Electrochemical capacitor
By employing graphene sheets with a three-dimensional structure and an ionic liquid electrolyte, the electrochemical capacitor achieves high energy density through enhanced adsorption and redox reactions, addressing the limitations of existing capacitors and expanding their application scope.
Patent Information
- Application Number
- PCT/JP2024/005847
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-02-19
- Publication Date
- 2024-10-03
AI Technical Summary
Existing electrochemical capacitors have low energy density, limiting their applications, and there is a need for higher energy density to expand their uses, particularly in ICT and power storage applications.
The use of graphene sheets stacked in a three-dimensional manner via carbon nanotubes as electrodes, combined with an ionic liquid electrolyte, allows for high voltage operation, enabling significant capacity and energy density through adsorption and redox reactions, with a focus on achieving an atomic ratio of F to C of 10% or more on the electrode surface.
This configuration results in a capacitor with high capacity and energy density, enabling efficient power storage and enhanced performance in applications such as personal computers, smartphones, and in-vehicle systems.
Smart Images

Figure JP2024005847_03102024_PF_FP_ABST
Abstract
Description
electrochemical capacitor
[0001] The present invention relates to an electrochemical capacitor.
[0002] With the increasing demand for ICT applications such as personal computers and smartphones, in-vehicle applications, and power storage applications, there is a demand for higher capacity electrochemical devices, such as capacitors.
[0003] Graphene has a theoretical specific surface area of approximately 2600 m 2 / g and has electrical conductivity, making it a promising electrode material for capacitors.
[0004] Patent Literature 1 proposes a graphene sheet film in which two or more graphene sheets are stacked in parallel via carbon nanotubes, and the graphene sheet stacks are electrically and mechanically connected to each other in a three-dimensional manner by the carbon nanotubes. The use of this film in an electrode has been reported to have a capacitance of 290.6 F / g.
[0005] International Publication No. 2012 / 073998
[0006] One aspect of the present invention relates to an electrochemical capacitor, the electrochemical capacitor comprising a first electrode containing a first active material, a second electrode containing a second active material, and an electrolyte, the electrolyte containing an ionic liquid, wherein when a surface of the first electrode is quantitatively analyzed by X-ray photon spectroscopy (XPS) based on a relative sensitivity factor, an atomic ratio R of element F to element C derived from the ionic liquid is 0.05: F is 10% or more.
[0007] According to the present disclosure, an electrochemical capacitor with high energy density can be realized.
[0008] 1 is a partially cutaway perspective view of an electrochemical capacitor according to an embodiment of the present disclosure, showing the applied voltage V 1 Single-pole capacity C 1 1 is a graph showing the change in F1s spectrum in XPS analysis of the negative electrode surface for the capacitors of Example 1 and Comparative Example 1.
[0009] The capacitor described in Patent Document 1 is capable of rapid charging and discharging and has a high output density compared to lithium-ion batteries, but its energy density is still low, limiting its applications. In order to expand the applications of electrochemical capacitors, there is a demand for a further increase in energy density.
[0010] The higher the operating voltage of a capacitor, the higher the energy density that can be obtained. Therefore, combinations of electrolytes and electrode materials that can operate at high voltages are being explored.
[0011] Hereinafter, the term "electrochemical capacitor" encompasses capacitors having various types of electricity storage mechanisms, and refers to an electricity storage device that at least partially has an electricity storage mechanism, such as an electric double layer capacitor or a lithium ion capacitor. An electricity storage device or electrochemical capacitor includes a pair of capacitor electrodes and an electrolyte. The electrodes contain an active material.
[0012] Active materials exhibit capacitance by, for example, doping and dedoping with ions. Doping an active material with ions is a concept that includes the adsorption of ions into the active material, the occlusion of ions by the active material, and chemical interactions between the active material and ions. Dedoping an active material with ions includes the desorption of ions from the active material, the release of ions from the active material, and the release of ions from the active material, as well as the release of ions from the active material. Here, doping an active material with ions primarily refers to the adsorption of ions into the active material, and dedoping an active material with ions primarily refers to the desorption of ions from the active material. When ions are adsorbed onto the active material, an electric double layer is formed, resulting in capacitance. In other words, a capacitor electrode primarily refers to a polarizable electrode, but it may also be an electrode that has the properties of a polarizable electrode while also contributing to capacitance through the Faraday reaction.
[0013] An electrochemical capacitor according to one embodiment of the present disclosure includes a first electrode containing a first active material, a second electrode containing a second active material, and an electrolyte. A separator is typically interposed between the first electrode and the second electrode. The electrolyte contains an ionic liquid. Hereinafter, the electrochemical capacitor according to the present disclosure may be simply referred to as a "capacitor."
[0014] In one embodiment, the electrochemical capacitor according to the present disclosure exhibits capacitance by forming an electric double layer when cations or anions constituting the ionic liquid are adsorbed to the first active material or the second active material. In addition, when a high voltage equal to or higher than a threshold is applied, a reduction reaction of the cations or an oxidation reaction of the anions constituting the ionic liquid occurs, and capacitance is also exhibited by charge transfer between the active material and the cations or anions due to the oxidation-reduction reaction.
[0015] A voltage of 4.0 V or more can be applied between the first electrode and the second electrode. In this case, capacitance is generated by an oxidation-reduction reaction, and a capacitor with high capacity and high energy density can be realized.
[0016] One of the first electrode and the second electrode is the positive electrode of the capacitor, and the other is the negative electrode. In the following description, the first electrode is the negative electrode and the second electrode is the positive electrode. That is, it is assumed that a lower potential is applied to the first electrode than to the second electrode. The first electrode and the second electrode may be the same electrode or different electrodes.
[0017] When the surface of the first electrode is quantitatively analyzed using X-ray photon spectroscopy (XPS) based on the relative sensitivity coefficient, the atomic ratio R of element F derived from the ionic liquid to element C is F is 10% or more. In this case, the capacitor can achieve high capacity and high energy density. The inventors' current knowledge suggests that the reason for this is as follows. However, the present invention is not limited to this.
[0018] The cations or anions contained in the ionic liquid can be reduced or oxidized by applying a high voltage, and the reaction products of the reduction or oxidation reaction can be generated in the electrolyte solution, and these reaction products can be adsorbed and deposited on the surface of the positive or negative electrode.
[0019] For example, at the negative electrode, the cations of the ionic liquid may be reduced to generate reduction products. The reduction products may then react with the anions of the ionic liquid to generate by-products. The reduction products may adsorb onto the negative electrode surface together with the anions, and / or an adsorption state may be formed in which the by-products adsorbed onto the negative electrode surface with the anions. As a result, when the surface of the negative electrode is analyzed using a surface analysis method such as XPS, elements derived from the ionic liquid are observed. For example, if the cations or anions of the ionic liquid contain F (fluorine), F is measured by XPS analysis. If the cations or anions of the ionic liquid contain B (boron), B is measured by XPS analysis.
[0020] The atomic ratio R of F to C on the negative electrode surface calculated by XPS F When the ratio R is 10% or more, the capacity due to the oxidation-reduction reaction increases significantly, and a capacitor with a high capacity and a high energy density can be realized. F The ratio R may be 14% or more. F The ratio R may be 14% or more. F may be 30% or less, or may be 14% or more and 30% or less.
[0021] The adsorption state formed on the surface of the negative electrode may contain B. In this case, the atomic ratio R of B to C calculated by the XPS method is B may be 1% or more.
[0022] Specifically, for example, 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIBF) represented by the following formula (1) can be used. 4 When 1-ethyl-3-methylimidazolium cation (EMI) is used as the ionic liquid, the 1-ethyl-3-methylimidazolium cation (EMI) + ) is reduced at the negative electrode, and EMI radicals can be generated by the reaction shown in formula (2) below.
[0023] Formula (1):
[0024]
[0025] Formula (2):
[0026]
[0027] On the other hand, during discharge, the reaction in reverse to formula (2) proceeds, and the EMI radical releases one electron to form the EMI + Therefore, in addition to the capacitance generated by the adsorption of cations or anions, the capacitor also generates additional capacitance through redox reactions, resulting in a significantly higher capacitance.
[0028] The radical that is the reaction product of formula (2) is the anion BF 4 - The reaction product can reach the surface of the negative electrode and form an adsorbed state. 4 - The ratio R F or ratio R B When the adsorbate contains F or B so that satisfies the above relational expression, high capacity and high energy density can be achieved.
[0029] X-ray photoelectron spectroscopy (XPS) is a technique for analyzing the composition and chemical bonding state of elements constituting a sample surface by irradiating the sample surface with X-rays and measuring the kinetic energy of photoelectrons emitted from the sample surface due to the ionization of atoms. The area of each peak in an XPS spectrum is proportional to the number of atoms of the corresponding element. However, because the ionization cross section for X-rays varies for each element and also depends on the instrument settings, it is not possible to determine the composition ratio between elements by comparing the areas of peaks corresponding to different elements. Therefore, measurements are performed on a sample with a known composition, and the relationship between the peak intensity and the number of atoms of each element is determined in advance. Using relative sensitivity factors (RSFs), the composition of elements constituting a sample surface can be accurately quantified.
[0030] An example of the conditions for XPS measurement is shown below: The C1s spectrum (248.5 eV) of graphite can be used to calibrate the binding energy.
[0031] Measurement equipment: ESCA5600 manufactured by ULVAC-PHI, Inc. X-ray source used: Al-Kα radiation, Mg-Kα radiation Analysis area: 800 μmΦ Quantitative conversion method: Quantitative value calculated from the ratio of the peak area of each element multiplied by the relative sensitivity coefficient. The first electrode and the second electrode may contain a fluorine-containing compound such as polyvinylidene fluoride (PVdF) or PTFE as a binder. In this case, in XPS measurement of the electrode surface, in addition to the peak derived from the ionic liquid, a peak derived from the C-F bond derived from the binder contained in the electrode appears in the peak of the C element. The peak derived from the C-F bond derived from the binder appears at a different binding energy position from the peak derived from the ionic liquid, so it is possible to determine whether the F present on the surface is derived from the ionic liquid based on the peak position. Ratio R F In calculating the ratio R, the number of F atoms originating from the binder is subtracted from the number of F atoms in the XPS spectrum to obtain the number of F atoms originating from the ionic liquid, and this is divided by the number of C atoms in the XPS spectrum to obtain the ratio R F Ask for.
[0032] Ratio R F (and the ratio R B ) is thought to depend on the types of anions and cations that make up the ionic liquid, the content (concentration) of the ionic liquid in the electrolyte, and also on the surface condition of the first electrode (first active material) on which the adsorbates accumulate. In order to obtain high capacity and high energy density, the ratio R F (and the ratio R B It is important to select an active material that satisfies the above relationship.
[0033] The first active material and / or the second active material may be a carbon material having a layered structure. That is, the carbon material includes a stacked structure of layers (commonly called graphene layers or graphene sheets) in which carbon atoms are bonded to form a hexagonal mesh in a plane. The carbon material may include graphene. The graphene may be reduced graphene oxide or graphene having a three-dimensional structure.
[0034] Graphene is a carbon material whose smallest unit is a graphene sheet having a thickness of one carbon atom, and is usually formed as a laminate of multiple graphene sheets. A graphene sheet is an aggregate or molecule made of sp2-bonded carbon having a thickness of one carbon atom, and has a honeycomb lattice structure that spreads out like a sheet.
[0035] Of the first active material and the second active material, at least the first active material may contain a carbon material having a layer structure.
[0036] The carbon material having a layer structure can be used as either the active material on the positive electrode side or the active material on the negative electrode side. However, in one embodiment, an electrode containing the carbon material as the first active material is used as the first electrode, and the ratio R F and the ratio R B becomes larger, and the capacity increases dramatically.
[0037] The carbon material preferably includes reduced graphene oxide, which can be obtained by reducing graphene oxide.
[0038] Graphene oxide (hereinafter also referred to as "GO") has a structure in which oxygen-containing groups are bonded to graphene sheets. The oxygen-containing groups are thought to be bonded mainly to the edge surfaces of the graphene sheet stack. The oxygen-containing groups are hydrophilic groups such as hydroxyl groups, carbonyl groups, carboxyl groups, and epoxy groups. Graphene oxide (GO) generally has dispersibility in polar solvents such as water. Graphene oxide (GO) generally has insulating properties because it contains sp3-bonded carbon.
[0039] By reducing graphene oxide (GO), oxygen-containing groups are removed to obtain reduced graphene oxide (hereinafter also referred to as "rGO"). Reduced graphene oxide (rGO) is a conductive graphene analog. Reduced graphene oxide may contain oxygen-containing groups that were not removed during the reduction process. Due to the presence of functional groups such as oxygen atoms in the graphene layers, the crystalline structure of the carbon material deviates from the ideal graphene or graphite structure, and the carbon atoms in the graphene layers have a mixture of sp2 and sp3 bonds. As a result, the application of high voltage facilitates the expansion of the spaces between the graphene layers, facilitating the insertion of cations and anions between the graphene layers and the expansion of the region where the electric double layer is formed. Therefore, using reduced graphene oxide as an active material can dramatically increase the capacitance of capacitors.
[0040] In addition, the presence of functional groups such as oxygen atoms can cause distortion in the planar structure of graphene, resulting in disorder in the layer structure (or disorder in the interlayer distance), or the graphene layers can bend or bent to form a three-dimensional structure. This increases the effective surface area available for adsorption of cations and anions, enabling high capacity to be achieved. In addition, adsorption by reaction with ionic liquids is easily formed, and R F and the ratio R B It is easy to control to a large value.
[0041] General graphene usually has a flat sheet shape. On the other hand, the graphene used in the capacitor of this embodiment may not be a flat sheet, but may be a graphene sheet laminate of various shapes having a disordered layer structure (or a disordered interlayer distance) (or having a three-dimensional structure). By using graphene having a three-dimensional structure (graphene sheet laminate) as the active material, the capacitance of the capacitor is dramatically increased.
[0042] The three-dimensional structure mainly refers to a microscopic three-dimensional structure (i.e., a microstructure) formed within a flake-like particle. The three-dimensional structure significantly reduces overlap between graphene sheets compared to flat sheet-like graphene, allowing the large surface area of graphene to be effectively utilized. A plurality of protrusions or depressions (i.e., folds) are formed on the main surface (mainly the 002 plane (basal plane)) of the graphene sheet stack having a three-dimensional structure. Such a three-dimensional structure allows the distance between graphene sheets to be appropriately controlled, effectively reducing overlap between graphene sheets.
[0043] The three-dimensional structure may include a folded structure in which a graphene sheet having folds is bent. A single graphene sheet may be folded across the bent portion in a direction intersecting the plane of the sheet to form a laminate. The radius of curvature of the bent portion in the folded structure is, for example, in the range of 10 to 1000 nm. The spacing between the folds is, for example, in the range of 10 to 100 nm.
[0044] The bent structure in the three-dimensional structure includes, for example, a crimped structure or a folded structure in the sheet portion between the bent portions. In this case, each graphene sheet stack may have a microporous structure. This improves ion diffusion near the surface of the stack. The presence of the crimped structure or the folded structure (i.e., the pleated portion) can be confirmed by an electron microscope (SEM, TEM, etc.) photograph of the graphene sheet stack.
[0045] The crimped structure may be, for example, a structure having a plurality of randomly formed fold-like protrusions and depressions. The folded structure is a structure having a folded portion formed by partially folding a single graphene sheet laminate multiple times, and is included in the category of the crimped structure. The height of the protrusions or the depth of the depressions formed in the folded portion may be greater than the thickness of the carbon portion of the graphene sheet laminate having that structure, and may be at least twice the thickness of the carbon portion.
[0046] Graphene having such a three-dimensional structure may have a logarithmic differential pore distribution with a peak in the pore diameter range of 2 nm to 4 nm, and further have a distribution in which the volume increases quadratically with increasing pore diameter in the pore diameter range of 4 nm to 50 nm. The total pore volume of mesopores in the pore diameter range of 2 nm to 50 nm is, for example, 0.20 cm 3 / g or more. The total mesopore volume can be 0.20 cm 3 / g to 0.5 cm 3 / g range, 0.25 cm 3 / g to 0.4 cm 3 / g range, or 0.25 cm 3 / g ~ 0.35 cm 3 The total volume of pores with diameters of 4 nm to 50 nm may be, for example, 15 times or more the total volume of pores with diameters of 2 nm to 4 nm.
[0047] The specific surface area and pore size distribution of graphene can be measured using a BELSORP 28SA device available from BEL Japan Co., Ltd. The Dollimore Heal method (DH method), which is calculated based on the capillary condensation theory (Kelvin's equation), is used as the analytical theory for mesopores.
[0048] Graphene having such a three-dimensional structure can provide a capacitor electrode in which the logarithmic differential pore volume distribution measured with a mercury porosimeter has a maximum peak in the range of 0.3 μm or more and 6 μm or less. The three-dimensional structure significantly reduces overlapping of graphene sheets compared to flat sheet-like graphene, allowing the surface area of the graphene to be effectively utilized for ion adsorption. The three-dimensional structure, in which multiple protrusions or multiple depressions are formed on the basal surface, appropriately controls the distance between graphene sheets, effectively reducing overlapping of graphene sheets. Therefore, the number of active sites of the active material can be increased without suppressing ion migration (diffusion), resulting in high capacity.
[0049] The average number of layers in the graphene sheet stack is, for example, 10 or less, and may be 5 or less. The graphene sheet stack is preferably as close to the smallest unit of a graphene sheet (i.e., a single-layer sheet) having a thickness of one carbon atom.
[0050] The average number of layers is estimated from the interplanar distance (d002) calculated from the diffraction peak assigned to the 002 plane (basal plane) in the X-ray diffraction profile (see, for example, Abstracts of the 2015 Autumn Meeting of the Physical Society of Japan, p. 1014). Alternatively, it may be an estimated value obtained from an electron microscope (SEM, etc.) photograph of graphene. For example, the number of layers of graphene sheets can be estimated from the scale of the SEM photograph of graphene and the interplanar distance of the 002 plane (basal plane) of the graphene sheet. For example, 20 arbitrary graphene sheet laminates are selected, the number of layers of each is estimated, the fifth largest and the fifth smallest values are omitted, and the average of the 10 middle values is taken as the average number of layers.
[0051] The interlayer distance between graphene sheets (i.e., the distance between basal planes) may vary randomly. Random variation in the interlayer distance means that the graphene sheet stack has low crystallinity. The greater the disorder in the stacking structure in the stack, the more significant the variation in the interlayer distance.
[0052] The X-ray diffraction profile of graphene usually has a diffraction peak attributable to the 002 plane. The greater the overlap between graphene sheets and the higher the crystallinity of graphene, the sharper the diffraction peak becomes.
[0053] On the other hand, when graphene has a three-dimensional structure, the diffraction peak becomes broad and can be separated into multiple peaks. A halo pattern attributed to an amorphous phase may be observed at higher angles than the diffraction peak.
[0054] The interplanar distance d002 of the 002 planes of graphene calculated from the X-ray diffraction profile is 0.330 nm or more and 0.360 nm or less. d002 is calculated by waveform separation of diffraction peaks observed in the region around 2θ = 26.38°, calculating d002 for each component, and averaging the results. The distance d002 of the 002 planes of graphene is preferably 0.340 nm (3.40 Å) or more, more preferably 0.360 nm (3.60 Å) or more, and even more preferably 0.370 nm (3.70 Å) or more.
[0055] The electrolyte solution contains an ionic liquid. As the ionic liquid, a salt compound that exists in a liquid state at room temperature (25°C) and normal pressure (atmospheric pressure) can be preferably used. Examples of cations constituting the salt compound include imidazolium-based cations, pyrrolidinium-based cations, pyridinium-based cations, piperidinium-based cations, ammonium-based cations, and phosphonium-based cations. Examples of anions include halide ions (Cl - ,Br - etc.), tetrafluoroborate ion (BF 4 - ), hexafluorophosphate ion (PF 6 - ), bis(fluorosulfonyl)imide ion ((FSO 2 ) 2 N - ), bis(trifluoromethylsulfonyl)imide ion ((CF 3 SO 2 ) 2 N - ) etc.
[0056] Among these cations, the use of heteroaromatic ring-containing cations can achieve extremely high capacities. The reason for this is currently being elucidated, but possible reasons include the delocalized π orbitals of the aromatic rings easily bond with the π orbitals of graphene, forming a uniquely stable adsorption state, and the radical compounds generated by the reduction reaction can exist stably by adopting resonance structures, which also easily form a stable adsorption state with the π orbitals of graphene.
[0057] The anion is a tetrafluoroborate ion (BF 4 - When the anion contains hexafluorophosphate ions (PF), the F1s spectrum in an XPS analysis of the negative electrode surface may have a peak in the binding energy range of 686 to 692 eV. 6 - ) is also included, BF 4 - In the XPS analysis of the negative electrode surface, the F1s spectrum may have a peak in the binding energy range of 686 to 692 eV. By analyzing the B1s spectrum and the P1s spectrum, it is possible to determine whether the anion is BF 4 - or PF 6 - It is possible to determine whether the document contains either (or both) of the above.
[0058] The cation having a heteroaromatic ring may be an imidazolium cation, which may be a cation in which some of the hydrogen atoms in the imidazole skeleton are substituted with an alkyl group or the like.
[0059] Examples of imidazolium cations include cations having a heteroaromatic ring, such as 1-C 1-3 Alkyl-3-C 1-3 It may be an alkylimidazolium cation, more specifically, it may include a 1-ethyl-3-methylimidazolium cation. At least 80 mol % of the cations are 1-C 1-3 Alkyl-3-C 1-3 It may also be an alkylimidazolium cation or a 1-ethyl-3-methylimidazolium cation.
[0060] In order to adjust the viscosity of the electrolyte and improve the output characteristics, the ionic liquid may be mixed with a solvent and used as the electrolyte. As the solvent, any solvent (non-aqueous solvent) conventionally used as an electrolyte for capacitors can be used as long as it is uniformly mixed with the ionic liquid.
[0061] The non-aqueous solvent is preferably a high-boiling solvent, for example, lactones such as γ-butyrolactone, carbonates such as propylene carbonate, polyhydric alcohols such as ethylene glycol and propylene glycol, cyclic sulfones such as sulfolane, amides such as N-methylacetamide, N,N-dimethylformamide and N-methyl-2-pyrrolidone, esters such as methyl acetate, ethers such as 1,4-dioxane, ketones such as methyl ethyl ketone, and formaldehyde.
[0062] When the electrolytic solution contains a solvent other than the ionic liquid, the proportion of the ionic liquid in the entire electrolytic solution may be 75 mass % or more, or 80 mass % or more, or even 90 mass % or more.
[0063] The graphene having the above structure is used as an active material to produce a first electrode and / or a second electrode as a capacitor electrode. The capacitor electrode may contain a binder. The binder plays a role in assisting the bonding of graphene to graphene and the bonding of graphene to a current collector when the graphene having the above three-dimensional structure is formed into an electrode layer.
[0064] Hereinafter, an example of a method for producing graphene according to an embodiment of the present disclosure and a method for producing a capacitor electrode using the graphene produced thereby will be described.
[0065] <Graphene Production Method> (i) Dispersion Preparation Step First, an aqueous dispersion containing graphene oxide is prepared. The aqueous dispersion may contain, in addition to graphene oxide and water, a dispersant such as carboxymethyl cellulose (CMC). Graphene oxide can be produced, for example, by exfoliating graphite in a single layer or multilayer state via graphite oxidation.
[0066] Graphite can be oxidized using an oxidizing agent in water, for example. Examples of the oxidizing agent include sulfuric acid, potassium permanganate, chromic acid, sodium dichromate, sodium nitrate, peroxide, persulfate, and organic peracid. A water-soluble solvent may be added to the water. Examples of the water-soluble solvent include alcohols, ketones such as acetone, and ethers such as dioxane and tetrahydrofuran. An aqueous dispersion of graphene oxide is produced by the oxidation reaction in water.
[0067] The oxygen content of the graphene oxide may be, for example, 10 to 60 mass %, 20 to 50 mass %, or 30 to 50 mass %.
[0068] (ii) Reduction Step Next, reduced graphene oxide is produced by reducing the graphene oxide in an aqueous dispersion containing the graphene oxide (first reduction step). A preferred reduction method is hydrothermal treatment. For example, the aqueous dispersion may be sealed in an autoclave and subjected to hydrothermal treatment to produce a gel-like product. The temperature for the hydrothermal treatment may be, for example, 150°C or higher, preferably 170°C or higher and 200°C or lower.
[0069] Although reduced graphene oxide having a three-dimensional structure can be obtained by hydrothermal treatment alone, the gel-like product may be contacted with a reducing agent to further promote the reduction (second reduction step). Examples of reducing agents include metal hydrides, borohydrides, boranes, hydrazines or hydrazides, ascorbic acids, thioglycolic acids, cysteines, sulfites, thiosulfates, and dithionites. For example, the gel-like product may be immersed in an aqueous solution containing a water-soluble reducing agent such as sodium ascorbate. The temperature of the aqueous solution may be, for example, 20 to 110°C, 40 to 100°C, or 50 to 100°C. The amount of reducing agent used may be adjusted appropriately depending on the type of reducing agent, the oxygen content of the first carbon raw material (graphene oxide), the amount of gel-like product, and the like.
[0070] The gel product may then be freeze-dried. Freeze-drying can produce a dry gel (xerogel) in which the three-dimensional structure of graphene is highly maintained. Freeze-drying can be carried out, for example, at a temperature of −50° C. to 0° C., preferably −50° C. to −20° C., under a reduced pressure of 100 Pa or less, and further 1 Pa or less.
[0071] Next, the dried gel is thermally reduced in a non-oxidizing atmosphere to eliminate the remaining functional groups (third reduction step).
[0072] The non-oxidizing atmosphere may be a reduced pressure atmosphere (for example, 0.1 MPa or less (preferably 10 Pa or less)), a reducing atmosphere (for example, a hydrogen atmosphere of 0.01 MPa or less), or an inert gas atmosphere (for example, N 2 , a flow atmosphere of Ar, Ne, He, etc.) may also be used.
[0073] The heating temperature in the non-oxidizing atmosphere is 700°C or higher, and may be 800°C or higher, 900°C or higher, 1000°C or higher, or 1200°C or higher. However, there is a limit to how much the oxygen content of reduced graphene oxide can be reduced. Taking production costs into consideration, the heating temperature in the non-oxidizing atmosphere may be 1800°C or lower, 1400°C or lower, or 1200°C or lower. When specifying a temperature range, these upper and lower limits may be combined in any manner. The temperature range may be, for example, 1000°C to 1800°C.
[0074] The heating time in the non-oxidizing atmosphere is appropriately selected depending on the heating conditions and the amount of carbon to be treated, but may be, for example, about 0.1 to 5 hours.
[0075] The oxygen content of the dried gel after thermal reduction is less than 5% by mass, and may be 4% by mass or less, 3% by mass or less, preferably less than 2.6% by mass, 2% by mass or less, or 1.5% by mass or less. When the oxygen content is reduced to less than 5% by mass, the amount of reactants produced by the oxidation-reduction reaction between the oxygen-containing groups and the electrolyte components decreases. These reactants clog the pores of the electrode, reducing ion diffusibility and reducing ion adsorption sites. Therefore, the less reactants there are, the less ion diffusibility is reduced and the less ion adsorption sites are reduced, allowing for higher capacity.
[0076] The dried gel after thermal reduction is pulverized to obtain reduced graphene oxide powder (rGO powder).
[0077] The above method produces graphene (reduced graphene oxide) having a three-dimensional structure. The produced graphene can be used to produce a capacitor electrode, for example, by the following method.
[0078] <<Method for Manufacturing a Capacitor Electrode>> (iii) Electrode Formation Step For example, rGO powder and a binder are dispersed in a dispersion medium such as water to prepare a slurry. The obtained slurry is applied to a conductive substrate (current collector), and the coating is dried to form an electrode layer supported on the current collector, thereby obtaining a capacitor electrode. The electrode layer may then be rolled.
[0079] Examples of binders that can be used include fluororesins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), and vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), and water-soluble resins such as carboxymethyl cellulose (CMC), polyethylene oxide (PEO), polyethylene glycol (PEG), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyacrylic acid (PAA), and polyvinyl acetate.
[0080] The electrode layer may contain, in addition to the graphene, other active materials such as activated carbon. The electrode layer may also contain carbon particles such as carbon fibers, such as carbon nanotubes (CNTs), carbon black, and graphite. However, from the viewpoint of achieving both high capacity and high reliability, graphene preferably constitutes 50% by mass or more of the electrode layer, and more preferably 65% by mass or more.
[0081] The current collector may be made of a metal foil, a porous metal body, or the like. The current collector may be made of aluminum, copper, nickel, iron, stainless steel, platinum, or the like. An alloy containing these metals as its main component may also be used. The metal foil may be a plain foil, or may be a foil that has been roughened by etching or the like, or a foil that has been subjected to plasma treatment. The porous metal body may have, for example, a three-dimensional mesh structure.
[0082] The mass per unit area of the metal porous body is, for example, 500 g / m 2 or less, 150 g / m 2 The porosity of the metal porous body may be, for example, 80% by volume to 98% by volume, or may be 90% by volume to 98% by volume.
[0083] The average pore size of the pores in the metal porous body may be, for example, 50 μm or more and 1000 μm or less, or may be 400 μm or more and 900 μm or less, or 450 μm or more and 850 μm or less.
[0084] <<Capacitor>> Next, an example of an electrochemical capacitor including the above-described capacitor electrodes as a first electrode and a second electrode will be described. Fig. 1 is a partially cutaway perspective view of a capacitor 10.
[0085] The illustrated capacitor 10 includes a wound capacitor element 1. The capacitor element 1 is constructed by winding a first electrode 2 and a second electrode 3, each of which is sheet-shaped, with a separator 4 interposed therebetween. The first electrode 2 and the second electrode 3 each include a first current collector and a second current collector, each made of metal, with a first electrode layer and a second electrode layer supported on the surfaces thereof, respectively, and exhibit capacitance by adsorbing and desorbing ions. The first and second current collectors may be made of, for example, aluminum foil. The surfaces of the current collectors may be roughened by etching or other techniques. Lead wires 5 a and 5 b are connected to the first electrode 2 and the second electrode 3, respectively, as lead members. The capacitor element 1 is housed in a cylindrical outer case 6 together with an electrolyte (not shown). The outer case 6 may be made of a metal such as aluminum, stainless steel, copper, iron, or brass. The opening of the outer case 6 is sealed with a sealing member 7. The lead wires 5a and 5b are led out to the outside so as to pass through the sealing member 7. The sealing member 7 is made of a rubber material such as butyl rubber.
[0086] The electrode layer contains an active material as an essential component and may contain optional components such as a binder and a conductive additive. The active material includes, for example, graphene having the characteristics already described. The electrode layer can be obtained, for example, by kneading the active material, a binder (e.g., carboxymethyl cellulose (CMC)), and water in a kneader to obtain a slurry, applying the slurry to the surface of a current collector, drying the coating, and rolling it.
[0087] The separator preferably contains cellulose or a derivative thereof. Cellulose is stable against both acids and alkalis, even in environments where high voltages are applied. It also has high tensile strength, providing sufficient strength even when the first electrode and the second electrode are wound together to form a wound electrode group. The separator may be in the form of, for example, a microporous membrane, a woven fabric, or a nonwoven fabric. The thickness of the separator is, for example, 8 to 50 μm, preferably 12 to 35 μm, and more preferably 14 to 35 μm or 16 to 35 μm.
[0088] In the above embodiment, a wound type capacitor has been described, but the scope of application of the present invention is not limited to this, and it can also be applied to capacitors of other structures, such as stacked type or coin type capacitors.
[0089] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0090] Example 1 (1) Preparation of Capacitor Electrode Graphite was oxidized in water using potassium permanganate as an oxidizing agent to obtain graphene oxide. An aqueous dispersion containing 1% by mass of graphene oxide was subjected to hydrothermal treatment at 180°C for 6 hours to obtain a gel-like product (first reduction step).
[0091] Subsequently, the gel product was immersed in an aqueous solution of sodium ascorbate (sodium ascorbate concentration: 1.0 mol / L) as a reducing agent, heated to 100° C., and maintained at this temperature for 2 hours to fully reduce the carbon (second reduction step).
[0092] The gel product was then freeze-dried at -20°C under a reduced pressure of 100 Pa to obtain a xerogel. The xerogel was then heat-treated at 1200°C for 2 hours under a nitrogen flow (third reduction step). The heat-treated xerogel was pulverized to obtain reduced graphene oxide powder.
[0093] A slurry was prepared by dispersing 100 parts by mass of reduced graphene oxide powder and 10 parts by mass of CMC (a binder) in an appropriate amount of water. The slurry was applied to a 30 μm-thick Al foil current collector, and the coating was vacuum dried at 110°C and rolled to form an electrode layer, thereby obtaining a capacitor electrode.
[0094] (2) Capacitor Fabrication A pair of capacitor electrodes was prepared and punched into a 20 mm x 20 mm square. Lead wires were connected to each of the capacitor electrodes, and the capacitor electrodes were stacked with a cellulose nonwoven fabric separator sandwiched between them so that the coated surfaces of the electrode layers faced each other, yielding a laminated capacitor element. The capacitor element was then housed in an aluminum laminate outer case together with the electrolyte and sealed with a sealing material to complete the capacitor A1 of Example 1. The capacitor was then subjected to an aging treatment at 60°C for 6 hours while applying 2.5 V.
[0095] The electrolyte of the capacitor A1 was 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIBF), an ionic liquid. 4 ) was used.
[0096] Comparative Example 1 Physically exfoliated graphene obtained by physically exfoliating graphite was prepared. This physically exfoliated graphene was used as the active material instead of the reduced graphene oxide used in Example 1 to produce a capacitor electrode, and this capacitor electrode was used to obtain a capacitor element.
[0097] Other than this, the capacitor B1 of Comparative Example 1 was fabricated in the same manner as in Example 1.
[0098] The capacitors A1 and B1 were each evaluated as follows.
[0099] <Evaluation> The capacitance of each of the capacitors A1 and B1 was evaluated by the following method.
[0100] The manufactured capacitor is connected to a set voltage V 1 The battery was charged at a constant current of 0.1 to 1 A / g relative to the weight of the active material of the cell (the total mass of the positive electrode active material and the negative electrode active material) until the set voltage V 1 The battery was charged at a constant voltage of 0.5 V for 8 minutes.
[0101] After completion of the constant voltage charge, the cells were discharged at a constant current of 0.1 to 1 A / g relative to the weight of the cell active material to 0 V. The capacity was calculated from the slope of the voltage change during discharge until the voltage decreased from 2.1 V to 0.1 V. The capacity was calculated using the following formula, where I (A) is the constant current value during discharge and t (sec) is the discharge time until the voltage decreased from 2.1 V to 0.1 V.
[0102] Capacity (F) = It / (2.1 - 0.1) From the calculated capacity, the single electrode capacity was calculated assuming that the positive and negative electrode capacities (mass of the positive and negative electrode active materials) were the same, and the voltage V 1 Single electrode capacity C per 1 g of positive and negative electrode active material when 1 (F / g) was calculated.
[0103] Set voltage V 1 While changing the voltage from 2.8 V to 5.0 V, the single electrode capacity C per 1 g of the positive and negative electrode active material was measured in the same manner. 1 (F / g) was calculated, and the single-electrode capacity C 1 Voltage V 1 The results are shown in the graph in Figure 2.
[0104] Furthermore, V 1 After completing the charging at V = 4.4 V, the negative electrode was removed from the capacitor. The removed negative electrode was washed with dimethyl carbonate and then dried. The dried negative electrode surface was subjected to XPS quantitative analysis, and the ratio R F and R B The results are shown in Table 1.
[0105]
[0106] From the graph of FIG. 2, the applied voltage V 1 As the voltage is increased to 4.0 V or more, the monoelectrode capacity C 1 On the other hand, in the capacitor B1, the monopole capacitance C 1 is smaller than that of the capacitor A1, and the applied voltage V 1 Even if the voltage is increased to 4.0 V or more, the single-electrode capacity C 1 The increase is small.
[0107] From Table 1, in the capacitor A1, the ratio R of F to C present on the negative electrode surface is F is large, more than 10%, and the ratio of B to C, R B The ratio R F and the ratio R B In capacitor B1, only minute amounts of B and F are present on the surface of the negative electrode, and it can be seen that no increase in capacity due to oxidation-reduction reactions occurs.
[0108] Figure 3 shows the F1s spectra of the negative electrode surfaces of capacitors A1 and B1 in XPS analysis. Capacitors A1 and B1 both show peaks in their F1s spectra, but the peak of capacitor B1 is smaller than that of capacitor A1 and the peak position is different. This is because the peak appearing in the F1s spectrum of capacitor B1 is due to BF present near the negative electrode surface. 4 - In contrast, in the capacitor A1, the peak appearing in the F1s spectrum is due to EMI. + The reaction product of the reduced cation is further treated with BF 4 - This is thought to be due to the by-products of the reaction with , and is thought to be due to the different bonding state of F.
[0109] According to the present invention, an electrochemical capacitor with high energy density can be obtained.
[0110] 1: capacitor element, 2: first electrode, 3: second electrode, 4: separator, 5a: first lead wire, 5b: second lead wire, 6: exterior case, 7: sealing member, 10: capacitor
Claims
1. A semiconductor device comprising: a first electrode including a first active material; a second electrode including a second active material; and an electrolyte, the electrolyte including an ionic liquid; and when a surface of the first electrode is quantitatively analyzed by X-ray photon spectroscopy (XPS) based on a relative sensitivity coefficient, an atomic ratio R of an element F derived from the ionic liquid to an element C is 1.0 to 1.0 atomic ratio R of an element F derived from the ionic liquid to an element C is 1.0 to 1.0 atomic ratio R of an element C derived from the ionic liquid to an element F derived from the ionic liquid. F is 10% or more.
2. The atomic ratio R F The electrochemical capacitor according to claim 1 , wherein the capacitance is 14% or more.
3. When the surface of the first electrode is quantitatively analyzed based on a relative sensitivity coefficient by using X-ray photon spectroscopy (XPS), the atomic ratio R of element B to element C is B The electrochemical capacitor of claim 1 , wherein the capacitance is 1% or more.
4. The electrochemical capacitor according to any one of claims 1 to 3, wherein a lower potential is applied to the first electrode than to the second electrode.
5. The electrochemical capacitor according to claim 4, wherein a voltage of 4.0 V or more is applied between the first electrode and the second electrode.
6. The electrochemical capacitor according to any one of claims 1 to 3, wherein the first active material includes reduced graphene oxide.
7. The electrochemical capacitor according to any one of claims 1 to 3, wherein the ionic liquid contains a cation having a heteroaromatic ring.
8. The electrochemical capacitor of claim 7, wherein the cation comprises a 1-ethyl-3-methylimidazolium cation.
9. The electrochemical capacitor according to any one of claims 1 to 3, wherein the ionic liquid contains tetrafluoroborate anions.
Citation Information
Patent Citations
Electrode film for electric double-layer capacitor and production method therefor
WO2013168762A1
Electrode for capacitor, manufacturing method therefor, and capacitor
WO2022065493A1