Gas diffusion electrode base material and fuel cell

The gas diffusion electrode base material with a microporous layer on a conductive porous base material addresses the challenge of moisture retention and drainage by using a carbonization yield and organic polymers, resulting in improved power generation performance across current densities.

WO2024203218A1PCT designated stage expired Publication Date: 2024-10-03TORAY INDUSTRIES INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009307
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-11
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Gas diffusion electrode base materials in fuel cells face challenges in achieving both moisture retention at low current densities and high drainage performance at high current densities, leading to deteriorated power generation performance due to clogging and insufficient gas supply.

Method used

A gas diffusion electrode base material with a microporous layer on a conductive porous base material, featuring a carbonization yield of 55% or more after heating at 1000°C, an average particle size of 5 to 60 μm, and a surface arithmetic mean roughness of 5 to 20 μm, incorporating organic polymers like phenol resin and carbon fine particles, which enhance moisture retention and drainage properties.

Benefits of technology

The solution achieves excellent power generation performance at both low and high current densities by effectively managing moisture and gas supply, preventing clogging and ensuring efficient gas diffusion and drainage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-M000001
    Figure JPOXMLDOC01-APPB-M000001
  • Figure JPOXMLDOC01-APPB-M000002
    Figure JPOXMLDOC01-APPB-M000002
  • Figure JPOXMLDOC01-APPB-M000003
    Figure JPOXMLDOC01-APPB-M000003
Patent Text Reader

Abstract

Provided is a gas diffusion electrode base material excellent in moisture retention and drainage and having good power generation performance at low current density and high current density in a fuel cell. Provided is a gas diffusion electrode base material that has a microporous layer on at least one surface of a conductive porous base material wherein, in the microporous layer, the carbonization yield after heating at 1,000°C for 10 minutes is 55% or more, a filler has an average particle diameter of 5-60 μm and contains an organic polymer, 100 mass% of the microporous layer contains 10-45 mass% of the filler, and the arithmetic average roughness Sa of the surface of the microporous layer is 5-20 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Gas diffusion electrode substrate and fuel cell

[0001] The present invention relates to a gas diffusion electrode substrate used in a fuel cell, particularly a polymer electrolyte fuel cell, and a fuel cell including the gas diffusion electrode substrate.

[0002] Polymer electrolyte fuel cells, which generate electromotive force by supplying a hydrogen-containing fuel gas to the anode and an oxygen-containing oxidizing gas to the cathode through an electrochemical reaction at both electrodes, are generally constructed by stacking a separator, a gas diffusion electrode substrate, a catalyst layer, an electrolyte membrane, a catalyst layer, a gas diffusion electrode substrate, and a separator in this order. The gas diffusion electrode substrate must have high gas diffusivity to diffuse the gas supplied from the separator to the catalyst layer, high drainage properties to discharge water produced by the electrochemical reaction to the separator, and high conductivity to extract the generated current. For this reason, gas diffusion electrode substrates, which have a carbon sheet made of carbon fiber or the like as a substrate and a microporous layer formed on the surface thereof, are widely used.

[0003] However, such gas diffusion electrode substrates have the following problems: (1) when a polymer electrolyte fuel cell is operated in a low current density region, the amount of water produced is small, resulting in dry conditions, causing the electrolyte membrane to dry out and reduced proton conductivity, resulting in reduced power generation performance; and (2) when a polymer electrolyte fuel cell is operated in a high current density region, the amount of water produced is large, resulting in wet conditions, causing the gas diffusion electrode substrate to become clogged with the produced water, resulting in insufficient gas supply and reduced power generation performance. Therefore, gas diffusion electrode substrates are required to have both high moisture retention in a low current density region and high drainage properties in a high current density region. To solve this problem, a method has been adopted in which a microporous layer is formed on the surface of the gas diffusion electrode substrate and particles are incorporated into the microporous layer to improve moisture retention and drainage properties.

[0004] For example, a gas diffusion electrode substrate containing spacer particles in a microporous layer has been proposed (Patent Document 1).

[0005] Furthermore, a gas diffusion electrode substrate containing carbon powder in the microporous layer has been proposed (Patent Document 2).

[0006] Furthermore, a gas diffusion electrode substrate containing a hydrophilic additive in the microporous layer has been proposed (Patent Document 3).

[0007] JP 2006-331717 A JP 2016-195060 A International Publication No. 2014 / 014463

[0008] However, the technology described in Patent Document 1 can improve gas diffusion and achieve high drainage using spacer particles, but does not claim to have any effect on moisture retention. Furthermore, the technology described in Patent Document 2 can improve adhesion to the catalyst layer and drainage by using surface irregularities with carbon powder, but this is also ineffective in terms of moisture retention. Furthermore, the technology described in Patent Document 3 can improve moisture retention and drainage using hydrophilic additives, but because it uses inorganic substances such as metal oxides and carbon black as hydrophilic additives, the effect is insufficient.

[0009] In view of the background of the above-mentioned conventional technology, an object of the present invention is to provide a gas diffusion electrode substrate which achieves both moisture retention and drainage properties, which have been difficult to achieve in the past, and which has excellent power generation performance at both low and high current densities.

[0010] Embodiments of the present invention are as follows. (1) A gas diffusion electrode substrate having a microporous layer on at least one surface of a conductive porous substrate, wherein the microporous layer contains a filler containing an organic polymer, the filler having a carbonization yield of 55% or more after heating at 1,000°C for 10 minutes and an average particle size of 5 to 60 μm, the filler comprising 10 to 45 mass% of the microporous layer in 100 mass% of the microporous layer, and the arithmetic mean roughness Sa of the surface of the microporous layer is 5 to 20 μm. (2) The gas diffusion electrode substrate according to (1), wherein the F / C ratio of the surface of the microporous layer is 0.2 to 0.6. (3) The gas diffusion electrode substrate according to (1) or (2), wherein the O / C ratio of the surface of the microporous layer is 0.1 or less. (4) The gas diffusion electrode substrate according to any of (1) to (3), wherein the average particle size of the filler is larger than the thickness of the microporous layer. (5) The gas diffusion electrode substrate according to any one of (1) to (4), wherein the filler has an average particle size of 10 to 30 μm. (6) The gas diffusion electrode substrate according to any one of (1) to (5), wherein the organic polymer is at least one resin selected from the group consisting of phenolic resins, acrylic resins, ester resins, and ether resins. (7) The gas diffusion electrode substrate according to any one of (1) to (6), wherein the organic polymer is a phenolic resin. (8) The gas diffusion electrode substrate according to any one of (1) to (7), wherein the microporous layer has a thickness of 3 to 55 μm. (9) The gas diffusion electrode substrate according to any one of (1) to (8), wherein the microporous layer has pores with an average diameter of 10 to 60 μm, and the area ratio of the pores formed across the entire cross section of the microporous layer is 10 to 50%. (10) The gas diffusion electrode substrate according to any one of (1) to (9), wherein the conductive porous substrate is carbon paper. (11) A fuel cell comprising the gas diffusion electrode substrate according to any one of (1) to (10).

[0011] According to the present invention, it is possible to obtain a gas diffusion electrode substrate which has both moisture retention and drainage properties, which have been difficult to achieve in the past, and which has excellent power generation performance at both low and high current densities.

[0012] The present invention provides a gas diffusion electrode substrate having a microporous layer on at least one surface of a conductive porous substrate, wherein the microporous layer contains a filler containing an organic polymer, the filler having a carbonization yield of 55% or more after heating at 1,000°C for 10 minutes and an average particle size of 5 to 60 μm, the filler being contained in an amount of 10 to 45 mass% per 100 mass% of the microporous layer, and the arithmetic mean roughness Sa of the surface of the microporous layer being 5 to 20 μm.

[0013] The conductive porous substrate, microporous layer, and fuel cell constituting the gas diffusion electrode substrate of the present invention are described in detail below. [Conductive Porous Substrate] Porous substrates containing carbon fibers and metal porous bodies are generally used as the conductive porous substrate in the present invention. Among these, porous substrates containing carbon fibers, such as carbon fiber woven fabrics, carbon fiber paper sheets, carbon felt, and carbon paper, are preferably used in the present invention. Here, carbon paper refers to a sheet formed by binding a carbon fiber paper sheet with a binder such as a resin carbide. Among these, carbon paper is more preferably used because of its excellent corrosion resistance and its ability to absorb dimensional changes in the thickness direction of the electrolyte membrane, i.e., its excellent "springiness."

[0014] Examples of carbon fibers that can be preferably used for the conductive porous substrate include polyacrylonitrile (PAN)-based, pitch-based, and rayon-based carbon fibers. PAN-based and pitch-based carbon fibers are particularly preferred due to their excellent mechanical strength. Natural and synthetic fibers, such as rayon, acrylic, and cellulose fibers, may also be mixed.

[0015] The average diameter of the carbon fiber single fibers is preferably 3 to 20 μm. When the average diameter is 3 μm or more, the pore size of the conductive porous substrate increases, improving gas diffusion and drainage, thereby improving the power generation performance of the fuel cell. On the other hand, when the average diameter is 20 μm or less, water vapor diffusion decreases, making it possible to prevent the electrolyte membrane and catalyst layer from drying out and resulting in a decrease in performance. In other words, moisture retention is improved. When the average diameter of the carbon fiber single fibers is 5 to 10 μm, these effects are enhanced, making it more preferable.

[0016] When a carbon fiber paper sheet or carbon paper is used as the conductive porous substrate, the average length of the carbon fiber single fibers is preferably 3 to 20 mm. When the average length is 3 mm or more, the mechanical strength, electrical conductivity, and thermal conductivity of the conductive porous substrate are improved. On the other hand, when the average length is 20 mm or less, the dispersion of the carbon fibers during papermaking is improved, and a homogeneous conductive porous substrate is obtained. When the average length of the carbon fiber single fibers is 5 to 15 mm, these effects are enhanced, and this is more preferable.

[0017] The mass per unit area of ​​the conductive porous substrate (basis weight) is 20 to 50 g / m 2 It is preferable that the basis weight is 20 g / m 2 When the basis weight is 50 g / m or more, the mechanical strength and conductivity of the conductive porous substrate are improved. 2 When the weight per unit area of ​​the conductive porous substrate is 30 to 40 g / m or less, the gas diffusibility of the conductive porous substrate is good. 2 This is more preferable because it enhances these effects.

[0018] The basis weight of the conductive porous substrate can be adjusted by controlling the amount of carbon fiber, resin carbide, or the like, which is a constituent material of the conductive porous substrate.

[0019] As the conductive porous substrate, a substrate that has a water-repellent resin attached to the inside by water-repellent treatment is preferably used.As the water-repellent resin, a fluororesin having a fluoroalkyl chain is preferred.As the fluororesin, PTFE (polytetrafluoroethylene), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), ETFE (tetrafluoroethylene-ethylene copolymer), PVDF (polyvinylidene fluoride), PVF (polyvinyl fluoride) and the like can be mentioned, and PTFE or FEP that exhibits high water repellency is preferred.

[0020] The amount of the water-repellent resin is not particularly limited, but is preferably 0.1 to 20% by mass relative to 100% by mass of the entire conductive porous substrate. Within this range, water repellency is sufficiently exhibited, while the water-repellent resin can be prevented from blocking pores that serve as gas diffusion paths and from increasing electrical resistance.

[0021] In polymer electrolyte fuel cells, the gas diffusion electrode substrate is required to have high gas diffusivity to diffuse the gas supplied from the separator to the catalyst and high drainage properties to discharge water generated during the electrochemical reaction to the separator. Therefore, the conductive porous substrate preferably has a pore size peak between 10 and 100 μm. The pore size and its distribution can be determined by pore size distribution measurement using a mercury porosimeter. To determine the pore size of the conductive porous substrate, the conductive porous substrate alone may be measured, or the gas diffusion electrode substrate after the microporous layer has been formed may be measured. When measuring the gas diffusion electrode substrate, the layer structure is confirmed by observing a cross section parallel to the thickness direction of the gas diffusion electrode substrate with a scanning electron microscope (SEM), and the pore size of the conductive porous substrate is roughly determined from the SEM image. Next, the pore size of the conductive porous substrate is determined by matching the multiple pore size peaks obtained by the mercury porosimeter with the approximate values ​​obtained from the SEM image.

[0022] In the present invention, the porosity of the conductive porous substrate is preferably 80 to 95%. When the porosity is 80% or more, gas diffusibility is increased and power generation performance is improved. On the other hand, when the porosity is 95% or less, the mechanical strength of the conductive porous substrate is increased and the conductivity is also improved. When the porosity of the conductive porous substrate is 85 to 90%, these effects are enhanced, and therefore it is more preferable. The porosity of the conductive porous substrate can be measured using a hydrometer or the like.

[0023] The thickness of the conductive porous substrate of the present invention is preferably 90 to 180 μm. Here, the thickness of the conductive porous substrate refers to the thickness when both surfaces are sandwiched under a pressure of 0.15 MPa. A thickness of 90 μm or more maintains mechanical strength and facilitates handling during the manufacturing process. In addition, the spring properties are enhanced, allowing the gas diffusion electrode substrate to absorb dimensional changes due to expansion and contraction of the electrolyte membrane during use in a fuel cell, and gas diffusion in the in-plane direction is improved, thereby improving power generation performance. On the other hand, when the thickness of the conductive porous substrate is 180 μm or less, gas diffusion in the thickness direction is enhanced, and the conductive path in the thickness direction is shortened, improving conductivity, thereby improving power generation performance. A thickness of 110 to 150 μm is more preferable because these effects are enhanced.

[0024] [Microporous Layer] Next, the microporous layer will be described. The gas diffusion electrode substrate of the present invention has a microporous layer on at least one surface of the conductive porous substrate, but preferably has a microporous layer on only one surface of the conductive porous substrate. The role of the microporous layer includes water management such as moisturizing the electrolyte membrane and catalyst layer and draining generated water, reducing the interfacial electrical resistance between the catalyst layer and the gas diffusion electrode substrate, and preventing damage to the electrolyte membrane due to carbon fibers protruding from the conductive porous substrate. In order to improve moisture retention and drainage, the microporous layer has a filler containing an organic polymer in the present invention. Furthermore, the layer preferably contains carbon fine particles and a water-repellent resin.

[0025] The filler component of the present invention is not particularly limited as long as it contains an organic polymer, but examples of usable fillers include phenolic resins, acrylic resins, ester resins, ether resins, fluororesins, styrene resins, urethane resins, and melamine resins, and the carbonization yield after heating at 1,000° C. for 10 minutes must be 55% or higher. If the carbonization yield after heating at 1,000° C. for 10 minutes is 55% or higher, a moderate amount of the organic polymer's hydroxyl groups and ester bond moieties that have an affinity for water remain, improving moisture retention and drainage, and the moderate progress of carbonization improves electrical conductivity, improving the power generation performance of the fuel cell.

[0026] As the organic polymer, it is preferable to use at least one resin selected from the group consisting of phenolic resin, acrylic resin, ester resin, and ether resin, and among these, it is particularly preferable to use phenolic resin. The carbonization yield can be measured using a TGA device such as an EXTRA TGA6200 manufactured by SII. Specifically, the temperature is increased from 50°C to 1,000°C at a heating rate of 10°C / min in a nitrogen atmosphere and held at 1,000°C for 10 minutes. The mass after being held at 1,000°C is then divided by the initial mass and multiplied by 100 to obtain the carbonization yield.

[0027] Furthermore, the carbon crystallite diameter Lc(002), which indicates the degree of graphitization of the filler containing the organic polymer of the present invention, is preferably 15 angstroms or less. When the crystallite diameter is 15 angstroms or less, the organic polymer is present in sufficient amount, thereby improving moisture retention and drainage. Note that the crystallite diameter of carbon black is usually greater than 20 angstroms, and that of graphite is greater than 100 angstroms.

[0028] The filler of the present invention has an average particle size of 5 to 60 μm. When the average particle size is 5 μm or more, moisture retention and drainage are improved, and power generation performance at low and high current densities is improved. On the other hand, when the average particle size is 60 μm or less, the conductivity of the microporous layer is increased, and power generation performance is improved. An average particle size of 10 to 30 μm is more preferable because it enhances these effects.

[0029] A method for measuring the average particle size from the gas diffusion electrode substrate will be described. First, an ion milling device is used to randomly prepare 10 samples for cross-sectional observation by cutting the gas diffusion electrode substrate parallel to the thickness direction. At this time, the cutting position of the gas diffusion electrode substrate is not particularly limited, and the size of the cross-sectional observation sample is 5 mm (width of the cross-sectional cut portion) × 12 mm. Next, a scanning electron microscope is used to obtain an image of the cross section of the microporous layer at any location on the sample, enlarged 1,000 times. The area of ​​each filler present in the microporous layer in the image is measured using the image analysis software "ImageJ", and the circle equivalent diameter is calculated using the following formula, and the average of the circle equivalent diameters obtained in the image is calculated. The same procedure is performed for the images of 10 samples, and the overall arithmetic mean value is taken as the average particle size of the filler.

[0030]

[0031] Furthermore, when the filler of the present invention is spherical, the conductivity of the microporous layer is increased, and the surface of the microporous layer is highly irregular, which makes it easier for water vapor to remain, leading to improved moisture retention, and is therefore preferred.

[0032] In the present invention, a filler is said to be spherical when the aspect ratio, calculated as the ratio of the major axis to the minor axis of the filler, is in the range of 1.0 to 1.3. Here, the major axis refers to the longest line segment connecting two points within the filler, and the minor axis refers to the longest line segment perpendicular to the major axis.

[0033] The method for measuring the aspect ratio will be described. Using an ion milling device, ten samples for cross-section observation are randomly prepared by cutting the gas diffusion electrode substrate parallel to the thickness direction. At this time, the cutting position of the gas diffusion electrode substrate is not particularly limited, and the size of the cross-section observation sample is 5 mm (width of the cross-section cut portion) × 12 mm. Next, using a scanning electron microscope, the cross section of the microporous layer at any location on the sample is magnified 300 times to obtain an image, and the image analysis software "ImageJ" is used to measure the major axis and minor axis of each filler present in the microporous layer in the image to determine the aspect ratio, and the average value is calculated. The same procedure is performed for the images of 10 samples, and the overall arithmetic average value is taken as the aspect ratio of the filler.

[0034] The filler content of the present invention is 10 to 45% by mass, preferably 20 to 30% by mass, based on 100% by mass of the microporous layer. A filler content of 10% by mass or more provides sufficient moisture retention and drainage. Furthermore, a filler content of 45% by mass or less provides high mechanical strength, electrical conductivity, and thermal conductivity of the microporous layer, resulting in good power generation performance. A filler content of 20 to 40% by mass is more preferred.

[0035] The method for measuring the filler content from a gas diffusion electrode substrate is as follows. First, a portion of the microporous layer is scraped off from the gas diffusion electrode substrate, and the mass is measured. Next, the scraped microporous layer is heated in air at 500°C for 1 hour, and only the filler is isolated from the remaining mixture of carbon fine particles and filler using, for example, a membrane filter, and the mass is measured to calculate the filler content in mass%.

[0036] Furthermore, the average particle size of the filler of the present invention is preferably larger than the thickness of the microporous layer. This increases the surface roughness of the microporous layer, making it easier for water vapor to remain, leading to improved moisture retention. When a microporous layer is formed on a conductive porous substrate, part of the microporous layer may penetrate into the conductive porous substrate. The thickness of the microporous layer here refers to the thickness of the part that does not penetrate into the conductive porous substrate, and can be calculated by subtracting the thickness of the conductive porous substrate from the thickness of the gas diffusion electrode substrate. The thickness of the conductive porous substrate can be measured before forming the microporous layer, or after removing the microporous layer from the gas diffusion electrode substrate by heating at 500°C in air for 1 hour and scrubbing it off, for example.

[0037] Next, the carbon fine particles preferably contained in the microporous layer will be described. Specific examples of carbon fine particles that can be used include carbon black, carbon nanofibers, carbon nanotubes, and graphene. Among these, inexpensive carbon black is preferably used.

[0038] The specific surface area of ​​carbon particles is 20 to 40 m 2 / g. The method for measuring the specific surface area is not particularly limited, but it can be determined, for example, by the nitrogen adsorption method. The nitrogen adsorption method is a technique in which degassed carbon fine particles are sealed together with nitrogen in a container cooled to the temperature of liquid nitrogen, the amount of nitrogen adsorbed on the surface of the carbon fine particles at equilibrium is measured, and the specific surface area is calculated from this value. When the specific surface area of ​​the carbon fine particles is 20 m 2 When the specific surface area of ​​the carbon fine particles is 40 m / g or more, the dispersibility of the carbon fine particles in the coating liquid for forming the microporous layer described below is improved, and a uniform microporous layer can be formed. In addition, the moisture retention and drainage properties of the microporous layer are improved, and power generation performance is improved. 2 When the carbon content is 0.1g or less, the oxidation corrosion reaction of carbon is suppressed, and the durability of the fuel cell is improved.

[0039] Furthermore, fibrous carbon particles such as carbon nanofibers and carbon nanotubes form conductive paths within the microporous layer, which has the effect of lowering the electrical resistance of the microporous layer.

[0040] The water-repellent resin preferably contained in the microporous layer is a fluororesin having a fluoroalkyl chain, from the viewpoints of chemical stability, water repellency, etc., and, like the fluororesins preferably used in the water-repellent treatment of conductive porous substrates, examples thereof include PTFE (polytetrafluoroethylene), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), and ETFE (tetrafluoroethylene-ethylene copolymer).

[0041] Since fluororesins are generally insoluble in water, organic solvents, etc., it is preferable to use a dispersion of a water-repellent resin processed into fine particles when producing a coating liquid for forming a microporous layer (described below). Examples of dispersions of fine particle water-repellent resins include "Polyflon (registered trademark)" D-210C and ND-110 (both manufactured by Daikin Industries, Ltd.), 120-JRB, and 31-JR (both manufactured by Mitsui-Chemours Fluoroproducts Co., Ltd.).

[0042] Silicone having a siloxane bond can also be used as the water-repellent resin.

[0043] In addition to the filler and water-repellent resin, which have a carbonization yield of 55% or more after heating at 1,000°C for 10 minutes and an average particle size of 5 to 60 μm, the composition may also contain a thermosetting resin, such as a phenolic resin, an epoxy resin, an acrylate resin, or a furan resin.

[0044] Furthermore, pores may be formed in the microporous layer to enhance moisture retention and drainage. The pores are preferably formed by impregnating the microporous layer with a pore-forming agent that is burned off at high temperatures, followed by sintering and burning off the pores.

[0045] The microporous layer of the present invention preferably has pores with an average diameter of 10 to 60 μm. When the average pore diameter is 10 μm or more, drainage is improved and power generation performance at high current densities is improved. On the other hand, when the average diameter is 60 μm or less, moisture retention is improved and power generation performance at low current densities is improved. An average diameter of 30 to 50 μm is more preferable because these effects are enhanced.

[0046] In the present invention, the average diameter of pores refers to the average value of the circle-equivalent diameters of pores. The measurement method involves cutting a gas diffusion electrode substrate parallel to the thickness direction using an ion milling device, magnifying the cross section of the sample with a scanning electron microscope by 1,000 times to obtain an image, and measuring the area of ​​each pore present in the microporous layer in the image using image analysis software "ImageJ." The circle-equivalent diameter is calculated using the following formula: The average value of the obtained circle-equivalent diameters of 1 μm or more is taken as the average diameter. Ten samples are cut out, and the arithmetic mean value of the average diameters of the 10 samples is taken as the average diameter of the microporous layer.

[0047]

[0048] Furthermore, the area ratio of pores formed across the entire cross section of the microporous layer (hereinafter referred to as cross-sectional porosity) is preferably 10 to 50%. A cross-sectional porosity of 10% or more improves drainage and power generation performance at high current densities. On the other hand, a cross-sectional porosity of 50% or less improves moisture retention and power generation performance at low current densities. A cross-sectional porosity of 15 to 30% is more preferable because it enhances these effects.

[0049] The cross-sectional porosity is the area ratio of pores to the entire cross section of a sample obtained by cutting the microporous layer parallel to the thickness direction. The measurement method involves obtaining an image of the cross section magnified 1,000 times with a scanning electron microscope, measuring the area of ​​pores with a circle-equivalent diameter of 1 μm or more using image analysis software "ImageJ," and determining the ratio of the area of ​​the pores to the entire cross-sectional area of ​​the microporous layer, which is then used to determine the cross-sectional porosity. Ten samples are cut out, and the arithmetic mean value of the cross-sectional porosities of the 10 samples is used as the cross-sectional porosity of the microporous layer.

[0050] Pores can be formed by, for example, blending a pore-forming agent in a coating liquid for forming a microporous layer, which will be described later, applying the coating liquid to a conductive porous substrate, and then sintering the substrate to burn off the pore-forming agent.

[0051] The pore-forming agent material is not particularly limited as long as it is a material that burns off or shrinks under the sintering conditions of the gas diffusion electrode substrate and forms pores in the microporous layer. Examples of suitable materials include acrylic resins, styrene resins, starch, polylactic acid resins, sublimable low molecular weight materials, and microballoons. Sublimable low molecular weight materials are typically low-molecular-weight organic powders with a molecular weight of 1,000 or less that sublimate and burn off at the sintering temperature. Examples of sublimable low molecular weight materials include anthracene, pentacene, and phenanthrene. Microballoons are hollow particles that expand significantly upon heating, forming pores around them. Eventually, the resin portion thermally decomposes or shrinks, leaving only the pores. Various materials are commercially available. Examples include "MatsumotoSphere (registered trademark)" (manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd.) and "Expancel (registered trademark)" (manufactured by Nippon Phillite Co., Ltd.).

[0052] When carbon fine particles are contained in the coating liquid for forming the microporous layer, the amount of the pore-forming agent is preferably 10 to 200 parts by mass, and more preferably 30 to 100 parts by mass, relative to 100 parts by mass of the carbon fine particles. When the amount of the pore-forming agent is 10 parts by mass or more, sufficient pores are present, resulting in good drainage. When the amount of the pore-forming agent is 200 parts by mass or less, the microporous layer has excellent mechanical strength, electrical conductivity, and thermal conductivity, and exhibits good power generation performance.

[0053] The electrolyte may also contain fine particles of iridium oxide, ruthenium oxide, titanium oxide, etc., which promote water electrolysis in a reverse potential state when hydrogen is deficient.Furthermore, the electrolyte may contain fine particles of cerium oxide, manganese oxide, etc., which inactivate hydroxide radicals generated at the anode electrode.

[0054] The basis weight of the microporous layer of the present invention is 5 to 35 g / m 2 It is preferable that the basis weight of the microporous layer is 5 g / m 2 When the microporous layer has a surface area of ​​35 g / m or more, the carbon fibers protruding from the surface of the conductive porous substrate are covered, thereby preventing damage to the electrolyte membrane. In addition, the contact resistance between the gas diffusion electrode substrate and the catalyst layer can be reduced, and the electrolyte membrane can be prevented from drying out. In addition, when the microporous layer has a surface area of ​​35 g / m or more, the carbon fibers protruding from the surface of the conductive porous substrate are covered, and the electrolyte membrane can be prevented from being damaged. 2 When the weight per unit area of ​​the microporous layer is 10 to 25 g / m or less, the drainage property is good. 2 This is more preferable because it enhances these effects.

[0055] The thickness of the microporous layer is preferably 3 to 55 μm. A thickness of 3 μm or more covers carbon fibers protruding from the surface of the conductive porous substrate, thereby preventing damage to the electrolyte membrane and further improving moisture retention. On the other hand, a thickness of 55 μm or less increases the conductivity of the gas diffusion electrode substrate and further improves drainage. A thickness of 5 to 40 μm is more preferable because it enhances these effects.

[0056] The thickness of the microporous layer can be determined by placing the conductive porous substrate on a smooth surface plate, measuring the thickness of the conductive porous substrate under a pressure of 0.15 MPa, then similarly measuring the thickness of the gas diffusion electrode substrate on which the microporous layer has been formed, and subtracting the thickness of the conductive porous substrate from the thickness of the gas diffusion electrode substrate. When measuring the thickness from the gas diffusion electrode substrate, the microporous layer is heated in air at 500°C for 1 hour and then removed by scraping, and only the conductive porous substrate is taken out, and the thickness can be calculated from the difference between the thickness before and after removing the microporous layer.

[0057] The arithmetic mean roughness Sa of the surface of the microporous layer of the present invention is 5 to 20 μm. When Sa is 5 μm or more, the surface has large irregularities, which makes it easier for water vapor to remain, increasing moisture retention and improving power generation performance at low current densities. On the other hand, when Sa is 20 μm or less, the adhesion between the microporous layer and the catalyst layer is improved, and the mechanical properties and durability of the microporous layer itself are also improved. An Sa of 6 to 15 μm is more preferable because it enhances these effects. The arithmetic mean roughness (Sa) can be determined by measuring Sa over an area of ​​8.4 mm × 6.0 mm at any four locations on the microporous layer side surface of a 30 mm × 30 mm gas diffusion electrode substrate sample using a laser microscope or the like, and calculating the average value.

[0058] The fluorine atom / carbon atom ratio (F / C ratio) on the surface of the microporous layer of the present invention is preferably 0.2 to 0.6. When the F / C ratio is 0.2 or more, the water repellency of the surface is enhanced and drainage is improved. On the other hand, when the F / C ratio is 0.6 or less, moisture retention is improved.

[0059] The oxygen atom / carbon atom ratio (O / C ratio) on the surface of the microporous layer of the present invention is preferably 0.1 or less. If the O / C ratio is more than 0.1, the electrical conductivity decreases, which may result in a decrease in power generation performance.

[0060] The F / C ratio and O / C ratio can be measured by performing elemental analysis at five random locations on the surface of the microporous layer side of the gas diffusion electrode substrate using an X-ray photoelectron spectroscopy (XPS), quantifying the element concentrations of fluorine (F), oxygen (O), and carbon (C), determining the F / C ratio and O / C ratio, and calculating the average values ​​of the five locations.

[0061] The microporous layer can be formed by applying a coating liquid for forming a microporous layer containing the above-mentioned filler and carbon fine particles to at least one surface of the conductive porous substrate.

[0062] The coating liquid may contain a dispersion medium such as water or an organic solvent, and may also contain a dispersion aid such as a surfactant. Water is preferred as the dispersion medium, and a nonionic surfactant is preferred as the dispersion aid.

[0063] The coating of the coating liquid onto the conductive porous substrate can be carried out using various commercially available coating devices. Coating methods that can be used include screen printing, rotary screen printing, spray atomization, intaglio printing, gravure printing, die coater coating, bar coating, and blade coating. The coating methods are merely examples and are not necessarily limited to these.

[0064] After the coating liquid is applied to the conductive porous substrate, it is preferable to dry the coating liquid at a temperature of 80 to 180°C. That is, the coated product is preferably placed in a dryer set at a temperature of 80 to 180°C and dried for 2 to 30 minutes. The drying air volume can be determined appropriately, but rapid drying may induce microcracks on the surface. After drying, the coated product is preferably placed in a muffle furnace, a baking furnace, or a high-temperature dryer and sintered preferably at a temperature of 300 to 380°C for 5 to 20 minutes to melt the water-repellent resin and use it as a binder between the carbon fine particles to form a microporous layer.

[0065] [Gas diffusion electrode substrate] The thickness of the gas diffusion electrode substrate of the present invention is preferably 130 to 190 μm. Here, the thickness of the gas diffusion electrode substrate is the thickness when both surfaces are sandwiched under a pressure of 0.15 MPa. When the thickness of the gas diffusion electrode substrate is 130 μm or more, mechanical strength is maintained and handling during the manufacturing process is easy. On the other hand, when the thickness of the gas diffusion electrode substrate is 190 μm or less, gas diffusivity is increased and electrical resistance is reduced, thereby improving the power generation performance of the fuel cell. The thickness of the gas diffusion electrode substrate can be adjusted by appropriately adjusting the thickness of the conductive porous substrate and the microporous layer.

[0066] [Membrane Electrode Assembly] In the present invention, a membrane electrode assembly can be formed by bonding the above-mentioned gas diffusion electrode substrate to at least one side of a solid polymer electrolyte membrane having catalyst layers on both sides. The solid polymer electrolyte membrane preferably has high proton conductivity and oxidation resistance and low gas crossover, and examples thereof include those made of fluorine-based polymers and hydrocarbon-based polymers. Furthermore, the catalyst layer is preferably made of a mixture of catalyst-supported carbon particles, in which catalyst fine particles made of a noble metal such as platinum, palladium, ruthenium, iridium, or rhodium, or an oxide thereof, are supported on carbon particles, and a proton-conducting polymer.

[0067] When joining a gas diffusion electrode substrate to a solid polymer electrolyte membrane having a catalyst layer, by placing the microporous layer side of the gas diffusion electrode substrate on the catalyst layer side, various effects are achieved, such as water management such as keeping the electrolyte membrane and catalyst layer moist and discharging generated water, reducing the interfacial electrical resistance between the catalyst layer and the gas diffusion electrode substrate, and suppressing damage to the electrolyte membrane due to carbon fibers or the like protruding from the conductive porous substrate.

[0068] [Fuel Cell] The fuel cell of the present invention includes the gas diffusion electrode substrate of the present invention. That is, the fuel cell of the present invention has separators on both sides of the membrane electrode assembly described above. That is, a fuel cell is constructed by disposing separators on both sides of the membrane electrode assembly described above. Typically, a polymer electrolyte fuel cell is constructed by stacking a plurality of such membrane electrode assemblies (fuel cell units) sandwiched between separators via gaskets on both sides. For example, by preparing 200 to 500 fuel cell units and connecting them in series, a high voltage of 40 to 200 kV can be generated, and such a fuel cell stack can be used as a power source for a fuel cell vehicle or the like.

[0069] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following descriptions.

[0070] [Raw material] Filler - Phenolic resin particles "Bellpearl (registered trademark)" C800 (manufactured by Air Water Bellpearl Inc., spherical, average particle size (catalog value): 15 μm, aspect ratio: 1.0, carbonization yield after heating at 1,000°C for 10 minutes: 95%, crystallite size Lc(002): 11 angstroms) - Phenolic resin particles "Bellpearl (registered trademark)" R700 (manufactured by Air Water Bellpearl Inc., spherical, average particle size (catalog value): 15 μm, aspect ratio: 1.0, carbonization yield after heating at 1,000°C for 10 minutes: 60%) - Phenolic resin particles "Bellpearl (registered trademark)" C2000SR (manufactured by Air Water Bellpearl Inc., spherical, average particle size (catalog value): 8 μm, aspect ratio: 1.0, carbonization yield after heating at 1,000°C for 10 minutes: 99%) Phenolic resin particles "LPS (registered trademark)" 50C (manufactured by Lignite Corporation, spherical, average particle size (catalog value): 50 μm, aspect ratio: 1.0, carbonization yield after heating at 1,000°C for 10 minutes: 56%) Phenolic resin particles "LPS (registered trademark)" 50A (manufactured by Lignite Corporation, spherical, average particle size: 50 μm, aspect ratio: 1.0, carbonization yield after heating at 1,000°C for 10 minutes: 52%) Phenolic resin particles "Bellpearl (registered trademark)" R100 (manufactured by Air Water Bellpearl Inc., spherical, average particle size (catalog value): 1.5 μm, aspect ratio: 1.0, carbonization yield after heating at 1,000°C for 10 minutes: 60%) Phenolic resin particles "LPS (registered trademark)" 100C (manufactured by Lignite Corporation, spherical, average particle size (catalog value): 100 μm, aspect ratio: 1.0, carbonization yield after heating at 1,000°C for 10 minutes: 57%); and fibrous conductive potassium titanate "Dentol (registered trademark)" WK-200B (manufactured by Otsuka Chemical Co., Ltd., fibrous, fiber length: 15 μm, aspect ratio: 50, carbonization yield after heating at 1,000°C for 10 minutes: 95%).

[0071] <Measurement of basis weight of microporous layer> The mass [g] of the conductive porous substrate was measured using a precision balance in a 10 cm square. Next, the mass [g] of the gas diffusion electrode substrate on which the microporous layer was formed was measured in a 10 cm square. The mass of the conductive porous substrate was subtracted from the mass of the gas diffusion electrode substrate to obtain the sample area (0.01 m). 2) is the basis weight [g / m 2 ].

[0072] <Measurement of microporous layer thickness> The conductive porous substrate was placed on a smooth surface plate, and a pressure of 0.15 MPa was applied to measure the difference in height between when the object to be measured (conductive porous substrate) was present and when it was absent. Sampling was performed at 10 different locations, and the average of the measured height differences was taken as the thickness, which was the thickness of the conductive porous substrate. Next, the thickness of the gas diffusion electrode substrate on which the microporous layer was formed was measured in the same manner. The thickness of the conductive porous substrate was subtracted from the thickness of the gas diffusion electrode substrate to obtain the thickness [μm] of the microporous layer.

[0073] <Measurement of carbonization yield of filler> The carbonization yield was measured using a TGA device (EXTRA TGA6200 manufactured by SII Corporation). The temperature was raised from 50°C to 1,000°C at a heating rate of 10°C / min in a nitrogen atmosphere and held at 1,000°C for 10 minutes. The mass after being held at 1,000°C was then divided by the initial mass and multiplied by 100 to obtain the carbonization yield [%].

[0074] <Calculation of Filler Content> The filler content can be calculated by the following formula.

[0075] Filler content [mass %] = mass of filler contained in microporous layer / mass of microporous layer.

[0076] Here, a method for measuring the filler content [mass %] of the microporous layer from the gas diffusion electrode substrate is described. First, a portion of the microporous layer is scraped off from the gas diffusion electrode substrate, and its mass is measured (mass A). Next, the scraped microporous layer is heated in air at 500°C for 1 hour, and the remaining mixture of carbon fine particles and filler is mixed with pure water. After that, the filler alone is isolated using a membrane filter with a pore size of 0.45 µm (manufactured by Advantec Toyo Co., Ltd.). After the membrane filter is dried, its mass is measured (mass B), and the mass is calculated as mass B / mass A x 100.

[0077] <Measurement of arithmetic mean roughness Sa of surface> The arithmetic mean roughness (Sa) of the microporous layer side surface of the gas diffusion electrode substrate was measured in an area of ​​8.4 mm × 6.0 mm using a laser microscope VK-X100 (manufactured by Keyence Corporation). Sa was measured at any four points on a 30 mm × 30 mm sample, and the average value was calculated.

[0078] <Measurement of Surface F / C Ratio> Elemental analysis was performed on five randomly selected locations on the surface of the microporous layer side of the gas diffusion electrode substrate using an X-ray photoelectron spectrometer (XPS) Model 5400 (manufactured by ULVAC-PHI, Inc.) The elemental concentrations [%] of fluorine (F) and carbon (C) were quantified, the F / C ratio was determined, and the average value of the five locations was calculated.

[0079] <Measurement of Surface O / C Ratio> Elemental analysis was performed on five randomly selected locations on the surface of the microporous layer side of the gas diffusion electrode substrate using an X-ray photoelectron spectrometer (XPS) Model 5400 (manufactured by ULVAC-PHI, Inc.) The elemental concentrations [%] of oxygen (O) and carbon (C) were quantified to determine the O / C ratio, and the average value of the five locations was calculated.

[0080] <Measurement of the average diameter of pores> First, using an ion milling apparatus IM4000 (manufactured by Hitachi High-Tech Corporation), 10 samples for cross-section observation were randomly prepared by cutting the gas diffusion electrode substrate parallel to the thickness direction. At this time, the cutting position of the gas diffusion electrode substrate was not particularly limited, and the size of the cross-section observation sample was 5 mm (width of the cross-sectional cut portion) × 12 mm. Next, using a scanning electron microscope SU8010 (manufactured by Hitachi High-Tech Corporation), an image of the cross section of the microporous layer at any location on the sample was obtained at a magnification of 1,000 times, and the area of ​​each pore in the image was measured using the image analysis software "ImageJ", and the circle equivalent diameter was calculated using the following formula. Of the obtained circle equivalent diameters, the average value of those with a diameter of 1 μm or more was calculated. The same procedure was performed on the images of 10 samples, and the overall arithmetic mean value was taken as the average diameter of the pores.

[0081]

[0082] <Measurement of cross-sectional porosity> In the same manner as in <Measurement of average pore diameter> above, 10 samples for cross-section observation were prepared by cutting the gas diffusion electrode substrate parallel to the thickness direction, and images of the cross section of the microporous layer at any location were obtained at a magnification of 1,000 times. Using the image analysis software "ImageJ," the area of ​​pores with a circle-equivalent diameter of 1 μm or more shown in <Measurement of average pore diameter> was measured, and the ratio of the area of ​​the pores to the area of ​​the entire microporous layer was calculated. The same procedure was performed on the images of the 10 samples, and the overall arithmetic average was taken as the cross-sectional porosity [%].

[0083] <Evaluation of power generation characteristics> A catalyst solution was prepared by sequentially adding 1.00 g of platinum-supported carbon (manufactured by Tanaka Kikinzoku Kogyo K.K., platinum support amount: 50% by mass), 1.00 g of purified water, 8.00 g of Nafion (registered trademark) solution (5.0% by mass of Nafion (registered trademark) manufactured by Sigma-Aldrich Corporation), and 18.00 g of isopropyl alcohol (manufactured by Nacalai Tesque, Inc.).

[0084] Next, the catalyst solution was sprayed onto a piece of "Naflon (registered trademark)" PTFE tape "TOMBO (registered trademark)" No. 9001 (manufactured by Nichias Corporation) cut to 50 mm x 50 mm, and the tape was dried at room temperature to obtain a platinum content of 0.3 mg / cm. 2 A PTFE sheet with a catalyst layer was produced. Subsequently, a solid polymer electrolyte membrane (thickness: 10 μm) was produced using a 10 mass % dispersion of "Nafion (registered trademark)" (manufactured by Sigma-Aldrich) and cut into an 80 mm × 80 mm size. The resulting solid polymer electrolyte membrane was sandwiched between two PTFE sheets with a catalyst layer and pressed at 130°C for 5 minutes while applying a pressure of 5 MPa using a flat plate press, thereby transferring the catalyst layer to the solid polymer electrolyte membrane. After pressing, the PTFE sheets were peeled off, and a solid polymer electrolyte membrane with a catalyst layer was produced.

[0085] Next, the catalyst layer-attached solid polymer electrolyte membrane was sandwiched between two gas diffusion electrode substrates cut to 50 mm × 50 mm, and pressed at 130°C for 5 minutes under a pressure of 3 MPa using a flat press to produce a membrane electrode assembly. The gas diffusion electrode substrate was positioned so that the surface having the microporous layer was in contact with the catalyst layer side.

[0086] The resulting membrane electrode assembly was assembled into a single cell for fuel cell evaluation, and the voltage was measured at various current densities. The evaluation was also performed by supplying unpressurized hydrogen to the anode side and unpressurized air to the cathode side.

[0087] The cell temperature was set to 65°C, and the supplied hydrogen and air were both humidified using a humidifying pot set to a temperature of 60°C, thereby keeping the humidity inside the cell at 80% and the utilization rates of oxygen in the hydrogen and air at 70% and 40%, respectively. Current density: 0.5 A / cm 2 or 2.0 A / cm 2 The output voltage was measured and used as an index of dry performance (moisture retention) and wet performance (drainage).

[0088] <Method for producing conductive porous substrate> Polyacrylonitrile carbon fiber "TORAYCA (registered trademark)" T300 (average fiber diameter: 7 μm) manufactured by Toray Industries, Inc. was cut to a length of 6 mm, dispersed in water, and continuously made into paper, which was then spray-coated with a 10% by mass aqueous solution of polyvinyl alcohol, dried, and made into a conductive porous substrate having a basis weight of 30 g / m. 2 A long paper sheet made of carbon fibers was obtained. The amount of polyvinyl alcohol attached was 15 parts by mass per 100 parts by mass of the paper sheet.

[0089] Next, a resin composition solution was prepared by mixing flake graphite (average particle size: 5 μm), phenolic resin (a mixture of resol-type phenolic resin and novolac-type phenolic resin in a mass ratio of 1:1), and methanol in a mass ratio of 5:10:85. The resin composition solution was then continuously applied to the paper body by spray coating so that the total amount of phenolic resin and flake graphite was 130 parts by mass per 100 parts by mass of carbon fiber in the conductive porous substrate, and dried at 100° C. for 5 minutes.

[0090] Next, the paper body with the resin composition attached was sandwiched between upper and lower hot plates in a press molding machine and subjected to heat compression treatment at 180 ° C for 5 minutes. Here, release paper was placed between the paper body and the hot plates to prevent the hot plates from adhering to the paper body substrate, and spacers were placed around the periphery of the upper and lower hot plates to adjust the thickness of the conductive porous substrate after heat compression. After that, it was heated to 2,400 ° C in a nitrogen atmosphere in a heating furnace and carbonized.

[0091] Furthermore, a water-repellent resin dispersion liquid obtained by mixing 5 parts by mass of FEP resin ("Neoflon (registered trademark)" FEP dispersion ND-110 (manufactured by Daikin Industries, Ltd.)) and 95 parts by mass of ion-exchanged water was spray-coated, and dried at 100°C for 5 minutes to form a film having a thickness of 150 μm at 0.15 MPa and a basis weight of 40 g / m. 2 Thus, a conductive porous substrate of 1000 .mu.m was obtained.

[0092] Example 1 A coating liquid for forming a microporous layer was prepared by mixing phenolic resin particles "Bellpearl (registered trademark)" C800 as a filler, powdered "Denka Black (registered trademark)" (manufactured by Denka Co., Ltd.) as carbon fine particles, the fluororesin PTFE as a water-repellent resin, "TRITON (registered trademark)" X-100 (manufactured by Nacalai Tesque, Inc.) as a dispersant, and purified water as a dispersion medium in the blending ratios shown in Table 1. Here, a dispersion of PTFE particles dispersed in water, "Polyflon (registered trademark)" D-210C (manufactured by Daikin Industries, Ltd.), was used as a supply source of PTFE. In addition, when preparing the coating liquid, a planetary mixer was used to disperse the raw materials so that the coating liquid composition was uniform.

[0093] The coating liquid for forming the microporous layer was applied to a conductive porous substrate prepared according to the above-described <Method for producing a conductive porous substrate> using a die coater, dried at 120°C for 10 minutes, and then heated at 380°C for 10 minutes to promote adhesion between the water-repellent resin and the carbon fine particles and to decompose and remove the dispersant, etc., to prepare a gas diffusion electrode substrate. Here, the basis weight of the microporous layer after heating was 12 g / m 2 The coating amount was adjusted so that the thickness of the obtained gas diffusion electrode substrate was 160 μm. The results of the evaluations according to the above <Calculation of filler content>, <Measurement of surface F / C ratio>, and <Measurement of surface O / C ratio> are shown in Table 1.

[0094] Next, the power generation performance was evaluated as described above in <Evaluation of power generation characteristics>. As shown in Table 1, the power generation performance was good.

[0095] Example 2 A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that phenolic resin particles "Bellpearl (registered trademark)" R700 were used as the filler, and various evaluations were carried out.

[0096] Example 3 A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that phenolic resin particles "Bellpearl (registered trademark)" C2000SR were used as the filler and the basis weight and thickness were as shown in Table 1, and various evaluations were performed.

[0097] Example 4 A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that phenolic resin particles "LPS (registered trademark)" 50C were used as the filler, and various evaluations were carried out.

[0098] Examples 5 and 6 Gas diffusion electrode substrates were prepared in the same manner as in Example 1, except that the coating liquid compositions for forming the microporous layer were as shown in Table 1, and various evaluations were carried out.

[0099] Example 7 A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that phenolic resin particles "LPS (registered trademark)" 50C were used as the filler and the basis weight and thickness were set as shown in Table 1, and various evaluations were performed.

[0100] Example 8 A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that phenolic resin particles "Bellpearl (registered trademark)" C2000SR were used as the filler, and various evaluations were carried out.

[0101] Example 9 A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that the basis weight and thickness shown in Table 2 were used, and various evaluations were carried out.

[0102] Examples 10 and 11 Gas diffusion electrode substrates were prepared in the same manner as in Example 1, except that the coating liquid composition, basis weight and thickness for forming the microporous layer were as shown in Table 2, and various evaluations were carried out.

[0103] Example 12 A gas diffusion electrode substrate was prepared and various evaluations were carried out in the same manner as in Example 1, except that the coating liquid composition, basis weight, and thickness for forming the microporous layer were as shown in Table 2. PMMA beads "Techpolymer (registered trademark)" MBX-40 (manufactured by Sekisui Plastics Co., Ltd., average particle size: 40 μm) were used as the pore-forming agent. The results of evaluation according to the above <Measurement of average pore diameter> and <Measurement of cross-sectional porosity> were as shown in Table 2.

[0104] Comparative Example 1 A gas diffusion electrode substrate was prepared in the same manner as in Example 1, except that phenolic resin particles "LPS (registered trademark)" 50A were used as the filler, and various evaluations were carried out. This gas diffusion electrode substrate had a low carbonization yield of the filler of 52%, reduced electrical conductivity, and reduced power generation characteristics on both the low current density side and the high current density side.

[0105] (Comparative Example 2) A gas diffusion electrode substrate was prepared and evaluated in the same manner as in Example 1, except that phenolic resin particles "Bellpearl (registered trademark)" R100 were used as the filler and the basis weight and thickness were set as shown in Table 3. This gas diffusion electrode substrate had a small average filler particle size of 1.4 μm, which resulted in reduced moisture retention and drainage, and reduced power generation characteristics on both the low current density side and the high current density side.

[0106] (Comparative Example 3) A gas diffusion electrode substrate was prepared in the same manner as in Example 1, except that phenolic resin particles "LPS (registered trademark)" 100C were used as the filler, and various evaluations were carried out. This gas diffusion electrode substrate had a large average filler particle size of 75 μm, which reduced the electrical conductivity and the power generation characteristics on both the low current density side and the high current density side.

[0107] Comparative Example 4 A gas diffusion electrode substrate was produced in the same manner as in Example 1, except that fibrous conductive potassium titanate "Dentol (registered trademark)" WK-200B (manufactured by Otsuka Chemical Co., Ltd., fiber length: 15 μm, carbonization yield after heating at 1,000° C. for 10 minutes: 95%) was used as the filler, and various evaluations were carried out. This gas diffusion electrode substrate had an average filler particle size of 0.6 μm, which reduced the electrical conductivity and the power generation characteristics on both the low current density side and the high current density side.

[0108] (Comparative Examples 5 and 6) Gas diffusion electrode substrates were prepared and evaluated in the same manner as in Example 1, except that the coating liquid composition for forming the microporous layer was as shown in Table 3. The gas diffusion electrode substrate of Comparative Example 5 had a low filler content of 4 mass%, which resulted in decreased moisture retention and drainage, and the power generation characteristics were decreased on both the low current density side and the high current density side. The gas diffusion electrode substrate of Comparative Example 6 had a high filler content of 48 mass%, which resulted in decreased conductivity, and the power generation characteristics were decreased on both the low current density side and the high current density side.

[0109] (Comparative Example 7) A gas diffusion electrode substrate was prepared and various evaluations were carried out in the same manner as in Example 1, except that no filler was added and the coating liquid composition for forming the microporous layer was as shown in Table 3. Because this gas diffusion electrode substrate did not contain a filler, both moisture retention and drainage were insufficient, and the power generation characteristics were reduced on both the low current density side and the high current density side.

[0110]

[0111]

[0112]

[0113] The gas diffusion electrode substrate of the present invention is excellent in moisture retention and drainage, and a fuel cell using the same has good power generation performance at both low and high current densities, making it useful.

Claims

1. A gas diffusion electrode substrate having a microporous layer on at least one surface of a conductive porous substrate, the microporous layer containing a filler having an average particle size of 5 to 60 μm and containing an organic polymer, the carbonization yield of which is 55% or more after heating at 1,000° C. for 10 minutes, the filler being contained in an amount of 10 to 45% by mass in 100% by mass of the microporous layer, and the arithmetic mean roughness Sa of the surface of the microporous layer being 5 to 20 μm.

2. The gas diffusion electrode substrate according to claim 1, wherein the F / C ratio of the surface of said microporous layer is 0.2 to 0.

6.

3. The gas diffusion electrode substrate according to claim 1 or 2, wherein the O / C ratio of the surface of said microporous layer is 0.1 or less.

4. The gas diffusion electrode substrate according to claim 1 or 2, wherein the average particle size of said filler is greater than the thickness of said microporous layer.

5. The gas diffusion electrode substrate according to claim 1 or 2, wherein the average particle size of said filler is 10 to 30 μm.

6. The gas diffusion electrode substrate according to claim 1 or 2, wherein the organic polymer is at least one resin selected from the group consisting of phenolic resins, acrylic resins, ester resins and ether resins.

7. The gas diffusion electrode substrate according to claim 1 or 2, wherein the organic polymer is a phenolic resin.

8. The gas diffusion electrode substrate according to claim 1 or 2, wherein the microporous layer has a thickness of 3 to 55 μm.

9. The gas diffusion electrode substrate according to claim 1 or 2, wherein the microporous layer has pores with an average diameter of 10 to 60 μm, and the area ratio of the pores formed in the entire cross section of the microporous layer is 10 to 50%.

10. The gas diffusion electrode substrate according to claim 1 or 2, wherein the conductive porous substrate is carbon paper.

11. A fuel cell comprising the gas diffusion electrode substrate according to claim 1 or 2.

Citation Information

Patent Citations

  • Gas diffusion electrode for polymer electrolyte fuel cell, membrane electrode assembly for polymer electrolyte fuel cell and its manufacturing method, and polymer electrolyte fuel cell

    JP2006331717A

  • Gas diffusion layer and production method thereof

    JP2016195060A

  • Manufacture of carbonaceous preformed body and electrode substrate

    JP1995057741A

  • Production of carbonaceous powder molding material, production of carbonaceous powder molded article, and carbonaceous powder molded article

    JP2001030241A

  • Gas diffusion medium and fuel cell

    JP2007273464A