Tial alloy material and rotor blade for jet engines
The TiAl alloy material with specific composition and precision casting method addresses the poor castability and performance issues of conventional TiAl alloys, achieving high-yield, durable, and impact-resistant jet engine rotor blades with enhanced high-temperature strength.
Patent Information
- Application Number
- PCT/JP2024/005329
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-02-15
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional TiAl alloy casting materials for jet engine rotor blades suffer from poor castability, impact resistance, high-temperature strength, and oxidation resistance, leading to shape defects and low yield of non-defective products due to insufficient fluidity and castability, and are prone to damage from debris impact.
A TiAl alloy material with a composition of 45.5 to 47.5 atomic% aluminum, 1.0 to 3.0 atomic% manganese, 0.3 to 1.0 atomic% iron, 0.5 to 2.0 atomic% vanadium, and 0.5 to 2.5 atomic% niobium, with the remainder being titanium and unavoidable impurities, optimized for precision casting to enhance castability, impact resistance, and high-temperature strength, and further containing 0.2 to 0.6 atomic% carbon for improved high-temperature strength.
The optimized TiAl alloy material achieves excellent castability, impact resistance, high-temperature strength, and oxidation resistance, enabling high-yield production of non-defective rotor blades with reduced machining requirements and improved durability against high-temperature and impact stresses.
Smart Images

Figure JP2024005329_03102024_PF_FP_ABST
Abstract
Description
TiAl alloy material and jet engine blade
[0001] The present invention relates to a TiAl alloy material and a jet engine rotor blade. This application claims priority to Japanese Patent Application No. 2023-049763, filed on March 27, 2023, the contents of which are incorporated herein by reference.
[0002] Conventionally, jet engine rotor blades have been made of Ni-based superalloys. In recent years, jet engine rotor blades made of TiAl alloys have been used. The density of TiAl alloys is about half that of Ni-based superalloys. Therefore, jet engine rotor blades made of TiAl alloys contribute significantly to improving engine efficiency and reducing fuel consumption by reducing the weight of the rotor blades.
[0003] Two types of TiAl alloys have been put to practical use as materials for jet engine blades. The first TiAl alloy to be put to practical use was TiAl4822 (Ti-48.0Al-2Nb-2Cr (atomic %)). TiAl4822 is currently used in large quantities as a material for the final stage turbine blades of jet engines such as LEAP (Leading Edge Aviation Propulsion). The next TiAl alloy to be put to practical use was TNM alloy (Ti-43.5Al-4.0Nb-1.0Mo-0.1B (atomic %)).
[0004] Currently, jet engine blades made of TiAl alloy material are manufactured by cutting them out of large rectangular ingots, which requires a large amount of cutting work during manufacturing, resulting in high processing costs.
[0005] For this reason, it has been considered to manufacture jet engine blades made of TiAl alloy material by using a precision casting method to manufacture a material having a shape similar to that of the jet engine blade, and then machining the material as necessary. In the precision casting method, a casting is manufactured using a mold having a cavity with an inner shape similar to that of the product. The mold adhering to the outside of the casting is then removed. This results in a material consisting of a casting having a shape similar to that of the product. Therefore, the use of precision casting can reduce the amount of machining, and can reduce the number of processing steps and the amount of machining allowance.
[0006] Patent Document 1 describes a precision casting method for Ti and Ti alloys. Patent Document 1 also describes melting a Ti or Ti alloy base material by induction heating and suction casting the molten Ti or Ti alloy body into a gas-permeable mold. Patent Document 1 also discloses a TiAl intermetallic compound as the Ti or Ti alloy base material.
[0007] Patent Document 2 describes a centrifugal casting method for metallic materials. Patent Document 2 also discloses a method in which a mold is placed on a rotating table and molten metal is poured into the mold while the rotating table is being rotated. Patent Document 2 also discloses that the metallic material is a TiAl alloy, a Ti alloy, or a Ni alloy.
[0008] Patent Document 3 describes a method for producing a Ti alloy casting, in which a cavity inside a mold is filled with molten Ti alloy, and the mold is rotated at high speed together with the molten metal inside to apply centrifugal force to the molten metal to perform casting. Patent Document 3 also discloses that the Ti alloy is a Ti alloy based on a TiAl intermetallic compound.
[0009] Japanese Unexamined Patent Publication No. 4-22562 (A) Japanese Unexamined Patent Publication No. 2016-78067 (A) Japanese Unexamined Patent Application No. 2008-254052 (A)
[0010] However, conventional TiAl alloy casting materials have insufficient castability due to the insufficient fluidity of the molten alloy obtained by melting raw materials corresponding to the casting composition. Therefore, for example, when a TiAl alloy casting material is produced by a precision casting method using raw materials corresponding to the composition of the TiAl alloy casting material, a defective shape is likely to occur due to poor molten alloy flow, in which an area is formed in the cavity of the mold where the molten alloy is not sufficiently filled. In particular, when a jet engine blade made of a TiAl alloy casting material is produced by a precision casting method, a defective shape is likely to occur due to poor molten alloy flow, resulting in a low yield of non-defective products. This is because the jet engine blade has a complex shape.
[0011] It is also important for jet engine blades to have good impact resistance. For example, TNM alloy, which has been put into practical use as a material for jet engine blades, was once used as the material for the turbine final stage blades of the PW1100G, a high-bypass geared turbofan engine, but was suddenly discontinued. The reason for this is said to be that a considerable number of blades were destroyed when debris flying from inside the engine collided with the turbine final stage blades made of TNM alloy at high speed during flight. In other words, the impact resistance of jet engine blades is an important characteristic that determines whether the product can continue to be used. The impact resistance of jet engine blades is determined by the material of the jet engine blades.
[0012] Furthermore, because jet engine blades are components used at high temperatures, they are naturally required to have good high-temperature strength and oxidation resistance. However, conventional TiAl alloy casting materials have not been able to have good castability and all of the properties of impact resistance, high-temperature strength, and oxidation resistance.
[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a TiAl alloy material that has good castability and is excellent in impact resistance, high-temperature strength, and oxidation resistance, and that can be suitably used as a material for jet engine blades. Another object of the present invention is to provide a jet engine blade made of a TiAl alloy material that can be produced with good yield and is excellent in impact resistance, high-temperature strength, and oxidation resistance.
[0014] In order to solve the above problems, the following means are provided.
[0015] [1] A TiAl alloy material containing 45.5 to 47.5 atomic percent aluminum, 1.0 to 3.0 atomic percent manganese, 0.3 to 1.0 atomic percent iron, 0.5 to 2.0 atomic percent vanadium, 0.5 to 2.5 atomic percent niobium, and the balance being titanium and inevitable impurities.
[0016] [2] The TiAl alloy material according to [1], further containing carbon: 0.6 atomic % or less. [3] The TiAl alloy material according to [2], further containing carbon: 0.2 atomic % or more.
[0017] [4] The TiAl alloy material according to [1], containing 46.0 to 47.0 atomic percent aluminum. [5] The TiAl alloy material according to [1], containing 1.2 to 2.8 atomic percent manganese. [6] The TiAl alloy material according to [1], containing 0.4 to 0.8 atomic percent iron. [7] The TiAl alloy material according to [1], containing 0.7 to 1.8 atomic percent vanadium. [8] The TiAl alloy material according to [1], containing 0.6 to 2.3 atomic percent niobium. [9] The TiAl alloy material according to [3], containing 0.3 to 0.5 atomic percent carbon.
[0018]
[10] A mold having a cavity that is rectangular in plan view, wherein the cavity has a side that is 80 mm long in a first direction and a side that is 80 mm long in a second direction that gradually decreases from a gate to a bottom surface, and the bottom surface is provided with a slit that is 80 mm long in the first direction and 1 mm long in the second direction, and when 500 g of molten alloy obtained by melting raw materials corresponding to a composition after casting is poured from the sprue, the amount of molten alloy that leaks from the slit is 20 g or more.
[0019]
[11] The absorbed energy of the Charpy impact test at 20 ° C is 4 J / cm 2
[12] The TiAl alloy material according to [1], having a tensile strength of 400 MPa or more at 800°C.
[13] The TiAl alloy material according to [1], having a weight increase of 0.2 kg / m when the surface is polished with water-resistant abrasive paper having a grit size of 600 and then maintained in air at 1000°C for 100 hours. 2 The TiAl alloy material according to [1] below.
[0020]
[14] A jet engine blade, characterized by comprising the TiAl alloy material according to any one of [1] to
[13] .
[0021] The TiAl alloy material of the present invention contains predetermined amounts of aluminum (Al), manganese (Mn), iron (Fe), vanadium (V), and niobium (Nb), with the balance being titanium (Ti) and unavoidable impurities. Therefore, the TiAl alloy material of the present invention has good castability. Therefore, the TiAl alloy material of the present invention can be manufactured with a high yield of good products using a casting method such as a precision casting method. Furthermore, the TiAl alloy material of the present invention has excellent impact resistance, high-temperature strength, and oxidation resistance. Therefore, the TiAl alloy material of the present invention can be preferably used as a material for jet engine blades. Furthermore, because the jet engine blade of the present invention is made of the TiAl alloy material of the present invention, it can be manufactured with a high yield and has excellent impact resistance, high-temperature strength, and oxidation resistance.
[0022] FIG. 1 is a plan view of a mold used in the examples. FIG. 2 is a cross-sectional view of a mold used in the examples. FIG. 2 is a photograph of an example of a TiAl alloy cast material obtained in the examples, and is a photograph of Alloy No. 2. FIG. 3 is a drawing showing the shape of a tensile test piece used to evaluate high-temperature strength. FIG. 1 is a photograph of Alloy No. 6 (comparative alloy), taken from the outer surface of the mold 10, showing molten alloy leaking from a slit in the bottom surface of the cavity 11 when the molten alloy was poured into the mold 10. FIG. 1 is a photograph of Alloy No. 8 (invention alloy), taken from the outer surface of the mold 10, showing molten alloy leaking from a slit in the bottom surface of the cavity 11 when the molten alloy was poured into the mold 10.
[0023] In order to solve the above problems, the present inventors have conducted extensive research focusing on the relationship between the composition of a TiAl alloy cast material and the castability, impact resistance, high-temperature strength, and oxidation resistance, and have found that a TiAl alloy cast material consisting of 45.5 to 47.5 atomic percent aluminum (Al), 1.0 to 3.0 atomic percent manganese (Mn), 0.3 to 1.0 atomic percent iron (Fe), 0.5 to 2.0 atomic percent vanadium (V), 0.5 to 2.5 atomic percent niobium (Nb), the balance being titanium (Ti) and unavoidable impurities, is sufficient.
[0024] More specifically, the inventors have found that by setting the Al content in the TiAl alloy cast material within the above-mentioned relatively narrow range, and then adding Mn and Fe within the above-mentioned ranges to improve castability, V within the above-mentioned ranges to improve impact resistance, and Nb within the above-mentioned ranges to improve oxidation resistance, all of the properties of castability, impact resistance, high-temperature strength, and oxidation resistance become suitable for use as a material for jet engine blades, and have arrived at the present invention.
[0025] The TiAl alloy material and the jet engine rotor blade of the present invention will be described in detail below. In this embodiment, as an example of the TiAl alloy material of the present invention, the TiAl alloy material will be described as a cast TiAl alloy material produced by a casting method.
[0026] [Cast TiAl Alloy] The cast TiAl alloy (TiAl alloy material) of this embodiment contains 45.5 to 47.5 atomic percent aluminum (Al), 1.0 to 3.0 atomic percent manganese (Mn), 0.3 to 1.0 atomic percent iron (Fe), 0.5 to 2.0 atomic percent vanadium (V), and 0.5 to 2.5 atomic percent niobium (Nb), with the balance consisting of titanium and inevitable impurities. The cast TiAl alloy of this embodiment is a casting produced by a casting method. Examples of the casting method that can be used include precision casting.
[0027] "Al" Al is a basic element of TiAl alloy together with Ti. Al, together with Ti, forms the TiAl phase in TiAl alloy castings, Ti 3 The Al phase constitutes the TiAl alloy. If the Al content is less than 45.5 atomic %, impact resistance becomes insufficient. If the Al content exceeds 47.5 atomic %, high-temperature strength and impact resistance become insufficient. Therefore, the Al content in the TiAl alloy casting material is set to 45.5 to 47.5 atomic %. In order to ensure high-temperature strength and oxidation resistance while ensuring impact resistance, the Al content is preferably 46.0 to 47.0 atomic %, and more preferably 46.2 to 46.8 atomic %.
[0028] "Mn" Mn improves castability when the Al content in the TiAl alloy cast material is within the above range. If the Mn content is less than 1.0 atomic %, the effect of improving castability is not sufficiently obtained. Furthermore, if the Mn content exceeds 3.0 atomic %, high-temperature strength and oxidation resistance become insufficient. Therefore, the amount of Mn added to the TiAl alloy cast material is set to 1.0 to 3.0 atomic %. In order to improve castability and ensure high-temperature strength and oxidation resistance, the Mn content is preferably 1.2 to 2.8 atomic %, and more preferably 1.5 to 2.5 atomic %.
[0029] "Fe" Fe improves castability when the Al content in the TiAl alloy cast material is within the above range. If the Fe content is less than 0.3 atomic %, the effect of improving castability is not sufficiently obtained. Furthermore, if the Fe content exceeds 1.0 atomic %, high-temperature strength and oxidation resistance become insufficient. Therefore, the Fe content in the TiAl alloy cast material is set to 0.3 to 1.0 atomic %. In order to improve castability and ensure high-temperature strength and oxidation resistance, the Fe content is preferably 0.4 to 0.8 atomic %, and more preferably 0.5 to 0.7 atomic %.
[0030] "V" V improves impact resistance when the Al content in the TiAl alloy cast material is within the above range. If the V content is less than 0.5 atomic %, the effect of improving impact resistance is not sufficiently obtained. Furthermore, if the V content exceeds 2.0 atomic %, the oxidation resistance becomes insufficient. Therefore, the V content in the TiAl alloy cast material is set to 0.5 to 2.0 atomic %. In order to improve impact resistance and ensure oxidation resistance, the V content is preferably 0.7 to 1.8 atomic %, and more preferably 0.9 to 1.6 atomic %.
[0031] "Nb" Nb improves oxidation resistance when the Al content in the TiAl alloy cast material is within the above range. If the Nb content is less than 0.5 atomic %, oxidation resistance is improved but not sufficiently achieved. Furthermore, if the Nb content exceeds 2.5 atomic %, impact resistance becomes insufficient. Therefore, the Nb content in the TiAl alloy cast material is set to 0.5 to 2.5 atomic %. In order to improve oxidation resistance and ensure impact resistance, the Nb content is preferably 0.6 to 2.3 atomic %, and more preferably 1.0 to 2.0 atomic %.
[0032] "C" The cast TiAl alloy material of this embodiment may further contain 0.6 atomic % or less of C. C further improves the high-temperature strength of the cast TiAl alloy material. However, if the C content exceeds 0.6 atomic %, the impact resistance decreases, which is undesirable. Therefore, when the cast TiAl alloy material of this embodiment further contains C, the C content is set to 0.6 atomic % or less. The C content is more preferably 0.5 atomic % or less, and even more preferably 0.32 to 0.40 atomic %.
[0033] Furthermore, when the cast TiAl alloy material of this embodiment further contains C, the C content is preferably 0.2 atomic % or more. This is because the effect of improving the high-temperature strength of the cast TiAl alloy material becomes significant. Therefore, when the cast TiAl alloy material of this embodiment further contains C, the C content is more preferably 0.3 atomic % or more, and even more preferably 0.32 to 0.40 atomic %.
[0034] [Method for Producing Cast TiAl Alloy Material] Next, an example of a method for producing a cast TiAl alloy material according to the present embodiment will be described. In the present embodiment, a case where a cast TiAl alloy material is produced by a precision casting method will be described.
[0035] To produce the TiAl alloy cast material of this embodiment, raw materials are first prepared. The composition of the raw materials is approximately the same as the composition of the TiAl alloy cast material obtained after casting. Therefore, raw materials having a composition corresponding to the desired cast composition are prepared. That is, in this embodiment, the composition of the raw materials is adjusted so that the composition of the TiAl alloy cast material obtained after casting is 45.5 to 47.5 atomic percent aluminum (Al), 1.0 to 3.0 atomic percent manganese (Mn), 0.3 to 1.0 atomic percent iron (Fe), 0.5 to 2.0 atomic percent vanadium (V), 0.5 to 2.5 atomic percent niobium (Nb), with the balance being titanium (Ti) and unavoidable impurities. If necessary, the composition of the raw materials may be adjusted so that the cast TiAl alloy cast material contains 0.6 atomic percent or less of carbon (C).
[0036] The shape of each component contained in the raw material corresponding to the composition after casting is not particularly limited. The shape of each component in the raw material may be partially or entirely different. The shape of each component in the raw material may be, for example, pellet-like, flake-like, granular, sponge-like, powder-like, or the like. Furthermore, the raw material may contain alloy raw materials such as AlV and ferroniobium. Furthermore, a master alloy ingot produced by melting raw materials corresponding to the composition after casting may be used as the raw material.
[0037] Next, raw materials corresponding to the composition after casting are melted to form a molten alloy. When melting the raw materials, it is preferable to use a crucible. For example, a water-cooled copper crucible, which is commonly used when melting TiAl alloys, can be used as the crucible. Alternatively, a ceramic crucible can be used. For example, an yttria crucible or a calcia crucible can be used as the crucible.
[0038] The method for melting the raw materials may be any method capable of melting the raw materials to form a molten alloy, and any melting method can be employed. Examples of methods that can be used for melting the raw materials include high-frequency melting. When using high-frequency melting, it is preferable to use a method in which, for example, a crucible containing the raw materials is placed in a chamber of a melting furnace, the chamber is evacuated, and an inert gas such as argon gas is introduced to melt the raw materials in an inert gas atmosphere. Furthermore, when using high-frequency melting, it is also possible to use a method in which, for example, a crucible containing the raw materials is placed in a chamber of a melting furnace, and the chamber is not evacuated, but an inert gas such as argon gas is introduced to replace the atmosphere in the chamber with an inert gas atmosphere, and the raw materials are melted.
[0039] The molten alloy is then poured into a mold. The mold may be made of a known material and have a cavity with an inner surface similar to the shape of the TiAl alloy casting product. For example, a mold made of zirconia-based ceramic, which is used as a mold in industrial precision casting of Ti-based alloys, may be used. The use of a mold made of zirconia-based ceramic is preferred because it is likely to produce a TiAl alloy casting product with reduced surface defects.
[0040] Known methods can be used to pour the molten alloy into the mold. For example, a suction casting method, in which the molten alloy is sucked into the mold, may be used. Alternatively, a centrifugal casting method, in which the mold is placed on a rotating table and the rotating table is rotated to apply centrifugal force to the molten alloy, may be used to pour the molten alloy into the mold. The use of suction casting and / or centrifugal casting can prevent the formation of defective shapes due to the formation of regions in the cavity of the mold that are not sufficiently filled with the molten alloy, thereby increasing the yield of non-defective products. In particular, when producing jet engine blades having complex shapes as a product of TiAl alloy casting material, the use of suction casting and / or centrifugal casting is preferred.
[0041] Alternatively, the molten alloy may be poured into the mold by preheating the mold to a predetermined temperature before pouring the molten alloy into the mold. Preheating the mold before pouring the molten alloy reduces the likelihood of forming an area in the cavity of the mold that is not sufficiently filled with the molten alloy, and reduces the likelihood of poor molten alloy flow. This results in improved castability and a higher yield of non-defective products, which is preferable.
[0042] After pouring the molten alloy into the mold, the mold is allowed to cool using a known method to produce a cast product having a shape similar to the desired TiAl alloy cast material. The mold is then removed from the cast product, and machining is performed as necessary. Through these steps, the TiAl alloy cast material of this embodiment is obtained.
[0043] The TiAl alloy cast material of this embodiment contains predetermined amounts of aluminum (Al), manganese (Mn), iron (Fe), vanadium (V), and niobium (Nb), with the remainder being titanium (Ti) and unavoidable impurities. Therefore, the TiAl alloy cast material of this embodiment has good castability. Therefore, even when produced using a precision casting method, it is possible to suppress the occurrence of shape defects due to poor molten metal flow, which results in the formation of areas in the cavity of the mold where the molten alloy is not sufficiently filled, and produce good products with a high yield. Furthermore, because the TiAl alloy cast material of this embodiment has the above composition, it has excellent impact resistance, high-temperature strength, and oxidation resistance. Therefore, the TiAl alloy cast material of this embodiment is suitable as a material for jet engine blades.
[0044] Furthermore, when the TiAl alloy cast material of this embodiment contains 0.6 atomic % or less of carbon (C), it has even better high-temperature strength, and therefore can be preferably used as a material for components used at higher temperatures, such as turbine blades in a stage preceding the final stage turbine blade, among other jet engine blades.
[0045] [Jet Engine Blade] The jet engine blade of this embodiment is made of the cast TiAl alloy material of this embodiment. Therefore, it can be manufactured with a high yield and has excellent impact resistance, high-temperature strength, and oxidation resistance. The jet engine blade of this embodiment can be manufactured, for example, by using the cast TiAl alloy material of this embodiment as a raw material and machining it using a known method as needed. Therefore, compared to manufacturing it by, for example, cutting a large rectangular ingot made of TiAl alloy, the amount of machining is small, and the number of processing steps and the amount of machining allowance can be reduced.
[0046] The above describes in detail an embodiment of the present invention, but the above embodiment is merely an example of the present invention, and additions, omissions, substitutions, and other modifications to the configuration are possible within the scope that does not deviate from the spirit of the present invention.
[0047] [Alloy No. 1 to Alloy No. 26] Using the casting method described below, cast TiAl alloy cast materials (Alloy No. 1 to Alloy No. 26) having the compositions shown in Table 1 or Table 2 were produced. First, raw materials having compositions corresponding to those shown in Table 1 or Table 2 were prepared. Specifically, sponge Ti, Al pellets, Mn flake raw material, Fe granular raw material, AlV master alloy granular raw material, Nb flake raw material, and TiC alloy powder were used as raw materials, and each was weighed and mixed so that the composition of the TiAl alloy cast material obtained after casting would be the composition shown in Table 1 or Table 2, and the total weight was adjusted to approximately 500 g.
[0048]
[0049]
[0050] Next, the raw materials were placed in an yttria crucible and melted using a high-frequency melting method to obtain a molten alloy. Specifically, the crucible containing the raw materials was placed in the chamber of a melting furnace, and evacuation of the chamber was initiated. After evacuating to a predetermined vacuum level, argon gas was introduced, and the argon gas pressure reached a predetermined value to create an argon atmosphere. Thereafter, the output of the high-frequency power supply was gradually increased to a maximum output of 5 kW, thereby raising the temperature of the raw materials and melting them. After all the raw materials had melted, the output of the high-frequency power supply was reduced to 3.5 kW and held for 3 minutes to obtain a molten alloy.
[0051] The molten alloy was then poured into the mold 10 shown in FIGS. 1A and 1B. FIG. 1A is a schematic plan view of the mold 10 used in the examples. FIG. 1B is a schematic cross-sectional view of the mold 10 used in the examples. As shown in FIGS. 1A and 1B, the mold 1 shown in FIGS. 1A and 1B has an outer shape of a substantially rectangular parallelepiped with a side length of 100 mm. The mold 1 comprises a first mold 10a and a second mold 10b arranged opposite the first mold 10a. The first mold 10a and the second mold 10b are substantially identical in shape. The first mold 10a and the second mold 10b are made of cast iron.
[0052] When pouring the molten alloy into the mold 10, the first and second molds 10a and 10b are clamped together from the outside with a clamp (not shown) to form a single unit. After the molten alloy is cooled to produce the TiAl alloy casting materials (Alloy No. 1 to Alloy No. 26), the clamp is removed to separate the first and second molds 10a and 10b. This allows the cast TiAl alloy casting materials (Alloy No. 1 to Alloy No. 26) to be removed from the mold 10.
[0053] 1A and 1B, a first mold 10a and a second mold 10b are arranged opposite each other to form a cavity 11. The cavity 11 has an inner surface similar to the shape of the TiAl alloy casting material produced in the examples. The inner surface of the cavity 11 is coated with a zirconia-based paint.
[0054] As shown in Fig. 1A, the cavity 11 is rectangular in plan view, with the length of a side extending in a first direction being 80 mm. The length of a side extending in a second direction, which is substantially perpendicular to the first direction in plan view of the cavity 11, gradually decreases from the gate toward the bottom, as shown in Fig. 1B.
[0055] Specifically, as shown in FIG. 1B, the length of the side of the cavity 11 extending in the second direction is 30 mm in the first region 11a, which extends from the gate to a bottom-side dimension of 30 mm or less; 20 mm in the second region 11b, which extends from the gate to a bottom-side dimension of more than 30 mm but not more than 55 mm; 15 mm in the third region 11c, which extends from the gate to a bottom-side dimension of more than 55 mm but not more than 80 mm; and 3 mm in the fourth region 11d, which extends from the gate to a bottom-side dimension of more than 80 mm but not more than 90 mm. Also, as shown in FIG. 1B, a slit 12 having a length of 80 mm along the first direction and a length of 1 mm along the second direction is provided on the bottom surface of the cavity 11. The slit 12 is a fifth region 11e, which extends from the gate to a bottom-side dimension of more than 90 mm but not more than 100 mm.
[0056] When pouring the molten alloy into the mold 10, an alumina funnel was placed over the cavity 11 of the mold 10. The funnel was placed with its inner surface aligned with the sprue of the cavity 11. The molten alloy was supplied into the cavity 11 through the funnel. The molten alloy was supplied until the liquid level of the poured molten alloy reached a position above the sprue of the cavity 11 on the inner wall of the funnel.
[0057] In this manner, the molten alloy was poured into the mold 10, and the mold 10 was allowed to cool, thereby producing the target TiAl alloy casting material. The clamp was then removed to separate the first mold 10a and the second mold 10b, and the cast TiAl alloy casting materials (Alloy No. 1 to Alloy No. 26) were removed from the mold 10. Figure 2 is a photograph of an example of the TiAl alloy casting material obtained in the example, showing Alloy No. 2.
[0058] The compositions of alloys No. 1 to No. 26 thus obtained were analyzed by inductively coupled plasma (ICP) atomic emission spectroscopy and combustion-infrared absorption spectroscopy, respectively, and the results confirmed that the compositions of alloys No. 1 to No. 26 were all as shown in Table 1 or Table 2.
[0059] Next, Alloy No. 1 to Alloy No. 26 obtained in this manner were evaluated for "(1) castability," "(2) impact resistance," "(3) high-temperature strength," and "(4) oxidation resistance" using the methods described below. The results are shown in Tables 3 and 4. Tables 1 to 4 also show the classification of Alloy No. 1 to Alloy No. 26 as "invention alloys," which are examples of the present invention, and "comparison alloys," which are comparative examples.
[0060] (1) Castability To produce Alloy No. 1 to Alloy No. 26, 500 g of molten alloy was poured into a mold 10, and the amount of molten alloy leaking through a slit 12 provided in the bottom surface of a cavity 11 was measured. The results were evaluated based on the following evaluation criteria.
[0061] [Evaluation criteria] A (superior castability): When 500 g of molten alloy is poured, the amount of molten alloy that flows out is 40 g or more. B (superior castability): When 500 g of molten alloy is poured, the amount of molten alloy that flows out is 20 g or more but less than 40 g. C (poor castability): When 500 g of molten alloy is poured, the amount of molten alloy that flows out is less than 20 g.
[0062] (2) Impact Resistance Generally, when manufacturing jet engine blades made of cast TiAl alloys, the cast TiAl alloys obtained after casting are subjected to HIP (hot isostatic pressing) treatment. Therefore, prior to evaluating the impact resistance (2), Alloy No. 1 to Alloy No. 26 were subjected to a heat treatment in which they were held at 1200°C for 4 hours, which corresponds to the general HIP conditions, and then cooled at a cooling rate of 10°C / min.
[0063] Furthermore, TiAl alloy cast materials are brittle materials. Therefore, if a 2 mm V-notch is made in a Charpy impact test specimen made of a TiAl alloy cast material, the absorbed energy measurement results will be smaller. As a result, the difference in the absorbed energy measurement results between each test specimen will be small, which may make it impossible to evaluate the differences between each test specimen. For this reason, in (2) Impact Resistance in this Example, flat Charpy impact test specimens without a V-notch were prepared as test specimens. Furthermore, a small hammer with a capacity of 15 J was used as the hammer for the Charpy impact test to minimize measurement error.
[0064] Specifically, Charpy impact test specimens were taken from each of Alloys No. 1 to No. 26, which had been subjected to heat treatment equivalent to HIP conditions, from a portion (second region 11b) of the cavity 11 of the mold 1 shown in FIGS. 1A and 1B, where the length of the side extending in the second direction was 20 mm. The Charpy impact test specimens were prepared in the form of flat plates measuring 10 mm in length, 10 mm in width, and 55 mm in length. Each Charpy impact test specimen was then subjected to a Charpy impact test at room temperature (20°C), and the absorbed energy was measured. The results were evaluated based on the following evaluation criteria.
[0065] [Evaluation Criteria] A (better impact resistance): Absorbed energy of 6 J / cm in a Charpy impact test at room temperature (20°C) 2 B (Excellent impact resistance): The absorbed energy in the Charpy impact test at room temperature (20°C) is 4 J / cm 2 6J / cm or more 2 C (poor impact resistance): The absorbed energy in a Charpy impact test at room temperature (20°C) is less than 4 J / cm 2 is less than.
[0066] (3) High-Temperature Strength (2) Impact Resistance (3) For Alloy No. 1 to Alloy No. 26, after Charpy impact test specimens were obtained, tensile test specimens were obtained from the cavity 11 of the mold 1 shown in Figures 1A and 1B, where the length of the side extending in the second direction was 15 mm (third region 11c). The tensile test specimens were circular in cross section, with shoulders provided between the parallel portion and the gripping portions provided at both ends of the parallel portion. Specifically, as shown in Figure 3, the parallel portion was cylindrical with a diameter of 4 mm ± 0.03 mm and a length of 28 mm, the rating distance located at the center of the parallel portion was 20 mm ± 0.1 mm, the gripping portion was a thread with an outer diameter of 10 mm and a pitch of 1.5 mm (M10 × P1.5), and the shoulder was a curve with a radius R of 15 mm in side view. Tensile test specimens were prepared with a total length of 60 mm. A tensile test was carried out on each of the tensile test pieces obtained in this manner at 800°C to measure the tensile strength at break, which is the maximum load, and the test pieces were evaluated based on the following evaluation criteria.
[0067] [Evaluation criteria] A (superior high-temperature strength): Tensile strength at 800°C is 500 MPa or more. B (superior high-temperature strength): Tensile strength at 800°C is 400 MPa or more and less than 500 MPa. C (poor high-temperature strength): Tensile strength at 800°C is less than 400 MPa.
[0068] (4) Oxidation Resistance (3) Oxidation test specimens were taken from the cavity 11 of the mold 1 shown in Figures 1A and 1B, where the length of the side extending in the second direction was 3 mm (fourth region 11d). The oxidation test specimens were prepared from flat plates measuring 10 mm in length, 20 mm in width, and 2 mm in thickness. The oxidation test specimens were prepared by cutting flat plates from the fourth region 11d of Alloys 1 to 26 after the tensile test specimens were taken from the fourth region 11d using a grindstone, and polishing the surfaces of the resulting flat plates using waterproof abrasive paper with a grit size of 600. Each oxidation test specimen thus obtained was subjected to an oxidation test in which it was held in air at 1000°C for 100 hours, and the oxidation mass gain after the oxidation test was measured. Evaluation was then performed based on the following evaluation criteria.
[0069] [Evaluation Criteria] A (better oxidation resistance): Weight increase after oxidation test is 0.1 kg / m 2 B (Excellent oxidation resistance): The weight increase after the oxidation test was 0.1 kg / m or less. 2 Super 0.2kg / m 2 C (poor oxidation resistance): Weight increase after oxidation test is 0.2 kg / m or less. 2 It's super.
[0070]
[0071]
[0072] As shown in Tables 3 and 4, it was confirmed that Alloy Nos. 2 to 4, 7, 8, 11, 12, 15, 16, 19, and 20, which are "invention alloys" consisting of 45.5 to 47.5 atomic % aluminum (Al), 1.0 to 3.0 atomic % manganese (Mn), 0.3 to 1.0 atomic % iron (Fe), 0.5 to 2.0 atomic % vanadium (V), 0.5 to 2.5 atomic % niobium (Nb), the balance being titanium (Ti) and inevitable impurities, and Alloy Nos. 22 to 25, which are "invention alloys" containing 0.6 atomic % or less of carbon (C), all have excellent castability, impact resistance, high-temperature strength, and oxidation resistance.
[0073] The following provides further details. [1] Regarding the Preferred Al Concentration: Alloys No. 1 to No. 5 are a group in which the Al content is varied. In this group, the contents of the components excluding Al, Ti, and irreversible impurities are within the appropriate range: manganese (Mn): 2.0 atomic %, iron (Fe): 0.5 atomic %, vanadium (V): 1.2 atomic %, and niobium (Nb): 1.5 atomic %.
[0074] When the Al content was 45.7 atomic % (Alloy No. 2), 46.5 atomic % (Alloy No. 3), or 47.3 atomic % (Alloy No. 4), the castability, impact resistance, high-temperature strength, and oxidation resistance were all good. On the other hand, when the Al content was low at 45.0 atomic % (Alloy No. 1 (Comparative Alloy)), the impact resistance was poor. Furthermore, when the Al content was high at 47.8 atomic % (Alloy No. 5 (Comparative Alloy)), the impact resistance and high-temperature strength were poor.
[0075] [2] Suitable Mn Concentration Alloy Nos. 6 to 9 are a group in which the Mn content is varied. In this group, the contents of the components excluding Mn, Ti, and irreversible impurities are within the appropriate range: aluminum (Al): 46.5 atomic %, iron (Fe): 0.5 atomic %, vanadium (V): 1.2 atomic %, and niobium (Nb): 1.5 atomic %.
[0076] When the Mn content was 1.2 atomic % (Alloy No. 7) or 2.8 atomic % (Alloy No. 8), the castability, impact resistance, high-temperature strength, and oxidation resistance were all good. In particular, Alloy No. 8 had excellent castability. On the other hand, when the Mn content was low, at 0.8 atomic % (Alloy No. 6 (Comparative Alloy)), the castability was poor. Furthermore, when the Mn content was high, at 3.3 atomic % (Alloy No. 9 (Comparative Alloy)), the castability was particularly good, but the high-temperature strength and oxidation resistance were poor.
[0077] Figure 4A is a photograph of Alloy No. 6 (comparative alloy) taken from the exterior of mold 10, showing molten alloy leaking from slit 12 provided in the bottom surface of cavity 11 when the molten alloy was poured into mold 10. Figure 4B is a photograph of Alloy No. 8 (invention alloy) taken from the exterior of mold 10, showing molten alloy leaking from slit 12 provided in the bottom surface of cavity 11 when the molten alloy was poured into mold 10.
[0078] 4A and 4B, it can be seen that Alloy No. 8 (invention alloy) had a larger amount of molten metal leaking out of the slits 12 than Alloy No. 6 (comparison alloy). The amount of molten metal leaking out of the slits 12 formed in the bottom surface of the cavity 11 is naturally closely related to the fluidity of the molten alloy. In other words, the greater the amount of molten metal leaking out of the slits 12, the better the fluidity of the molten alloy, and the better the castability can be evaluated to be.
[0079] [3] Regarding the Suitable Concentration of Fe: Alloys No. 10 to No. 13 are a group in which the Fe content is varied. In this group, the contents of the components excluding Fe, Ti, and irreversible impurities are aluminum (Al): 46.5 atomic %, manganese (Mn): 2.0 atomic %, vanadium (V): 1.2 atomic %, and niobium (Nb): 1.5 atomic %, all of which are within the suitable range.
[0080] When the Fe content was 0.4 atomic % (Alloy No. 11) and 0.8 atomic % (Alloy No. 12), the castability, impact resistance, high-temperature strength, and oxidation resistance were all good. In particular, Alloy No. 12 had excellent castability. On the other hand, when the Fe content was low, at 0.2 atomic % (Alloy No. 10 (Comparative Alloy)), the castability was poor. Furthermore, when the Fe content was high, at 1.2 atomic % (Alloy No. 13 (Comparative Alloy)), the castability was particularly good, but the high-temperature strength and oxidation resistance were poor.
[0081] [4] Regarding the Suitable Concentration of V Alloy Nos. 14 to 17 are a group in which the content of V is varied. In this group, the contents of components excluding V, Ti, and irreversible impurities are aluminum (Al): 46.5 atomic %, manganese (Mn): 2.0 atomic %, iron (Fe): 0.5 atomic %, and niobium (Nb): 1.5 atomic %, which are within the suitable range.
[0082] When the V content was 0.7 atomic % (Alloy No. 15) or 1.8 atomic % (Alloy No. 16), the castability, impact resistance, high-temperature strength, and oxidation resistance were all good. In particular, Alloy No. 16 had excellent impact resistance. On the other hand, when the V content was low at 0.4 atomic % (Alloy No. 14 (Comparative Alloy)), the impact resistance was poor. Furthermore, when the V content was high at 2.2 atomic % (Alloy No. 17 (Comparative Alloy)), the impact resistance and high-temperature strength were particularly excellent, but the oxidation resistance was poor.
[0083] [5] Regarding the Suitable Nb Concentration Alloy Nos. 18 to 21 are a group in which the Nb content is varied. In this group, the contents of the components excluding Nb, Ti, and irreversible impurities are aluminum (Al): 46.5 atomic %, manganese (Mn): 2.0 atomic %, iron (Fe): 0.5 atomic %, and vanadium (V): 1.2 atomic %, all of which are within the suitable range.
[0084] When the Nb content was 0.6 atomic % (Alloy No. 19) or 2.3 atomic % (Alloy No. 20), the castability, impact resistance, high-temperature strength, and oxidation resistance were all good. In particular, Alloy No. 20 had excellent oxidation resistance. On the other hand, when the Nb content was low, at 0.4 atomic % (Alloy No. 18 (Comparative Alloy)), the oxidation resistance was poor. Furthermore, when the Nb content was high, at 2.7 atomic % (Alloy No. 21 (Comparative Alloy)), the oxidation resistance was particularly excellent, but the impact resistance was poor.
[0085] [6] Regarding the Suitable Concentration of C Alloy Nos. 22 to 26 are a group in which the content of additionally added C was varied. In this group, the contents of the components excluding C, Ti, and irreversible impurities were aluminum (Al): 46.5 atomic %, manganese (Mn): 2.0 atomic %, iron (Fe): 0.5 atomic %, vanadium (V): 1.2 atomic %, and niobium (Nb): 1.5 atomic %, all of which were within the suitable range.
[0086] When the C content was 0.3 atomic % (Alloy No. 23), 0.4 atomic % (Alloy No. 24), or 0.5 atomic % (Alloy No. 250), the castability, impact resistance, and oxidation resistance were all good, and the high-temperature strength was particularly excellent. On the other hand, when the C content was relatively low at 0.1 atomic % (Alloy No. 22), the castability, impact resistance, high-temperature strength, and oxidation resistance were all good, but the high-temperature strength was not particularly excellent. Furthermore, when the C content was high at 0.7 atomic % (Alloy No. 26 (comparison alloy)), the high-temperature strength was significantly excellent, but the impact resistance was poor.
[0087] [7] Summary As described above, the "invention alloys" shown in Tables 1 to 4 have been shown to exhibit superior properties compared to the "comparison alloys" that do not satisfy the composition of the TiAl alloy cast material of the present application. Furthermore, among the "invention alloys" shown in Tables 1 to 4, the "invention alloys" that further contain 0.2 to 0.6 atomic % of carbon (C) have been shown to have good castability, impact resistance, and oxidation resistance, and also to have superior high-temperature strength.
[0088] The TiAl alloy cast material of the present invention has good castability. Therefore, even when produced using a precision casting method, it is possible to suppress the occurrence of shape defects due to poor molten alloy flow, which results in the formation of regions in which the molten alloy is not sufficiently filled in the cavity of the mold, and produce good products with a high yield. Furthermore, the TiAl alloy cast material of the present invention has excellent impact resistance. Therefore, even when used in components that are subject to collision with foreign objects during use, such as jet engine blades, it is less likely to suffer impact fracture. Furthermore, the TiAl alloy cast material of the present invention has excellent high-temperature strength and oxidation resistance. Therefore, it can be suitably used in components used at high temperatures, such as jet engine blades. For these reasons, the TiAl alloy cast material of the present invention can be suitably used as a material for jet engine blades, such as jet engine turbine final stage blades.
[0089] Furthermore, when the TiAl alloy cast material of the present invention contains 0.6 atomic % or less of carbon (C), the high-temperature strength is further improved, and therefore the material can be preferably used as a material for components used at higher temperatures, such as turbine blades in a stage preceding the final stage turbine blade, among other jet engine blades.
[0090] 1 Mold 10a First mold 10b Second mold 11 Cavity 12 Slit
Claims
1. A TiAl alloy material containing 45.5 to 47.5 atomic percent aluminum, 1.0 to 3.0 atomic percent manganese, 0.3 to 1.0 atomic percent iron, 0.5 to 2.0 atomic percent vanadium, 0.5 to 2.5 atomic percent niobium, with the balance being titanium and unavoidable impurities.
2. The TiAl alloy material according to claim 1, further containing carbon: 0.6 atomic % or less.
3. The TiAl alloy material according to claim 2, further containing carbon: 0.2 atomic % or more.
4. The TiAl alloy material according to claim 1, containing 46.0 to 47.0 atomic percent aluminum.
5. The TiAl alloy material according to claim 1, containing manganese: 1.2 to 2.8 atomic %.
6. The TiAl alloy material according to claim 1, containing 0.4 to 0.8 atomic percent iron.
7. The TiAl alloy material according to claim 1, containing vanadium: 0.7 to 1.8 atomic %.
8. The TiAl alloy material according to claim 1, containing niobium: 0.6 to 2.3 atomic %.
9. The TiAl alloy material according to claim 3, containing 0.3 to 0.5 atomic % carbon.
10. A TiAl alloy material as described in claim 1, comprising a mold having a rectangular cavity in a plan view, the cavity having sides each extending in a first direction that are 80 mm long and sides each extending in a second direction that are gradually shortened from a spout to a bottom surface, the bottom surface being provided with a slit having a length of 80 mm along the first direction and a length of 1 mm along the second direction, and when 500 g of molten alloy made by melting raw materials corresponding to the composition after casting is poured from the spout, the amount of molten alloy leaking out from the slit is 20 g or more.
11. The absorbed energy in the Charpy impact test at 20°C is 4 J / cm 2 The TiAl alloy material according to claim 1 .
12. The TiAl alloy material according to claim 1, having a tensile strength of 400 MPa or more at 800°C.
13. After polishing the surface with 600 grit waterproof abrasive paper, the weight increase by holding it in air at 1000°C for 100 hours is 0.2 kg / m 2 2. The TiAl alloy material of claim 1, wherein:
14. A jet engine rotor blade, comprising the TiAl alloy material according to any one of claims 1 to 13.
Citation Information
Patent Citations
Precision casting method for ti, ti alloy and precision casting device
JP1992022562A
METHOD FOR PRODUCING Ti ALLOY CASTING
JP2008254052A
Metallic material centrifugal casting method
JP2016078067A
Sensor device
JP2023049763A
Production of alloy based on tial intermetallic compound
JP1993255827A