Electrochemical capacitor

By employing a positive electrode with activated carbon, a negative electrode with non-graphitizable carbon, and a specific electrolyte composition, the electrochemical capacitor achieves low internal resistance and high output, addressing the temperature-related performance issues.

WO2024202996A1PCT designated stage expired Publication Date: 2024-10-03PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008136
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-04
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Electrochemical capacitors face high internal resistance, especially at low temperatures, and increased resistance during float charging at high temperatures, limiting their output performance.

Method used

The use of a positive electrode with a composite layer containing activated carbon, a negative electrode with non-graphitizable carbon, and an electrolyte with a specific anion-to-surface area ratio, along with a surface layer containing lithium carbonate, to reduce internal resistance and maintain high output characteristics.

Benefits of technology

This configuration results in electrochemical capacitors with low internal resistance and high output performance, both initially and after repeated charge/discharge cycles, even at low temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008136_03102024_PF_FP_ABST
    Figure JP2024008136_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed is an electrochemical capacitor comprising: a positive electrode including a positive electrode current collector and a positive electrode mixture layer that contains activated carbon and that is supported on the positive electrode current collector; a negative electrode including a negative electrode current collector and a negative electrode mixture layer that contains a negative electrode active material reversibly doped with lithium ions and that is supported on the negative electrode current collector; and an electrolytic solution including a nonaqueous solvent and an electrolyte that contains lithium ions and anions. The ratio of the anion amount to the surface area of the positive electrode mixture layer is 1.5-2.4 μmol / m2. <sp / >
Need to check novelty before this filing date? Find Prior Art

Description

electrochemical capacitor CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This disclosure claims the benefit of priority to Japanese Patent Application No. 2023-050796, filed on March 28, 2023, in the Japan Patent Office, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to an electrochemical capacitor.

[0003] In recent years, electrochemical capacitors that combine the energy storage principles of lithium-ion secondary batteries and electric double-layer capacitors have attracted attention. Such electrochemical capacitors typically use a polarizable electrode as the positive electrode and a non-polarizable electrode as the negative electrode. As a result, electrochemical capacitors are expected to combine the high energy density of lithium-ion secondary batteries with the high output characteristics of electric double-layer capacitors.

[0004] Patent Document 1 proposes a positive electrode for a lithium ion capacitor, characterized in that the pore volume of pores with diameters of 1.0 nm or more and less than 1.4 nm in the positive electrode layer calculated by the HK method is 0.11 cc / g or more, and the total pore volume calculated by the BET method is 1.1 cc / g or less.

[0005] Patent Document 2 proposes a lithium ion capacitor having a positive electrode, a negative electrode, and an electrolyte solution in contact with the positive electrode and the negative electrode, in which the electrolyte solution contains an organic solvent and a lithium salt electrolyte having an imide structure, and the organic solvent contains ethylene carbonate and propylene carbonate.

[0006] Patent No. 6422483 Patent No. 7103376

[0007] However, further improvements are required for the electrochemical capacitors described above in order to achieve a higher level of high output.

[0008] Electrochemical capacitors tend to have a large internal resistance (DCR), especially at low temperatures. Furthermore, when float charging, in which a constant voltage is applied to an electrochemical capacitor using an external DC power supply, is performed at high temperatures, the internal resistance tends to increase. To achieve high output characteristics, it is necessary to reduce the initial internal resistance and the internal resistance after a float test.

[0009] The present invention provides a battery comprising: a positive electrode including a positive electrode current collector and a positive electrode mixture layer containing activated carbon and supported on the positive electrode current collector; a negative electrode including a negative electrode current collector and a negative electrode mixture layer containing a negative electrode active material that is reversibly doped with lithium ions and supported on the negative electrode current collector; and an electrolytic solution including an electrolyte containing lithium ions and an anion, and a non-aqueous solvent, wherein the ratio of the amount of the anion to the surface area of ​​the positive electrode mixture layer is 1.5 μmol / m 2 Above, 2.4 μmol / m 2 The following relates to an electrochemical capacitor.

[0010] According to the present invention, it is possible to provide an electrochemical capacitor with low internal resistance and high output.

[0011] The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.

[0012] 1 is a vertical cross-sectional view of an electrochemical capacitor according to one embodiment of the present invention.

[0013] Hereinafter, embodiments of the present disclosure will be described using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values, materials, etc. may be exemplified, but other numerical values, materials, etc. may be applied as long as the effects of the present disclosure are obtained. Note that known components may be applied to components other than those characteristic of the present disclosure. In this specification, when a "range from numerical value A to numerical value B" is mentioned, the range includes numerical value A and numerical value B.

[0014] In the following description, when lower and upper limits of numerical values ​​relating to specific physical properties, conditions, etc. are exemplified, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit. When multiple materials are exemplified, one of them may be selected and used alone, or two or more may be used in combination, unless otherwise specified.

[0015] The present disclosure also encompasses combinations of two or more features arbitrarily selected from the appended claims, i.e., two or more features arbitrarily selected from the appended claims can be combined unless a technical contradiction arises.

[0016] An electrochemical capacitor according to an embodiment of the present invention includes a positive electrode, a negative electrode, and an electrolyte. Generally, the positive electrode and the negative electrode, together with a separator interposed therebetween, constitute an electrode assembly. The electrode assembly is formed, for example, as a columnar wound body by winding a strip-shaped positive electrode and a strip-shaped negative electrode with a separator interposed therebetween. Alternatively, the electrode assembly may be formed as a laminate by stacking a plate-shaped positive electrode and a strip-shaped negative electrode with a separator interposed therebetween.

[0017] The positive electrode includes, for example, a positive electrode current collector and a positive electrode composite layer containing activated carbon and supported on the positive electrode current collector. The positive electrode composite layer contains a positive electrode active material such as activated carbon that reversibly dopes anions. When anions are adsorbed onto the positive electrode active material such as activated carbon, an electric double layer is formed, thereby generating capacitance. The positive electrode may be a polarizable electrode, or may be an electrode that has the properties of a polarizable electrode but also contributes to capacitance through a Faraday reaction.

[0018] Doping a positive electrode active material such as activated carbon with anions is a concept that includes at least the phenomenon of anions being adsorbed onto a positive electrode active material such as activated carbon, and may also include the occlusion of anions by a positive electrode active material such as activated carbon, and chemical interactions between a positive electrode active material such as activated carbon and anions.

[0019] The negative electrode includes a negative electrode current collector and a negative electrode composite layer supported on the negative electrode current collector. The negative electrode active material contains a negative electrode active material that reversibly dopes lithium ions. A Faraday reaction occurs in the negative electrode active material, causing the lithium ions to reversibly absorb and release, thereby generating capacity. The doping of the negative electrode active material with lithium ions includes at least the phenomenon of lithium ion absorption into the negative electrode active material, and may also include the adsorption of lithium ions into the negative electrode active material and chemical interactions between the negative electrode active material and the lithium ions.

[0020] Hereinafter, the positive electrode and the negative electrode may be collectively referred to as electrodes. The positive electrode current collector and the negative electrode current collector may be collectively referred to as current collectors (or electrode current collectors). The positive electrode composite layer and the negative electrode composite layer may be collectively referred to as composite layers (or electrode composite layers). The positive electrode active material and the negative electrode active material may be collectively referred to as active materials (or electrode active materials).

[0021] The electrolyte solution includes an electrolyte containing lithium ions and anions, and a non-aqueous solvent. The electrolyte solution has lithium ion conductivity, and the anions are reversibly doped and dedoped to the positive electrode. The lithium ions are reversibly absorbed and released to the negative electrode.

[0022] The ratio of the amount of anions to the surface area of ​​the positive electrode mixture layer is 1.5 μmol / m 2 Above, 2.4 μmol / m 2 This allows the initial internal resistance of the electrochemical capacitor to be reduced. Furthermore, since deterioration of the positive electrode can be suppressed, the internal resistance can be maintained low even after numerous charge-discharge cycles, enabling high output characteristics to be achieved.

[0023] The ratio of the amount of anions to the surface area of ​​the positive electrode mixture layer is an index showing the ratio of the amount of anions that reversibly repeat doping and dedoping on the surface of the positive electrode mixture layer to the surface area of ​​the positive electrode mixture layer, and is expressed as the amount of anions divided by the surface area of ​​the positive electrode mixture layer.

[0024] The amount of anions is represented by the molar amount A of anions contained per cell of the electrochemical capacitor. The surface area of ​​the positive electrode mixture layer is represented by the surface area B of the positive electrode mixture layer per cell of the electrochemical capacitor, and is calculated from the specific surface area b of the positive electrode mixture layer.

[0025] The ratio of the amount of anions to the surface area of ​​the positive electrode mixture layer is expressed as A / B, which is the amount of anions A divided by the surface area B of the positive electrode mixture layer.

[0026] Here, the deterioration of the positive electrode is typically evaluated by the rate of increase in the low-temperature DCR of an electrochemical capacitor when float charging is performed at a high temperature, in which a constant voltage is applied to the electrochemical capacitor using an external DC power source. The rate of increase in the low-temperature DCR is the ratio of the difference (ΔDCR) between the initial low-temperature DCR and the low-temperature DCR after float charging to the initial low-temperature DCR of the electrochemical capacitor. The smaller the rate of increase in the low-temperature DCR, the smaller the deterioration of the positive electrode.

[0027] When the ratio A / B of the amount of anions to the surface area of ​​the positive electrode composite layer is small, the amount of anions A that reversibly repeats doping and dedoping on the surface of the positive electrode composite layer is small, so sufficient capacity is not developed and the initial internal resistance also becomes high. On the other hand, when A / B is large, although the capacity increases, the deterioration of the positive electrode tends to progress. For example, the internal resistance after the float test tends to increase, and the difference between the internal resistance at the initial stage and that after the float charge becomes large, resulting in a high internal resistance after the float charge. When A / B is 1.5 μmol / m 2 If A / B is less than 2.4 μmol / m, the initial internal resistance increases significantly. 2 If A / B is more than 1.5 to 2.4 μmol / m, deterioration of the positive electrode will progress rapidly and the internal resistance after float charging will increase excessively. 2 Within this range, both a low initial internal resistance and a low internal resistance after float charging can be achieved, and high output characteristics can be maintained.

[0028] The ratio A / B of the amount of anions to the surface area of ​​the positive electrode mixture layer is 1.7 μmol / m 2 Above, 2.2 μmol / m 2In this case, the initial internal resistance and the internal resistance after float charging are significantly reduced, and the output characteristics of the electrochemical capacitor can be further improved.

[0029] The amount of anions A (mmol) contained in one cell of an electrochemical capacitor depends on the molar concentration (M) of the electrolyte contained in the electrolyte solution, the mass (g) of the electrolyte solution, and the specific gravity (g / cm 3 ) is expressed by the following formula:

[0030] Amount of anion A=(molar concentration of electrolyte contained in electrolyte solution)×(mass of electrolyte solution) / (specific gravity of electrolyte solution)

[0031] The surface area B (m 2 ) is expressed by the following formula: The surface area per unit mass of the positive electrode mixture layer (specific surface area b of the positive electrode mixture layer) (m 2 / g) and the mass of the positive electrode mixture layer (mass of the positive electrode - mass of the positive electrode current collector) (g).

[0032] Surface area B of positive electrode mixture layer = (specific surface area b of positive electrode mixture layer) × (mass of positive electrode - mass of positive electrode current collector)

[0033] The ratio A / B (μmol / m 2 ) is expressed by the following formula: 2 ) and expressed as a division by

[0034] Ratio of the amount of anions to the surface area of ​​the positive electrode mixture layer A / B=(amount of anions A) / (surface area of ​​the positive electrode mixture layer B)×1000

[0035] When electrode mixture layers are provided on both surfaces of the current collector, the surface area B of the positive electrode mixture layer is calculated by multiplying the total mass of the positive electrode mixture layers on both surfaces of the current collector by the surface area per unit mass of the positive electrode mixture layer (specific surface area b of the positive electrode mixture layer), as derived from the above definition.

[0036] The specific surface area b of the positive electrode composite layer is the BET specific surface area determined using a measuring device conforming to JIS Z8830 (e.g., a Tristar II 3020 manufactured by Shimadzu Corporation). Specifically, the electrochemical capacitor is disassembled, and the positive electrode is removed. The positive electrode composite layer is then peeled off from the positive electrode current collector, and approximately 0.5 g of a sample of the positive electrode composite layer is taken.

[0037] Next, the collected sample is heated at 150°C for 12 hours under a reduced pressure of 95 kPa or less, and then nitrogen gas is adsorbed onto a sample of known mass to obtain an adsorption isotherm over a relative pressure range of 0 to 1. The surface area of ​​the sample is then calculated from the monolayer adsorption amount of gas obtained from the adsorption isotherm. Here, the specific surface area b is calculated using the BET single-point method (relative pressure 0.3) using the BET formula below.

[0038] P / V(P0-P)={1 / (Vm・C)}+{(C-1) / (Vm・C)}(P / P0)...(1)

[0039] S=kVm...(2)

[0040] P0: saturated vapor pressure P: adsorption equilibrium pressure V: adsorption amount at adsorption equilibrium pressure P Vm: monolayer adsorption amount C: parameters related to heat of adsorption etc. S: specific surface area b k: nitrogen monomolecular occupied area 0.162 nm 2

[0041] The specific surface area of ​​the positive electrode mixture layer generally reflects the specific surface area of ​​the positive electrode active material, but the specific surface area also depends on the specific surface area and content of materials other than the positive electrode active material, such as a conductive additive and a binder, that may be contained in the positive electrode mixture layer, and the distribution of these materials within the mixture layer.

[0042] The negative electrode active material preferably contains non-graphitizable carbon. Non-graphitizable carbon is also called hard carbon. By using non-graphitizable carbon, high cycle characteristics can be obtained even under charge-discharge conditions in which rapid charging and rapid discharging are repeated. In addition, the internal resistance (DCR) is small even at low temperatures, making it possible to realize a high-output electrochemical capacitor.

[0043] A surface layer portion is formed on the surface of the negative electrode mixture layer. The surface layer portion may have a first layer containing lithium carbonate (lithium carbonate-containing layer). The first layer is formed mainly on the surface of the negative electrode active material. By forming the first layer containing lithium carbonate, deterioration of the negative electrode is significantly suppressed.

[0044] The surface layer formed on the negative electrode composite layer may further include a second layer (solid electrolyte layer) including a solid electrolyte layer. The second layer may be formed to cover at least a portion of the surface of the first layer. The second layer has a different composition from the first layer, making the second layer distinguishable from the first layer. In an electrochemical capacitor using lithium ions, a solid electrolyte interfacial film (i.e., an SEI film) is formed on the negative electrode composite layer during charge and discharge. The second layer may be formed as an SEI film. The SEI film plays an important role in charge and discharge reactions, but if the SEI film is formed too thick, the negative electrode will deteriorate significantly. In contrast, the first layer containing lithium carbonate promotes the formation of a good SEI film and maintains the SEI film in good condition during repeated charge and discharge. That is, the first layer is interposed between the surface of the negative electrode active material and the second layer, serving as a base layer for the second layer, thereby forming the second layer as a good SEI film. Therefore, by having the first layer in the surface layer portion, deterioration of the negative electrode can be significantly suppressed even when the specific surface area of ​​the negative electrode mixture layer is increased to suppress an increase in low-temperature DCR.

[0045] The second layer may also contain lithium carbonate. When the second layer contains lithium carbonate, the lithium carbonate content in the second layer is less than the lithium carbonate content in the first layer. Using the first layer containing a large amount of lithium carbonate as an underlayer is a necessary condition for the second layer to be formed as a good SEI coating.

[0046] The first layer is formed as at least a portion of the surface layer on the surface of the negative electrode composite layer before assembling the electrochemical capacitor. In an electrochemical capacitor assembled using the negative electrode, a homogeneous, moderately thick second layer (SEI coating) is formed on the surface of the negative electrode active material through subsequent charging and discharging. The SEI coating is formed, for example, by a reaction between the electrolyte and the negative electrode in the electrochemical capacitor. Because the electrolyte can pass through not only the second layer but also the first layer, the entire surface layer including the first and second layers may be referred to as the SEI coating. However, for convenience, the second layer will be referred to as the SEI coating in this specification to distinguish it from the first layer.

[0047] The presence of a region containing lithium carbonate such as the first layer can be confirmed by analyzing the surface layer by, for example, X-ray photoelectron spectroscopy (XPS), although the analysis method is not limited to XPS.

[0048] The thickness of the first layer may be, for example, 1 nm or more, 5 nm or more if a longer-term effect is expected, or 10 nm or more if a more reliable effect is expected. However, if the thickness of the first layer exceeds 50 nm, the first layer itself may become a resistance component. Therefore, the thickness of the first layer may be 50 nm or less, or may be 30 nm or less.

[0049] The thickness of the second layer may be, for example, 1 nm or more, or may be 3 nm or more, or 5 nm or more is sufficient. However, if the thickness of the second layer exceeds 20 nm, the second layer itself may become a resistance component. Therefore, the thickness of the second layer may be 20 nm or less, or may be 10 nm or less.

[0050] The ratio T1 / T2 of the thickness T1 of the first layer to the thickness T2 of the second layer is preferably 1 or less from the viewpoint of reducing the initial low-temperature DCR. In this case, the thickness of the second layer is preferably 20 nm or less, and may be 10 nm or less. However, from the viewpoint of forming a second layer in good condition, it is desirable that the T1 / T2 ratio be 0.1 or more, and for example, the T1 / T2 ratio may be 0.2 or more.

[0051] The thicknesses of the first and second layers are measured by analyzing the surface layer portion formed on the surface of the negative electrode composite layer at multiple locations (at least five locations) of the negative electrode composite layer. The average thickness of the first or second layer measured at multiple locations may be used as the thickness of the first or second layer. The negative electrode composite layer used as the measurement sample may be peeled off from the negative electrode current collector. In this case, the coating formed on the surface of the negative electrode active material constituting the vicinity of the surface layer portion of the negative electrode composite layer may be analyzed. Specifically, the coating-covered negative electrode active material may be collected from the region of the negative electrode composite layer disposed on the side opposite to the surface bonded to the negative electrode current collector and used for analysis.

[0052] XPS analysis of the surface layer portion formed on the surface of the negative electrode composite layer is performed, for example, by irradiating an argon beam onto the surface layer portion or a coating formed on the surface of the negative electrode active material in the chamber of an X-ray photoelectron spectrometer, and observing and recording changes in the spectra attributable to C1s, O1s electrons, etc. with respect to irradiation time. In this case, the spectrum of the outermost surface of the surface layer portion may be ignored to avoid analytical errors. The thickness of the region where peaks attributable to lithium carbonate are stably observed corresponds to the thickness of the first layer.

[0053] In the case of a negative electrode removed from a completed electrochemical capacitor that has undergone a predetermined aging process or at least one charge / discharge cycle, the surface layer formed on the surface of the negative electrode composite layer has an SEI coating (i.e., second layer) containing a solid electrolyte. The thickness of the region where peaks attributable to bonds possessed by compounds contained in the SEI coating are stably observed corresponds to the thickness of the SEI coating (i.e., the thickness of the second layer).

[0054] The compound contained in the SEI coating is selected to contain an element that can be a label for the second layer. The element that can be a label for the second layer may be, for example, an element (e.g., F) that is contained in the electrolyte and is substantially not contained in the first layer. LiF, for example, may be selected as the compound that contains the element that can be a label for the second layer.

[0055] When the second layer contains LiF, a substantial F1s peak attributed to LiF bonds is observed when the second layer is measured by X-ray photoelectron spectroscopy. In this case, the thickness of the region where the peak attributed to LiF bonds is stably observed corresponds to the thickness of the second layer.

[0056] On the other hand, the first layer usually does not contain LiF, and when the first layer is measured by X-ray photoelectron spectroscopy, a substantial F1s peak attributed to the LiF bond is not observed. Therefore, the thickness of the region where a peak attributed to the LiF bond is not stably observed may be defined as the thickness of the first layer.

[0057] An O1s peak attributed to lithium carbonate can also be observed in the SEI coating. However, the SEI coating formed in the electrochemical capacitor has a different composition from the pre-formed first layer, making it possible to distinguish between the two. For example, in an XPS analysis of the SEI coating, an F1s peak attributed to LiF bonds is observed, but a substantial F1s peak attributed to LiF bonds is not observed in the first layer. Furthermore, the amount of lithium carbonate contained in the SEI coating is very small. Note that, as the Li1s peak, peaks attributed to compounds such as ROCOLi and ROLi can be detected.

[0058] When the first layer is analyzed by XPS, in addition to the first peak of O1s attributed to the C=O bond, a second peak of O1s attributed to the Li-O bond may be observed. The region of the coating present near the surface of the negative electrode active material contains a small amount of LiOH or Li 2 It may contain O.

[0059] Specifically, when the first layer included in the surface layer portion formed on the surface of the negative electrode composite layer is analyzed in the depth direction, a first region in which a first peak (O1s attributable to a C═O bond) and a second peak (O1s attributable to a Li—O bond) are observed, and the first peak intensity is greater than the second peak intensity, and a second region in which the first peak and the second peak are observed and the second peak intensity is greater than the first peak intensity may be observed, in order of increasing distance from the outermost surface of the surface layer portion. Furthermore, a third region may also be present that is closer to the outermost surface of the surface layer portion than the first region, and in which the first peak is observed but the second peak is not observed. The third region is more likely to be observed when the thickness of the lithium carbonate-containing region is large. The magnitude of the peak intensity may be determined by the height of the peak from the baseline.

[0060] At the center in the thickness direction of the first layer, the C1s peak attributed to a C—C bond is generally not observed, or even if observed, its intensity is half or less of the peak intensity attributed to a C═O bond.

[0061] Next, a method for forming the first layer containing lithium carbonate on the surface of the negative electrode mixture layer will be described. The step of forming the first layer can be performed by, for example, a vapor phase method, a coating method, or a transfer method.

[0062] Examples of the gas phase method include chemical vapor deposition, physical vapor deposition, and sputtering. For example, lithium carbonate may be deposited on the surface of the negative electrode composite layer using a vacuum deposition device. The pressure in the device chamber during deposition is, for example, 10 -2 ~10 -5 The temperature of the lithium carbonate evaporation source may be 400 to 600°C, and the temperature of the negative electrode mixture layer may be -20 to 80°C.

[0063] As a coating method, a solution or dispersion containing lithium carbonate can be applied to the surface of the negative electrode mixture layer using, for example, a microgravure coater, followed by drying to form the first layer. The lithium carbonate content in the solution or dispersion is, for example, 0.3 to 2 mass %, and when a solution is used, the concentration may be equal to or lower than the solubility (for example, about 0.9 to 1.3 mass % in an aqueous solution at room temperature).

[0064] Furthermore, a negative electrode can be obtained by forming a second layer containing a solid electrolyte so as to cover at least a portion of the first layer. That is, a surface layer portion can be formed on the surface of the negative electrode composite layer. The obtained surface layer portion has a first layer and a second layer. The second layer is formed so that at least a portion of it covers at least a portion (preferably the entire) of the surface of the negative electrode active material via the first layer (i.e., the first layer serves as a base layer).

[0065] The step of forming the second layer is performed in a state where the negative electrode mixture layer is in contact with the electrolyte, and therefore may also serve as at least a part of a step of pre-doping the negative electrode mixture layer with lithium ions. For example, metallic lithium may be used as a source of the pre-doped lithium ions.

[0066] The metallic lithium may be attached to the surface of the negative electrode mixture layer. Note that, for example, a first layer containing lithium carbonate having a thickness of 1 nm or more and 50 nm or less can also be formed by exposing a negative electrode having a negative electrode mixture layer to which metallic lithium is attached to a carbon dioxide gas atmosphere.

[0067] The step of attaching metallic lithium to the surface of the negative electrode mixture layer can be carried out by, for example, a vapor phase method, transfer, or the like. Examples of the vapor phase method include chemical vapor deposition, physical vapor deposition, and sputtering. For example, metallic lithium may be formed in the form of a film on the surface of the negative electrode mixture layer using a vacuum deposition device. The pressure in the chamber of the device during deposition is, for example, 10 -2 ~10 -5 The temperature of the lithium evaporation source may be 400 to 600°C, and the temperature of the negative electrode mixture layer may be -20 to 80°C.

[0068] The carbon dioxide gas atmosphere is preferably a dry atmosphere containing no moisture, and may have a dew point of, for example, -40°C or lower or -50°C or lower. The carbon dioxide gas atmosphere may contain gases other than carbon dioxide, but the molar fraction of carbon dioxide is preferably 80% or higher, and more preferably 95% or higher. It is preferable that the atmosphere does not contain any oxidizing gases, and the molar fraction of oxygen should be 0.1% or lower.

[0069] To form a thicker first layer, the partial pressure of carbon dioxide is set to, for example, 0.5 atmospheres (5.05×10 4It is efficient if the pressure is greater than 1 atmosphere (1.01 x 10 5 Pa) or more.

[0070] The temperature of the negative electrode exposed to the carbon dioxide gas atmosphere may be, for example, in the range of 15° C. to 120° C. The higher the temperature, the thicker the first layer becomes.

[0071] The thickness of the first layer can be easily controlled by changing the time for which the negative electrode is exposed to the carbon dioxide gas atmosphere. The exposure time may be, for example, 12 hours or more and less than 10 days.

[0072] The step of forming the first layer is preferably carried out before constructing the electrode body, but may be carried out after constructing the electrode body. That is, a positive electrode may be prepared, a negative electrode having a negative electrode mixture layer to which metallic lithium is attached may be prepared, a separator may be interposed between the positive electrode and the negative electrode to form an electrode body, and the electrode body may be exposed to a carbon dioxide gas atmosphere to form the first layer on the surface of the negative electrode mixture layer.

[0073] The pre-doping process of lithium ions into the negative electrode composite layer can be further carried out, for example, by subsequently contacting the negative electrode composite layer with an electrolyte and then leaving it for a predetermined period of time to complete the process. This process can be a process of forming a second layer to cover at least a portion of the first layer. For example, by charging and discharging the electrochemical capacitor at least once, the second layer can be formed in the negative electrode composite layer and the pre-doping of lithium ions into the negative electrode can be completed. Furthermore, for example, the pre-doping of lithium ions into the negative electrode can also be completed by applying a predetermined charging voltage (e.g., 3.4 to 4.0 V) between the terminals of the positive electrode and the negative electrode for a predetermined period of time (e.g., 1 to 75 hours).

[0074] Pre-doping of the negative electrode with lithium ions may be performed by contacting the negative electrode with an electrolyte solution having lithium ion conductivity before assembling the electrochemical capacitor. Metallic lithium may be used as the lithium ion source used for pre-doping. For example, a working electrode (e.g., a SUS metal plate) to which a negative electrode and a lithium ion source are attached is placed in a battery container filled with an electrolyte solution having lithium ion conductivity, with a separator interposed between the negative electrode and the working electrode. Pre-doping can be performed by applying a voltage between the positive electrode and the negative electrode, with the working electrode serving as the positive electrode (liquid-phase doping method). The voltage application can be performed, for example, under conditions in which a predetermined constant current flows between the positive electrode and the negative electrode. The voltage application time is, for example, 1 to 75 hours.

[0075] Metallic lithium as a lithium ion source may be attached to the surface of the negative electrode composite layer in advance, and the negative electrode with the attached metallic lithium may be placed in a battery container, and a voltage may be applied between the negative electrode and the working electrode to perform pre-doping (solid-phase doping method).

[0076] In the case of the liquid-phase doping method, if the concentration of the lithium salt in the electrolyte is reduced, the ionic conductivity of the electrolyte decreases, and the pre-doping process takes a long time. On the other hand, in the solid-phase doping method, metallic lithium is attached to the surface of the negative electrode mixture layer in advance, so the concentration of the lithium salt in the electrolyte has little effect on the processing time required for the pre-doping process.

[0077] Furthermore, in the process of forming the second layer (SEI coating) in the electrochemical capacitor, the amount of lithium salt required to react with the negative electrode composite layer is smaller when the first layer is formed using the solid-phase doping method than when the liquid-phase doping method is used. This is thought to be because the first layer formed by the solid-phase doping method is advantageous in that it coats the entire surface of the negative electrode composite layer and ensures a sufficient coating thickness. This prevents excessive increases in the amount of electrolyte and electrolyte concentration in the electrochemical capacitor, making it easier to obtain an electrochemical capacitor with low internal resistance and high output.

[0078] FIG. 1 schematically illustrates the configuration of an electrochemical capacitor 200 according to one embodiment of the present invention. The electrochemical capacitor 200 includes an electrode assembly 100, a nonaqueous electrolyte (not shown), a metal cell case 210 with a bottom that accommodates the electrode assembly 100 and the nonaqueous electrolyte, and a sealing plate 220 that seals the opening of the cell case 210. A gasket 221 is disposed around the periphery of the sealing plate 220, and the interior of the cell case 210 is sealed by crimping the open edge of the cell case 210 to the gasket 221. A positive electrode current collector 13 having a central through-hole 13h is welded to the positive electrode current collector exposed portion 11x. One end of a tab lead 15 is connected to the positive electrode current collector 13, and the other end is connected to the inner surface of the sealing plate 220. Thus, the sealing plate 220 functions as an external positive electrode terminal. On the other hand, the negative electrode current collector 23 is welded to the negative electrode current collector exposed portion 21x. The negative electrode current collector 23 is directly welded to a welding member provided on the inner bottom surface of the cell case 210. Therefore, the cell case 210 functions as an external negative electrode terminal.

[0079] Hereinafter, each component of the electrochemical capacitor according to the embodiment of the present invention will be described in more detail.

[0080] (Negative Electrode) The negative electrode comprises a negative electrode current collector and a negative electrode composite layer supported on the negative electrode current collector. The negative electrode composite layer contains a negative electrode active material that reversibly dopes with lithium ions. The negative electrode active material preferably contains non-graphitizable carbon (i.e., hard carbon). The thickness of the negative electrode composite layer is, for example, 10 to 300 μm per side of the negative electrode current collector.

[0081] The negative electrode current collector is made of a sheet-like metal material, such as a metal foil, a porous metal, or an etched metal. Examples of the metal material include copper, a copper alloy, nickel, and stainless steel.

[0082] The negative electrode current collector is a generally disk-shaped metal plate. The material of the negative electrode current collector is, for example, copper, copper alloy, nickel, stainless steel, etc. The material of the negative electrode current collector may be the same as the material of the negative electrode current collector.

[0083] The non-graphitizable carbon may have a (002) plane spacing (i.e., the spacing between carbon layers) d002 of 3.8 Å or more as measured by X-ray diffraction. The theoretical capacity of the non-graphitizable carbon is preferably, for example, 150 mAh / g or more. The use of non-graphitizable carbon makes it easier to obtain a negative electrode with a small low-temperature DCR and small expansion and contraction during charge and discharge. The non-graphitizable carbon preferably accounts for 50% by mass or more, more preferably 80% by mass or more, and even 95% by mass or more of the negative electrode active material. Furthermore, the non-graphitizable carbon preferably accounts for 40% by mass or more, more preferably 70% by mass or more, and even 90% by mass or more of the negative electrode composite layer.

[0084] As the negative electrode active material, non-graphitizable carbon and a material other than non-graphitizable carbon may be used in combination. Examples of materials other than non-graphitizable carbon that can be used as the negative electrode active material include graphitizable carbon (soft carbon), graphite (natural graphite, artificial graphite, etc.), lithium titanium oxide (spinel-type lithium titanium oxide, etc.), silicon oxide, silicon alloy, tin oxide, tin alloy, etc.

[0085] From the viewpoint of achieving high packing properties of the negative electrode active material in the negative electrode and easily suppressing side reactions with the electrolyte, the average particle size of the negative electrode active material (particularly non-graphitizable carbon) is preferably 1 μm to 20 μm, and more preferably 2 μm to 15 μm.

[0086] In this specification, the average particle size means the volume-based median diameter (D50) in the particle size distribution obtained by laser diffraction particle size distribution measurement.

[0087] The negative electrode mixture layer contains a negative electrode active material as an essential component, and optionally contains a conductive agent (conductive assistant), a binder, etc. Examples of the conductive agent include carbon black and carbon fiber. Examples of the binder include fluororesin, acrylic resin, rubber material, and cellulose derivative.

[0088] The negative electrode composite layer is formed, for example, by mixing a negative electrode active material with a conductive agent, a binder, and the like together with a dispersion medium to prepare a negative electrode composite slurry, applying the negative electrode composite slurry to a negative electrode current collector, and then drying the slurry.

[0089] The negative electrode mixture layer is pre-doped with lithium ions. This reduces the potential of the negative electrode, increasing the potential difference (i.e., voltage) between the positive electrode and the negative electrode, thereby improving the energy density of the electrochemical capacitor. The amount of lithium pre-doped may be, for example, approximately 50% to 95% of the maximum amount that can be occluded in the negative electrode mixture layer.

[0090] The potential of the negative electrode is, for example, 0.2 V or less relative to lithium. The above-mentioned potential of the negative electrode is the potential (25 ° C.) of the negative electrode at the completion of pre-doping of lithium ions (or during charging). Lithium ions are pre-doped in the first and second regions of the negative electrode (negative electrode composite layer). This reduces the potential of the negative electrode, increasing the potential difference (i.e., voltage) between the positive electrode and the negative electrode, and improving the energy density of the electrochemical capacitor. The amount of lithium to be pre-doped is set so that the potential of the negative electrode in the electrolyte after pre-doping is 0.2 V or less relative to metallic lithium.

[0091] The capacitance per unit mass of the negative electrode active material may be, for example, 1000 F / g or more. From the viewpoint of increasing the capacitance density of the electrochemical capacitor, the capacitance per unit mass of the negative electrode active material may be, for example, 30,000 F / g or less. The capacitance per unit mass of the negative electrode active material is usually larger than the capacitance per unit mass of the positive electrode active material, for example, 20 to 800 times the capacitance per unit mass of the positive electrode active material. The capacitance per unit mass of the negative electrode active material can be measured by the following method.

[0092] First, a negative electrode for evaluation was prepared by cutting it to a size of 31 mm x 41 mm. A 100 μm thick lithium metal foil was prepared as a counter electrode for the negative electrode by cutting it to a size of 40 mm x 50 mm. A 25 μm thick cellulose paper (e.g., product number TF4425) manufactured by Nippon Kodoshi Kogyo Co., Ltd. was used as a separator, and the negative electrode composite layer and the lithium metal foil were placed opposite each other to form an electrode assembly. The electrode assembly was then immersed in the electrolyte solution of Example 1 described below to form a cell.

[0093] The battery is charged at a constant current (CC) of 0.5 mA until the cell voltage reaches 0.01 V, then charged at a constant voltage (CV) for 1 hour, and then discharged at 0.5 mA until the cell voltage reaches 1.5 V. The capacitance per unit mass of the negative electrode active material is determined from the discharge time required for the negative electrode potential to change by 0.1 V from the potential of the negative electrode 1 minute after the start of discharge.

[0094] (Positive Electrode) The positive electrode includes a positive electrode current collector and a positive electrode mixture layer containing activated carbon and supported on the positive electrode current collector. The positive electrode mixture layer includes a positive electrode active material that is reversibly doped with anions, and the positive electrode active material includes activated carbon. The thickness of the positive electrode mixture layer is, for example, 10 to 300 μm per side of the positive electrode current collector.

[0095] The positive electrode current collector is made of a sheet-like metal material, such as a metal foil, a porous metal, or an etched metal. Examples of the metal material include aluminum, an aluminum alloy, nickel, and titanium.

[0096] The positive electrode current collector is a generally disk-shaped metal plate. A through-hole is preferably formed in the center of the positive electrode current collector to serve as a passage for the nonaqueous electrolyte. The material of the positive electrode current collector is, for example, aluminum, aluminum alloy, titanium, stainless steel, or the like. The material of the positive electrode current collector may be the same as the material of the positive electrode current collector.

[0097] The carbon material used as the positive electrode active material is preferably a porous carbon material, such as activated carbon or the carbon materials exemplified as the negative electrode active material (e.g., non-graphitizable carbon). Examples of raw materials for activated carbon include wood, coconut shells, coal, pitch, and phenolic resin. The activated carbon is preferably activated.

[0098] The average particle size of the activated carbon is not particularly limited, but is preferably 20 μm or less, and more preferably 3 μm to 15 μm.

[0099] The specific surface area of ​​the positive electrode mixture layer generally reflects the specific surface area of ​​the positive electrode active material. 2 / g or more, 2000m 2 / g or less is sufficient, and 2 / g or more, 1800m2 / g or less is desirable. The specific surface area of ​​the positive electrode composite layer is the BET specific surface area determined using a measuring device conforming to JIS Z8830 (e.g., a Tristar II 3020 manufactured by Shimadzu Corporation). Specifically, the electrochemical capacitor is disassembled, and the positive electrode is removed. Next, the positive electrode is washed with DMC and dried. Thereafter, the positive electrode composite layer is peeled from the positive electrode current collector, and approximately 0.5 g of a sample of the positive electrode composite layer is collected. Next, the specific surface area of ​​the collected sample is determined in accordance with the method for measuring the specific surface area of ​​the negative electrode composite layer already described.

[0100] The activated carbon preferably accounts for 50% by mass or more, more preferably 80% by mass or more, and even 95% by mass or more of the positive electrode active material, and more preferably 40% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more of the positive electrode mixture layer.

[0101] The positive electrode mixture layer contains a positive electrode active material as an essential component, and optionally contains a conductive agent, a binder, etc. Examples of the conductive agent include carbon black and carbon fiber. Examples of the binder include fluororesin, acrylic resin, rubber material, and cellulose derivative.

[0102] The positive electrode composite layer is formed, for example, by mixing a positive electrode active material, a conductive agent, a binder, and the like together with a dispersion medium to prepare a positive electrode composite slurry, applying the positive electrode composite slurry to a positive electrode current collector, and then drying the slurry.

[0103] (Separator) The separator may be a nonwoven fabric made of cellulose fiber, a nonwoven fabric made of glass fiber, a microporous membrane made of polyolefin, a woven fabric or a nonwoven fabric, etc. The thickness of the separator is, for example, 8 to 300 μm, and preferably 8 to 40 μm.

[0104] (Electrolyte) The electrolyte has lithium ion conductivity and contains, for example, a lithium salt and a solvent that dissolves the lithium salt. The lithium salt dissolved in the solvent contains lithium ions and anions. The anions of the lithium salt are reversibly doped and dedoped into the positive electrode. The lithium ions derived from the lithium salt are reversibly absorbed into and released from the negative electrode.

[0105] Examples of lithium salts include LiClO4 , LiBF 4 , LiPF 6 , LiAlCl 4 , LiSbF 6 , LiSCN, LiCF 3 SO 3 , LiFSO 3 , LiCF 3 CO 2 , LiAsF 6 , LiB 10 Cl 10 , LiCl, LiBr, LiI, LiBCl 4 , LiN(FSO 2 ) 2 , LiN(CF 3 SO 2 ) 2 These may be used alone or in combination of two or more. Among them, salts having a fluorine-containing anion are preferred, and lithium bis(fluorosulfonyl)imide, i.e., LiN(SO 2 F) 2 The concentration of the lithium salt in the electrolyte in a charged state (state of charge (SOC) 90 to 100%) is, for example, 0.2 to 5 mol / L. Hereinafter, LiN(SO 2 F) 2 For example, 80 mass % or more of the lithium salt may be LiFSI.

[0106] The use of LiFSI tends to significantly reduce the rate of increase in low-temperature DCR. LiFSI is thought to have the effect of reducing the degradation of positive and negative electrode active materials. Among salts having fluorine-containing anions, the FSI anion is highly stable, so it is thought to be less likely to produce by-products and contribute to smooth charge and discharge without damaging the surface of the active material. In particular, when increasing the capacity of the positive electrode and the specific surface area of ​​the negative electrode composite layer, the effect of suppressing degradation (the effect of suppressing the increase in low-temperature DCR) by using LiFSI, which significantly reduces the impact of by-products on each active material, becomes significant.

[0107] Examples of solvents that can be used include cyclic carbonates such as ethylene carbonate, propylene carbonate, and butylene carbonate, chain carbonates such as dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate, aliphatic carboxylic acid esters such as methyl formate, methyl acetate, methyl propionate, and ethyl propionate, lactones such as γ-butyrolactone and γ-valerolactone, chain ethers such as 1,2-dimethoxyethane (DME), 1,2-diethoxyethane (DEE), and ethoxymethoxyethane (EME), cyclic ethers such as tetrahydrofuran and 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, acetamide, dimethylformamide, dioxolane, acetonitrile, propionitrile, nitromethane, ethyl monoglyme, trimethoxymethane, sulfolane, methyl sulfolane, and 1,3-propane sultone. These may be used alone or in combination of two or more.

[0108] The electrolyte solution may contain various additives as needed. For example, an unsaturated carbonate such as vinylene carbonate, vinylethylene carbonate, or divinylethylene carbonate may be added as an additive for forming a lithium ion conductive coating on the surface of the negative electrode.

[0109] (Additional Note) The above description discloses the following technology: (Technology 1) A battery comprising: a positive electrode including a positive electrode current collector and a positive electrode mixture layer containing activated carbon and supported on the positive electrode current collector; a negative electrode including a negative electrode current collector and a negative electrode mixture layer containing a negative electrode active material that reversibly dopes lithium ions and supported on the negative electrode current collector; and an electrolytic solution including an electrolyte containing lithium ions and an anion and a non-aqueous solvent, wherein the ratio of the amount of the anion to the surface area of ​​the positive electrode mixture layer is 1.5 μmol / m 2 Above, 2.4 μmol / m 2 (Technology 2) An electrochemical capacitor in which the ratio of the amount of the anions to the surface area of ​​the positive electrode mixture layer is 1.7 μmol / m or less. 2 Above, 2.2 μmol / m 2The electrochemical capacitor according to Technology 1, wherein the electrolytic solution contains lithium bis(fluorosulfonyl)imide. (Technology 3) The electrochemical capacitor according to Technology 1 or 2, wherein the electrolytic solution contains lithium bis(fluorosulfonyl)imide. (Technology 4) The electrochemical capacitor according to any one of Technology 1 to 3, wherein the negative electrode active material contains non-graphitizable carbon. (Technology 5) The electrochemical capacitor according to any one of Technology 1 to 4, wherein the potential of the negative electrode is 0.2 V or less vs. lithium. (Technology 6) The electrochemical capacitor according to Technology 1, wherein a surface layer portion having a first layer containing lithium carbonate is formed on the surface of the negative electrode mixture layer. (Technology 7) The electrochemical capacitor according to Technology 6, wherein the surface layer portion formed on the surface of the negative electrode mixture layer has a second layer containing a solid electrolyte, and at least a portion of the second layer covers at least a portion of the surface of the negative electrode mixture layer via the first layer. (Technology 8) The electrochemical capacitor according to Technology 7, wherein the second layer contains lithium carbonate, and the content of the lithium carbonate in the second layer is lower than the content of the lithium carbonate in the first layer. (Technology 9) The electrochemical capacitor according to any one of Techniques 6 to 8, wherein the first layer has a thickness of 1 nm or more and 50 nm or less. (Technology 10) The electrochemical capacitor according to Technique 7 or 8, wherein when the first layer is measured by X-ray photoelectron spectroscopy, a substantial F1s peak assigned to a LiF bond is not observed, and when the second layer is measured by X-ray photoelectron spectroscopy, a substantial F1s peak assigned to a LiF bond is observed.

[0110] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.

[0111] [Examples] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples. Table 1 shows an outline of the configuration of each electrochemical capacitor fabricated below.

[0112] (Electrochemical Capacitors A1-A5, B1-B2) (1) Preparation of Positive Electrode A 20 μm thick aluminum foil (positive electrode current collector) was prepared. Separately, 88 parts by mass of activated carbon (average particle size 5.5 μm) as the positive electrode active material, 2 parts by mass of polytetrafluoroethylene (PTFE) as a binder, 4 parts by mass of carboxymethyl cellulose (CMC) as a thickener, and 6 parts by mass of acetylene black (AB) as a conductive additive were dispersed in water to prepare a positive electrode composite slurry. The resulting positive electrode composite slurry was applied to both sides of aluminum foil, and the coating was dried and rolled to form a positive electrode composite layer, thereby obtaining a positive electrode. A 10 mm wide positive electrode current collector exposed portion was formed at the longitudinal end of the positive electrode current collector. The weight of the positive electrode composite layer contained per cell of the electrochemical capacitor in the resulting positive electrode was 2.3 g. The specific surface area b of the positive electrode mixture layer is 1407 m 2 / g, and the surface area B of the positive electrode composite layer is 3285 m per cell of the electrochemical capacitor. 2 It was.

[0113] (2) Preparation of Negative Electrode A copper foil (negative electrode current collector) with a thickness of 8 μm was prepared. Meanwhile, the negative electrode active material, non-graphitizable carbon (HC) (average particle size 5 μm), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR), were dispersed in water to prepare a negative electrode composite slurry. The resulting negative electrode composite slurry was applied to both sides of copper foil, and the coating was dried and rolled to form a negative electrode composite layer, resulting in a negative electrode.

[0114] Thereafter, a thin film of metallic lithium for pre-doping was formed on the entire surface of the negative electrode mixture layer by vacuum deposition. The amount of lithium to be pre-doped was set so that the potential of the negative electrode in the non-aqueous electrolyte after pre-doping was 0.2 V or less relative to metallic lithium.

[0115] Thereafter, the chamber of the device was purged with carbon dioxide to create a carbon dioxide gas atmosphere, thereby forming a first layer containing lithium carbonate on the surface of the negative electrode mixture layer. The carbon dioxide gas atmosphere had a dew point of −40° C., a molar fraction of carbon dioxide of 100%, and a pressure in the chamber of 1 atmosphere (1.01×10 5The temperature of the negative electrode exposed to the carbon dioxide gas atmosphere at 1 atmosphere was 25°C. The time for exposing the negative electrode to the carbon dioxide gas atmosphere was 22 hours. The first layer did not substantially contain F (or LiF).

[0116] The mixing ratio of non-graphitizable carbon (HC), carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) in the negative electrode mixture slurry was HC:CMC:SBR=97:1:2 by mass.

[0117] (3) Fabrication of Electrode Assembly The positive and negative electrodes were wound into a cylindrical shape with a cellulose nonwoven separator (25 μm thick) interposed therebetween to form an electrode assembly. The exposed portion of the positive electrode current collector protruded from one end of the wound assembly, and the exposed portion of the negative electrode current collector protruded from the other end of the electrode assembly. A disk-shaped positive electrode current collector and a disk-shaped negative electrode current collector were welded to the exposed portion of the positive electrode current collector and the exposed portion of the negative electrode current collector, respectively.

[0118] (4) Preparation of Non-Aqueous Electrolyte Solution Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 3:5:2, and 0.2 mass% of vinylene carbonate (VC) was added to prepare a solvent. LiFSI was dissolved in the resulting solvent as a lithium salt at the molar concentration shown in Table 1 to prepare a non-aqueous electrolyte solution.

[0119] (5) Assembly of an electrochemical capacitor The electrode assembly was housed in a bottomed cell case having an opening, a tab lead connected to the positive electrode current collector was connected to the inner surface of the sealing plate, and a negative electrode current collector was welded to the inner bottom surface of the cell case. After pouring a nonaqueous electrolyte into the cell case in the amount shown in Table 1, the opening of the cell case was sealed with a sealing plate to assemble an electrochemical capacitor as shown in FIG.

[0120]

[0121] Thereafter, aging was performed at 60° C. while a charging voltage of 3.8 V was applied between the terminals of the positive electrode and the negative electrode to complete pre-doping of lithium ions into the negative electrode.

[0122] In this way, a plurality of electrochemical capacitors A1 to A5 and B1 to B2 were produced while varying the molar concentration of the electrolyte contained in the electrolytic solution and the mass of the electrolytic solution, and the following evaluations were carried out.

[0123] (6) Evaluation (Measurement of Internal Resistance of Electrochemical Capacitor) Immediately after aging, the electrochemical capacitor was subjected to a current of 2 mA / cm per positive electrode area in an environment of −30° C. until the voltage reached 3.8 V. 2 After that, the battery was charged at a constant current density of 2 mA / cm per positive electrode area in an environment of −30° C. until the voltage reached 2.2 V. 2 A constant current discharge was carried out at a current density of .

[0124] For the discharge curve (vertical axis: discharge voltage, horizontal axis: discharge time) obtained by the above discharge, a linear approximation line was calculated for the range of 0.5 to 2 seconds after the start of discharge of the discharge curve, and the voltage VS at the intercept of the approximation line was calculated. The value (V0-VS) obtained by subtracting the voltage VS from the voltage VO at the start of discharge (0 seconds after the start of discharge) was calculated as ΔV. ΔV (V) and the current value during discharge (current density per positive electrode area 2 mA / cm 2 × positive electrode area) was used to calculate the internal resistance (DCR) R1 (Ω) of the electrochemical capacitor according to the following formula.

[0125] Internal resistance R1=ΔV / Id

[0126] (Float Test of Electrochemical Capacitor) Next, a float test was performed in which a constant voltage of 3.8 V was applied to the electrochemical capacitor in an environment of 85° C. for 1000 hours. Thereafter, the internal resistance (DCR) R2 (Ω) of the electrochemical capacitor was determined in an environment of −30° C. in the same manner as R1.

[0127] Table 2 shows the capacitances C2 and internal resistances R2 of electrochemical capacitors A1 to A5 and B1 to B2 after the float test. In Table 2, C2 and R2 are shown as relative values, with the capacitances C2 and R2 of electrochemical capacitor A3 after the float test set at 100. Electrochemical capacitors A1 to A5 are examples, and B1 and B2 are comparative examples. Table 2 also shows the ratio A / B of the amount of anion to the surface area of ​​the positive electrode composite layer, along with the evaluation results after the float test.

[0128] From Table 2, A / B is 1.5 to 2.4 μmol / m 2 The electrochemical capacitors A1 to A5 in the range of 2 In the electrochemical capacitors A2 to A4, the internal resistance R2 after the float test was significantly reduced, and excellent output characteristics were obtained.

[0129] On the other hand, electrochemical capacitor B1 not only did not exhibit sufficient capacity due to its small A / B ratio, but also showed an increase in internal resistance R2 after the float test. This is presumably due to an insufficient amount of anions A reversibly doped onto the surface of the positive electrode composite layer. Electrochemical capacitor B2, on the other hand, exhibited sufficient capacity due to its large A / B ratio, but showed an increase in internal resistance R2 after the float test.

[0130] Comparing electrochemical capacitors A1 to A5, B1 and B2, the internal resistance R2 after the float test was 2.0 μmol / m 2 The lowest value was found in electrochemical capacitor A3, where A / B was 1.5 to 2.4 μmol / m 2 It was found that the internal resistance R2 after the float test could be maintained at a sufficiently low value within this range.

[0131]

[0132] The electrochemical capacitor according to the present invention is suitable for use in vehicles, for example.

[0133] 100: Electrode body 10: Positive electrode 11x: Positive electrode current collector exposed portion 13: Positive electrode current collector plate 15: Tab lead 20: Negative electrode 21x: Negative electrode current collector exposed portion 23: Negative electrode current collector plate 30: Separator 200: Electrochemical capacitor 210: Cell case 220: Sealing plate 221: Gasket

Claims

1. A battery comprising: a positive electrode including a positive electrode current collector and a positive electrode mixture layer including activated carbon and supported on the positive electrode current collector; a negative electrode including a negative electrode current collector and a negative electrode mixture layer including a negative electrode active material that reversibly dopes lithium ions and supported on the negative electrode current collector; and an electrolyte solution including an electrolyte including lithium ions and an anion and a non-aqueous solvent, wherein the ratio of the amount of the anion to the surface area of ​​the positive electrode mixture layer is 1.5 μmol / m 2 Above, 2.4 μmol / m 2 An electrochemical capacitor.

2. The ratio of the amount of the anion to the surface area of ​​the positive electrode mixture layer is 1.7 μmol / m 2 Above, 2.2 μmol / m 2 2. The electrochemical capacitor of claim 1 , wherein:

3. The electrochemical capacitor of claim 1 or 2, wherein the electrolyte contains lithium bis(fluorosulfonyl)imide.

4. The electrochemical capacitor according to claim 1 or 2, wherein the negative electrode active material comprises non-graphitizable carbon.

5. The electrochemical capacitor according to claim 1 or 2, wherein the potential of the negative electrode is 0.2 V or less versus lithium.

6. The electrochemical capacitor according to claim 1, wherein a surface portion having a first layer containing lithium carbonate is formed on the surface of the negative electrode mixture layer.

7. The electrochemical capacitor according to claim 6, wherein a surface layer portion formed on the surface of the negative electrode mixture layer has a second layer containing a solid electrolyte, and at least a portion of the second layer covers at least a portion of the surface of the negative electrode mixture layer via the first layer.

8. The electrochemical capacitor according to claim 7, wherein the second layer contains lithium carbonate, and the content of the lithium carbonate contained in the second layer is less than the content of the lithium carbonate contained in the first layer.

9. The electrochemical capacitor according to any one of claims 6 to 8, wherein the first layer has a thickness of 1 nm or more and 50 nm or less.

10. The electrochemical capacitor according to claim 7 or 8, wherein, when the first layer is measured by X-ray photoelectron spectroscopy, a substantial F1s peak attributable to a LiF bond is not observed, and when the second layer is measured by X-ray photoelectron spectroscopy, a substantial F1s peak attributable to a LiF bond is observed.

Citation Information

Patent Citations

  • Capacitor

    JP2013165161A

  • Nonaqueous electrolyte and power storage device including the same

    JP2015191851A

  • Lithium ion battery and negative electrode active material for lithium ion capacitor

    JP2017195102A

  • Electrochemical device

    WO2023026921A1