressing the Cr content as described above, a balance is achieved with other elements that improve mechanical performance, and excessive strength of the weld metal can be suppressed.

[0047] (Mo: 1.00 mass% or less (including 0 mass%)) When Mo is contained in the welding wire, the effect of improving the mechanical performance of the weld metal can be obtained. The Mo content can be adjusted appropriately depending on the required strength. In this embodiment, however, if strength can be ensured by other elements, Mo does not need to be contained in the welding wire, and the Mo content may be 0 mass%. Note that, when the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa class steel plates used in automobile suspension parts, the Mo content is preferably 1.00 mass% or less with respect to the total mass of the welding wire. By suppressing the Mo content as described above, a balance is achieved with other elements that improve mechanical performance, and excessive strength of the weld metal can be suppressed.

[0048] (Cu: 1.00 mass% or less (including 0 mass%)) When the welding wire contains Cu, the effect of improving the mechanical performance of the weld metal can be obtained. The Cu content can be adjusted appropriately depending on the required strength. In this embodiment, however, as long as strength can be ensured by other elements, the welding wire does not need to contain Cu, and the Cu content can be 0 mass%. Here, the Cu content in this specification also includes Cu in a plating that may be formed on the surface of the welding wire. Note that, when the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa class steel sheets used in automobile suspension parts, the Cu content in the welding wire including the plating is preferably 1.00 mass% or less with respect to the total mass of the welding wire. By suppressing the Cu content as described above, a balance with other elements that improve mechanical performance can be achieved, and excessive strength of the weld metal can be suppressed.

[0049] (Mg: 0.10% by mass or less (including 0% by mass)) (Zr: 0.10% by mass or less (including 0% by mass)) Like Al and Ti, Mg and Zr are strong deoxidizing elements, and preferentially form oxides through their deoxidizing action. The higher the Mg and Zr contents in the welding wire, the more the slag composition changes, and there is a possibility that the slag dispersion effect cannot be obtained. Therefore, in order to obtain the deoxidizing effect by including Mg and Zr in the welding wire without reducing the slag dispersion effect, it is preferable that the Mg content and the Zr content are each 0.10% by mass or less with respect to the total mass of the welding wire.

[0050] (Nb: 0.10 mass% or less (including 0 mass%)) (V: 0.10 mass% or less (including 0 mass%)) When the welding wire contains Nb or V, it is possible to obtain the effect of improving the mechanical performance of the weld metal. The contents of Nb and V can be adjusted appropriately depending on the required strength. In this embodiment, however, as long as strength can be ensured with other elements, the welding wire does not need to contain Nb or V, and may contain 0 mass% Nb or V. When the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa class steel plates used in automobile suspension parts, it is preferable that the Nb content and V content in the welding wire are each 0.10 mass% or less with respect to the total mass of the welding wire. By suppressing the Nb content and V content as described above, a balance is achieved with other elements that improve mechanical performance, and excessive strength of the weld metal can be suppressed.

[0051] (B: 0.0050 mass% or less (including 0 mass%)) When the welding wire contains B, it is possible to obtain the effect of improving the mechanical properties of the weld metal. The B content can be adjusted appropriately depending on the required strength. In this embodiment, however, if strength can be ensured by other elements, the welding wire does not need to contain B, and B may be 0 mass%. Note that, when the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa class steel plates used in automobile suspension parts, the B content is preferably 0.0050 mass% or less with respect to the total mass of the welding wire. By suppressing the B content as described above, a balance is achieved with other elements that improve mechanical properties, and excessive strength of the weld metal can be suppressed.

[0052] (Sn: 0.01% by mass or less (including 0% by mass)) Sn is a low-melting-point element, and if the Sn content in the welding wire exceeds a predetermined range, hot cracking is likely to occur. Therefore, the Sn content in the welding wire is preferably at the impurity level, and may be 0% by mass. Note that, when the welding wire contains Sn, the Sn content in the welding wire is preferably suppressed to less than 0.01% by mass with respect to the total mass of the welding wire.

[0053] (Sb: Less than 0.01% by mass (including 0% by mass)) Sb is an element that affects the physical properties of molten metal, and Sb in the welding wire affects the behavior of the molten pool. Specifically, the boiling point of Sb is 1587°C, and it easily vaporizes in the molten pool, which can cause porosity defects (pits and blowholes) and disrupt convection on the molten pool surface due to the release of pores. Therefore, if the welding wire contains Sb at a content equal to or greater than a predetermined range, slag particles may collide with each other, which may promote slag aggregation. Therefore, the Sb content in the welding wire is preferably at the impurity level and may be 0% by mass. Note that when the welding wire contains Sb, the Sb content in the welding wire is preferably limited to less than 0.01% by mass with respect to the total mass of the welding wire.

[0054] (P: 0.050% by mass or less (including 0% by mass)) P is an element that affects the cracking tendency of the weld metal, and the lower the P content in the welding wire, the better the cracking resistance of the weld metal. Therefore, the welding wire according to this embodiment may not contain P, or may contain 0% by mass. Note that, when the welding wire contains P, from the viewpoint of cracking resistance, the P content in the welding wire is preferably 0.050% by mass or less with respect to the total mass of the welding wire.

[0055] (S: 0.050% by mass or less (including 0% by mass)) S is an element that reduces the surface tension of molten metal, and when S is contained in a welding wire, the effect of forming a flat weld bead can be obtained. The effect of forming a flat weld bead can be obtained by substituting other surface active elements (oxygen, selenium, tellurium, etc.), so there is no particular lower limit for the S content, and it may be 0% by mass. However, when a flat weld bead is formed by containing S in the welding wire, the S content in the welding wire is preferably 0.001% by mass or more with respect to the total mass of the welding wire. On the other hand, the higher the S content in the welding wire, the more likely sulfides are generated, which changes the slag composition, and there is a possibility that the desired slag dispersion effect cannot be obtained. Therefore, the S content in the welding wire is preferably 0.050% by mass or less with respect to the total mass of the welding wire.

[0056] (Remainder of alloying elements: Fe and inevitable impurities) In this embodiment, the remainder of the alloying elements of the wire preferably used is Fe and inevitable impurities. Examples of inevitable impurities include O, N, Li, Bi, and As. The content of each of these inevitable impurities is preferably 0.0100 mass% or less, and more preferably 0.0050 mass% or less, relative to the total mass of the wire. Furthermore, the total content of these inevitable impurities is preferably 0.0200 mass% or less, relative to the total mass of the wire.

[0057] The welding wire according to the present embodiment may be a flux-containing welding wire containing alloy components and compounds contained in the flux. In this way, in the case of a slag-based flux-cored wire containing compounds in the flux, in addition to the above-mentioned alloy components, the flux may further contain compounds in an amount of more than 0 mass % and not more than 5 mass % relative to the total mass of the wire, more preferably not more than 3 mass %, and even more preferably not more than 1 mass %. Examples of compounds include oxides, sulfides, carbides, nitrides, fluorides, etc., and for example, B 2 O 3 , Na 2 O.K. 2 Even if the welding wire is a slag-based flux-cored wire, the preferred range of the content of each alloy component is as described above.

[0058] In this embodiment, by specifying the ratio of the Si content to the Mn content in the welding wire, it is possible to adjust the mechanical properties of the weld metal and obtain a more excellent slag dispersion effect. Furthermore, by specifying the values ​​calculated by a specific formula using the contents of Mn, Al, and Ti, an even more excellent slag dispersion effect can be obtained. The limited ranges for these values ​​and the reasons therefor will be explained below.

[0059] (M3: Less than 0.25) Because Si is an element that reduces electrodeposition coatability, it is preferable to reduce the Si content in the welding wire as much as possible. However, because Si is also an element that has the effect of improving the mechanical properties of the weld metal, reducing the Si content requires supplementing the mechanical properties of the weld metal with another element. In this embodiment, as described above, the relationship between the Al content and the Ti content is adjusted to control the slag composition and achieve an excellent slag dispersion effect. Therefore, a preferred method for adjusting the mechanical properties is to increase the Mn content and minimize the addition of other elements. Setting the ratio of the Si content to the Mn content, i.e., the value M3 calculated by the following (Equation 3), to less than 0.25 can further improve the mechanical properties of the weld metal and the slag dispersion effect. Therefore, it is preferable to adjust the Mn content and Si content so that M3 is less than 0.25, more preferably so that M3 is 0.20 or less, and even more preferably so that M3 is 0.15 or less.

[0060] M3=[Si] / [Mn] (Equation 3) Here, [Si] is a value representing the amount of Si contained in the welding wire, expressed as mass % with respect to the total mass of the welding wire, and [Mn] is a value representing the amount of Mn contained in the welding wire, expressed as mass % with respect to the total mass of the welding wire.

[0061] (M4: 0.70 or more and 0.95 or less) In this embodiment, by appropriately defining the ratio of the Mn content to the total value of the contents of Mn, Al, and Ti in the welding wire, i.e., the value M4 calculated by the following (Equation 4), a slag composition that can obtain an even better slag dispersion effect is obtained. Therefore, M4 is preferably 0.70 or more, and more preferably 0.80 or more. Moreover, M4 is preferably 0.95 or less, and more preferably 0.90 or less.

[0062] M4=[Mn] / ([Mn]+[Al]+[Ti]) (Formula 4) Here, [Mn] is a value representing the amount of Mn contained in the welding wire, expressed as mass %, with respect to the total mass of the welding wire; [Al] is a value representing the amount of Al contained in the welding wire, expressed as mass %, with respect to the total mass of the welding wire; and [Ti] is a value representing the amount of Ti contained in the welding wire, expressed as mass %, with respect to the total mass of the welding wire.

[0063] (Wire Diameter) In the welding wire according to the present embodiment, the wire diameter (diameter) is not particularly limited, but a wire having a diameter specified in a welding material standard such as AWS or JIS can be used.

[0064] (Wire Manufacturing) The welding wire according to this embodiment is not particularly limited in its manufacturing method, and no special manufacturing conditions are required, and it can be manufactured by a conventional method. For example, in the case of a solid wire, steel containing the above-mentioned alloy elements in specified contents is melted to obtain an ingot. Next, the ingot is subjected to hot forging or the like as needed, followed by hot rolling and cold wire drawing to form a wire. Thereafter, the obtained wire is annealed at a temperature of about 500 to 900°C as needed, pickled, copper plated as needed, and further subjected to finish wire drawing as needed to obtain a target wire diameter. Thereafter, a lubricant is applied as needed, and the welding wire can be manufactured.

[0065] Next, the gas-shielded arc welding method according to this embodiment will be described below.

[0066] [Gas-shielded arc welding method] The gas-shielded arc welding method according to this embodiment is a method of performing welding while supplying a shielding gas using the welding wire according to the above-described embodiment. The contents of Si, Mn, Ti, and Al in the welding wire and the values ​​of M1 and M2 calculated based on the Ti content and Al content are as described above. Furthermore, the preferred ranges of the other alloying elements are also as described above.

[0067] (Shielding Gas) In the gas-shielded arc welding method according to this embodiment, the shielding gas to be used is not particularly limited, but in view of the control characteristics that are preferred for use in this embodiment, it is preferable that the gas composition has a globule transition form. Specifically, it is preferable that at least one gas among carbon dioxide gas, nitrogen gas, hydrogen gas, and oxygen gas, which have a high potential gradient, is included. In addition, from the viewpoint of versatility, Ar and CO 2 It is preferable to use a shielding gas containing at least one gas selected from the group consisting of: For example, when using a mixed gas containing argon gas (hereinafter also referred to as "Ar gas"), it is more preferable to use a mixed gas containing at least 10% by volume of carbon dioxide gas; furthermore, it is preferable to use a mixed gas containing 90% by volume or more of carbon dioxide gas, and it is particularly preferable to use a shielding gas consisting of carbon dioxide gas alone.

[0068] By performing welding using the gas-shielded arc welding method according to the present embodiment, it is possible to form a weld bead that has excellent surface electrodeposition paintability and in which the generation of lumpy slag is suppressed.

[0069] In the gas-shielded arc welding method according to the present embodiment, other welding conditions for using the welding wire according to the present embodiment and the predetermined shielding gas are not particularly limited. For example, a pulsed MAG welding method or a feed control method may be used, but from the viewpoint of welding workability, it is preferable to use the feed control method. The feed control method will be described in detail below.

[0070] (Feed Control Method) The feed control method is a method of welding by alternately switching the feed of the welding wire between a forward feed period and a reverse feed period. The feed control method can be further classified into a "short-circuit feed control method" and a "short-circuit suppression feed control method." The short-circuit feed control method is a type of welding based on a short-circuit transition mode in which the welding wire feed rate is alternately switched between a forward feed period and a reverse feed period, thereby generating a short-circuit period and an arc period. The short-circuit suppression feed control method is a type of welding based on a globule transition mode in which the welding wire feed rate is alternately switched between a forward feed period and a reverse feed period, thereby suppressing the occurrence of a short-circuit period. In the gas-shielded arc welding method according to this embodiment, it is more preferable to use the short-circuit suppression feed control method, which can produce a weld bead with a better appearance and also improve welding workability. Furthermore, when a galvanized steel sheet is used as the base metal, the occurrence of porosity defects (pits or blowholes), which are problematic in welding of galvanized steel sheets, can be suppressed.

[0071] The short circuit suppression type feed control method that is preferably used in this embodiment will be described in further detail.

[0072] FIG. 1 is a waveform diagram illustrating the change in the wire feed speed Fw over time, with the vertical axis representing the wire feed speed Fw and the horizontal axis representing time (phase). The vertical axis is expressed in meters per minute or revolutions per minute. In FIG. 1, the period during which the speed is higher than the average feed speed Fave is referred to as the "normal feed period T P " and the period during which the speed is lower than the average feeding speed Fave is referred to as the "reverse feeding period T N ". The first half of each feeding period is called the "early period" and the second half is called the "late period." Here, the average feeding speed Fave can be regarded as the wire melting speed Fm.

[0073] 2 is a waveform diagram illustrating the change over time in the wire tip position, with the vertical axis representing the tip position of the welding wire (hereinafter also referred to as the "wire tip position") and the horizontal axis representing time (phase). In FIG. 2, the position (height) when the welding wire is fed at the maximum or minimum feed rate is used as the reference distance. In FIG. 2, the times when the tip position of the welding wire is closest to the base metal (hereinafter also referred to as the "lowest end") are represented by T0 and T4, and the time when the tip position of the welding wire is farthest from the base metal and closest to the power feed tip (hereinafter also referred to as the "upper end") is represented by T2.

[0074] As shown in FIG. 2, the period during which the tip position of the welding wire approaches the base metal with the passage of time, specifically, the period during which the tip position of the welding wire moves from the uppermost end to the lowermost end, is called the “normal feeding period T P ". The period during which the tip position of the welding wire approaches the power feed tip side with the passage of time, specifically, the period during which the tip position of the welding wire moves from the lowermost end to the uppermost end, is called the "reverse feeding period T N "

[0075] Furthermore, the time points corresponding to the reference distance are designated as T1 and T3. T1 is an intermediate point from the bottom end, where the tip of the welding wire is closest to the base metal, to the top end, where the tip is closest to the power feed tip. Meanwhile, T3 is an intermediate point from the top end to the bottom end. As shown in FIG. 2 , the change in the wave height from the top end to the bottom end is the "wave height Wh."

[0076] 3 is a diagram showing an example of control of the current setting signal, with the vertical axis representing the current detection signal Io and the horizontal axis representing time. Times T0, T1, T2, T3, and T4 in the diagram correspond to times T0, T1, T2, T3, and T4 in FIG. 2, respectively.

[0077] In this embodiment, the welding current supplied to the welding wire is controlled based on at least one of information on a phase representing the feed speed of the welding wire as shown in FIG. 1 (hereinafter also referred to as a "feed speed phase") and information on a phase representing the tip position of the welding wire as shown in FIG. 2 (hereinafter also referred to as a "wire position phase") during a current non-suppression period T IP and the current suppression period TIB For example, the welding current is controlled to be switched between the current suppression period T and the current suppression period T based on the wire position phase of 0 to 360 degrees (0 to 2π), where 0 degrees is the position when the wire tip is closest to the power feed tip side and 180 degrees is the position when the wire tip is closest to the base metal side. IB and the current non-suppression period T IP In addition, the current non-suppression period T IP The set current value Ip is also called the peak current, and the current suppression period T IB The set current value Ib is also called the base current. IP The time when the peak current starts is called the peak current start time, and the current non-suppression period T IP The time when the peak current ends can be expressed as the peak current end time.

[0078] As shown in FIG. 3 , the timing of the peak current end time is preferably determined by a set period d1 that starts when the wire position phase becomes 0 degrees, and the timing of the peak current start time is preferably determined by a set period d2 that starts when the peak current end time is started. This set period may be set by phase. For example, if d1 is set to 190° and d2 is set to 120°, the peak current ends when the wire position phase is 190° (d1) and starts when the wire position phase is 310° (d1 + d2). Note that the current suppression period T IB includes the falling period, and the current non-suppression period T IP includes the rise period.

[0079] In the above-described short-circuit suppression type feed control method, it is preferable to set the wire forward / reverse frequency, which is the frequency when the forward feed period and the reverse feed period are defined as one cycle, within a predetermined range. For example, it is preferable from the viewpoint of welding workability to set the wire forward / reverse frequency to a range of 50 Hz or more and 150 Hz or less, and the wire amplitude indicated by the wave height Wh to a range of 3.3 mm or more and 6.3 mm or less.

[0080] (Welding Position) In the gas-shielded arc welding method according to the present embodiment, the welding position is not particularly limited. However, the welding wire according to the present embodiment is preferably used for horizontal lap fillet welding, and the welding position is preferably a flat position or a horizontal position.

[0081] (Base Metal) In the gas-shielded arc welding method according to the present embodiment, the base metal is not particularly limited. The steel sheet may have any composition, and a galvanized steel sheet having a surface coated with zinc may be used.

[0082] [Method for producing weld metal] The method for producing weld metal according to this embodiment is a method for producing weld metal using the welding wire according to the embodiment described above. The method for producing weld metal according to this embodiment is also a method for producing weld metal using the gas-shielded arc welding method according to the embodiment described above. Specific examples of the method for producing weld metal according to this embodiment are as described in the embodiments relating to the welding wire and the gas-shielded arc welding method. The weld metal produced by the method for producing weld metal according to this embodiment has excellent electrodeposition coatability on the surface, is free from lumpy slag, and has an excellent appearance.

[0083] [Weld Metal] The weld metal obtained by the method for producing a weld metal according to this embodiment preferably contains predetermined components. The composition of the weld metal is affected by the component composition of the welding wire according to this embodiment and the component composition of the base metal. In this embodiment, the content of each element in the weld metal relative to the total mass of the weld metal is preferably within the following ranges.

[0084] That is, the weld metal contains Mn: more than 0.50 mass% and less than 2.00 mass%, Ti: 0.005 mass% or more and 0.10 mass% or less, and Al: more than 0.005 mass% and 0.15 mass% or less. Contains, Si: 0.45% by mass or less, C: 0.30% by mass or less, Ni: 1.00% by mass or less, Cr: 1.00% by mass or less, Mo: 1.00% by mass or less, Cu: 1.00% by mass or less. Preferably, the alloy contains at least one selected from Mg: 0.10% by mass or less, Zr: 0.10% by mass or less, Nb: 0.10% by mass or less, V: 0.10% by mass or less, B: 0.0050% by mass or less, Sn: 0.01% by mass or less, Sb: less than 0.01% by mass, P: 0.050% by mass or less, and S: 0.050% by mass or less, with the balance being Fe and inevitable impurities.

[0085] The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples and can be implemented with modifications within the scope of the present invention, all of which are included in the technical scope of the present invention. Furthermore, the welding conditions described here are merely examples, and the present embodiment is not limited to the following welding conditions.

[0086] Gas-shielded arc welding was performed using welding wires having various compositions. Fig. 4 is a schematic diagram showing the welding position during gas-shielded arc welding used in this example. As shown in Fig. 4, steel sheets 1 and 2 were positioned offset from each other, and welding was performed toward a fillet formed between the top surface of steel sheet 1 and the end surface of steel sheet 2 while controlling the feed rate of welding wire 4 with power feed tip 3 and flowing shielding gas. The compositions of the welding wires used are shown in Table 1 below, and the feed control conditions and other welding conditions are shown below.

[0087] <Feed control conditions> Wire frequency: 70 Hz Wave height: 5 mm (amplitude ±2.5 mm) Current control switching timing: Wire position phase 100 to 150 degrees when peak current ends Wire position phase 300 to 360 degrees when base current ends

[0088] <Other welding conditions> Steel plate 1, steel plate 2: 200 mm length x 50 mm width x 2.3 mm thickness, galvanized steel plate (SGAH440) Welding position: horizontal lap fillet welding Torch angle (angle between steel plate 1 and welding wire 4) θ: 60° Shielding gas: 100% by volume CO 2 Gas Average current: 200-250A Average voltage: 19-27V Wire feed: 7.0m / min Welding speed: 100cm / min Welding length: 150mm

[0089] <Evaluation Test> (Observation of Bead Appearance After Welding) A photograph of the surface of the obtained weld bead was taken, and the bead appearance was evaluated. In this example, the bead appearance was evaluated by taking a photograph of the surface of the weld bead within 20 mm 2 Slag with an area of ​​150 mm or more was judged to be lumpy slag, and if even one lump of slag was formed within a weld length of 150 mm, it was deemed to have failed and was marked C. 2 If no lumpy slag of an area of ​​2 mm or more is formed, it is considered to be a pass. 2 More than 20 mm 2 The case where a small slag with an area of ​​less than 2 mm was formed was designated as B. 2 A case in which only lumpy slag of less than 100000000 or no lumpy slag was formed was evaluated as a more favorable result and was designated as A.

[0090] (Bead appearance after electrodeposition coating) Next, the obtained joint was subjected to electrodeposition coating to form an electrodeposition coating film on the surface. In this example, the bead appearance was observed, and when an electrodeposition coating film was formed on the entire surface of the weld bead, it was judged as passing and marked as "Good." Furthermore, when there was a portion where an electrodeposition coating film was not formed, it was judged as failing and marked as "Bad."

[0091] (Bead appearance after impact application) For joints on which an electrodeposition coating film had been formed, multiple impacts were applied with a hammer to the back side of the weld bead, and the presence or absence of peeling of the electrodeposition coating film was observed. In this example, the presence or absence of peeling of slag was observed over the entire surface of the weld bead, and a case in which no peeling of slag (electrodeposition coating film) occurred was considered to be pass and indicated as Good. Furthermore, a case in which peeling of slag (electrodeposition coating film) occurred in even one location was considered to be fail and indicated as Bad.

[0092] (Observation of pits) The surface of the weld metal was visually observed for the presence or absence of pits. In this example, when no pits were observed over a weld length of 150 mm, this was recorded as "absent," and when pits were observed, this was recorded as "present."

[0093] 5 to 8 are photographs showing the bead appearance after welding, after electrodeposition coating, and after impact for each of the invention examples and comparative examples. The evaluation results obtained from these appearances are shown in Table 2 below.

[0094] The remainder other than the components shown in Table 1 below is Fe and inevitable impurities. In Table 1, in the column for the content of a component, "-" indicates that the content was below the detection limit. Furthermore, the M2 values ​​of Comparative Examples 4 and 5 and the M4 values ​​of Comparative Examples 6 and 7 were calculated assuming that the contents of Ti and Al were 0 mass%. The M2 values ​​of Comparative Examples 6 and 7 could not be calculated, so they were represented as "-". In Table 1 below, M1 to M4 are values ​​obtained from the following (Equation 1) to (Equation 4), respectively.

[0095] M1 = [Al] + [Ti] (Formula 1) M2 = [Ti] / [Al] (Formula 2) M3 = [Si] / [Mn] (Formula 3) M4 = [Mn] / ([Mn] + [Al] + [Ti]) (Formula 4) where, [Al] is the content of Al contained in the welding wire expressed as a mass % with respect to the total mass of the welding wire, [Ti] is the content of Ti contained in the welding wire expressed as a mass % with respect to the total mass of the welding wire, [Si] is the content of Si contained in the welding wire expressed as a mass % with respect to the total mass of the welding wire, and [Mn] is the content of Mn contained in the welding wire expressed as a mass % with respect to the total mass of the welding wire.

[0096]

[0097]

[0098] In the columns of the post-weld bead appearance in Figures 5 to 8, the black areas indicate the formation of lumpy slag, and in the columns of the post-impact bead appearance, the white areas indicate peeling of the electrodeposition coating.

[0099] 5 to 8 and Tables 1 and 2, in Invention Examples Nos. 1 to 8, the contents of Mn, Ti, Al, and Si in the welding wire, and the values ​​of M1 and M2, were within the ranges specified in the present invention, and therefore the electrodeposition coatability of the surface was excellent, no lumpy slag was formed, and a weld bead with excellent appearance could be obtained. Therefore, even when an impact was applied after electrodeposition coating, the slag did not peel off, and an excellent joint could be obtained.

[0100] On the other hand, in Comparative Examples 1 to 7, the contents of Mn, Ti, Al, and Si in the welding wire and at least one of the values ​​of M1 and M2 were outside the ranges specified in the present invention. Therefore, although the electrodeposition coatability of the surface was excellent, lumpy slag was formed, and when an impact was applied after electrodeposition coating, the electrodeposition coating film peeled off together with the slag.

[0101] Although various embodiments have been described above, it goes without saying that the present invention is not limited to such examples. It is clear that a person skilled in the art can conceive of various modifications or alterations within the scope of the claims, and it is understood that these also naturally fall within the technical scope of the present invention. Furthermore, the components of the above embodiments may be combined in any manner as long as they do not deviate from the spirit of the invention.

[0102] This application is based on a Japanese patent application (Patent Application No. 2023-059088) filed on March 31, 2023, the contents of which are incorporated herein by reference.

[0103] 1, 2 Steel plate 3 Power supply tip 4 Welding wire

Claims

1. A welding wire used for gas shielded arc welding, containing, relative to the total mass of the welding wire, Mn: more than 1.80 mass% and less than 2.20 mass%, Ti: 0.05 mass% or more and 0.23 mass% or less, Al: more than 0.10 mass% and 0.25 mass% or less, and Si: 0.45 mass% or less, wherein, when the content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, and the content of Ti contained in the welding wire is expressed as [Ti] in mass% relative to the total mass of the welding wire, the value M1 calculated by the following (formula 1) is 0.45 or less, and the value M2 calculated by the following (formula 2) is 0.30 or more and 2.50 or less. M1 = [Al] + [Ti] ... (formula 1) M2 = [Ti] / [Al] ... (formula 2) 2. The welding wire according to claim 1, further comprising at least one selected from the following, relative to the total mass of the welding wire: C: 0.30 mass% or less, Ni: 1.00 mass% or less, Cr: 1.00 mass% or less, Mo: 1.00 mass% or less, Cu: 1.00 mass% or less, Mg: 0.10 mass% or less, Zr: 0.10 mass% or less, Nb: 0.10 mass% or less, V: 0.10 mass% or less, B: 0.0050 mass% or less, Sn: 0.01 mass% or less, Sb: less than 0.01 mass%, P: 0.050 mass% or less, and S: 0.050 mass% or less, with the remainder being Fe and unavoidable impurities.

3. A welding wire containing flux, comprising an alloy component and a compound contained in the flux, the alloy component being at least one selected from the following, relative to the total mass of the welding wire: C: 0.30 mass% or less, Ni: 1.00 mass% or less, Cr: 1.00 mass% or less, Mo: 1.00 mass% or less, Cu: 1.00 mass% or less, Mg: 0.10 mass% or less, Zr: 0.10 mass% or less, Nb: 0.10 mass% or less, V: 0.10 mass% or less, B: 0.0050 mass% or less, Sn: 0.01 mass% or less, Sb: less than 0.01 mass%, P: 0.050 mass% or less, and S: 0.050 mass% or less, with the remainder being Fe and inevitable impurities; The welding wire according to claim 1 , wherein the compound is more than 0 mass % and 5 mass % or less with respect to a total mass of the welding wire.

4. The welding wire according to any one of claims 1 to 3, characterized in that, when the content of Si contained in the welding wire is expressed as [Si] in mass % relative to the total mass of the welding wire, and the content of Mn contained in the welding wire is expressed as [Mn] in mass % relative to the total mass of the welding wire, a value M3 calculated by the following (Equation 3) is less than 0.

25. M3 = [Si] / [Mn] ... (Equation 3) 5. The welding wire according to any one of claims 1 to 3, characterized in that, when the content of Mn contained in the welding wire is expressed as [Mn] in mass % relative to the total mass of the welding wire, the value M4 calculated by the following (Equation 4) is 0.70 or more and 0.95 or less. M4 = [Mn] / ([Mn] + [Al] + [Ti]) ... (Equation 4) 6. A gas-shielded arc welding method in which welding is performed while supplying a shielding gas using a welding wire, wherein the welding wire contains, relative to a total mass of the welding wire, Mn: more than 1.80 mass% and less than 2.20 mass%, Ti: 0.05 mass% or more and 0.23 mass% or less, Al: more than 0.10 mass% and 0.25 mass% or less, and Si: 0.45 mass% or less, wherein the content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, and the content of Ti contained in the welding wire is expressed as [Ti] in mass% relative to the total mass of the welding wire, a value M1 calculated by the following (Equation 1) is 0.45 or less, and a value M2 calculated by the following (Equation 2) is 0.30 or more and 2.50 or less. M1=[Al]+[Ti]...(Formula 1) M2=[Ti] / [Al]...(Formula 2) 7. The shielding gas is Ar and CO 2 7. The gas-shielded arc welding method according to claim 6, further comprising at least one gas selected from the group consisting of:

8. A gas-shielded arc welding method according to claim 6, characterized in that welding is performed using a feed control method in which the feeding of the welding wire is alternately switched between a forward feed period and a reverse feed period.

9. The gas-shielded arc welding method according to claim 8, wherein in said feed control method, a frequency when the forward feed period and the reverse feed period are defined as one cycle is set within a predetermined range, and the welding current supplied to the welding wire is switched between a current suppression period and a current non-suppression period based on information on at least one of a phase representing the feed speed of the welding wire and a phase representing the tip position of the welding wire.

10. A method for producing weld metal, in which welding is performed using a welding wire while supplying a shielding gas to produce weld metal, wherein the shielding gas is Ar and CO 2 a welding wire containing at least one gas selected from the group consisting of Mn: more than 1.80 mass% and less than 2.20 mass%, Ti: 0.05 mass% or more and 0.23 mass% or less, Al: more than 0.10 mass% and 0.25 mass% or less, and Si: 0.45 mass% or less, relative to a total mass of the welding wire, wherein the content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, and the content of Ti contained in the welding wire is expressed as [Ti] in mass% relative to the total mass of the welding wire, a value M1 calculated by the following (Formula 1) is 0.45 or less, and a value M2 calculated by the following (Formula 2) is 0.30 or more and 2.50 or less. M1=[Al]+[Ti] (Formula 1) M2=[Ti] / [Al] (Formula 2)

Citation Information

Patent Citations

  • Gas shield arc welding flux-cored wire

    JP2017185521A

  • Gas shield arc welding solid wire

    JP2019107697A

  • Solid wire

    JP2021003717A

  • Welding wire

    JP2022165315A

  • Welding wire

    JP2024006295A

Cited By

  • Welding wire, welding method, and method for manufacturing weld metal

    WO2025187756A1