Epitaxial silicon wafer and manufacturing method therefor

The method optimizes epitaxial silicon wafer manufacturing by controlling the backside oxide film thickness to minimize warpage and autodoping, achieving improved flatness and resistivity uniformity, thus addressing the challenges of warpage and autodoping in existing technologies.

WO2024202965A1PCT designated stage expired Publication Date: 2024-10-03SUMCO CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/007987
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-04
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Epitaxial silicon wafers face issues with warpage and autodoping due to dopant concentration differences and thermal expansion coefficient disparities, which affect wafer bonding and pattern overlay accuracy, and existing methods for reducing warpage are either costly or difficult to implement with high precision, especially for large-diameter wafers.

Method used

A method for manufacturing epitaxial silicon wafers with a 300 mm diameter and 761 to 795 μm thickness, involving a boron-doped bulk silicon substrate with a backside oxide film thickness of 50 to 150 nm, and an epitaxial silicon film with a resistivity of 8 to 12 Ω·cm, where the backside oxide film thickness is optimized to minimize warpage by balancing film stress and thermal expansion, thereby reducing in-plane resistivity variations and warpage.

Benefits of technology

The method achieves a warp of 10 μm or less and Bow of ±5 μm or less, enhancing the flatness and reducing defects in the wafer bonding process and improving pattern overlay accuracy, leading to increased semiconductor device manufacturing yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024007987_03102024_PF_FP_ABST
    Figure JP2024007987_03102024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide: an epitaxial silicon wafer having a small in-plane variation in resistivity and a small amount of warpage; and a manufacturing method therefor. [Solution] This epitaxial silicon wafer 1 having a diameter of 300 mm and a thickness of 761-795 μm comprises: a boron-doped bulk silicon substrate 2 having a resistivity of 8-20 mΩ∙cm; an epitaxial silicon film 3 formed on a front surface 2a of the bulk silicon substrate 2; and a rear-surface oxide film 4 formed on a rear surface 2b of the bulk silicon substrate 2. The epitaxial silicon film 3 has a thickness of 1.7-2.7 μm, is boron-doped, has a resistivity of 8-12 Ω∙cm, and has an in-plane distribution of resistivity of at most 3%. The rear-surface oxide film 4 has a thickness of 50-150 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Epitaxial silicon wafer and method for manufacturing the same

[0001] The present invention relates to an epitaxial silicon wafer and a manufacturing method thereof, and more particularly to an epitaxial silicon wafer with measures taken to reduce warpage and a manufacturing method thereof.

[0002] Epitaxial silicon wafers are widely used as substrate materials for semiconductor devices. Epitaxial silicon wafers are made by forming an epitaxial silicon film on the main surface of a bulk silicon substrate, and their high crystalline perfection makes it possible to manufacture high-quality, highly reliable semiconductor devices.

[0003] Bulk silicon substrates, which are the substrate material for epitaxial silicon wafers, are manufactured by sequentially subjecting a silicon single crystal ingot grown by the Czochralski method (CZ method) to processes such as periphery grinding, slicing, lapping, etching, double-side polishing, single-side polishing, and cleaning. Then, an epitaxial film is vapor-grown on the surface of the bulk silicon substrate using an epitaxial growth apparatus, thereby completing the epitaxial silicon wafer.

[0004] Recently, there has been a demand for large-diameter epitaxial silicon wafers, in which a high-resistivity epitaxial film with a low dopant concentration is grown on a low-resistivity bulk silicon substrate with a high dopant concentration, for applications such as BSI-CIS (backside illuminated CMOS image sensors) and BSPDN (backside power distribution networks). In these applications, the dopant concentration difference is used as an etch stop after the bonding process.

[0005] In the production of such epitaxial silicon wafers, there is a problem of so-called autodoping, in which dopants contained in the bulk silicon substrate volatilize during the epitaxial process and are incorporated into the epitaxial film, resulting in a locally high dopant concentration in the epitaxial film. A known method for preventing autodoping is to form an oxide film (SiOx) on the back surface of the bulk silicon substrate to prevent dopant volatilization.

[0006] Furthermore, warpage is a problem with such epitaxial silicon wafers. This is mainly caused by the difference in dopant concentration between the bulk silicon substrate and the epitaxial silicon film. In addition, if an oxide film is formed on the backside of the bulk silicon substrate, the problem of wafer warpage after epitaxial growth becomes even more complicated due to the difference in thermal expansion coefficient between the epitaxial wafer and the oxide film, and the imbalance between the warpage of the epitaxial wafer and the film stress of the oxide film. Warpage of epitaxial silicon wafers affects the wafer bonding process and the overlay control of patterns on the wafer.

[0007] Regarding measures to reduce wafer warpage, Patent Document 1 describes a method of predicting the amount of wafer warpage due to epitaxial growth and producing a substrate wafer having warpage in the opposite direction to the warpage due to epitaxial growth by grinding or polishing.

[0008] Furthermore, Patent Document 2 describes a method for producing a high-quality semiconductor epitaxial wafer having a polysilicon film with minimal wafer warpage and a high gettering capability. This method involves forming a protective film for preventing dopant volatilization on the front and back surfaces of a semiconductor wafer, removing the protective film from the front surface, and then simultaneously forming an epitaxial film on the front surface of the semiconductor wafer and a polysilicon film on the back surface in a reactor. According to this production method, films of the same material are formed on the front and back surfaces of the semiconductor wafer, which reduces stress on the semiconductor wafer, maintains the flatness of the wafer surface, and produces an epitaxial wafer with minimal warpage.

[0009] JP 2008-140856 A JP 2003-188107 A

[0010] However, in the production of epitaxial silicon wafers described in Patent Document 1, the substrate wafer must be ground or polished, which poses a problem of difficulty in processing the substrate wafer with high precision. Furthermore, Patent Document 1 does not disclose anything about a backside oxide film. Patent Document 2 describes setting the thickness of the backside oxide film to 50 to 10,000 Å (5 to 1,000 nm) to prevent dopant volatilization, but the formation of a polysilicon film on the backside balances the amount of warpage of the epitaxial film on the front side, and the impact of the backside oxide film on wafer warpage is largely ignored. However, in recent applications as an etch stop after a bonding process, backside polysilicon is unnecessary, and forming it is pointless considering the cost. Furthermore, the larger the diameter of the wafer, the greater the impact of the backside oxide film on wafer warpage. Therefore, strict control of the thickness of the backside oxide film is required for wafers with a diameter of 300 mm or more.

[0011] Therefore, an object of the present invention is to provide an epitaxial silicon wafer having small in-plane variation in resistivity and small amount of warpage, and a method for manufacturing the same.

[0012] It has been thought that a sufficiently thick backside oxide film is necessary to suppress autodoping. However, as a result of extensive research by the present inventors, it has become clear that an excessively thick backside oxide film can worsen the warpage of epitaxial silicon wafers. It has also become clear that not only can the backside oxide film be made somewhat thin to suppress autodoping, but also that thinning the backside oxide film can reduce the warpage of epitaxial wafers.

[0013] The present invention is based on this technical finding, and the epitaxial silicon wafer according to the present invention is an epitaxial silicon wafer having a diameter of 300 mm and a thickness of 761 to 795 μm, and comprises a boron-doped bulk silicon substrate having a resistivity of 8 to 20 mΩ cm, an epitaxial silicon film formed on the front surface of the bulk silicon substrate, and a back surface oxide film formed on the back surface of the bulk silicon substrate, wherein the epitaxial silicon film has a thickness of 1.7 to 2.7 μm, is boron-doped, and has a resistivity of 8 to 12 Ω cm with an in-plane variation in resistivity of 3% or less, and the back surface oxide film has a thickness of 50 to 150 nm.

[0014] Furthermore, a method for producing an epitaxial silicon wafer according to the present invention is a method for producing an epitaxial silicon wafer having a diameter of 300 mm and a thickness of 761 to 795 μm, and is characterized by comprising the steps of: preparing a boron-doped bulk silicon substrate having a resistivity of 8 to 20 mΩ cm; forming a back surface oxide film having a thickness of 50 to 150 nm on the back surface of the bulk silicon substrate; and forming a boron-doped epitaxial silicon film having a thickness of 1.7 to 2.7 μm, a resistivity of 8 to 12 Ω cm, and an in-plane variation in resistivity of 3% or less on the front surface of the bulk silicon substrate.

[0015] According to the present invention, the warpage of the wafer caused by the epitaxial silicon film can be offset by the film stress of the backside oxide film, thereby realizing a large-diameter epitaxial silicon wafer with a small amount of warpage.

[0016] The epitaxial silicon wafer according to the present invention preferably has a Warp-bf of 10 μm or less, and a Bow-bf of ±5 μm or less. Such high wafer flatness quality can suppress defects such as voids during the wafer bonding process and improve the overlay accuracy of patterns on the wafer. This can increase the manufacturing yield of semiconductor devices.

[0017] The method for producing an epitaxial silicon wafer according to the present invention is a method for producing an epitaxial silicon wafer having a diameter of 300 mm and a thickness of 761 to 795 μm, and includes the steps of: preparing a boron-doped bulk silicon substrate having a resistivity of 8 to 20 mΩ cm; and determining the boron concentration and thickness of the bulk silicon substrate and the thickness t of the epitaxial silicon film. epi The amount of warpage of the epitaxial wafer δ is calculated using the relational equation 1 and calculating the amount of warpage δ of the silicon wafer on which the rear surface oxide film is formed using a relational expression between the diameter and thickness of the bulk silicon substrate and the thickness of the rear surface oxide film. 2 and calculating the amount of warpage δ 1 and the amount of warping δ 2 The thickness t of the backside oxide film at which Warp-bf and Bow-bf are minimum is f and forming a thickness t f forming a backside oxide film of thickness t on the surface of the bulk silicon substrate; epi and forming an epitaxial silicon film on the substrate.

[0018] In the manufacturing method according to the present invention, the estimated thickness t f It is preferable to experimentally determine the thickness of the rear surface oxide film that actually minimizes Warp-bf and Bow-bf based on the above. 1 in the positive direction, and the warpage amount δ 2 It is preferable to calculate the sum of the negative values ​​as Bow-bf, and it is more preferable to calculate the absolute value of the calculated Bow-bf as Warp-b.

[0019] According to the present invention, it is possible to provide an epitaxial silicon wafer having small in-plane variation in resistivity and small amount of warpage, and a method for manufacturing the same.

[0020] FIG. 1 is a schematic cross-sectional view showing the structure of an epitaxial silicon wafer according to an embodiment of the present invention. FIG. 2 is an explanatory diagram of a prediction formula for the amount of warpage of an epitaxial silicon wafer without a backside oxide film. FIG. 3 is an explanatory diagram of a prediction formula for the warpage of a silicon wafer with a backside oxide film formed thereon. FIG. 4 is a graph showing the relationship between the thickness of the backside oxide film and the Bow of the wafer. FIG. 5 is a graph showing the relationship between the thickness of the backside oxide film and the Warp of the wafer. FIG. 6 is a graph showing the relationship between the thickness of the backside oxide film and the Bow-bf of the wafer. FIG. 7 is a graph showing the relationship between the thickness of the backside oxide film and the Warp-bf of the wafer. FIG. 8 is a schematic diagram explaining measurement points of resistivity. FIG. 9 is a graph showing the relationship between the thickness of the backside oxide film and the in-plane variation in resistivity of the epitaxial silicon film.

[0021] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0022] FIG. 1 is a schematic cross-sectional view showing the structure of an epitaxial silicon wafer according to an embodiment of the present invention.

[0023] 1, the epitaxial silicon wafer 1 includes a bulk silicon substrate 2 cut from a CZ silicon single crystal, an epitaxial silicon film 3 formed on a front surface 2a of the bulk silicon substrate 2, and a back surface oxide film 4 formed on a back surface 2b of the bulk silicon substrate 2. In this embodiment, the epitaxial silicon wafer 1 has a diameter of 300 mm and a thickness of 761 to 795 μm. The 300 mm diameter wafer conforms to the SEMI standard, which allows for an error of ±0.2 mm.

[0024] The bulk silicon substrate 2 is a p-type semiconductor silicon doped with boron (B) and having a resistivity of 8 to 20 mΩ·cm. Although it depends on the specifications, the resistivity of the bulk silicon substrate 2 is preferably 8 to 10 mΩ·cm.

[0025] An epitaxial silicon film 3 is formed on the surface 2a (main surface) of the bulk silicon substrate 2. That is, the surface of the epitaxial silicon wafer 1 is composed of the epitaxial silicon film 3. There are no particular limitations on the thickness of the epitaxial silicon film 3, but it is preferably 1.7 to 2.7 μm. The thickness of the epitaxial silicon film 3 is determined based on the type and characteristics of the semiconductor device that will be fabricated by processing it.

[0026] The epitaxial silicon film 3 is p-type semiconductor silicon doped with boron (B), and the resistivity of the epitaxial silicon film 3 is 8 to 12 Ω·cm. Because the dopant concentration of the epitaxial silicon film 3 is much lower than that of the bulk silicon substrate 2, when the bulk silicon substrate 2, which is highly doped with dopant, is heated during the epitaxial growth process, the dopant volatilizes from the back surface 2b of the bulk silicon substrate 2, moves around to the front surface 2a, and is partially incorporated into the epitaxial silicon film 3 during growth, resulting in an autodoping phenomenon. This causes a problem of a worsening in-plane distribution of the resistivity of the epitaxial silicon film 3.

[0027] A back surface oxide film 4 made of SiOx is formed on the back surface 2b of the bulk silicon substrate 2. That is, the back surface of the epitaxial silicon wafer 1 is composed of the back surface oxide film 4. The back surface oxide film 4 serves to prevent the volatilization of dopants from the bulk silicon substrate 2 during the formation of the epitaxial silicon film 3.

[0028] The thickness of the backside oxide film 4 is preferably 50 to 150 nm (500 to 1500 Å). In this embodiment, the backside oxide film 4 not only suppresses autodoping but also suppresses wafer warpage. If the thickness of the backside oxide film 4 is greater than 150 nm, the effect of suppressing wafer warpage may not be obtained, and if the thickness of the backside oxide film 4 is less than 50 nm, the effect of suppressing autodoping may not be obtained. However, if the thickness of the backside oxide film 4 is 50 to 150 nm, it is possible to suppress warpage of the epitaxial silicon wafer 1 while suppressing autodoping.

[0029] It is preferable that the in-plane variation in resistivity of the epitaxial silicon film 3 is 3% or less. When autodoping is suppressed by using the back surface oxide film 4, it is possible to suppress deterioration of the in-plane distribution of resistivity of the epitaxial silicon film 3, and it is possible to suppress the in-plane variation in resistivity to 3% or less.

[0030] The in-plane variation in resistivity of the outer periphery of the epitaxial silicon film 3 is preferably 1.5% or less. Here, the outer periphery of the epitaxial silicon film 3 refers to the region within 100 mm inward from the outermost periphery of the wafer. When autodoping is suppressed using the backside oxide film 4, it is possible to suppress changes in the resistivity of the outer periphery of the epitaxial silicon film 3, and the in-plane variation in resistivity of the outer periphery can be suppressed to 1.5% or less.

[0031] Fig. 2 is an explanatory diagram of a prediction formula for the amount of warpage of an epitaxial silicon wafer without a backside oxide film, and Fig. 3 is an explanatory diagram of a prediction formula for the amount of warpage of a silicon wafer with a backside oxide film formed thereon.

[0032] As shown in Figure 2, a simple epitaxial silicon wafer without a backside oxide film has an epitaxial silicon film formed on the surface of a silicon substrate. However, due to the difference in boron concentration between the silicon substrate and the epitaxial silicon film, the epitaxial silicon wafer develops a convex upward warp due to the difference in atomic radius between silicon atoms and boron atoms, and the amount of warp δ 1 can be expressed by the following equation:

[0033]

[0034] where r is the radius of the bulk silicon substrate 2, and t si is the thickness of the bulk silicon substrate 2, [B] is the boron concentration in the bulk silicon substrate 2, t epi is the thickness of the epitaxial silicon film 3. The boron concentration in the epitaxial silicon film is negligibly small compared to the boron concentration in the bulk silicon substrate 2, and is therefore not taken into consideration.

[0035] As shown in FIG. 3, a silicon wafer on which an oxide film is formed on the rear surface has a downward convex warp, and the amount of warp δ 2 can be expressed by the following equation:

[0036]

[0037] Here, R s is the radius of the silicon wafer, t s is the thickness of the silicon wafer, Es is the Young's modulus of silicon, v s is the Poisson's ratio of silicon, t f is the thickness of the rear surface oxide film 4, σ f is the film stress of the rear surface oxide film 4.

[0038] And the two warpage amounts δ 1 , δ 2 When the balance is achieved, the amount of warpage of the epitaxial silicon wafer on which the backside oxide film is formed is minimized.

[0039] In this embodiment, the Warp of the epitaxial silicon wafer 1, in which the upward convex warp and the downward convex warp are offset, is preferably 10 μm or less, and the Bow is preferably within ±5 μm. Here, Warp is a value expressed as the difference between the maximum and minimum displacements from the best fit plane of thickness central plane of the wafer without suction fixation to the central plane in the wafer thickness direction (Warp-bf: SEMI-MF657, SEMI-MF1390). Bow is a value expressed as the amount of displacement from the best fit plane of thickness central plane of the wafer without suction fixation to the center point of the thickness at the center of the wafer, with the concave surface being the front side (upper side) (Bow-bf: SEMI-MF534). Warp-bf and Bow-bf can be measured, for example, using a capacitance-type flatness measuring instrument.

[0040] The epitaxial silicon wafer 1 according to this embodiment is manufactured by forming a backside oxide film 4 on the backside 2b of a bulk silicon substrate 2, and then forming an epitaxial silicon film 3 on the frontside 2a of the bulk silicon substrate 2. The backside oxide film 4 can be formed using, for example, a single-wafer atmospheric pressure CVD (Chemical Vapor Deposition) apparatus.

[0041] The epitaxial silicon film 3 can be formed by vapor-phase growing silicon at a temperature in the range of, for example, 900 to 1200° C. while supplying a source gas to the surface 2 a of the bulk silicon substrate 2. Here, the source gas may be, for example, Si 3 H 8 , SiH 2 Cl 2 , SiHCl 3 , SiCl 4 etc. can be used.

[0042] As described above, the epitaxial silicon wafer 1 according to this embodiment comprises a boron-doped bulk silicon substrate 2 having a resistivity of 8 to 20 mΩ cm, an epitaxial silicon film 3 formed on the front surface 2a of the bulk silicon substrate 2, and a back surface oxide film 4 formed on the back surface 2b of the bulk silicon substrate 2. The epitaxial silicon film 3 has a thickness of 1.7 to 2.7 μm, is boron-doped, has a resistivity of 8 to 12 Ω cm, and an in-plane variation in resistivity of 3% or less, and the back surface oxide film 4 has a thickness of 50 nm or more and 150 nm or less. Therefore, the Warp-bf of the epitaxial silicon wafer 1 can be suppressed to 10 μm or less and the Bow-bf to within ±5 μm while suppressing autodoping. The final epitaxial silicon wafer 1 has a diameter of 300 mm and a thickness of 761 to 795 μm, for example.

[0043] The present invention is not limited to the above-described embodiments, and various modifications can be made without departing from the spirit of the present invention, and it goes without saying that these modifications are also included in the scope of the present invention.

[0044] The amount of warpage δ of the epitaxial wafer only is calculated using equation (1). 1Then, using equation (2), the amount of warpage due to the rear surface oxide film δ 2 The calculated amount of warpage in the positive direction δ 1 The amount of warpage in the negative direction δ 2 The sum of these values ​​was calculated as Bow. The absolute value of the calculated Bow was taken as Warp. Figures 4 and 5 show the results of calculating Bow and Warp when backside oxide films of 50 nm, 100 nm, 150 nm, and 200 nm were formed on wafers with various silicon substrate resistivities, silicon substrate thicknesses, and epitaxial silicon film thicknesses. From Figures 4 and 5, it was estimated that both Bow-bf and Warp-bf could be reduced by setting the backside oxide film thickness to around 150 nm.

[0045] Based on the estimation results, epitaxial silicon wafers according to Examples 1 to 3 and Comparative Examples 1 to 3 were prepared, each having a different thickness of a backside oxide film formed on the backside of a p-type silicon substrate made of a bulk silicon wafer with a diameter of 300 mm. The resistivity of the p-type silicon substrate was set to 8 to 10 mΩ cm. The backside oxide film was formed using a single-wafer atmospheric pressure CVD method at a film formation rate of 400 to 800 Å / min. In all Examples and Comparative Examples, no particular edge treatment was performed on the backside oxide film, and wafers with an oxide film formed on the entire backside were used.

[0046] The thicknesses of the rear surface oxide films of the epitaxial silicon wafers according to Examples 1 to 3 were 50 nm, 100 nm, and 150 nm, respectively, and the thicknesses of the rear surface oxide films of the epitaxial silicon wafers according to Comparative Examples 1 and 2 were 200 nm and 300 nm, respectively. A mass-produced epitaxial silicon wafer having a rear surface oxide film thickness of 300 to 400 nm was designated Comparative Example 3. The thickness of the epitaxial film formed on the surface of the bulk silicon substrate was 1.7 to 2.7 μm, and the resistivity was 8 to 12 Ω cm. The number of samples of the epitaxial silicon wafers according to Examples 1 to 3 was 14, 15, and 15, respectively. The number of samples of the epitaxial silicon wafers according to Comparative Examples 1 and 2 was 14 and 15, respectively. The number of samples of the epitaxial silicon wafer according to Comparative Example 3 was 1,500.

[0047] Next, the Bow-bf and Warp-bf of each epitaxial silicon wafer sample were measured using a flatness measurement device manufactured by ADE Corporation. The outer peripheral portion of the wafer within 2 mm from the outermost periphery was excluded from the flatness measurement. The results are shown in Tables 1 and 2.

[0048]

[0049]

[0050] Fig. 6 is a graph showing the relationship between the thickness of the rear surface oxide film and the Bow-bf of the wafer shown in Table 1. Fig. 7 is a graph showing the relationship between the thickness of the rear surface oxide film and the Warp-bf of the wafer shown in Table 2.

[0051] As shown in Fig. 6 and Table 1, the average Bow-bf value of the 14 wafer samples according to Example 1, each having a backside oxide film thickness of 50 nm, was 2.0504 µm, and the standard deviation of Bow-bf was 0.6137 µm. As shown in Fig. 7 and Table 2, the average Warp-bf value of the 14 wafer samples according to Example 1 was 6.9674 µm, and the standard deviation of Warp-bf was 0.9572 µm.

[0052] The average Bow-bf value of the 15 wafer samples according to Example 2, each having a backside oxide film thickness of 100 nm, was 0.64 μm, with a standard deviation of 0.2517 μm. The average Warp-bf value of the 15 wafer samples according to Example 2 was 4.2153 μm, with a standard deviation of 0.3328 μm.

[0053] The average Bow-bf value of the 15 wafer samples according to Example 3, each having a backside oxide film thickness of 150 nm, was −2.592 μm, with a standard deviation of 0.2682 μm. The average Warp-bf value of the 15 wafer samples according to Example 3 was 7.5999 μm, with a standard deviation of 0.4470 μm.

[0054] The average Bow-bf value of the 15 wafer samples according to Comparative Example 1, each having a backside oxide film thickness of 200 nm, was −5.791 μm with a standard deviation of 0.1598 μm. The average Warp-bf value of the 15 wafer samples according to Comparative Example 1 was 13.666 μm with a standard deviation of 0.2092 μm.

[0055] The average Bow-bf value of the 14 wafer samples according to Comparative Example 2, each having a backside oxide film thickness of 300 nm, was −11.33 μm, with a standard deviation of 0.2664 μm. The average Warp-bf value of the 14 wafer samples according to Comparative Example 2 was 25.079 μm, with a standard deviation of 0.3819 μm.

[0056] The average Bow-bf value of 1,500 wafer samples according to Comparative Example 3, in which the backside oxide film thickness was 300 to 400 nm, was -14.66 μm, with a standard deviation of 0.89 μm. The average Warp-bf value of 1,500 wafer samples according to Comparative Example 3 was 33.1 μm, with a standard deviation of 2.9139 μm.

[0057] From the above results, it was confirmed that the amount of warpage of the epitaxial silicon wafer tends to decrease as the thickness of the backside oxide film decreases. Furthermore, in Examples 1 to 3, in which the thickness of the backside oxide film was 150 nm or less, Bow-bf was within ±5 μm and Warp-bf was 10 μm or less, and the amount of warpage of the epitaxial silicon wafer was able to be made sufficiently smaller than that of Comparative Example 3, which is a mass-produced product. In Example 2, in which the thickness of the backside oxide film was 100 nm, Bow-bf was within ±1 μm and Warp-bf was 5 μm or less, and it was found that the amount of warpage of the epitaxial silicon wafer could be minimized.

[0058] Estimation using equations (1) and (2) showed that a thickness of approximately 150 nm for the backside oxide film was optimal, but in reality, better results were obtained with a thinner film. The reasons for this include the fact that equation (2) quantifies the deflection at the center of the wafer, whereas the actual backside oxide film expands three-dimensionally, and that the Young's modulus and Poisson's ratio actually change depending on the resistivity.

[0059] Next, the resistivity distribution of each sample of epitaxial silicon wafers according to Examples 1 to 3 and Comparative Examples 1 to 3 was measured using an SCP (Surface Charge Profiler) to evaluate the uniformity of the resistivity of the epitaxial silicon film. From the viewpoint of measurement reproducibility, pretreatment was performed by heating (200 to 300°C, 30 seconds or more), and measurements were performed with a light source wavelength of 450 nm. Furthermore, a map measurement of 4,253 points was performed at a 4 mm pitch, excluding the outer peripheral area within 2 mm inward from the outermost periphery of the wafer. Next, of all the measurement points, measurement points within the outer peripheral area within 6 mm inward from the outermost periphery of the wafer were excluded, and 145 points on the cross line shown in Figure 8 were extracted. Then, the maximum value ρ of the extracted values ​​was calculated. max , and the minimum value ρ min was applied to the following formula (3) to calculate the resistivity uniformity U (%). Furthermore, from the above 145 points, 48 ​​points (12 × 4 points) in the region outside the position 100 mm from the center of the wafer (100 to 150 mm) were extracted, and the resistivity uniformity U (%) was calculated in the same manner.

[0060]

[0061] FIG. 9 is a graph showing the relationship between the thickness of the backside oxide film and the uniformity of the resistivity of the epitaxial silicon film.

[0062] 9, the resistivity uniformity measured at 145 measurement points, including the wafer center, was 2.7% or less for all of Examples 1 to 3 and Comparative Examples 1 to 3, a good result below 3%. Furthermore, the resistivity uniformity measured at 48 measurement points on the wafer periphery was 1.2% or less for all of Examples 1 to 3, a good result below 1.5%. These results confirm that, as long as the backside oxide film thickness is 50 nm or greater, the effect of differences in the backside oxide film thickness on autodoping is negligible, and resistivity uniformity is ensured.

[0063] REFERENCE SIGNS LIST 1 epitaxial silicon wafer 2 bulk silicon substrate 2a front surface of bulk silicon substrate 2b rear surface of bulk silicon substrate 3 epitaxial silicon film 4 rear surface oxide film

Claims

1. An epitaxial silicon wafer having a diameter of 300 mm and a thickness of 761 to 795 μm, comprising: a boron-doped bulk silicon substrate having a resistivity of 8 to 20 mΩ·cm; an epitaxial silicon film formed on the front surface of the bulk silicon substrate; and a back surface oxide film formed on the back surface of the bulk silicon substrate, wherein the epitaxial silicon film has a thickness of 1.7 to 2.7 μm, is boron-doped and has a resistivity of 8 to 12 Ω·cm, with an in-plane variation in resistivity of 3% or less, and the back surface oxide film has a thickness of 50 to 150 nm.

2. The epitaxial silicon wafer according to claim 1, wherein Warp-bf is 10 μm or less.

3. The epitaxial silicon wafer according to claim 1, wherein the Bow-bf is ±5 μm or less.

4. A method for manufacturing an epitaxial silicon wafer having a diameter of 300 mm and a thickness of 761 to 795 μm, comprising the steps of: preparing a boron-doped bulk silicon substrate having a resistivity of 8 to 20 mΩ·cm; forming a back surface oxide film having a thickness of 50 to 150 nm on the back surface of the bulk silicon substrate; and forming an epitaxial silicon film having a thickness of 1.7 to 2.7 μm, which is boron-doped and has a resistivity of 8 to 12 Ω·cm and an in-plane variation in resistivity of 3% or less on the front surface of the bulk silicon substrate.

5. A method for manufacturing an epitaxial silicon wafer having a diameter of 300 mm and a thickness of 761 to 765 μm, comprising the steps of: preparing a bulk silicon substrate doped with boron and having a resistivity of 8 to 20 mΩ·cm; and determining the boron concentration and thickness of the bulk silicon substrate and the thickness t of the epitaxial silicon film. epi The amount of warpage of the epitaxial wafer δ is calculated using the relational equation 1 and calculating a warpage amount δ of the silicon wafer on which the back surface oxide film is formed, using a relational expression between the diameter and thickness of the bulk silicon substrate and the thickness of the back surface oxide film. 2 and calculating the amount of warpage δ 1 and the warpage amount δ 2 The thickness t of the back surface oxide film at which Warp-bf and Bow-bf are minimized is f and forming a thickness t f forming a back surface oxide film of thickness t on the front surface of the bulk silicon substrate; epi and forming an epitaxial silicon film on the substrate.

6. The estimated thickness t of the back surface oxide film f 6. The method for producing an epitaxial silicon wafer according to claim 5, wherein the thickness of the back surface oxide film at which Warp-bf and Bow-bf are actually minimized is experimentally determined based on the above.

7. Amount of warpage δ 1 in the positive direction, and the warpage amount δ 2 6. The method for producing an epitaxial silicon wafer according to claim 5, wherein the sum of the values ​​is calculated as Bow-bf in a negative direction.

8. The method for producing an epitaxial silicon wafer according to claim 6, wherein the absolute value of the calculated Bow-bf is calculated as Warp-bf.

Citation Information

Patent Citations

  • Manufacture of semiconductor wafer

    JP1993343276A

  • Production of epitaxial wafer

    JP1997194296A

  • Si substrate for epitaxial wafer and its manufacturing method

    JP1997199380A

  • Manufacturing method for semiconductor epitaxial wafer and the semiconductor epitaxial wafer

    JP2003188107A

  • Epitaxial silicon wafer, manufacturing method thereof and silicon wafer for epitaxial growth