Method for manufacturing surface-emitting semiconductor laser element, and surface-emitting semiconductor laser element

The method of forming a buried layer structure and annealing in a hydrogen atmosphere allows for closer proximity of the active and vacancy layers in surface-emitting semiconductor laser devices, enhancing the resonance effect and achieving high efficiency and low threshold currents.

WO2024203480A1PCT designated stage expired Publication Date: 2024-10-03KYOTO UNIV +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010328
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for manufacturing surface-emitting semiconductor laser devices with photonic crystals face challenges in enhancing the resonance effect and reducing the threshold current while maintaining high output efficiency, as they struggle to bring the vacancy layer and active layer close enough to achieve these goals.

Method used

A method involving the formation of a hole formation preparation layer, two-dimensionally arranged holes, facet growth to form a first buried layer, and a second buried layer that embeds the first buried layer, followed by hydrogen annealing to etch the second buried layer, allowing for closer proximity of the active layer to the void layer, thereby enhancing the resonance effect and achieving high efficiency.

Benefits of technology

This approach enables a surface-emitting semiconductor laser device with a high-quality active layer, low threshold value, and high efficiency by bringing the vacancy layer and active layer within 200 nm of each other, thereby increasing the resonance effect and output efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010328_03102024_PF_FP_ABST
    Figure JP2024010328_03102024_PF_FP_ABST
Patent Text Reader

Abstract

According to the present invention, (a) a hole formation preparation layer is formed on a substrate, (b) holes are formed in the hole formation preparation layer such that the holes are two-dimensionally arranged on lattice points, thereby forming a hole formation layer, (c) facet growth for plugging the holes is performed so as to form a first embedded layer, (d) a second embedded layer for embedding the first embedded layer flatly is grown so as to form a vacancy layer that has vacancies corresponding to the holes, (e) flat etching of the second embedded layer is performed by means of annealing in a hydrogen atmosphere, and (f) crystal growth of a semiconductor layer comprising an active layer is performed on the flat etched second embedded layer.
Need to check novelty before this filing date? Find Prior Art

Description

Surface-emitting semiconductor laser element manufacturing method and surface-emitting semiconductor laser element

[0001] The present invention relates to a method for manufacturing a surface-emitting semiconductor laser element having a photonic crystal, and to a surface-emitting semiconductor laser element.

[0002] In recent years, development of a photonic-crystal surface-emitting laser (PCSEL) using a photonic crystal (PC) has been progressing.

[0003] For example, Patent Document 1 proposes a method of embedding holes with a hexagonal columnar structure with side surfaces consisting of {10-10} in a group III nitride semiconductor layer using facet selective growth in order to enhance the diffraction effect in the hole layer in a photonic crystal laser and obtain a high resonance effect. It describes how this method realizes a photonic crystal laser element equipped with a photonic crystal having a large filling factor and a large optical confinement coefficient.

[0004] Furthermore, Patent Document 2 proposes a method for embedding holes in a group III nitride semiconductor layer using mass transport in a photonic crystal laser, and describes how this method results in a photonic crystal laser with a large coupling coefficient for light waves propagating through the photonic crystal layer.

[0005] Japanese Patent No. 7101370 Japanese Patent Application Laid-Open No. 2020-38892

[0006] However, when the technique described in Patent Document 1 is used, although a hole layer with a sufficient hole filling rate can be formed, the layer thickness for embedding the hole layer becomes thick, and the distance between the hole layer and the active layer cannot be reduced, which means that the resonance effect in the hole layer cannot be enhanced.

[0007] Furthermore, Patent Document 2 proposes a hole filling method using mass transport, but when this method is used, the holes are filled with a columnar structure, i.e., a regular hexagonal columnar structure, which has the most thermally stable cross-sectional shape. Therefore, it is difficult to introduce asymmetry into the cross-sectional shape of the holes, and high extraction efficiency cannot be obtained. In other words, high-power operation is not possible.

[0008] For these reasons, it has been difficult in the prior art to increase the resonance effect and lower the threshold current while maintaining a high output.

[0009] An object of the present invention is to provide a surface-emitting semiconductor laser device that can enhance the resonance effect by bringing the air hole layer and the active layer close to each other, has a high-quality active layer, has a low threshold value, and is highly efficient, and to provide a manufacturing method for the surface-emitting semiconductor laser device.

[0010] A method of manufacturing a surface-emitting semiconductor laser element according to one embodiment of the present invention includes: forming a hole formation preparation layer on a substrate; forming holes in the hole formation preparation layer, which are two-dimensionally arranged at each of the lattice points, to form a hole formation layer; forming a first burying layer by facet growth that closes the holes; growing a second burying layer that flatly buries the first burying layer to form a void layer having voids corresponding to the holes; flattening the second burying layer by annealing in a hydrogen atmosphere; and performing crystal growth of a semiconductor layer including an active layer on the flat-etched second burying layer.

[0011] A surface-emitting semiconductor laser element according to one embodiment of the present invention is a surface-emitting semiconductor laser element manufactured by the above manufacturing method, in which the distance between the active layer and the hole layer is 200 nm or less.

[0012] 1B is a cross-sectional view schematically showing an example of the structure of a PCSEL device according to a first embodiment; FIG. 1C is an enlarged cross-sectional view schematically showing holes arranged in the hole layer shown in FIG. 1A; FIG. 1D is a plan view schematically showing the top surface of a PCSEL device; FIG. 1E is a cross-sectional view schematically showing a cross section in a plane parallel to the n-side guide layer; FIG. 1F is a plan view schematically showing the bottom surface of a PCSEL device; FIG. 1G is a flowchart showing a method for manufacturing a PCSEL device according to a first embodiment; FIG. 1H is a cross-sectional view schematically showing a cross section of an n-side guide layer in steps S0 to S3 of forming a buried layer; FIG. 1J is a plan view schematically showing main and sub-openings in a resist, and main and sub-holes after etching; FIG. 1J is a diagram schematically showing a cross section perpendicular to the central axis CX of a formed hole layer; FIG. 1I is an SEM image of a cross section of a wafer when the etching time is (i) 5 minutes; FIG. 1J is an SEM image of a cross section of a wafer when the etching time is (ii) 20 minutes; FIG. 1J is an SEM image of a cross section of a wafer when the etching time is (iii) 50 minutes; and FIG. 1J is an AFM image of the surface of an active layer. 1A and 1B are diagrams showing the results of measuring the surface roughness when the etching time is (ii) 20 minutes, (iii) 50 minutes, and (iv) 50 minutes, respectively. 1A and 1B are diagrams showing the measured values ​​of the surface roughness Ra of a 20 μm×20 μm area versus the layer thickness of the buried layer.

[0013] In the following, preferred embodiments of the present invention will be described, but these may be modified and combined as appropriate. In the following description and accompanying drawings, substantially the same or equivalent parts are designated by the same reference numerals.

[0014] [First Embodiment] 1. Structure of Photonic Crystal Surface-Emitting Laser Element A photonic crystal surface-emitting laser element (PCSEL element) is a surface-emitting semiconductor laser element that has a resonator layer in a direction parallel to semiconductor light-emitting structure layers (n-side guide layer, light-emitting layer, p-side guide layer) that constitute a light-emitting element, and emits coherent light in a direction perpendicular to the resonator layer.

[0015] That is, in a PCSEL element, light waves propagating in a plane parallel to the air hole layer (photonic crystal layer) are diffracted by the diffraction effect of the photonic crystal to form a two-dimensional resonance mode, and are also diffracted in a direction perpendicular to the parallel plane. That is, in a PCSEL element, the light extraction direction is perpendicular to the resonance direction (in the plane parallel to the air hole layer).

[0016] Fig. 1A is a cross-sectional view schematically illustrating an example of the structure of a photonic crystal surface-emitting laser device (PCSEL device) 10 according to an embodiment of the present invention, and Fig. 1B is an enlarged cross-sectional view schematically illustrating an air hole layer 14P and air holes 14K arranged in the air hole layer 14P in Fig. 1A.

[0017] 2A is a plan view schematically showing the upper surface of the PCSEL device 10. Also, Fig. 2B is a cross-sectional view schematically showing a cross section of the hole layer 14P in a plane parallel to the n-side guide layer 14, and Fig. 2C is a plan view schematically showing the lower surface of the PCSEL device 10. As shown in Fig. 1A, a semiconductor structure layer 11 is formed on a light-transmitting device substrate 12. The semiconductor layers are stacked perpendicular to the central axis CX of the semiconductor structure layer 11.

[0018] The semiconductor structure layer 11 is made of a hexagonal nitride semiconductor, for example, a GaN-based semiconductor, in this embodiment.

[0019] More specifically, a semiconductor structure layer 11 consisting of a plurality of semiconductor layers is formed on an element substrate 12, in this order: an n-clad layer (first clad layer of a first conductivity type) 13; an n-side guide layer (first guide layer) 14 which is a guide layer provided on the n-side; a light distribution adjustment layer 23; an active layer (ACT) 15; a p-side guide layer (second guide layer) 16 which is a guide layer provided on the p-side; an electron barrier layer (EBL: Electron Blocking Layer) 17; a p-clad layer (second clad layer of a second conductivity type) 18; and a p-contact layer 19.

[0020] Although the case where the first conductivity type is n-type and the second conductivity type opposite to the first conductivity type is p-type will be described, the first conductivity type and the second conductivity type may be p-type and n-type, respectively.

[0021] The element substrate 12 is a hexagonal GaN single crystal substrate that has a high transmittance for light emitted from the active layer 15. More specifically, the element substrate 12 is a hexagonal GaN single crystal substrate whose main surface (crystal growth surface) is a +c plane, which is a {0001} plane in which Ga atoms are arranged on the outermost surface. The back surface (light emission surface) is a -c plane, which is a (000-1) plane in which N atoms are arranged on the outermost surface. The -c plane is suitable as a light emission surface because it is resistant to oxidation and the like.

[0022] Although the element substrate 12 is not limited to this, a so-called just substrate or, for example, a substrate whose main surface is offset by about 1° in the m-axis direction is preferable. For example, a substrate whose main surface is offset by about 0.3 to 0.7° in the m-axis direction can obtain mirror-finish growth under a wide range of growth conditions.

[0023] The rear surface of the substrate opposite to the main surface is the light emitting surface, which is the "-c" plane, which is the (000-1) plane with N atoms arranged on the outermost surface. The -c plane is resistant to oxidation and is therefore suitable as a light extraction surface.

[0024] The composition, thickness, and other configurations of each semiconductor layer will be explained below, but these are merely examples and can be modified as appropriate.

[0025] The n-clad layer 13 is, for example, n-Al having an Al composition of 4%. 0.04 Ga 0.96 The aluminum (Al) composition ratio is set so that the refractive index is smaller than that of the layer adjacent to the active layer 15 (i.e., the n-side guide layer 14).

[0026] The n-side guide layer 14 is composed of a lower guide layer 14A, an air-hole layer (or PC layer) 14P, which is a photonic crystal layer, and a buried layer 14B. As shown in FIG. 1B, the air-hole layer 14P has a thickness d PC The buried layer 14B has a thickness D. For example, the hole layer 14P has a thickness d PC is 40 to 180 nm.

[0027] In this specification, the air hole layer 14P refers to a layer portion of the n-side guide layer 14 extending from the upper end to the lower end of the air holes 14K (see FIG. 1B). PC is equal to the height of the hole.

[0028] The lower guide layer 14A is made of n-GaN and has a thickness of 100 to 400 nm, for example. The air hole layer 14P is made of n-GaN and has a thickness (or the height of the air holes 14K) of 40 to 180 nm.

[0029] The buried layer 14B is made of n-GaN or n-InGaN, or undoped GaN or undoped InGaN. Alternatively, it may be a layer in which these semiconductor layers are stacked. The layer thickness D of the buried layer 14B is, for example, 30 to 150 nm. The buried layer 14B is made of a first buried layer 14B1 and a second buried layer 14B2. In other words, the buried layer 14B is a stacked buried layer in which the second buried layer 14B2 is stacked on the first buried layer 14B1.

[0030] On the second buried layer 14B2, which is the surface layer of the buried layer 14B, there is provided a light distribution adjustment layer 23, which is a hetero semiconductor layer (dissimilar semiconductor layer) that has a different crystal composition from that of the second buried layer 14B2 and forms a hetero structure with the second buried layer 14B2.

[0031] The light distribution-adjusting layer 23 may be a semiconductor layer of the same conductivity type as the second buried layer 14B2, or at least one of them may be an i-layer (intrinsic semiconductor layer).

[0032] The light distribution adjustment layer 23 is provided between the buried layer 14B and the active layer 15, and has the function of adjusting the coupling efficiency between the light propagating in the hole layer 14P and the hole layer 14P acting as a resonator.

[0033] In this embodiment, the light distribution adjustment layer 23 is made of undoped In. 0.03 Ga 0.97 The light distribution adjustment layer 23 is an N layer, and has a thickness of, for example, 50 nm. The thickness of the light distribution adjustment layer 23 is selected depending on the composition or refractive index of the light distribution adjustment layer 23 and the adjustment of the coupling efficiency.

[0034] The n-side semiconductor layer including the n-side guide layer 14 and the light distribution-adjusting layer 23 is also referred to as a first semiconductor layer, but the light distribution-adjusting layer 23 does not necessarily have to be provided.

[0035] The active layer 15, which is a light-emitting layer, is a multiple quantum well (MQW) layer having, for example, two quantum well layers. The barrier layer and quantum well layer of the MQW are made of GaN (layer thickness 6.0 nm) and InGaN (layer thickness 4.0 nm), respectively. The central emission wavelength of the active layer 15 is 440 nm.

[0036] The active layer 15 is preferably disposed within 180 nm of the hole layer 14P (i.e., within the period PK of the holes 14K). In this case, a high resonance effect can be obtained by the hole layer 14P.

[0037] The p-side guide layer 16 is an undoped In 0.02 Ga 0.98 It consists of a p-side guide layer (1) 16A which is an N layer (layer thickness 70 nm) and a p-side guide layer (2) 16B which is an undoped GaN layer (layer thickness 180 nm).

[0038] The p-side guide layer 16 is an undoped layer in consideration of light absorption by a dopant (Mg: magnesium, etc.), but may be doped to obtain good electrical conductivity. In addition, the In composition and layer thickness of the p-side guide layer (1) 16A can be appropriately selected to adjust the electric field distribution in the oscillation operation mode.

[0039] The electron barrier layer (EBL) 17 is a p-type Al doped with magnesium (Mg). 0.2 Ga 0.8 The N layer has a thickness of, for example, 15 nm.

[0040] The p-cladding layer 18 is made of Mg-doped p-Al 0.06 Ga 0.94 The p-cladding layer 18 is an N layer having a thickness of, for example, 600 nm. The Al composition of the p-cladding layer 18 is preferably selected so that the refractive index is smaller than that of the p-side guide layer 16. The p-cladding layer 18 functions as a first p-cladding layer.

[0041] The p-contact layer 19 is an Mg-doped p-GaN layer having a thickness of, for example, 20 nm. The carrier density of the p-contact layer 19 is set to a concentration that allows for ohmic contact with the transparent electrode 29, which is a transparent conductive layer provided on the surface of the p-contact layer 19. Instead of p-type GaN, p-type or undoped InGaN may be used. Alternatively, a layer in which a GaN layer and an InGaN layer are stacked may be used.

[0042] The layer consisting of the p-side guide layer 16, the electron barrier layer 17, the p-cladding layer 18 and the p-contact layer 19 is also referred to as a second semiconductor layer.

[0043] In this specification, the terms "n-side" and "p-side" do not necessarily mean n-type and p-type. For example, an n-side guide layer refers to a guide layer provided on the n-side of the active layer, and may be an undoped layer (or i-layer).

[0044] The n-cladding layer 13 may be composed of multiple layers instead of a single layer, and in that case, all layers do not need to be n-layers (n-doped layers) and may include an undoped layer (i-layer). The same applies to the p-side guide layer 16 and the p-cladding layer 18.

[0045] Furthermore, it is not necessary to provide all of the semiconductor layers described above, and it is sufficient to have a configuration having a first semiconductor layer of a first conductivity type, a second semiconductor layer of a second conductivity type, and an active layer (light-emitting layer) sandwiched between these layers.

[0046] Furthermore, in this embodiment, the case where the void layer 14P is provided in the first semiconductor layer (n-type semiconductor layer) has been described, but the void layer may also be provided in the second semiconductor layer (p-type semiconductor layer). On the p-contact layer 19, a p-electrode 20B (second electrode) is formed as a transparent electrode / Ag / Au layer, in which a transparent electrode 29 (not shown), a silver (Ag) layer, and a gold (Au) layer are stacked in this order. That is, the p-electrode 20B functions as a light-reflecting layer, and the interface between the transparent electrode 29 and the Ag layer of the p-electrode 20B is a reflective surface SR. The reflective surface SR is provided parallel to the void layer 14P.

[0047] The p-electrode 20B has a circular shape with a diameter RA centered on the central axis CX of the void formation region 14R. Specifically, the translucent electrode 29 has a diameter RA of, for example, 300 μm in top view (i.e., when viewed from a direction perpendicular to the semiconductor structure layer 11).

[0048] The p-electrode 20B may also be made of Pd, Al, an Al alloy, etc. A pad electrode or the like may be provided on the p-electrode 20B.

[0049] The transparent electrode 29 is formed of a transparent conductor, such as indium tin oxide (ITO). Note that the transparent electrode 29 is not limited to ITO, and other transparent conductors such as zinc tin oxide (ZTO), GZO (ZnO:Ga), and AZO (ZnO:Al) can be used.

[0050] The side and top surfaces of the semiconductor structure layer 11 and the side surfaces of the p-electrode 20B are made of SiO 2 The insulating film 21 is formed so as to overlap the p-electrode 20B and cover the edge of the upper surface of the p-electrode 20B.

[0051] The insulating film 21 also functions as a protective film, protecting the aluminum (Al)-containing crystal layer that constitutes the PCSEL element 10 from corrosive gases and the like. It also prevents short circuits caused by deposits or solder creeping up during mounting, contributing to improved reliability and yield. The insulating film 21 is made of SiO 2 Not limited to ZrO 2 , HfO 2 , TiO 2 , Al 2 O 3 , SiNx, etc. can be selected.

[0052] A circular cathode electrode 20A (first electrode) (see FIG. 2C) is formed on the rear surface of the element substrate 12. An anti-reflection (AR) coating layer 27 is formed on the inner surface of the cathode electrode 20A.

[0053] The cathode electrode 20A is made of Ti / Au and is in ohmic contact with the element substrate 12. In addition to Ti / Au, the electrode material can be selected from Ti / Al, Ti / Rh, Ti / Al / Pt / Au, Ti / Pt / Au, and the like.

[0054] The light emitted from the active layer 15 is diffracted by the air hole layer (PC layer) 14P. The light is diffracted by the air hole layer 14P (diffraction surface WS), and the light directly emitted from the air hole layer 14P (direct diffracted light Ld: first diffracted light) and the light diffracted by the air hole layer 14P and reflected by the reflection surface SR (reflected diffracted light Lr: second diffracted light) are emitted to the outside from a light emission region 20L ( FIG. 2C ) on the rear surface (emission surface) 12R of the element substrate 12.

[0055] 2B, in the hole layer 14P, the holes 14K are periodically arranged within, for example, a rectangular hole-forming region 14R. As shown in FIG. 2C, the anode region RA is formed so as to be included within the hole-forming region 14R.

[0056] The cathode electrode 20A is provided as a ring-shaped electrode outside the p-electrode 20B so as not to overlap the p-electrode 20B when viewed from a direction perpendicular to the pore layer 14P.

[0057] The region inside the cathode electrode 20A is a light emitting region 20L. Also provided is a bonding pad 20C that is electrically connected to the cathode electrode 20A and to which a wire for supplying power from an external source is connected.

[0058] 2. Manufacturing Method of Hole Layer and Recrystallization Growth The manufacturing process of the hole layer and recrystallization growth are described below. Metalorganic Vapor Phase Epitaxy (MOVPE) was used as the crystal growth method. Note that the following describes the formation method using the case where the hole layer 14P is a double-lattice photonic crystal layer as an example, but single-lattice photonic crystal layers and multi-lattice photonic crystal layers can also be formed in the same way.

[0059] (a) Manufacturing Flow Fig. 3 is a flowchart showing a manufacturing method of the PCSEL device 10. Below, with reference to Fig. 3, a detailed description will be given of the process of manufacturing the PCSEL device 10 by forming air holes in the vacancy layer by filling the recesses (holes) with growth, and then growing the active layer and p-side guide layer.

[0060] 4 is a cross-sectional view schematically showing the cross section of the n-side guide layer 14 in steps S0 to S3 of forming the buried layer 14B. For ease of explanation and understanding, Fig. 4 illustrates a case where the hole layer 14P is a single-lattice photonic crystal layer, but a multi-lattice photonic crystal layer can also be formed in the same manner.

[0061] The buried layer 14B (laminated buried layer) formed on the air-holes by recrystallization growth will be described in detail below with reference to FIGS.

[0062] (Step S0) Formation of Holes First, an n-type Al layer having an Al composition of 4% is formed on the element substrate 12 as the n-clad layer 13. 0.04 Ga 0.96 An N layer was grown on the n-cladding layer 13. Subsequently, a hole formation preparation layer 14E, which is an n-type GaN layer, was grown on the n-cladding layer 13. This hole formation preparation layer 14E is a preparation layer for forming the lower guide layer 14A and the hole layer 14P containing the holes 14K. The hole formation preparation layer 14E has a surface (upper surface) consisting of a flat (0001) plane.

[0063] After forming the hole formation preparation layer 14E, the substrate was removed from the chamber of the MOVPE apparatus, and fine recesses (holes) were formed on the surface of the growth layer. After obtaining a clean surface by cleaning, a silicon nitride film (SiN x A resist for electron beam lithography was applied thereon, and the substrate was placed in an electron beam lithography system to pattern a two-dimensional periodic structure.

[0064] 5 is a plan view schematically showing the main opening K1 and sub-opening K2 in the resist, and the main hole 14H1 and sub-hole 14H2 after etching. As shown in FIG. 5, a pattern was performed in which pairs of openings, each consisting of an oval-shaped main opening K1 and a sub-opening K2 smaller than the main opening K1, were two-dimensionally arranged in the plane of the resist in a square lattice pattern with a period PK. Note that for clarity of the drawing, the openings are shown hatched.

[0065] More specifically, the main apertures K1 are arranged two-dimensionally with their centers of gravity CD1 in two mutually orthogonal directions (x direction and y direction) on lattice points of a square lattice with a period P K. Similarly, the sub-apertures K2 are arranged two-dimensionally with their centers of gravity CD2 in the x direction and y direction on lattice points of a square lattice with a period P K.

[0066] The major axes of the main aperture K1 and the sub aperture K2 are parallel to the <11-20> direction of the crystal orientation, and the minor axes of the main aperture K1 and the sub aperture K2 are parallel to the <1-100> direction.

[0067] The center of gravity CD2 of the sub-opening K2 is spaced apart from the center of gravity CD1 of the main opening K1 by Δx and Δy. Here, Δx=Δy. That is, the center of gravity CD2 of the sub-opening K2 is spaced apart from the center of gravity CD1 of the main opening K1 in the <1-100> direction.

[0068] The distance Δx, Δy between the centers of gravity of the main opening K1 and the sub-opening K2 was set to Δx=Δy=0.46PK. After the patterned resist was developed, SiN x The film was selectively dry-etched to form main openings K1 and sub-openings K2 arranged two-dimensionally on the lattice points of a square lattice with a period PK. x formed to penetrate the membrane.

[0069] The period (hole spacing) PK was set to PK=177.5 nm in order to set the oscillation wavelength (λ) to 438 nm.

[0070] Subsequently, the resist is removed, and the patterned SiN xUsing the film as a hard mask, recesses (holes) were formed in the GaN surface. The GaN was dry-etched in the depth direction using a chlorine-based gas and argon gas in an ICP-RIE apparatus, thereby forming a main hole 14H1 and a sub-hole 14H2, which were oblong cylindrical recesses dug perpendicular to the GaN surface.

[0071] The recesses dug in the surface portion of the hole formation preparation layer 14E (GaN) by the above etching are simply referred to as holes to distinguish them from air holes in the void layer 14P. When there is no particular need to distinguish between the main holes 14H1 and the sub-holes 14H2, they may be referred to as holes 14H.

[0072] The shape of the hole 14H is not limited to an elongated cylindrical shape, but may be a cylindrical shape, a polygonal shape, or the like.

[0073] As a result of the above, holes 14H were formed in the hole formation preparation layer 14E, and a hole formation layer 14J was formed (FIG. 4, S0).

[0074] (Step S1) Hole Closure - First Burying Growth First, the substrate (FIG. 4, SO) with the hole 14H formed therein was cleaned, and then it was introduced back into the reactor of the MOVPE apparatus to perform recrystallization growth. Specifically, ammonia (NH) and trimethylgallium (TMG) were supplied to perform the first burying growth by facet growth, and the opening of the hole 14H was closed.

[0075] Specifically, the first burying growth was performed at a first temperature (920° C.) at which the shape of the hole 14H was transformed by mass transport into a shape composed of thermally stable surfaces.

[0076] More specifically, in this first temperature region, N atoms are attached to the outermost surface of the growth substrate, so that N-polar faces are selectively grown. Therefore, as shown in FIG. 4, crystals with {1-101} facets are selectively grown. When the opposing {1-101} facets collide, the holes 14H are blocked and filled (facet growth). This facet growth results in first filling growth, and vacancies 14K are formed corresponding to the holes 14H. Note that the hole-forming layer 14J (GaN layer) before the filling layer 14B is formed is indicated by a dashed line in FIG. 4.

[0077] (Step S2) Planarization Filling - Second Filling Growth Next, the hole 14H was closed by facet growth, and then a second filling layer 14B2 with a thickness D2 of 50 nm was grown. The second filling layer 14B2 was grown by raising the substrate temperature (growth temperature) to 1050°C (second filling temperature) and then supplying triethylgallium (TEG) and NH3. The second filling temperature was higher than the first filling temperature. However, the temperature relationship between the second filling temperature and the first filling temperature may be reversed as long as the growth surface of the second filling layer 14B2 can be grown to a (0001) plane.

[0078] 4, a second buried layer 14B2 having a (0001) plane at its surface is formed by a thermal effect to generate mass transport, and a second buried layer 14B2 is formed by the first and second buried layer growth processes.

[0079] For ease of explanation, the layer extending from the upper surface of the void layer 14P (the surface closer to the active layer 15) to the upper surface 14JS of the hole-forming layer 14J (including a part of the hole-forming layer 14J) is referred to as the first buried layer 14B1, and the layer extending from the upper surface 14JS of the hole-forming layer 14J to the flat surface formed by the second buried growth is referred to as the second buried layer 14B2 (see S3 in FIG. 4).

[0080] The entire semiconductor layer from the upper surface of the void layer 14P to the upper surface of the second buried layer 14B2 (including a part of the hole-forming layer 14J) is referred to as the buried layer 14B.

[0081] Here, the thickness of the first buried layer 14B1 is defined as D1, and the thickness of the second buried layer 14B2 is defined as D2. Therefore, the thickness of the buried layer 14B is given by D = D1 + D2. In this specification, the "top surface" of each semiconductor layer of the n-side guide layer (first guide layer) 14 refers to the surface closer to the active layer 15.

[0082] In this embodiment, GaN is used for the second burying growth. The second burying layer 14B2 also functions as a light distribution adjusting layer for adjusting the coupling efficiency (light field) between light and the hole layer 14P.

[0083] That is, in this embodiment, undoped GaN is used for the first buried growth and the second buried growth, but the first buried growth and the second buried growth are not limited to GaN, and n-GaN, n-InGaN, undoped GaN, undoped InGaN, or a combination of these semiconductors can also be used.

[0084] (Step S3) H 2 Etching by annealing. Then, hydrogen (H 2 5 shows the second buried layer 14B2 after being etched flat by a thickness TE from its surface.

[0085] More specifically, H 2 In annealing in an atmosphere, the (0001) plane is a thermally stable plane, and the buried layer 14B can be etched and thinned while maintaining the flatness of the surface. Therefore, a high-quality active layer with high flatness can be grown on the buried layer 14B. The annealing atmosphere may contain Group III and Group V materials.

[0086] More specifically, in the case of a group III nitride semiconductor, H 2High-temperature annealing in a high-temperature atmosphere causes surface atoms to be desorbed, resulting in etching of the surface. Since the surface with the slowest etching rate remains, the most thermally stable (0001) plane is formed on the surface. Therefore, when a +c-plane substrate is used, etching can be performed while maintaining the (0001) plane parallel to the substrate. This allows the second buried layer 14B2 to be made thinner, thereby reducing the distance between the vacancy layer 14P and the active layer 15.

[0087] H in Group III nitride semiconductors 2 The annealing is preferably carried out at a temperature in the range of 900 to 1100°C.

[0088] In the etching process of the second buried layer 14B2, H 2 N as appropriate 2 In this case, since the etching rate decreases when the partial pressure of the inert gas is increased, the etching rate can be controlled by controlling the partial pressure of the gas.

[0089] In addition, the group III nitride semiconductor is 2 When annealing in an atmosphere, nitrogen atoms are more likely to be desorbed than group III atoms, which leads to the formation of nitrogen vacancies and Ga droplets. 3 It is useful to incorporate gases such as NH 3 Gas may be mixed as appropriate.

[0090] (Step S4) Recrystallization Growth Subsequently, crystal growth of a layer above the light distribution adjustment layer 23 was further carried out in the reactor on the substrate on which the etching of the buried layer 14B had been performed.

[0091] Specifically, the light distribution adjustment layer 23 is grown on the second burying layer 14B2. Specifically, the light distribution adjustment layer 23 is made of undoped In 0.03 Ga 0.97 It is an N layer, and is a semiconductor layer (heterogeneous semiconductor layer) having a different crystal composition from the buried layer 14B (GaN layer).

[0092] Next, an active layer 15, a p-side guide layer (second guide layer) 16, an electron barrier layer (EBL) 17, a p-cladding layer 18, and a p-contact layer 19 were grown in this order on the light distribution-adjusting layer 23. In this way, the PCSEL device 10 was fabricated.

[0093] (b) Hole Layer The above-described filling process resulted in the formation of a hole layer 14P having a double lattice structure in which holes 14K, each consisting of a pair of a main hole 14K1 and a sub-hole 14K2, are arranged two-dimensionally at each square lattice point. Here, the sub-holes 14K2 have a smaller diameter and height than the main holes 14K1. In the present invention, the upper surface of the holes 14K in the hole layer 14P having a multi-lattice structure refers to the upper surface of the main holes 14K1 or the sub-holes 14K2 that is closer to the upper layer (active layer) (i.e., the hole with the shallower upper surface). The holes 14K may have a single lattice structure in which holes of the same size are arranged two-dimensionally at each square lattice point, rather than the main holes 14K1 and sub-holes 14K2 having different sizes.

[0094] 6 is a diagram showing a schematic cross section of the formed void layer 14P perpendicular to the central axis CX. When the holes 14H are filled with the group III nitride, the shape of the holes 14H is deformed by mass transport into a shape formed by thermally stable surfaces, and voids 14K are formed.

[0095] That is, in the +c-plane substrate, the inner side surface of the hole 14H changes shape to the (1-100) plane (i.e., m-plane), that is, changes shape from an oval cylindrical shape to an oval hexagonal prism-shaped hole 14K whose side surface is formed by the m-plane.

[0096] The formed primary voids 14K1 had a long hexagonal prism shape with a major axis of 72.5 nm and a minor axis of 43.5 nm, and a major axis / minor axis ratio of 1.67. The secondary voids 14K2 had a long hexagonal prism shape with a major axis of 44.6 nm and a minor axis of 38.3 nm, and a major axis / minor axis ratio of 1.16, and were closer to a regular hexagonal prism than the primary voids 14K1.

[0097] Furthermore, it was confirmed that the distances Δx and Δy between the centers of gravity of the main void 14K1 and the subvoid 14K2 were 81.6 nm (Δx=Δy=0.46PK), which had not changed since before filling. It was also confirmed that the major axes of the main void 14K1 and the subvoid 14K2 were parallel to the <11-20> axis (i.e., the a-axis).

[0098] Furthermore, the void filling factors FF1 and FF2 of the main voids 14K1 and the sub-voids 14K2 were calculated to be 8.8% and 4.2%, respectively. Here, the void filling factor is the ratio of the area occupied by each void per unit area in a two-dimensional regular array. Specifically, when the areas of the main voids 14K1 and the sub-voids 14K2 in the void layer 14P are S1 and S2, respectively, the void filling factors FF1 and FF2 of the main voids 14K1 and the sub-voids 14K2 are given by the following equations:

[0099] FF1 = S1 / PK 2 , FF2=S2 / PK 2 Through the above steps, the formation of the n-side guide layer 14 including the vacancy layer 14P is completed.

[0100] (c) Etched buried layer and its planarity. The buried layer 14B was etched by H annealing at a temperature of 1,050° C. for annealing times of (i) 5 minutes, (ii) 20 minutes, and (iii) 50 minutes. 2 After etching by annealing, the light distribution control layer 23 and the active layer 15 were grown on the buried layer 14B, and the cross section was observed with a SEM (Scanning Electron Microscope) and the surface of the active layer 15 with an AFM (Atomic Force Microscope).

[0101] 7A-7C are SEM images of the cross section of the wafer obtained when the etching times were (i) 5 minutes, (ii) 20 minutes, and (iii) 50 minutes, respectively. In the figures, D denotes the thickness of the buried layer 14B after etching (i.e., the total thickness of the first buried layer 14B1 and the second buried layer 14B2 after etching), and DE denotes the thickness of the second buried layer 14B2 after etching. In the SEM images of FIGS. 7A-7C, the cross section of the hole formation layer 14J is observed with slight variations in shading. For clarity, the semiconductor layers of the buried layer 14B, the active layer 15, and the light distribution adjustment layer 23 are indicated by their respective reference numerals.

[0102] When the etching time was 5 minutes, D=140 nm and DE=60 nm, when it was 20 minutes, D=109 nm and DE=31 nm, and when it was 20 minutes, D=82 nm and DE<2 nm.

[0103] 8 shows an AFM image of the surface of the active layer 15. The surface roughness was Ra = 0.602 nm and 0.210 nm in the 20 μm × 20 μm and 2 μm × 2 μm regions when the etching time was 5 minutes, Ra = 0.576 nm and 0.197 nm when the etching time was 20 minutes, and Ra = 2.06 nm and 0.634 nm when the etching time was 50 minutes.

[0104] It was found that the surface roughness increased with increasing etching time, and that when the etching time was 50 minutes or longer, i.e., when the DE was less than 2 nm, the surface roughness was so large that an active layer with good crystalline quality could not be obtained on such a surface.

[0105] H 2 It is believed that the reason why the surface roughness occurs when the etching time by annealing is long is because a large amount of Si is deposited on the surface of the hole formation layer 14J in which the holes 14H are formed. More specifically, the Si is deposited by the hard mask (SiN film or the like) used when forming the holes 14H and siloxane in the atmosphere adhering to the surface of the hole formation layer 14J.

[0106] Highly reactive nitrogen atmosphere (i.e., NH 3In an atmosphere where Si is dissociated at high temperatures, Si reacts with N on the semiconductor (GaN) surface to form SiN. SiN forms inversion domains on the GaN surface, causing local inversion of the polarity of the GaN layer and significant surface roughness during shape changes due to mass transport. Figure 8 shows that the surface roughness caused by the inversion domains generated on the semiconductor (GaN) surface appears on the upper surface of the active layer 15 even after the active layer has been formed.

[0107] 9A and 9B show the results of measuring the surface roughness (surface height) along line M-M (see FIG. 8) in a 20 μm × 20 μm area for etching times of (ii) 20 minutes and (iii) 50 minutes, respectively.

[0108] When the etching time is (ii) 20 minutes, the surface condition of the active layer 15 is not rough enough to affect the threshold current. On the other hand, when the etching time is (iii) 50 minutes, the surface roughness of the active layer 15 is large, making it difficult to grow an active layer of good quality.

[0109] 10 shows the measured values ​​of the surface roughness Ra of a 20 μm×20 μm area when the thickness DE of the second buried layer 14B2 after etching is changed. The boundary (DE=0 nm) between the top surface of the hole formation layer 14J and the second buried layer 14B2 is indicated by a dashed line. The arrows also indicate the thickness at which the surface roughness Ra changes critically with respect to the thickness DE of the second buried layer 14B2.

[0110] As shown in Figure 10, when the layer thickness DE of the second buried layer 14B2 after etching is 2 nm or more, the surface roughness Ra is at most less than 1.0 nm, whereas when the layer thickness DE is less than 2 nm, the surface roughness increases significantly, making it difficult to grow an active layer with good crystal quality.

[0111] Therefore, H 2 By etching the surface of the second buried layer 14B2 to make it flat by annealing and setting the layer thickness DE of the second buried layer 14B2 to 2 nm or more, it is possible to grow an active layer and a semiconductor layer with good crystal quality on the second buried layer 14B2.

[0112] From the viewpoint of the coupling efficiency between the active layer 15 and the air hole layer 14P, it is preferable that the distance between the active layer 15 and the air hole layer 14P, i.e., the distance between the upper surfaces of the air holes 14K in the air hole layer 14P and the active layer 15, be 200 nm or less. Furthermore, from the viewpoint of obtaining high coupling efficiency, it is even more preferable that the distance between the upper surfaces of the air holes 14K in the air hole layer 14P and the active layer 15 be 150 nm or less.

[0113] In addition, when the active layer 15 is an active layer with a quantum well structure, the distance between the upper surface of the air hole 14K and the active layer 15 refers to the distance between the upper surface of the air hole 14K and the first quantum well layer (i.e., the quantum well layer closest to the air hole layer 14P).

[0114] Furthermore, while conventionally, in order to obtain a high hole filling rate in a hole layer with a multi-lattice structure, a thicker burying layer may be required than in a hole layer with a single lattice structure, the present invention makes it possible to use a thinner burying layer even in such a case, thereby achieving a high coupling efficiency (resonance effect) between the hole layer and the active layer.

[0115] As described above in detail, according to the present invention, it is possible to provide a method for manufacturing a photonic crystal surface-emitting laser element that can bring the air hole layer and the active layer close to each other to increase the resonance effect, has a high-quality active layer, and has a low threshold and high efficiency, and also provides the photonic crystal surface-emitting laser element.

[0116] The numerical values ​​and the like in the above-described embodiments are merely examples unless otherwise specified, and can be modified as appropriate. Furthermore, although a PCSEL element having a double grating structure has been exemplified, the present invention can also be applied to a PCSEL element having a single grating structure and, in general, to a PCSEL element having a multi-grating structure.

[0117] Furthermore, although the present invention has been exemplified with respect to a photonic crystal layer (hole layer) in which the holes have a hexagonal columnar shape, the present invention can also be applied to cases in which the holes in the photonic crystal layer have an irregular columnar shape such as a cylindrical, rectangular, polygonal, or teardrop shape.

[0118] 10: PCSEL element 12: Element substrate 13: First cladding layer 14: First guide layer 14A: Lower guide layer 14B: Buried layer 14B1: First buried layer 14B2: Second buried layer 14E: Hole formation preparation layer 14J: Hole formation layer 14K: Hole / hole pair 14K1 / 14K2: Main / sub-hole 14P: Hole layer (photonic crystal layer) 15: Active layer 16: Second guide layer 17: Electron barrier layer 18: Second cladding layer 19: Contact layer 23: Light distribution adjustment layer

Claims

1. A method for manufacturing a surface-emitting semiconductor laser element, comprising the steps of: (a) forming a hole-formation preparation layer on a substrate; (b) forming holes in the hole-formation preparation layer at each of lattice points so as to form a hole-formation layer; (c) forming a first burying layer by facet growth that closes the holes; (d) growing a second burying layer that flatly buries the first burying layer to form a vacancy layer having vacancies corresponding to the holes; (e) flattening the second burying layer by annealing in a hydrogen atmosphere; and (f) performing crystal growth of a semiconductor layer including an active layer on the flattened etched second burying layer.

2. The method according to claim 1, wherein the surface emitting semiconductor laser element is a GaN-based semiconductor laser element, the crystal growth surface of the substrate is a {0001} plane, and the surface of the second buried layer after the flattening etching is a {0001} plane.

3. The method according to claim 1, wherein the thickness of the second buried layer on the upper surface of the hole forming layer after the flattening etching is 2 nm or more.

4. The method according to claim 1, wherein the distance from the upper surface of the hole in the hole layer to the active layer is 200 nm or less.

5. The method of claim 2, wherein the facet growth is performed by selectively growing a crystal whose surface is a {1-101} facet.

6. A surface emitting semiconductor laser device manufactured by the method according to any one of claims 1 to 4, wherein the distance between the active layer and the hole layer is 200 nm or less.

7. A surface emitting semiconductor laser device manufactured by the method according to any one of claims 1 to 4, wherein the distance between the active layer and the hole layer is 150 nm or less.

8. A surface-emitting semiconductor laser element made of a nitride semiconductor, comprising: a light-transmitting substrate; a first semiconductor layer provided on the substrate; an active layer provided on the first semiconductor layer; and a second semiconductor layer provided on the active layer and having an opposite conductivity type to the first semiconductor layer, wherein the first semiconductor layer has a hole layer which is a photonic crystal layer having holes arranged with two-dimensional periodicity in a plane parallel to the active layer; and a burying layer, wherein the burying layer has a first burying layer closing the holes, and a second burying layer provided on the first burying layer, and the distance between the hole layer and the active layer is 200 nm or less.

9. The surface emitting semiconductor laser element according to claim 8, wherein the buried layer has a thickness of 30 nm or more and 200 nm or less.

10. The surface emitting semiconductor laser element according to claim 8 or 9, wherein the second buried layer has a thickness of 2 nm or more.

11. The surface emitting semiconductor laser element according to claim 8, wherein the surface roughness Ra measured over a 20 μm×20 μm area of ​​the upper surface of said second buried layer is less than 1.0 nm.

Citation Information

Patent Citations

  • Semiconductor device

    JP2009094210A

  • Surface emitting laser element and manufacturing method of the same

    JP2019114663A

  • Surface-emitting laser element and manufacturing method of surface-emitting laser element

    JP2020038892A

  • Surface-emitting laser element and surface-emitting laser element manufacturing method

    WO2021186965A1