Optical film and method for manufacturing same, retardation film, and circularly polarizing plate

The optical film with controlled in-plane birefringence and retardation values addresses the challenge of phase difference unevenness in polarizing plates for curved surfaces, ensuring improved optical performance by processing retardation films into curved surfaces with strategically arranged high and low retardation regions.

WO2024203389A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009990
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-14
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for creating polarizing plates for curved surfaces face challenges in reducing phase difference unevenness, making it difficult to achieve uniform optical performance when integrated with optical elements like lenses.

Method used

An optical film with in-plane birefringence less than 0.008 and a curved surface portion, where the in-plane retardation value is 95% to 105% of the average value, is developed, along with a method to process retardation films into curved surfaces with high and low retardation regions arranged perpendicular to the slow axis direction to minimize phase difference unevenness.

Benefits of technology

The solution effectively reduces phase difference unevenness in the optical film, enhancing the uniformity and performance of optical systems by ensuring the in-plane retardation values remain consistent across the curved surface, thereby improving the optical properties of the film when integrated with curved optical elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009990_03102024_PF_FP_ABST
    Figure JP2024009990_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an optical film having a curved surface part and an in-plane birefringence of less than 0.008, the in-plane phase difference value in the curved surface part being 95-105% of the average value of the in-plane phase difference in the curved surface part.
Need to check novelty before this filing date? Find Prior Art

Description

Optical film and method for producing the same, retardation film, and circularly polarizing plate

[0001] The present invention relates to an optical film and a method for producing the same, a retardation film, and a circularly polarizing plate.

[0002] Curved polarizing plates for laminating on optical elements having curved surfaces, such as lenses, are known (see, for example, Patent Document 1). In the technology of Patent Document 1, a polarizer and a retardation film having a predetermined in-plane retardation are bonded together so that the slow axis of the retardation film and the absorption axis of the polarizer are parallel to each other to obtain a curved polarizing plate. Patent Document 1 describes that even when a curved polarizing plate is laminated on the curved surface of an adherend to form an optical laminate, the retardation film is unlikely to have birefringence in a direction at an angle 45° to the absorption axis or transmission axis of the polarizer.

[0003] Patent No. 6581798

[0004] For example, a retardation film having an in-plane retardation functioning as a quarter-wave plate can be curved, combined with an optical element such as a lens, and incorporated into the optical system of an image display device such as a stereoscopic image display device. However, curved processing of a retardation film having an in-plane retardation may cause unevenness in the in-plane retardation value (retardation unevenness) in the retardation film. Such retardation unevenness can degrade the performance of the optical system, so it is necessary to reduce the retardation unevenness. However, with the technology of Patent Document 1, it was sometimes difficult to reduce the retardation unevenness that occurs after curved processing.

[0005] Therefore, there is a need for a novel optical film with reduced retardation unevenness; a method for producing such an optical film; a retardation film that can be used in the production of such an optical film; and a circular polarizing plate including such an optical film.

[0006] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, they have found that the above-mentioned problems can be solved by an optical film having an in-plane birefringence of less than 0.008 and a specific curved surface portion, and have completed the present invention. That is, the present invention provides the following.

[0007] <1> An optical film having an in-plane birefringence of less than 0.008, having a curved surface portion, and an in-plane retardation value at the curved surface portion of 95% to 105% of the average value of the in-plane retardation at the curved surface portion. <2> The optical film according to <1>, wherein the curved surface portion is spherical and has a radius of curvature of 66 mm to 130 mm. <3> The optical film according to <1> or <2>, wherein the curved surface portion functions as a quarter-wave plate. <4> The optical film according to any one of <1> to <3>, which is a multi-layered body and functions as a broadband quarter-wave plate. <5> The method for producing an optical film according to any one of <1> to <4>, comprising: a step of curvedly processing a retardation film to obtain an optical film, wherein the curved retardation film includes a high retardation region, the high retardation region is aligned in a direction perpendicular to an in-plane slow axis direction of the retardation film, and an in-plane retardation value of the high retardation region is 105% or more of the in-plane retardation value of the retardation film. <6> The method for producing an optical film according to <5>, further comprising: a step of contacting a region of the stretched film that is aligned in a direction perpendicular to the in-plane slow axis direction of the stretched film with a solvent to form the high retardation region, thereby obtaining the retardation film. <7> The method for producing an optical film according to any one of <1> to <4>, comprising a step of curvedly processing a retardation film to obtain an optical film, wherein the curved retardation film is a multilayer body of two or more retardation layers, and an angle formed by in-plane slow axes of two of the two or more retardation layers is 25° or more and 95° or less.<8> The method for producing an optical film according to any one of <1> to <4>, comprising: step (1) of curving a first retardation film to obtain a second retardation film having a curved portion; and step (2) of changing an in-plane retardation value in the curved portion of the second retardation film to obtain the optical film, wherein the curved portion of the second retardation film comprises low retardation regions aligned in a direction perpendicular to an in-plane slow axis direction of the curved portion, and the change in the in-plane retardation value in step (2) is achieved by increasing the in-plane retardation value of the low retardation regions by 5% or more. <9> The method for producing an optical film according to <8>, wherein the change in the in-plane retardation value in step (2) is achieved by contacting the low retardation regions with a solvent. <10> A retardation film, comprising a high-retardation region, the high-retardation region being aligned in a direction perpendicular to a slow axis direction of the retardation film, and an in-plane retardation value of the high-retardation region being 105% or more of an in-plane retardation value of the retardation film. <11> A circularly polarizing plate comprising the optical film according to any one of <1> to <4> and a polarizer.

[0008] According to the present invention, it is possible to provide an optical film with reduced retardation unevenness; a method for producing such an optical film; a retardation film that can be used in the production of such an optical film; and a circularly polarizing plate including such an optical film.

[0009] Fig. 1 is a perspective view schematically showing an example of an optical film of the present invention. Fig. 2 is a schematic diagram showing an example of a specific retardation film of the present invention. Fig. 3 is a schematic diagram showing the positional relationship of 17 points used to determine Re(ave) in Examples and Comparative Examples.

[0010] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and can be implemented with any modifications within the scope of the claims of the present invention and their equivalents. The components of the embodiments shown below can be combined as appropriate. In addition, in the drawings, the same components are designated by the same reference numerals, and their description may be omitted.

[0011] In the following description, unless otherwise specified, the slow axis of a film or layer refers to the slow axis in the plane of the film or layer.

[0012] In the following description, the angle formed by the optical axis (slow axis, transmission axis, absorption axis, etc.) of each layer in a member having multiple layers represents the angle when the layer is viewed from the thickness direction, unless otherwise specified.

[0013] In the following description, the angular relationship between the direction of the in-plane optical axis (slow axis, transmission axis, absorption axis, etc.) and the geometric direction (longitudinal direction and width direction of the film, etc.) of a certain product (optical film, retardation film, circular polarizer, etc.) is defined as a shift in one direction being positive and a shift in another direction being negative, unless otherwise specified, and the positive and negative directions are defined commonly for the components within the product. For example, in the case of a certain circular polarizer, "the angle between the absorption axis of the circular polarizer and the slow axis of the first λ / 2 plate is A°, the angle between the slow axis of the first λ / 2 plate and the slow axis of the second λ / 2 plate is B°, and the angle between the slow axis of the first λ / 2 plate and the slow axis of the λ / 4 plate is C°" means the following two cases: When the circular polarizer is observed from one side, the slow axis of the first λ / 2 plate is shifted clockwise by A° from the absorption axis of the circular polarizer, and the slow axis of the second λ / 2 plate is shifted clockwise by B° from the slow axis of the first λ / 2 plate, and the slow axis of the λ / 4 plate is shifted clockwise by C° from the slow axis of the first λ / 2 plate. When the circular polarizer is observed from one side, the slow axis of the first λ / 2 plate is shifted counterclockwise by A° from the absorption axis of the circular polarizer, the slow axis of the second λ / 2 plate is shifted counterclockwise by B° from the slow axis of the first λ / 2 plate, and the slow axis of the λ / 4 plate is shifted counterclockwise by C° from the slow axis of the first λ / 2 plate.

[0014] In the following description, unless otherwise specified, the oblique direction of a long film refers to an in-plane direction of the film, which is neither parallel nor perpendicular to the longitudinal direction of the film.

[0015] In the following description, unless otherwise specified, the front direction of a layer or film means the normal direction of the main surface of the film, and specifically refers to the direction of the polar angle of 0° and the azimuthal angle of 0° of the main surface.

[0016] In the following description, unless otherwise specified, the tilt direction of a layer or film means a direction that is neither parallel nor perpendicular to the main surface of the film, and specifically refers to a direction in which the polar angle of the main surface is in the range of greater than 0° and less than 90°.

[0017] In the following description, the in-plane retardation Re of a layer or film is a value expressed by Re = (nx - ny) x d unless otherwise specified. Furthermore, the retardation Rth in the thickness direction of a layer is a value expressed by Rth = [{(nx + ny) / 2} - nz] x d unless otherwise specified. Here, nx represents the refractive index in the direction perpendicular to the thickness direction of the layer (in-plane direction) that gives the maximum refractive index. ny represents the refractive index in the in-plane direction of the layer that is perpendicular to the nx direction. nz represents the refractive index in the thickness direction of the layer. d represents the thickness of the layer. The measurement wavelength is 543 nm unless otherwise specified.

[0018] In the following description, unless otherwise specified, the directions of elements as "parallel," "vertical," and "orthogonal" may include an error within a range that does not impair the effects of the present invention, for example, within a range of ±3°, ±2°, or ±1°.

[0019] In the following description, the term "plate" is not limited to rigid members but also includes flexible members such as resin films, and is not limited to flat plate-like members but also includes members with curved surfaces.

[0020] In the following description, unless otherwise specified, the term "adhesive" includes not only adhesives in the narrow sense (adhesives having a shear storage modulus of 1 MPa to 500 MPa at 23° C. after energy ray irradiation or heat treatment) but also pressure-sensitive adhesives having a shear storage modulus of less than 1 MPa at 23° C. Therefore, the term "adhesive layer" includes not only adhesive layers in the narrow sense but also pressure-sensitive adhesive layers.

[0021] 1. Optical Film 1.1. Overview An optical film according to one embodiment of the present invention has an in-plane birefringence of less than 0.008, has a curved surface portion, and has an in-plane retardation value at the curved surface portion that is 95% to 105% of the average value of the in-plane retardation at the curved surface portion. The optical film according to one embodiment of the present invention can provide a novel retardation film that can be combined with an optical element having a curved surface and has reduced retardation unevenness.

[0022] 1.2. Shape and Configuration of Optical Film The optical film of the present disclosure has a curved surface portion. FIG. 1 is a perspective view schematically illustrating an example of the optical film of the present invention. As shown in FIG. 1 , the optical film 10 has a flat portion 2 in addition to a curved surface portion 1. The curved surface portion 1 has a peripheral edge 1E at the boundary with the flat portion 2. In another embodiment, the optical film may have only the curved surface portion 1 without having the flat portion 2.

[0023] The curved surface of the curved portion is a plane perpendicular to the plane including the periphery of the curved portion and passing through the center of the curved portion, and when the optical film is cut, the curve defined in the cross section may have a single radius of curvature, or may be a combination of curves having two or more radii of curvature. Preferably, the curved surface of the curved portion is a spherical surface, such that when the optical film is cut along a plane perpendicular to the plane including the periphery of the curved portion and passing through the center of the curved portion, the curve defined in the cross section has a single radius of curvature. Hereinafter, when the radius of curvature is referred to for a spherical curved portion, it means the spherical radius.

[0024] The curved surface of the curved portion is preferably spherical. The radius of curvature of the curved portion when it is spherical is not particularly limited, but may be the same as or close to the radius of curvature of the concave or convex surface of a commonly used lens, preferably the radius of curvature of the convex surface. For example, the radius of curvature of the curved portion may be in the range of 130.75 mm ± 5 mm (corresponding to 4 curves), 87.16 mm ± 5 mm (corresponding to 6 curves), or 65.38 mm ± 5 mm (corresponding to 8 curves). When it is spherical, the radius of curvature of the curved portion is preferably 66 mm or more, more preferably 70 mm or more, and preferably 130 mm or less, more preferably 75 mm or less. Since the thickness of the optical film is sufficiently smaller than the normal radius of curvature, the radius of curvature of the curved portion can be the value for the concave surface of a normal curved portion.

[0025] The radius of the periphery of the curved surface portion that is a spherical surface is preferably 40 mm or more, more preferably 45 mm or more, and although there is no particular upper limit, it may be, for example, 90 mm or less.

[0026] The optical film may be composed of a single layer or a multi-layer structure. When the optical film is a multi-layer structure, any layer such as a retardation layer or an adhesive layer may be used as each layer constituting the multi-layer structure.

[0027] For example, the optical film may be a multi-layer structure including a first λ / 2 plate, a second λ / 2 plate, and a λ / 4 plate in this order. The optical film may also include a first λ / 2 plate, a second λ / 2 plate, a λ / 4 plate, and an optional retardation layer. When the optical film is a multi-layer structure including multiple retardation layers, the optical film can function as a broadband quarter-wave plate that imparts a quarter-wave retardation to incident light over a wide wavelength range.

[0028] In the present disclosure, a λ / 2 plate refers to a plate having an in-plane retardation Re(λ) at a wavelength λ of approximately λ / 2. A λ / 4 plate refers to a plate having an in-plane retardation Re(λ) at a wavelength λ of approximately λ / 4. The in-plane retardation Re(λ) of a λ / 2 plate is preferably within the range of (λ / 2±35) nm, more preferably within the range of (λ / 2±15) nm, and ideally λ / 2 nm. The in-plane retardation Re(λ) of a λ / 4 plate is preferably within the range of (λ / 4±30) nm, more preferably within the range of (λ / 4±10) nm, and ideally λ / 4 nm. When λ is 550 nm, the in-plane retardation Re(550) of a λ / 2 plate is preferably 240 nm or more, more preferably 260 nm or more, and preferably 310 nm or less, more preferably 290 nm or less. When λ is 550 nm, the in-plane retardation Re(550) of the λ / 4 plate is preferably 110 nm or more, more preferably 130 nm or more, and preferably 170 nm or less, more preferably 150 nm or less.

[0029] Preferably, the angle formed by the slow axis of the first λ / 2 plate and the slow axis of the second λ / 2 plate is 24.6° or more and 30.6° or less, the angle formed by the slow axis of the first λ / 2 plate and the slow axis of the λ / 4 plate is 90.5° or more and 96.5° or less, and the first λ / 2 plate satisfies any of the following formulas (1a), (1b), and (1c): nx1>ny1≒nz1 (1a) nx1>ny1>nz1 (1b) nx1>nz1>ny1 (1c) wherein nx1 represents the refractive index in an in-plane direction of the first λ / 2 plate that gives the maximum refractive index, ny1 represents the refractive index in the in-plane direction of the first λ / 2 plate that is perpendicular to the nx1 direction, and nz1 represents the refractive index in the thickness direction of the first λ / 2 plate, and the second λ / 2 plate satisfies any of the following formulas (2a), (2b), and (2c): nx2>ny2≈nz2 (2a) nx2>ny2>nz2 (2b) nx2>nz2>ny2 (2c) wherein nx2 represents the refractive index in an in-plane direction of the second λ / 2 plate that gives the maximum refractive index, ny2 represents the refractive index in the in-plane direction of the second λ / 2 plate that is perpendicular to the nx2 direction, and nz2 represents the refractive index in the thickness direction of the second λ / 2 plate, The λ / 4 plate satisfies any of the following formulas (3a), (3b), and (3c): nx3>ny3≒nz3 (3a) nx3>ny3>nz3 (3b) nx3>nz3>ny3 (3c) where nx3 represents the refractive index in an in-plane direction of the λ / 4 plate that gives the maximum refractive index, ny3 represents the refractive index in the in-plane direction of the λ / 4 plate that is perpendicular to the direction of nx3, and nz3 represents the refractive index in the thickness direction of the λ / 4 plate.

[0030] Here, the relationship ny1 ≒ nz1 means that |ny1 - nz1| is 0 or close to 0, and |ny1 - nz1| is preferably 0.1 or less, more preferably 0.05 or less, even more preferably 0.03 or less, and usually 0 or more and may be 0. Furthermore, the relationship ny2 ≒ nz2 means that |ny2 - nz2| is 0 or close to 0, and |ny2 - nz2| is preferably 0.1 or less, more preferably 0.05 or less, even more preferably 0.03 or less, and usually 0 or more and may be 0. Furthermore, the relationship ny3 ≒ nz3 means that |ny3 - nz3| is 0 or close to 0, and |ny3 - nz3| is preferably 0.1 or less, more preferably 0.05 or less, even more preferably 0.03 or less, and usually 0 or more and may be 0.

[0031] When the optical film is a multi-layer structure, in addition to the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate, an example of an optional retardation layer that may be further included in the optical film is a layer that functions as a so-called positive C plate. The positive C plate is a layer that satisfies nx4 ≒ ny4 < nz4. Here, nx4 represents the refractive index in the in-plane direction of the layer that gives the maximum refractive index, ny4 represents the refractive index in the in-plane direction of the layer that is perpendicular to the nx4 direction, and nz4 represents the refractive index in the thickness direction of the layer. The retardation layer that functions as a positive C plate can be arranged at any position in the multi-layer structure. In addition to the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate, if a retardation layer that functions as a positive C plate is included, the function of the optical film as a wideband quarter-wave plate can be improved, and the function as a wideband quarter-wave plate in the tilt direction can be improved in particular.

[0032] <1.3. In-plane birefringence of optical film> The in-plane birefringence Δn of an optical film is usually less than 0.008. The value of the in-plane birefringence Δn of the optical film can be calculated from the average value of the in-plane retardation at the curved surface portion and the thickness of the curved surface portion of the optical film. When the in-plane birefringence of the optical film is less than the upper limit, the optical film can be made thin. The lower limit of the in-plane birefringence of the optical film is not particularly limited, but may be, for example, 0.001 or more. The average value of the in-plane retardation at the curved surface portion can be determined by the method described below. The in-plane birefringence of the optical film can be adjusted, for example, by adjusting the type and weight fraction of the material forming the optical film, or by adjusting the stretching ratio.

[0033] <1.4. In-plane retardation value> The in-plane retardation value of the curved surface portion of the optical film is 95% to 105% of the average value of the in-plane retardation of the curved surface portion. That the in-plane retardation value of the curved surface portion is 95% to 105% of the average value of the in-plane retardation of the curved surface portion can be confirmed by the value of {maximum in-plane retardation value Re(max)−minimum in-plane retardation value Re(min)} / 2 being 5% or less of the average value of the in-plane retardation Re(ave) of the curved surface portion.

[0034] The in-plane retardation value and its average value in the curved portion can be measured, for example, by the following method. The in-plane retardation Re is measured for a region including the center C of the curved portion (e.g., a circular region with a radius of 25 mm) to obtain in-plane retardation mapping data. The in-plane retardation value can be measured using, for example, an offline birefringence measurement device ("KAMAKIRI-Offline" manufactured by Photron). The measurement wavelength can be 543 nm. In the obtained in-plane retardation mapping, the average values ​​of all five points, including the in-plane retardation value at point C, the in-plane retardation value at the intersection of the circumference of a circle with a radius of 10 mm and the diameter direction, and the in-plane retardation value at the intersection of the circumference of a circle with a radius of 20 mm and the diameter direction, are calculated for all directions centered on point C, and the direction with the largest average value is defined as the reference direction (0°). Next, the in-plane retardation values ​​are calculated for a total of 17 points as follows: The in-plane retardation value at point C. - In-plane retardation values ​​at four intersections of the reference direction with a circumference of a 10 mm radius and a circumference of a 20 mm radius, each centered at point C. - In-plane retardation values ​​at four intersections of a direction forming an angle of 45° with the reference direction with a circumference of a 10 mm radius and a circumference of a 20 mm radius, each centered at point C. - In-plane retardation values ​​at four intersections of a direction forming an angle of 90° with the reference direction with a circumference of a 10 mm radius and a circumference of a 20 mm radius, each centered at point C. - In-plane retardation values ​​at four intersections of a direction forming an angle of 135° with the reference direction with a circumference of a 10 mm radius and a circumference of a 20 mm radius, each centered at point C. The arithmetic mean value of the in-plane retardations at these 17 points can be used as the average value of the in-plane retardation in the curved surface portion. The maximum value among the 17 in-plane retardation values ​​can be set as the maximum in-plane retardation value Re(max) in the curved surface portion, and the minimum value can be set as the minimum in-plane retardation value Re(min) in the curved surface portion.

[0035] 1.5. Characteristics of Optical Film The optical film can be a film that imparts a predetermined in-plane retardation to incident light, such as a quarter-wave plate or a half-wave plate, depending on the in-plane retardation value of the curved surface portion. For example, the curved surface portion of the optical film can have an in-plane retardation value that can function as a quarter-wave plate. In one embodiment, the in-plane retardation value of the curved surface portion of the optical film is, where the measurement wavelength is λ nm, preferably within the range of (λ / 4±30) nm, more preferably within the range of (λ / 4±10) nm, and ideally λ / 4 nm. Here, the average value of the in-plane retardation value can be used as the in-plane retardation value of the curved surface portion of the optical film.

[0036] The optical film preferably functions as a quarter-wave plate in a broadband. The optical film being a broadband quarter-wave plate can be confirmed by the fact that the ellipticity in the front direction measured at a measurement wavelength of 450 nm, 550 nm, or 650 nm for a circular polarizing plate obtained by combining the optical film with a linear polarizer is 0.9 or more. The ellipticity is the value obtained by dividing the length of the minor axis of elliptically polarized light by the length of the major axis, and the closer the ellipticity is to 1 (i.e., circular polarization), the more preferable it is.

[0037] <1.6. Materials of Optical Film> The optical film contains a resin, and preferably consists of only a resin. The material resin of the optical film usually contains a polymer and optional components that may be included as needed. The material resin may be a resin having a positive intrinsic birefringence value or a resin having a negative intrinsic birefringence value, and is preferably a resin having a positive intrinsic birefringence value.

[0038] Here, unless otherwise specified, a resin with positive intrinsic birefringence means a resin whose refractive index in the stretching direction is greater than the refractive index in the direction perpendicular to the stretching direction. Furthermore, a material with negative intrinsic birefringence means a material whose refractive index in the stretching direction is smaller than the refractive index in the direction perpendicular to the stretching direction, unless otherwise specified. The value of intrinsic birefringence can be calculated from the dielectric constant distribution.

[0039] Examples of resins with positive intrinsic birefringence include resins containing cyclic olefin polymers (e.g., resins containing norbornene polymers), polyolefin resins, and polyethylene terephthalate (PET) resins. Examples of resins with negative intrinsic birefringence include polystyrene resins and polymethyl methacrylate resins.

[0040] The resin may be a crystalline resin having crystallinity, or an amorphous resin having no crystallinity. Here, "crystalline resin" means a resin having a melting point Tm. The melting point of the resin having a melting point Tm can be observed using a differential scanning calorimeter (DSC).

[0041] Examples of optional components include stabilizers such as antioxidants, heat stabilizers, light stabilizers, weather stabilizers, ultraviolet absorbers, and near-infrared absorbers; plasticizers; solvents; etc. These components may be used alone or in combination of two or more in any ratio.

[0042] The absolute value of the photoelastic coefficient of the resin is preferably low. The absolute value of the photoelastic coefficient of the resin forming the optical film is preferably 10×10 -13 cm 2 / dyn or less, more preferably 8 × 10 -13 cm 2 / dyn or less, more preferably 6 × 10 -13 cm 2 / dyn or less, more preferably 5 × 10 -13 cm 2 / dyn or less, more preferably 4×10 -13 cm 2 When an optical film is formed using a resin having a low absolute value of the photoelastic coefficient, the fluctuation in the retardation value when the resin is deformed by applying stress is small, and therefore, the retardation unevenness of the optical film can be effectively reduced.

[0043] 2. Manufacturing Method of Optical Film The optical film may be manufactured by any method. For example, the optical film may be manufactured by a manufacturing method including a step of preparing a film having an in-plane retardation and processing the film into a curved surface.

[0044] The curved surface processing of a film can be performed, for example, by fixing the film with a jig and pressing a mold having a desired curved surface against the film while heating it. This allows a curved surface portion having a curved surface corresponding to the curved surface of the mold to be formed on the film. When obtaining an optical film having a spherical curved surface portion, a mold having a spherical surface can be used.

[0045] As a mold having a spherical surface, a mold may be used in which the radius of curvature of the spherical portion pressed against the film is, for example, in the range of 130.75 mm ± 5 mm (corresponding to 4 curves), for example, in the range of 87.16 mm ± 5 mm (corresponding to 6 curves), or for example, in the range of 65.38 mm ± 5 mm (corresponding to 8 curves).

[0046] The heating temperature of the film in curved surface processing may be set appropriately depending on the glass transition temperature of the resin constituting the film, and is, for example, 60° C. or higher, for example, 70° C. or higher, for example, 75° C. or higher, and for example, 140° C. or lower, for example, 135° C. or lower, for example, 130° C. or lower. When a heated mold is used in curved surface processing, the heating temperature of the film usually matches the mold temperature.

[0047] The heating time of the film in the curved surface processing is, for example, 30 seconds or more and, for example, 90 seconds or less, as the time during which the mold is pressed against the film.

[0048] In the curved surface processing, the pressure with which the mold is pressed against the film is, for example, 0.1 MPa or more and, for example, 0.5 MPa or less.

[0049] Usually, when a film having in-plane retardation is spherically processed by, for example, pressing a mold having a spherical surface against the film, the film is stretched radially around the apex of the spherical surface of the mold.When the film is formed from a resin having a positive intrinsic birefringence value, usually, by stretching in the direction parallel to the in-plane slow axis direction of the film before curved processing and stretching in the direction perpendicular to the in-plane slow axis direction of the film, the in-plane retardation value becomes large in the direction corresponding to the in-plane slow axis direction of the film before curved processing, and the in-plane retardation value becomes small in the direction corresponding to the direction perpendicular to the in-plane slow axis direction of the film before curved processing.Therefore, even if the in-plane retardation value of the film before curved processing is uniform or nearly uniform, unevenness (retardation unevenness) may occur in the in-plane retardation value of the film after curved processing. On the other hand, when the film is formed from a resin having a negative intrinsic birefringence value, the stretching during curved processing reduces the in-plane retardation value in the direction corresponding to the in-plane slow axis direction of the film before curved processing, and increases the in-plane retardation value in the direction corresponding to the direction perpendicular to the in-plane slow axis direction of the film before curved processing.

[0050] Therefore, by previously setting a region of the film before curved surface processing, which corresponds to a region where the in-plane retardation value of the film after curved surface processing is smaller than that before curved surface processing, as a region having a high retardation value (high retardation region), it is possible to reduce retardation unevenness of the film after curved surface processing. An example of a manufacturing method based on such a mechanism will be described later as embodiment M1.

[0051] Alternatively, an optical film with reduced retardation unevenness can be obtained by increasing the in-plane retardation value of a region (low retardation region) in which the in-plane retardation value is smaller in the film after curved surface processing than before curved surface processing. An example of a manufacturing method based on such a mechanism will be described later as embodiment M2.

[0052] Alternatively, by using a film capable of reducing fluctuations in in-plane retardation caused by radial stretching during curved surface processing as a film for curved surface processing, an optical film with reduced retardation unevenness can be obtained. An example of a manufacturing method based on such a mechanism will be described later as embodiment M3.

[0053] 2.1. Embodiment M1 of the method for producing an optical film> Embodiment M1 of the method for producing an optical film of the present invention is a method for producing an optical film, comprising: a step of curved-processing a retardation film to obtain an optical film; the curved retardation film comprises high-retardation regions, the high-retardation regions are aligned in a direction perpendicular to an in-plane slow axis direction of the retardation film, and an in-plane retardation value of the high-retardation regions is 105% or more of the in-plane retardation value of the retardation film.

[0054] In the method for producing an optical film according to embodiment M1, a specific retardation film is curved to obtain an optical film. Hereinafter, the specific retardation film according to embodiment M1 is also referred to as a specific retardation film.

[0055] (Material of specific retardation film) The retardation film usually contains the same resin as the optical film after curved surface processing, and preferably contains only the same resin.The specific retardation film can effectively reduce retardation unevenness, so it is preferable to contain a resin with a positive intrinsic birefringence value, more preferably only a resin with a positive intrinsic birefringence value.Examples of resins with a positive intrinsic birefringence value that can form the specific retardation film include the above-mentioned examples, and among them, resins containing cyclic olefin polymers are preferred in terms of transparency, mechanical strength, moisture resistance, and low photoelastic coefficient.

[0056] As the cyclic olefin polymer, norbornene polymers are particularly preferred. Examples of norbornene polymers include ring-opening polymers of monomers containing a norbornene structure, ring-opening copolymers of monomers containing a norbornene structure with other monomers copolymerizable by ring-opening, and hydrogenated versions thereof; addition polymers of monomers containing a norbornene structure, and addition copolymers of monomers containing a norbornene structure with other monomers copolymerizable by ring-opening. Among these, from the viewpoint of transparency, hydrogenated ring-opening polymers of monomers containing a norbornene structure are particularly preferred. The cyclic olefin polymer can be selected from, for example, the polymers disclosed in JP 2002-321302 A and the polymers obtained by the production method disclosed in WO 2018 / 062067 A.

[0057] (High-Retardation Region Contained in Specific Retardation Film) The high-retardation region contained in the specific retardation film is a region in which the in-plane retardation value is 105% or more of the in-plane retardation value of the specific retardation film. Here, as the in-plane retardation value of the specific retardation film, the in-plane slow axis direction at point C, which is the center of the curved surface when the specific retardation film is curved, and the direction passing through point C may be defined as a reference direction (0 °), and an average value of the in-plane retardations at a plurality of points along the reference direction may be used.

[0058] FIG. 2 is a schematic diagram showing an example of a specific retardation film according to the present invention. The retardation film 100 has high retardation regions 100A1 and 100A2 aligned in a direction 100D2 passing through point C, which is perpendicular to the direction 100D1 of the in-plane slow axis. Point C is the point that becomes the center of the curved surface after curved surface processing. In this example, the point that becomes the center of the spherical surface when the retardation film 100 is spherically processed is shown. The dotted line 100E indicates a position corresponding to the periphery of the curved surface portion obtained after the retardation film is curved (in this example, spherical processing). In the example shown in FIG. 2, the high retardation regions 100A1 and 100A2 each have a fan-shaped or fan-like shape. In the example shown in FIG. 2, the high retardation regions 100A1 and 100A2 are two discontinuous regions separated near point C. In another embodiment, the high retardation regions 100A1 and 100A2 may be connected to form a single continuous region. For example, the high retardation regions 100A1 and 100A2 may be connected near point C to form a dumbbell shape. The high retardation region may also be two or more regions (for example, three or four). The shapes of the high retardation regions 100A1 and 100A2 viewed from a direction perpendicular to the surface of the retardation film 100 each have a line symmetry axis, and the line symmetry axis coincides with the direction 100D2. The high retardation regions 100A1 and 100A2 have a shape that is two-fold symmetric with a line passing through point C and perpendicular to the surface of the retardation film 100 as the rotation axis. In curved surface processing, a retardation film is usually stretched radially around the point C. Therefore, when the high retardation region has a shape of two-fold symmetry with a straight line passing through the point C and perpendicular to the plane of the retardation film as the axis of rotation, it is possible to reduce unevenness in the in-plane retardation value in the curved surface portion of the optical film obtained by curved surface processing the retardation film, thereby reducing retardation unevenness.

[0059] The specific retardation film may have a single-layer structure or a multi-layer structure.

[0060] As described above, the specific retardation film includes a high-retardation region, the high-retardation region is aligned in a direction perpendicular to the slow axis direction of the retardation film, and the in-plane retardation value of the high-retardation region is 105% or more of the in-plane retardation value of the retardation film. The specific retardation film is useful for obtaining an optical film with reduced retardation unevenness.

[0061] The manufacturing method according to embodiment M1 may further include a step of forming a high retardation region in a resin film having an in-plane retardation.

[0062] The in-plane retardation value of the resin film having an in-plane retardation may be set to a value corresponding to the desired in-plane retardation value of the optical film. When the optical film is used as a quarter-wave plate, the in-plane retardation value of the resin film is preferably in the range of (λ / 4±30) nm, more preferably in the range of (λ / 4±10) nm, and ideally λ / 4 nm, where λ is the measurement wavelength.

[0063] When the optical film is used as a broadband quarter-wave plate, it is preferable that the resin film also has an in-plane retardation value that allows it to function as a broadband quarter-wave plate.

[0064] As a resin film having an in-plane retardation, a stretched film is preferred because it is easy to manufacture. The manufacturing method of the stretched film is not particularly limited, and the resin material is formed into a film using any molding method such as melt extrusion or solution casting, and the obtained resin film is stretched to obtain a stretched film. Examples of the stretching method are not particularly limited, and include uniaxial stretching methods such as a method of uniaxially stretching a resin film in the longitudinal direction (longitudinal uniaxial stretching method) and a method of uniaxially stretching a resin film in the width direction (transverse uniaxial stretching method); biaxial stretching methods such as a simultaneous biaxial stretching method in which a resin film is stretched in the longitudinal direction and at the same time in the width direction, and a sequential biaxial stretching method in which a resin film is stretched in one of the longitudinal direction and the width direction and then stretched in the other direction; and a method of stretching a resin film in an oblique direction (oblique stretching method);

[0065] As an example of a process for forming a high retardation region in a resin film having an in-plane retardation, a process for using a stretched film as a resin film having an in-plane retardation will be described below.

[0066] In one embodiment, the method for producing an optical film further includes a step of contacting a region of the stretched film that is aligned in a direction perpendicular to an in-plane slow axis direction of the stretched film with a solvent to form the high retardation region, thereby obtaining the retardation film.

[0067] The region of the stretched film that is aligned in a direction perpendicular to the in-plane slow axis direction of the stretched film and that is brought into contact with the solvent is a region that corresponds to the high retardation region contained in the retardation film, and the shape and arrangement thereof can be the same as the shape and arrangement of the desired high retardation region.

[0068] By contacting a predetermined region of a stretched film with a solvent, the orientation of polymer molecules in that region is promoted, and the in-plane retardation value of the region of the stretched film contacted with the solvent can be made larger than that before the contact, resulting in a retardation film having a high retardation region formed.

[0069] As the solvent to be brought into contact with the stretched film, an organic solvent that does not easily dissolve the stretched film but can penetrate into the stretched film can be preferably used. The solvent may be a single solvent or a mixed solvent of two or more solvents. Examples of the solvent are not particularly limited, but include alicyclic hydrocarbon solvents such as cyclohexane and decalin; aromatic hydrocarbon solvents such as toluene, xylene, and tetralin; terpene solvents such as limonene; halogenated hydrocarbon solvents such as carbon tetrachloride; ether solvents such as tetrahydrofuran; and mixed solvents thereof.

[0070] The method for contacting the solvent with a predetermined region of the stretched film is preferably a coating method, and examples of the coating method include, but are not limited to, an inkjet method, a wire bar coating method, a spray method, a roll coating method, a gravure coating method, a die coating method, a curtain coating method, a slide coating method, and an extrusion coating method.

[0071] The in-plane retardation value in the high retardation region can be adjusted by appropriately adjusting contact conditions such as the type of solvent brought into contact with the stretched film, the time for which the solvent is brought into contact with the stretched film, the amount of solvent applied to the stretched film in the coating method, etc. For example, the in-plane retardation value of the high retardation region can be increased by increasing the thickness of the solvent layer formed on the stretched film in the coating method.

[0072] After contacting the solvent with the predetermined region of the stretched film, the stretched film is usually dried. Examples of the method for drying the solvent include, but are not limited to, natural drying, heat drying, drying under reduced pressure, and heat drying under reduced pressure.

[0073] The production method according to embodiment M1 may include any optional steps in addition to the steps described above. Examples of the optional steps include cutting the resulting optical film and drying the solvent.

[0074] 2.2. Embodiment M2 of the method for producing an optical film Embodiment M2 of the method for producing an optical film of the present invention is a method for producing an optical film, comprising: a step (1) of curvedly processing a first retardation film to obtain a second retardation film having a curved portion; and a step (2) of changing an in-plane retardation value in the curved portion of the second retardation film to obtain the optical film, wherein the curved portion of the second retardation film comprises low retardation regions aligned in a direction perpendicular to an in-plane slow axis direction of the curved portion; and the change in the in-plane retardation value in the step (2) is performed by increasing the in-plane retardation value of the low retardation regions by 5% or more.

[0075] (Step (1)) In step (1), the first retardation film is curved to obtain a second retardation film having a curved portion. As the first retardation film, a flat film having an in-plane retardation can be used. The first retardation film may have a single-layer structure or a multi-layer structure.

[0076] The first retardation film usually contains the same resin as the optical film after the curved surface processing, and preferably contains only the same resin. Preferred examples of the resin that can be contained in the first retardation film include the resins exemplified as the resin that can be contained in the specific retardation film in the above-mentioned embodiment M1.

[0077] The in-plane retardation value of the first retardation film may be a value corresponding to the desired in-plane retardation value of the optical film. When the optical film is used as a quarter-wave plate, the in-plane retardation value of the first retardation film is preferably in the range of (λ / 4±30) nm, more preferably in the range of (λ / 4±10) nm, where λ is the measurement wavelength, and is ideally λ / 4 nm.

[0078] When the optical film is used as a broadband quarter-wave plate, it is preferable that the first retardation film also has an in-plane retardation value that allows it to function as a broadband quarter-wave plate.

[0079] The first retardation film is preferably a stretched film because it is easy to produce. Examples of the method for producing a stretched film are the same as those described above.

[0080] The first retardation film is curved to obtain a second retardation film having a curved surface portion. Preferably, the curved surface portion of the second retardation film is curved to have the same dimensions and shape as the curved surface portion of the desired optical film.

[0081] (Step (2)) In step (2), an optical film is obtained by changing the in-plane retardation value in the curved portion of the second retardation film. The curved portion of the second retardation film includes a low retardation region. The low retardation region is aligned in a direction perpendicular to the in-plane slow axis direction of the curved portion. The low retardation region is a region having an in-plane retardation value that is less than 95% of the average in-plane retardation value in the curved portion of the second retardation film.

[0082] The shape of the low retardation region depends on the type of material constituting the first retardation film and the conditions for curved processing of the first retardation film, but usually has a shape of dyad symmetry with a straight line passing through point C, which is the center of curved processing, and perpendicular to the surface of the second retardation film as the axis of rotation. The low retardation region may be, for example, two or more discontinuous regions separated near point C, or two or more discontinuous regions may be connected to form one continuous region.

[0083] In the step (2), the in-plane retardation value in the curved portion is changed by increasing the in-plane retardation value of the low retardation region by 5% or more. The upper limit of the increase in the in-plane retardation value of the low retardation region is preferably set to 105% or less of the average in-plane retardation value of the curved portion of the obtained optical film.

[0084] An example of a method for increasing the in-plane retardation value of the low retardation region by 5% or more and changing the in-plane retardation value of the curved surface portion is to bring the low retardation region into contact with a solvent.

[0085] Examples of the solvent to be brought into contact with the low retardation region and the method for bringing the solvent into contact with the low retardation region include the same examples as those of the solvent to be brought into contact with the stretched film and the contact method thereof.

[0086] The degree of change in the in-plane retardation value in the low retardation region can be adjusted by appropriately adjusting contact conditions such as the type of solvent brought into contact with the low retardation region, the time for which the solvent is brought into contact with the low retardation region, the amount of solvent applied to the low retardation region in the coating method, etc. For example, by increasing the thickness of the solvent layer formed in the low retardation region in the coating method, the in-plane retardation value of the low retardation region can be changed to a higher value.

[0087] After contacting the low retardation region with the solvent, the second retardation film is usually dried. Examples of the method for drying the second retardation film include the same methods as those exemplified for drying the stretched film.

[0088] The production method according to embodiment M2 may include optional steps in addition to the steps described above. Examples of optional steps include the same optional steps as those included in the production method according to embodiment M1.

[0089] 2.3. Embodiment M3 of the method for producing an optical film Embodiment M3 of the method for producing an optical film of the present invention is a method for producing an optical film, comprising: a step of curve-processing a retardation film to obtain the optical film; wherein the retardation film is a multi-layer body having two or more retardation layers, and an angle formed by in-plane slow axes of each of two of the two or more retardation layers is 25° or more and 95° or less.

[0090] The retardation layer is a layer having at least an in-plane retardation, and may or may not have a retardation in the thickness direction. The retardation film may have three or more retardation layers, for example, four or more retardation layers. The retardation film may include any layer, such as an adhesive layer, in addition to the retardation layer.

[0091] The angle formed by the in-plane slow axes of each of the two retardation layers is preferably 15° or more, preferably 20° or more, more preferably 25° or more, and is preferably 96.5° or less, more preferably 95.5° or less, even more preferably 95.0° or less, and still more preferably 94.5° or less.

[0092] When the angle formed by the in-plane slow axes of each of the two retardation layers contained in the retardation film is within the above-mentioned range, by the radial stretching during curved surface processing, the in-plane slow axis direction of one retardation layer and the in-plane retardation value increase / decrease tendency along the direction passing through the center point C of curved surface processing, and the in-plane slow axis direction of the other retardation layer and the in-plane retardation value increase / decrease tendency along the direction passing through the point C coincide.As a result, in the direction in which the in-plane retardation value of one retardation layer decreases, the in-plane retardation value of the other retardation increases, and the increase and decrease of the in-plane retardation value of the entire multilayer body are offset.Therefore, it is possible to obtain an optical film with reduced retardation unevenness.

[0093] An example of a retardation film that can be used in embodiment M3 is a laminated body comprising a first λ / 2 plate, a second λ / 2 plate, and a λ / 4 plate in this order.Preferably, the angle between the slow axis of the first λ / 2 plate and the slow axis of the second λ / 2 plate is 24.6 ° or more and 30.6 ° or less, the angle between the slow axis of the first λ / 2 plate and the slow axis of the λ / 4 plate is 90.5 ° or more and 96.5 ° or less, the first λ / 2 plate satisfies any of the formulas (1a), (1b), and (1c), the second λ / 2 plate satisfies any of the formulas (2a), (2b), and (2c), and the λ / 4 plate satisfies any of the formulas (3a), (3b), and (3c).This laminated body can function well as a broadband λ / 4 plate.

[0094] Each of the two or more retardation layers included in the retardation film preferably contains a resin having a positive intrinsic birefringence value, and more preferably contains only a resin having a positive intrinsic birefringence value, since this can effectively reduce retardation unevenness. Examples and preferred examples of the resin having a positive intrinsic birefringence value that can be included in the retardation layer include the same examples as those listed as the materials for the specific retardation film.

[0095] In addition to the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate, an example of an optional retardation layer that may be further included in the retardation film is a layer that functions as a so-called positive C plate. The retardation layer that functions as a positive C plate can be disposed at any position in the retardation film.

[0096] 3. Uses of the Optical Film The optical film has a curved surface portion with reduced retardation unevenness, and therefore can be attached to an optical member (e.g., a lens) having a curved surface to form an optical element with excellent uniformity in desired optical properties.

[0097] <4. Circularly Polarizing Plate> The optical film can be suitably used as a component of a circularly polarizing plate. The circularly polarizing plate can include the optical film and a polarizer. The polarizer is usually a linear polarizer. A circularly polarizing plate including the optical film can convert linearly polarized light into circularly polarized light.

[0098] When the optical film is a film that can function as a quarter-wave plate, the angle between the transmission axis of the linear polarizer of the circular polarizing plate and the in-plane slow axis of the optical film is preferably 40° or more, more preferably 42° or more, even more preferably 43° or more, still more preferably 44° or more, and is preferably 50° or less, more preferably 47° or less, still more preferably 46° or less, and ideally 45°.

[0099] When the optical film is a multi-layer structure including a first λ / 2 plate, a second λ / 2 plate, and a λ / 4 plate in this order, the circularly polarizing plate including the multi-layer structure preferably includes a linear polarizer, a first λ / 2 plate, a second λ / 2 plate, and a λ / 4 plate in this order in the thickness direction. The angle between the absorption axis of the linear polarizer and the in-plane slow axis of the first λ / 2 plate is preferably 2 ° or more, more preferably 4 ° or more, and preferably 12 ° or less, more preferably 10 ° or less. Alternatively, the angle between the transmission axis of the linear polarizer and the slow axis of the first λ / 2 plate is preferably 29 ° or more, more preferably 31 ° or more, and preferably 40 ° or less, more preferably 38 ° or less.

[0100] Examples of the linear polarizer included in the circular polarizer are not particularly limited, and include an absorptive polarizer and a reflective polarizer.

[0101] An example of an absorptive polarizer is a polarizer that can be produced by a production method including a step of adsorbing a dichroic dye onto a polyvinyl alcohol-based resin film.

[0102] Examples of reflective polarizers include polarizers that are laminates of thin films with different birefringence; wire grid polarizers; and polarizers that are laminates of a layer having cholesteric regularity that has the function of separating left-handed circularly polarized light and a λ / 4 plate.

[0103] The circular polarizer according to the embodiment of the present invention has excellent uniformity in transmitted light intensity.

[0104] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be practiced with any modifications within the scope of the claims of the present invention and their equivalents.

[0105] In the following description, the "%" and "parts" that represent amounts are by weight unless otherwise specified. Furthermore, the operations described below were carried out at room temperature (20°C ± 15°C) and atmospheric pressure (1 atm) unless otherwise specified.

[0106] <Evaluation Method> (1. In-Plane Retardation Value and In-Plane Slow Axis Direction of Retardation Film and Optical Film) Using an offline birefringence measuring device (model: KAMAKIRI-offline) manufactured by Photoron Co., Ltd., the in-plane retardation Re values ​​of the retardation films and optical films obtained in the examples and comparative examples were evaluated by the following method. For laminated films, the in-plane retardation Re value was calculated by regarding the laminated films as a single film. The measurement wavelength was 543 nm, and the measurement temperature was 23°C.

[0107] (Retardation film before curved surface processing) An arbitrary point C of the retardation film was determined as the center position of the spherical portion after spherical processing. The in-plane retardation Re was measured for a circular region with a radius of 25 mm centered on point C to obtain in-plane retardation mapping data. The direction of the in-plane slow axis of the retardation film and passing through point C was determined as the reference direction (0 °), and the average of the in-plane retardation values ​​in the reference direction was taken as the in-plane retardation value of the retardation film before curved surface processing. In addition, the average of the in-plane retardation values ​​in a direction (90 °) passing through point C and perpendicular to the reference direction (0 °) was calculated.

[0108] (Retardation film and optical film after curved surface processing) The in-plane retardation Re was measured for a circular region of a radius of 25 mm centered on the center C of the curved surface (spherical portion) of the retardation film (second retardation film) or optical film after spherical processing, to obtain in-plane retardation mapping data. The in-plane retardation Re was measured by placing a spherical (dome-shaped) sample on a measuring device so that the top was convex. In the obtained in-plane retardation mapping, the average values ​​of all five points, including the in-plane retardation value at point C, the in-plane retardation value at the intersection of the circumference of a circle with a radius of 10 mm and the diameter direction, and the in-plane retardation value at the intersection of the circumference of a circle with a radius of 20 mm and the diameter direction, were calculated in all directions centered on point C, and the direction with the largest average value was defined as the reference direction (0 °). Next, the arithmetic average value Re (ave) of the in-plane retardation values ​​of a total of 17 points was calculated as follows. 3 is a schematic diagram showing the positional relationships of 17 points used to determine Re(ave) in Examples and Comparative Examples. - In-plane retardation value at point C. - In-plane retardation values ​​at four intersections of reference direction D0 with circumference CL1 of a 10 mm radius and circumference CL2 of a 20 mm radius, centered at point C. - In-plane retardation values ​​at four intersections of direction D45, which forms an angle of 45° with reference direction D0, with circumference CL1 of a 10 mm radius and circumference CL2 of a 20 mm radius, centered at point C. - In-plane retardation values ​​at four intersections of direction D90, which forms an angle of 90° with reference direction D0, with circumference CL1 of a 10 mm radius and circumference CL2 of a 20 mm radius, centered at point C. In-plane retardation values ​​at four intersections of a direction D135 forming an angle of 135° with the reference direction D0, a circumference CL1 having a radius of 10 mm, and a circumference CL2 having a radius of 20 mm, each centered at point C. The arithmetic average value Re(ave) of the determined in-plane retardation values ​​was taken as the average value of the in-plane retardation values ​​in the curved portion. The reference direction was taken as the direction of the in-plane slow axis of the retardation film or optical film after curved surface processing.

[0109] (2. Evaluation of Retardation Unevenness) The in-plane retardation values ​​of the optical film at 17 points in the method for evaluating the in-plane retardation value and the in-plane slow axis direction were calculated. The difference (Re(max)-Re(min)) between the maximum value Re(max) and the minimum value Re(min) was calculated, divided by the average value Re(ave) of the in-plane retardation values ​​at 17 points, and multiplied by 100 to calculate a percentage P(%), which was used for evaluating retardation unevenness. Percentage P(%)=(Re(max)-Re(min)) / Re(ave)×100 The smaller the value of percentage P, the more preferable. It can be said that the in-plane retardation value at the curved surface portion falls within a range of (-P / 2)% or more and (P / 2)% or less of Re(ave).

[0110] (3. Evaluation of Retardation Unevenness Using Polarizing Plate) A λ / 4 retardation plate was attached to a linear polarizing plate so that its in-plane slow axis was at a 45° angle with respect to the transmission axis of the linear polarizing plate to prepare a circular polarizing plate. The backlight, circular polarizing plate, spherically processed dome-shaped optical film sample, and linear polarizing plate were arranged in this order and observed. The polarizing plate on the viewing side with respect to the dome-shaped optical film sample was rotated, and the presence or absence of unevenness in light intensity was visually evaluated. If unevenness was not observed even after rotating the polarizing plate once, it was evaluated as "no unevenness." If unevenness was observed, the angle of the polarizing plate on the viewing side was adjusted to a position where unevenness was most noticeable, and the degree of unevenness was evaluated.

[0111] (4. Thickness) The thickness of each layer was measured using a film thickness measurement system (F20 manufactured by Filmetrics).

[0112] (5. In-Plane Birefringence Value) Using the method described above, the average value Re(ave) of the in-plane retardation in the curved portion of the optical film was determined, and divided by the thickness d of the optical film before curved surface processing (thickness excluding the thickness of the adhesive layer if the optical film includes an adhesive layer). It was assumed that the thickness at the center point C of the curved surface processing did not change before and after curved surface processing, and the obtained value Re(ave) / d was defined as the in-plane birefringence value Δn of the optical film.

[0113] (6. Photoelastic Coefficient) The photoelastic coefficient was measured by the following method. The resin material to be measured was fed into an extruder, passed through a polymer filter, and extruded into a sheet form from a T-die onto a casting drum. The extruded film was cooled to a thickness of 40 μm (in the case of a norbornene-based resin (ZEONOR1430 manufactured by ZEON CORPORATION)) or 35 μm (in the case of a norbornene-based resin (ZEONEX (registered trademark) C2420 manufactured by ZEON CORPORATION)). The extruded film thus obtained was cut into a 100 mm × 10 mm rectangle to obtain a test piece. The test piece was cut so that the long side was parallel to the film transport direction. Tensile loads of 0 g, 100 g, 200 g, 300 g, 400 g, 500 g, and 600 g were applied to the long side of the obtained test piece at 25° C., and the in-plane retardation was measured. The retardation in the in-plane direction was measured using an ellipsometer at a wavelength of 550 nm. The stress was calculated as the load per cross-sectional area of ​​the film, where d is the thickness of the film, and the photoelastic coefficient was calculated as the rate of change in Re(550) / d, which is the ratio of the retardation Re(550) in the in-plane direction to the thickness d, relative to the stress.

[0114] (7. Method for Calculating Ellipticity by Simulation) The ellipticity of the circular polarizing plate provided with the retardation film before the optical film was curved, manufactured in Example 1, was determined by simulation. The retardation film of the Example was modeled using "LCD Master" manufactured by Shintech Co., Ltd. as simulation software. In the simulation model, a structure was set in which the retardation film of the Example before the curved surface processing was attached to a linear polarizer as the circular polarizing plate. Therefore, in this model, the polarizer, the first λ / 2 plate of the retardation film, the second λ / 2 plate, and the λ / 4 plate were arranged in this order in the thickness direction, and a structure was set in which the absorption axis direction of the linear polarizer and the slow axis of the first λ / 2 plate provided in the retardation film formed an angle of 6.9°. Then, in the model, the ellipticity of light transmitted when the circular polarizing plate was irradiated with light from a D65 light source was calculated in the front direction. Here, calculations were performed at a polar angle of 0° in azimuth angle increments of 5° in the azimuth angle range of 0° to 360°, and the average of these calculated values ​​was used as the ellipticity in the front direction. Ellipticity is the amplitude of the minor axis of circular or elliptically polarized light divided by the amplitude of the major axis, and can take values ​​between 0 and 1. The closer the value is to 1, the more perfectly circular the light is, indicating excellent performance as a circular polarizer. The ellipticity was calculated at wavelengths of 450 nm, 550 nm, and 650 nm.

[0115] Example 1 (1-1. Production of COP (λ / 2)) A COP (λ / 2) half-wave plate was produced by the following procedure. Pellets of a norbornene resin (ZEONOR (registered trademark) 1430 manufactured by Zeon Corporation) were dried at 100°C for 5 hours. After drying, the pellets were fed into an extruder, passed through a polymer filter, and extruded into a sheet form from a T-die onto a casting drum. The sheet was then cooled to obtain an unstretched film with a thickness of 60 μm. This unstretched film was fed into a roll-type longitudinal stretching machine and subjected to a longitudinal uniaxial stretching treatment in which the film was stretched in the longitudinal direction at a temperature of 135°C and a magnification of 2.7 times, thereby obtaining a 35 μm-thick half-wave film (λ / 2 plate, COP (λ / 2)). The in-plane retardation value Re of the obtained half-wave film was 270 nm.

[0116] (1-2. Production of COP (λ / 4)) A quarter-wave plate, COP (λ / 4), was produced by the following procedure. In the production of COP (λ / 2), the extrusion conditions were changed. Except for the above, the same procedure as in the production of COP (λ / 2) was performed to obtain an unstretched film with a thickness of 42 μm. This unstretched film was supplied to a roll-type longitudinal stretching machine and subjected to a longitudinal uniaxial stretching treatment in which it was stretched in the longitudinal direction of the film at a temperature of 139°C and a magnification of 2.0 times, thereby obtaining a quarter-wave film (λ / 4 plate, COP (λ / 4)) with a thickness of 30 μm. The in-plane retardation value Re of the obtained quarter-wave film was 140 nm.

[0117] (1-3. Production of Retardation Film) Two sheets of the COP (λ / 2) produced in (1-1) above were used as the first λ / 2 plate and the second λ / 2 plate, respectively, and the COP (λ / 4) produced in (1-2) above was used as the λ / 4 plate, and an optical laminate was produced by the following procedure. Nitto Denko Corporation's pressure-sensitive adhesive sheet "CS9621" (a layer of acrylic pressure-sensitive adhesive) was used as the adhesive layer. First, the first λ / 2 plate and the second λ / 2 plate were bonded together via the adhesive layer to obtain an intermediate laminate. A λ / 4 plate was bonded to the surface of the second λ / 2 plate provided on the intermediate laminate via the adhesive layer to obtain an optical laminate as a retardation film for curved surface processing. The bonding was performed so that the angle between the first λ / 2 plate and the second λ / 2 plate was 27.6°, and the angle between the first λ / 2 plate and the λ / 4 plate was 93.5°.

[0118] (1-4. Curved Surface (Spherical) Processing) The end of the obtained retardation film was fixed with a circular jig, and a heated mold having a curved surface with 6 curves (radius of curvature 87.16 mm) was pressed against the center of the retardation film fixed with the circular jig from the first λ / 2 plate side of the retardation film. The mold was pressed so that the radius of the periphery of the curved surface portion was 50 mm and the height of the rise of the curved surface portion was 15.8 mm. The retardation film was pressed at 110 ° C. for 60 seconds to perform curved processing, thereby obtaining a film having a curved surface portion (spherical portion). The radius of curvature of the spherical portion corresponds to the radius of curvature of the mold and is approximately 87 mm. As a result, an optical film having a 50 mm radius of the periphery of the curved surface portion, which is a spherical surface, was obtained. The obtained optical film was evaluated by the above-mentioned method. The ellipticities of the retardation film at measurement wavelengths of 450 nm, 550 nm, and 650 nm determined by the above method were 0.99, 1.00, and 0.99, respectively, and the retardation film functioned as a quarter-wave plate in a wide band. Therefore, it was strongly inferred that an optical film obtained by curved processing of the retardation film also functions as a quarter-wave plate in a wide band.

[0119] Example 2 (2-1. Production of Crystalline COP (λ / 4)) Pellets of a crystalline norbornene-based resin (ZEON Corporation's "ZEONEX (registered trademark) C2420") were dried at 70°C for 5 hours. After drying, the pellets were fed into an extruder, passed through a polymer filter, and extruded into a sheet form from a T-die onto a casting drum. The sheet was then cooled to obtain an unstretched film having a thickness of 68 μm. This unstretched film was subjected to a fixed uniaxial stretching process using a batch stretching machine, stretching the film in the width direction at a temperature of 110°C and a stretching ratio of 1.5 to obtain a 1 / 4 wavelength film (crystalline COP (λ / 4)) having a thickness of 44 μm. The in-plane retardation value Re of the obtained 1 / 4 wavelength film was 120 nm.

[0120] (2-2. Formation of high retardation region) An arbitrary point C of the obtained flat quarter-wave film was determined as the position that would become the center of the spherical portion after spherical processing. With the direction of the in-plane slow axis of the film as the reference direction (0 °), from point C in a direction that forms 90 ° with the reference direction, the surface of the film was lightly traced with a Kimtowel (registered trademark) soaked in toluene, to the outside of a circle with a radius of about 50 mm centered at point C. Similarly, from point C, the direction that forms an angle of 75 ° with the reference direction, the direction that forms an angle of 105 ° with the reference direction, the direction that forms an angle of 60 ° with the reference direction, the direction that forms an angle of 120 ° with the reference direction, the direction that forms an angle of 45 ° with the reference direction, and the direction that forms an angle of 135 ° with the reference direction were traced in order. The film was then air-dried to obtain a retardation film for curved surface processing. When the in-plane retardation value Re of the obtained retardation film was measured, the average in-plane retardation value Re at points along the reference direction (0 °) was 120 nm, while the average in-plane retardation value Re at points along a direction forming an angle of 90 ° with the reference direction was 140 nm. Therefore, the in-plane retardation value of the retardation film was 120 nm. In the in-plane retardation mapping of the obtained retardation film, the region (high retardation region) of the in-plane retardation value of the retardation film of 105% (126 nm) or more was approximately coincident with the region contacted with toluene, and was two approximately fan-shaped.

[0121] (2-3. Curved Surface (Spherical Surface) Processing) In the above (1-4), the retardation film obtained in the above (2-2) was used as the retardation film. In addition, the press temperature was changed to 80°C. Except for the above, the same operation as in the above (1-4) was performed to obtain an optical film having a peripheral radius of a spherical curved surface portion of 50 mm. The obtained optical film was evaluated by the above method.

[0122] Example 3 (3-1. Production of crystalline COP (λ / 4)) In the same manner as in (2-1) above, a quarter-wave film (crystalline COP (λ / 4)) having the same properties as the quarter-wave film (crystalline COP (λ / 4)) obtained in (2-1) above was produced as a first retardation film.

[0123] (3-2. Curved Surface (Spherical Surface) Processing) In the above (1-4), the first retardation film obtained in the above (3-1) was used instead of the retardation film. In addition, the press temperature was changed to 80°C. Except for the above, the same operation as in the above (1-4) was performed to obtain a second retardation film having a peripheral radius of a spherical curved surface portion of 50 mm. The obtained second retardation film was evaluated by the above-mentioned method. The average in-plane retardation value Re at points along the reference direction (0°) was 131 nm, while the average in-plane retardation value Re at points along a direction forming an angle of 90° with the reference direction was 110 nm. The evaluation results are shown in Table 1 as the evaluation of the optical film in Comparative Example 2. From the mapping data of the in-plane retardation measured for the second retardation film, it was confirmed that the curved surface portion of the second retardation film has a low retardation region having an in-plane retardation value Re that is less than 95% (less than 114 nm) of the average value (120 nm) of the in-plane retardation value in the curved surface portion. The low retardation region was two approximately sector-shaped regions that were approximately symmetrical with respect to a line passing through the center C of the curved surface portion in a direction perpendicular to the in-plane slow axis direction (reference direction 0 °) in the curved surface portion of the second retardation film. The two approximately sector-shaped regions were aligned in a direction perpendicular to the in-plane slow axis direction in the curved surface portion of the second retardation film.

[0124] (3-3. Solvent Contact Step) The surface of the film was lightly traced with a Kimtowel (registered trademark) soaked in toluene from the center C of the curved surface of the obtained dome-shaped second retardation film in a direction that forms an angle of 90° with the reference direction (0°) to the outside of a circle with a radius of approximately 50 mm centered at the center C. In the same manner, from the center C, the film was traced in the following directions in order: a direction that forms an angle of 75° with the reference direction, a direction that forms an angle of 105° with the reference direction, a direction that forms an angle of 60° with the reference direction, a direction that forms an angle of 120° with the reference direction, a direction that forms an angle of 45° with the reference direction, and a direction that forms an angle of 135° with the reference direction. The film was then air-dried to obtain an optical film. The in-plane retardation value Re of the obtained optical film was measured, and the average in-plane retardation value Re at a point along the reference direction (0 °) was 131 nm, while the average in-plane retardation value Re at a point along a direction forming an angle of 90 ° with the reference direction was 126 nm. Therefore, the average in-plane retardation value Re at a point along a direction forming an angle of 90 ° with the reference direction included in the low retardation region of the second retardation film changed from 110 nm to 126 nm (an increase of 14.5% from 110 nm). The obtained optical film was evaluated by the above-mentioned method.

[0125] Comparative Example 1 In the above (1-4), the quarter-wave film (COP(λ / 4)) obtained in the above (1-2) was used as the retardation film. Except for this, the retardation film was subjected to curved processing in the same manner as in the above (1-4), to obtain an optical film having a spherical curved portion with a peripheral radius of 50 mm. The obtained optical film was evaluated by the above-mentioned method.

[0126] Comparative Example 2 As an optical film of Comparative Example 2, the second retardation film obtained in Example 3 (3-2) was evaluated by the above-mentioned method.

[0127] <Results> The results are shown in Table 1. In Table 1, the abbreviations have the following meanings: "COP": Amorphous norbornene-based resin ("ZEONOR (registered trademark) 1430" manufactured by Nippon Zeon Co., Ltd.) "Crystalline COP": Crystalline norbornene-based resin ("ZEONEX (registered trademark) C2420" manufactured by Nippon Zeon Co., Ltd.)

[0128]

[0129] From the above results, it can be seen that the optical films according to Examples 1 to 3, which have an in-plane birefringence Δn of less than 0.008 and a P / 2 of 5% or less, are free of unevenness when observed with a polarizing plate. On the other hand, the optical films according to Comparative Examples 1 and 2, which have a P / 2 of more than 5%, are found to have unevenness when observed with a polarizing plate.

[0130] REFERENCE SIGNS LIST 1 curved surface portion 1E peripheral edge 2 flat portion 10 optical film 100 retardation film C point 100D1 direction 100D2 direction 100A1 high retardation region 100A2 high retardation region CL1, CL2 circumference D0 reference direction D45, D90, D135 directions

Claims

1. An optical film having an in-plane birefringence of less than 0.008, having a curved surface portion, and an in-plane retardation value in the curved surface portion being 95% or more and 105% or less of the average value of the in-plane retardation in the curved surface portion.

2. The optical film according to claim 1, wherein the curved surface portion is spherical, and the radius of curvature of the spherical curved surface portion is 66 mm or more and 130 mm or less.

3. The optical film according to claim 1, wherein the curved surface portion functions as a quarter-wave plate.

4. The optical film according to claim 1, which is a multi-layered body and functions as a broadband quarter-wave plate.

5. A method for producing an optical film according to any one of claims 1 to 4, comprising a step of curved processing a retardation film to obtain an optical film, wherein the curved retardation film includes high retardation regions, the high retardation regions are aligned in a direction perpendicular to an in-plane slow axis direction of the retardation film, and the in-plane retardation value of the high retardation regions is 105% or more of the in-plane retardation value of the retardation film.

6. The method for producing an optical film according to claim 5, further comprising the step of contacting a region of the stretched film aligned in a direction perpendicular to the in-plane slow axis direction of the stretched film with a solvent to form the high retardation region, thereby obtaining the retardation film.

7. A method for producing an optical film according to any one of claims 1 to 4, comprising a step of obtaining an optical film by curved processing of a retardation film, wherein the retardation film to be curved is a laminate of two or more retardation layers, and an angle formed by in-plane slow axes of each of two of the two or more retardation layers is 25° or more and 95° or less.

8. A method for producing an optical film according to any one of claims 1 to 4, comprising: a step (1) of curvedly processing a first retardation film to obtain a second retardation film having a curved portion; and a step (2) of changing an in-plane retardation value in the curved portion of the second retardation film to obtain the optical film, wherein the curved portion of the second retardation film includes low retardation regions aligned in a direction perpendicular to an in-plane slow axis direction of the curved portion; and the change in the in-plane retardation value in the step (2) is carried out by increasing the in-plane retardation value of the low retardation regions by 5% or more.

9. The method for producing an optical film according to claim 8, wherein the in-plane retardation value is changed in the step (2) by contacting the low retardation region with a solvent.

10. A retardation film comprising a high retardation region, the high retardation region being aligned in a direction perpendicular to a slow axis direction of the retardation film, and an in-plane retardation value of the high retardation region being 105% or more of the in-plane retardation value of the retardation film.

11. A circularly polarizing plate comprising the optical film according to any one of claims 1 to 4 and a polarizer.

Citation Information

Patent Citations

  • Optical laminate, its manufacturing method, and luminance improved film

    JP2005037657A

  • Optical laminate and method for manufacturing broad-band circularly polarizing element

    JP2010033080A

  • Polarizing optical article with color irregularity improved

    JP2012215724A

  • Circular polarization lens for 3-d viewing, and glasses using the same

    JP2013020079A

  • Polarizing plate for curve surface and optical laminate

    JP2016200731A