Thermally conductive sheet
A thermally conductive sheet with specific composition and structural features addresses the need for enhanced thermal conductivity and step followability, effectively managing heat dissipation in miniaturized electronic devices by achieving optimal thermal resistance and flexibility.
Patent Information
- Application Number
- PCT/JP2024/010529
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-03
AI Technical Summary
The challenge is to develop a thermally conductive sheet with enhanced thermal conductivity and step followability to effectively manage heat dissipation in miniaturized electronic devices with increasing heat generation, particularly for components mounted on surfaces with steps.
A thermally conductive sheet with a storage modulus of 0.3×10^9 to 1.2×10^9 Pa, containing silicone resin, unreacted silicone oil, and spherical filler particles with controlled BN orientation, optimized particle size distribution, and crushing strength, to achieve improved thermal conductivity and flexibility.
The sheet achieves thermal resistance of 0.07 to 0.12 K/W and excellent step followability, ensuring effective heat dissipation and mechanical flexibility for complex electronic components.
Smart Images

Figure JP2024010529_03102024_PF_FP_ABST
Abstract
Description
Thermally conductive sheet
[0001] The present invention relates to a thermally conductive sheet.
[0002] For heat-generating electronic components such as power devices, transistors, thyristors, and CPUs, efficient heat dissipation is an important issue. Conventional heat dissipation strategies include (1) increasing the thermal conductivity of the insulating layer of the printed wiring board on which the heat-generating electronic components are mounted, and (2) attaching the heat-generating electronic components or the printed wiring board on which the heat-generating electronic components are mounted to a heat sink via electrically insulating thermal interface materials. Silicone resin or epoxy resin filled with ceramic powder is commonly used as the insulating layer and thermal interface material for printed wiring boards.
[0003] As a ceramic powder, boron nitride powder has attracted attention due to its properties such as high thermal conductivity, high insulation, low dielectric constant, etc. For example, Patent Document 1 discloses a boron nitride powder formed by agglomeration of primary particles of boron nitride, which has, in its volumetric particle size distribution, Peak A existing in a region of 5 μm or more and less than 30 μm, and Peak B existing in a region of 50 μm or more and less than 100 μm.
[0004] Japanese Patent Application Laid-Open No. 2020-164365
[0005] Using the boron nitride powder described in Patent Document 1, a thermally conductive sheet with excellent thermal conductivity and electrical insulation can be obtained. However, with the recent trend toward miniaturization of electronic devices and the increase in the amount of heat generated by heat-generating electronic components, a thermally conductive sheet with even better thermal conductivity is required. Furthermore, with the recent increase in the complexity of electronic devices, heat-generating electronic components are sometimes mounted on mounting surfaces with uneven surfaces, and thermally conductive sheets are required to have excellent unevenness-conforming capabilities. Therefore, an object of the present invention is to provide a thermally conductive sheet with excellent thermal conductivity and unevenness-conforming capabilities.
[0006] The present inventors have conducted extensive research to achieve the above object, and have found that they have been able to achieve the above object by controlling the storage modulus and thermal resistance of a thermal conductive sheet. The present invention is based on the above findings and is summarized as follows: [1] A thermal conductive sheet having a storage modulus of 0.3 × 10 9 ~1.2 × 10 9 A thermally conductive sheet having a thermal resistance of 0.07 to 0.12 K / W measured at a clamping torque of 0.5 N m and a pressure of 100 psi. [2] The thermally conductive sheet according to the above item [1], which contains a silicone resin and unreacted silicone oil. [3] The thermally conductive sheet according to the above item [1] or [2], which contains spherical filler. [4] The thermally conductive sheet according to the above item [3], wherein the spherical filler is an agglomerated particle formed by agglomeration of primary particles. [5] The thermally conductive sheet according to any one of the above items [1] to [3], which has a BN orientation degree of 6 to 70.
[0007] According to the present invention, it is possible to provide a thermally conductive sheet having excellent thermal conductivity and step-conforming ability.
[0008] FIG. 1 is a conceptual diagram of the particle size distribution of a thermally conductive filler.
[0009] [Thermal Conductive Sheet] The thermal conductive sheet of the present invention has a storage modulus of 0.3 × 10 9 ~1.2 × 10 9 The thermal resistance measured when the tightening torque is 0.5 N·m is 0.07 to 0.12 K / W. This makes it possible to improve the thermal conductivity and step-following ability of the thermally conductive sheet.
[0010] (Storage Modulus) The storage modulus of the thermally conductive sheet of the present invention is 0.3×10 9 ~1.2 × 10 9 The storage modulus of the thermal conductive sheet is 0.3 × 10 9 If the storage modulus of the thermal conductive sheet is less than 1.2×10 Pa, the thermal conductive sheet may be too soft and may not have sufficient strength. 9 If the storage modulus of the thermal conductive sheet is greater than 1.2 × 10 Pa, the interface thermal resistance of the thermal conductive sheet increases, which may result in poor thermal conductivity of the thermal conductive sheet. 9If the storage modulus is greater than 1.1 × 10 Pa, the flexibility of the thermally conductive sheet may be poor, and the ability to conform to uneven surfaces may be poor. From this viewpoint, the storage modulus of the thermally conductive sheet of the present invention is preferably 1.1 × 10 9 ~0.4 × 10 9 Pa, and more preferably 1.0×10 9 ~0.45 × 10 9 Pa, and more preferably 0.95×10 9 ~0.5 x 10 9 The storage modulus of the thermally conductive sheet can be measured by the method described in the Examples below. The storage modulus of the thermally conductive sheet can be adjusted by adding unreacted silicone oil.
[0011] (Thermal Resistance) The thermal resistance of the thermally conductive sheet of the present invention measured at a tightening torque of 0.5 N·m is 0.07 to 0.12 K / W. It is difficult to achieve a thermal resistance of less than 0.07°C / W (while maintaining electrical insulation). If the thermal resistance of the thermally conductive sheet is greater than 0.12°C / W, it may not be possible to meet the increasingly stringent requirements for thermal conductivity of thermally conductive sheets due to the recent trend toward miniaturization of electronic devices and the increased heat generation of heat-generating electronic components. From this perspective, the thermal resistance of the thermally conductive sheet is preferably 0.07 to 0.11°C / W, and more preferably 0.07 to 0.10°C / W. The thermal resistance of the thermally conductive sheet can be measured using the method described in the Examples below. The thermal resistance of the thermally conductive sheet can also be adjusted by improving the thermal conductivity or flexibility of the sheet.
[0012] (BN Orientation Degree in Sheet) The BN orientation degree in the thermal conductive sheet of the present invention is preferably 6 to 70. When the BN orientation degree in the thermal conductive sheet is 6 to 70, this indicates that the direction of low thermal conductivity of the thermal conductive filler is not aligned in the thickness direction of the thermal conductive sheet, and the thermal conductivity of the thermal conductive sheet can be further improved. From this perspective, the BN orientation degree in the thermal conductive sheet of the present invention is more preferably 7 to 60, even more preferably 8 to 50, and even more preferably 10 to 40. The BN orientation degree in the thermal conductive sheet can be measured by the method described in the Examples below. The BN orientation degree in the thermal conductive sheet can also be adjusted by adjusting the press pressure during sheet preparation, which improves the crushing strength of the filler used.
[0013] (Breakdown voltage) The breakdown voltage of the thermal conductive sheet of the present invention is preferably 15 kV / mm or more. A breakdown voltage of 15 kV / mm or more can meet the increasingly stringent requirements for insulation of thermal conductive sheets due to the recent trend toward miniaturization of electronic devices and the increase in the heat generation of heat-generating electronic components. From this perspective, the breakdown voltage of the thermal conductive sheet is more preferably 20 kV / mm or more, and even more preferably 25 kV / mm or more. The upper limit of the range of the breakdown voltage of the thermal conductive sheet is not particularly limited, but is usually 50 kV / mm. The breakdown voltage of the thermal conductive sheet can be measured by the method described in the Examples below. The breakdown voltage of the thermal conductive sheet can also be adjusted by reducing the filler loading.
[0014] (Thickness) The thickness of the thermally conductive sheet of the present invention is not particularly limited, but is preferably 0.1 to 1 mm, more preferably 0.15 to 0.9 mm, and even more preferably 0.2 to 0.8 mm.
[0015] (Thermal Conductive Filler) The thermally conductive sheet of the present invention preferably contains a thermally conductive filler. The thermally conductive filler used in the thermally conductive sheet of the present invention is not particularly limited as long as it is a thermally conductive filler commonly used in thermally conductive sheets. Examples of thermally conductive fillers used in the thermally conductive sheet of the present invention include amorphous granular fillers, spherical fillers, needle-like fillers, fibrous fillers, and plate-like fillers. These thermally conductive fillers can be used alone or in combination of two or more. Among these thermally conductive fillers, spherical fillers are preferred from the viewpoint of increasing the filling rate of the thermally conductive filler in the thermally conductive sheet and thereby increasing the thermal conductivity of the thermally conductive sheet. Examples of spherical fillers include alumina, silica, calcium carbonate, aluminum nitride, and magnesium oxide. Furthermore, even if the primary particles are not spherical, spherical aggregated fillers can be obtained by agglomerating the primary particles. These spherical fillers can be used alone or in combination of two or more. From the viewpoint of further increasing the thermal conductivity of the thermally conductive sheet, among these spherical fillers, agglomerated particles formed by agglomeration of primary particles are preferred, and agglomerated boron nitride particles formed by agglomeration of primary particles of boron nitride are more preferred.
[0016] <Crushing Strength> The crushing strength of the agglomerated particles formed by agglomeration of primary particles used in the thermal conductive sheet of the present invention is preferably 5 to 15 MPa. If the crushing strength of the agglomerated particles formed by agglomeration of primary particles is 5 MPa or more, the agglomerated particles will collapse during the production of the thermal conductive sheet, preventing the degree of BN orientation in the thermal conductive sheet from increasing. Furthermore, if the crushing strength of the agglomerated particles formed by agglomeration of primary particles is 15 MPa or less, the deformation of the agglomerated particles can reduce voids within the sheet, further improving thermal conductivity. From this perspective, the crushing strength of the agglomerated particles formed by agglomeration of primary particles is more preferably 6 to 13 MPa, and even more preferably 7 to 11 MPa. The crushing strength of the agglomerated particles formed by agglomeration of primary particles can be measured by the method described in the Examples below.
[0017] <Particle Size Distribution of Thermally Conductive Filler> The particle size distribution of the thermally conductive filler is not particularly limited. For example, the particle size distribution of the thermally conductive filler used in the thermally conductive sheet of the present invention may have only a first maximum point, or may have only a first maximum point and a second maximum point whose particle size is larger than that of the first maximum point. However, as shown in FIG. 1 , the particle size distribution of the thermally conductive filler used in the thermally conductive sheet of the present invention preferably has at least a first maximum point (MAX1), a second maximum point (MAX2) whose particle size is larger than that of the first maximum point (MAX1), and a third maximum point (MAX3) whose particle size is larger than that of the second maximum point (MAX2). It is preferable that the particle size at the first maximum point (MAX1) is 0.4 μm or more and less than 10 μm, the particle size at the second maximum point (MAX2) is 10 μm or more and less than 40 μm, and the particle size at the third maximum point (MAX3) is 40 μm or more and 110 μm or less. This can improve the filling efficiency of the thermally conductive filler in the thermally conductive sheet, thereby further improving the thermal conductivity of the thermally conductive sheet. The particle size distribution of the thermally conductive filler used in the thermally conductive sheet of the present invention can be measured by the method described in the Examples below.
[0018] The particle size at the first maximum point (MAX1) is preferably 0.4 μm or more and less than 10 μm. When the particle size at the first maximum point (MAX1) is 0.4 μm or more and less than 10 μm, the filling efficiency of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the particle size at the first maximum point (MAX1) is more preferably 1.0 to 9.0 μm, and even more preferably 2.0 to 8.0 μm.
[0019] The particle size at the second maximum point (MAX2) is preferably 10 μm or more and less than 40 μm. When the particle size at the second maximum point (MAX2) is 10 μm or more and less than 40 μm, the filling efficiency of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the particle size at the second maximum point (MAX2) is more preferably 15 to 36 μm, and even more preferably 18 to 30 μm.
[0020] The particle size at the third maximum point (MAX3) is preferably 40 to 110 μm. When the particle size at the third maximum point (MAX3) is 40 to 110 μm, the filling efficiency of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the particle size at the third maximum point (MAX3) is more preferably 50 to 100 μm, and even more preferably 65 to 90 μm.
[0021] The integrated value (V1) of the frequency between the peak start and peak end in a peak having a first maximum point (MAX1) is preferably 1 to 27% by volume. When the integrated value (V1) is 1 to 27% by volume, the packing density of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the integrated value (V1) is more preferably 5 to 20% by volume. The peak start in a peak having a first maximum point (MAX1) is a minimum point on the smaller particle size side relative to the first maximum point (MAX1). If there is no minimum point on the smaller particle size side relative to the first maximum point (MAX1), the peak start is the end (DS) of the particle size distribution on the smaller particle size side. Furthermore, the peak end in a peak having a first maximum point (MAX1) is a minimum point (MIN1) on the larger particle size side relative to the first maximum point (MAX1). The integrated amount of frequency (V1) is a value obtained by subtracting the frequency of the particle size of the minimum point (MIN1) on the larger particle size side than the first maximum point (MAX1) from the integrated amount of frequency from the particle size of the minimum point on the smaller particle size side than the first maximum point (MAX1) or the particle size at the end (DS) of the particle size distribution on the smaller particle size side to the particle size of the minimum point (MIN1) on the larger particle size side than the first maximum point (MAX1). The reason for subtracting the frequency of the particle size of the minimum point (MIN1) on the larger particle size side than the first maximum point (MAX1) is to prevent the frequency of the particle size of the minimum point (MIN1) on the larger particle size side than the first maximum point (MAX1) from being added to both the integrated amount of frequency from the peak start to the peak end of the peak having the first maximum point (MAX1) and the integrated amount of frequency from the peak start to the peak end of the peak having the second maximum point (MAX2).
[0022] The integrated value (V2) of the frequency between the peak start and peak end in the peak having the second maximum point (MAX2) is preferably 5 to 40% by volume. When the integrated value (V2) is 5 to 40% by volume, the filling efficiency of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the integrated value (V2) is more preferably 10 to 30% by volume. Note that the peak start in the peak having the second maximum point (MAX2) is the minimum point (MIN1) on the smaller particle size side relative to the second maximum point (MAX2). Furthermore, the peak end in the peak having the second maximum point (MAX2) is the minimum point (MIN2) on the larger particle size side relative to the second maximum point (MAX2). The integrated quantity of frequency (V2) is a value obtained by subtracting the frequency of the particle size at the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2) from the integrated quantity of frequency from the particle size at the minimum point (MIN1) on the smaller particle size side of the second maximum point (MAX2) to the particle size at the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2). The reason for subtracting the frequency of the particle size at the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2) is to prevent the frequency of the particle size at the minimum point (MIN2) on the larger particle size side of the second maximum point (MAX2) from being added to both the integrated quantity of frequency from the peak start to the peak end at the peak having the second maximum point (MAX2) and the integrated quantity of frequency from the peak start to the peak end at the peak having the third maximum point (MAX3).
[0023] The integrated value (V3) of the frequency between the peak start and peak end in a peak having a third maximum point (MAX3) is preferably 50 to 90% by volume. When the integrated value (V3) is 50 to 90% by volume, the filling of the thermally conductive filler in the thermally conductive sheet can be further increased, and the thermal conductivity of the thermally conductive sheet can be further improved. From this perspective, the integrated value (V3) is more preferably 60 to 80% by volume. The peak start in a peak having a third maximum point (MAX3) is the minimum point (MIN2) on the smaller particle size side relative to the third maximum point (MAX3). The peak end in a peak having a third maximum point (MAX3) is the minimum point on the larger particle size side relative to the third maximum point (MAX3). If there is no minimum point on the larger particle size side relative to the third maximum point (MAX3), the peak end is the end (DE) of the particle size distribution on the larger particle size side. The integrated amount of frequency (V3) is the value obtained by subtracting the frequency of the particle size of the minimum point (MIN2) on the larger particle size side than the third maximum point (MAX3) from the integrated amount of frequency from the particle size of the minimum point (MIN2) on the smaller particle size side than the third maximum point (MAX3) to the particle size of the minimum point on the larger particle size side than the third maximum point (MAX3), or is the integrated amount of frequency from the particle size of the minimum point (MIN2) on the smaller particle size side than the third maximum point (MAX3) to the particle size at the larger particle size end (DE) of the particle size distribution. The frequency of particle sizes at minimum points on the larger particle size side of the third maximum point (MAX3) is subtracted to prevent the frequency of particle sizes at minimum points on the larger particle size side of the third maximum point (MAX3) from being added to both the cumulative amount of frequency from the peak start to the peak end of a peak having the third maximum point (MAX3) and the cumulative amount of frequency from the peak start to the peak end of a peak having a maximum point adjacent to the third maximum point (MAX3) on the larger particle size side of the third maximum point.
[0024] As long as the filling ability of the thermally conductive filler in the thermally conductive sheet can be improved, the particle size distribution of the thermally conductive filler used in the thermally conductive sheet of the present invention may have other maximum points in addition to the first to third maximum points described above.
[0025] <Method for producing thermally conductive filler> An example of a method for producing the thermally conductive filler used in the thermally conductive sheet of the present invention is described below. The boron nitride particles used in the thermally conductive sheet of the present invention can be produced, for example, by preparing a first thermally conductive filler having a particle size distribution with the first maximum point, a second thermally conductive filler having a particle size distribution with the second maximum point, and a third thermally conductive filler having a particle size distribution with the third maximum point, and then mixing the first to third thermally conductive fillers thus prepared.
[0026] Of the first to third thermally conductive fillers, the second and third thermally conductive fillers each preferably contain at least aggregate boron nitride particles. The first thermally conductive filler may be aggregate boron nitride particles, but is preferably hexagonal boron nitride primary particles. The maximum point of each of the first to third thermally conductive fillers refers to the apex of the peak in the particle size distribution of each of the first to third thermally conductive fillers. The particle size distributions of the first to third thermally conductive fillers are measured in the same manner as the particle size distribution of the thermally conductive fillers described above.
[0027] In the mixing step, the first to third thermally conductive fillers may be mixed so that the volume fraction of the third thermally conductive filler is greater than the volume fraction of the first thermally conductive filler and the volume fraction of the second thermally conductive filler. This can further enhance the packing properties of the thermally conductive fillers. From the viewpoint of improving the thermal conductivity of the thermally conductive sheet, the volume fraction of the third thermally conductive filler is preferably 50 to 90 parts by volume, more preferably 60 to 80 parts by volume, per 100 parts by volume of the first to third thermally conductive fillers combined. From the viewpoint of improving the thermal conductivity of the thermally conductive sheet, the volume fraction of the second thermally conductive filler is preferably 5 to 40 parts by volume, more preferably 10 to 30 parts by volume, per 100 parts by volume of the first to third thermally conductive fillers combined. From the viewpoint of improving the thermal conductivity of the thermal conductive sheet, the volume ratio of the first thermally conductive filler is preferably 1 to 27 parts by volume, and more preferably 5 to 20 parts by volume, relative to 100 parts by volume of the total of the first to third thermally conductive fillers.
[0028] Each of the aggregate boron nitride particles used as the thermally conductive filler can be produced by a production method including, for example, a crushing step of crushing aggregate boron carbide, a nitriding step of nitriding the crushed boron carbide to obtain boron carbonitride, and a decarburizing step of decarburizing the boron carbonitride.
[0029] In the pulverization step, lumped boron carbide (boron carbide lumps) are pulverized using a general pulverizer or crusher. At this time, for example, by adjusting the pulverization time and the amount of boron carbide lumps charged, boron carbide powder having a desired maximum point can be obtained. The maximum point of the boron carbide powder can be measured in the same manner as the maximum point of the boron nitride particles described above. In this way, by adjusting the maximum point of the boron carbide powder to approach the maximum point of the desired boron nitride particles, the first to third boron nitride particles having the above-described maximum points can be obtained.
[0030] Subsequently, in the nitriding step, the boron carbide powder is fired under pressure in an atmosphere that promotes the nitriding reaction, thereby obtaining boron carbonitride.
[0031] The atmosphere in the nitriding step is an atmosphere that promotes the nitriding reaction, and may be, for example, nitrogen gas, ammonia gas, or the like, either alone or in combination. From the viewpoints of ease of nitriding and cost, the atmosphere is preferably nitrogen gas. The content of nitrogen gas in the atmosphere is preferably 95% by volume or more, more preferably 99.9% by volume or more.
[0032] The pressure in the nitriding step is preferably 0.6 MPa or more, more preferably 0.7 MPa or more, and preferably 1.0 MPa or less, more preferably 0.9 MPa or less. The pressure is further preferably 0.7 to 1.0 MPa. The firing temperature in the nitriding step is preferably 1800°C or more, more preferably 1900°C or more, and preferably 2400°C or less, more preferably 2200°C or less. The firing temperature is further preferably 1800 to 2200°C. The pressure conditions and firing temperature are preferably 1800°C or more and 0.7 to 1.0 MPa, as these conditions further favorably promote the nitriding of boron carbide and are industrially appropriate.
[0033] The firing time in the nitriding step is appropriately selected within a range in which nitriding proceeds sufficiently, and is preferably 6 hours or more, more preferably 8 hours or more, and is preferably 30 hours or less, more preferably 20 hours or less.
[0034] In the decarburization step, the boron carbonitride obtained in the nitriding step is subjected to a heat treatment in an atmosphere of atmospheric pressure or higher at a predetermined holding temperature for a certain period of time, thereby obtaining aggregated boron nitride particles formed by aggregation of decarburized and crystallized hexagonal boron nitride primary particles.
[0035] The atmosphere in the decarburization step may be an atmosphere of normal pressure (atmospheric pressure) or a pressurized atmosphere. In the case of a pressurized atmosphere, the pressure may be, for example, 0.5 MPa or less, preferably 0.3 MPa or less.
[0036] In the decarburization step, for example, the temperature is first raised to a predetermined temperature (the temperature at which decarburization can begin), and then further raised to a holding temperature at a predetermined heating rate. The predetermined temperature (the temperature at which decarburization can begin) can be set depending on the system, and may be, for example, 1000°C or higher, 1500°C or lower, and preferably 1200°C or lower. The rate at which the temperature is raised from the predetermined temperature (the temperature at which decarburization can begin) to the holding temperature may be, for example, 5°C / min or lower, and preferably 4°C / min or lower, 3°C / min or lower, or 2°C / min or lower.
[0037] The holding temperature is preferably 1800°C or higher, more preferably 2000°C or higher, from the viewpoint of favorable grain growth and further improving the thermal conductivity of the obtained boron nitride particles. The holding temperature may be preferably 2200°C or lower, more preferably 2100°C or lower.
[0038] The holding time at the holding temperature is appropriately selected within a range in which crystallization sufficiently progresses, and may be, for example, more than 0.5 hours, and from the viewpoint of favorable grain growth, is preferably 1 hour or more, more preferably 3 hours or more, even more preferably 5 hours or more, and particularly preferably 10 hours or more. The holding time at the holding temperature may be, for example, less than 40 hours, and from the viewpoint of preventing excessive grain growth and reducing particle strength, is preferably 30 hours or less, more preferably 20 hours or less.
[0039] In the decarburization step, a boron source may be mixed with the boron carbonitride obtained in the nitriding step as a raw material to carry out decarburization and crystallization. Examples of the boron source include boric acid, boron oxide, or a mixture thereof. In this case, other additives used in the art may be further used as necessary.
[0040] The mixing ratio of boron carbonitride and the boron source is appropriately selected. When boric acid or boron oxide is used as the boron source, the ratio of boric acid or boron oxide may be, for example, 100 parts by mass or more, preferably 150 parts by mass or more, and may be, for example, 300 parts by mass or less, preferably 250 parts by mass or less, relative to 100 parts by mass of boron carbonitride.
[0041] The boron nitride particles obtained as described above may be subjected to a step of classifying them using a sieve to obtain boron nitride particles having a desired particle size distribution (classification step), thereby obtaining the first to third aggregate boron nitride particles usable as the first to third thermally conductive fillers.
[0042] The resulting first to third aggregate boron nitride particles can be mixed to obtain a blend having the particle size distributions with the above-mentioned first to third maximum points. The mixing method is not particularly limited as long as it can uniformly mix the first to third aggregate boron nitride particles. For example, the first to third aggregate boron nitride particles may be mixed using a container rotation type mixer, a container fixed type mixer, or a fluid motion type mixer.
[0043] (Resin) The thermally conductive sheet of the present invention preferably contains a resin. The resin contained in the thermally conductive sheet is not particularly limited, but examples thereof include thermosetting resins such as silicone resin, epoxy resin, phenolic resin, cyanate resin, melamine resin, urea resin, thermosetting polyimide, and unsaturated polyester resin; and thermoplastic resins such as acrylic resin, polyolefin resin, polycarbonate resin, polyester resin, vinyl chloride resin, urethane resin, polyamide resin, and ABS (acrylonitrile-butadiene-styrene) resin. Among these, silicone-based resins and epoxy-based resins are preferred, and silicone resins are more preferred.
[0044] (Silicone Resin and Unreacted Silicone Oil) When the thermally conductive sheet of the present invention contains a silicone resin, it preferably further contains unreacted silicone oil. By containing unreacted silicone oil in addition to the silicone resin, the thermally conductive sheet of the present invention has improved flexibility. As a result, the interfacial thermal resistance of the thermally conductive sheet is further reduced, and the thermal conductivity and step-following ability of the thermally conductive sheet can be further improved.
[0045] <Silicone Resin> The silicone resin used in the thermally conductive sheet of the present invention is not particularly limited, as long as it is a silicone resin commonly used in thermally conductive sheets. Examples of silicone resins used in the thermally conductive sheet of the present invention include radical-curable silicone resins cured with organic peroxides such as acyl-based organic peroxides and alkyl-based organic peroxides, and addition-reaction-curable silicone resins cured with platinum catalysts. Among these silicone resins, radical-curable silicone resins are preferred. Examples of radical-curable silicone resins include silicone polymers with a degree of polymerization of approximately 4,000 to 10,000. Examples of silicone polymers include methyl vinyl-based silicone polymers, methyl phenyl vinyl-based silicone polymers, and methyl fluoroalkyl-based silicone polymers. The silicone resin may also contain additives such as silica fillers and dispersants. The content of the radical-curable silicone resin in the silicone resin is preferably 80 to 100% by volume, more preferably 90 to 100% by volume, and even more preferably 95 to 100% by volume.
[0046] <Unreacted silicone oil> Unreacted silicone oil is a silicone oil that does not have an unsaturated group. Examples of silicone oil that does not have an unsaturated group include methyl silicone oil, in which all organic substituents are methyl groups, and methylphenyl silicone oil, in which all organic substituents are methyl groups and phenyl groups. From the viewpoint of the flexibility of the thermal conductive sheet, among these silicone oils, methyl silicone oil is preferred, and dimethyl silicone oil is more preferred.
[0047] The kinematic viscosity of the unreacted silicone oil is 1 x 10 -2 m 2 It is preferable that the kinematic viscosity of the unreacted silicone oil is 1×10 / s or more. -2 m 2 From this viewpoint, the kinematic viscosity of the unreacted silicone oil is 5×10 / s or more, and therefore, the unreacted silicone oil can be prevented from seeping out from the thermal conductive sheet. -2 m 2 / s or more, and more preferably 6×10-2 m 2 From the viewpoint of further improving the flexibility of the thermally conductive sheet, the kinematic viscosity of the unreacted silicone oil is preferably m / s or more. 2 / s or less, and 2 / s or less is more preferable, and 0.5 m 2 The kinematic viscosity of the unreacted silicone oil can be measured by the method described in the Examples below.
[0048] <Weight Average Molecular Weight> The weight average molecular weight of the silicone resin used in the thermally conductive sheet of the present invention is preferably 30,000 to 1,000,000, more preferably 40,000 to 800,000, and even more preferably 50,000 to 600,000. Furthermore, from the viewpoint of improving the thermal conductivity and step-conforming ability of the thermally conductive sheet, the weight average molecular weight of the unreacted silicone oil is preferably 50,000 to 1,500,000, more preferably 60,000 to 1,200,000, and even more preferably 70,000 to 1,000,000. The weight average molecular weights of the silicone resin and unreacted silicone oil can be measured using gel permeation chromatography.
[0049] (Thermal Conductive Filler Content) The thermal conductive filler content in the thermal conductive sheet of the present invention is preferably 20 to 90 vol%, more preferably 25 to 85 vol%, based on the total 100 vol% of the thermal conductive filler and resin content, or, if unreacted silicone oil is included, based on the total 100 vol% of the thermal conductive filler, silicone resin, and unreacted silicone oil content. A thermal conductive filler content of 20 vol% or more tends to further improve the thermal conductivity of the thermal conductive sheet. Furthermore, a thermal conductive filler content of 90 vol% or less improves the dispersibility of the thermal conductive filler in the thermal conductive sheet.
[0050] (Content of Unreacted Silicone Oil) When the thermally conductive sheet of the present invention contains a silicone resin and unreacted silicone oil, the content of unreacted silicone oil in the thermally conductive sheet of the present invention is preferably 1 to 15% by mass. When the content of unreacted silicone oil in the thermally conductive sheet is 1% by mass or more, the flexibility of the thermally conductive sheet can be further improved, and the storage modulus and thermal resistance of the thermally conductive sheet can be further reduced. When the content of unreacted silicone oil in the thermally conductive sheet is 15% by mass or less, the seepage of unreacted silicone oil from the thermally conductive sheet can be suppressed. From this perspective, the content of unreacted silicone oil in the thermally conductive sheet of the present invention is more preferably 2 to 12% by mass, and even more preferably 5 to 8% by mass.
[0051] The content of unreacted silicone oil in a thermally conductive sheet can be measured, for example, as follows. The initial mass of a 50 mm x 50 mm thermally conductive and heat-dissipating sheet was measured (A), and the sheet was immersed in toluene at a volume 250 times or more the initial mass at room temperature for 24 hours. After immersion, the sample was removed and dried in a dryer at 130°C for 2 hours to remove the toluene, and the dry mass (B) was measured. The content of unreacted silicone oil was calculated from A and B using the following formula: Content (%) of unreacted silicone oil = (A - B) / A x 100
[0052] (Ratio of Unreacted Silicone Oil to Silicone Resin and Unreacted Silicone Oil) When the thermally conductive sheet of the present invention contains a silicone resin and an unreacted silicone oil, the ratio of the content (volume %) of the unreacted silicone oil to the total content (volume %) of the silicone resin and the unreacted silicone oil in the thermally conductive sheet (unreacted silicone oil content / (silicone resin content + unreacted silicone oil content)) is preferably 5 to 55%. When the content of unreacted silicone oil is 5% or more, the flexibility of the thermally conductive sheet can be further improved, and the storage modulus and thermal resistance of the thermally conductive sheet can be further reduced. When the content of unreacted silicone oil is 55% or less, insufficient curing of the thermally conductive sheet can be suppressed. From this perspective, the content of unreacted silicone oil is more preferably 7 to 40%, and even more preferably 10 to 30%.
[0053] (Method for producing thermally conductive sheet) The thermally conductive sheet of the present invention can be produced by a production method including, for example, a step (A) of blending a thermally conductive filler, a silicone resin, and unreacted silicone oil to produce a thermally conductive resin composition, a step (B) of forming the thermally conductive resin composition into a sheet to produce a thermally conductive resin composition sheet, and a step (C) of heating and pressurizing the thermally conductive resin composition sheet.
[0054] (Step (A)) In step (A), a thermally conductive resin composition is prepared by blending a thermally conductive filler, a silicone resin, and unreacted silicone oil. The thermally conductive filler, silicone resin, and unreacted silicone oil used in step (A) have already been described, so further description will be omitted.
[0055] (Step (B)) In step (B), the thermally conductive resin composition is formed into a sheet to produce a thermally conductive resin composition sheet. For example, the thermally conductive resin composition can be formed into a sheet by a doctor blade method or calendar processing. However, if the thermally conductive filler is in the form of agglomerated particles, the agglomerated particles in the thermally conductive resin composition may break down when the thermally conductive resin composition passes through a calendar roll. Therefore, it is preferable to form the thermally conductive resin composition into a sheet by a doctor blade method.
[0056] (Step (C)) In step (C), the thermally conductive resin composition sheet is heated and pressurized. This can further increase the filling of the thermally conductive filler in the thermally conductive sheet, thereby further improving the thermal conductivity of the thermally conductive sheet. From the viewpoint of improving the filling of the thermally conductive filler, the heating temperature of the thermally conductive resin composition sheet is preferably 120 to 200°C, more preferably 130 to 180°C. Furthermore, the pressure applied when pressing the thermally conductive resin composition sheet is preferably 1 to 25 MPa, more preferably 5 to 20 MPa.
[0057] In step (C), a laminate of the thermally conductive resin composition sheet and the glass cloth may be prepared, and the laminate may be heated and pressurized under vacuum to prepare a thermally conductive sheet including the glass cloth.
[0058] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0059] In the thermally conductive sheets of the Examples and Comparative Examples, boron nitride particles were used as the thermally conductive filler. Three types of raw boron nitride particles, each with a specific particle size maximum point, were mixed to produce boron nitride particles with three maximum points. The raw boron nitride particles used as the raw material for the boron nitride particles used in the thermally conductive sheets of the Examples and Comparative Examples were evaluated as follows. (Average Particle Size) The average particle size of the raw boron nitride particles was measured using a Beckman Coulter laser diffraction scattering particle size distribution analyzer (LS-13 320). The obtained average particle size was measured on the raw boron nitride particles without using a homogenizer before the measurement process. The obtained average particle size was the average particle size measured by volume statistics.
[0060] The following evaluations were carried out on boron nitride particles produced by mixing three types of raw material boron nitride particles. (Crushing Strength) The crushing strength of the boron nitride particles was measured in accordance with JIS R1639-5:2007. Specifically, the boron nitride particles were scattered on the sample stage of a microcompression tester ("MCT-211", manufactured by Shimadzu Corporation), and then 20 agglomerated boron nitride particles were selected from the boron nitride particles and subjected to a compression test one by one. The crushing strength (σ: MPa) was calculated using the dimensionless number (α = 2.48) that changes depending on the position within the particle, the crushing test force (P: N), and the particle size (d: μm), as follows: σ = α × P / (π × d 2 The crushing strength of 20 inorganic filler components was plotted in accordance with JIS R1625:2010, and the crushing strength at which the cumulative failure rate was 63.2% was determined as the crushing strength of the boron nitride particles.
[0061] (Particle size distribution) The particle size distribution of the boron nitride particles was measured using a laser diffraction scattering particle size distribution analyzer (LS-13 320) manufactured by Beckman Coulter Co., Ltd. Note that prior to measuring the particle size distribution, the boron nitride particles were not dispersed using a homogenizer or the like.
[0062] Unreacted silicone oil was used to prepare the thermally conductive sheets of the Examples and Comparative Examples. The unreacted silicone oil used in the thermally conductive sheets of the Examples and Comparative Examples was evaluated as follows. (Kinematic Viscosity) The kinematic viscosity of the unreacted silicone oil at 25°C was measured in accordance with the method described in JIS Z 8803:2011.
[0063] The thermally conductive sheets of the examples and comparative examples were evaluated as follows. (Storage modulus) A dynamic viscoelasticity measuring device (Hitachi High-Tech Science Corporation, DMA7100) was used to measure at a frequency of 1 Hz and in a temperature range of 0°C to +200°C. Measurement samples (7 mm x 40 mm) were cut out from films with a thickness of approximately 0.1 to 0.3 mm and measured to determine the storage modulus at 50°C. The main measurement parameters involved in the measurement were as follows: Measurement frequency: 1 Hz; Heating rate: 5°C / min; Sample measurement length: 20 mm; Strain: 0.1%.
[0064] (Thermal resistance) A thermally conductive sheet was placed between a TO-3 model heater and a copper plate. The thermally conductive sheet was then fastened using screws with a nominal diameter of 4 mm and a tightening torque of 0.5 N m. The contact area between one TO-3 model heater and the heat dissipation sheet was approximately 6 cm. 2 Thereafter, a power supply device (manufactured by Kikusui Electronics Co., Ltd., model number: PMC35-3) was used to apply 15 W of power to the TO-3 model heater. Then, 10 minutes after the application of 15 W of power, the temperature (T1) of the TO-3 model heater and the temperature (T2) of the copper plate were measured, and the thermal resistance was calculated using the following formula: Thermal resistance (°C / W) = (T1 - T2) / 15
[0065] (BN orientation degree in sheet) The BN orientation degree in the sheet was measured using an X-ray diffractometer (ULTIMA-IV manufactured by Rigaku Corporation). A sample cut to 1.5 cm x 1.5 cm was prepared, and the sample was irradiated with X-rays to calculate and evaluate the peak intensity ratio (002) / (100) of the (002) plane and the (100) plane.
[0066] (Breakdown voltage) The breakdown voltage of the thermal conductive sheet was calculated based on the value measured in a short-time breakdown test (room temperature 23°C) in accordance with JIS C 2110. The evaluation criteria for insulation are as follows: ◎: Breakdown voltage is 20 kV / mm or more ○: Breakdown voltage is 10 kV / mm or more but less than 20 kV / mm ×: Breakdown voltage is less than 10 kV / mm.
[0067] (Thermal Conductivity) The thermal conductivity of the thermally conductive sheet was measured according to the method described in ASTM D5470:2017. The evaluation criteria for thermal conductivity are as follows: ◎: Thermal conductivity is 5 W / (m·K) or more ○: Thermal conductivity is 3 W / (m·K) or more but less than 5 W / (m·K) ×: Thermal conductivity is less than 3 W / (m·K)
[0068] (Step-following ability) A thermally conductive sheet cut to a length of 20 cm and a width of 5 cm was placed across two glass plates with a height of 0.5 cm. The distance between the two glass plates was gradually increased, and the length between the glass plates was measured when the thermally conductive sheet was placed on the table. The evaluation criteria for step-following ability were as follows: ◎: Distance between the glass plates was less than 8 cm; ○: Distance between the glass plates was 8 cm or more but less than 10 cm; ×: Distance between the glass plates was 10 cm or more.
[0069] The following materials were prepared as raw materials for the thermally conductive sheet. (1) Silicone resin - Silicone resin containing vinyl groups at both ends: manufactured by Dow-Toray Industries, Inc., trade name "CF-3110" (2) Unreacted silicone oil - Unreacted silicone oil 1: Dimethyl silicone oil, manufactured by Wacker Asahi Kasei Co., Ltd., trade name "SILICONE FLUID AK1000000", kinematic viscosity 1 m 2 / s (1 million cSt) Unreacted silicone oil 2: dimethyl silicone oil, manufactured by Wacker Asahi Kasei Co., Ltd., trade name "SILICONE FLUID AK100000", kinematic viscosity 0.1 m 2 / s (100,000 cSt)
[0070] Boron nitride particles A to E each having one maximum point, which serve as raw materials for boron nitride particles having three maximum points, were prepared as follows.
[0071] (Boron nitride particles A) Boron nitride particles A were produced by the following boron carbide synthesis, pressure nitriding step, and decarburization crystallization step.
[0072] (Boron carbide synthesis step) 100 parts by mass of orthoboric acid (hereinafter referred to as boric acid) manufactured by Nippon Denko Corporation and 35 parts by mass of acetylene black (HS100) manufactured by Denka Co., Ltd. were mixed using a Henschel mixer, and then the mixture was filled into a graphite crucible and heated in an arc furnace in an argon atmosphere at 2200°C for 5 hours to produce boron carbide (B 4 The synthesized boron carbide block was pulverized in a ball mill for 3 hours, sieved using a sieve to have a particle size of 75 μm or less, washed with an aqueous nitric acid solution to remove impurities such as iron, and then filtered and dried to produce boron carbide powder with an average particle size of 55 μm.
[0073] (Pressure nitriding step) The synthesized boron carbide was filled into a boron nitride crucible, and then heated in a resistance heating furnace under conditions of 2000°C and 9 atmospheres (0.8 MPa) for 10 hours in a nitrogen gas atmosphere to produce boron carbonitride (B 4 CN 4 ) was obtained.
[0074] (Decarburization crystallization process) 100 parts by mass of the synthesized boron carbonitride and 90 parts by mass of boric acid were mixed using a Henschel mixer, then filled into a boron nitride crucible, and heated in a resistance heating furnace under a pressure of 0.2 MPa in a nitrogen gas atmosphere at a temperature increase rate of 10 ° C. / min from room temperature to 1000 ° C., and then at a temperature increase rate of 2 ° C. / min from 1000 ° C., and a holding time of 10 hours at a firing temperature of 2020 ° C. to synthesize aggregated boron nitride particles in which primary particles aggregated into clumps. The synthesized aggregated boron nitride particles were decomposed and crushed using a Henschel mixer, and then classified using a nylon sieve with 150 μm mesh size. Boron nitride particles A were obtained by crushing and classifying the fired product.
[0075] The average particle diameter (D50) of the obtained boron nitride particles A measured by a laser scattering method was 70 μm. SEM observation revealed that the obtained boron nitride particles A were aggregated boron nitride particles formed by aggregation of primary particles. The obtained boron nitride particles A had a crushing strength of 9 MPa.
[0076] (Boron nitride particles B) Boric acid, melamine, and calcium carbonate (all special reagent grade) were mixed in a mass ratio of 70:50:5, and the mixture was heated from room temperature to 1400°C over 1 hour in a nitrogen gas atmosphere, held at 1400°C for 3 hours, then heated to 1900°C over 4 hours, held at 1900°C for 2 hours, and then cooled to room temperature to produce hexagonal boron nitride. The mixture was then crushed, pulverized, and sieved to prepare boron nitride particles B. The average particle diameter (D50) of boron nitride particles B measured by a laser scattering method was 70 μm. SEM observation revealed that boron nitride particles B were aggregated boron nitride particles formed by aggregation of primary particles. The crushing strength of boron nitride particles B was 2 MPa.
[0077] (Boron nitride particles C) Boron nitride particles C were produced in the same manner as boron nitride particles A, except that boron carbide powder having an average particle size of 10 μm was used. The average particle size (D50) of the obtained boron nitride particles C measured by a laser scattering method was 20 μm. SEM observation revealed that the obtained boron nitride particles C were agglomerated boron nitride particles formed by agglomeration of primary particles. The crushing strength of the obtained boron nitride particles C was 8 MPa.
[0078] (Boron nitride particles D) Boric acid, melamine, and calcium carbonate (all special reagent grade) were mixed in a mass ratio of 70:50:5, and in a nitrogen gas atmosphere, the mixture was heated from room temperature to 1400°C over 1 hour, held at 1400°C for 3 hours, then heated to 1900°C over 4 hours, held at 1900°C for 2 hours, and then cooled to room temperature to produce hexagonal boron nitride. The mixture was then crushed, pulverized, and sieved to prepare boron nitride particles D. The average particle diameter (D50) of boron nitride particles D measured by a laser scattering method was 20 μm. SEM observation revealed that boron nitride particles D were aggregated boron nitride particles formed by aggregation of primary particles. The crushing strength of boron nitride particles D was 1.5 MPa.
[0079] (Boron nitride particles E) Commercially available boron nitride particles (trade name "HGP", manufactured by Denka Co., Ltd.) were used as the boron nitride particles E. The average particle diameter (D50) of the boron nitride particles E measured by a laser scattering method was 3.0 μm. As a result of SEM observation, the boron nitride particles E were found to be scaly primary particles.
[0080] Boron nitride particles 1 and 2 were prepared as follows: [Boron nitride particles 1] Boron nitride particles A, C, and E were mixed together so that the volume ratio of boron nitride particles A, C, and E was 70:15:15, thereby preparing boron nitride particles 1.
[0081] [Boron nitride particles 2] Boron nitride particles B, D, and E were mixed so that the volume ratio of boron nitride particles B, D, and E was 70:15:15 to produce boron nitride particles 2. [Boron nitride particles 3] Boron nitride particles A, B, C, and E were mixed so that the volume ratio of boron nitride particles A, B, C, and E was 35:35:15:15 to produce boron nitride particles 3.
[0082] A thermally conductive sheet was prepared as follows. [Preparation of Thermally Conductive Sheet 1] Boron nitride particles 1, silicone resin, and unreacted silicone oil were weighed out so that the ratio of boron nitride particles 1 was 55 parts by volume, the ratio of silicone resin was 40.5 parts by volume, and the ratio of unreacted silicone oil 1 was 4.5 parts by volume, and then placed in a mixer (product name: Three-One Motor, manufactured by HEIDON). Furthermore, 1 part by mass of curing agent (2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, manufactured by Kayaku Nouryon Co., Ltd., product name "Trigonox 101") per 100 parts by mass of silicone resin, 0.5% by mass of silane coupling agent (dimethyldimethoxysilane, manufactured by Dow-Toray Co., Ltd., product name "DOWSIL Z-6329 Silane", viscosity at 25 ° C: 1 cp) per 100 parts by mass of boron nitride powder, and 15 parts by mass of water per 100 parts by mass of silane coupling agent were added. 100 parts by mass of toluene was further added to the mixer relative to a total of 100 parts by mass of the above-mentioned raw materials, and then the mixture was mixed for 15 hours using a turbine-type mixing blade to produce a thermally conductive resin composition slurry. The slurry was then coated to a thickness of 0.2 mm on a 0.05 mm thick PET film (carrier film) using the doctor blade method and dried at 75 ° C for 5 minutes to produce a sheet-like molded product with a PET film. Two sheets of the sheet-like molded product with a PET film and a glass cloth (manufactured by Unitika, product name "H25") as a reinforcing layer were laminated to produce a laminate. The layer structure of this laminate was PET film / thermally conductive resin composition / glass cloth / thermally conductive resin composition / PET film. The obtained laminate was then heated and pressed for 30 minutes under vacuum (pressure 3.5 kPa), at a temperature of 150 ° C, and a pressure of 15 MPa, and the PET films on both sides were peeled off to produce a 0.2 mm thick sheet. Then, the sheet was subjected to secondary heating at 150° C. under atmospheric pressure for 4 hours to obtain a thermally conductive sheet.
[0083] [Preparation of Thermally Conductive Sheets 2 to 23] Thermally conductive sheets 2 to 23 were prepared in the same manner as thermally conductive sheet 1, except that the type and amount of boron nitride particles, the amount of silicone resin, and the type and amount of unreacted silicone oil were changed as shown in Table 1. The coating thickness of samples with different thicknesses was 0.3 mm.
[0084] The evaluation results of the boron nitride particles, unreacted silicone oil, and thermally conductive sheet are shown in Tables 1 to 4.
[0085]
[0086]
[0087]
[0088]
[0089] From the above evaluation results, the storage modulus of the thermal conductive sheet was determined to be 0.3 × 10 9 ~1.2 × 10 9 It was found that by setting the thermal resistance measured at a tightening torque of 0.5 N·m to 0.07 to 0.12 K / W, a thermally conductive sheet with high thermal conductivity and excellent step-following ability can be obtained.
Claims
1. Storage modulus is 0.3 x 10 9 ~1.2 x 10 9 A thermally conductive sheet having a thermal resistance of 0.07 to 0.12 K / W measured at a clamping torque of 0.5 N·m and a pressure of 100 MPa.
2. The thermally conductive sheet according to claim 1, which contains a silicone resin and unreacted silicone oil.
3. The thermally conductive sheet according to claim 1 or 2, which contains spherical fillers.
4. The thermally conductive sheet according to claim 3, wherein the spherical filler is an agglomerated particle formed by agglomeration of primary particles.
5. The thermally conductive sheet according to claim 3, wherein the degree of BN orientation in the sheet is 6-70.
Citation Information
Patent Citations
Thermally conductive sheet, method for manufacturing thermally conductive sheet, and method for using thermally conductive sheet
WO2019189626A1
Boron nitride powder, heat dissipation sheet, and method for producing heat dissipation sheet
WO2022149435A1
Cited By
Heat dissipation sheet and method for producing heat dissipation sheet
WO2026186734A1