Biaxially oriented polyarylene sulfide film, method for producing biaxially oriented polyarylene sulfide film, electrolyte membrane-reinforcing member, fuel cell, and water electrolysis device

A biaxially oriented polyarylene sulfide film with tailored properties addresses the mechanical strength issues of solid polymer membranes at high temperatures, offering enhanced durability and stability for fuel cells and water electrolysis devices.

WO2024203383A1PCT designated stage expired Publication Date: 2024-10-03TORAY INDUSTRIES INC

Patent Information

Application Number
PCT/JP2024/009959
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-14
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current solid polymer membranes used in fuel cells and water electrolysis devices exhibit low mechanical strength and are prone to breakage and distortion at operating temperatures exceeding 100°C due to thermal shrinkage and deformation.

Method used

A biaxially oriented polyarylene sulfide film with specific elastic modulus ratios, heat shrinkage rates, and glass transition temperatures is developed, combined with a method of production involving melt-extrusion, stretching, and heat setting to create a reinforcing member for electrolyte membranes, enhancing durability and dimensional stability.

Benefits of technology

The biaxially oriented polyarylene sulfide film provides excellent durability and dimensional stability, suitable for high-temperature applications in fuel cells, water electrolyzers, and other electronic components, maintaining structural integrity and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing a polyarylene sulfide film which is unlikely to break and in which wrinkles and distortion are unlikely to occur, in a temperature range exceeding 100°C. A solution to the problem is a biaxially oriented polyarylene sulfide film which contains a polyarylene sulfide (PAS) resin as the main component and in which the ratio YA130 / YA25 between the elastic modulus (YA25) at 25°C in a direction orthogonal to a main orientation axis and the elastic modulus (YA130) measured at 130°C in the direction orthogonal to the main orientation axis is 0.25-0.80, and the 130°C-thermal shrinkage ratio in said direction is -1.2% to 1.2%.
Need to check novelty before this filing date? Find Prior Art

Description

Biaxially oriented polyarylene sulfide film, method for producing biaxially oriented polyarylene sulfide film, electrolyte membrane reinforcing member, fuel cell, and water electrolysis device

[0001] The present invention relates to a biaxially oriented polyarylene sulfide film, a method for producing a biaxially oriented polyarylene sulfide film, an electrolyte membrane reinforcing member, a fuel cell, and a water electrolysis device.

[0002] In recent years, efforts to achieve carbon neutrality have led to the development of fuel cells that use hydrogen as energy and water electrolysis equipment for generating hydrogen. Among these, polymer electrolyte fuel cells have a relatively low reaction temperature and high energy density, and are therefore expected to have a wide range of applications as power generation equipment for relatively small-scale distributed power generation facilities and mobile vehicles such as automobiles and ships.

[0003] The solid polymer membranes currently being considered for use in polymer electrolyte fuel cells are proton-conductive ion exchange membranes with a thickness of approximately 50 to 100 μm, and in particular, cation exchange membranes made of perfluorosulfonic acid containing sulfonic acid groups, such as "Nafion" (registered trademark), are being widely considered.

[0004] Recently, there has been a demand for thinner solid polymer membranes, but the low mechanical strength of solid polymer membranes has become a problem in terms of productivity of fuel cells and water electrolysis devices.

[0005] Patent Document 1 describes the use of a reinforcing member made of polyethylene naphthalate at the periphery of a fuel cell. Patent Document 2 also discloses a reinforcing member for a solid electrolyte membrane made of polyphenylene sulfide (hereinafter sometimes abbreviated as PPS) resin with reduced metal element-containing components. Patent Document 3 also discloses a reinforcing member for an electrolyte membrane made of a laminate with a fluororesin. Patent Document 4 also discloses a technology for reducing the thermal shrinkage of PPS film.

[0006] Japanese Patent Application Publication No. 2007-103170 Japanese Patent Application Publication No. 2016-219136 Japanese Patent Application Publication No. 2013-110048 International Publication No. 2021 / 045076

[0007] In recent years, with the expansion of fuel cells to large mobile objects, development has been carried out to increase the output and extend the life of fuel cells themselves, and fuel cells with operating temperatures exceeding 100°C, higher than the conventional operating temperatures of 50 to 100°C, are being developed. Among these materials, the reinforcing members are also required to have long-term durability at higher temperatures.

[0008] However, it was found that even the technology described in the above patent documents has problems such as the material being prone to breakage and wrinkles and distortions caused by shrinkage deformation due to thermal movement when used as an electrolyte membrane reinforcing member in an operating temperature range exceeding 100°C.

[0009] The object of the present invention is to solve the above-mentioned problems, that is, to provide a polyarylene sulfide film that is resistant to breaking and wrinkles and distortions at temperatures exceeding 100°C.

[0010] A preferred embodiment of the present invention is as follows: (1) A film having a polyarylene sulfide (PAS) resin as a main component, and having an elastic modulus (Y A25 ) and the elastic modulus (Y A130 ) ratio Y A130 / Y A25 (1) A biaxially oriented polyarylene sulfide film having a modulus of elasticity (Y) of 0.25 or more and 0.80 or less, and a 130°C heat shrinkage rate in the same direction of the film of -1.2% or more and 1.2% or less. (2) A biaxially oriented polyarylene sulfide film having a glass transition temperature (Tg) of 110°C or more and 140°C or less as determined by temperature-modulated differential scanning calorimetry (temperature-modulated DSC), and having a mobile amorphous content of 5% or more and 25% or less relative to the entire film. (3) A biaxially oriented polyarylene sulfide film having a modulus of elasticity (Y) of 0.25 or more and 0.80 or less at 25°C in the main orientation axis direction of the film of the present invention. B25 ) and the elastic modulus (Y B130 ) ratio Y B130 / Y B25(4) A biaxially oriented polyarylene sulfide film according to any one of (1) to (3), having a modulus of elasticity measured at 130°C of 1.0 GPa or more in both the main orientation axis direction and the direction perpendicular to the main orientation axis. (5) A biaxially oriented polyarylene sulfide film according to any one of (1) to (4), having a resonance parameter (Q value) determined by microwave orientation measurement of 4,600 or more and 5,000 or less. (6) A biaxially oriented polyarylene sulfide film according to any one of (1) to (5), having a weight average molecular weight (Mw) of 60,000 or more and 150,000 or less. (7) A biaxially oriented polyarylene sulfide film having a density of 1.3450 g / cm 3 More than 1.3550g / cm 3(8) The biaxially oriented polyarylene sulfide film according to any one of (1) to (7), wherein the biaxially oriented polyarylene sulfide film has a minute endothermic peak temperature (Tmeta) (°C) determined by differential scanning calorimetry (DSC) of (melting point (Tm) of the film - 100)°C or higher and (Tm - 20)°C or lower. (9) A method for producing a biaxially oriented polyarylene sulfide film according to any one of (1) to (8), comprising melt-extruding a polyarylene sulfide resin composition, cooling and solidifying the composition, stretching the film in the running direction (MD stretching), and then stretching the film in the width direction (TD stretching) while holding the film with clips to form a biaxially oriented film, followed by successively carrying out a heat-setting step in an initial stage at a heat-setting temperature (Ths1) of 150°C or higher and 230°C or lower, and a heat-setting step in a final stage at a heat-setting temperature (Ths2) of 1 or higher and 265°C or lower. (10) An electrolyte membrane reinforcing member using the biaxially oriented polyarylene sulfide film according to any one of (1) to (8). (11) An electrolyte membrane reinforcing member according to (10), comprising a component having at least a biaxially oriented polyarylene sulfide film, an organic resin layer, and a biaxially oriented polyarylene sulfide film, in this order. (12) An electrolyte membrane reinforcing member according to (10) or (11), in which the thermal expansion coefficient measured in the temperature range of 100°C to 130°C in the direction in which the thermal expansion coefficient is highest when measured in the temperature range of 100°C to 130°C is 40 ppm / °C or more and 65 ppm / °C or less. Measurement method: The thermal expansion coefficient is measured in the temperature range of 100°C to 130°C, with the long side direction and / or the short side direction of the rectangle being set as 0°, and the value in the direction in which the thermal expansion coefficient is highest is calculated. (13) A fuel cell having the electrolyte membrane reinforcing member according to any one of (10) to (12). (14) A water electrolysis device having the electrolyte membrane reinforcing member according to any one of (10) to (12).

[0011] The present invention can provide a polyarylene sulfide film excellent in durability and dimensional stability. The biaxially oriented polyarylene sulfide film of the present invention can be suitably used for automobiles, various parts of electric and electronic materials, circuit substrates, heat-resistant tape substrates, films for toner stirrers for printing, release films, and particularly for electrolyte membrane reinforcing members and film capacitors for fuel cells and water electrolysis devices, which require durability and dimensional stability, and battery current collector foil substrates for lithium ion secondary batteries and the like.

[0012] FIG. 1 is a schematic oblique overhead view showing an example of the configuration of an electrolyte membrane reinforced with a polyarylene sulfide film and an organic resin layer.

[0013] The present invention will be described below.

[0014] A preferred embodiment of the present invention is a film having a polyarylene sulfide (PAS) resin as a main component, and having an elastic modulus (Y A25 ) and the elastic modulus (Y A130 ) ratio Y A130 / Y A25 and a biaxially oriented polyarylene sulfide film having a 130°C heat shrinkage rate in the same direction of the axial direction of the film of from -1.2% to 1.2%.

[0015] In the present invention, the biaxially oriented polyarylene sulfide film is preferably a biaxially oriented film containing polyarylene sulfide (hereinafter, PAS) resin as a main component. The film can be obtained by melt-molding a resin composition containing PAS resin as a main component into a sheet, biaxially stretching the sheet, and heat-treating the sheet.

[0016] In the present invention, "having PAS resin as the main constituent" means that the film contains 80% by mass or more of PAS resin. Furthermore, it preferably contains 90% by mass or more, and more preferably 95% by mass or more. If the PAS resin content is less than 80% by mass, the heat resistance, dimensional stability, electrical properties, and mechanical properties, which are characteristic of PAS films, may be impaired. Furthermore, if a large amount of components other than PAS resin is contained, peeling, cracks, voids, etc. may occur at the interface with the PAS resin, accelerating deterioration and resulting in poor durability and barrier properties. Furthermore, in the present invention, recycled PAS resin raw materials may also be used within a range that does not impair the effects of the invention.

[0017] The PAS resin used in the present invention is a copolymer having a repeating unit of -(Ar-S)-, where Ar includes units represented by the following formulas (A) to (K).

[0018]

[0019] (R1 and R2 are substituents selected from hydrogen, an alkyl group, an alkoxy group, and a halogen group, and R1 and R2 may be the same or different.) The repeating unit is preferably a p-arylene sulfide unit represented by the above formula (A), and representative examples thereof include polyphenylene sulfide, polysulfone, polyethersulfone, polyphenylene sulfide sulfone, and polyphenylene sulfide ketone. From the viewpoints of film properties and economic efficiency, a particularly preferred p-arylene sulfide unit is a p-phenylene sulfide unit.

[0020] The PAS resin used in the present invention preferably comprises p-phenylene sulfide units represented by the following structural formula as the main structural unit, in an amount of 80 mol % to 99.9 mol % of all repeating units. More preferably, it is 90 mol % to 99.9 mol %, and most preferably, it is 95 mol % to 99.9 mol %. By achieving the above composition, excellent heat resistance and chemical resistance can be achieved. If the p-phenylene sulfide units account for less than 80 mol % of all repeating units, durability may be impaired due to reduced crystallinity and reduced degree of orientation.

[0021]

[0022] Furthermore, it can also be copolymerized with copolymerization units in an amount of 0.01 mol % to 20 mol % of the repeating units.

[0023] Preferred copolymerized units are

[0024]

[0025]

[0026]

[0027] (wherein X is alkylene, CO, SO 2 Indicates the unit.)

[0028]

[0029]

[0030] (wherein R represents an alkyl, nitro, phenylene or alkoxy group).

[0031] The mode of copolymerization is not particularly limited, but a random copolymer is preferred.

[0032] The weight-average molecular weight of the biaxially oriented polyarylene sulfide film of the present invention is preferably 60,000 or more, more preferably 65,000 or more, and even more preferably 70,000 or more. A weight-average molecular weight of 60,000 or more tends to provide sufficient mechanical strength as a biaxially oriented film, and thickness unevenness can also be reduced. Furthermore, a preferred range for the weight-average molecular weight is 150,000 or less, more preferably 120,000 or less, and even more preferably 100,000 or less. By keeping the weight-average molecular weight within this range, the tensile elongation and durability of the biaxially oriented film can be improved. The weight-average molecular weight is a value measured using a gel permeation chromatograph (hereinafter sometimes abbreviated as GPC) equipped with a differential refractive index detector. More specifically, the value was calculated using GPC with a column temperature of 210°C and a detector temperature of 210°C, 1-chloronaphthalene as the eluent, at a flow rate of 1.0 mL / min, using a 1-chloronaphthalene solution with a PAS concentration of 0.1% by mass, and polystyrene as the standard substance.

[0033] The biaxially oriented polyarylene sulfide film of the present invention has a modulus of elasticity at 25°C (Y A25 ) and the elastic modulus (Y A130 ) ratio Y A130 / Y A25is preferably 0.25 or more and 0.80 or less. The elastic modulus ratio indicates the ratio of the elastic modulus at 130 ° C to the elastic modulus at 25 ° C, and a larger elastic modulus ratio indicates the formation of a strong thermostable structure that can suppress relaxation up to 130 ° C. By having this strong thermostable structure, when used as an electrolyte membrane reinforcing member for a fuel cell, the rigidity as a reinforcing member can be maintained in an environment where temperatures exceeding 100 ° C are repeatedly used, and deformation of the electrolyte membrane can be suppressed in the environment. If the ratio of the elastic modulus in the direction perpendicular to the main orientation axis is less than 0.25, a strong thermostable structure cannot be formed, and durability may be poor. If the ratio of the elastic modulus in the direction perpendicular to the main orientation axis exceeds 0.80, high orientation occurs too much, and the tensile elongation of the film decreases, which may cause breakage due to tension during processing in the coating process or punching process, resulting in a poor yield. The ratio of the elastic modulus in the direction perpendicular to the main orientation axis is more preferably 0.27 or more, even more preferably 0.30 or more, and particularly preferably 0.33 or more. The ratio of the elastic modulus in the direction perpendicular to the main orientation axis is more preferably 0.75 or less, even more preferably 0.70 or less.

[0034] In the present invention, the main orientation axis direction is determined by measuring the modulus of elasticity at 25°C while changing the direction in the film plane from -90° to 90° in 10° increments, with any direction being set to 0°, and the direction with the highest modulus of elasticity is determined to be the main orientation axis direction of the film.

[0035] In the present invention, the direction perpendicular to the main orientation axis is the point in the film plane where orientation is most difficult to form and strength is weakest. Therefore, when the elastic modulus in the perpendicular direction satisfies the above-mentioned elastic modulus ratio, the film will have a stable structure in the film plane.

[0036] Regarding the ratio of the elastic modulus in the direction perpendicular to the main orientation axis of the present invention, among the film-forming conditions described below, the elastic modulus ratio tends to increase when the longitudinal stretching ratio is increased. Also, the elastic modulus ratio tends to decrease when the heat setting temperature is increased. The elastic modulus is determined by the method using a tensile tester described in the examples.

[0037] The biaxially oriented polyarylene sulfide film of the present invention has a modulus of elasticity in the direction of the main orientation axis (Y B25) and the modulus of elasticity in the direction of the main orientation axis measured at 130°C (Y B130 ) ratio Y B130 / Y B25 Preferably, the ratio of the modulus of elasticity in the main orientation axis direction is 0.25 or more and 0.80 or less. Having the ratio of the modulus of elasticity in the above range indicates that a strong, thermostable structure is formed in the film plane, and that the structure is stable even at operating temperatures exceeding 100°C when used as a reinforcing member for an electrolyte membrane. If the modulus of elasticity in the main orientation axis direction is less than 0.25, a strong, thermostable structure cannot be formed, and durability may be poor. If the ratio of the modulus of elasticity exceeds 0.80, high orientation occurs too much, resulting in a decrease in the tensile elongation of the film, which may cause breakage due to tension during processing in the coating or punching process, resulting in a decrease in yield. The ratio of the modulus of elasticity in the main orientation axis direction is more preferably 0.27 or more, even more preferably 0.30 or more, and particularly preferably 0.33 or more. Furthermore, the ratio of the modulus of elasticity in the main orientation axis direction is more preferably 0.75 or less, even more preferably 0.70 or less. The ratio of the modulus of elasticity in the main orientation axis direction can be controlled by the film formation conditions described below.

[0038] The biaxially oriented polyarylene sulfide film of the present invention has an elastic modulus measured at 130° C. in the direction of the main orientation axis (Y B130 ) and the direction perpendicular to the main alignment axis (Y A130 ) are preferably 1.0 GPa or more. If the elastic modulus measured at 130°C is within the above range, it indicates that a large amount of a strong thermally stable structure is formed even at operating temperatures exceeding 130°C, and when used as a reinforcing member for an electrolyte membrane, deformation under the operating environmental pressure can be suppressed and thermal stability can be maintained at the operating environmental temperature, improving durability, which is preferable. If the elastic modulus measured at 130°C is less than 1.0 GPa, the rigidity is low and deformation including the electrolyte membrane may occur in an environment of operating temperatures exceeding 100°C, or thermal stability may be reduced, resulting in a deterioration in durability. The elastic modulus measured at 130°C is Y B130 and Y A130In either case, the elastic modulus measured at 130°C is more preferably 1.2 GPa or more, and even more preferably 1.4 GPa or more. A preferred range for the elastic modulus measured at 130°C is 4.0 GPa or less, and more preferably 3.5 GPa or less. Within this range, the orientation does not increase too much, and the heat shrinkage of the film can be kept within a preferred range. Among the film-forming conditions described below, increasing the draw ratio tends to increase the elastic modulus measured at 130°C, while increasing the heat setting temperature tends to decrease the elastic modulus measured at 130°C.

[0039] The biaxially oriented polyarylene sulfide film of the present invention has an elastic modulus measured at 25° C. in the direction of the main orientation axis (Y B25 ) and the direction perpendicular to the main alignment axis (Y A25 ) are preferably 3.0 GPa or more. When the elastic modulus measured at 25°C is within the above range, it indicates that the molecular chains are aligned and the film strength is sufficient, and when used as a reinforcing member for an electrolyte membrane, deformation under the operating environmental pressure can be suppressed and durability can be improved, which is preferable. When the elastic modulus measured at 25°C is less than 3.0 GPa, the molecular chains are not aligned sufficiently and the durability of the film may be reduced. The elastic modulus measured at 25°C is Y B25 and Y A25 In either case, the elastic modulus measured at 25°C is more preferably 3.3 GPa or more, and even more preferably 3.5 GPa or more. In addition, a preferable range for the elastic modulus measured at 25°C is 5.0 GPa or less. Within this range, the orientation does not increase too much, and the heat shrinkage rate of the film can be set within a preferable range. Among the film-forming conditions described below, increasing the stretching ratio tends to increase the elastic modulus measured at 25°C.

[0040] The biaxially oriented polyarylene sulfide film of the present invention preferably has a 130°C heat shrinkage measured in a direction perpendicular to the main orientation axis of from -1.2% to 1.2%. When the heat shrinkage in the direction perpendicular to the main orientation axis is within the above range, dimensional change during processing and in operating temperature environments exceeding 100°C is reduced, and internal residual stress is less likely to occur, resulting in improved dimensional stability and durability. When processed using a roll-to-roll process, if the direction perpendicular to the main orientation axis is the width direction of the film, no tension is applied in the width direction, and dimensional change due to heat shrinkage at the processing temperature may become dominant. Therefore, it is preferable to set the 130°C heat shrinkage in the direction perpendicular to the main orientation axis within the above range. A 130°C heat shrinkage in the direction perpendicular to the main orientation axis of less than -1.2% indicates expansion exceeding 1.2%, which may result in deterioration of dimensional stability or generation of residual stress in the usage environment, deforming the electrolyte membrane and reducing durability. If the 130°C heat shrinkage in the direction perpendicular to the main orientation axis exceeds 1.2%, deformation during processing may become significant, resulting in poor dimensional stability. The 130°C heat shrinkage in the direction perpendicular to the main orientation axis is more preferably -1.0% or more, and even more preferably -0.8% or more. The 130°C heat shrinkage in the direction perpendicular to the main orientation axis is more preferably 1.0% or less, and even more preferably 0.8% or less. Among the film-forming conditions described below, increasing the relaxation rate in the relaxation treatment after heat setting tends to decrease the 130°C heat shrinkage in that direction. The heat shrinkage is determined by the method described in the Examples.

[0041] The biaxially oriented polyarylene sulfide film of the present invention preferably has a 130°C heat shrinkage rate in the main orientation axis direction of -1.2% or more and 1.2% or less. When the 130°C heat shrinkage rate is within the above range, dimensional change during processing is small, thereby improving dimensional stability. When the 130°C heat shrinkage rate in the main orientation axis direction is less than -1.2%, expansion exceeds 1.2%, which may result in deterioration of dimensional stability or generation of residual stress in the usage environment, deforming the electrolyte membrane and reducing durability. When the 130°C heat shrinkage rate in the main orientation axis direction is more than 1.2%, deformation during processing may become significant, resulting in deterioration of dimensional stability. The 130°C heat shrinkage rate in the main orientation axis direction is more preferably -1.0% or more, and even more preferably -0.8% or more. Furthermore, the 130°C heat shrinkage rate in the main orientation axis direction is more preferably 1.0% or less, and even more preferably 0.8% or less. Under the film-forming conditions described below, increasing the longitudinal stretching ratio tends to increase the 130°C heat shrinkage in that direction, and increasing the heat setting temperature tends to decrease the 130°C heat shrinkage in that direction.

[0042] The biaxially oriented polyarylene sulfide film of the present invention preferably has a glass transition temperature (Tg) determined by temperature-modulated differential scanning calorimetry (temperature-modulated DSC) of 110°C or higher and 140°C or lower. Temperature-modulated DSC is a technique that can measure the glass transition temperature of a biaxially oriented film, which is difficult to determine by DSC (see SENI GAKKAISHI (SENSI TO KOGYO) Vol. 65, No. 11 (2009)). The specific measurement method is the method described in the Examples. It is preferable that the Tg determined by temperature-modulated DSC is within the above range, since rigidity can be maintained even at operating temperatures exceeding 100°C. If the Tg determined by temperature-modulated DSC is lower than 110°C, molecular chain orientation is insufficient, which may result in poor durability in environments with operating temperatures exceeding 100°C. If the Tg determined by temperature-modulated DSC exceeds 140°C, it indicates that the orientation of molecular chains is extremely high, and the tensile elongation of the film decreases, and breakage or the like may occur due to the tension during processing in the coating process or punching process, resulting in a deterioration in yield. The Tg determined by temperature-modulated DSC is more preferably 115°C or higher, and even more preferably 118°C or higher. Furthermore, the Tg determined by temperature-modulated DSC is more preferably 135°C or lower. Regarding the Tg determined by temperature-modulated DSC, among the film-forming conditions described below, increasing the draw ratio tends to increase the Tg. Furthermore, increasing the heat setting temperature tends to decrease the Tg.

[0043] The biaxially oriented polyarylene sulfide film of the present invention preferably has a mobile amorphous content of 5% or more and 25% or less relative to the entire film. The film primarily contains mobile amorphous components, rigid amorphous components with their ends fixed to crystalline components, and crystalline components. Having a mobile amorphous content within the above range is preferable because it indicates reduced molecular chain movement at temperatures above 100°C, thereby improving durability. If the mobile amorphous content is less than 5%, the film will contain a large amount of crystals and rigid amorphous components, resulting in a loss of toughness and film deterioration or cracking due to temperature cycles or vibration in the usage environment, which may affect durability. If the mobile amorphous content exceeds 25%, it indicates a large amount of amorphous content that moves at temperatures above 100°C, which may lead to deterioration of the amorphous portion in the usage environment, resulting in a decrease in durability. The mobile amorphous content of the entire film is more preferably 12% or more. Furthermore, the mobile amorphous content of the entire film is more preferably 23% or less, and even more preferably 20% or less. The specific method for measuring the mobile amorphous content of the entire film is the method described in the Examples. Among the film-forming conditions described below, lowering the heat setting temperature tends to decrease the mobile amorphous amount relative to the entire film, but below a specific heat setting temperature, the mobile amorphous amount relative to the entire film tends to increase. Increasing the stretch ratio tends to decrease the mobile amorphous amount relative to the entire film. Increasing the temperature of the relaxation treatment tends to increase the mobile amorphous amount relative to the entire film. Furthermore, increasing the relaxation rate of the relaxation treatment tends to decrease the mobile amorphous amount relative to the entire film. Furthermore, performing the relaxation treatment in stages tends to decrease the mobile amorphous amount relative to the entire film.

[0044] The biaxially oriented polyarylene sulfide film of the present invention preferably has a resonance parameter (Q value) determined by microwave orientation measurement of 4600 or more and 5200 or less. In the present invention, the Q value is measured using a molecular orientation meter (MOA-6015, manufactured by Oji Scientific Instruments) and is the average value of 10 measurements of the parameter (Q value) indicating the sharpness of the resonance of the biaxially oriented polyarylene sulfide film, and the detailed measurement method is as described in the Examples. The Q value increases as the orientation of the molecular chains in the film increases. A resonance parameter (Q value) within the above range is preferable because it indicates that the molecular chains are sufficiently oriented, suppressing molecular motion and improving durability. A resonance parameter (Q value) of less than 4600 is insufficient, and the mobility of amorphous portions may remain in the usage environment of a fuel cell or water electrolysis device, resulting in poor durability. If the resonance parameter (Q value) exceeds 5200, it indicates that the molecular chains are extremely oriented, and the tensile elongation of the film decreases, which can cause breakage due to the tension during processing in the coating process or punching process, resulting in a decrease in yield. The resonance parameter (Q value) is more preferably 4700 or more, even more preferably 4800 or more, and particularly preferably 4850 or more. The resonance parameter (Q value) is more preferably 5000 or less. Among the film-forming conditions described below, the resonance parameter (Q value) tends to increase when the stretching ratio is increased, and the resonance parameter (Q value) tends to decrease when the stretching temperature is increased.

[0045] From the viewpoint of further improving thermal stability, the biaxially oriented polyarylene sulfide film of the present invention preferably has a minute endothermic peak temperature (T-meta) (°C) determined by differential scanning calorimetry (DSC) of (the melting point (Tm) of the film - 100)°C or higher and (Tm - 20)°C or lower. The minute endothermic peak temperature (T-meta) in the present invention indicates that the film has undergone thermal history. When the T-meta is within the above range, orientation relaxation during the film formation process is suppressed, and a film with excellent durability can be obtained that is likely to form a thermally stable structure required for operating temperatures exceeding 100°C. Furthermore, when the T-meta is less than (the melting point (Tm) of the film - 100)°C, the thermal history is low and thermal dimensional change is large, which may result in poor dimensional stability. When the T-meta exceeds (Tm - 20), orientation relaxation proceeds, which may result in poor durability at operating temperatures exceeding 100°C. T-meta is more preferably 200°C or higher but lower than 240°C, and even more preferably 210°C or higher but lower than 235°C. T-meta can be controlled by the heat setting temperature. T-meta varies depending on the film forming machine and film formation speed, but generally increases with increasing heat setting temperature.

[0046] In order to further improve durability, the biaxially oriented polyarylene sulfide film of the present invention has a film density of 1.3450 g / cm 3 More than 1.3550g / cm 3 When the density is within the above range, the crystallinity is increased while maintaining the oriented structure, and a film with excellent durability can be obtained that is likely to form a thermally stable structure required for operating temperatures exceeding 100°C. 3 If the density is less than 1.3550 g / cm, the crystallization may not be advanced, resulting in poor durability and dimensional stability. 3 If the density exceeds 1.3480 g / cm, the crystallinity becomes too high, which may result in a decrease in orientation and poor durability. 3 The film density is more preferably 1.3520 g / cm 3 The density can be evaluated by the method described below. Among the film-forming conditions described below, increasing the heat setting temperature tends to increase the density.

[0047] The biaxially oriented polyarylene sulfide film of the present invention can be obtained by biaxial stretching. As the biaxial stretching method, any of an inflation simultaneous biaxial stretching method, a stenter simultaneous biaxial stretching method, and a stenter sequential biaxial stretching method can be used. Among these, it is preferable to employ a stenter sequential biaxial stretching method in terms of controlling the film formation stability, film durability, and dimensional stability.

[0048] The thickness of the biaxially oriented polyarylene sulfide film of the present invention is not particularly limited, but from the viewpoint of film formability, a film thickness of 0.5 μm or more and 300 μm or less is preferred. For electrolyte membrane reinforcing members, from the viewpoint of handleability, a film thickness of 10 to 150 μm is more preferred, 20 to 125 μm is even more preferred, and 35 to 100 μm is particularly preferred. Furthermore, for applications as a film capacitor or a battery current collector foil substrate for lithium ion secondary batteries, a film thickness of 0.5 μm or more and 15 μm or less is preferred from the viewpoint of a balance between durability and thinness, and the thickness is more preferably 9.0 μm or less, even more preferably 6.0 μm or less, and most preferably 4.0 μm or less. Film thickness can be measured with a micrometer, and details will be described later.

[0049] The method for producing the biaxially oriented polyarylene sulfide film of the present invention will be explained using an example of a film production method in which polyphenylene sulfide resin (hereinafter sometimes abbreviated as PPS resin) is used as the polyarylene sulfide resin, but the present invention is not limited to this example.

[0050] Sodium sulfide and p-dichlorobenzene are blended and reacted under high temperature and pressure in an amide-based polar solvent such as N-methyl-2-pyrrolidone (NMP). If necessary, copolymerization components such as m-dichlorobenzene or trihalobenzene can also be added. Caustic potassium or an alkali metal carboxylate is added as a polymerization degree modifier, and the polymerization reaction is carried out at 230-290°C. After polymerization, the polymer is cooled, and the polymer is made into a water slurry and filtered through a filter to obtain a wet granular polymer. An amide-based polar solvent is added to the granular polymer, followed by stirring and washing at a temperature of 30-100°C, washing several times with ion-exchanged water at 30-80°C, washing several times with a metal salt aqueous solution such as calcium acetate aqueous solution, and drying to obtain a polyphenylene sulfide granular polymer. This granular polymer is fed into a vented extruder and melt-extruded into strands. It is then cooled with water at 25°C and cut into chips to produce PPS chips.

[0051] The resulting PPS granular polymer is preliminarily melt-kneaded (pelletized) with polyphenylsulfone resin under the above-mentioned conditions to prepare a master chip.

[0052] In the present invention, it is preferable to first mix PPS chips, which have been dried under reduced pressure at 180°C for 3 hours as needed, with a masterbatch in a predetermined ratio, feed the mixture into a full-flight single-screw extruder with the melting zone set at 300 to 350°C, pass the mixture through a filter, and then extrude the mixture from a T-die nozzle.Then, while applying a static charge to a cooling drum having a surface temperature of 20 to 70°C, the mixture is rapidly cooled and solidified, thereby obtaining an unstretched film in a substantially unoriented state.

[0053] Next, the unstretched film obtained above is biaxially stretched using a sequential biaxial stretching machine or a simultaneous biaxial stretching machine in a temperature range equal to or higher than the glass transition temperature (Tg) of the polyarylene sulfide resin, followed by a one-stage or multi-stage heat treatment at a temperature range of 150 to 280°C to obtain a biaxially oriented film. As the stretching method, a sequential biaxial stretching method (a stretching method combining stretching in one direction at a time, such as a method in which stretching in the longitudinal direction is performed followed by stretching in the width direction), a simultaneous biaxial stretching method (a method in which stretching in the longitudinal direction and then the width direction is performed simultaneously), or a combination thereof can be used. Here, a sequential biaxial stretching method in which stretching in the longitudinal direction is performed first and then in the width direction is illustrated as an example.

[0054] The unstretched film is heated by a group of heating rolls and stretched in the longitudinal (MD) direction to a magnification of 2.5 times or more, more preferably 3.0 times or more, even more preferably 3.3 times or more, particularly preferably 3.5 times or more, and most preferably 3.8 times or more in one or two or more stages (MD stretching). By maintaining the MD stretching within the above range and aligning the molecular chains in the longitudinal direction, stress can be uniformly propagated during the transverse (TD) stretching described below, thereby enhancing amorphous orientation in the transverse direction and improving durability and dimensional stability. Furthermore, a preferred range for the MD stretching ratio is 5.0 times or less, more preferably 4.8 times or less, even more preferably 4.5 times or less, and particularly preferably 4.3 times or less. If this range is exceeded, excessive orientation in one direction during MD stretching may result in poor film formability during transverse stretching. The stretching temperature is Tg to Tcc (heat-up crystallization peak temperature), preferably in the range of (Tg + 5) to (Tcc - 5) °C. Thereafter, the sheet is cooled with a group of cooling rolls at 20 to 50°C.

[0055] As a method for stretching in the width direction (TD direction) following MD stretching, for example, a method using a tenter is common. Both ends of the film are held with clips and introduced into the tenter, where TD stretching in the width direction is performed. The stretching temperature for TD stretching is preferably 90°C or higher and 200°C or lower, more preferably 90°C or higher, and even more preferably 95°C or higher. The TD stretching temperature is more preferably 180°C or lower, and even more preferably 160°C or lower. From the viewpoint of the flatness of the film, the stretching ratio for TD stretching is preferably 1.2 times or higher and 4.0 times or lower. The TD stretching ratio is more preferably 3.0 times or higher, even more preferably 3.3 times or higher, and the TD stretching ratio is more preferably 3.8 times or lower, even more preferably 3.6 times or lower.

[0056] In this case, the ratio of the stretching magnification of the film in MD to TD (stretching magnification ratio = MD / TD) is preferably greater than 1.0, more preferably 1.1 or more, and even more preferably 1.2 or more. By setting the ratio within the above range, an oriented structure can be effectively formed by TD stretching due to the structure formed by MD stretching.

[0057] Next, in the present invention, it is preferable to perform heat setting after stretching in two or more steps at different temperatures, and to perform the setting in stages. It is preferable to perform heat setting continuously. In the present invention, "continuously" means performing heat setting in stages without a cooling step in between. The above-mentioned heat setting treatment is preferable because it can suppress rapid orientation relaxation due to heat setting, form a strong heat-stable structure, and improve durability. The heat setting temperature is preferably a heat setting temperature Ths1 (°C) of the first step of 150°C or higher and 230°C or lower, and a heat setting temperature Ths2 (°C) of the final step of 150°C or higher and 265°C or lower. The "first step" in the present invention refers to the steps excluding the final step of a heat setting treatment process performed in two or more steps. For example, if a heat setting treatment process consists of three steps, the first and second steps correspond to the first step, and the third step corresponds to the final step. Setting the heat setting temperature in the first stage (hereinafter sometimes abbreviated as Ths1) within the above range allows the structure to be fixed at a temperature at which crystallization proceeds while orientation relaxation is unlikely to proceed, and this is a preferred embodiment because orientation relaxation can be suppressed in the subsequent heat setting treatment. Specifically, as described above, Ths1 is preferably 150°C or higher and 230°C or lower, and Ths1 is more preferably 150°C or higher, and even more preferably 160°C or higher. Furthermore, Ths1 is more preferably 200°C or lower, and even more preferably 190°C or lower. Setting the heat setting temperature in the final stage (hereinafter sometimes abbreviated as Ths2) to Ths1 or higher and 265°C or lower is preferable because stretching strain can be removed without relaxing the crystals and orientation structure formed in the previous stage, improving durability and dimensional stability. Ths2 is more preferably 200°C or higher, and even more preferably 215°C or higher. Furthermore, Ths2 is more preferably 245°C or less, even more preferably less than 240°C, and most preferably 235°C or less. When the heat setting treatment of the present invention is carried out in three or more stages, it is preferable that the heat setting temperature is gradually increased from the first stage to the second stage and the third stage within the above-mentioned preferred temperature ranges of Ths1 and Ths2. The heat setting time for each stage of the preceding heat setting is preferably 1 second to 1000 seconds, more preferably 1 second to 60 seconds, and even more preferably 1 second to 30 seconds.The time for the final heat setting is preferably 1 to 1000 seconds, more preferably 1 to 60 seconds, and even more preferably 1 to 10 seconds. The total heat setting time is preferably not longer than 2000 seconds, more preferably not longer than 120 seconds, even more preferably not longer than 30 seconds, and particularly preferably not longer than 20 seconds. In the present invention, the heat setting process is preferably two or more stages, but in consideration of the total heat setting time, two to three stages is more preferred.

[0058] Next, it is preferable to perform a relaxation treatment in the width direction while holding the heat-set biaxially oriented film with clips. In the present invention, it is preferable to perform the relaxation treatment in two or more stages at different temperatures. Performing the relaxation treatment in two or more stages at different temperatures allows the tension chains that cause thermal shrinkage to be relaxed without suddenly relaxing the molecular chains that have been tensioned by stretching, while maintaining an amorphous oriented structure, thereby improving durability and dimensional stability, making this a preferred embodiment. In the present invention, the relaxation rate is the ratio of the difference between the width between the clips before treatment and the width after treatment. For example, a relaxation rate of 2% indicates that if the width before treatment is 100 mm, 2 mm is relaxed, resulting in 98 mm after treatment. The relaxation rate of the previous stage of relaxation treatment (hereinafter sometimes abbreviated as Rx1) is preferably 1.0 to 10.0%, more preferably 3.0 to 7.0%. Furthermore, the temperature Trx1 during the relaxation treatment (Rx1) is preferably (Ths2-50)°C or higher and Ths2°C or lower, more preferably (Ths2-40)°C or higher and (Ths2-20)°C or lower. The relaxation rate of the subsequent relaxation treatment (hereinafter sometimes abbreviated as Rx2) is preferably 0.1 to 10%, more preferably 1.5 to 5%. The temperature Trx2 during the subsequent relaxation treatment (Rx2) is preferably (Trx1-40°C) or higher and (Trx1-10)°C or lower.

[0059] Thereafter, the film is cooled to a temperature preferably below 35°C, more preferably below 25°C, and then the film edges are removed and wound onto a core. Furthermore, from the viewpoint of improving thermal dimensional stability, the wound PPS film may be annealed while being conveyed under tension under certain temperature conditions. The annealing temperature is more preferably 130°C or higher and 200°C or lower. If the temperature exceeds 200°C, shrinkage deformation during the annealing treatment may deteriorate flatness. If the temperature is lower than 130°C, the removal of molecular structure distortion due to the annealing treatment may be incomplete, resulting in deterioration of durability and dimensional stability. The annealing temperature is preferably 150°C or higher and 180°C or lower. The annealing time is preferably 1 to 200 seconds, more preferably 10 to 100 seconds, and the annealing treatment is performed while conveying at a speed of 1 to 100 m / min, thereby obtaining the PAS film of the present invention.

[0060] In the present invention, the polyarylene sulfide film or its film roll may be subjected to any processing such as molding, surface treatment, lamination, coating, printing, embossing, etching, etc. In particular, from the viewpoint of improving adhesion to the organic resin layer, corona treatment is a preferred embodiment as the surface treatment.

[0061] The biaxially oriented polyarylene sulfide film of the present invention may contain inert particles to the extent that the effects of the invention are not impaired. Examples of inert particles include inorganic fillers such as silica, alumina, calcium carbonate, barium carbonate, barium titanate, barium sulfate, calcium silicate, magnesium oxide, titanium oxide, and zinc oxide, as well as particles of organic polymer compounds that do not melt at 300°C (e.g., cross-linked polystyrene). Adding inert particles can improve the slipperiness of the film during the film stretching process, suppress the occurrence of wrinkles when the film runs between rolls, and maintain the surface irregularities of the film even when the heat setting temperature following transverse stretching is increased, thereby suppressing surface scratches and improving runnability.

[0062] The biaxially oriented polyarylene sulfide film of the present invention has excellent durability and can therefore be suitably used for automobiles, various parts of electric and electronic materials, circuit substrates, heat-resistant tape substrates, films for toner stirrers for printing, release films, and particularly for electrolyte membrane reinforcing members and film capacitors for fuel cells and water electrolysis devices that require durability and dimensional stability, as well as battery current collector foil substrates for lithium ion secondary batteries and the like.

[0063] In the present invention, the electrolyte membrane reinforcing member is punched into a frame or picture frame shape and attached to the peripheral edge of the electrolyte membrane. The frame-shaped electrolyte membrane reinforcing member has the central portion where the electrodes are stacked cut out to the shape of the electrodes, with the electrolyte membrane reinforcing member present only at the peripheral edge. The electrolyte membrane reinforcing member can be used by attaching at least one electrolyte membrane reinforcing member to the peripheral edge of the electrolyte membrane. Another preferred embodiment is to use two electrolyte membrane reinforcing members stacked one on top of the other. Specifically, one embodiment is to sandwich the peripheral edge of the electrolyte membrane and use one electrolyte membrane reinforcing member on each side of the electrolyte membrane. Furthermore, two or more electrolyte membrane reinforcing members may be stacked on each side of the electrolyte membrane, with the peripheral edge of the electrolyte membrane sandwiched between them.

[0064] The electrolyte membrane reinforcing member may be bonded to the electrolyte membrane via an organic resin layer, and known methods (e.g., JP-A-2015-2029 and JP-A-2022-69952) can be applied to the biaxially oriented polyarylene sulfide film of the present invention.

[0065] The electrolyte membrane reinforcing member of the present invention preferably includes a component having at least the biaxially oriented polyarylene sulfide film of the present invention, an organic resin layer, and the biaxially oriented polyarylene sulfide film of the present invention, in this order. In the present invention, the organic resin layer is used as an adhesive layer and is used to bond the biaxially oriented polyarylene sulfide, the organic resin layers to each other, and the electrolyte membrane. The organic resin layer may be thermosetting, thermoplastic (hot melt), or UV-curable. Examples of adhesives and / or pressure-sensitive adhesives that can be used for the organic resin layer include polyester resins, modified olefin resins, epoxy resins, acrylic resins, silicone resins, urethane resins, and ethylene vinyl resins, and these can be formed by various coating methods (e.g., gravure coating, metaling bar coating, reverse roll coating, etc.). As the organic resin layer, a hot melt adhesive is preferred from the viewpoint of handling of the film, and examples thereof include "Aronmelt" (registered trademark) PES-120L, PES-140H, PES-111EE, PES310S30, PES375S40, PPET1008, PPET1025, PPET2102, and PPET1303S (all manufactured by Toagosei Co., Ltd.), Y-167, H-930-S, and H-180S (all manufactured by Tanaka Chemical Co., Ltd.). Examples of suitable organic resins include "Nichigo Polyester" (registered trademark) SP-154, SP-165, SP-170, and SP-176 (all manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), "Vylon" (registered trademark) 200, 240, 300, 550, and BX1001 (all manufactured by Toyobo Co., Ltd.), and "Polysol" (registered trademark) SE-1720, SE-4210E, SE-6210, and SE-6210L (all manufactured by Showa Denko K.K.). The thickness of the organic resin layer is preferably in the range of 1 to 50 μm. By bonding the electrolyte membrane reinforcing member via the organic resin layer, it is possible to bond the organic resin layer and the electrolyte membrane, improving adhesion and further improving durability when used as an electrolyte membrane reinforcing member.

[0066] The electrolyte membrane reinforcing member of the present invention preferably has a thermal expansion coefficient measured in a temperature range of 100°C to 130°C of 40 ppm / °C or more and 65 ppm / °C or less in the direction in which the thermal expansion coefficient measured in a temperature range of 100°C to 130°C is the highest.

[0067] In the present invention, the direction with the highest thermal expansion coefficient refers to the direction with the highest thermal expansion coefficient in the temperature range of 100°C to 130°C when a rectangular piece is cut out and the thermal expansion coefficient is measured in 10° increments, with the long side direction and / or the short side direction of the rectangle being set at 0°. A thermal expansion coefficient within the above range is preferable because it reduces the internal stress on the fastened electrolyte membrane reinforcing member when operating at temperatures of 100°C or higher, thereby improving durability. A thermal expansion coefficient of less than 40 ppm / °C indicates extremely high orientation, which may result in poor film formability for producing an electrolyte membrane reinforcing member. A thermal expansion coefficient of more than 65 ppm / °C may lead to deterioration such as deformation and cracking due to internal stress when repeatedly operating at temperatures of 100°C or higher, resulting in poor durability. The thermal expansion coefficient is more preferably 60 ppm / °C or less. The detailed method for measuring the thermal expansion coefficient is as described in the Examples. Among the film-forming conditions described above, the thermal expansion coefficient tends to decrease as the stretch ratio increases, and tends to increase as the heat setting temperature increases.Furthermore, among the manufacturing conditions for the electrolyte membrane reinforcing member described below, the thermal expansion coefficient tends to increase as the processing temperature increases.

[0068] The cells used in fuel cells and water electrolysis devices have a structure in which a catalyst layer, an electrode substrate, and a separator are sequentially laminated on both sides of an electrolyte membrane having the biaxially oriented polyarylene sulfide film of the present invention as a reinforcing member. Of these, a CCM in which a catalyst layer is laminated on both sides of the electrolyte membrane (i.e., a layer structure of catalyst layer / electrolyte membrane / catalyst layer) is called a catalyst-coated electrolyte membrane (CCM), and a CCM in which a catalyst layer and a gas diffusion substrate are sequentially laminated on both sides of the electrolyte membrane (i.e., a layer structure of gas diffusion substrate / catalyst layer / electrolyte membrane / catalyst layer / gas diffusion substrate) is called a membrane electrode assembly (MEA).

[0069] Common methods for manufacturing a CCM include a coating method in which a catalyst layer paste composition for forming a catalyst layer is applied to the surface of an electrolyte membrane and dried, and a method in which only the catalyst layer is prepared on a substrate and then this catalyst layer is transferred to laminate the catalyst layer on the electrolyte membrane (transfer method).The edge of the electrolyte membrane in this CCM and the peripheral edge of the opening of the film of the present application to which the organic resin layer has been applied and cut into a frame shape are overlapped, and the CCM and electrolyte membrane reinforcing member are attached by heat pressing.

[0070] When an MEA is produced by pressing, known methods (e.g., the chemical plating method described in Electrochemistry, 1985, 53, p. 269, or the hot press bonding method of gas diffusion electrodes described in Electrochemical Science and Technology, edited by the Electrochemical Society (J. Electrochem. Soc.), 1988, 135, 9, p. 2209) can be applied. The temperature and pressure during pressing may be appropriately selected depending on the thickness and moisture content of the electrolyte membrane, the catalyst layer, and the electrode substrate. Specific pressing methods include roll pressing with specified pressure and clearance, and flat plate pressing with specified pressure.

[0071] The temperature during pressing of the present film is preferably 50°C or higher and 140°C or lower. Within this range, the durability of the electrolyte membrane reinforcing member can be improved without impairing the properties of the biaxially oriented film. If the pressing temperature is lower than 50°C, the biaxially oriented film will begin to adhere from around room temperature and will remain adhesive even at room temperature, which may result in poor handling during production. If the pressing temperature exceeds 140°C, excessive heat will be applied to the biaxially oriented film, which may cause structural changes and poor dimensional stability and durability. The pressing temperature is more preferably 130°C or lower, and even more preferably 120°C or lower. The pressing pressure is preferably 0.1 MPa or higher and 10 MPa or lower. If the pressing pressure is lower than 0.1 MPa, the pressure may not be applied, which may result in poor appearance, such as wrinkles. If the pressing pressure exceeds 10 MPa, the organic resin layer may deform, resulting in poor appearance. The pressing time is preferably 0.5 seconds or higher and 300 seconds or lower.

[0072] The fuel cell and water electrolysis device of the present invention will be described below.

[0073] The fuel cell of the present invention has an MEA using the biaxially oriented polyarylene sulfide film for reinforcing an electrolyte membrane of the present invention. By using the biaxially oriented polyarylene sulfide film for reinforcing an electrolyte membrane of the present invention in a fuel cell, the reinforcing effect can be enhanced even in a temperature range exceeding 100°C, leading to a longer life, etc.

[0074] The water electrolysis device of the present invention has an MEA using the biaxially oriented polyarylene sulfide film for reinforcing an electrolyte membrane of the present invention. By using the biaxially oriented polyarylene sulfide film for reinforcing an electrolyte membrane of the present invention in the water electrolysis device, a stable reinforcing effect against environmental fluctuations in output is achieved, leading to a longer life, etc.

[0075] [Method for measuring properties] (1) Content of polyarylene sulfide resin The infrared absorption spectrum of the film is measured by the ATR method using an infrared spectrophotometer (PerkinElmer, Spectorum 100 / Universal ATR (single reflection, crystal used: diamond / ZnSe)). From the obtained infrared absorption spectrum, the content of polyarylene sulfide resin is determined from the ratio of the peak due to the φ-S stretching vibration group based on the sulfide bond of polyarylene sulfide to the peak due to other substances. In order to convert the peak height ratio to a mass ratio, a calibration curve was created in advance using samples with known mass ratios (for example, olefins used as incompatible resins), and the content of polyarylene sulfide resin was calculated from the ratio to the total amount of polyarylene sulfide and other substances.

[0076] (2) Elastic Modulus at 25°C and Elastic Modulus at 130°C First, the direction of the main orientation axis was identified. One of the directions was set to 0°, and the elastic modulus was measured at 25°C by the following method while changing the direction in the film plane from -90° to 90° in 10° increments. The direction with the highest elastic modulus value was determined to be the main orientation axis direction of the film.

[0077] According to JIS K7127 (1999), a tensile test was performed using a tensile tester (RTG-1210 manufactured by A&D Company, Limited) with a width of 10 mm, set so that the length between chucks was 50 mm, and at a temperature of 25°C or 130°C and a pulling rate of 300 mm / min.

[0078] The elastic modulus was determined by calculating the load difference at a 0.2 mm interval within the measurement range of 0 mm to 10 mm displacement, with the start point of the displacement set to 0 mm and the end point set to 10 mm. The second, third, and fourth coordinates from the maximum were used as the original data, and the line was linearized using the least squares method. The slope was used as the elastic modulus. Five samples were cut so that the direction of the test length was in the desired direction, and measurements were taken, and the average was calculated. Measuring device: RTG-1210 manufactured by A&D Company, Limited. Test size: Test length 150 mm x width 10 mm. Chuck length: 50 mm. Tensile speed: 300 mm / min. Measurement environment: 25°C, 55% RH, or 130°C. Analysis conditions: Displacement mode. Start point: 0 mm. End point: 10 mm. Interval: 0.2 mm.

[0079] (3) 130°C Heat Shrinkage The film was cut into 10 mm x 150 mm strips with the sample length direction being the main alignment axis and the direction perpendicular to the main alignment axis, and a mark was made at the center 100 mm. The distance between the markings was measured using the following device (marking distance before heat treatment). Next, a 3 g weight was hung from the film, and the film was heat-treated for 30 minutes in a hot air oven heated to 130°C, and the distance between the markings was measured in the same manner as above (marking distance after heat treatment). The obtained marking distance was used to calculate the 130°C heat shrinkage using the following formula. Five samples were measured in both the main alignment axis direction and the direction perpendicular to the main alignment axis, and the average was calculated. Measurement device: Universal projector Sample size: Sample length 150 mm × width 10 mm Heat treatment device: Gear oven Heat treatment conditions: 130°C, 30 minutes Load: 3 g Calculation method: 130°C heat shrinkage (%) = {(gauge line distance before heat treatment) - (gauge line distance after heat treatment)} / gauge line distance before heat treatment × 100 (4) Glass transition temperature (°C), mobile amorphous amount (%) Using a temperature modulation DSC (Q1000) manufactured by TA Instruments, 5 mg of a sample was measured in a nitrogen atmosphere from 0°C to 200°C at a heating rate of 2°C / min, with a temperature modulation amplitude of ±1°C and a temperature modulation period of 60 seconds. The glass transition temperature (Tg) was determined as the intersection of a straight line drawn by extending the high-temperature baseline toward the low-temperature side of the curve obtained by the measurement in accordance with JIS 7121 (2012) and a tangent drawn at the point where the gradient of the stepwise change portion of the curve is maximum. The specific heat difference (ΔCp) calculated from the baseline above Tg and the baseline below Tg in accordance with JIS was determined, and the mobile amorphous amount (Xma) was calculated using the following formula: Mobile amorphous amount: Xma (%) = ΔCp / ΔCp0 × 100 Here, ΔCp0 represents the specific heat difference before and after the Tg of completely amorphous PPS, and ΔCp0 = 0.2699 J / g°C was used. The values ​​are based on Wunderlich B., Thermal Analysis of Polymeric Materials, Appendix 1 (The ATHAS Data Bank), Springer (2005).

[0080] (5) Weight-average molecular weight The molecular weight of the PAS resin or film was calculated in terms of polystyrene using GPC. The measurement conditions for GPC are as follows: Apparatus: SSC-7110 manufactured by Senshu Scientific Column: Shodex UT-G + Shodex UT-806M x 2 manufactured by Showa Denko Eluent: 1-chloronaphthalene Detector: Differential refractive index detector Column temperature: 210°C Pre-thermostat temperature: 250°C Pump thermostat temperature: 50°C Detector temperature: 210°C Flow rate: 1.0 mL / min Sample injection amount: 300 μL (concentration: 0.1% by mass) Standard sample: polystyrene.

[0081] (6) Resonance parameter (Q value) The film was cut into a 5 cm x 5 cm square and evaluated at a frequency of 15 GHz using a microwave molecular orientation meter (MOA-6015, manufactured by Oji Scientific Instruments Co., Ltd.). The film was rotated by 30° at a time, and measurements were taken at six points up to 150°, and the average value was calculated. Measurements were taken for one sample, and the average value of the minimum and maximum values ​​of the degree of orientation (Q) was adopted as the value. Measurements were taken 10 times for one sample, and the average value of the obtained values ​​was taken as the Q value of that sample.

[0082] (7) Melting point (Tm), minute endothermic peak temperature (T-meta) According to JIS K7121 (1999), a differential scanning calorimeter was used, using a Rigaku DSC (Thermo plus EVO2 DSCvesta-SL), 5 mg of the sample was sealed in an aluminum pan and heated from 25 ° C to 350 ° C at a heating rate of 20 ° C / min. At that time, the peak temperature of the observed endothermic peak of melting was taken as the melting point (Tm), and the minute endothermic peak temperature appearing in the temperature range of 150 ° C or more and Tm ° C or less was taken as T-meta. The melting point here was taken as the point at which the difference from the baseline of the DSC chart was greatest. Since the minute endothermic peak was observed in the first run of DSC and was not observed in the second run in which the temperature was raised to above Tm and the thermal history was erased, it can be confirmed by comparing both DSC charts. The measurement was carried out three times for each sample, and the average values ​​obtained were taken as the melting point (° C.) and the minute endothermic peak (T-meta) of the sample.

[0083] (8) Film Thickness The thickness of the biaxially oriented polyarylene sulfide film was measured at 10 random locations in an atmosphere of 23°C and 65% RH using a contact-type electronic micrometer (K-312A model) manufactured by Anritsu Corporation. The arithmetic mean value of the thicknesses at the 10 locations was taken as the film thickness (unit: μm) of the biaxially oriented polyarylene sulfide film.

[0084] (9) Film Density According to JIS K7112, a sample cut into an approximately square shape (approximately 5 mm x 5 mm) was placed in a density gradient tube (NaBr aqueous solution, 25°C), and after overnight, the measurement was performed by reading the scale on the gradient tube. Four floats with known densities were placed in the density gradient tube, and a calibration curve was prepared in advance from the positions and densities of the floats. The density of each sample was calculated based on the calibration curve. Three samples were placed in each tube, and the average value was used as the film density of that sample.

[0085] (10) Thermal expansion coefficient from 100 ° C to 130 ° C In the case of a biaxially oriented polyarylene sulfide film, a hot melt adhesive (manufactured by Toagosei Co., Ltd.: "Aronmelt" (registered trademark) PPET1303S) was applied to the polyarylene sulfide film as the organic resin layer of the electrolyte membrane reinforcing member using a bar coater, and dried for 60 seconds in an oven heated to 100 ° C. to obtain a biaxially oriented polyarylene sulfide / organic resin layer polyarylene sulfide film laminate with an organic resin layer thickness of 10 μm. Next, two polyarylene sulfide laminates were stacked so that the organic resin layers were in contact with each other and bonded under the conditions shown in the table to obtain a biaxially oriented polyarylene sulfide / organic resin layer / biaxially oriented polyarylene sulfide laminate, which was then subjected to thermal expansion coefficient evaluation.

[0086] In addition, when the biaxially oriented polyarylene sulfide film was coated with an organic resin layer other than the above-mentioned layers, the organic resin layers were stacked so that they were in contact with each other and bonded under the conditions shown in the table to form a biaxially oriented polyarylene sulfide film / organic resin layer / biaxially oriented polyarylene sulfide film laminate, which was then subjected to thermal expansion coefficient evaluation.

[0087] The thermal expansion coefficient was measured by cutting the above-mentioned sample into a rectangular shape, changing the direction in 10° increments over a temperature range from 100°C to 130°C, with the long side direction and / or short side direction of the rectangle being set as 0°, and the thermal expansion coefficient in the highest direction was taken as the thermal expansion coefficient of the electrolyte membrane reinforcing member.

[0088] The thermal expansion coefficient was measured in accordance with JIS K7197-1991 during the cooling process after heating up to 200°C. The average thermal expansion coefficient from T1 to T2 was calculated using the following formula, where the initial sample length at 25°C and 65% RH is L0, the sample length at temperature T1 is L1 (mm), and the sample length at temperature T2 is L2 (mm).

[0089] Note that T2=100 (°C), T1=130 (°C), and L0=20 mm.

[0090] Thermal expansion coefficient (ppm / °C) = (((L2 - L1) / L0) / (T2 - T1)) x 1000000 Heating and cooling rate: 5°C / min Sample width: 4 mm Load: 29.4 mN (11) Durability A rectangular specimen of 150 mm length x 10 mm width cut from the sample film was placed in an environmental tester (Highly Accelerated Life Tester PC-R8D manufactured by Hirayama Manufacturing Co., Ltd.) set to 125°C, 2 atm, wet saturation mode, and 100% RH for 500 hours, and the specimen was removed and its breaking strength was measured. Five samples were taken so that the direction of the specimen length was parallel to the main orientation axis and the direction perpendicular to the main orientation axis, and measurements were performed, with the average value of each sample being used for evaluation. The breaking elongation retention rate, expressed by the following formula (1), was calculated from the average values ​​in each direction. Durability was evaluated according to the following criteria. A: Breaking elongation retention rate is 85% or more B: Breaking elongation retention rate is 80% or more C: Breaking elongation retention rate is 75% or more D: Breaking elongation retention rate is less than 75% Measuring device: RTG-1210 manufactured by A&D Company, Limited Tensile speed: 300 mm / min Measurement environment: 25°C, 55% RH Breaking elongation retention rate (%) = (breaking elongation X / initial breaking elongation X0) × 100 (1) (In the formula, breaking elongation X represents the breaking elongation (unit: %) after treatment for 500 hours under conditions of 125°C, 2 atm, and 100% RH, and breaking elongation X0 represents the initial breaking elongation (unit: %) before treatment.

[0091] (12) Dimensional Stability A film (periphery 100 mm x 100 mm, inner circumference 80 mm x 80 mm) cut into a rectangular frame was placed on a press heated to 80°C so that the main orientation axis direction and the direction perpendicular to the main orientation axis were parallel to the sides of the frame, and pressurized to 10 MPa. The temperature was raised to 130°C under pressure, and the film was treated for 1 hour. After that, the temperature was lowered to 80°C under pressure, and the pressure was released at 80°C, and the film was removed. Compared with the film before treatment, dimensional stability was evaluated according to the following criteria, including the 130°C heat shrinkage rate described in (2). A: No changes such as wrinkles or distortion were observed in the film, and the 130°C heat shrinkage rate of the film was -1.0% to 1.0% in both the main orientation axis direction and the direction perpendicular to the main orientation axis. B: Slight changes such as wrinkles and distortions are observed in the film, and the 130°C heat shrinkage of the film in either the main orientation axis direction or the direction perpendicular to the main orientation axis is -1.2% or more but less than -1.0%, and / or more than 1.0% but not more than 1.2%. C: Wrinkles and distortions are observed in the film, and the 130°C heat shrinkage of the film in both the main orientation axis direction and the direction perpendicular to the main orientation axis direction is -1.2% or more but less than -1.0%, more than 1.0% but not more than 1.2%, and / or the 130°C heat shrinkage in either direction is less than -1.2% or more than 1.2%. D: Wrinkles and distortions are observed in the film, and the 130°C heat shrinkage of the film in both the main orientation axis direction and the direction perpendicular to the main orientation axis direction is less than -1.2% or more than 1.2%.

[0092] (13) Appearance of Electrolyte Membrane Reinforcement Member A hot melt adhesive ("Aronmelt" (registered trademark) PPET1303S, manufactured by Toagosei Co., Ltd.) was applied to a polyarylene sulfide film as an organic resin layer using a bar coater, and the film was dried for 60 seconds in an oven heated to 100°C to obtain a biaxially oriented polyarylene sulfide / polyarylene sulfide film laminate of an organic resin layer having a thickness of 10 µm.

[0093] Next, an 85 mm x 85 mm perfluorosulfonic acid resin (DuPont: "Nafion" (registered trademark) 117) was used as the electrolyte membrane, and polyarylene sulfide film laminates (outer periphery 100 mm x 100 mm, inner periphery 80 mm x 80 mm) were placed on both sides of the electrolyte membrane. The films were set around the electrolyte membrane as shown in Figure 1, and the organic resin layers were overlapped so that they were in contact with each other, and bonded under the conditions shown in the table. After removal, the electrolyte membrane reinforcing member was visually inspected for deformation such as wrinkles and distortion, and the appearance of the electrolyte membrane reinforcing member was evaluated according to the following criteria: AA: Almost no deformation of the film was observed. A: The film was slightly distorted, but there was no problem in practical use. B: The film was distorted, but it was usable. C: The film was distorted overall, and it was usable in practical use. D: The entire film was significantly distorted, and it was not usable in practical use.

[0094] (14) Cell durability (I) A hot melt adhesive (manufactured by Toagosei Co., Ltd.: "Aronmelt" (registered trademark) PPET1303S) was applied to a polyarylene sulfide film as an organic resin layer using a bar coater, and then dried for 60 seconds in an oven heated to 100 ° C. to obtain a biaxially oriented polyarylene sulfide / organic resin layer polyarylene sulfide film laminate with an organic resin layer thickness of 10 μm. Next, a 50 mm × 50 mm perfluorosulfonic acid resin (manufactured by DuPont: "Nafion" (registered trademark) 117) was used as an electrolyte membrane, and polyarylene sulfide film laminates (outer circumference 80 mm × 80 mm, inner circumference 48 mm × 48 mm) were placed on both sides of the electrolyte membrane, and the organic resin layers were stacked so that they were in contact with each other, and bonded under the conditions shown in the table to produce an electrolyte membrane with a subgasket. A commercially available electrode, a gas diffusion electrode for fuel cells "ELAT (registered trademark) LT120ENSI" manufactured by BASF, 5 g / m 2 A pair of Pt-attached electrodes cut to 5 cm x 5 cm was prepared and stacked facing each other so as to sandwich the electrolyte membrane, forming a JARI standard cell (electrode area 25 cm). 2 ) and used as a tightening evaluation cell so as to obtain a predetermined surface pressure.

[0095] The evaluation cell was placed in an environmental tester (Highly Accelerated Life Tester PC-R8D manufactured by Hirayama Manufacturing Co., Ltd.) set to 125°C, 2 atm, wet saturation mode, and 100% RH, and treated for 500 hours. Nitrogen gas was sealed into the gas flow path of the JARI standard cell to a pressure of 300 kPa, and the cell was left to stand for one hour. The presence or absence of gas leaks was evaluated based on the change in pressure, and the durability of the cell was evaluated according to the following criteria: A: There was no change in the pressure of the sealed gas, and it was suitable for practical use. B: The pressure of the sealed gas decreased slightly, but it was still suitable for practical use. C: The pressure of the sealed gas decreased, causing gas leaks and making it unsuitable for practical use.

[0096] (15) Cell Durability (II) An evaluation cell was prepared in the same manner as in Cell Durability (I). The evaluation cell was subjected to 2000 cycles of -40°C for 30 minutes and 125°C for 30 minutes using a thermal shock tester (Espec Corporation, thermal shock tester TSE-11), with 500 hours of treatment. Nitrogen gas was sealed into the gas flow path of the JARI standard cell to a pressure of 300 kPa, and the cell was left to stand for 1 hour. The presence or absence of gas leakage was evaluated based on the change in pressure, and the durability of the cell was evaluated according to the following criteria. A: There was no change in the pressure of the sealed gas, and there was no problem in practical use. B: The pressure of the sealed gas decreased slightly, but it was still usable in practical use. C: The pressure of the sealed gas decreased, causing gas leakage, making it impossible to use.

[0097] Reference Example 1: Preparation of Polyphenylene Sulfide Resin Granules (PPS Granules 1) A 1-kilometer SUS vessel equipped with a stirrer was charged with 1 kmole of 47% sodium hydrosulfide, 1.02 kmole of 47% sodium hydroxide, 1.6 kmole of N-methyl-2-pyrrolidone (NMP), 0.3 kmole of sodium acetate, and 100 kg of ion-exchanged water. While stirring at 240 rpm and passing nitrogen through at atmospheric pressure, the mixture was gradually heated to 235°C over approximately 180 minutes. After distilling 209 kg of water and 0.4 kg of NMP, the reactor was cooled to 160°C. The amount of hydrogen sulfide released was 0.02 kmole. To the remaining mixture, 1.02 kmole of p-dichlorobenzene (p-DCB) and 2.40 kmole of NMP were added. The reactor was then sealed under nitrogen gas. The temperature was raised from 160 ° C to 220 ° C over 100 minutes while stirring at 400 rpm, and the reaction was carried out at 220 ° C for 300 minutes. Next, the temperature was raised from 220 ° C to 255 ° C over 60 minutes, 0.8 kmol of water was poured into the system over 10 minutes, and the reaction was continued for 440 minutes. Thereafter, the mixture was cooled from 255 ° C to 200 ° C over 100 minutes. After reaching 150 ° C, the mixture was rapidly cooled to near room temperature using a blower. The contents were removed, 1 kiloliter of NMP was added, and the mixture was stirred at 85 ° C for 30 minutes, after which the solvent and solids were filtered off using an 80 mesh sieve. 1 kiloliter of NMP was added to the obtained solid, and the mixture was stirred at 85 ° C for 30 minutes and filtered off. This operation of adding 1 kiloliter of warm water to the obtained solid, stirring at 70 ° C for 30 minutes, and filtering was repeated three times. To the obtained solid, 0.3 kg of calcium acetate monohydrate and 1 kiloliter of warm water were added, and the mixture was stirred at 70°C for 30 minutes and filtered. To the obtained solid, 1 kiloliter of warm water was added, and the mixture was stirred at 70°C for 30 minutes and filtered. This procedure was repeated three times. The solid was then dried under reduced pressure at 120°C for 5 hours to obtain PPS granules 1.

[0098] (Reference Example 2) Preparation of polyphenylene sulfide resin granules (PPS granules 2) PPS granules 2 were obtained by the same procedure as in Reference Example 1, except that the reaction temperature and time were the same as in Reference Example 1, in which the temperature was raised from 160°C to 270°C over 180 minutes, the reaction was carried out at 270°C for 135 minutes, and the reaction was then cooled from 270°C to 200°C over 100 minutes.

[0099] Reference Example 3: Method for producing PPS pellets (PPS1) The PPS granules 1 produced in Reference Example 1 were charged into a vented co-rotating twin-screw kneading extruder (manufactured by The Japan Steel Works, Ltd., screw diameter 30 mm, screw length / screw diameter = 45.5) heated to 315°C, melt-extruded at a residence time of 90 seconds and a screw rotation speed of 150 rpm, and discharged in the form of strands. These were cooled with water at a temperature of 25°C and then immediately cut into chips to obtain PPS pellets (PPS1) having a weight-average molecular weight of 75,000 and a melting point of 280°C.

[0100] Reference Example 4: Method for producing PPS pellets (PPS2) The PPS granules 2 produced in Reference Example 2 were charged into a vented co-rotating twin-screw kneading extruder (manufactured by The Japan Steel Works, Ltd., screw diameter 30 mm, screw length / screw diameter = 45.5) heated to 315°C, melt-extruded at a residence time of 90 seconds and a screw rotation speed of 150 rpm, and discharged in the form of strands. These were cooled with water at a temperature of 25°C and then immediately cut into chips to obtain PPS pellets (PPS2) having a weight-average molecular weight of 55,000 and a melting point of 280°C.

[0101] Example 1 The PPS pellets (PPS1) prepared in Reference Example 3 were dried under reduced pressure at 180°C for 3 hours. They were then fed into an extruder, melted at 310°C under a nitrogen atmosphere, and introduced into a T-die die. The pellets were then extruded into a sheet form from the T-die die to form a molten monolayer sheet. The molten monolayer sheet was cast onto a casting drum rotating at 3.5 m / min and maintained at a surface temperature of 25°C, while being cooled and solidified by electrostatic application to obtain an unstretched film. The unstretched film was then stretched in the longitudinal direction of the film at 3.9 times its original size at 100°C using a longitudinal stretching machine consisting of a group of heated rolls (MD stretching) utilizing the difference in peripheral speed between the rolls. The film was then held at both ends with clips and introduced into a tenter, where it was stretched 3.5 times in the width direction (TD stretching) at a stretching temperature of 105 ° C. The first heat treatment (Ths1) was performed for 10 seconds using a tenter heated to 180 ° C., followed by a second heat treatment (Ths2) for 10 seconds using a tenter heated to 228 ° C. Next, the first relaxation treatment (Rx1) was performed at a relaxation rate of 5% using a tenter at 199 ° C., followed by a second relaxation treatment (Rx2) at a relaxation rate of 3% using a tenter at 178 ° C. After cooling to room temperature, the film edges were removed to obtain a 50 μm thick biaxially oriented polyarylene sulfide film. The physical properties and characteristics of the resulting film and electrolyte membrane reinforcement member are shown in Table 1.

[0102] Examples 2 to 14, Comparative Examples 1 to 6 Biaxially oriented polyarylene sulfide films were obtained in the same manner as in Example 1, except that the raw materials and film-forming conditions were changed to those shown in the table while adjusting the extrusion rate.

[0103] (Comparative Example 7) A biaxially oriented polyarylene sulfide film was produced in the same manner as in Example 1, except that the raw materials and film-forming conditions were changed to those shown in the table while adjusting the extrusion rate. Many stretching fractures occurred, so only a small number of samples were collected and their properties were evaluated.

[0104] Examples 15 to 17, Comparative Example 8 The film obtained in Example 1 was used, but the bonding conditions with the electrolyte membrane were changed as shown in the table to produce electrolyte membrane reinforcing members. The physical properties and characteristics are shown in the table.

[0105]

[0106]

[0107]

[0108]

[0109]

[0110]

[0111]

[0112]

[0113]

[0114]

[0115] 1: Polyarylene sulfide film 2: Organic resin layer 3: Electrolyte membrane

Claims

1. The main component is polyarylene sulfide (PAS) resin, and the elastic modulus at 25°C in the direction perpendicular to the main orientation axis (Y A25 ) and the elastic modulus (Y A130 ) ratio Y A130 / Y A25 A biaxially oriented polyarylene sulfide film having a thermal shrinkage ratio at 130° C. in the same direction of 0.25 to 0.80, and a thermal shrinkage ratio at 130° C. in the same direction of -1.2% to 1.2%.

2. A biaxially oriented polyarylene sulfide film having a glass transition temperature (Tg) of 110°C or higher and 140°C or lower as determined by temperature-modulated differential scanning calorimetry (temperature-modulated DSC) and having a mobile amorphous content of 5% or higher and 25% or lower relative to the entire film.

3. Elastic modulus at 25°C in the main orientation axis direction (Y B25 ) and the elastic modulus (Y B130 ) ratio Y B130 / Y B25 3. The biaxially oriented polyarylene sulfide film according to claim 1, wherein the linear modulus is 0.25 or more and 0.80 or less, and the thermal shrinkage rate at 130° C. in the same direction is −1.2% or more and 1.2% or less.

4. A biaxially oriented polyarylene sulfide film according to claim 1 or 2, in which the elastic modulus measured at 130°C is 1.0 GPa or more in both the direction of the main orientation axis and the direction perpendicular to the main orientation axis.

5. A biaxially oriented polyarylene sulfide film according to claim 1 or 2, in which the resonance parameter (Q value) determined by microwave orientation measurement is 4,600 or more and 5,200 or less.

6. The biaxially oriented polyarylene sulfide film according to claim 1 or 2, having a weight average molecular weight (Mw) of 60,000 or more and 150,000 or less.

7. Density is 1.3450 g / cm 3 More than 1.3550g / cm 3 3. The biaxially oriented polyarylene sulfide film according to claim 1 or 2, wherein:

8. The biaxially oriented polyarylene sulfide film according to claim 1 or 2, wherein the minute endothermic peak temperature (Tmeta) (°C) determined by differential scanning calorimetry (DSC) is (the melting point (Tm) of the film - 100)°C or higher and (Tm - 20)°C or lower.

9. A method for producing a biaxially oriented polyarylene sulfide film as described in claim 1 or 2, comprising the steps of melt extruding a polyarylene sulfide resin composition, cooling and solidifying the composition, stretching the film in the running direction (MD stretching), and then holding the film with clips and stretching it in the width direction of the film (TD stretching) to form a biaxially oriented film, and then successively carrying out a process of heat setting treatment at a heat setting temperature (Ths1) in the first stage of 150°C or higher and 230°C or lower, and a process of heat setting treatment at a heat setting temperature (Ths2) in the final stage of 265°C or higher.

10. An electrolyte membrane reinforcing member using the biaxially oriented polyarylene sulfide film according to claim 1 or 2.

11. The electrolyte membrane reinforcing member according to claim 10, comprising a component having at least a biaxially oriented polyarylene sulfide film, an organic resin layer and a biaxially oriented polyarylene sulfide film, in this order.

12. The electrolyte membrane reinforcing member according to claim 10, wherein the thermal expansion coefficient measured in the temperature range of 100° C. to 130° C. in the direction in which the thermal expansion coefficient is highest measured in the temperature range of 100° C. to 130° C. is 40 ppm / ° C. or more and 65 ppm / ° C. or less. Measurement method: When the thermal expansion coefficient is measured in the temperature range of 100° C. to 130° C. by changing the direction in increments of 10° with the long side direction and / or the short side direction of the rectangle set as 0°, the value in the direction in which the thermal expansion coefficient is highest is calculated.

13. A fuel cell having the electrolyte membrane reinforcing member according to claim 10.

14. A water electrolysis device having the electrolyte membrane reinforcing member according to claim 10.

Citation Information

Patent Citations

  • Seal integrated membrane-electrode assembly

    JP2007250249A

  • Biaxially oriented polyarylene sulfide film, metallized film, and capacitor

    JP2009132874A

  • Biaxially oriented polyarylene sulfide film and adhesive material using the same

    JP2010070630A

  • Composite polymer electrolyte membrane, electrolyte membrane with catalyst layer, membrane electrode complex and solid polymer fuel cell

    JP2021051994A

Cited By

  • Polyphenylene sulfide film, and polyphenylene sulfide film for electrolyte membrane reinforcement.

    JP2026145894A

  • Polyphenylene sulfide film for electrolyte membrane reinforcement

    JP2026147884A