Silicon nitride powder and resin composition using same

By optimizing the angle of repose and compaction of silicon nitride powder, its adhesion to other members is reduced, enhancing thermal diffusivity in resin compositions for improved heat dissipation.

WO2024202728A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO CHEM CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006269
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Silicon nitride powder tends to adhere to other members when used as a filler in resin compositions, which hampers its effectiveness in heat dissipation applications.

Method used

The silicon nitride powder is characterized by an angle of repose greater than 40°, a degree of compaction less than 34.4%, and specific particle size distribution, which reduces adhesion and enhances thermal diffusivity when used in a resin composition.

Benefits of technology

The modified silicon nitride powder effectively suppresses adhesion to other members and improves the thermal diffusivity of the resin composition, allowing for more efficient heat dissipation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This silicon nitride powder contains a plurality of silicon nitride particles and has a repose angle of more than 40°.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon nitride powder and resin composition using same

[0001] The present disclosure relates to a silicon nitride powder and a resin composition using the same.

[0002] Heat generated by passing current through an electronic component is dissipated via a heat sink. To improve heat dissipation efficiency, a technique for filling the space between the electronic component and the heat sink with a heat dissipation material is known. One heat dissipation material is a resin composition containing a resin and inorganic particles, and it is known that silicon nitride powder can be used as the inorganic particles (see, for example, Patent Document 1).

[0003] Patent Document 1 discloses a low-aluminum spherical β-silicon nitride powder for use as a filler in electronic packaging materials. The silicon nitride powder is characterized by a sphericity of 0.5 to 0.99, an Al impurity content of less than 500 ppm, and a particle size range of 0.5 μm to 50 μm.

[0004] Patent Document 2 discloses a method for producing silicon nitride powder suitable for producing silicon nitride sintered bodies, and silicon nitride powder obtained by said method. The silicon nitride powder has an average particle size of 1 to 50 μm, a metal oxide content of 0 to 10 wt %, and an impurity content of less than 1 wt %, preferably the metal oxide content in the silicon nitride powder is less than 1 wt %, and the sintered body has a thermal conductivity of 90 W / mK or more and a bending strength of 700 MPa or more, and preferably the sintering conditions for the sintered body are as follows: the silicon nitride powder is mixed with MgO, Y 2 O 3 The powder is mixed with the above powder, polished, and the powder is dry-press molded, and the powder is gas-pressure sintered at 1900°C and a nitrogen gas pressure of 1 MPa for 8 hours.

[0005] Patent Document 3 discloses a silicon nitride powder suitable for producing a highly thermally conductive silicon nitride sintered body. The silicon nitride powder is characterized by having a β fraction of 30 to 100%, an oxygen content of less than 0.5 wt%, an average particle size of 0.2 to 10 μm, an aspect ratio of 10 or less, and containing columnar particles with grooves formed in the long axis direction of the particle.

[0006] JP 2022-522814 A JP 2022-541208 A JP 2004-262756 A

[0007] As described above, while silicon nitride powder is increasingly being used, when attempts were made to further improve its productivity, it was discovered that silicon nitride powder has a problem in that it tends to adhere to other components.

[0008] In view of these circumstances, an object of one embodiment of the present invention is to provide a silicon nitride powder for use as a filler for a resin composition, which is capable of suppressing adhesion to other components. Furthermore, an object of another embodiment of the present invention is to provide a resin composition using the silicon nitride powder.

[0009] A first aspect of the present invention is a silicon nitride powder comprising a plurality of silicon nitride particles, the silicon nitride powder having an angle of repose of greater than 40°.

[0010] A second aspect of the present invention is the silicon nitride powder according to the first aspect, wherein the degree of compression is less than 34.4%.

[0011] A third aspect of the present invention is the silicon nitride powder according to the first or second aspect, wherein the difference between the particle diameter D90 at 90% cumulative from the fine side of the volume-based cumulative particle size distribution and the particle diameter D10 at 10% cumulative from the fine side of the volume-based cumulative particle size distribution is 150.0 μm or less.

[0012] A fourth aspect of the present invention is the silicon nitride powder according to any one of the first to third aspects, wherein the silicon nitride particles have an average aspect ratio of their minor axis to their major axis of greater than 0.50.

[0013] A fifth aspect of the present invention is the silicon nitride powder according to any one of the first to fourth aspects, wherein the ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge is 1% or less, and the maximum particle size of the silicon nitride particles is 6.8 μm or more.

[0014] A sixth aspect of the present invention is a resin composition comprising a resin and the silicon nitride powder according to any one of the first to fifth aspects.

[0015] According to one embodiment of the present invention, it is possible to provide silicon nitride powder that can suppress adhesion to other members.

[0016] [Silicon Nitride Powder] The present inventors conducted research from various perspectives to realize a silicon nitride powder that can suppress adhesion to other components, and focused on the angle of repose. A common approach to suppress adhesion to other components is to lower the angle of repose to improve fluidity. However, the present inventors discovered that by increasing the angle of repose to a predetermined value or higher, the silicon nitride powder becomes more easily aggregated, resulting in less adhesion to other components (e.g., polystyrene components). Details of each requirement stipulated in the embodiments of the present invention are provided below.

[0017] (Angle of repose) The silicon nitride powder according to an embodiment of the present invention comprises a plurality of silicon nitride particles and has an angle of repose of more than 40°. This reduces adhesion to other components (e.g., polystyrene components). Furthermore, by setting the angle of repose within the above range, the silicon nitride powder in a resin composition containing the silicon nitride powder tends to aggregate to some extent and form a thermal diffusion path, thereby improving the thermal diffusivity of the resin composition. The angle of repose is preferably 41° or more. On the other hand, the angle of repose is preferably 60° or less. This allows the silicon nitride powder to maintain a certain degree of fluidity, making it easier to disperse the silicon nitride powder in the resin composition and improving the thermal diffusivity of the resin composition. The angle of repose is more preferably 58° or less, even more preferably less than 56°, even more preferably 50° or less, even more preferably 47° or less, and particularly preferably 45° or less.

[0018] The angle of repose of silicon nitride powder is measured in accordance with the description of JIS R 9301-2-2: 1999. The ambient atmosphere during the angle of repose measurement is set to a temperature of 23°C and a humidity of 40%.

[0019] (Degree of Compression) The silicon nitride powder according to the embodiment of the present invention preferably has a degree of compression of less than 34.4%. This improves the fluidity of the silicon nitride powder, allowing the silicon nitride powder to be better dispersed in the resin composition, and further improving the thermal diffusivity of the resin composition. The degree of compression is more preferably 34.0% or less, even more preferably less than 33.6%, even more preferably less than 24.1%, and particularly preferably 17.0% or less. On the other hand, the degree of compression is preferably 3.0% or more, which makes the silicon nitride powder less likely to scatter. The degree of compression is more preferably 5.0% or more, even more preferably 7.0% or more, and even more preferably 8.0% or more.

[0020] The degree of compression of the silicon nitride powder was measured by measuring the tap density in accordance with JIS Z2512:2012 "Metal powder - Tap density measurement method", and the bulk density before tapping was calculated as D 0 (g / cm 3 ) and the bulk density after tapping (i.e., tap density) is D 1 (g / cm 3 ) and then (D 1 -D 0 ) / D 1 It is calculated as follows.

[0021] The bulk density after tapping (i.e., tap density) D 1 (g / cm 3 A high tap density means that the silicon nitride powder can be densely packed. Furthermore, if a resin composition is formed using silicon nitride powder with a high tap density, it is expected that a larger amount of silicon nitride powder can be kneaded, thereby increasing the thermal diffusivity of the resin composition. 1 is 0.54 g / cm 3 It is preferable that the density is greater than 1.00 g / cm 3 More preferably, it is 1.17 g / cm 3 On the other hand, by keeping the tap density low to a certain extent, the particles are less likely to be compressed together, and the dispersibility can be improved. 1 is 2.00 g / cm 3 It is preferable that the density is 1.90 g / cm or less. 3More preferably, it is 1.80 g / cm or less. 3 The bulk density D before tapping is more preferably less than 10 ... 0 (g / cm 3 ) is not particularly limited, but is, for example, 0.35 to 1.60 g / cm 3 It could be.

[0022] (Difference between particle diameter D90 at 90% cumulative from the fine particle side of the volume-based cumulative particle size distribution and particle diameter D10 at 10% cumulative from the fine particle side of the volume-based cumulative particle size distribution) Silicon nitride powders with a sharp particle size distribution are preferred because they are easy to use as fillers for resin compositions and increase the selectivity and flexibility when mixing with other powders (particles). For example, the difference between particle diameter D90 at 90% cumulative from the fine particle side of the volume-based cumulative particle size distribution (hereinafter sometimes simply referred to as "D90") and particle diameter D10 at 10% cumulative from the fine particle side of the volume-based cumulative particle size distribution (hereinafter sometimes simply referred to as "D10") is preferably 150.0 μm or less. More preferably, it is 130.0 μm or less. As described above, the difference between D90 and the particle size D50 (hereinafter sometimes simply referred to as "D50") of the cumulative 50% from the fine particle side of the volume-based cumulative particle size distribution is preferably 100.0 μm or less, and more preferably 80.0 μm or less.

[0023] On the other hand, if the particle size distribution of the silicon nitride powder is broad to a certain extent, the filling ability is improved by allowing small particles to enter the gaps between large particles, and more silicon nitride powder can be kneaded into the resin, which can contribute to improving the thermal diffusivity of the resin composition. Therefore, the difference between D90 and D10 is preferably 3.0 μm or more, more preferably greater than 3.3 μm, even more preferably greater than 6.6 μm, even more preferably 20.0 μm or more, and particularly preferably 40.0 μm or more. As above, the difference between D90 and D50 is preferably 1.5 μm or more, more preferably greater than 2.0 μm, even more preferably greater than 5.0 μm, even more preferably greater than 5.5 μm, even more preferably 20.0 μm or more, and particularly preferably 25.0 μm or more.

[0024] The D90, D50, and D10 of silicon nitride powder are measured by laser diffraction. Specifically, the powder dispersed in water is irradiated with a laser beam, and the diffraction is measured to determine each particle size. A measuring device such as the 1090L manufactured by CILAS can be used.

[0025] (Average aspect ratio of silicon nitride particles) The average aspect ratio of the minor axis to the major axis of the silicon nitride particles contained in the silicon nitride powder is preferably greater than 0.50, more preferably greater than 0.60, and even more preferably 0.65 or more. On the other hand, the average aspect ratio of the silicon nitride particles is preferably less than 0.87, more preferably 0.86 or less, and even more preferably 0.85 or less. When the average aspect ratio of the silicon nitride particles is within an appropriate range, the filling rate in the resin composition can be further improved, and a resin composition with a higher thermal diffusivity can be obtained.

[0026] The average aspect ratio of silicon nitride particles is measured as follows. SEM images of silicon nitride particles contained in silicon nitride powder are analyzed using image processing software (e.g., Image J (manufactured by the National Institute of Health)). The maximum particle size of the silicon nitride particles (referred to as the "major axis") is identified, and the particle size in the direction perpendicular to the major axis is referred to as the "minor axis". The major and minor axes are measured for 20 random silicon nitride particles, and the ratio of the minor axis to the major axis (minor axis / major axis) is determined for each particle. The arithmetic mean value of these ratios is taken as the average aspect ratio of the silicon nitride particles.

[0027] (The maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundaries to the outer edge length L1 of 1% or less is 6.8 μm or more.) The fewer grain boundaries and cavities there are inside the silicon nitride particles, the more this can contribute to improving the thermal diffusivity of the silicon nitride particles. Therefore, the ratio (L2 / L1) of the total length L2 of the boundaries to the outer edge length L1 is introduced as an indicator of the content of grain boundaries inside the silicon nitride particles. L1 and L2 are determined by observing the cross section of the silicon nitride particle. Note that here, "grain boundary" and "boundary line" refer to boundaries (also called high-angle grain boundaries) where, as a result of EBSD analysis, the crystal orientation misorientation (oblique angle) exceeds 15°.

[0028] When the length of the outer edge of one silicon nitride particle is L1 and the total length of the boundary lines of that silicon nitride particle is L2, silicon nitride particles with a small L2 / L1 value are said to have a low content of boundary lines. In this embodiment, silicon nitride particles with an L2 / L1 ratio of 1% or less are considered to be silicon nitride particles made of a single crystal (referred to as "single crystal particles"). Single crystal particles have a high thermal diffusivity, so they are likely to improve thermal diffusivity when used as a filler for resin compositions.

[0029] In this embodiment, the maximum particle size of silicon nitride particles having an L2 / L1 ratio of 1% or less (i.e., single crystal) is preferably 6.8 μm or more, more preferably 10.0 μm or more, even more preferably 15.0 μm or more, still more preferably 30.0 μm or more, even more preferably 45.0 μm or more, and particularly preferably 55.0 μm or more. Such silicon nitride particles form long heat conduction paths when filled into a resin, thereby improving the thermal diffusivity of the resin composition.

[0030] (β-phase ratio) The β-phase ratio of the silicon nitride powder is preferably 65% ​​or more. A β-phase ratio of 65% or more can improve the thermal diffusivity of the silicon nitride powder and the resin composition. The β-phase ratio is more preferably 70% or more, even more preferably 80% or more, even more preferably 85% or more, and particularly preferably 90% or more.

[0031] In this specification, the "β-phase ratio" refers to the content (volume %) of β-type silicon nitride relative to all silicon nitrides contained in the silicon nitride powder.

[0032] In calculating the β-phase ratio, a diffraction pattern of silicon nitride powder was obtained by powder X-ray diffraction (X-ray source: CuKα ray), and the diffraction pattern was analyzed by the Gazzara & Messier method (G.P. Gazzara and D.P. Messier, "Determination of Phase Content of Si 3 N 4The β-phase ratio is calculated by analyzing the β-phase by X-ray Diffraction Analysis, Am. Ceram. Soc. Bull., 56[9]777-80 (1977)).

[0033] [Method for Producing Silicon Nitride Powder] The silicon nitride powder according to an embodiment of the present invention can be produced by a production method comprising the steps of: (1) synthesizing silicon nitride synthetic crystals by combustion synthesis in a nitrogen atmosphere using raw materials containing Si; (2) crushing the silicon nitride synthetic crystals to obtain coarsely pulverized silicon nitride powder; and (3) finely pulverizing the coarsely pulverized silicon nitride powder to obtain finely pulverized silicon nitride powder. Optionally, the method may further comprise the step of: (4) heat-treating the finely pulverized silicon nitride powder. Each step is described in detail below.

[0034] Step (1): Synthesizing silicon nitride composite crystals. For example, Si powder is used as the raw material containing Si. The average particle diameter D50 of the raw material is, for example, within the range of 2 to 10 μm. This allows the amount of oxygen impurities to be suppressed, and the combustion rate to be increased, allowing for a higher synthesis temperature, resulting in good crystal growth. As an example, the average particle diameter D50 of Si is 5 μm.

[0035] The diluent is used to adjust the amount of Si in the raw materials. A separately prepared silicon nitride powder is used as the diluent. The diluent may be either α-type silicon nitride powder or β-type silicon nitride powder, or a mixture of these. The average particle diameter D50 of the diluent is preferably in the range of 0.5 to 2.0 μm. For example, the average particle diameter D50 of the diluent is 1.0 μm. The amount of diluent added is less than 10% by mass of the total raw materials (including the diluent). For example, the diluent is added in an amount of 5 to 8% by mass of the total raw materials. By adding the amount of diluent within the above range, it becomes easier to obtain silicon nitride powder with the desired angle of repose, compressibility, etc.

[0036] In this embodiment, a diluent is mixed with the raw materials and filled into an insulated heat-resistant container. This insulated heat-resistant container has a thermal conductivity of 1 W / mK or less, and although alumina or zirconia can be used as the material, carbon is preferred in consideration of the risk of impurities being mixed in. After the raw materials are filled, the container is covered with a lid made of the same material as the insulated heat-resistant container. Furthermore, to increase the temperature inside the composite during combustion, the thickness of the mixed raw materials is set to more than 100 mm, preferably more than 100 mm and not more than 150 mm. Combustion synthesis is performed under a nitrogen atmosphere in the range of 0.5 to 1 MPa (e.g., 0.9 MPa). Adjusting the pressure range within the above range enables efficient synthesis while suppressing increases in equipment costs.

[0037] When the mixed raw material is filled into the crucible, a layer of powder (silicon nitride) having a thickness of 1 mm to 80 mm is laid on the bottom and sides of the crucible, the mixed raw material is then filled, and the top surface is covered with a layer of powder having a thickness of 1 mm to 80 mm. The thickness of the powder is 100 mm or less, preferably 1 mm to 80 mm. Covering the powder with the powder keeps the mixed raw material warm, making it easier to obtain silicon nitride powder having the desired angle of repose, compressibility, etc.

[0038] To promote crystal growth more effectively, a catalyst may be used, for example, Y 2 O 3 , Fe 2 O 3 , CaO, Ni, Co, C, etc. are added in an amount of about 0.01 to 0.1 mass %. In addition, external auxiliary heating is performed in the range of 500°C to 1700°C (for example, 1500°C), and the combustion temperature is also increased in the combustion synthesis method by self-ignition.

[0039] Step (2): Obtaining a coarsely pulverized silicon nitride powder. The silicon nitride composite crystal is in the form of an agglomeration of multiple silicon nitride particles. In step (2), the silicon nitride composite crystal is crushed to obtain a coarsely pulverized silicon nitride powder. For example, the composite is crushed using a common crushing device such as a hammer mill or a disk mill until it passes through a sieve with a specified mesh size (for example, a sieve with mesh sizes in the range of 400 μm to 500 μm).

[0040] Step (3): Obtaining a finely pulverized silicon nitride powder The coarsely pulverized silicon nitride powder is further pulverized to obtain a finely pulverized silicon nitride powder. The pulverization is carried out using a pulverizing device such as a jet mill or a ball mill. If necessary, the obtained finely pulverized powder may be classified. Classification can be carried out by sieving, wet classification, or the like.

[0041] Step (4): Heat-treating the finely pulverized silicon nitride powder. Optionally, the finely pulverized silicon nitride powder may be heat-treated. Heat treatment forms an oxide film on the surface of the silicon nitride particles, which has the effect of chemically stabilizing the silicon nitride particles. The heat treatment is carried out, for example, in air at a temperature of 500°C or higher and 1200°C or lower. The heat treatment time can be adjusted appropriately according to the heat treatment temperature. The heat treatment time is, for example, 5 hours.

[0042] In the method for producing silicon nitride powder, silicon nitride synthetic crystals are synthesized using the heat generated by combustion synthesis, and then the silicon nitride powder according to this embodiment can be produced by crushing, classifying, and pulverizing the synthesized crystals.

[0043] [Resin Composition] The resin composition according to the embodiment of the present invention contains a resin and the silicon nitride powder according to the embodiment of the present invention. The resin / silicon nitride powder blending ratio of the resin composition according to the embodiment of the present invention can be appropriately determined depending on the purpose and / or application. As an example, the resin composition (composite) may contain 5 to 75 volume % of resin and 95 to 25 volume % of silicon nitride powder. The filling rate of the silicon nitride powder in the resin composition refers to the content (vol %) of the silicon nitride powder when the volume of the resin composition (including the silicon nitride powder) is taken as 100 volume %.

[0044] A method for producing a resin composition will be described. A resin composition can be obtained by mixing silicon nitride powder and a resin using a commonly used known method. For example, when the resin is liquid (e.g., liquid epoxy resin), the resin composition can be obtained by mixing the liquid resin, silicon nitride powder, and a curing agent, and then curing the mixture with heat or ultraviolet light. Known curing agents, mixing methods, and curing methods can be used. On the other hand, when the resin is solid, the desired resin composition can be obtained by mixing the silicon nitride powder and the resin, and then kneading the mixture using a known method such as melt kneading.

[0045] The resin used in the resin composition can be a known resin such as an epoxy resin. The type of resin can be selected from thermoplastic resins, thermoplastic elastomers, and thermosetting resins. The resins can be used alone or in combination of two or more.

[0046] Furthermore, these resin compositions may contain, as needed, known additives such as plasticizers, curing accelerators, coupling agents, fillers, pigments, flame retardants, antioxidants, surfactants, compatibilizers, weather resistance agents, antiblocking agents, antistatic agents, leveling agents, and release agents, either singly or in combination, within the scope of the invention.

[0047] The silicon nitride powder according to the embodiment and the resin composition containing the silicon nitride powder are particularly suitable for use as heat-dissipating materials. Thus, one aspect of the present disclosure can provide a heat-dissipating silicon nitride powder and a heat-dissipating resin composition.

[0048] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples carried out to clarify the effects of the embodiments of the present invention. However, the embodiments of the present invention are not limited to the following examples.

[0049] <Preparation of Silicon Nitride Powder> Si powder (particle size = 5 μm) and silicon nitride powder (particle size = 1 μm) prepared separately as a diluent were mixed in a tumbling ball mill. The amount of diluent added was 5 to 8 mass% of the total raw materials (including diluent). The mixed powder was filled into a carbonaceous, heat-resistant container with a layer of powder 1 mm to 80 mm thick on the bottom and sides, so that the raw material layer was thicker than 100 mm and not more than 150 mm. The raw material layer was then covered with a layer of powder 1 mm to 80 mm thick. A lid made of a carbonaceous, heat-resistant material was then placed in the container, and synthesis was carried out under a nitrogen atmosphere at 0.9 MPa. After synthesis, the mixture was coarsely crushed (disintegrated) in a mortar until it passed through a sieve with the specified mesh size. The mesh size of the sieve for each sample is shown in Table 1.

[0050] (Samples Nos. 1 to 3) The obtained coarsely pulverized powder was further finely pulverized using a nanojetmizer (manufactured by Aisin Nano Technologies Co., Ltd.). For the fine pulverization, a nanojetmizer with the model number shown in Table 1 was used. The obtained finely pulverized powder was classified using the method shown in Table 1. Note that a portion of the finely pulverized powder (referred to as Sample No. 2) was not classified. Thereafter, the obtained classified powders (Samples Nos. 1 and 3) and the finely pulverized powder (Sample No. 2) were placed in an alumina crucible and heat-treated in an air atmosphere using a small powder programmable electric furnace (MMF series, manufactured by AS ONE) under the conditions (heat treatment temperature, heat treatment time) shown in Table 1 to obtain silicon nitride powders (Samples Nos. 1 to 3).

[0051] (Samples No. 5 to 10) Coarsely pulverized powders were prepared in the same manner as in "Samples No. 1 to 3" above. The sieve used during coarse pulverization (disintegration) had a mesh size of 500 μm. The obtained coarsely pulverized powders were then finely pulverized in a ball mill. The obtained finely pulverized powders were subjected to sieve classification using a vibrating sieve according to the following procedure, and then further subjected to wet classification to obtain silicon nitride powders (Samples No. 5 to 10) having the desired D50. - Powder remaining on the sieve when sieving using a 150 μm sieve (Sample No. 5, D50 was 192.0 μm) - Powder remaining on the sieve when sieving using a 150 μm sieve and then sieving the powder remaining below the sieve using a 106 μm sieve (Sample No. 6, D50 was 118.0 μm) - Powder remaining on the sieve when sieving using a 106 μm sieve and then sieving the powder remaining below the sieve using a 75 μm sieve (Sample No. 7, D50 was 83.0 μm) The powder remaining on the sieve after sieving using a 75 μm sieve and then sieving it further using a 63 μm sieve (sample No. 8, D50 was 58.0 μm). The powder remaining on the sieve after sieving using a 63 μm sieve (sample No. 9, D50 was 22.0 μm). The powder remaining on the sieve after sieving the powder of sample No. 9 using a 10 μm sieve (sample No. 10, D50 was 3.5 μm).

[0052]

[0053] Various measurements were performed on the obtained Samples Nos. 1 to 3 and 5 to 10 (Examples) and, as a comparative example, a commercially available silicon nitride powder (manufactured by Aldrich, silicon nitride (predominantly β-phase, ≦10 micron primary particle size, product code 248622); hereinafter referred to as “Sample No. 4”).

[0054] (1) Angle of Repose The angle of repose of a sample (silicon nitride powder) was measured in accordance with the description of JIS R 9301-2-2: 1999. The amount of sample used for measuring the angle of repose was 20 ml, and the ambient atmosphere was a temperature of 23°C and a humidity of 40%.

[0055] (2) Compressibility The compressibility of the sample (silicon nitride powder) was measured for tap density in accordance with JIS Z2512:2012 "Metal powder - Tap density measurement method", and the bulk density before tapping was D 0 The bulk density after tapping (i.e., tap density) is D 1 As such, (D 1 -D 0 ) / D 1 It was calculated by:

[0056] (3) (D90-D10) and (D90-D50) The particle size distribution of the sample (silicon nitride powder) was measured to determine D90, D50, and D10, and these were used to calculate (D90-D10) and (D90-D50). The particle size distribution of the silicon nitride powder was measured by laser diffraction. A sample dispersed in water was irradiated with a laser beam, and the diffraction was measured to determine the particle size. The measuring device used was a CILAS 1090L model. The particle size was taken as the circle-equivalent particle size. The circle-equivalent particle size is the particle size of a perfect circle that has the same area as a projected particle image. The particle size was measured by volume.

[0057] (4) Average aspect ratio of silicon nitride particles SEM images of the sample (silicon nitride powder) were taken. The following equipment was used for taking the images. Equipment used: Scanning electron microscope: JSM-IT200 (manufactured by JEOL Ltd.) The imaging conditions were as follows: Acceleration voltage: 5.0 kV Signal: SED Probe current: Std. -PC55 Magnification: 1000x

[0058] The SEM images were processed using image processing software Image J (manufactured by the National Institute of Health), and the aspect ratios of 20 randomly selected silicon nitride particles in the SEM images were determined. The maximum diameter of the silicon nitride particles was taken as the major axis, and the particle size in the direction perpendicular to the major axis was taken as the minor axis. The major and minor axes of 20 randomly selected silicon nitride particles were measured, and the ratio of the minor axis to the major axis (minor axis / major axis) was determined for each particle. The arithmetic mean value of these ratios was taken as the average aspect ratio of the silicon nitride particles (referred to as "aspect ratio" in Table 2).

[0059] (5) Maximum particle size of silicon nitride particles with an L2 / L1 ratio of 1% or less (maximum particle size of single-crystal particles) A ​​cross-sectional observation specimen was prepared using the sample (silicon nitride particles). To prepare the cross-sectional observation specimen, the silicon nitride particles were embedded in resin, and then the resin and silicon nitride particles were cut using a diamond cutter. Subsequently, a protective film of platinum was vapor-deposited on the cross-section, and the cross-section was prepared by Ar ion milling. The specimen was then fixed to the SEM sample stage with Cu double-sided tape, and SEM-EBSD measurement was performed without vapor deposition. The observation position was determined so that two or more silicon nitride particles were completely contained within the observation region (i.e., two or more silicon nitride particles did not come into contact with the frame of the observation region). Measurements were performed using β-type silicon nitride particles.

[0060] The following equipment was used for sample pretreatment and EBSD measurement: Equipment used Ion milling equipment: E-3500 (manufactured by Hitachi High-Tech Corporation) Ion sputtering equipment: E-1030 (manufactured by Hitachi, Ltd.) Schottky scanning electron microscope: SU5000 (manufactured by Hitachi High-Tech Corporation) Backscattered electron diffraction equipment: Velocity (manufactured by METEK Corporation)

[0061] The conditions for the EBSD measurement were as follows: Measurement area: 500.0 μm×400.0 μm Acceleration voltage: 15.0 kV Magnification: ×500 Vacuum degree: 30 Pa

[0062] In the obtained EBSD image, two or more silicon nitride particles that were not in contact with the frame of the observation area were selected, and the average of the outer edge length L1 of each silicon nitride particle was calculated using image processing software Image J (manufactured by the National Institute of Health). The total length L2 of the boundary lines was also calculated. The "total length L2 of the boundary lines" is the sum of the boundary lines contained within the silicon nitride particle and does not include the outer edge of the silicon nitride particle. The total length L2 of the boundary lines was calculated by adding the total length of the grain boundaries within the silicon nitride particle and the total length of the inner wall of the cavity (if there was a cavity within the silicon nitride particle). Note that here, "grain boundary" and "boundary line" refer to boundaries (also called high-angle grain boundaries) where the crystal orientation misorientation (oblique angle) exceeds 15° as a result of EBSD analysis.

[0063] This measurement was performed once for 20 random silicon nitride particles. Silicon nitride particles with an L2 / L1 ratio of 1% or less were considered to be single crystal particles, and the length of their major axis was measured and defined as the "maximum particle size of the single crystal particles." If the 20 silicon nitride particles measured contained multiple single crystal particles, the arithmetic average of their maximum particle sizes was calculated. (6) β-Proportion A diffraction pattern of the sample (silicon nitride powder) was obtained using a powder X-ray diffractometer (manufactured by Rigaku Denki). The measurement conditions were as follows: X-ray source: CuKα radiation X-ray output: 45 kV, 200 mA Graphite monochromator Diffraction angle (2θ): Step scan in 0.02° increments in the range of 2 to 90° Scanning speed: 21.7 deg / min

[0064] When a sample contained components other than silicon nitride, the peaks of those components were compared with the corresponding peaks of standard samples of those components to determine the proportions of those components. For Samples No. 1 to 4, the powder X-ray diffraction patterns obtained confirmed that the sample consisted solely of α-type silicon nitride and β-type silicon nitride. The proportion of β-type silicon nitride in the sample (β-conversion ratio) was then calculated using the Gazzara & Messier method.

[0065] (7) Adhesion to other materials Polystyrene medicine spoon (medicine spoon surface area: 236 mm 2 ), one scoop (1 g) of sample (silicon nitride powder) was scooped out and placed in another container, and the adhesion of the powder to the surface of the medicine spoon was evaluated as follows: ○: Powder adhesion area is 5 mm 2 x: Powder adhesion area is less than 5 mm 2 That's all

[0066] (8) Thermal diffusivity of resin composition (composite) Epoxy resin (main agent: room temperature curing potting resin 53 type (manufactured by Sankei Co., Ltd.) 010-8140, curing agent: room temperature curing potting resin 53 type (manufactured by Sankei Co., Ltd.) 010-8143) and a sample (silicon nitride powder) were mixed in a blending ratio (volume ratio) of 50:50, and the mixture was stirred and mixed using a Foam Mixer (manufactured by Thinky Corporation) to obtain an epoxy resin-filler (silicon nitride powder) composite. The filling rate of the resin composition was 50% by volume.

[0067] A 1 mm thick aluminum plate with a 1 cm x 10 cm rectangular hole was prepared as a mold frame. A PET film (back side film) coated with a release agent was attached to the back side of the mold frame so as to cover the rectangular hole, with the release agent-coated surface facing the mold frame. After the stirred composite was poured into the rectangular hole of the mold frame, a PET film (front side film) coated with a release agent was attached on top of it, with the release agent-coated surface facing the mold frame and resin composition. Furthermore, light pressure was applied from above with a metal roller to fit the composite into the rectangular hole of the mold frame. Another aluminum plate was placed on top of the front side film, and the composite was cured by heating at 100°C for 1 hour. After curing was complete, the aluminum plate was allowed to cool, and when the temperature of the aluminum plate had dropped to approximately room temperature, the aluminum plate was removed. The PET films on the front and back sides of the cured composite were then peeled off, respectively, to obtain a sheet-like sample for measuring thermal diffusivity.

[0068] The thermal diffusivity of the obtained sheet-like sample was measured. Measurement specimens measuring 10 mm in length, 10 mm in width, and 1 mm in thickness were prepared from the sheet-like sample of the resin composition described above, and the thermal diffusivity was measured at room temperature using temperature wave thermal analysis (TWA). The measurement device used was an iPhase Mobile manufactured by iPhase Corporation. The thermal diffusivity was measured at three random points on one measurement specimen, and the average value was calculated from the measurement results of the three points.

[0069] The measurement results are summarized in Tables 2 and 3.

[0070]

[0071]

[0072] The measurement results are discussed below. The silicon nitride powders of Samples Nos. 1 to 3 and 5 to 10, which satisfied the requirements of this embodiment, were inhibited from adhering to other members. On the other hand, the silicon nitride powder of Sample No. 4, which did not satisfy the requirements of this embodiment, adhered to other members in large amounts. Furthermore, the resin compositions containing Samples Nos. 1 to 3 and 5 to 10 had superior thermal diffusivities compared to the resin composition containing Sample No. 4.

[0073] This application claims priority from Japanese Patent Application No. 2023-058723, filed March 31, 2023. Japanese Patent Application No. 2023-058723 is incorporated herein by reference.

Claims

1. A silicon nitride powder comprising a plurality of silicon nitride particles, the silicon nitride powder having an angle of repose of greater than 40°.

2. The silicon nitride powder according to claim 1, having a degree of compression of less than 34.4%.

3. The silicon nitride powder according to claim 1, wherein the difference between the particle diameter D90 of the cumulative 90% from the fine side of the volume-based cumulative particle size distribution and the particle diameter D10 of the cumulative 10% from the fine side of the volume-based cumulative particle size distribution is 150.0 μm or less.

4. The silicon nitride powder according to claim 1, wherein the silicon nitride particles have an average aspect ratio of the minor axis to the major axis greater than 0.

50.

5. The silicon nitride powder according to claim 1, wherein the ratio (L2 / L1) of the total length L2 of the internal boundary line to the length L1 of the outer edge is 1% or less and the maximum particle size of the silicon nitride particles is 6.8 μm or more.

6. A resin composition comprising a resin and the silicon nitride powder according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Production of sintered silicon nitride

    JP1992083758A

  • Method of producing high purity silicon nitride powder

    JP2020023406A