Optical element, lens unit, and camera module
The optical element with a specific thickness range of the hard coat layer and an antireflection film configuration addresses durability and distortion issues in plastic lenses, ensuring enhanced performance under environmental stress.
Patent Information
- Application Number
- PCT/JP2024/010433
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-03
AI Technical Summary
Existing optical elements, such as plastic lenses, face durability issues due to peeling of the antireflection layer and damage to the hard coat layer, especially when exposed to outdoor environments, which can lead to reduced durability and optical distortion.
An optical element with a plastic lens, a hard coat layer, and an antireflection film, where the hard coat layer has a thickness of 2 μm or more but no more than 20 μm along the optical axis, and the antireflection film is made of alternating high and low refractive index layers, providing enhanced durability and preventing optical distortion.
The solution effectively prevents peeling of the antireflection film and damage to the hard coat layer, maintaining the optical element's durability and suppressing optical distortion, even under exposure to environmental stressors like ultraviolet radiation.
Smart Images

Figure JP2024010433_03102024_PF_FP_ABST
Abstract
Description
Optical element, lens unit and camera module
[0001] The present invention relates to an optical element, a lens unit, and a camera module.
[0002] In order to protect a light-transmitting plastic lens substrate, it is known to coat the plastic lens substrate with a hard coat layer that is harder than the plastic lens substrate, and to provide an antireflection layer on the surface of the hard coat layer to prevent light reflection (see, for example, Patent Document 1).
[0003] Patent Document 1 describes the use of a plastic lens as an eyeglass lens, which has an anti-reflection layer on a hard coat layer covering a plastic lens substrate. In the plastic lens of Patent Document 1, the anti-reflection layer is a multilayer film in which low-refractive-index films made of silicon dioxide (SiO2) and high-refractive-index films made of trisilicon tetranitride (Si3N4) are alternately laminated, and the durability of the plastic lens is improved by setting the low-refractive-index films and high-refractive-index films of the anti-reflection layer to specific film thicknesses.
[0004] Japanese Patent Publication No. 2008-76598
[0005] However, even with the plastic lens of Patent Document 1, there is a risk that the durability of the optical element will decrease due to peeling of the antireflection layer or damage to the hard coat layer caused by the surrounding environment. On the other hand, if the hard coat layer of a plastic lens is made thick, the decrease in durability can be suppressed, but optical distortion may occur, resulting in a decrease in optical properties.
[0006] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide an optical element, a lens unit, and a camera module that are capable of improving durability and suppressing deterioration of optical characteristics.
[0007] An exemplary optical element of the present invention is an optical element having an optical axis, comprising a plastic lens, an anti-reflection film disposed on at least one surface of the plastic lens, and a hard coat layer positioned between the plastic lens and the anti-reflection film, wherein the thickness of the hard coat layer along the optical axis is 2 μm or more and 20 μm or less.
[0008] An exemplary lens unit of the present invention includes a plurality of lenses and a housing member that houses the plurality of lenses, the plurality of lenses being arranged in order from an opening of the housing member, and the outermost lens of the plurality of lenses located on the opening side of the housing member being the optical element described above.
[0009] An exemplary camera module of the present invention includes the lens unit described above and an image sensor.
[0010] The present invention, exemplified by the above, can provide an optical element, a lens unit, and a camera module that are capable of improving durability and suppressing deterioration of optical characteristics.
[0011] FIG. 1A is a schematic diagram of an example of an optical element according to the present embodiment. FIG. 1B is a partially enlarged view of FIG. 1A. FIG. 2A is a schematic diagram of a camera module according to the present embodiment. FIG. 2B is a partially enlarged view of FIG. 2A. FIG. 3A is a schematic diagram of a camera module according to the present embodiment. FIG. 3B is a partially enlarged view of FIG. 3A. FIG. 4A is an exploded view of a camera module according to the present embodiment. FIG. 4B is a schematic view of a manufacturing process of a camera module according to the present embodiment. FIG. 4C is a schematic view showing a camera module according to the present embodiment.
[0012] Hereinafter, optical elements, lens units, and camera modules according to embodiments of the present invention will be described with reference to the drawings as appropriate. Note that the same or corresponding parts in the drawings are designated by the same reference numerals, and descriptions thereof will not be repeated. The dimensions, shapes, and relative sizes of components in the drawings are not necessarily identical to the actual dimensions, shapes, and relative sizes of components. In particular, the thicknesses of the anti-reflection coating, hard coat layer, and plastic lens in the drawings may differ significantly from the actual thicknesses of the anti-reflection coating, hard coat layer, and plastic lens. Note that, in this specification, the "thickness" of each part of the optical element refers to the length parallel to the optical axis direction of the optical element.
[0013] An optical element 10 according to this embodiment will be described below with reference to Figures 1A and 1B. Figure 1A is a schematic diagram of the optical element 10 according to this embodiment. Figure 1B is an enlarged view of a portion of Figure 1A.
[0014] 1A and 1B, the optical element 10 has a curved shape. Typically, the optical element 10 has a spherical shape. The optical element 10 has a spherical shape centered on a central axis.
[0015] The optical element 10 has an optical axis Lx. The optical axis Lx passes through the center of the curved surface shape of the optical element 10. The optical element 10 has a symmetric structure with respect to the optical axis Lx. Typically, the optical element 10 has a rotationally symmetric structure with respect to the optical axis Lx. Light is incident on the optical element 10 from a direction along the optical axis Lx.
[0016] The optical element 10 includes a plastic lens 11, a hard coat layer 12, and an anti-reflection film 13. The plastic lens 11, the hard coat layer 12, and the anti-reflection film 13 are laminated in this order. Typically, the plastic lens 11, the hard coat layer 12, and the anti-reflection film 13 are disposed in this order in close contact with each other.
[0017] [Plastic Lens 11] The plastic lens 11 transmits light. For example, the plastic lens 11 is transparent. Alternatively, the plastic lens 11 may be translucent or translucent.
[0018] Typically, the plastic lens 11 is made of resin. The plastic lens 11 may be composed of a single member. For example, the plastic lens 11 includes a resin having a cyclic imide structure as a ring structure. Examples of such resins include AZP manufactured by Asahi Kasei Corporation, and RM-104, RM-250, and RM-100-Z manufactured by Nippon Shokubai Co., Ltd.
[0019] The plastic lens 11 has a curved shape. Typically, the plastic lens 11 has a spherical shape. At least one surface of the plastic lens 11 may be a convex or concave surface. When the plastic lens 11 has a convex or concave surface, the plastic lens 11 functions as a lens (specifically, for example, a biconvex lens, a plano-convex lens, a convex meniscus lens, or a concave meniscus lens).
[0020] The plastic lens 11 may have a convex surface. For example, the radius of curvature of the plastic lens 11 is equal to or greater than 9 mm and equal to or less than 16 mm.
[0021] The thermal expansion coefficient of the plastic lens 11 is preferably 60 ppm / K or more and 150 ppm / K or less, so that the influence of thermal stress between the plastic lens 11 and the anti-reflection film 13 can be suppressed.
[0022] [Hard Coat Layer 12] The hard coat layer 12 coats the plastic lens 11. For example, the hard coat layer 12 coats one surface of the plastic lens 11 that is located on the object side in the direction in which the optical axis Lx extends. The hard coat layer 12 has a higher hardness than the plastic lens 11. The hard coat layer 12 imparts scratch resistance to the plastic lens 11 and improves adhesion between the plastic lens 11 and the antireflection coating 13.
[0023] The hard coat layer 12 transmits light. For example, the hard coat layer 12 is transparent. Alternatively, the hard coat layer 12 may be semi-transparent or translucent.
[0024] The hard coat layer 12 may have a base layer. Typically, the base layer includes an organic material layer or an organosilicon compound layer. In the hard coat layer 12, metal oxide fine particles may be dispersed in the base layer.
[0025] The elastic modulus of the hard coat layer 12 is preferably 5 GPa or more and 12 GPa or less. When the elastic modulus of the hard coat layer 12 is 5 GPa or more, damage to the plastic lens 11 can be suppressed. Furthermore, when the elastic modulus of the hard coat layer 12 is 12 GPa or less, cracks caused by temperature changes can be suppressed in the hard coat layer 12.
[0026] Typically, the hard coat layer 12 can be formed by drying the component liquids attached to the surface of the plastic lens 11, and then curing the film of the component liquids with electromagnetic waves such as ultraviolet rays or electron beams. The component liquids may be heated when drying them.
[0027] In one example, the hard coat layer 12 may be formed by a spin coating method, in which component liquids of the hard coat layer 12 are ejected onto the plastic lens 11 rotating at a predetermined rotation speed, and the component liquids of the hard coat layer 12 are cured by applying electromagnetic waves such as ultraviolet rays or electron beams to the component liquids.
[0028] Alternatively, the hard coat layer 12 may be formed by a dipping method. In this case, the plastic lens 11 is immersed in a component liquid of the hard coat layer 12, and then the component liquid of the hard coat layer 12 is applied to the plastic lens 11 rotating at a predetermined rotation speed by electromagnetic waves such as ultraviolet rays or an electron beam to harden the component liquid.
[0029] When the hard coat layer 12 is formed on the surface of the plastic lens 11 while the plastic lens 11 is rotated, the thickness of the hard coat layer 12 varies depending on the distance from the optical axis Lx. Typically, the thickness of the hard coat layer 12 decreases as the distance from the optical axis Lx increases.
[0030] [Anti-reflection film 13] The anti-reflection film 13 covers the hard coat layer 12. For example, the anti-reflection film 13 covers the air side of the hard coat layer 12. The anti-reflection film 13 suppresses reflection of light incident on the anti-reflection film 13. The anti-reflection film 13 suppresses reflection of at least a portion of light traveling in a direction incident on the plastic lens 11 from the surface side of the plastic lens 11. For example, the anti-reflection film 13 suppresses reflection of visible light traveling in a direction incident on the plastic lens 11 from the surface side of the plastic lens 11.
[0031] The anti-reflection film 13 transmits light. For example, the anti-reflection film 13 is transparent. Alternatively, the anti-reflection film 13 may be semi-transparent or translucent.
[0032] The thickness of the antireflection film 13 is 100 nm or more and 1000 nm or less. The thickness of the antireflection film 13 may be 200 nm or more and 900 nm or less, or may be 300 nm or more and 800 nm or less.
[0033] The thermal expansion coefficient of the anti-reflection coating 13 is preferably 1 ppm / K or more and 10 ppm / K or less, so that the influence of thermal stress between the plastic lens 11 and the anti-reflection coating 13 can be suppressed.
[0034] The anti-reflection film 13 may have a laminated film structure. For example, in the anti-reflection film 13, layers with different compositions are laminated.
[0035] For example, the anti-reflection film 13 is made of an inorganic oxide. Examples of the inorganic oxide in the anti-reflection film 13 include metal oxides such as silicon oxide, titanium oxide, lanthanum titanate, tantalum oxide, and niobium oxide. For example, the anti-reflection film 13 has layers of multiple types of metal oxides stacked thereon.
[0036] For example, the anti-reflection film 13 has a high refractive index film and a low refractive index film, and is configured so that the high refractive index film and the low refractive index film are alternately stacked.
[0037] The refractive index of the high refractive index film is higher than the refractive index of the low refractive index film, and typically, in the visible range, the refractive index of the high refractive index film is higher than the refractive index of the low refractive index film.
[0038] The high-refractive-index film contains trisilicon tetranitride (Si3N4). The low-refractive-index film contains silicon dioxide (SiO2). In this way, the high-refractive-index film contains trisilicon tetranitride (Si3N4) and the low-refractive-index film contains silicon dioxide (SiO2), thereby improving thermal shock resistance.
[0039] For example, the high refractive index film is 1.9 or more. In one example, the high refractive index film is 1.9 or more and 2.3 or less.
[0040] For example, the refractive index of the low refractive index film is 1.5 or more and 1.8 or less. In one example, the refractive index of the low refractive index film is 1.6 or more and 1.75 or less.
[0041] The thickness of the high-refractive-index film and the low-refractive-index film is 5 nm or more and 200 nm or less. This allows the high-refractive-index film and the low-refractive-index film to be formed uniformly, and allows a plurality of high-refractive-index films and low-refractive-index films to be arranged in the anti-reflection film 13. The thickness of the high-refractive-index film and the low-refractive-index film may be 10 nm or more and 180 nm or less, or may be 20 nm or more and 170 nm or less.
[0042] The anti-reflection film 13 preferably transmits light in the visible range while reflecting light in the ultraviolet range. The average reflectance of the anti-reflection film 13 for visible light wavelengths is preferably lower than the average reflectance for ultraviolet light wavelengths.
[0043] From the viewpoint of further suppressing the influence of thermal stress between the plastic lens 11 and the anti-reflection coating 13, it is preferable that the difference between the thermal expansion coefficient of the plastic lens 11 and the thermal expansion coefficient of the anti-reflection coating 13 is relatively small. For example, it is preferable that the thermal expansion coefficient of the plastic lens 11 is 60 ppm / K or more and 100 ppm / K or less, and the thermal expansion coefficient of the anti-reflection coating 13 is 5 ppm / K or more and 10 ppm / K or less.
[0044] 1B, the plastic lens 11 has a curved shape. Here, one surface of the plastic lens 11 is curved and the other surface is flat. The thickness of the plastic lens 11 varies depending on the distance from the optical axis Lx.
[0045] The thickness of the hard coat layer 12 varies depending on the distance from the optical axis Lx. Typically, the thickness of the hard coat layer 12 is greatest at the center of the optical axis Lx. Also, typically, the thickness of the hard coat layer 12 is smallest at the outer edge.
[0046] Typically, the thickness Lx2 of the outer edge of the hard coat layer 12 is smaller than the thickness Lx1 of the hard coat layer 12 on the optical axis Lx. However, it is preferable that the difference between the thickness Lx1 of the hard coat layer 12 on the optical axis Lx and the thickness Lx1 of the outer edge of the hard coat layer 12 is relatively small. For example, the difference between the thickness Lx1 of the hard coat layer 12 on the optical axis Lx and the thickness Lx2 of the outer edge of the hard coat layer 12 is preferably 15 μm or less, and more preferably 6 μm or less.
[0047] If the thickness of the hard coat layer on the optical axis Lx is small, when the optical element is exposed to an outdoor environment and the adhesion at the interface between the hard coat layer and the antireflection film is reduced, the antireflection film may peel off from the hard coat layer or the hard coat layer may be damaged, resulting in a decrease in the durability of the optical element.
[0048] On the other hand, if the thickness of the hard coat layer along the optical axis Lx is large, optical distortion occurs in the optical element, and the optical characteristics of the optical element may be deteriorated. Furthermore, if the thickness of the hard coat layer along the optical axis Lx is further increased, the film state of the hard coat layer becomes non-uniform, and cracks may occur in the hard coat layer.
[0049] In the optical element 10 of this embodiment, the thickness Lx1 of the hard coat layer 12 on the optical axis Lx is 2 μm or more, so that even when the optical element 10 is exposed to an outdoor environment, it is possible to prevent the antireflection film 13 from peeling off from the hard coat layer 12 or the hard coat layer 12 from being damaged along the optical axis Lx through which a high amount of light transmits, thereby preventing a decrease in the durability of the optical element 10. Furthermore, in the optical element 10 of this embodiment, the thickness Lx1 of the hard coat layer 12 on the optical axis Lx is 20 μm or less, so that it is possible to prevent a decrease in the optical properties of the optical element 10 along the optical axis Lx through which a high amount of light transmits.
[0050] In the optical element 10 of this embodiment, the thickness Lx1 of the hard coat layer 12 along the optical axis Lx is 2 μm or more and 20 μm or less. Since the thickness Lx1 of the hard coat layer 12 along the optical axis Lx is 2 μm or more, peeling of the antireflection film 13 from the hard coat layer 12 can be suppressed even when light is irradiated onto the optical element 10 along the optical axis Lx, through which a high amount of light passes through the optical element 10. Furthermore, since the thickness of the hard coat layer 12 along the optical axis Lx is 20 μm or less, optical distortion can be suppressed and cracks can be suppressed from occurring in the hard coat layer 12.
[0051] The minimum thickness of the hard coat layer 12 is preferably 2 μm or more, which can prevent the durability of the entire optical element 10 from decreasing.
[0052] The maximum thickness of the hard coat layer 12 is preferably 20 μm or less, which can prevent the optical properties of the entire optical element 10 from being deteriorated.
[0053] The optical element 10 of this embodiment has relatively little optical distortion and exhibits relatively high durability. Therefore, the optical element 10 is suitable for use in a surveillance camera or an in-vehicle camera. The optical element 10 can be used continuously even when the surveillance camera or the in-vehicle camera is used in an outdoor environment for a long period of time.
[0054] In this embodiment, the optical element 10 has an optical axis Lx. The optical element 10 includes a plastic lens 11, a hard coat layer 12, and an anti-reflection film 13. The hard coat layer 12 is located between the plastic lens 11 and the anti-reflection film 13. The anti-reflection film 13 is disposed on at least one surface of the plastic lens 11. The hard coat layer 12 has a thickness Lx1 on the optical axis Lx of 2 μm or more and 20 μm or less.
[0055] By setting the thickness Lx1 of the hard coat layer 12 on the optical axis Lx to 2 μm or more, peeling of the antireflection film 13 from the hard coat layer 12 can be suppressed even when ultraviolet light is irradiated onto the optical element 10 on the optical axis Lx of the hard coat layer 12. Furthermore, by setting the thickness Lx1 of the hard coat layer 12 on the optical axis Lx to 20 μm or less, optical distortion can be suppressed and cracks can be suppressed from occurring in the hard coat layer 12.
[0056] Generally, when an optical element is exposed to ultraviolet light in an outdoor environment, deterioration occurs on the surface of the hard coat layer, which can reduce the adhesion at the interface between the hard coat layer and the anti-reflection coating. In contrast, by setting the thickness Lx1 of the hard coat layer 12 along the optical axis Lx to 2 μm or more, peeling of the anti-reflection coating 13 from the hard coat layer 12 and loss of the hard coat layer 12 can be suppressed even when the optical element 10 is irradiated with light. This makes it possible to provide an optical element 10 that has excellent weather resistance and is suppressed from deteriorating in its optical properties.
[0057] The hard coat layer 12 has a minimum thickness of 2 μm or more and a maximum thickness of 20 μm or less. When the hard coat layer 12 has a minimum thickness of 2 μm or more, peeling of the antireflection film 13 can be suppressed even when light is irradiated onto the optical element 10. Furthermore, when the hard coat layer 12 has a maximum thickness of 20 μm or less, optical distortion can be suppressed and cracks can be suppressed from occurring in the hard coat layer 12.
[0058] The hard coat layer 12 has an elastic modulus of 5 GPa or more and 12 GPa or less. When the hard coat layer 12 has an elastic modulus of 5 GPa or more, it is possible to prevent damage to the plastic lens 11. Furthermore, when the hard coat layer 12 has an elastic modulus of 12 GPa or less, it is possible to prevent cracks from occurring in the hard coat layer 12 due to thermal stress.
[0059] The thermal expansion coefficient of the plastic lens 11 is 60 ppm / K or more and 150 ppm / K or less. When the thermal expansion coefficient of the plastic lens 11 is 60 ppm / K or more and 150 ppm / K or less, the influence of thermal stress between the plastic lens 11 and the anti-reflection coating 13 can be reduced.
[0060] The thermal expansion coefficient of the anti-reflection coating 13 is 1 ppm / K or more and 10 ppm / K or less. When the thermal expansion coefficient of the anti-reflection coating 13 is 1 ppm / K or more and 10 ppm / K or less, the influence of thermal stress between the plastic lens 11 and the anti-reflection coating 13 can be reduced.
[0061] The thermal expansion coefficient of the plastic lens 11 is 60 ppm / K or more and 100 ppm / K or less, and the thermal expansion coefficient of the anti-reflection coating 13 is 5 ppm / K or more and 10 ppm / K or less. By having the thermal expansion coefficient of the plastic lens 11 be 60 ppm / K or more and 100 ppm / K or less, and the thermal expansion coefficient of the anti-reflection coating 13 be 5 ppm / K or more and 10 ppm / K or less, the influence of thermal stress between the plastic lens 11 and the anti-reflection coating 13 can be further reduced.
[0062] The difference between the thickness Lx1 of the hard coat layer 12 on the optical axis Lx and the thickness Lx2 of the outer edge is 15 μm or less. By making the difference between the thickness Lx1 of the hard coat layer 12 on the optical axis Lx and the thickness Lx2 of the outer edge 12 15 μm or less, a relatively thin hard coat layer 12 can be suitably formed on the surface of the plastic lens 11 while rotating the component liquid of the hard coat layer 12 at a predetermined speed.
[0063] 1A and 1B, the hard coat layer 12 and the anti-reflection film 13 are disposed on one side of the plastic lens 11, but this embodiment is not limited to this. The hard coat layer 12 and the anti-reflection film 13 may be disposed on both sides of the plastic lens 11.
[0064] Next, a camera module 200 according to this embodiment will be described with reference to Figures 1A, 1B, 2A, and 2B. Figure 2A is a schematic diagram showing an example of the camera module 200 according to this embodiment, and Figure 2B is an enlarged view of a portion of Figure 2A. The camera module 200 captures an image of the surroundings.
[0065] 2A, the camera module 200 includes the lens unit 100 and an image sensor 210. The image sensor 210 receives light that passes through the lens unit 100 and captures an image of the surroundings.
[0066] The lens unit 100 includes a plurality of lenses 110. At least one of the plurality of lenses 110 is an optical element 10.
[0067] The plurality of lenses 110 include a first lens 110a, a second lens 110b, a third lens 110c, a fourth lens 110d, and a fifth lens 110e, which are arranged in order from the object side to the image side.
[0068] For example, the first lens 110a is the above-described optical element 10. That is, the first lens 110a includes the above-described plastic lens 11, hard coat layer 12, and anti-reflection film 13.
[0069] The lens unit 100 further includes a housing member 120, a fixing member 122, a filter 130, and a sealing member 140. The housing member 120 is tubular. Typically, the housing member 120 is cylindrical. Note that the inner circumferential surface of the housing member 120 may be provided with irregularities.
[0070] The housing member 120 houses the lenses 110 and the filters 130. The housing member 120 is made of a material that does not transmit light. For example, the housing member 120 is made of a material that does not transmit visible light and ultraviolet light.
[0071] The fixing member 122 fixes at least one lens of the plurality of lenses 110 to the housing member 120. The fixing member 122 penetrates the housing member 120 in a direction perpendicular to the optical axis Lx and fixes the at least one lens to the housing member 120.
[0072] The first lens 110a, the second lens 110b, the third lens 110c, the fourth lens 110d, and the fifth lens 110e are disposed in the housing member 120. At least a portion of at least one of the first lens 110a, the second lens 110b, the third lens 110c, the fourth lens 110d, and the fifth lens 110e may be disposed so as to be exposed from the housing member 120. For example, the first lens 110a is disposed so as to be exposed from the housing member 120, and the other lenses, the second lens 110b, the third lens 110c, the fourth lens 110d, and the fifth lens 110e, are disposed within the housing member 120.
[0073] Here, the diameter of the first lens 110a is larger than the diameters of the second lens 110b, the third lens 110c, the fourth lens 110d, and the fifth lens 110e, and the diameter of the fifth lens 110e is larger than the diameters of the second lens 110b, the third lens 110c, and the fourth lens 110d.
[0074] The fixing member 122 fixes the first lens 110a to the housing member 120. The fixing member 122 presses the edge surface of the first lens 110a to fix the first lens 110a to the housing member 120.
[0075] The filter 130 is disk-shaped. The filter 130 selectively transmits incident light. For example, the filter 130 selectively transmits light of a specific wavelength from the incident light. Here, the filter 130 is disposed in the housing member 120. For example, as shown in FIG. 2A , the image sensor 210 is disposed outside the lens unit 100.
[0076] The filter 130 is disposed on the image side relative to the fifth lens 110e. The filter 130 can select the wavelength of light that reaches the image sensor 210. The image sensor 210 is a photoelectric conversion element that converts irradiated light into an electrical signal. The image sensor 210 is, for example, a CMOS image sensor or a CCD image sensor. However, the image sensor 210 is not limited to these. The image sensor 210 captures an image of a subject formed by the multiple lenses 110. Note that the image sensor 210 may be disposed on the image side relative to the filter 130 (lens unit 100).
[0077] The first lens 110a is a negative meniscus lens with a convex surface facing the object side. In this embodiment, the convex surface of the first lens 110a facing the object side is spherical, and the concave surface facing the image side is aspherical.
[0078] The second lens 110b, the third lens 110c, the fourth lens 110d, and the fifth lens 110e may be made of resin (plastic lenses) or glass.
[0079] The second lens 110b, the third lens 110c, the fourth lens 110d, and the fifth lens 110e may be any of a biconvex lens, a plano-convex lens, a convex meniscus lens, and a concave meniscus lens.
[0080] As described above, the lens unit 100 includes a plurality of lenses 110, and at least one of the plurality of lenses 110 is the optical element 10, so that deterioration of the lenses 110 in the lens unit 100 can be suppressed.
[0081] Furthermore, the first lens 110a, which is equipped with the above-mentioned plastic lens 11, hard coat layer 12, and anti-reflection film 13, is positioned exposed from the housing member 120, and the remaining lenses (the second lens 110b, the third lens 110c, the fourth lens 110d, and the fifth lens 110e) are positioned within the housing member 120, thereby suppressing deterioration of lenses other than the highly durable first lens 110a.
[0082] The sealing member 140 deforms between the first lens 110a and the housing member 120 to seal the gap between the first lens 110a and the housing member 120. For example, the sealing member 140 is an annular elastic body. In one example, the sealing member 140 is an O-ring.
[0083] The lens unit 100 is suitable for use as an in-vehicle lens for capturing images of the surroundings of a vehicle. For example, the lens unit 100 is used as an in-vehicle lens for capturing images of the rear or side of a vehicle.
[0084] Since the lens unit 100 includes the sealing member 140, even if water is splashed onto the lens unit 100 from the outside, the water can be prevented from entering the inside of the lens unit 100 (i.e., the inside of the housing member 120).
[0085] The first lens 110a includes the above-described plastic lens 11, hard coat layer 12, and anti-reflection film 13, and thus can effectively suppress ultraviolet light from entering the housing member 120. This makes it possible to suppress deterioration of the lens in the housing member 120.
[0086] For example, the diameter Ld of the first lens 110a may be 1 mm or more and 100 mm or less, or 2 mm or more and 50 mm or less. In one example, the diameter Ld of the first lens 110a is 13.70 mm or more and 13.75 mm or less.
[0087] According to this embodiment, the lens unit 100 includes a plurality of lenses 110 and a housing member 120 that houses the plurality of lenses 110. The plurality of lenses 110 are arranged in order from the opening of the housing member 120. Of the plurality of lenses 110, the outermost lens located on the opening side of the housing member 120 is the optical element 10 described above. This can improve the weather resistance of the lens unit 100.
[0088] The camera module 200 includes the lens unit 100 described above and an image sensor 210. This allows the weather resistance of the camera module 200 to be improved.
[0089] Next, a camera module 200 according to this embodiment will be described with reference to Figures 1 to 3B. Figure 3A is a schematic diagram showing an example of a camera module 200 according to this embodiment, and Figure 3B is an enlarged view of a portion of Figure 3A. The camera module 200 in Figures 3A and 3B has the same configuration as the camera module 200 described above with reference to Figures 2A and 2B, except that it further includes a light-blocking member 150 instead of the fixing member 122. Therefore, in order to avoid redundancy, a duplicated description will be omitted.
[0090] 3A , the camera module 200 includes a lens unit 100 and an image sensor 210. The lens unit 100 includes a plurality of lenses 110. At least one of the plurality of lenses 110 is the optical element 10.
[0091] The plurality of lenses 110 include a first lens 110a, a second lens 110b, a third lens 110c, a fourth lens 110d, and a fifth lens 110e, which are arranged in order from the object side to the image side.
[0092] For example, the first lens 110a is the above-described optical element 10. That is, the first lens 110a includes the above-described plastic lens 11, hard coat layer 12, and anti-reflection film 13.
[0093] The lens unit 100 further includes a housing member 120, a filter 130, a sealing member 140, and a light blocking member 150. The housing member 120 is tubular. Typically, the housing member 120 is cylindrical. Note that the inner circumferential surface of the housing member 120 may be provided with irregularities.
[0094] The housing member 120 houses the lenses 110 and the filters 130. The housing member 120 is made of a material that does not transmit light. The housing member 120 is made of a material that does not transmit visible light and ultraviolet light.
[0095] The light blocking member 150 blocks light from the first lens 110a. The light blocking member 150 blocks light from the periphery of the first lens 110a. The light blocking member 150 extends in a direction perpendicular to the optical axis Lx with respect to the housing member 120. The light blocking member 150 extends along the periphery of the first lens 110a. The light blocking member 150 prevents the first lens 110a from detaching from the housing member 120. The light blocking member 150 may be a single member together with the housing member 120.
[0096] The light blocking member 150 covers the periphery of the first lens 110a over a length that is 0.5% to 10% of the diameter of the first lens 110a, so that the effective diameter Ed of the first lens 110a is smaller than the diameter Ld of the first lens 110a.
[0097] For example, the diameter Ld of the first lens 110a is 1 mm or more and 100 mm or less, and may be 2 mm or more and 50 mm or less. The length Sd of the light blocking member 150 along the direction perpendicular to the optical axis Lx is 0.005 mm or more and 10 mm or less, and may be 0.01 mm or more and 5 mm or less.
[0098] For example, the diameter Ld of the first lens 110a is 13.70 mm or more and 13.75 mm or less. In one example, the light blocking member 150 covers the periphery of the first lens 110a over a length of 0.1 mm or more and 1.0 mm or less from the outer edge of the first lens 110a. Therefore, the length Sd of the light blocking member 150 along a direction perpendicular to the optical axis Lx is 0.1 mm or more and 1.0 mm or less. Therefore, the effective diameter Ed of the first lens 110a is 11.70 mm or more and 13.55 mm or less.
[0099] In this embodiment, the lens unit 100 includes the light blocking member 150 , and therefore, the first lens 110 a can be prevented from being detached from the housing member 120 .
[0100] Next, a camera module 200 according to this embodiment will be described with reference to Figures 1 to 4C. Figure 4A is an exploded view of the camera module 200 according to this embodiment. Figure 4B is a schematic view of the manufacturing process of the camera module 200 according to this embodiment. Figure 4C is a schematic view showing the camera module 200 according to this embodiment.
[0101] 4A, the housing member 120 can house a plurality of lenses 110. At least one of the plurality of lenses 110 is the optical element 10.
[0102] The accommodation member 120 has a cylindrical shape. Typically, the accommodation member 120 has a cylindrical shape.
[0103] The plurality of lenses 110 include a first lens 110a, a second lens 110b, a third lens 110c, a fourth lens 110d, and a fifth lens 110e. The housing member 120 has housing portions capable of housing the first lens 110a, the second lens 110b, the third lens 110c, the fourth lens 110d, and the fifth lens 110e, respectively.
[0104] Note that here, a protrusion 150a is provided on the outer edge on one side of the housing member 120. Typically, the protrusion 150a is formed from the same material as the housing member 120. The protrusion 150a is a single member together with the housing member 120. The protrusion 150a extends from the housing member 120 parallel to the optical axis Lx.
[0105] 4B , the plurality of lenses 110, the filter 130, and the sealing member 140 are housed in the housing member 120. Here, the first lens 110a, the second lens 110b, the third lens 110c, and the sealing member 140 are inserted from one side to the other side into the housing member 120. The fourth lens 110d, the fifth lens 110e, and the filter 130 are inserted from the other side to one side into the housing member 120. The filter 130 is located between the plurality of lenses 110 and the image sensor 210.
[0106] As shown in FIG. 4C , the light-blocking member 150 is formed by bending the protrusion 150a relative to the housing member 120 in a direction perpendicular to the optical axis Lx. The protrusion 150a is pressed in a heated state, causing it to bend relative to the housing member 120 in a direction perpendicular to the optical axis Lx. The light-blocking member 150 blocks the first lens 110a, which is the outermost lens. The light-blocking member 150 prevents light incident on the lens unit 100 from entering the outer edge of the first lens 110a. The light-blocking member 150 also prevents the first lens 110a from detaching from the housing member 120.
[0107] According to this embodiment, the lens unit 100 further includes a light-shielding member 150 that shields the outer edge of the outermost lens from light, in addition to the multiple lenses 110, the housing member 120, the filter 130, and the sealing member 140. As a result, even if the outer edge of the hard coat layer 12 on the outermost lens is thin, the light-shielding member 150 can block light, thereby preventing a decrease in adhesion at the interface between the anti-reflection film 13 and the hard coat layer 12 and preventing deterioration of the hard coat layer 12.
[0108] The light-shielding member 150 is a single member together with the housing member 120. This makes it possible to prevent an increase in the number of parts due to the light-shielding member 150 that shields the outer edge of the hard coat layer 12 from light.
[0109] Examples of the present invention will be described below, but the present invention is not limited to the scope of the following examples.
[0110] Example 1 First, an optical element 10 of Example 1 was fabricated.
[0111] A plastic lens 11 was prepared using RM-104 manufactured by Nippon Shokubai Co., Ltd. The plastic lens 11 was a meniscus lens with its convex surface facing the object side, and the outer diameter of the plastic lens 11 was approximately 14 mm.
[0112] The surface of the plastic lens 11 was coated with a hard coat layer 12. The hard coat layer 12 was a photocurable resin material made of urethane or the like. The hard coat layer 12 was formed by applying a component liquid of the hard coat layer 12 to the plastic lens 11 by spin coating, heating and drying the component liquid film, and then curing the film with electromagnetic waves such as ultraviolet rays or an electron beam.
[0113] The surface of the hard coat layer 12 was coated with an antireflection film 13. The antireflection film 13 was formed by alternately depositing high-refractive-index films made of SiN and low-refractive-index films made of SiO by sputtering. In this manner, the optical element 10 of Example 1 was fabricated.
[0114] The thickness of the hard coat layer 12 was measured in the optical element 10 of Example 1. The thickness Lx1 of the hard coat layer 12 on the optical axis Lx was 5.4 μm, while the thickness Lx2 of the hard coat layer 12 at the outer edge was 2.1 μm.
[0115] Next, the optical element 10 of Example 1 was subjected to an optical property test and a weather resistance test under the following conditions.
[0116] [Optical Property Test] The optical element 10 of Example 1 was irradiated with fluorescent light from a fluorescent light source and visually inspected for optical distortion.
[0117] [Weathering Test] A weathering test was carried out using a highly accelerated weathering tester, a 7.5 kW super xenon weather meter. In the weathering test, the irradiance was 180 W / m 2 One cycle consisted of 18 minutes of irradiation and rainfall followed by 102 minutes of irradiation alone, and this cycle was repeated 500 times. During and after the weather resistance test, it was checked whether the anti-reflection film 13 had peeled off and whether the hard coat layer 12 had been damaged.
[0118] Table 1 shows the thickness of the hard coat layer 12 at the optical axis of the optical element 10 of Example 1, the thickness of the outer edge of the hard coat layer 12, and the results of the optical property test and weather resistance test of the optical element 10. In this specification, a sample that shows no optical distortion in a visual inspection under a fluorescent light source is marked with "O," and a sample that shows optical distortion is marked with "X." Also in this specification, a sample that shows no peeling of the antireflection film or damage to the hard coat layer in a visual inspection after the weather resistance test is marked with "O," and a sample that shows either peeling of the antireflection film or damage to the hard coat layer is marked with "X."
[0119]
[0120] As shown in Table 1, in the optical element 10 of Example 1, no distortion occurred in the light transmitted through the optical element 10. Furthermore, in the optical element 10 of Example 1, peeling of the antireflection film 13 and damage to the hard coat layer 12 were not observed even after the weather resistance test.
[0121] The optical elements 10 of Examples 2 to 3 were fabricated in the same manner as the optical element 10 of Example 1, and the optical properties tests and weather resistance tests were also carried out on the optical elements 10 of Examples 2 to 3 in the same manner as the optical element 10 of Example 1. In addition, the optical elements of Comparative Examples 1 to 3 were fabricated, and the optical properties tests and weather resistance tests were also carried out on the optical elements of Comparative Examples 1 to 3 in the same manner as the optical element 10 of Example 1. Table 1 shows the thickness of the hard coat layer on the optical axis, the thickness of the outer edge of the hard coat layer, and the results of the optical properties tests and weather resistance tests for the optical elements of Examples 1 to 3 and Comparative Examples 1 to 3.
[0122] In the optical element 10 of Example 2, the thickness of the hard coat layer 12 on the optical axis and the thickness of the outer edge were 8.6 μm and 2.7 μm, respectively, and no distortion occurred in the light transmitted through the optical element 10. Furthermore, even after a weather resistance test, no peeling of the antireflection film 13 or damage to the hard coat layer 12 was confirmed.
[0123] In the optical element 10 of Example 3, the thickness of the hard coat layer 12 on the optical axis and the thickness of the outer edge were 15.8 μm and 5.2 μm, respectively, and no distortion occurred in the light transmitted through the optical element 10. Furthermore, even after a weather resistance test, no peeling of the antireflection film 13 or damage to the hard coat layer 12 was confirmed.
[0124] In the optical element of Comparative Example 1, the thickness of the hard coat layer on the optical axis and the thickness of the outer edge were 1.4 μm and 0.3 μm, respectively, and no distortion occurred in the light transmitted through the optical element of Comparative Example 1. However, after the weather resistance test, either peeling of the antireflection film or damage to the hard coat layer occurred.
[0125] In the optical element of Comparative Example 2, the thickness of the hard coat layer on the optical axis and the thickness of the outer edge were 23.5 μm and 8.3 μm, respectively, and distortion occurred in the light transmitted through the optical element of Comparative Example 2. On the other hand, even after the weather resistance test, no peeling of the antireflection film or damage to the hard coat layer was confirmed.
[0126] In the optical element of Comparative Example 3, the thickness of the hard coat layer at the optical axis and the thickness of the outer edge were 33.9 μm and 10.2 μm, respectively, and distortion occurred in the light transmitted through the optical element of Comparative Example 3. Furthermore, after the weather resistance test, either peeling of the antireflection film or damage to the hard coat layer occurred.
[0127] In the optical elements 10 of Examples 1 to 3, there was no optical distortion, and no peeling of the antireflection film 13 or damage to the hard coat layer 12 occurred. On the other hand, in the optical element of Comparative Example 1, there was no optical distortion, but either peeling of the antireflection film or damage to the hard coat layer occurred. In the optical element of Comparative Example 2, there was no peeling of the antireflection film or damage to the hard coat layer, but there was optical distortion. In the optical element of Comparative Example 3, there was optical distortion, and either peeling of the antireflection film or damage to the hard coat layer occurred.
[0128] The present technology may have the following configurations: (1) An optical element having an optical axis, comprising: a plastic lens; an anti-reflection film disposed on at least one surface of the plastic lens; and a hard coat layer positioned between the plastic lens and the anti-reflection film, wherein the thickness of the hard coat layer on the optical axis is 2 μm or more and 20 μm or less.
[0129] (2) The optical element according to (1), wherein the hard coat layer has a minimum thickness of 2 μm or more and a maximum thickness of 20 μm or less.
[0130] (3) The optical element according to (1) or (2), wherein the hard coat layer has a modulus of elasticity of 5 GPa or more and 12 GPa or less.
[0131] (4) The optical element according to any one of (1) to (3), wherein the plastic lens has a thermal expansion coefficient of 60 ppm / K or more and 150 ppm / K or less.
[0132] (5) The optical element according to any one of (1) to (4), wherein the antireflection film has a thermal expansion coefficient of 1 ppm / K or more and 10 ppm / K or less.
[0133] (6) The optical element according to any one of (1) to (5), wherein the thermal expansion coefficient of the plastic lens is 60 ppm / K or more and 100 ppm / K or less, and the thermal expansion coefficient of the antireflection film is 5 ppm / K or more and 10 ppm / K or less.
[0134] (7) The optical element according to any one of (1) to (6), wherein the difference between the thickness of the hard coat layer on the optical axis and the thickness of the outer edge is 15 μm or less.
[0135] (8) A lens unit comprising: a plurality of lenses; and a housing member that houses the plurality of lenses; wherein the plurality of lenses are arranged in order from the opening of the housing member; and the outermost lens of the plurality of lenses that is located on the opening side of the housing member is an optical element described in any one of (1) to (7).
[0136] (9) The lens unit according to (8), further comprising a light-shielding member that shields the outer edge of the outermost lens from light.
[0137] (10) The lens unit according to (9), wherein the light blocking member is a single member together with the housing member.
[0138] (11) A camera module comprising: the lens unit according to any one of (8) to (10); and an imaging element.
[0139] 10 Optical element 11 Plastic lens 12 Hard coat layer 13 Anti-reflection film
Claims
1. An optical element having an optical axis, comprising: a plastic lens; an anti-reflection film disposed on at least one surface side of the plastic lens; and a hard coat layer located between the plastic lens and the anti-reflection film, wherein the thickness of the hard coat layer on the optical axis is 2 μm or more and 20 μm or less.
2. The optical element according to claim 1, wherein the hard coat layer has a minimum thickness of 2 μm or more and a maximum thickness of 20 μm or less.
3. The optical element according to claim 1 or 2, wherein the hard coat layer has a modulus of elasticity of 5 GPa or more and 12 GPa or less.
4. The optical element according to claim 1 or 2, wherein the thermal expansion coefficient of the plastic lens is 60 ppm / K or more and 150 ppm / K or less.
5. The optical element according to claim 1 or 2, wherein the thermal expansion coefficient of the antireflection film is 1 ppm / K or more and 10 ppm / K or less.
6. The optical element according to claim 1 or 2, wherein the thermal expansion coefficient of the plastic lens is 60 ppm / K or more and 100 ppm / K or less, and the thermal expansion coefficient of the anti-reflection film is 5 ppm / K or more and 10 ppm / K or less.
7. The optical element according to claim 1 or 2, wherein the difference between the thickness of said hard coat layer on said optical axis and the thickness of said outer edge is 15 μm or less.
8. A lens unit comprising: a plurality of lenses; and a housing member that houses the plurality of lenses, wherein the plurality of lenses are arranged in order from an opening of the housing member; and an outermost lens of the plurality of lenses that is located on the opening side of the housing member is an optical element as described in claim 1 or 2.
9. The lens unit according to claim 8, further comprising a light shielding member for shielding an outer edge of the outermost lens from light.
10. The lens unit according to claim 9, wherein the light blocking member is a single member together with the housing member.
11. A camera module comprising the lens unit according to claim 8 and an imaging element.
Citation Information
Patent Citations
Infrared transmission member, infrared camera using the same and method for producing infrared transmission member
JP2006138898A
Plastic lens and method for manufacturing plastic lens
JP2006146131A
Optical product and its manufacturing method
JP2007156342A
Coating material composition for forming primer layer film, and plastic lens
JP2011099074A
Optical lens with scratch-resistant antireflection layer
JP2012088700A