Method for manufacturing surface-emitting semiconductor laser element, and surface-emitting semiconductor laser element
The method of forming a hole layer with oxidized surface treatment and hydrogen annealing in the manufacturing of surface-emitting semiconductor laser devices addresses the challenges of resonance enhancement and threshold reduction, resulting in devices with enhanced efficiency and quality.
Patent Information
- Application Number
- PCT/JP2024/010552
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional methods for manufacturing surface-emitting semiconductor laser devices with photonic crystals face challenges in enhancing the resonance effect and reducing the threshold current while maintaining high output, due to issues with pore filling rates, surface roughness, and Si deposition, which hinder the proximity of the hole and active layers, leading to low coupling efficiency and poor crystallinity.
A method involving the formation of a hole layer with oxidized surface treatment, followed by facet growth and subsequent buried layer growth, including a hydrogen annealing step to achieve a flat and thin buried layer, allowing for closer proximity of the hole and active layers, thereby enhancing the resonance effect and reducing surface roughness and Si concentration.
This approach enables the production of surface-emitting semiconductor laser devices with improved resonance effects, lower threshold values, and higher efficiency by ensuring a high-quality active layer with reduced surface roughness and Si concentration, facilitating better coupling between the void and active layers.
Smart Images

Figure JP2024010552_03102024_PF_FP_ABST
Abstract
Description
Surface-emitting semiconductor laser element manufacturing method and surface-emitting semiconductor laser element
[0001] The present invention relates to a method for manufacturing a surface-emitting semiconductor laser element having a photonic crystal, and to a surface-emitting semiconductor laser element.
[0002] In recent years, development of a photonic-crystal surface-emitting laser (PCSEL) using a photonic crystal (PC) has been progressing.
[0003] For example, Patent Document 1 proposes a method of embedding holes with a hexagonal columnar structure with side surfaces consisting of {10-10} in a group III nitride semiconductor layer using facet selective growth in order to enhance the diffraction effect in the hole layer in a photonic crystal laser and obtain a high resonance effect. It describes how this method realizes a photonic crystal laser element equipped with a photonic crystal having a large filling factor and a large optical confinement coefficient.
[0004] Furthermore, Patent Document 2 proposes a method for embedding holes in a group III nitride semiconductor layer using mass transport in a photonic crystal laser, and describes how this method results in a photonic crystal laser with a large coupling coefficient for light waves propagating through the photonic crystal layer.
[0005] Furthermore, Patent Document 3 discloses that a photonic crystal layer (hole layer) is formed by performing a first burying growth for burying holes by facet growth and a second burying growth for flattening the surface.
[0006] Japanese Patent No. 7101370 JP 2020-38892 A WO2018 / 155710 A1
[0007] However, when the technique described in Patent Document 1 is used, although a hole layer with a sufficient hole filling rate can be formed, the thickness of the layer for embedding the hole layer becomes large, and the distance between the hole layer and the active layer cannot be reduced, and therefore the resonance effect in the hole layer cannot be enhanced.
[0008] The inventors of the present application have also discovered that when voids are filled using mass transport, a large amount of Si deposited on the surface where the voids are formed causes significant surface roughness. This surface roughness hinders the growth of a high-quality active layer with high flatness on the filling layer, and also prevents the void layer and the active layer from being brought sufficiently close together, making it difficult to improve the coupling efficiency between the void layer and the active layer. Furthermore, when a high concentration of Si is introduced into a GaN film, point defects are likely to be introduced into the film. Therefore, it is preferable to remove the large amount of Si deposited on the surface from this perspective as well.
[0009] For these reasons, it has been difficult in the prior art to increase the resonance effect and lower the threshold current while maintaining a high output.
[0010] An object of the present invention is to provide a method for manufacturing a surface-emitting semiconductor laser device that can increase the resonance effect by bringing the air hole layer and the active layer close to each other, has a high-quality active layer, has a low threshold value, and is highly efficient, and to provide such a surface-emitting semiconductor laser device.
[0011] A method for manufacturing a surface-emitting semiconductor laser element according to one embodiment of the present invention includes: (a) forming a hole-formation preparation layer on a substrate; (b) forming holes in the hole-formation preparation layer, arranged two-dimensionally at each of lattice points, to form a hole-formation layer; (c) oxidizing the surface of the hole-formation layer to form an oxide film, and then removing the oxide film; (d) forming a first burying layer by facet growth that closes the holes; (e) growing a second burying layer that flatly buries the first burying layer, to form a first guiding layer that includes a vacancy layer having vacancies corresponding to the holes; and (f) performing crystal growth of a semiconductor layer including an active layer on the first guiding layer.
[0012] A method for manufacturing a surface-emitting semiconductor laser element according to another embodiment of the present invention is a method for manufacturing a surface-emitting semiconductor laser element, comprising: (a) forming a hole formation preparation layer on a substrate; (b) forming holes in the hole formation preparation layer, which are two-dimensionally arranged at each of lattice points, to form a hole formation layer; (c) oxidizing the surface of the hole formation layer to form an oxide film, and then removing the oxide film; (d) forming a first burying layer by facet growth that closes the holes; (e) growing a second burying layer that flatly buries the first burying layer, to form a first guiding layer that includes a vacancy layer having vacancies corresponding to the holes; (f) flattening the surface of the first guiding layer by annealing in a hydrogen atmosphere; and (g) performing crystal growth of a semiconductor layer including an active layer on the flat-etched first guiding layer.
[0013] According to yet another embodiment of the present invention, there is provided a surface-emitting semiconductor laser element comprising: an n-type semiconductor layer; a first guide layer having an vacancy layer formed on the n-type semiconductor layer, the vacancy layer having vacancies arranged two-dimensionally at each lattice point; and a buried layer formed on the vacancy layer and closing the vacancies; a semiconductor layer formed on the buried layer and including an active layer; and a second guide layer formed on the semiconductor layer including the active layer, wherein the distance from the top surfaces of the vacancies in the vacancy layer to the active layer is 4 to 200 nm.
[0014] 1A is a cross-sectional view schematically showing an example of the structure of a PCSEL device according to a first embodiment; FIG. 1B is an enlarged cross-sectional view schematically showing holes arranged in the hole layer shown in FIG. 1A; FIG. 1C is a plan view schematically showing the top surface of a PCSEL device; FIG. 1D is a cross-sectional view schematically showing a cross section in a plane parallel to the n-side guide layer; FIG. 1E is a plan view schematically showing the bottom surface of a PCSEL device; FIG. 1F is a flowchart showing a method for manufacturing a PCSEL device according to a first embodiment; FIG. 1G is a cross-sectional view schematically showing a cross section of an n-side guide layer in steps S0 to S3 of forming a buried layer; FIG. 1H is a plan view schematically showing main and sub-openings in a resist, and main and sub-holes after etching; FIG. 1I is a diagram schematically showing a cross section perpendicular to the central axis CX of a formed hole layer; FIG. 1I shows a SIMS profile in the depth direction of a PCSEL device (EMB) manufactured by performing a surface oxidation / oxide film removal process (step S1); and FIG. 1J shows a SIMS profile in the depth direction of a PCSEL device (CMP) manufactured without performing the surface oxidation / oxide film removal process (step S1). 9A is an enlarged cross-sectional view showing an example of the structure of a PCSEL element according to a second embodiment; FIG. 9B is an enlarged cross-sectional view showing an example of the structure of the void layer and voids arranged in the void layer in FIG. 9A; FIG. 9C is a flowchart showing a method for manufacturing a PCSEL element according to a second embodiment; FIG. 9D is a cross-sectional view showing an example of the structure of a PCSEL element according to a second embodiment; FIG. 9E is a schematic cross-sectional view showing the cross section of an n-side guide layer in step S3A; 2 13 is a SEM image showing a cross section after etching by annealing. 14 is a diagram showing an AFM image of the surface of samples (i) to (iv) shown in Fig. 12. 15 is a graph plotting the surface roughness Ra in a 20 μm × 20 μm area against the thickness DE of the buried layer after etching.
[0015] In the following, preferred embodiments of the present invention will be described, but these may be modified and combined as appropriate. In the following description and accompanying drawings, substantially the same or equivalent parts are designated by the same reference numerals.
[0016] [First Embodiment] 1. Structure of Photonic Crystal Surface-Emitting Laser Element A photonic crystal surface-emitting laser element (PCSEL element) is a surface-emitting semiconductor laser element that has a resonator layer in a direction parallel to semiconductor light-emitting structure layers (n-side guide layer, light-emitting layer, p-side guide layer) that constitute a light-emitting element, and emits coherent light in a direction perpendicular to the resonator layer.
[0017] That is, in a PCSEL element, light waves propagating in a plane parallel to the air hole layer (photonic crystal layer) are diffracted by the diffraction effect of the photonic crystal to form a two-dimensional resonance mode, and are also diffracted in a direction perpendicular to the parallel plane. That is, in a PCSEL element, the light extraction direction is perpendicular to the resonance direction (in the plane parallel to the air hole layer).
[0018] Fig. 1A is a cross-sectional view schematically illustrating an example of the structure of a photonic crystal surface-emitting laser device (PCSEL device) 10 according to an embodiment of the present invention, and Fig. 1B is an enlarged cross-sectional view schematically illustrating an air hole layer 14P and air holes 14K arranged in the air hole layer 14P in Fig. 1A.
[0019] 2A is a plan view schematically showing the upper surface of the PCSEL device 10. FIG. 2B is a cross-sectional view schematically showing the cross section of the hole layer 14P in a plane parallel to the n-side guide layer 14, and FIG. 2C is a plan view schematically showing the lower surface of the PCSEL device 10.
[0020] 1A, a semiconductor structure layer 11 is formed on a light-transmitting device substrate 12. The semiconductor layers are stacked perpendicularly to the central axis CX of the semiconductor structure layer 11.
[0021] The semiconductor structure layer 11 is made of a hexagonal nitride semiconductor, for example, a GaN-based semiconductor, in this embodiment.
[0022] More specifically, a semiconductor structure layer 11 consisting of a plurality of semiconductor layers is formed on an element substrate 12, in this order: an n-clad layer (first clad layer of a first conductivity type) 13; an n-side guide layer (first guide layer) 14 which is a guide layer provided on the n-side; a light distribution adjustment layer 23; an active layer (ACT) 15; a p-side guide layer (second guide layer) 16 which is a guide layer provided on the p-side; an electron barrier layer (EBL: Electron Blocking Layer) 17; a p-clad layer (second clad layer of a second conductivity type) 18; and a p-contact layer 19.
[0023] Although the case where the first conductivity type is n-type and the second conductivity type opposite to the first conductivity type is p-type will be described, the first conductivity type and the second conductivity type may be p-type and n-type, respectively.
[0024] The element substrate 12 is a hexagonal GaN single crystal substrate that has a high transmittance for light emitted from the active layer 15. More specifically, the element substrate 12 is a hexagonal GaN single crystal substrate whose main surface (crystal growth surface) is a +c plane, which is a {0001} plane in which Ga atoms are arranged on the outermost surface. The back surface (light emission surface) is a -c plane, which is a (000-1) plane in which N atoms are arranged on the outermost surface. The -c plane is suitable as a light emission surface because it is resistant to oxidation and the like.
[0025] Although the element substrate 12 is not limited to this, a so-called just substrate or, for example, a substrate whose main surface is offset by about 1° in the m-axis direction is preferable. For example, a substrate whose main surface is offset by about 0.3 to 0.7° in the m-axis direction can obtain mirror-finish growth under a wide range of growth conditions.
[0026] The rear surface of the substrate opposite to the main surface is the light emitting surface, which is the "-c" plane, which is the (000-1) plane with N atoms arranged on the outermost surface. The -c plane is resistant to oxidation and is therefore suitable as a light extraction surface.
[0027] The composition, thickness, and other configurations of each semiconductor layer will be explained below, but these are merely examples and can be modified as appropriate.
[0028] The n-clad layer 13 is, for example, n-Al having an Al composition of 4%. 0.04 Ga 0.96The aluminum (Al) composition ratio is set so that the refractive index is smaller than that of the layer adjacent to the active layer 15 (i.e., the n-side guide layer 14).
[0029] The n-side guide layer 14 is composed of a lower guide layer 14A, an air-hole layer 14P, which is a photonic crystal layer (PC layer), and a buried layer 14B. As shown in FIG. 1B, the air-hole layer 14P has a thickness d PC The buried layer 14B has a thickness DE. For example, the hole layer 14P has a thickness d PC is 40 to 180 nm.
[0030] In this specification, the air hole layer 14P refers to the layer portion of the n-side guide layer 14 that extends from the upper end to the lower end of the air holes (see FIG. 1B). PC is equal to the height of the hole.
[0031] The lower guide layer 14A is made of n-GaN and has a thickness of 100 to 400 nm, for example. The air hole layer 14P is made of n-GaN and has a thickness (or the height of the air holes 14K) of 40 to 180 nm.
[0032] The buried layer 14B is made of n-GaN or n-InGaN, or undoped GaN or undoped InGaN. Alternatively, it may be a layer in which these semiconductor layers are stacked. The thickness DE of the buried layer 14B is, for example, 4 to 200 nm. The buried layer 14B is made of a first buried layer 14B1 and a second buried layer 14B2. In other words, the buried layer 14B is a stacked buried layer in which the second buried layer 14B2 is stacked on the first buried layer 14B1.
[0033] On the second buried layer 14B2, which is the surface layer of the buried layer 14B, there is provided a light distribution adjustment layer 23, which is a hetero semiconductor layer (dissimilar semiconductor layer) that has a different crystal composition from that of the second buried layer 14B2 and forms a hetero structure with the second buried layer 14B2.
[0034] The light distribution-adjusting layer 23 may be a semiconductor layer of the same conductivity type as the second buried layer 14B2, or at least one of them may be an i-layer (intrinsic semiconductor layer).
[0035] The light distribution adjustment layer 23 is provided between the buried layer 14B and the active layer 15, and has a function of adjusting the coupling efficiency between the light propagating in the hole layer 14P and the hole layer 14P serving as a resonator. Alternatively, the light distribution adjustment layer 23 may function as an SCH (Separate Confinement Heterostructure) layer used for the active layer of a bulk structure and a quantum well structure. In this embodiment, the light distribution adjustment layer 23 is made of undoped In 0.03 Ga 0.97 The composition or refractive index and layer thickness of the light distribution adjustment layer 23 are selected depending on the adjustment of coupling efficiency.
[0036] The n-side semiconductor layer including the n-side guide layer 14 and the light distribution-adjusting layer 23 is also referred to as a first semiconductor layer, but the light distribution-adjusting layer 23 does not necessarily have to be provided.
[0037] The active layer 15, which is a light-emitting layer, is a multiple quantum well (MQW) layer having, for example, two quantum well layers. The barrier layer and quantum well layer of the MQW are made of GaN (layer thickness 6.0 nm) and InGaN (layer thickness 4.0 nm), respectively. The central emission wavelength of the active layer 15 is 440 nm.
[0038] The active layer 15 is preferably located within 180 nm of the air hole layer 14P (i.e., within the period PK of the air holes), in which case a high resonance effect can be obtained by the air hole layer 14P.
[0039] The p-side guide layer 16 is an undoped In 0.02 Ga 0.98 It consists of a p-side guide layer (1) 16A which is an N layer (layer thickness 70 nm) and a p-side guide layer (2) 16B which is an undoped GaN layer (layer thickness 180 nm).
[0040] The p-side guide layer 16 is an undoped layer in consideration of light absorption by a dopant (Mg: magnesium, etc.), but may be doped to obtain good electrical conductivity. In addition, the In composition and layer thickness of the p-side guide layer (1) 16A can be appropriately selected to adjust the electric field distribution in the oscillation operation mode.
[0041] The electron barrier layer (EBL) 17 is a p-type Al doped with magnesium (Mg). 0.2 Ga 0.8 The N layer has a thickness of, for example, 15 nm.
[0042] The p-cladding layer 18 is made of Mg-doped p-Al 0.06 Ga 0.94 The p-cladding layer 18 is an N layer having a thickness of, for example, 600 nm. The Al composition of the p-cladding layer 18 is preferably selected so that the refractive index is smaller than that of the p-side guide layer 16. The p-cladding layer 18 functions as a first p-cladding layer.
[0043] The p-contact layer 19 is an Mg-doped p-GaN layer having a thickness of, for example, 20 nm. The carrier density of the p-contact layer 19 is set to a concentration that allows for ohmic contact with the transparent electrode 29, which is a transparent conductive layer provided on the surface of the p-contact layer 19. Instead of p-type GaN, p-type or undoped InGaN may be used. Alternatively, a layer in which a GaN layer and an InGaN layer are stacked may be used.
[0044] The layer consisting of the p-side guide layer 16, the electron barrier layer 17, the p-cladding layer 18 and the p-contact layer 19 is also referred to as a second semiconductor layer.
[0045] In this specification, the terms "n-side" and "p-side" do not necessarily mean n-type and p-type. For example, an n-side guide layer refers to a guide layer provided on the n-side of the active layer, and may be an undoped layer (or i-layer).
[0046] The n-cladding layer 13 may be composed of multiple layers instead of a single layer, and in that case, all layers do not need to be n-layers (n-doped layers) and may include an undoped layer (i-layer). The same applies to the p-side guide layer 16 and the p-cladding layer 18.
[0047] Furthermore, it is not necessary to provide all of the semiconductor layers described above, and it is sufficient to have a configuration having a first semiconductor layer of a first conductivity type, a second semiconductor layer of a second conductivity type, and an active layer (light-emitting layer) sandwiched between these layers.
[0048] Furthermore, in this embodiment, the case where the void layer 14P (photonic crystal layer) is provided in the first semiconductor layer (n-type semiconductor layer) has been described, but the void layer may be provided in the second semiconductor layer (p-type semiconductor layer).
[0049] On the p-contact layer 19, a p-electrode 20B (second electrode) is formed as a transparent electrode / Ag / Au layer, in which a transparent electrode 29 (not shown), a silver (Ag) layer, and a gold (Au) layer are laminated in this order. That is, the p-electrode 20B functions as a light-reflecting layer, and the interface between the transparent electrode 29 and the Ag layer of the p-electrode 20B is a reflective surface SR. The reflective surface SR is provided parallel to the pore layer 14P.
[0050] The p-electrode 20B has a circular shape with a diameter RA centered on the central axis CX of the void formation region 14R. Specifically, the transparent electrode 29 has a diameter RA of, for example, 300 μm when viewed from above (i.e., when viewed from a direction perpendicular to the semiconductor structure layer 11). Note that Pd, Al, Al alloys, etc. may also be used for the p-electrode 20B. A pad electrode, etc. may also be provided on the p-electrode 20B.
[0051] The transparent electrode 29 is formed of a transparent conductor, such as indium tin oxide (ITO). Note that the transparent electrode 29 is not limited to ITO, and other transparent conductors such as zinc tin oxide (ZTO), GZO (ZnO:Ga), and AZO (ZnO:Al) can be used.
[0052] The side and top surfaces of the semiconductor structure layer 11 and the side surfaces of the p-electrode 20B are made of SiO 2 The insulating film 21 is formed so as to overlap the p-electrode 20B and cover the edge of the upper surface of the p-electrode 20B.
[0053] The insulating film 21 also functions as a protective film, protecting the aluminum (Al)-containing crystal layer that constitutes the PCSEL element 10 from corrosive gases and the like. It also prevents short circuits caused by deposits or solder creeping up during mounting, contributing to improved reliability and yield. The insulating film 21 is made of SiO 2 Not limited to ZrO 2 , HfO 2 , TiO2 , Al 2 O 3 , SiNx, Si, etc. can be selected.
[0054] A circular cathode electrode 20A (first electrode) (see FIG. 2C) is formed on the rear surface of the element substrate 12. An anti-reflection (AR) coating layer 27 is formed on the inner surface of the cathode electrode 20A.
[0055] The cathode electrode 20A is made of Ti / Au and is in ohmic contact with the element substrate 12. In addition to Ti / Au, the electrode material can be selected from Ti / Al, Ti / Rh, Ti / Al / Pt / Au, Ti / Pt / Au, and the like.
[0056] The light emitted from the active layer 15 is diffracted by the air hole layer (PC layer) 14P. The light is diffracted by the air hole layer 14P (diffraction surface WS), and the light directly emitted from the air hole layer 14P (direct diffracted light Ld: first diffracted light) and the light diffracted by the air hole layer 14P and reflected by the reflection surface SR (reflected diffracted light Lr: second diffracted light) are emitted to the outside from a light emission region 20L ( FIG. 2C ) on the rear surface (emission surface) 12R of the element substrate 12.
[0057] 2B, in the hole layer 14P, the holes 14K are periodically arranged within, for example, a rectangular hole-forming region 14R. As shown in FIG. 2C, the anode region RA is formed so as to be included within the hole-forming region 14R.
[0058] The cathode electrode 20A is provided as a ring-shaped electrode outside the p-electrode 20B so as not to overlap the p-electrode 20B when viewed from a direction perpendicular to the pore layer 14P.
[0059] The region inside the cathode electrode 20A is a light emitting region 20L. Also provided is a bonding pad 20C that is electrically connected to the cathode electrode 20A and to which a wire for supplying power from an external source is connected.
[0060] 2. Manufacturing Method of Hole Layer and Recrystallization Growth The manufacturing process of the hole layer and recrystallization growth are described below. Metalorganic Vapor Phase Epitaxy (MOVPE) was used as the crystal growth method. Note that the following describes the formation method using the case where the hole layer 14P is a double-lattice photonic crystal layer as an example, but single-lattice photonic crystal layers and multi-lattice photonic crystal layers can also be formed in the same way.
[0061] (a) Manufacturing Flow Fig. 3 is a flowchart showing a manufacturing method of the PCSEL device 10. Below, with reference to Fig. 3, a detailed description will be given of the process of manufacturing the PCSEL device 10 by forming air holes in the vacancy layer by filling the recesses (holes) with growth, and then growing the active layer and p-side guide layer.
[0062] 4 is a cross-sectional view schematically showing the cross section of the n-side guide layer 14 in steps S0 to S3 of forming the buried layer 14B. For ease of explanation and understanding, Fig. 4 illustrates a case where the hole layer 14P is a single-lattice photonic crystal layer, but a multi-lattice photonic crystal layer can also be formed in the same manner.
[0063] The buried layer 14B (laminated buried layer) formed by recrystallization growth on the air-hole will be described in detail below with reference to Figures 3 and 4. (Step S0) Formation of Holes First, an n-type Al layer having an Al composition of 4% is formed on the element substrate 12 as the n-clad layer 13. 0.04 Ga 0.96 An N layer was grown on the n-cladding layer 13. Subsequently, as shown in FIG. 4, a hole formation preparation layer 14E, which is an n-type GaN layer, was grown on the n-cladding layer 13. This hole formation preparation layer 14E is a preparation layer for forming the lower guide layer 14A and the air hole layer 14P containing air holes. The hole formation preparation layer 14E has a surface (upper surface) consisting of a flat (0001) plane.
[0064] After forming the hole formation preparation layer 14E, the substrate was removed from the chamber of the MOVPE apparatus, and fine recesses (holes) were formed on the surface of the growth layer. After obtaining a clean surface by cleaning, a silicon nitride film (SiN x A resist for electron beam lithography was applied thereon, and the substrate was placed in an electron beam lithography system to pattern a two-dimensional periodic structure.
[0065] 5 is a plan view schematically showing the main opening K1 and sub-opening K2 in the resist, and the main hole 14H1 and sub-hole 14H2 after etching. As shown in FIG. 5, a pattern was performed in which pairs of openings, each consisting of an oval-shaped main opening K1 and a sub-opening K2 smaller than the main opening K1, were two-dimensionally arranged in the plane of the resist in a square lattice pattern with a period PK. Note that for clarity of the drawing, the openings are shown hatched.
[0066] More specifically, the main apertures K1 are arranged two-dimensionally with their centers of gravity CD1 in two mutually orthogonal directions (x direction and y direction) on lattice points of a square lattice with a period P K. Similarly, the sub-apertures K2 are arranged two-dimensionally with their centers of gravity CD2 in the x direction and y direction on lattice points of a square lattice with a period P K.
[0067] The major axes of the main aperture K1 and the sub aperture K2 are parallel to the <11-20> direction of the crystal orientation, and the minor axes of the main aperture K1 and the sub aperture K2 are parallel to the <1-100> direction.
[0068] The center of gravity CD2 of the sub-opening K2 is spaced apart from the center of gravity CD1 of the main opening K1 by Δx and Δy. Here, Δx=Δy. That is, the center of gravity CD2 of the sub-opening K2 is spaced apart from the center of gravity CD1 of the main opening K1 in the <1-100> direction.
[0069] The distance Δx, Δy between the centers of gravity of the main opening K1 and the sub-opening K2 was set to Δx=Δy=0.46PK. After the patterned resist was developed, SiN x The film was selectively dry-etched to form main openings K1 and sub-openings K2 arranged two-dimensionally on the lattice points of a square lattice with a period PK.x formed to penetrate the membrane.
[0070] The period (hole spacing) PK was set to PK=177.5 nm in order to set the oscillation wavelength (λ) to 438 nm.
[0071] Subsequently, the resist is removed, and the patterned SiN x Using the film as a hard mask, recesses (holes) were formed in the GaN surface. The GaN was dry-etched in the depth direction using a chlorine-based gas and argon gas in an ICP-RIE apparatus, thereby forming a main hole 14H1 and a sub-hole 14H2, which were oblong cylindrical recesses dug perpendicular to the GaN surface.
[0072] The recesses (holes) dug in the GaN surface by the etching are simply referred to as holes to distinguish them from air holes in the vacancy layer 14P. When there is no particular need to distinguish between the main holes 14H1 and the sub-holes 14H2, they may be collectively referred to as holes 14H.
[0073] The shape of the hole 14H is not limited to an elongated cylindrical shape, but may be a cylindrical shape, a polygonal shape, or the like.
[0074] As a result of the above, holes 14H were formed in the hole formation preparation layer 14E, and a hole formation layer 14J was formed (FIG. 4, S0).
[0075] (Step S1) Surface Oxidation / Oxide Film Removal The substrate in which the holes 14H are formed is degreased and cleaned, and then the SiN x The membrane was removed.
[0076] SiN x After removing the film, the 2 UV light (ultraviolet light) is irradiated while gas is flowing. 2 The gas was activated, and the surface of the hole forming layer 14J was oxidized (for 10 minutes) by the generated ozone. 2 (glass) was formed on the upper surface of the hole-forming layer 14J and on the surface inside the hole 14H.
[0077] After the ozone treatment, the substrate was immersed in buffered hydrofluoric acid (BHF) to remove the oxide film formed on the surface. Through the above steps, Si bonded to Ga was removed.
[0078] Finally, the substrate was immersed in a semiconductor cleaning solution (Furuuchi Chemical: SemicoClean23) containing about 1% tetramethylammonium hydroxide (TMAH) for 10 minutes, and then rinsed with water.
[0079] (Step S2) Hole Closure - First Burying Growth Next, the substrate (FIG. 4) in which the hole 14H was formed (Step S0) and the surface oxidation / oxide film removal process (Step S1) was performed was degreased and cleaned, and then it was introduced back into the reactor of the MOVPE apparatus and recrystallization growth was performed. Specifically, ammonia (NH) and trimethylgallium (TMG) were supplied to perform the first burying growth by facet growth, and the opening of the hole 14H was closed.
[0080] Specifically, the first burying growth was performed at a first temperature (920° C.) at which the shape of the hole 14H was transformed by mass transport into a shape composed of thermally stable surfaces.
[0081] More specifically, in this first temperature region, N atoms are attached to the top surface of the growth substrate, so that N-polar faces are selectively grown. Therefore, as shown in FIG. 4, crystals with {1-101} facets are selectively grown. When the opposing {1-101} facets collide, the holes 14H are blocked and filled (facet growth). This facet growth results in a first filling growth, forming vacancies 14K corresponding to the holes 14H.
[0082] In FIG. 4, the hole formation layer 14J (GaN layer) before the buried layer 14B is formed is indicated by a broken line.
[0083] (Step S3) Planarization Filling - Second Filling Growth Next, the hole 14H was closed by facet growth, and then a second filling layer 14B2 with a thickness of 50 nm was grown. The second filling layer 14B2 was grown by raising the substrate temperature (growth temperature) to 1050°C (second filling temperature) and then supplying trimethylgallium (TMG) and NH3. The second filling temperature was higher than the first filling temperature. However, the temperature relationship between the second filling temperature and the first filling temperature may be reversed as long as the growth surface of the second filling layer 14B2 can be grown to a (0001) plane.
[0084] 4, a second buried layer 14B2 having a (0001) plane at its surface is formed by a thermal effect to generate mass transport, and a second buried layer 14B2 is formed by the first and second buried layer growth processes.
[0085] For ease of explanation, the layer extending from the upper surface of the void layer 14P (the surface closer to the active layer 15) to the upper surface 14JS of the hole-forming layer 14J (including a part of the hole-forming layer 14J) is referred to as the first buried layer 14B1, and the layer extending from the upper surface 14JS of the hole-forming layer 14J to the flat surface formed by the second buried growth is referred to as the second buried layer 14B2 (see S3 in FIG. 4).
[0086] The entire semiconductor layer from the upper surface of the void layer 14P to the upper surface of the second buried layer 14B2 (including a part of the hole-forming layer 14J) is referred to as the buried layer 14B.
[0087] Here, the thickness of the first buried layer 14B1 is defined as D1, and the thickness of the second buried layer 14B2 is defined as D2. Therefore, the thickness of the buried layer 14B is given by D = D1 + D2. In this specification, the "top surface" of each semiconductor layer of the n-side guide layer (first guide layer) 14 refers to the surface closer to the active layer 15.
[0088] In this embodiment, GaN is used for the second burying growth. The second burying layer 14B2 also functions as a light distribution adjusting layer for adjusting the coupling efficiency (light field) between light and the hole layer 14P.
[0089] That is, in this embodiment, undoped GaN is used for the first buried growth and the second buried growth, but the first buried growth and the second buried growth are not limited to GaN, and n-GaN, n-InGaN, undoped GaN, undoped InGaN, or a combination of these semiconductors can also be used.
[0090] (Step S4) Recrystallization Growth Subsequently, crystal growth of the layer above the light distribution adjustment layer 23 was carried out in the reactor on the substrate on which the etching of the buried layer 14B had been performed.
[0091] Specifically, the light distribution adjustment layer 23 is grown on the second burying layer 14B2. Specifically, the light distribution adjustment layer 23 is made of undoped In 0.03 Ga 0.97 It is an N layer, and is a semiconductor layer (heterogeneous semiconductor layer) having a different crystal composition from the buried layer 14B (GaN layer).
[0092] Next, an active layer 15, a p-side guide layer (second guide layer) 16, an electron barrier layer (EBL) 17, a p-cladding layer 18, and a p-contact layer 19 were grown in this order on the light distribution-adjusting layer 23. In this way, the PCSEL device 10 was fabricated.
[0093] (b) Vacancy Layer The above-described filling process formed a vacancy layer 14P with a double lattice structure in which vacancies 14K, each consisting of a pair of a main vacancy 14K1 and a subvacancy 14K2, are two-dimensionally arranged at each square lattice point. Here, the subvacancies 14K2 have a smaller vacancy diameter and height than the main vacancies 14K1. In the present invention, the upper surface of the vacancies in the vacancy layer 14P with a multi-lattice structure refers to the upper surface of the main vacancies 14K1 or the subvacancies 14K2 that is closer to the upper layer (active layer) (i.e., the vacancies having a shallower upper surface). The vacancies 14K are not limited to vacancies consisting of a main vacancy 14K1 and a subvacancy 14K2 of different sizes (vacancy pairs), but may also be configured as a single lattice structure in which vacancies of the same size are two-dimensionally arranged at each square lattice point.
[0094] 6 is a diagram showing a schematic cross section of the formed void layer 14P perpendicular to the central axis CX. When the holes 14H are filled with the group III nitride, the shape of the holes 14H is deformed by mass transport into a shape formed by thermally stable surfaces, and voids 14K are formed.
[0095] That is, in the +c-plane substrate, the inner side surface of the hole 14H changes shape to the (1-100) plane (i.e., m-plane), that is, changes shape from an oval cylindrical shape to an oval hexagonal prism-shaped hole 14K whose side surface is formed by the m-plane.
[0096] The formed primary voids 14K1 had a long hexagonal prism shape with a major axis of 72.5 nm and a minor axis of 43.5 nm, and a major axis / minor axis ratio of 1.67. The secondary voids 14K2 had a long hexagonal prism shape with a major axis of 44.6 nm and a minor axis of 38.3 nm, and a major axis / minor axis ratio of 1.16, and were closer to a regular hexagonal prism than the primary voids 14K1.
[0097] Furthermore, it was confirmed that the distances Δx and Δy between the centers of gravity of the main void 14K1 and the subvoid 14K2 were 81.6 nm (Δx=Δy=0.46PK), which had not changed since before filling. It was also confirmed that the major axes of the main void 14K1 and the subvoid 14K2 were parallel to the <11-20> axis (i.e., the a-axis).
[0098] Furthermore, the void filling factors FF1 and FF2 of the main voids 14K1 and the sub-voids 14K2 were calculated to be 8.8% and 4.2%, respectively. Here, the void filling factor is the ratio of the area occupied by each void per unit area in a two-dimensional regular array. Specifically, when the areas of the main voids 14K1 and the sub-voids 14K2 in the void layer 14P are S1 and S2, respectively, the void filling factors FF1 and FF2 of the main voids 14K1 and the sub-voids 14K2 are given by the following equations:
[0099] FF1 = S1 / PK 2 , FF2=S2 / PK 2 Through the above steps, the formation of the n-side guide layer 14 including the vacancy layer 14P is completed.
[0100] 3. Effects of Surface Oxidation / Oxide Film Removal (a) Reduction of Interface Si Concentration Figure 7 shows the results of SIMS (Secondary Ion Mass Spectroscopy) measurements (SIMS profile) in the depth direction of a PCSEL device 10 (EMB) fabricated by performing the surface oxidation / oxide film removal process (step S1) on a substrate with holes 14H formed therein. For clarity, each semiconductor layer is indicated by its reference numeral. For example, "14B1" indicates the first buried layer 14B1, "14B2" indicates the second buried layer 14B2, and "23" indicates the light distribution-adjusting layer 23.
[0101] FIG. 8 shows the SIMS profile in the depth direction of a PCSEL device (CMP) manufactured without performing the surface oxidation / oxide film removal process (step S1).
[0102] In the PCSEL element (CMP) in which surface oxidation / oxide film removal was not performed, the interface between the first buried layer 14B1 and the second buried layer 14B2 and the interface between the second buried layer 14B2 and the light distribution adjustment layer 23 had a SiO 2 concentration of 1×10 20 cm -3 A high concentration of Si was present.
[0103] On the other hand, as shown in FIG. 7, the Si concentration at the interface was reduced to 2×10 by oxidizing the surface Si through ozone treatment and removing the oxide film through BHF treatment. 19 cm -3 The reduction can be reduced to about 1 / 4 or less.
[0104] (b) Flatness of Regrowth Layer A large amount of Si was deposited on the semiconductor surface where the hole 14H was formed due to the adhesion of the SiNx film as a hard mask and siloxane in the atmosphere. During crystal growth, a highly reactive nitrogen atmosphere (e.g., NH 3In an atmosphere where Si is dissociated at high temperatures, the surface Si reacts with N to form SiN. The SiN forms an inversion domain on the GaN surface, which locally inverts the polarity of the GaN formed in the region contaminated with SiN on the top surface of the first buried layer due to facet growth. This inversion domain is formed during shape changes due to mass transport during the formation of the second buried layer 14B2, resulting in significant surface roughness. Furthermore, when Si is doped at a level that forms an inversion domain, point defects are likely to be introduced even if the buried layer can be grown while maintaining surface flatness.
[0105] That is, in the conventional technology, it is not possible to obtain a highly flat growth surface, and it is not possible to reduce the oscillation threshold current of the surface-emitting laser element. Furthermore, since the hole layer 14P and the active layer 15 cannot be brought sufficiently close to each other, it is difficult to obtain a surface-emitting laser element with high coupling efficiency between the hole layer 14P and the active layer 15 and good characteristics. Furthermore, a large number of point defects are introduced into the film, which deteriorates the crystallinity, making it difficult to obtain a surface-emitting laser element with good characteristics.
[0106] As described above, by performing the surface oxidation and oxide film removal treatment, the Si concentration at the interface can be significantly reduced, the formation of inversion domains can be suppressed, and a high-quality active layer with high flatness can be grown.
[0107] Therefore, it is possible to provide a surface-emitting semiconductor laser device with a low threshold and high efficiency.
[0108] [Second Embodiment] Fig. 9A is a cross-sectional view schematically illustrating an example of the structure of a photonic crystal surface-emitting laser device (PCSEL device) 30 according to a second embodiment. Fig. 9B is an enlarged cross-sectional view schematically illustrating an air hole layer 14P and air holes 14K arranged in the air hole layer 14P in Fig. 9A.
[0109] 10 is a flowchart showing a method for manufacturing the PCSEL device 30 of the second embodiment. Note that the same steps as those in the method for manufacturing the PCSEL device 10 of the first embodiment are denoted by the same reference numerals.
[0110] FIG. 11 is a cross-sectional view schematically showing a cross section of the n-side guide layer 14 in step S3A of the manufacturing method.
[0111] (a) Manufacturing Method and Structure of PCSEL Device As shown in FIG. 10, in the PCSEL device 30, after performing a surface oxidation and oxide film removal process (step S1), the buried layer 14B is grown (steps S2 and S3). 2 The buried layer 14B was etched by annealing (step S3A).
[0112] 11, the semiconductor layer on the void layer 14P was etched by TE from the surface of the buried layer 14B (thickness D). The thickness of the remaining buried layer 14B is DE (= D - TE). That is, the thickness from the top surface of the void 14K to the surface (upper surface) of the remaining buried layer 14B is DE.
[0113] In other words, the buried layer 14BE (thinned buried layer, hereinafter also referred to as thinned buried layer) having the thickness DE is formed by the etching in step S3A.
[0114] That is, the PCSEL device 30 differs from the PCSEL device 10 of the first embodiment in that it has a thinned buried layer 14BE formed by etching, but is otherwise the same as the PCSEL device 10 of the first embodiment.
[0115] (b) Thinning of the buried layer - H 2 Annealing and etching: The buried layer 14B is etched from the surface of the buried layer 14B by H 2 The surface morphology of the buried layer 14B (thinned buried layer 14BE) after etching by annealing was evaluated.
[0116] Specifically, samples (i) to (iv) were fabricated in which the thickness DE of the thinned buried layer 14BE (that is, the buried layer 14B after etching) was changed by changing the etching time.
[0117] As described above, the Si concentration at the interface is reduced to 2×10 19 cm -3 has been reduced to a certain extent.
[0118] FIG. 12 shows a state in which the surface of the semiconductor layer on which the buried layer 14B is regrown after the surface oxidation / oxide film removal process (step S1) is performed. 2 10 is an SEM image showing a cross section after etching by annealing.
[0119] As shown in FIG. 12, the thickness DE of the thinned buried layer 14BE was (i) DE=114 nm, (ii) DE=66 nm, (iii) DE=4 nm, and (iv) DE<1 nm.
[0120] Hydrogen (H 2 In annealing in a (0001) atmosphere, the (0001) plane is a thermally stable plane, and the buried layer 14B can be etched and thinned while maintaining the flatness of the surface. Therefore, a high-quality active layer with high flatness can be grown on the buried layer 14B. The annealing atmosphere may contain Group III and Group V materials.
[0121] More specifically, in the case of a group III nitride semiconductor, H 2 High-temperature annealing in a high-temperature atmosphere causes surface atoms to be desorbed, resulting in etching of the surface. Since the surface with the slowest etching rate remains, the most thermally stable (0001) plane is formed on the surface. Therefore, when a +c-plane substrate is used, etching can be performed while maintaining the (0001) plane parallel to the substrate. This allows the buried layer 14B to be made thinner, thereby reducing the gap (distance) between the vacancy layer 14P (vacancy layer) and the active layer 15.
[0122] The surface morphologies of samples (i) to (iv) were observed using an AFM (atomic force microscope). Figure 13 shows AFM images of the surfaces of samples (i) to (iv).
[0123] When the thickness DE of the thinned buried layer 14BE was (i) DE = 114 nm, (ii) DE = 66 nm, (iii) DE = 4 nm, or (iv) DE < 1 nm, the surface roughness was Ra = 0.633 nm, 0.508 nm, 0.532 nm, and 2.43 nm, respectively, in an area of 20 μm × 20 μm.
[0124] It was found that a sufficiently flat surface could be obtained in the cases of (i) to (iii). It was also found that good flatness could be obtained even when the thickness was extremely thin, at DE = 4 nm (iii). In the case of (iv) DE < 1 nm, significant surface roughness was observed.
[0125] FIG. 14 is a graph plotting the surface roughness Ra in a 20 μm×20 μm area against the thickness DE of the thinned buried layer 14BE.
[0126] 14, it can be seen that a sufficiently flat surface can be obtained if DE≧4 nm. More specifically, it can be seen that if the thickness DE of the thin-film buried layer 14BE is 4 nm or more, the surface roughness Ra in a 20 μm×20 μm area can be Ra≦0.7 nm.
[0127] (c) Distance Between the Air Hole Layer and the Active Layer From the above results, it can be seen that if the distance between the air hole layer 14P and the active layer 15, i.e., the distance between the upper surface of the air holes 14K in the air hole layer 14P and the active layer 15, is 4 nm or more, a sufficiently flat active layer 15 can be obtained, and a surface-emitting laser element with good characteristics and high coupling efficiency between the air hole layer 14P and the active layer 15 can be obtained.
[0128] In order to obtain high coupling efficiency, the distance between the hole layer 14P and the active layer 15 is preferably 200 nm or less.
[0129] Furthermore, by setting the distance between the air hole layer 14P and the active layer 15 to 4 to 150 nm, a surface-emitting semiconductor laser device with a higher resonance effect, a low threshold value, and high efficiency can be obtained.
[0130] In addition, when the active layer 15 is an active layer with a quantum well structure, the distance between the upper surface of the air hole 14K and the active layer 15 refers to the distance between the upper surface of the air hole 14K and the first quantum well layer (i.e., the quantum well layer closest to the air hole layer 14P).
[0131] Furthermore, in the past, in order to obtain a high hole filling rate in a hole layer with a multi-lattice structure, a thicker burying layer was sometimes required than in a hole layer with a single lattice structure. However, according to the present invention, even in such a case, a thin burying layer can be used, and a high coupling efficiency (resonance effect) between the hole layer and the active layer can be obtained.
[0132] According to this embodiment, the void layer 14P and the highly flat active layer 15 can be provided in close proximity to each other. Specifically, as described above, if the thickness of the buried layer 14BE is 4 nm or more, the surface roughness Ra of the buried layer 14BE is Ra≦0.7 nm.
[0133] As shown in the SIMS measurement results of FIGS. 7 and 8, in the portion where the Si concentration in the first buried layer 14B1 is flat, the Si concentration is about 4.5×10 after the oxide film removal (step S1) of the hole formation layer 14J (FIG. 7). 18 cm -3 When the oxide film was not removed (FIG. 8), the 18 cm -3 It can be seen that it is reduced compared to
[0134] Therefore, it can be understood that by oxidizing the surface of the hole formation layer 14J and removing the oxide film, the Si concentration in the buried layer 14B is reduced, and a semiconductor layer with high flatness can be regrown.
[0135] The first and second embodiments have been described in detail above. In the first and second embodiments, the case where the light distribution adjustment layer 23 is provided has been described. However, the active layer 15 may be formed directly on the buried layer 14B or the buried layer 14BE without providing the light distribution adjustment layer 23. In this case, the hole layer 14P and the active layer 15 having high flatness may be provided in close proximity to each other.
[0136] As described above in detail, according to the present invention, it is possible to provide a method for manufacturing a surface-emitting semiconductor laser device and a photonic crystal surface-emitting laser device that can increase the resonance effect by bringing the air hole layer and the active layer close to each other and have a high-quality active layer, low threshold, and high efficiency.
[0137] The numerical values and the like in the above-described embodiments are merely examples unless otherwise specified, and can be modified as appropriate. Furthermore, although a PCSEL element having a double grating structure has been exemplified, the present invention can also be applied to a PCSEL element having a single grating structure and, in general, to a PCSEL element having a multi-grating structure.
[0138] Furthermore, although the present invention has been exemplified with respect to a photonic crystal layer in which the holes have a hexagonal columnar shape, the present invention can also be applied to photonic crystal layers in which the holes have an irregular columnar shape such as a cylindrical, rectangular, polygonal, or teardrop shape.
[0139] 10: PCSEL element 12: Element substrate 13: First cladding layer 14: First guide layer 14A: Lower guide layer 14B: Buried layer 14BE: Buried layer 14B1: First buried layer 14B2: Second buried layer 14B2: Second buried layer 14E: Hole formation preparation layer 14J: Hole formation layer 14K: Hole / hole pair 14K1 / 14K2: Main / sub-hole 14P: Photonic crystal layer (hole layer) 15: Active layer 16: Second guide layer 17: Electron barrier layer 18: Second cladding layer 19: Contact layer 23: Light distribution adjustment layer
Claims
1. A method for manufacturing a surface-emitting semiconductor laser element, comprising the steps of: (a) forming a hole-formation preparation layer on a substrate; (b) forming holes in the hole-formation preparation layer, which are two-dimensionally arranged at each of lattice points, to form a hole-formation layer; (c) oxidizing the surface of the hole-formation layer to form an oxide film, and then removing the oxide film; (d) forming a first burying layer by facet growth that closes the holes; (e) growing a second burying layer that flatly buries the first burying layer, to form a first guide layer including a vacancy layer having vacancies corresponding to the holes; and (f) performing crystal growth of a semiconductor layer including an active layer on the first guiding layer.
2. A method for manufacturing a surface-emitting semiconductor laser element, comprising the steps of: (a) forming a hole-formation preparation layer on a substrate; (b) forming holes in the hole-formation preparation layer, which are two-dimensionally arranged at each of lattice points, to form a hole-formation layer; (c) oxidizing the surface of the hole-formation layer to form an oxide film, and then removing the oxide film; (d) forming a first burying layer by facet growth that closes the holes; (e) growing a second burying layer that flatly buries the first burying layer, to form a first guide layer including a vacancy layer having vacancies corresponding to the holes; (f) annealing in a hydrogen atmosphere to flatten the surface of the first guiding layer, and (g) performing crystal growth of a semiconductor layer including an active layer on the flat-etched first guiding layer.
3. The method according to claim 1 or 2, wherein the step of forming the oxide film is a step of oxidizing the surface of the hole formation layer with ozone.
4. The surface emitting semiconductor laser element is a GaN-based semiconductor laser element, and the Si concentration at the interface between the first guide layer and the semiconductor layer including the active layer is 2×10 19 cm -3 The method according to claim 1 or 2, wherein:
5. The manufacturing method according to claim 1 or 2, wherein the surface emitting semiconductor laser element is a GaN-based semiconductor laser element, the crystal growth surface of the substrate is a {0001} surface, and the facet surface of the facet growth is a {1-101} surface.
6. The method according to claim 1 or 2, wherein the distance from the upper surface of the hole in the hole layer to the active layer is 200 nm or less.
7. The method according to claim 2, wherein the thickness of the second buried layer on the upper surface of the hole forming layer after the flattening etching is 4 nm or more.
8. A surface emitting semiconductor laser element comprising: an n-type semiconductor layer; a first guide layer having a hole layer formed on the n-type semiconductor layer, the hole layer having holes arranged two-dimensionally at each of lattice points, and a buried layer formed on the hole layer and closing the holes; a semiconductor layer formed on the buried layer and including an active layer; and a second guide layer formed on the semiconductor layer including the active layer, wherein the distance from an upper surface of the hole in the hole layer to the active layer is 4 to 200 nm.
9. The surface emitting semiconductor laser device according to claim 8, wherein the surface roughness Ra of said buried layer is Ra≦0.7 nm.
10. The surface emitting semiconductor laser element according to claim 8, wherein the active layer has a quantum well structure, and the distance to the active layer is the distance between a quantum well closest to the hole layer and an upper surface of the hole.
11. The surface-emitting semiconductor laser element according to claim 8, wherein the semiconductor layer including the active layer is provided between the buried layer and the active layer, and includes a heterogeneous semiconductor layer having a crystal composition different from that of the buried layer.
Citation Information
Patent Citations
2.5-dimensional photon crystal-face transmitting laser
CN1897375A
Group-iii nitride surface light-emitting element and its manufacturing method
JP2009130110A
Photonic crystalline surface light-emitting laser, and method of manufacturing the same
JP2010114384A
Surface emitting laser element and method of manufacturing surface emitting laser element
JP2021097115A
Photonic crystal surface emission laser element
JP2022018026A