Electromagnetic wave shielding material, electronic component, and electronic device

The multilayer electromagnetic shielding material with a magnetic layer and specific metal layers provides excellent heat resistance and durability, effectively addressing the challenges of maintaining shielding ability under high temperatures and external forces in electronic components and devices.

WO2024203029A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008284
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-05
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Electromagnetic shielding materials face challenges in maintaining high shielding ability under high temperatures and durability against external forces, especially when incorporated into electronic components and devices.

Method used

A multilayer electromagnetic shielding material is developed, comprising a magnetic layer with magnetic particles and an acrylic resin sandwiched between two metal layers, with specific organic solvent content and molecular weight ranges, and using metals like Cu and Al for enhanced performance.

Benefits of technology

The material exhibits excellent heat resistance and durability, effectively shielding electromagnetic waves and withstanding external forces, thus protecting electronic components and devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure 00000049_0000
    Figure 00000049_0000
Patent Text Reader

Abstract

Provided are: an electromagnetic wave shielding material which has, between two metal layers, a magnetic layer containing magnetic particles and an acrylic resin, and in which the content of an organic solvent in the magnetic layer is not less than 5 ppm but less than 1000 ppm in terms of mass; and an electronic component and an electronic device which include the electromagnetic wave shielding material.
Need to check novelty before this filing date? Find Prior Art

Description

Electromagnetic wave shielding materials, electronic components and electronic equipment

[0001] The present invention relates to an electromagnetic wave shielding material, an electronic component, and an electronic device.

[0002] Patent Document 1 discloses a noise suppression sheet that includes at least one of a soft magnetic material and a dielectric material.

[0003] JP 2010-97969 A

[0004] In recent years, electromagnetic wave shielding materials have been attracting attention as materials for reducing the effects of electromagnetic waves in various electronic components and electronic devices. Electromagnetic wave shielding materials can exhibit electromagnetic wave shielding performance (hereinafter also referred to as "electromagnetic wave shielding ability" or "shielding ability") by reflecting and / or attenuating electromagnetic waves incident on the electromagnetic wave shielding material. For example, the noise suppression sheet described in Patent Document 1 can function as an electromagnetic wave shielding material.

[0005] Electromagnetic wave shielding materials may be exposed to high temperatures when incorporated into electronic components or various electronic devices. Therefore, it is desirable for electromagnetic wave shielding materials to be able to exhibit high shielding ability after being exposed to high temperatures. Electromagnetic wave shielding materials that exhibit high shielding ability against electromagnetic waves after being exposed to high temperatures can contribute to significantly reducing the effects of electromagnetic waves in electronic components and electronic devices. Hereinafter, exhibiting high shielding ability after being exposed to high temperatures is also referred to as having high heat resistance or excellent heat resistance.

[0006] Furthermore, an external force may be applied to an electromagnetic wave shielding material during molding, and even after molding and incorporation into an electronic component or electronic device, an external force may be applied thereto due to, for example, a drop, a collision, etc. Durability that can withstand such external forces is also one of the properties desired for an electromagnetic wave shielding material.

[0007] In view of the above, an object of one aspect of the present invention is to provide an electromagnetic wave shielding material that is excellent in heat resistance and durability.

[0008] One aspect of the present invention is as follows: [1] An electromagnetic shielding material having a magnetic layer containing magnetic particles and an acrylic resin between two metal layers, wherein the magnetic layer contains an organic solvent in an amount of 5 ppm or more and less than 1,000 ppm by mass. [2] The electromagnetic shielding material according to [1], wherein the acrylic resin has a weight-average molecular weight of 100,000 or more. [3] The electromagnetic shielding material according to [1] or [2], wherein the acrylic resin has a weight-average molecular weight of 800,000 or more and 2,000,000 or less. [4] The electromagnetic shielding material according to any one of [1] to [3], wherein the organic solvent in the magnetic layer contains 10 ppm or more and 100 ppm or less. [5] The electromagnetic shielding material according to any one of [1] to [4], wherein the organic solvent is selected from the group consisting of methyl ethyl ketone and cyclohexanone. [6] The electromagnetic shielding material according to any one of [1] to [5], wherein one or more layers containing a resin are disposed between the magnetic layer sandwiched between the two metal layers and one or both of the two metal layers. [7] The electromagnetic shielding material according to any one of [1] to [6], comprising two or more multilayer structures each having the magnetic layer between two metal layers. [8] The electromagnetic shielding material according to any one of [1] to [7], wherein at least one of the metal layers has a Cu content of 80.0% by mass or more. [9] The electromagnetic shielding material according to any one of [1] to [8], wherein at least one of the metal layers has an Al content of 80.0% by mass or more.

[10] The electromagnetic shielding material according to any one of [1] to [9], wherein the acrylic resin has a weight-average molecular weight of 800,000 to 2,000,000, the magnetic layer has an organic solvent content of 10 ppm to 100 ppm, and the organic solvent is selected from the group consisting of methyl ethyl ketone and cyclohexanone, the electromagnetic shielding material comprises two or more multilayer structures each having the magnetic layer between two metal layers, and at least one of the metal layers has a Cu content of 80.0% by mass or more.

[11] The electromagnetic wave shielding material according to any one of [1] to [9], wherein the weight-average molecular weight of the acrylic resin is 800,000 or more and 2,000,000 or less, the organic solvent content of the magnetic layer is 10 ppm or more and 100 ppm or less, the organic solvent is selected from the group consisting of methyl ethyl ketone and cyclohexanone, the material includes two or more multilayer structures having the magnetic layer between two metal layers, and at least one of the metal layers has an Al content of 80.0 mass % or more.

[12] An electronic component comprising the electromagnetic wave shielding material according to any one of [1] to

[11] .

[13] An electronic device comprising the electromagnetic wave shielding material according to any one of [1] to

[11] .

[0009] According to one aspect of the present invention, it is possible to provide an electromagnetic wave shielding material having excellent heat resistance and durability, and also to provide an electronic component and an electronic device including the electromagnetic wave shielding material.

[0010] 1 is an explanatory diagram relating to measurement of peel strength;

[0011] [Electromagnetic wave shielding material] One aspect of the present invention relates to an electromagnetic wave shielding material having a magnetic layer containing magnetic particles and an acrylic resin between two metal layers, and the organic solvent content of the magnetic layer is 5 ppm or more and less than 1000 ppm by mass.

[0012] In the present invention and this specification, the term "electromagnetic wave shielding material" refers to a material that can exhibit shielding ability against electromagnetic waves of at least one frequency or at least a part of a frequency band. "Electromagnetic waves" include magnetic waves and electric waves. An "electromagnetic wave shielding material" can be a material that can exhibit shielding ability against one or both of magnetic waves of at least one frequency or at least a part of a frequency band, and electric waves of at least one frequency or at least a part of a frequency band.

[0013] In the present invention and this specification, the term "magnetic" means ferromagnetic property. The magnetic layer will be described in detail later.

[0014] The inventors speculate that the electromagnetic wave shielding material's multilayer structure, in which a magnetic layer is sandwiched between two metal layers, contributes to the material's ability to exhibit high shielding capability against electromagnetic waves. More specifically, to achieve high shielding capability against electromagnetic waves in an electromagnetic wave shielding material, it is desirable to enhance the electromagnetic wave attenuation capability as well as increase reflection at the interface. That is, it is desirable for electromagnetic waves to be significantly attenuated by repeatedly reflecting at the interface and passing through the electromagnetic wave shielding material multiple times. However, in terms of the behavior of the metal layer and the magnetic layer with respect to electromagnetic waves, the metal layer tends to have a high electromagnetic wave attenuation capability but low magnetic wave reflection at the interface, while the magnetic layer tends to have a lower electromagnetic wave attenuation capability than the metal layer but high magnetic wave reflection at the interface. Therefore, it is difficult for a metal layer or a magnetic layer alone to achieve both high reflection and attenuation of magnetic waves, especially electromagnetic waves. In contrast, the electromagnetic wave shielding material can achieve both high interface reflection and attenuation within the layers by including a multilayer structure with a magnetic layer between two metal layers. The inventors believe that this is the reason why the electromagnetic wave shielding material exhibits high shielding ability against magnetic waves. Furthermore, the magnetic layer included in the multilayer structure contains an acrylic resin. It is believed that the main chain of acrylic resin is resistant to thermal decomposition due to the carbon-carbon saturated bonds in the main chain. The inventors believe that the inclusion of an acrylic resin in the magnetic layer contributes to the electromagnetic wave shielding material being able to exhibit high shielding ability without a significant decrease even after being exposed to high temperatures. Additionally, the inventors believe that an organic solvent content of 5 ppm or more and less than 1000 ppm by mass in the magnetic layer included in the multilayer structure can contribute to improving the durability of the electromagnetic wave shielding material. The inventors believe that an organic solvent content of 5 ppm or more contributes to improving adhesion between the magnetic layer and adjacent layers, and that an organic solvent content of less than 1000 ppm contributes to making the magnetic layer less susceptible to plastic deformation, thereby improving the durability of the electromagnetic wave shielding material. However, the present invention is not limited to the speculations described herein.

[0015] <Magnetic Layer> (Magnetic Particles) The magnetic particles may be one selected from the group consisting of magnetic particles generally called soft magnetic particles, such as metal particles and ferrite particles, or a combination of two or more types. Metal particles generally have a saturation magnetic flux density about two to three times that of ferrite particles, and therefore can maintain relative permeability without magnetic saturation even under strong magnetic fields, thereby exhibiting shielding capability. Therefore, it is preferable that the magnetic particles contained in the magnetic layer are metal particles. In the present invention and this specification, a layer containing metal particles as magnetic particles is considered to be a "magnetic layer."

[0016] Metal Particles Examples of metal particles serving as the magnetic particles include particles of sendust (Fe—Si—Al alloy), permalloy (Fe—Ni alloy), molybdenum permalloy (Fe—Ni—Mo alloy), Fe—Si alloy, Fe—Cr alloy, Fe-containing alloy generally referred to as iron-based amorphous alloy, Co-containing alloy generally referred to as cobalt-based amorphous alloy, alloy generally referred to as nanocrystalline alloy, iron, permendur (Fe—Co alloy), and the like. Among these, sendust is preferred because it exhibits high saturation magnetic flux density and relative permeability. In addition to the constituent elements of the metal (including alloys), the metal particles may contain, in any content, elements contained in additives that may be added optionally and / or elements contained in impurities that may be unintentionally mixed in during the manufacturing process of the metal particles. In the metal particles, the content of the constituent elements of the metal (including alloys) is preferably 90.0% by mass or more, more preferably 95.0% by mass or more, and may also be 100% by mass, less than 100% by mass, 99.9% by mass or less, or 99.0% by mass or less.

[0017] In one embodiment, the electromagnetic wave shielding ability of an electromagnetic wave shielding material against electromagnetic waves can be evaluated using the magnetic permeability (more specifically, the real part of the complex relative magnetic permeability) of the magnetic layer included in the electromagnetic wave shielding material as an index. An electromagnetic wave shielding material having a magnetic layer exhibiting high magnetic permeability (more specifically, the real part of the complex relative magnetic permeability) is preferred because it can exhibit high shielding ability against electromagnetic waves.

[0018] When complex relative permeability is measured using a magnetic permeability measuring device, a real part μ' and an imaginary part μ" are usually displayed. In the present invention and this specification, the real part of complex relative permeability refers to this real part μ'. Hereinafter, the real part of complex relative permeability at a frequency of 3 MHz (megahertz) will also be referred to simply as "magnetic permeability" or "magnetic permeability μ'". Magnetic permeability can be measured using a commercially available magnetic permeability measuring device or a magnetic permeability measuring device with a known configuration. The measurement temperature is 25°C. By setting the ambient temperature surrounding the measurement sample to the measurement temperature, temperature equilibrium is established, and the temperature of the measurement sample can be set to the measurement temperature. From the perspective of being able to exhibit even better electromagnetic wave shielding ability, the magnetic permeability (real part of complex relative permeability at a frequency of 3 MHz) of the magnetic layer contained in the electromagnetic wave shielding material is preferably 40 or more, and more preferably 100 or more, before and after thermal aging at 80°C, as determined by the method described in the Examples section below. The magnetic permeability may be, for example, 500 or less, 300 or less, or 200 or less, and may even exceed the values ​​exemplified here. Electromagnetic shielding materials with high magnetic permeability are preferred because they can exhibit excellent electromagnetic shielding ability.

[0019] From the viewpoint of forming a magnetic layer exhibiting high magnetic permeability, the magnetic particles are preferably particles having a flat shape (flat-shaped particles), and more preferably metal particles having a flat shape. By arranging the long side direction of the flat-shaped particles so that they are more parallel to the in-plane direction of the magnetic layer, the long side direction of the particles is more aligned with the vibration direction of the electromagnetic waves incident perpendicular to the electromagnetic wave shielding material, thereby reducing the demagnetizing field, and the magnetic layer can exhibit higher magnetic permeability. In the present invention and this specification, "flat-shaped particles" refers to particles having an aspect ratio of 0.200 or less. The aspect ratio of flat-shaped particles is preferably 0.150 or less, more preferably 0.100 or less. The aspect ratio of flat-shaped particles can be, for example, 0.010 or more, 0.020 or more, or 0.030 or more. For example, the particle shape can be made flat by flattening using a known method. For details on the flattening process, see, for example, the description in JP 2018-131640 A, including paragraphs 0016 and 0017 and the Examples therein. An example of a magnetic layer exhibiting high magnetic permeability is a magnetic layer containing flat particles of sendust.

[0020] As described above, from the viewpoint of forming a magnetic layer that exhibits high magnetic permeability, it is preferable to arrange the long side direction of the flat particles so that it is closer to parallel to the in-plane direction of the magnetic layer.From this point of view, the orientation degree, which is the sum of the absolute value of the average orientation angle of the flat particles relative to the surface of the magnetic layer and the variance of the orientation angle, is preferably 30° or less, more preferably 25° or less, even more preferably 20° or less, and even more preferably 15° or less.The orientation degree can be, for example, 3° or more, 5° or more, or 10° or more, and can also be lower than the values ​​exemplified here.The method for controlling the orientation degree will be described later.

[0021] In the present invention and this specification, the aspect ratio of the magnetic particles and the degree of orientation are determined by the following method. A cross section of the magnetic layer is exposed by a known method. A cross section image of a randomly selected region of this cross section is obtained as a scanning electron microscope (SEM) image. The imaging conditions are an acceleration voltage of 2 kV and a magnification of 1000x, and an SEM image is obtained as a backscattered electron image. The second argument is set to 0 using the cv2.imread() function of the image processing library OpenCV4 (manufactured by Intel Corporation), and the image is read in grayscale. A binarized image is obtained using the cv2.threshold() function, with the intermediate brightness between the high-brightness and low-brightness areas as the boundary. White areas (high-brightness areas) in the binarized image are identified as magnetic particles. The obtained binarized image is subjected to cv2.imread(). A rotated circumscribing rectangle corresponding to each magnetic particle portion is calculated using the minAreaRect() function, and the long side length, short side length, and rotation angle are calculated as the return values ​​of the cv2.minAreaRect() function. When calculating the total number of magnetic particles contained in the binarized image, particles in which only a portion of the particle is included in the binarized image are also included. For particles in which only a portion of the particle is included in the binarized image, the long side length, short side length, and rotation angle are calculated for the portion included in the binarized image. The ratio of the short side length to the long side length calculated in this manner (short side length / long side length) is used as the aspect ratio of each magnetic particle. In the present invention and this specification, if the number of magnetic particles identified as flat-shaped particles with an aspect ratio of 0.200 or less is 10% or more by number of the total number of magnetic particles contained in the binarized image, the magnetic layer is determined to be a "magnetic layer containing flat-shaped particles as magnetic particles." Furthermore, from the rotation angle determined above, the "orientation angle" is determined as the rotation angle relative to the horizontal plane (surface of the magnetic layer). Particles with an aspect ratio of 0.200 or less determined in the binarized image are identified as flat-shaped particles. The sum of the absolute value of the average value (arithmetic mean) and the variance of the orientation angles of all flat-shaped particles contained in the binarized image is determined. The sum thus determined is the "degree of orientation."The coordinates of the circumscribed rectangle are calculated using the cv2.boxPoints() function, and an image is created by overlaying the rotated circumscribed rectangle on the original image using the cv2.drawContours() function. Any rotated circumscribed rectangles that are clearly misdetected are excluded from the calculation of the aspect ratio and degree of orientation. The average value (arithmetic mean) of the aspect ratios of particles identified as flat-shaped particles is used as the aspect ratio of the flat-shaped particles contained in the magnetic layer to be measured. This aspect ratio is 0.200 or less, preferably 0.150 or less, and more preferably 0.100 or less. The aspect ratio can be, for example, 0.010 or more, 0.020 or more, or 0.030 or more.

[0022] The content of magnetic particles in the magnetic layer can be, for example, 50 parts by weight or more, 60 parts by weight or more, 70 parts by weight or more, or 80 parts by weight or more, and can be, for example, 87 parts by weight or less, 85 parts by weight or less, 80 parts by weight or less, or 75 parts by weight or less, based on 100 parts by weight of the total weight of the magnetic layer. The magnetic layer can contain only one type of magnetic particle, or two or more types of magnetic particles in any ratio. In the present invention and this specification, when two or more types of a component are contained, the "content" refers to the total content of those components. The content of various components in the magnetic layer can be determined by known methods such as TG / DTA (Thermogram / Differential Thermal Analysis) or extraction of various components using a solvent. "TG / DTA" is generally referred to as thermogravimetry / differential thermal analysis. When the composition of the magnetic layer-forming composition used to form the magnetic layer is known, the contents of the various components in the magnetic layer can also be determined from this known composition.

[0023] In one embodiment, the magnetic layer can be an insulating layer. In the present invention and this specification, "insulating" refers to an electrical conductivity of less than 1 S (Siemens) / m. The electrical conductivity of a certain layer is calculated from the surface electrical resistivity of the layer and the thickness of the layer using the following formula. Electrical conductivity can be measured using a known method. Electrical conductivity [S / m] = 1 / (surface electrical resistivity [Ω] × thickness [m])

[0024] The present inventors believe that the magnetic layer being an insulating layer is preferable for the electromagnetic wave shielding material to exhibit even higher electromagnetic wave shielding ability. From this point of view, the electrical conductivity of the magnetic layer is preferably less than 1 S / m, more preferably 0.5 S / m or less, even more preferably 0.1 S / m or less, and even more preferably 0.05 S / m or less. The electrical conductivity of the magnetic layer is, for example, 1.0×10 -12 S / m or more or 1.0 x 10 -10 It can be S / m or more.

[0025] (Acrylic Resin) In this invention and this specification, a layer containing both magnetic particles and a resin is considered to be a "magnetic layer." The resin can function as a binder in the magnetic layer. The magnetic layer of the above-mentioned electromagnetic wave shielding material contains an acrylic resin. In this invention and this specification, "acrylic resin" refers to a (meth)acrylate polymer. The polymer includes homopolymers and copolymers. In this invention and this specification, "(meth)acrylate" refers to a compound containing one or more (meth)acryloyl groups per molecule, and the term "(meth)acryloyl group" is used to refer to either or both of an acryloyl group and a methacryloyl group. Furthermore, a (meth)acryloyl group may be contained in a (meth)acrylate in the form of a (meth)acryloyloxy group. The term "(meth)acryloyloxy group" is used to refer to either or both of an acryloyloxy group and a methacryloyloxy group.

[0026] Examples of (meth)acrylates include acrylic acid esters such as methyl acrylate, ethyl acrylate, n-(normal)-butyl acrylate, isobutyl acrylate, t-(tertiary)-butyl acrylate, cyclohexyl acrylate, and benzyl acrylate; and methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, t-butyl methacrylate, cyclohexyl methacrylate, and benzyl methacrylate; and these may be used alone or in combination of two or more. In one embodiment, ethyl acrylate and n-butyl acrylate are preferred as the (meth)acrylate.

[0027] An example of the acrylic resin is a copolymer of at least one selected from the group consisting of a hydroxyl group-containing compound, an unsaturated carboxylic acid, and a compound represented by the following general formula 1 with a (meth)acrylate.

[0028] General formula 1 CH 2 = C(X)R 1

[0029] In general formula 1, R 1 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group, a —CN group, or a —CO—R 2 group, —O—CO—R 3 group, -OR 4 group or -(CH 2 ) n -O-R 5 represents a group. 2 , R 3 , R 4 and R 5 each independently represents a hydrogen atom or an organic group having 1 to 20 carbon atoms, and the organic group may contain a halogen atom, a glycidyl group, etc. n represents an integer of 1 or more and 6 or less.

[0030] Examples of the hydroxy group-containing compound include 2-(hydroxyalkyl)acrylic acid esters such as α-hydroxymethylstyrene, α-hydroxyethylstyrene, and methyl 2-(hydroxyethyl)acrylate; and 2-(hydroxyalkyl)acrylic acids such as 2-(hydroxyethyl)acrylic acid; and these may be used alone or in combination of two or more.

[0031] Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, crotonic acid, α-substituted acrylic acid, and α-substituted methacrylic acid. These may be used alone or in combination of two or more.

[0032] Examples of the compound represented by general formula (1) include styrene, vinyl toluene, α-methyl styrene, acrylonitrile, methyl vinyl ketone, ethylene, propylene, vinyl acetate, 2-chloroethyl vinyl ether, vinyl chloroacetate, allyl glycidyl ether, glycidyl methacrylate, and glycidyl acrylate, and these may be used alone or in combination of two or more.

[0033] The acrylic resin contained in the magnetic layer may be a commercially available acrylic resin or an acrylic resin synthesized by a known method.

[0034] From the viewpoint of further improving heat resistance, the molecular weight of the acrylic resin is preferably 10,000 or more, more preferably 50,000 or more, and even more preferably 100,000 or more, more preferably more than 100,000, more preferably 300,000 or more, more preferably 500,000 or more, and even more preferably 800,000 or more. The weight average molecular weight of the acrylic resin can be, for example, 3,000,000 or less, 2,500,000 or less, or 2,000,000 or less. However, from the viewpoint of improving heat resistance, a high molecular weight acrylic resin is preferable, and therefore the weight average molecular weight of the acrylic resin may exceed the range exemplified here.

[0035] The weight average molecular weight in the present invention and this specification is a value measured by gel permeation chromatography (GPC). For measurements using gel permeation chromatography (GPC), an HLC (registered trademark)-8320GPC (manufactured by Tosoh Corporation) can be used as the measuring device, and a TSKgel (registered trademark) Super HZ-H (4.6 mm ID x 15 cm, manufactured by Tosoh Corporation), a Super HZ4000 (4.6 mm ID x 15 cm, manufactured by Tosoh Corporation), and a Super HZ2000 (4.6 mm ID x 15 cm, manufactured by Tosoh Corporation) connected in series can be used as the column, and THF (tetrahydrofuran) can be used as the eluent. Measurement conditions can be a sample concentration of 0.2% by mass, a flow rate of 0.35 mL / min, a sample injection volume of 10 μL, and a measurement temperature of 40°C. A refractive index (RI) detector can be used as the detector. The calibration curve can be prepared using the following standard samples manufactured by Tosoh Corporation: "TSK standard, polystyrene," "F-288," "F-80," "F-20," "F-4," "F-2," "A-5000," and "A-1000."

[0036] From the viewpoint of further improving heat resistance and further from the viewpoint of the self-supporting properties of the magnetic layer, the content of the acrylic resin in the magnetic layer is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, where the total mass of the magnetic layer is 100 parts by mass. Also, from the viewpoint of further improving the shielding ability of the electromagnetic wave shielding material, the total content of the acrylic resin in the magnetic layer is preferably less than 30 parts by mass, more preferably 28 parts by mass or less, even more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, where the total mass of the magnetic layer is 100 parts by mass.

[0037] In addition to the above components, the magnetic layer may also contain any amount of one or more known additives such as a hardener, dispersant, stabilizer, coupling agent, etc.

[0038] For example, the magnetic layer may contain one or more coupling agents. As the coupling agent, a silane coupling agent is preferred, and a silane coupling agent having a hydrolyzable group is more preferred. By using a silane coupling agent having a hydrolyzable group, it is expected that the affinity between the magnetic particles and the acrylic resin will be increased by modifying the magnetic particle surface, and that mechanical properties will be improved. Examples of the hydrolyzable group include an alkoxy group, an acyloxy group, and a halogeno group.

[0039] The silane coupling agent may have a hydrophobic group as a functional group. Examples of the silane coupling agent having a hydrophobic group as a functional group include alkoxysilanes such as methyltrimethoxysilane (MTMS), dimethyldimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, and decyltrimethoxysilane; chlorosilanes such as methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, and phenyltrichlorosilane; and hexamethyldisilazane (HMDS).

[0040] The silane coupling agent may also have a vinyl group as a functional group. Examples of the silane coupling agent having a vinyl group as a functional group include alkoxysilanes such as methacryloxypropyltriethoxysilane, methacryloxypropyltrimethoxysilane, methacryloxypropylmethyldiethoxysilane, methacryloxypropylmethyldimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, and vinylmethyldimethoxysilane; chlorosilanes such as vinyltrichlorosilane and vinylmethyldichlorosilane; and divinyltetramethyldisilazane.

[0041] The silane coupling agent may have an amino group as a functional group. Examples of the silane coupling agent having an amino group as a functional group include aminopropyltriethoxysilane, aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-8-aminooctyltrimethoxysilane, aminoalkoxysilanes having amines at both ends (e.g., FM-3311, FM-3321, and FM-3325 manufactured by JNC Corporation), and polyfunctional amine aminoalkoxysilanes (e.g., X-12-972F manufactured by Shin-Etsu Chemical Co., Ltd.).

[0042] When the electromagnetic wave shielding material includes only one magnetic layer, the thickness of this magnetic layer can be, for example, 5 μm or more. From the viewpoint of further improving the shielding ability of the electromagnetic wave shielding material, it is preferably 10 μm or more, and more preferably 20 μm or more. On the other hand, the thickness of this magnetic layer can be, for example, 100 μm or less or 90 μm or less. From the viewpoint of further improving moldability, it is preferably less than 90 μm, more preferably 80 μm or less, and even more preferably 70 μm or less. When the electromagnetic wave shielding material includes two or more magnetic layers, the thickness of each of these two or more magnetic layers (i.e., the thickness per layer) can be, for example, 5 μm or more. From the viewpoint of further improving the shielding ability of the electromagnetic wave shielding material, it is preferably 10 μm or more, and more preferably 20 μm or more. On the other hand, this magnetic layer can be, for example, 100 μm or less or 90 μm or less, and preferably less than 90 μm, and more preferably 80 μm or less. The thickness of each of the two or more magnetic layers can be the same or different.

[0043] The thickness of each layer included in the electromagnetic wave shielding material is determined by photographing a cross section exposed by a known method with a scanning electron microscope (SEM) and calculating the arithmetic mean of the thicknesses at five randomly selected points in the resulting SEM image.

[0044] (Organic Solvent Content of Magnetic Layer) In the electromagnetic wave shielding material, the organic solvent content of the magnetic layer sandwiched between two metal layers and containing magnetic particles and an acrylic resin is 5 ppm or more and less than 1000 ppm by mass. The unit "ppm" is an abbreviation for "parts per million." In the present invention and this specification, ppm is based on mass, and will hereinafter also be referred to simply as ppm. From the viewpoint of improving durability, the organic solvent content of the magnetic layer is 5 ppm or more and preferably 10 ppm or more. Furthermore, from the viewpoint of improving durability, the organic solvent content of the magnetic layer is preferably less than 1000 ppm and 800 ppm or less, and more preferably 600 ppm or less, 400 ppm or less, 200 ppm or less, 100 ppm or less, and less than 100 ppm, in that order.

[0045] In the present invention and this specification, the "organic solvent content of the magnetic layer" is determined by the following method in an environment with an ambient temperature of 23°C. The magnetic layer of an electromagnetic shielding material, or the magnetic layer of a sample cut out from the electromagnetic shielding material, is exposed by peeling off adjacent layers, for example. Approximately 0.03 to 0.5 g of the exposed magnetic layer is scraped off to obtain a magnetic layer sample. The obtained magnetic layer sample is placed in a headspace glass bottle and sealed. This is used as an HS-GC / MS (Headspace-Gas Chromatography / Mass Spectrometer) sample. HS-GC / MS measurement of the HS-GC / MS sample is performed under the following conditions, and the amount of organic solvent is quantified by the multiple headspace extraction method (MHE). The MHE method is a method that can measure the content of a target component in a sample from the decay curve of the peak area by repeatedly performing headspace analysis under the same conditions. The amount of each organic solvent can be calculated according to the description in the following reference: Reference: Shen W., Wang C. , Multiple Headspace Extraction for the Quantitative Determination of Residual Monomer and Solvents in Polystyrene Pellets Using the Agilent 7697A Headspace Sampler, Agilent Technologies publication 5991-0974EN (can be calculated according to the formula described on page 9). The organic solvent content (unit: ppm) is calculated from the quantified amount of organic solvent and the amount of magnetic layer sample. The amount of organic solvent calculated in this way is the organic solvent content of the magnetic layer to be measured.

[0046] Gas chromatograph mass spectrometer (GC / MS) apparatus: Shimadzu Corporation headspace-GC / MS (HS-GC / MS) Headspace conditions: heating temperature 250°C, heating time 20 minutes Measurement method: Multiple headspace extraction method (Multiple Headspace Extraction / MHE method) Number of injections: 5 times Vial pressurization gas pressure: 90 kPa Load time: 0.5 minutes Injection time: 1 minute GC / MS conditions: Column: Agilent Technologies PoraBond Q (25 m, 3 μm, 0.25 mm ID (Inner Diameter)) Oven temperature: 50°C (1 minute) → heating at 35°C / minute → 300°C (5 minutes) Linear velocity: 50 cm / sec Split ratio: 10 Interface temperature: 300°C Detector: EI (electron ionization)-MS (Scan: m / z 29 to 600, SIM (selected ion monitoring): m / z 43, 55, 91)

[0047] The organic solvent content of the magnetic layer can be controlled, for example, by the drying conditions during the preparation of the magnetic layer.

[0048] In the present invention and this specification, the term "organic solvent" refers to an organic compound that is liquid at room temperature. With respect to organic solvents, "room temperature" refers to 23°C. Examples of organic solvents contained in the magnetic layer include ketone-based solvents such as acetone, methyl ethyl ketone, and cyclohexanone; acetate ester-based solvents such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitols such as cellosolve and butyl carbitol; aromatic hydrocarbon-based solvents such as toluene and xylene; and amide-based solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone. In one embodiment, the organic solvent contained in the magnetic layer can be a ketone-based solvent such as acetone, methyl ethyl ketone, or cyclohexanone, or can be methyl ethyl ketone and / or cyclohexanone.

[0049] <Metal Layer> The electromagnetic shielding material has a multilayer structure in which a magnetic layer is sandwiched between two metal layers. The electromagnetic shielding material may include one or more such multilayer structures, and may also include two or more. That is, the electromagnetic shielding material may include at least two metal layers, and may also include three or more metal layers, or may include at least one magnetic layer, and may also include two or more magnetic layers. In one embodiment, the two or more metal layers included in the electromagnetic shielding material have the same composition and thickness, and in another embodiment, they have different compositions and / or thicknesses. This also applies when the electromagnetic shielding material includes two or more magnetic layers, and when the electromagnetic shielding material includes two or more other layers, such as a resin layer, as described below.

[0050] In the present invention and this specification, the term "metal layer" refers to a layer containing a metal. The metal layer may be a layer containing one or more metals as a pure metal consisting of a single metal element, as an alloy of two or more metal elements, or as an alloy of one or more metal elements and one or more non-metal elements.

[0051] The metal layer included in the electromagnetic wave shielding material can be a layer containing one or more metals selected from the group consisting of various pure metals and various alloys. The metal layer can exhibit an attenuation effect in the electromagnetic wave shielding material. This is preferable from the perspective of improving the shielding ability of the electromagnetic wave shielding material. The attenuation effect is greater with a larger propagation constant, and the propagation constant is greater with a higher electrical conductivity. Therefore, it is preferable that the metal layer contain a metal element with high electrical conductivity. From this perspective, it is preferable that the metal layer contain a pure metal such as Ag, Cu, Au, or Al, or an alloy containing any of these as a main component. A pure metal is a metal consisting of a single metal element and may contain trace amounts of impurities. Generally, a metal consisting of a single metal element with a purity of 99.0% or higher is called a pure metal. Purity is measured by mass. An alloy is generally a pure metal with a composition adjusted by adding one or more metal or non-metallic elements to a pure metal for corrosion prevention, strength improvement, etc. The main component of an alloy is the component with the highest proportion by mass, and can be, for example, a component that accounts for 80.0% by mass or more (e.g., 99.8% by mass or less) in the alloy. From the viewpoint of economy, pure metal Cu or Al or an alloy containing Cu or Al as a main component is preferred, and from the viewpoint of high electrical conductivity, pure metal Cu or an alloy containing Cu as a main component is more preferred.

[0052] In one embodiment, the purity of the metal in the metal layer, i.e., the metal content in the metal layer, can be 99.0% by mass or more, 99.5% by mass or more, or 99.8% by mass or more, relative to the total mass of the metal layer. The metal content in the metal layer refers to the content by mass unless otherwise specified. For example, the metal layer can be a pure metal or alloy processed into a sheet. For example, a commercially available metal foil or a metal foil prepared by a known method can be used as the metal layer. Pure Cu metal sheets (so-called copper foils) of various thicknesses are commercially available. For example, such copper foils can be used as the metal layer. Copper foils include electrolytic copper foils obtained by electroplating copper foils on a cathode, and rolled copper foils obtained by thinly rolling an ingot under heat and pressure. Both copper foils can be used as the metal layer of the electromagnetic wave shielding material. Furthermore, Al sheets (so-called aluminum foils) of various thicknesses are commercially available. For example, such aluminum foils can be used as the metal layer.

[0053] From the perspective of reducing the weight of the electromagnetic wave shielding material, it is preferable that one or both (preferably both) of the two metal layers sandwiching the magnetic layer be a metal layer containing a metal selected from the group consisting of Al and Mg, and more preferably a layer containing a metal selected from the group consisting of Al and Mg as its main component. The main component of a metal layer is the component with the highest proportion by mass. In a layer containing a metal selected from the group consisting of Al and Mg as its main component, Al or Mg is the component with the highest proportion by mass in this layer. Such a layer may contain only Al or Mg, or may contain Al and Mg. Both Al and Mg have a small value obtained by dividing the specific gravity by the electrical conductivity (specific gravity / electrical conductivity). The smaller this value, the lighter the electromagnetic wave shielding material that exhibits high shielding ability can be. For example, the value obtained by dividing the specific gravity by the electrical conductivity of Cu, Al, and Mg (specific gravity / electrical conductivity) calculated from literature values ​​is as follows: Cu: 1.5 × 10 -7 m / S, Al: 7.6×10 -8 m / S, Mg: 7.6×10 -8m / S. From the above values, Al and Mg can be said to be preferred metals from the viewpoint of reducing the weight of the electromagnetic shielding material. In one embodiment, the metal layer containing a metal selected from the group consisting of Al and Mg can contain only one of Al and Mg, and in another embodiment, it can contain both. From the viewpoint of reducing the weight of the electromagnetic shielding material, it is more preferable that one or both (preferably both) of the two metal layers sandwiching the magnetic layer be a metal layer having a metal content selected from the group consisting of Al and Mg of 80.0% by mass or more, and even more preferable that the metal content selected from the group consisting of Al and Mg be a metal layer having a metal content selected from the group consisting of Al and Mg of 90.0% by mass or more. Of Al and Mg, the metal layer containing at least Al can be a metal layer having an Al content of 80.0% by mass or more, or can also be a metal layer having an Al content of 90.0% by mass or more. Of Al and Mg, the metal layer containing at least Mg can be a metal layer having an Mg content of 80.0% by mass or more, or can also be a metal layer having an Mg content of 90.0% by mass or more. The content of the metal selected from the group consisting of Al and Mg, the Al content, and the Mg content can each be, for example, 99.9 mass % or less. The content of the metal selected from the group consisting of Al and Mg, the Al content, and the Mg content are each expressed as a percentage relative to the total mass of the metal layer.

[0054] From one or more of the viewpoints of economy, high electrical conductivity, and weight reduction of the electromagnetic wave shielding material, it is preferable that one or both (preferably both) of the two metal layers sandwiching the magnetic layer be a metal layer containing a metal selected from the group consisting of Al, Mg, and Cu, and more preferably a layer containing a metal selected from the group consisting of Al, Mg, and Cu as a primary component. In a layer containing a metal selected from the group consisting of Al, Mg, and Cu as a primary component, Al, Mg, or Cu is the component with the highest proportion by mass in this layer. Such a layer may contain only one, two, or three metals selected from Al, Mg, and Cu. From one or more of the above viewpoints, it is more preferable that one or both (preferably both) of the two metal layers sandwiching the magnetic layer be a metal layer containing 80.0% by mass or more of a metal selected from the group consisting of Al, Mg, and Cu, and even more preferably a metal layer containing 90.0% by mass or more of a metal selected from the group consisting of Al, Mg, and Cu. A metal layer containing at least Al among Al, Mg, and Cu can be a metal layer with an Al content of 80.0 mass% or more, or can be a metal layer with an Al content of 90.0 mass% or more. A metal layer containing at least Mg among Al, Mg, and Cu can be a metal layer with an Mg content of 80.0 mass% or more, or can be a metal layer with an Mg content of 90.0 mass% or more. A metal layer containing at least Cu among Al, Mg, and Cu can be a metal layer with a Cu content of 80.0 mass% or more, or can be a metal layer with a Cu content of 90.0 mass% or more. The content of the metal selected from the group consisting of Al, Mg, and Cu, the Al content, the Mg content, and the Cu content can each be, for example, 99.9 mass% or less. The content of the metal selected from the group consisting of Al, Mg, and Cu, the Al content, the Mg content, and the Cu content are each expressed as a percentage relative to the total mass of the metal layer.

[0055] With regard to the thickness of the metal layer, from the viewpoint of further improving the processability of the metal layer and the shielding ability of the electromagnetic wave shielding material, the thickness per layer is preferably 4 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. On the other hand, from the viewpoint of the processability of the metal layer, the thickness per layer is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less. In the electromagnetic wave shielding material, the thicknesses of the multiple metal layers can be the same or different.

[0056] In one embodiment, one or both outermost layers of the electromagnetic shielding material can be a metal layer. This can contribute to the electromagnetic shielding material being able to exhibit high shielding ability against magnetic fields in the low-frequency range of around 100 kHz to 1 MHz. Furthermore, having at least one outermost layer of the electromagnetic shielding material be a metal layer can also contribute to suppressing edge peeling in a molded product obtained by molding. In one embodiment, one or both outermost layers of the electromagnetic shielding material can be a metal layer that sandwiches a magnetic layer with another metal layer.

[0057] In one embodiment, in the multilayer structure of the electromagnetic wave shielding material in which a magnetic layer is sandwiched between two metal layers, one or both of the two metal layers can be disposed as layers in direct contact with the magnetic layer. That is, one or both of the two metal layers can be adjacent to the magnetic layer without any other layer interposed therebetween. Also, in one embodiment, the multilayer structure of the electromagnetic wave shielding material in which a magnetic layer is sandwiched between two metal layers can have one or more resin-containing layers between one or both of the two metal layers and the magnetic layer. The resin-containing layer is a layer containing one or more types of resin. Specific embodiments of the resin-containing layer are described below.

[0058] <Layer Containing Resin> (Adhesive Layer) One example of a resin-containing layer is an adhesive layer. In the present invention and this specification, the term "adhesive layer" refers to a layer having tackiness on its surface at room temperature. With regard to tackiness, "room temperature" refers to 23°C. Such a layer adheres to an adherend due to its adhesive force when it comes into contact with the adherend. Tackiness generally refers to the property of exhibiting adhesive strength in a short time after contact with the adherend with very little force. In the present invention and this specification, the term "having tackiness" refers to a result of No. 1 to No. 32 in the inclined ball tack test (measurement environment: temperature 23°C, relative humidity 50%) specified in JIS Z 0237:2009. When another layer is laminated on the surface of the adhesive layer, for example, the other layer can be peeled off and the exposed adhesive layer surface can be subjected to the above test. When another layer is laminated on both one surface and the other surface of the adhesive layer, the other layer on either surface may be peeled off.

[0059] The adhesive layer can be formed by coating an adhesive layer-forming composition containing an adhesive such as an acrylic adhesive, a rubber adhesive, a silicone adhesive, or a urethane adhesive and processing it into a film. The adhesive layer-forming composition can be applied, for example, to a support. Coating can be performed using a known coating device such as a blade coater or a die coater. Coating can be performed using a so-called roll-to-roll method or a batch method. Examples of supports to which the adhesive layer-forming composition is applied include films made of various resins such as polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), acrylics such as polycarbonate (PC) and polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, and polyimides. Supports whose surfaces (coated surfaces) to which the adhesive layer-forming composition is applied (the surfaces to be coated) have been subjected to a release treatment by a known method can be used. One form of release treatment is the formation of a release layer. Alternatively, commercially available release-treated resin films can be used as the support. By using a support whose surface to be coated has been subjected to a release treatment, the adhesive layer and the support can be easily separated after film formation. An adhesive layer can be formed by applying an adhesive layer-forming composition, in which an adhesive is dissolved and / or dispersed in a solvent, to the surface to be coated and drying the composition. Alternatively, an adhesive tape including an adhesive layer can be used. Examples of the adhesive tape include double-sided tape. Double-sided tape has adhesive layers on both sides of the support. Alternatively, an adhesive tape having an adhesive layer on one side of the support can be used. Examples of the support include films, nonwoven fabrics, and paper made of various resins such as polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polycarbonate (PC), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, and polyimide.As the adhesive tape having an adhesive layer on one or both sides of a support, a commercially available product can be used, and an adhesive tape produced by a known method can also be used.

[0060] The thickness of the adhesive layer is not particularly limited, and the thickness per layer can be, for example, 1 μm or more and 30 μm or less.

[0061] (Adhesive Layer) One form of a resin-containing layer is an adhesive layer. In the present invention and this specification, an "adhesive layer" refers to a layer in which a liquid or gel adhesive contacts an adherend and solidifies through a state change such as drying or curing, thereby exerting adhesion to the adherend through an anchoring effect, physical interaction, or the formation of a chemical bond. In one form, the adhesive layer may be a layer that has no tackiness on the surface at room temperature. The adhesive includes a resin that solidifies after drying or curing. Examples of such resins include vinyl acetate resin, ethylene vinyl acetate resin, epoxy resin, cyanoacrylate resin, acrylic resin, polyurethane resin, chloroprene rubber, styrene butadiene rubber, etc. These resins may themselves be liquid or gel-like. Alternatively, a solid resin may dissolve in a solvent to become liquid or gel-like. Examples of solvents contained in the adhesive include ketone-based solvents such as water, acetone, methyl ethyl ketone, and cyclohexanone; acetate ester-based solvents such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitols such as cellosolve and butyl carbitol; aromatic hydrocarbon-based solvents such as toluene and xylene; amide-based solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; alcohol-based solvents such as ethanol, methanol, and propanol; and halogen-based solvents such as dichloromethane, trichloroethylene, and dichlorofluoroethane.

[0062] The thickness of the adhesive layer is not particularly limited, and the thickness per layer can be, for example, 1 μm or more and 30 μm or less.

[0063] (Resin Layer) One form of layer containing a resin can be a resin layer. In the present invention and this specification, the term "resin layer" refers to a resin film formed from a thermoplastic resin such as a synthetic resin in a film-like shape, and the resin film has a film-like structure by itself and is not tacky at room temperature. Examples of thermoplastic resins contained in the resin film include polyethylene (PE) resin, polypropylene (PP) resin, polyvinyl chloride (PVC) resin, polystyrene (PS) resin, vinyl acetate resin, polyurethane resin, polyvinyl alcohol resin, ethylene vinyl acetate resin, styrene butadiene rubber, acrylonitrile butadiene rubber, silicone rubber, olefin elastomer (PP), styrene elastomer, ABS (acrylonitrile-butadiene-styrene) resin, polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polycarbonate (PC) resin, acrylic resins such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), and other various resins.

[0064] The resin layer can be bonded to a metal layer or a magnetic layer via an adhesive layer or a pressure-sensitive adhesive layer. Since the resin layer contains a thermoplastic resin, it softens when heated. When pressed against an adherend in a heated state, it flows and conforms to minute irregularities on the adherend surface, exerting adhesive strength through an anchoring effect. The adhesive state can then be maintained by cooling. Therefore, in one embodiment, the resin layer can be bonded to another layer without an adhesive layer or a pressure-sensitive adhesive layer.

[0065] The thickness of the resin layer, as measured per resin layer, is preferably 10 μm or more, and more preferably 12 μm or more. The thickness of the resin layer, as measured per resin layer, is preferably 250 μm or less, more preferably 230 μm or less, even more preferably 210 μm or less, and even more preferably 190 μm or less. In one embodiment, the electromagnetic wave shielding material has a multilayer structure in which a magnetic layer is sandwiched between two metal layers, and can include one or more resin layers having a thickness within the above range between one or both of the two metal layers and the magnetic layer. For example, the multilayer structure can include one magnetic layer having a thickness within the above range between one of the two metal layers and the magnetic layer, and / or between the other metal layer and the magnetic layer.

[0066] <Specific Example of Layer Configuration> The total number of magnetic layers included in the electromagnetic shielding material is one or more, and can be two or more, or can be, for example, four or less. On the other hand, the total number of metal layers included in the electromagnetic shielding material is two or more, and can be, for example, two to five. When the electromagnetic shielding material includes only one magnetic layer, this one magnetic layer is a magnetic layer sandwiched between two metal layers. When the electromagnetic shielding material includes two or more magnetic layers, at least one of these two or more magnetic layers is a magnetic layer sandwiched between two metal layers. More specifically, all or only a portion of the magnetic layers included in the electromagnetic shielding material are magnetic layers sandwiched between two metal layers.

[0067] In one embodiment, in a multilayer structure in which a magnetic layer is sandwiched between two metal layers, the magnetic layer can be in direct contact with both metal layers. In this case, specific examples of the layer configuration of the electromagnetic shielding material include the following: Example A1: "Metal layer / Magnetic layer / Metal layer" Example A2: "Metal layer / Magnetic layer / Metal layer / Magnetic layer / Metal layer" Example A3: "Metal layer / Magnetic layer / Metal layer / Magnetic layer / Metal layer / Magnetic layer / Metal layer" In an electromagnetic shielding material including two or more multilayer structures each including a magnetic layer between two metal layers, as in Examples A2 and A3, the metal layers sandwiching the magnetic layer in one multilayer structure can also be the metal layers sandwiching the magnetic layer in another multilayer structure. In the electromagnetic shielding material, the total number of multilayer structures each including the magnetic layer between two metal layers can be, for example, one to four. The total number of multilayer structures is one in Example A1, two in Example A2, and three in Example A3. It is preferable that the total number of the multilayer structure is two or more (e.g., two, three, or four) from the viewpoint of further improving the shielding ability of the electromagnetic wave shielding material. In the above, the symbol " / " means that the layer written to the left of this symbol and the layer written to the right of this symbol are in direct contact with each other without any other layer in between. This point also applies to the following description unless otherwise specified.

[0068] In another embodiment, the multilayer structure of the electromagnetic wave shielding material, in which a magnetic layer is sandwiched between two metal layers, can include one or more resin-containing layers between one or both of the two metal layers and the magnetic layer. In the multilayer structure, one of the two metal layers can be adjacent to the magnetic layer without any other layer in between, and one or more resin-containing layers can be included between the other metal layer and the magnetic layer. Alternatively, the multilayer structure can have one or more resin-containing layers between each of the two metal layers and the magnetic layer. As the resin-containing layer located between the metal layer and the magnetic layer, at least a resin layer is preferred. In one embodiment, the electromagnetic wave shielding material can include one or more polyester resin-containing layers between one or both of the two metal layers and the magnetic layer, and the polyester resin-containing layer is preferably a resin layer.

[0069] The multilayer structure may include an adhesive layer and / or a bonding layer between the resin layer and the metal layer. In one embodiment, the adhesive layer and / or the bonding layer may be included between the resin layer and the magnetic layer. In another embodiment, the resin layer and the magnetic layer may be in direct contact with each other in the multilayer structure. That is, the resin layer and the magnetic layer may be adjacent to each other without any other layer interposed therebetween.

[0070] The electromagnetic wave shielding material may include, for example, a total of 1 to 12 resin-containing layers. The total number of resin layers included in the electromagnetic wave shielding material (preferably resin layers having the thickness described above) may be, for example, 1 to 4. The total number of layers selected from the group consisting of pressure-sensitive adhesive layers and adhesive layers included in the electromagnetic wave shielding material may be, for example, 1 to 4 or 1 to 8.

[0071] The following are examples of the arrangement of the "magnetic layer," "metal layer," "resin layer," and "adhesive or bonding layer" in the electromagnetic wave shielding material. In the following examples, the "adhesive layer" may include a support, or the "adhesive layer" may be an adhesive tape having an adhesive layer on one or both sides of the support. For example, as in Example B3, the metal layer sandwiching one magnetic layer may also be the metal layer sandwiching another magnetic layer. For example, in Example B3, metal layer 2 is one of the two metal layers sandwiching magnetic layer 1 and is also one of the two metal layers sandwiching magnetic layer 2. Furthermore, in Example B3, the outermost layer on one side of the electromagnetic wave shielding material is metal layer 1, which sandwiches magnetic layer 1 together with metal layer 2, and the outermost layer on the other side of the electromagnetic wave shielding material is metal layer 3, which sandwiches magnetic layer 2 together with metal layer 2. Example B1: "Metal layer 1 / adhesive layer 1 or adhesive layer 1 / resin layer 1 / magnetic layer 1 / resin layer 2 / adhesive layer 2 or adhesive layer 2 / metal layer 2" Example B2: "Metal layer 1 / adhesive layer 1 or adhesive layer 1 / resin layer 1 / magnetic layer 1 / metal layer 2 / adhesive layer 2 or adhesive layer 2 / resin layer 2" Example B3: "Metal layer 1 / adhesive layer 1 or adhesive layer 1 / resin layer 1 / magnetic layer 1 / resin layer 2 / adhesive layer 2 or adhesive layer 2 / metal layer 2 / adhesive layer 3 or adhesive layer 3 / resin layer 3 / magnetic layer 2 / resin layer 4 / adhesive layer 4 or adhesive layer 4 / metal layer 3" Example B4: "Metal layer 1 / adhesive layer 1 or adhesive layer 1 / resin layer 1 / magnetic layer 1 / metal layer 2 / adhesive layer 2 or adhesive layer 2 / resin layer 2 / magnetic layer 2 / resin layer 3 / adhesive layer 3 or adhesive layer 3 / metal layer 3" Example B5: "Metal layer 1 / adhesive layer 1 or adhesive layer 1 / resin layer 1 / magnetic layer 1 / metal layer 2 / adhesive layer 2 or adhesive layer 2 / resin layer 2 / magnetic layer 2 / metal layer 3 / adhesive layer 3 or adhesive layer 3 / resin layer 3" Example B6: "Metal layer 1 / adhesive layer 1 or adhesive layer 1 / resin layer 1 / magnetic layer 1 / metal layer 2 / magnetic layer 2 / resin layer 2 / adhesive layer 2 or adhesive layer 2 / metal layer 3" Example B7: "Metal layer 1 / adhesive layer 1 or adhesive layer 1 / resin layer 1 / magnetic layer 1 / metal layer 2 / magnetic layer 2 / metal layer 3 / adhesive layer 2 or adhesive layer 2 / resin layer 2" Example B8: "Metal layer 1 / adhesive layer 1 or adhesive layer 1 / resin layer 1 / magnetic layer 1 / resin layer 2 / adhesive layer 2 or adhesive layer 2 / metal layer 2 / magnetic layer 2 / resin layer 3 / adhesive layer 3 or adhesive layer 3 / metal layer 3"

[0072] <Method for manufacturing electromagnetic wave shielding material> (Method for forming magnetic layer) The magnetic layer can be produced, for example, by applying a magnetic layer-forming composition and drying the resulting coating layer. The magnetic layer-forming composition can contain the components described above and can further contain one or more solvents. Examples of the solvent include the various organic solvents described above as organic solvents contained in the magnetic layer. One solvent selected in consideration of the solubility of the components used in preparing the magnetic layer-forming composition, or two or more solvents mixed in any ratio, can be used. The solvent content of the magnetic layer-forming composition is not particularly limited and can be determined in consideration of the coatability of the magnetic layer-forming composition, etc.

[0073] The magnetic layer-forming composition can be prepared by mixing the various components sequentially in any order or simultaneously. If necessary, dispersion treatment can be carried out using a known dispersing machine such as a ball mill, bead mill, sand mill, or roll mill, and / or stirring treatment can be carried out using a known stirring machine such as a vibration stirring machine.

[0074] The magnetic layer-forming composition can be applied onto a support, for example. The application can be carried out using a known application device such as a blade coater or a die coater. The application can be carried out by a so-called roll-to-roll method or a batch method.

[0075] Examples of substrates onto which the magnetic layer-forming composition is applied include films of various resins, such as polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), acrylics such as polycarbonate (PC) and polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, and polyimide. For details of these resin films, see paragraphs 0081 to 0086 of JP 2015-187260 A. As the substrate, a substrate whose surface (the surface to be coated) onto which the magnetic layer-forming composition is applied has been subjected to a release treatment by a known method can be used. One form of release treatment is the formation of a release layer. For details of the release layer, see paragraph 0084 of JP 2015-187260 A. Alternatively, commercially available release-treated resin films can be used as the substrate. By using a substrate whose surface to be coated has been subjected to a release treatment, the magnetic layer and the substrate can be easily separated after film formation.

[0076] The coating layer formed by applying the magnetic layer-forming composition can be dried by known methods such as heating or hot air blowing. The drying can be carried out under conditions that allow the solvent contained in the magnetic layer-forming composition to volatilize. As an example, the drying can be carried out for 6 minutes to 2 hours in a heated atmosphere at an ambient temperature of 80 to 150°C. The organic solvent content of the magnetic layer contained in the electromagnetic wave shielding material can be controlled by the drying conditions, such as the temperature and time, during the drying process.

[0077] The degree of orientation of the flat particles described above can be controlled by the type of solvent, amount of solvent, liquid viscosity, coating thickness, etc., of the magnetic layer-forming composition. For example, if the boiling point of the solvent is low, convection occurs upon drying, which tends to increase the degree of orientation. If the amount of solvent is small, the degree of orientation tends to increase due to physical interference between adjacent flat particles. On the other hand, if the liquid viscosity is low, the flat particles are more likely to rotate, which tends to decrease the degree of orientation. If the coating thickness is made thinner, the degree of orientation tends to decrease. In addition, performing the pressure treatment described below can contribute to reducing the degree of orientation. By adjusting the various manufacturing conditions described above, the degree of orientation of the flat particles can be controlled within the range described above.

[0078] (Pressure treatment of magnetic layer) The magnetic layer can also be pressure treated after deposition. By pressure treating a magnetic layer containing magnetic particles, the magnetic particle density in the magnetic layer can be increased, resulting in higher magnetic permeability. Furthermore, for a magnetic layer containing flat-shaped particles, the degree of orientation can be reduced by pressure treatment, resulting in higher magnetic permeability.

[0079] The pressure treatment can be carried out by applying pressure in the thickness direction of the magnetic layer using a plate press, a roll press, or the like. With a plate press, the object to be pressed is placed between two flat press plates arranged above and below, and pressure can be applied to the object by bringing the two press plates together using mechanical or hydraulic pressure. With a roll press, the object to be pressed is passed between rotating pressure rolls arranged above and below, and pressure can be applied by applying mechanical or hydraulic pressure to the pressure rolls or by making the distance between the pressure rolls smaller than the thickness of the object to be pressed.

[0080] The pressure during the pressurization can be set arbitrarily. For example, in the case of a plate-type press, the pressure is set to, for example, 1 to 50 N (Newton) / mm 2In the case of a roll press, the linear pressure is, for example, 20 to 400 N / mm. The pressure application time can be set as desired. When a plate press is used, the time is, for example, 5 seconds to 30 minutes. When a roll press is used, the pressure application time can be controlled by the conveying speed of the material to be pressed, for example, 10 cm / min to 200 m / min. The materials of the press plate and pressure roll can be selected from metal, ceramic, plastic, rubber, etc. During pressure treatment, heat can be applied to both the upper and lower press plates of a plate press or to one of the press plates or one of the upper and lower rolls of a roll press. Heating can soften the magnetic layer, thereby achieving a high compression effect when pressure is applied. The heating temperature can be set as desired, for example, from 50°C to 200°C. The heating temperature can be the internal temperature of the press plate or roll. This temperature can be measured using a thermometer installed inside the press plate or roll. After heating and pressurizing treatment in a plate-type press, the magnetic layer can be removed, for example, by separating the press plate while the temperature of the press plate is still high. Alternatively, the press plate can be cooled by water cooling, air cooling, or the like while maintaining the pressure, and then the press plate can be separated and the magnetic layer can be removed. In a roll press, the magnetic layer can be cooled by water cooling, air cooling, or the like immediately after pressing. It is also possible to repeat the pressure treatment two or more times. When the magnetic layer is formed on a release film, for example, the magnetic layer can be subjected to pressure treatment while laminated on the release film. Alternatively, the magnetic layer can be peeled off from the release film and subjected to pressure treatment as a single layer.

[0081] (Bonding of Various Layers) An adhesive layer or a bonding layer can be used to bond the various layers together. The adhesive layer and the bonding layer are as described above. In the electromagnetic wave shielding material, two adjacent layers can also be bonded together by applying pressure and heat, for example. A plate-type press, a roll press, or the like can be used for the bonding. For example, when a magnetic layer is disposed as a layer that directly contacts an adjacent layer, the magnetic layer softens in the bonding step, promoting contact with the surface of the adjacent layer, allowing the magnetic layer and the adjacent layer to be bonded together without any other layer interposed. The pressure during bonding can be set as desired. In the case of a plate-type press, for example, a pressure of 1 to 50 N / mm 2 In the case of a roll press, the linear pressure is, for example, 20 to 400 N / mm. The pressure application time during compression can be set as desired. When a plate press is used, it is, for example, 5 seconds to 30 minutes. When a roll press is used, it can be controlled by the conveying speed of the material to be pressed, and the conveying speed is, for example, 10 cm / min to 200 m / min. The temperature during compression can be selected as desired, and is, for example, 20°C or higher and 200°C or lower. The temperature during compression can be, for example, the internal temperature of the press plate or roll.

[0082] The electromagnetic shielding material can be incorporated into electronic components or electronic devices in any shape. The electromagnetic shielding material can be in sheet form, and its size is not particularly limited. In the present invention and this specification, "sheet" is synonymous with "film." The electromagnetic shielding material can also be a three-dimensionally molded product obtained by three-dimensionally molding a sheet-like electromagnetic shielding material, or a sheet-like electromagnetic shielding material for three-dimensional molding. Various molding methods, such as mold press molding, vacuum molding, and pressure molding, can be used. Regarding molding methods, for example, molding performed without heating the object and / or mold, or by heating at a low temperature, is generally called cold forming. Examples of cold forming methods include drawing and stretch forming. Drawing is a molding method in which a sheet-like object is pressed using a pair of dies, consisting of a female and a male die, to form a container with a bottom of various shapes, such as a cylinder, a rectangular tube, or a cone. In contrast, stretch forming is a method in which a sheet-like object is molded into an article with a curved surface that extends from a flat surface. Stretch forming can also be performed using a press with only a male die and no female die. Drawing is broadly divided into deep drawing and shallow drawing. Shallow drawing produces shallow molded products, while deep drawing produces deep molded products (for example, products deeper than the diameter of a cylinder or cone or the length of one side of a pyramid). Publicly known techniques can be applied to three-dimensional forming methods.

[0083] [Electronic Component] One aspect of the present invention relates to an electronic component comprising the electromagnetic wave shielding material. Examples of the electronic component include various electronic components such as electronic components contained in electronic devices such as mobile phones, personal digital assistants, and medical devices, as well as semiconductor elements, capacitors, coils, and cables. The electromagnetic wave shielding material can be three-dimensionally molded into any shape depending on the shape of the electronic component and placed inside the electronic component, or three-dimensionally molded into the shape of a cover material that covers the outside of the electronic component and placed as a cover material. Alternatively, it can be three-dimensionally molded into a cylindrical shape and placed as a cover material that covers the outside of a cable.

[0084] [Electronic Device] One aspect of the present invention relates to an electronic device including the electromagnetic shielding material. Examples of the electronic device include electronic devices such as mobile phones, personal digital assistants, and medical devices; electronic devices including various electronic components such as semiconductor elements, capacitors, coils, and cables; and electronic devices in which electronic components are mounted on a circuit board. Such electronic devices can include the electromagnetic shielding material as a component of the electronic components included in the device. Furthermore, as a component of the electronic device, the electromagnetic shielding material can be disposed inside the electronic device, or can be disposed as a cover material that covers the outside of the electronic device. Alternatively, the electromagnetic shielding material can be three-dimensionally molded into a cylindrical shape and disposed as a cover material that covers the outside of a cable.

[0085] One example of a use of the electromagnetic shielding material is to cover a semiconductor package on a printed circuit board with the electromagnetic shielding material. For example, "Electromagnetic Shielding Technology for Semiconductor Packages" (Toshiba Review Vol. 67 No. 2 (2012) p. 8) discloses a method for achieving high shielding effectiveness by electrically connecting a side via at the end of the package substrate to the inner surface of the electromagnetic shielding material when covering a semiconductor package with the electromagnetic shielding material, thereby achieving ground wiring. To achieve such wiring, it is desirable for the outermost layer of the electromagnetic shielding material on the electronic component side to be a metal layer. When one or both outermost layers of the electromagnetic shielding material are metal layers, the electromagnetic shielding material can be suitably used for such wiring.

[0086] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the embodiments shown in the examples.

[0087] [Resin of Magnetic Layer] The resins of the magnetic layer shown in Table 1 are the following resins: Acrylic resin 1: Acrylic rubber manufactured by Nippon Zeon Co., Ltd., trade name Nipol, model number AR71 Acrylic resin 2: Acrylic rubber manufactured by Nippon Zeon Co., Ltd., trade name Nipol, model number AR51 Acrylic resin 3: Polyethyl acrylate solution manufactured by Aldrich Corporation, trade name Acrylic resin 4: Hexane reprecipitate of acrylic resin 3 NBR (acrylonitrile butadiene rubber): Nipol, model number DN003 manufactured by Nippon Zeon Co., Ltd. The above acrylic resin 4 was prepared by pouring acrylic resin 3 into a large amount of hexane to precipitate it, collecting the precipitate by filtration, and then vacuum drying it in a vacuum dryer with an internal temperature of 80°C.

[0088] The weight-average molecular weight of each of the above resins was measured by gel permeation chromatography (GPC) as described below. The weight-average molecular weights thus determined are shown in Table 1. The measurement apparatus used was an HLC (registered trademark)-8320GPC (manufactured by Tosoh Corporation). The columns used were a TSKgel (registered trademark) Super HZ-H (4.6 mm ID x 15 cm, manufactured by Tosoh Corporation), a Super HZ4000 (4.6 mm ID x 15 cm, manufactured by Tosoh Corporation), and a Super HZ2000 (4.6 mm ID x 15 cm, manufactured by Tosoh Corporation), connected in series, and THF (tetrahydrofuran) was used as the eluent. The measurement conditions were a sample concentration of 0.2% by mass, a flow rate of 0.35 mL / min, a sample injection volume of 10 μL, and a measurement temperature of 40°C. A refractive index (RI) detector was used as the detector. The calibration curve was prepared using the following standard samples manufactured by Tosoh Corporation: "TSK standard, polystyrene," "F-288," "F-80," "F-20," "F-4," "F-2," "A-5000," and "A-1000."

[0089] Example 1 Preparation of magnetic layer-forming composition (coating liquid) 10 g of Fe—Si—Al flat magnetic particles (Sendust MFS-SUH manufactured by MKT Corporation), 2.5 g of acrylic resin (see Table 1, solids concentration 100% by mass), and 36 g of cyclohexanone were added to a plastic bottle and mixed for 96 hours with a shaking stirrer to prepare a coating liquid. The total mass of the magnetic layer formed from the prepared magnetic layer-forming composition was taken as 100 parts by mass, and the content of the acrylic resin was 20 parts by mass.

[0090] <Preparation of Magnetic Layer> (Deposition of Magnetic Layer) The coating liquid was applied to the release surface of a release-treated PET film (PET75-JOL manufactured by Nippa Corporation) using a blade coater with a coating gap of 650 μm, and the film was dried for 8 minutes (hereinafter referred to as "drying time") in a drying device with an internal atmosphere temperature of 90°C, thereby forming a film-like magnetic layer on the release-treated PET film.

[0091] (Pressure treatment of magnetic layer) The upper and lower press plates of a plate-type press (Mini Test Press manufactured by Toyo Seiki) were heated to 140°C (internal temperature of the press plates), and the magnetic layer from which the release-treated PET film had been peeled off was sandwiched between two 1 mm thick Teflon (registered trademark) sheets and subjected to a pressure of 30 N / mm. 2 The magnetic layer was then held for 10 minutes with a pressure of 0.05 MPa applied. While maintaining the pressure, the upper and lower press plates were cooled to 50°C (internal temperature of the press plates), and the magnetic layer was then removed from between the two Teflon (registered trademark) sheets. Measurement samples for the various evaluations described below were cut out from a portion of the resulting magnetic layer.

[0092] <Preparation of Electromagnetic Wave Shielding Material> Using the magnetic layer obtained above as the magnetic layer and 30 μm thick aluminum foil (JIS H4160:2006 compliant, alloy number 1N30 temper (1)O, Al content of 99.3 mass% or more) as the metal layer, a laminate was prepared by overlapping five layers of "aluminum foil (metal layer) / magnetic layer / aluminum foil (metal layer) / magnetic layer / aluminum foil (metal layer)" without any other layer between adjacent two layers. The upper and lower press plates of a plate press (large hot press TA-200-1W manufactured by Yamamoto Iron Works) were heated to 140°C (internal temperature of the press plates), and the laminate was placed at the center of the press plates, and a pressure of 4.66 N / mm was applied. 2The aluminum foil and the magnetic layer were thermocompression-bonded by applying a pressure of 0.05 W and maintaining this pressure for 10 minutes. The upper and lower press plates were cooled to 50°C (internal temperature of the press plates) while maintaining the pressure, and then the laminate was removed from the plate press. Thus, the electromagnetic shielding material of Example 1 was obtained. The electromagnetic shielding material of Example 1 includes two multilayer structures of "aluminum foil (metal layer) / magnetic layer / aluminum foil (metal layer)".

[0093] [Evaluation Method] <Measurement of magnetic permeability before and after thermal aging at 80°C> A measurement sample measuring 28 mm x 10 mm was cut out from the magnetic layer, and the magnetic permeability was measured using a magnetic permeability measuring device (Per01 manufactured by Keycom Corporation). The magnetic permeability was calculated as the real part of the complex relative magnetic permeability (μ') at a frequency of 3 MHz (measurement temperature: 25°C). The magnetic permeability calculated in this manner is referred to as the "magnetic permeability before thermal aging at 80°C." After measuring the magnetic permeability before thermal aging at 80°C, the measurement sample was placed in a high-temperature atmosphere at 80°C for 24 hours, and then the magnetic permeability was calculated using the above method (measurement temperature: 25°C). The magnetic permeability calculated in this manner is referred to as the "magnetic permeability after thermal aging at 80°C." Table 2 shows the evaluation results of the "magnetic permeability before thermal aging at 80°C" and the "magnetic permeability after thermal aging at 80°C" evaluated according to the following evaluation criteria. A: Magnetic permeability μ' is 100 or more B: Magnetic permeability μ' is 40 or more and less than 100 C: Magnetic permeability μ' is less than 40

[0094] <Measurement of Electrical Conductivity> A cylindrical main electrode with a diameter of 30 mm was connected to the negative pole of a digital insulation resistance meter (TR-811A manufactured by Takeda Riken), and a ring electrode with an inner diameter of 40 mm and an outer diameter of 50 mm was connected to the positive pole. The main electrode and the ring electrode were placed in a position surrounding it on a sample piece of the magnetic layer cut to a size of 60 mm x 60 mm, and a voltage of 25 V was applied to both poles to measure the surface electrical resistivity of the magnetic layer alone. The electrical conductivity of the magnetic layer was calculated from the surface electrical resistivity and the following formula. The calculated electrical conductivity was 1.1 x 10 -2 The thickness was determined by the following method: Electrical conductivity [S / m] = 1 / (surface electrical resistivity [Ω] × thickness [m])

[0095] <Obtaining a Cross-Sectional Image of the Electromagnetic Shielding Material> Cross-section processing was performed to expose the cross section of the electromagnetic shielding material using the following method. The electromagnetic shielding material cut into a size of 3 mm x 3 mm was embedded in resin, and the cross section of the electromagnetic shielding material was cut using an ion milling device (IM4000PLUS, manufactured by Hitachi High-Technologies Corporation). The cross section of the exposed electromagnetic shielding material was observed using a scanning electron microscope (SU8220, manufactured by Hitachi High-Technologies Corporation) at an acceleration voltage of 2 kV and a magnification of 100x to obtain a backscattered electron image. Using the scale bar as a reference, the thickness of each of the two magnetic layers and the three metal layers was measured at five locations on the obtained image. The arithmetic mean was used to represent the thickness of each magnetic layer, the thickness of each metal layer, and the total thickness of the electromagnetic shielding material. The thickness of each magnetic layer was 30 μm, and the thickness of each metal layer was 30 μm.

[0096] <Obtaining a cross-sectional image of the magnetic layer> In a cross-section of the electromagnetic wave shielding material that had been exposed by cross-section processing in the same manner as above, the magnetic layer portion was observed with a scanning electron microscope (SU8220 manufactured by Hitachi High-Technologies Corporation) under conditions of an acceleration voltage of 2 kV and a magnification of 1000 times, and a backscattered electron image was obtained.

[0097] <Measurement of aspect ratio of magnetic particles and degree of orientation of flat-shaped particles> Using the backscattered electron image obtained above, the aspect ratio of the magnetic particles was determined by the method described above, and the flat-shaped particles were identified from the aspect ratio value. Whether or not the magnetic layer contained flat-shaped particles was determined as described above, and it was determined that the magnetic layer contained flat-shaped particles. Furthermore, the degree of orientation of the magnetic particles identified as flat-shaped particles was determined by the method described above, and it was 13°. The average value (arithmetic mean) of the aspect ratios of all particles identified as flat-shaped particles was also determined as the aspect ratio of the flat-shaped particles contained in the magnetic layer. The determined aspect ratio was 0.071.

[0098] <Measurement of Organic Solvent Content in Magnetic Layer> The organic solvent content of the magnetic layer was determined in an ambient temperature of 23°C using the following method. The aluminum foil on one of the outermost layers of an electromagnetic wave shielding material cut to a size of 15 cm x 15 cm was peeled off with tweezers, and the exposed magnetic layer was scraped off to obtain a 0.5 g magnetic layer sample. Using the obtained magnetic layer sample, the organic solvent content of the magnetic layer was determined using the method described above. The determined organic solvent amount and the type of organic solvent detected by HS-GC / MS measurement are shown in Table 1. The amount of each organic solvent was calculated according to the description in the reference cited above. The electromagnetic wave shielding material of Example 1 has two magnetic layers. The two magnetic layers were prepared using the same method and underwent the same processing to prepare the electromagnetic wave shielding material, so the measurement results for the organic solvent obtained for one magnetic layer using the above method can also be used as the measurement results for the other magnetic layer.

[0099] <Evaluation of Shielding Ability Before and After Heat Aging at 80°C (KEC Method)> An electromagnetic shielding material cut to a size of 15 cm x 15 cm was placed between the antennas of a KEC method evaluation device including a signal generator, an amplifier, a pair of magnetic field antennas, and a spectrum analyzer. The ratio of the received signal strength without the electromagnetic shielding material to the received signal strength with the electromagnetic shielding material at a frequency of 100 kHz was calculated as the shielding ability. This was performed on the magnetic field antenna to determine the electromagnetic shielding ability (magnetic field shielding ability). KEC is an abbreviation for Kansai Electronics Industry Development Center. The shielding ability evaluated from the thus obtained value according to the following evaluation criteria is referred to as "shielding ability before aging at 80°C." After measuring the shielding ability before aging at 80°C, the electromagnetic shielding material was placed in a high-temperature atmosphere at 80°C for 24 hours, and then the shielding ability was determined using the above method. The shielding ability evaluated from the thus obtained value according to the following evaluation criteria is referred to as "shielding ability after aging at 80°C." The evaluation results are shown in Table 2. (Evaluation criteria) A: 30 dB or more B: 25 dB or more but less than 30 dB C: Less than 25 dB

[0100] <Peel Strength> Figures 1 and 2 are explanatory diagrams for measuring peel strength. The peel strength of the electromagnetic shielding material was measured using the following method. A measurement sample with a short side length of 2.5 cm and a long side length of 5 cm was cut from a 10 cm x 10 cm electromagnetic shielding material near the center, excluding the four edge surfaces of the electromagnetic shielding material. Aluminum foil (manufactured by Takeuchi Metal Foil & Powder Co., Ltd., model number A1N30H-O, thickness 50 μm) with a short side length of 2.5 cm and a long side length of 15 cm was prepared. One of the outermost metal layers (aluminum foil) of the measurement sample and the aluminum foil were bonded together using instant adhesive so that one short side of each foil overlapped, creating a tension margin. This tension margin was the 10 cm long portion of the aluminum foil to which the measurement sample was not bonded (see Figure 1). Thereafter, the outermost metal foil (copper foil) of the other side of the measurement sample (i.e., the side without the tensile margin) was placed in the center of the copper plate (manufactured by Hikari Co., Ltd., size: thickness 1 mm, short side length 5 cm, long side length 10 cm) and bonded to it using double-sided tape (see Figure 2). The portion of the copper plate where the electromagnetic wave shielding material was not attached was fixed to the lower chuck of the testing machine (see Figure 2). The tensile margin was then folded back 180° and fixed to the upper chuck of the testing machine, and a peel test was performed under the following measurement conditions. The measured load (unit: N (Newton)) was divided by the short side length (2.5 cm) to calculate the peel strength. (Measurement Conditions) Testing machine: Tensilon universal material testing machine (RTF-1310) manufactured by A&D Co., Ltd. Measurement environment: temperature 23°C, relative humidity 50% Load cell: 500 N (Newton) Pulling speed: 30 mm / min

[0101] The peel strength measured by the above method can be said to be an index of the adhesive strength between two adjacent layers in a laminate, and the higher the peel strength value measured by the above method, the higher the adhesive strength between the metal layer and the magnetic layer, and the more durable the electromagnetic wave shielding material. From the perspective of excellent durability, the peel strength measured by the above method is preferably 0.5 N / cm or more, and more preferably 2.0 N / cm or more. The durability of the electromagnetic wave shielding material was evaluated from the values ​​obtained above using the following evaluation criteria. The evaluation results are shown in Table 2. (Evaluation criteria) A: 2.0 N / cm or more B: 0.5 N / cm or more but less than 2.0 N / cm C: 0 N / cm or more but less than 0.5 N / cm

[0102] Example 2 An electromagnetic wave shielding material was produced and various evaluations were carried out in the same manner as in Example 1, except that the drying time in the film formation of the magnetic layer was changed to 15 minutes.

[0103] Example 3 An electromagnetic wave shielding material was produced and various evaluations were carried out in the same manner as in Example 1, except that the drying time in the film formation of the magnetic layer was changed to 30 minutes.

[0104] Example 4 An electromagnetic wave shielding material was produced and various evaluations were carried out in the same manner as in Example 1, except that the drying time in the film formation of the magnetic layer was changed to 120 minutes.

[0105] [Examples 5 to 7] Electromagnetic wave shielding materials were prepared and various evaluations were carried out in the same manner as in Example 1, except that the acrylic resins shown in Table 1 were used and the drying time in the film formation of the magnetic layer was changed to 30 minutes.

[0106] Example 8 A magnetic layer was produced by the method described for Example 1, except that the drying time in the film formation of the magnetic layer was changed to 30 minutes. The magnetic layer obtained above was used as the magnetic layer, and aluminum foil (JIS H4160:2006 standard compliant, alloy number 1N30 temper (1)O, Al content 99.3 mass% or more) having a thickness of 30 μm was used as the metal layer, and a laminate was produced by overlapping three layers of "aluminum foil (metal layer) / magnetic layer / aluminum foil (metal layer)" without interposing another layer between two adjacent layers. The upper and lower press plates of a plate-shaped press (large hot press TA-200-1W manufactured by Yamamoto Iron Works) were heated to 140°C (internal temperature of the press plate), and the laminate was placed at the center of the press plate, and a pressure of 4.66 N / mm was applied. 2 The aluminum foil and the magnetic layer were thermocompression-bonded by applying a pressure of 0.05 W and maintaining this pressure for 10 minutes. The upper and lower press plates were cooled to 50°C (internal temperature of the press plates) while maintaining the pressure, and then the laminate was removed from the plate press. Thus, the electromagnetic shielding material of Example 8 was obtained. The electromagnetic shielding material of Example 8 includes one multilayer structure of "aluminum foil (metal layer) / magnetic layer / aluminum foil (metal layer)." Various evaluations were performed on Example 8 using the methods described for Example 1.

[0107] Example 9 An electromagnetic wave shielding material was produced and various evaluations were performed using the same method as in Example 1, except that a 20 μm thick copper foil (JIS H3100:2018 compliant, alloy number C1020R-H, Cu content of 99.9% by mass or more) was used as the metal layer instead of the aluminum foil, and the drying time in the deposition of the magnetic layer was changed to 30 minutes.

[0108] [Example 10] An electromagnetic wave shielding material was prepared and various evaluations were carried out using the same method as in Example 1, except that the organic solvent in the magnetic layer-forming composition was changed to methyl ethyl ketone and the drying time in the magnetic layer formation was changed to 10 minutes.

[0109] Example 11 An electromagnetic wave shielding material was produced and various evaluations were performed using the same method as in Example 1, with the following exceptions: The drying time in the deposition of the magnetic layer was changed to 30 minutes; and Alpet 30-50 manufactured by Panac (a laminate formed by bonding a 30 μm-thick aluminum foil (metal layer with an Al content of 99.0% by mass or more) and a 50 μm-thick polyester film (resin layer) via a 3 μm-thick adhesive layer) was used instead of aluminum foil.

[0110] For the electromagnetic wave shielding materials of Examples 2 to 10, the thickness of each magnetic layer and each metal layer (aluminum foil or copper foil) was determined by the method described for Example 1. In all Examples, the thickness of each magnetic layer was 30 μm. The thickness of the metal layer (aluminum foil) was 30 μm, and the thickness of the metal layer (copper foil) was 20 μm. For the electromagnetic wave shielding material of Example 11, the thickness of each layer was also determined by the method described for Example 1, and the thickness of each layer was the above-mentioned thickness.

[0111] Comparative Example 1 An electromagnetic wave shielding material was prepared and various evaluations were carried out in the same manner as in Example 1, except that the resin shown in Table 1 was used instead of the acrylic resin and the drying time in the film formation of the magnetic layer was changed to 30 minutes.

[0112] [Comparative Example 2] A magnetic layer was produced by the method described for Example 1, except that the drying time in the film formation of the magnetic layer was changed to 30 minutes. The magnetic layer obtained above was used as the magnetic layer, and aluminum foil (JIS H4160:2006 standard compliant, alloy number 1N30 temper (1)O, Al content 99.3 mass% or more) having a thickness of 100 μm was used as the metal layer, and a laminate was produced by overlapping two layers of "aluminum foil (metal layer) / magnetic layer" without any other layer interposed therebetween. The upper and lower press plates of a plate-shaped press (large hot press TA-200-1W manufactured by Yamamoto Iron Works) were heated to 140°C (internal temperature of the press plates), and the laminate was placed at the center of the press plates, and a pressure of 4.66 N / mm was applied. 2The aluminum foil and the magnetic layer were thermocompression-bonded by applying a pressure of 0.05 W and maintaining this pressure for 10 minutes. The upper and lower press plates were cooled to 50°C (internal temperature of the press plates) while maintaining the pressure, and then the laminate was removed from the plate press. Thus, an electromagnetic wave shielding material of Comparative Example 2 was obtained. The electromagnetic wave shielding material of Comparative Example 2 consisted of two layers: "aluminum foil (metal layer) / magnetic layer." Various evaluations were performed on Comparative Example 2 using the methods described for Example 1.

[0113] [Comparative Example 3] An electromagnetic wave shielding material was produced and various evaluations were carried out in the same manner as in Example 1, except that the drying time in the formation of the magnetic layer was changed to 30 minutes and an additional 2 hours of drying was carried out in a vacuum dryer (internal atmosphere temperature 80°C).

[0114] Comparative Example 4 An electromagnetic wave shielding material was produced and various evaluations were carried out in the same manner as in Example 1, except that the drying time in the film formation of the magnetic layer was changed to 5 minutes.

[0115]

[0116]

[0117] The results shown in Table 2 confirm that the electromagnetic shielding materials of Examples 1 to 11 are excellent in heat resistance and durability.

[0118] One aspect of the present invention is useful in the technical fields of various electronic components and various electronic devices.

Claims

1. An electromagnetic wave shielding material having a magnetic layer containing magnetic particles and an acrylic resin between two metal layers, and the organic solvent content of the magnetic layer is 5 ppm or more and less than 1000 ppm by mass.

2. The electromagnetic shielding material according to claim 1, wherein the weight average molecular weight of the acrylic resin is 100,000 or more.

3. The electromagnetic shielding material according to claim 1, wherein the weight average molecular weight of the acrylic resin is from 800,000 to 2,000,000.

4. The electromagnetic shielding material according to claim 1, wherein the organic solvent content of the magnetic layer is 10 ppm or more and 100 ppm or less.

5. The electromagnetic shielding material according to claim 1, wherein the organic solvent is selected from the group consisting of methyl ethyl ketone and cyclohexanone.

6. The electromagnetic shielding material according to claim 1, further comprising one or more layers containing a resin between the magnetic layer sandwiched between the two metal layers and one or both of the two metal layers.

7. The electromagnetic shielding material according to claim 1, comprising two or more multi-layer structures each having the magnetic layer between two metal layers.

8. The electromagnetic shielding material according to claim 1, wherein one or more of the metal layers has a Cu content of 80.0 mass % or more.

9. The electromagnetic shielding material according to claim 1, wherein one or more of the metal layers has an Al content of 80.0 mass % or more.

10. The electromagnetic shielding material according to claim 1, wherein the weight-average molecular weight of the acrylic resin is 800,000 or more and 2,000,000 or less, the organic solvent content of the magnetic layer is 10 ppm or more and 100 ppm or less, the organic solvent is selected from the group consisting of methyl ethyl ketone and cyclohexanone, the material includes two or more multilayer structures having the magnetic layer between two metal layers, and at least one of the metal layers is a metal layer having a Cu content of 80.0 mass % or more.

11. The electromagnetic shielding material according to claim 1, wherein the weight-average molecular weight of the acrylic resin is 800,000 or more and 2,000,000 or less, the organic solvent content of the magnetic layer is 10 ppm or more and 100 ppm or less, the organic solvent is selected from the group consisting of methyl ethyl ketone and cyclohexanone, the material includes two or more multilayer structures having the magnetic layer between two metal layers, and at least one of the metal layers is a metal layer having an Al content of 80.0 mass % or more.

12. An electronic component comprising the electromagnetic shielding material according to any one of claims 1 to 11.

13. An electronic device comprising the electromagnetic shielding material according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Noise suppression sheet

    JP2010097969A

  • Adhesive film

    JP2015187260A

  • Soft magnetic flat powder

    JP2018131640A

  • Electromagnetic-wave absorber, its manufacturing method and various applications using the same

    JP2001358493A

  • Electromagnetic wave shield film

    JP2018088510A