Plated steel sheet and method for manufacturing same
The development of a plated steel sheet with a specific composition and manufacturing process addresses the issue of inconsistent tensile strength in plated steel sheets, achieving high strength, yield ratio, and workability, ensuring improved collision safety and manufacturing efficiency.
Patent Information
- Application Number
- PCT/JP2024/010715
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-02-19
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-03
AI Technical Summary
Plated steel sheets used in automobile bodies face challenges in maintaining consistent tensile strength across the sheet width direction, which can compromise collision safety and workability due to variations in mechanical properties.
A plated steel sheet composition with specific elements (C, Si, Mn, Al, Ti, P, S, N, and a metal structure of ferrite, upper bainite, tempered martensite, and retained austenite, along with a manufacturing process involving controlled heating, cooling, and oxidation treatments, is developed to achieve uniform tensile strength and high workability.
The solution results in a plated steel sheet with high tensile strength, a predetermined yield ratio, and enhanced workability, while minimizing variations in tensile strength across the sheet width direction, thereby improving collision safety and manufacturing efficiency.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Coated steel sheet and its manufacturing method
[0001] The present disclosure relates to plated steel sheets and methods for producing the same.
[0002] There has been a demand for improved occupant safety in vehicles, and for this purpose, the strength of vehicle body materials has been improved. On the other hand, against the backdrop of worsening issues such as global warming, there has been an accelerating movement to improve automobile fuel efficiency. It is known that reducing the weight of vehicle bodies is an effective way to improve fuel efficiency.
[0003] Plated steel sheets used in automobile bodies are required to have greater strength in order to ensure safety in the event of a collision while reducing the weight of the vehicle body. For example, tensile strength and yield ratio are mechanical properties that have a significant impact on safety in the event of a collision.
[0004] On the other hand, excellent formability is also required for plated steel sheets to be used in components such as automobile bodies with complex shapes. Mechanical properties that greatly contribute to formability include, for example, ductility and hole expandability.
[0005] As a technique for achieving both collision safety (high strength, predetermined yield ratio) and high formability, mainly the use of retained austenite (utilizing the TRIP (Transformation Induced Plasticity) phenomenon) as well as soft ferrite (and upper bainite) have been proposed. Patent Document 1 discloses a plated steel sheet that has a tensile strength of 980 MPa or more and good formability by including ferrite and controlling the structural ratio of MA and retained austenite.
[0006] JP 2016-194139 A
[0007] If the tensile strength of a plated steel sheet varies in the sheet width direction, portions with lower strength may deform preferentially, which may reduce collision safety when the plated steel sheet is applied to, for example, an automobile body. However, in the prior art, the variation in tensile strength in the sheet width direction has not been taken into consideration, and there is room for further improvement.
[0008] The present disclosure has been made in view of the above circumstances, and one of its objectives is to provide a plated steel sheet that has high strength, can contribute to weight reduction of a vehicle body, has a predetermined yield ratio and high formability, and has reduced variation in tensile strength in the sheet width direction, and a method for manufacturing the same.
[0009] A first aspect of the present invention is a plated steel sheet comprising a steel sheet and a plating layer disposed on a surface of the steel sheet, and satisfying the following formulas (1) and (2), wherein the steel sheet contained in the plated steel sheet has a component composition consisting of: C: 0.150 to 0.300 mass%, Si: 0.80 to 2.20 mass%, Mn: 1.60 to 2.80 mass%, Al: 0.300 to 0.800 mass%, Ti: 0.010 to 0.050 mass%, P: 0.050 mass% or less (including 0 mass%), S: 0.0100 mass% or less (including 0 mass%), N: 0.0100 mass% or less (including 0 mass%), and the balance: iron and inevitable impurities; and The plated steel sheet has a metallographic structure in which the total of ferrite and upper bainite is 30 to 70 area %, tempered martensite is 10 to 45 area %, MA is 5 to 35 area %, and retained austenite is 5 to 20 volume %. max -TS min <20MPa...(1) TS min ≧980 MPa (2) In the formulas (1) and (2), TS max is the maximum value of the tensile strength at five different points in the sheet width direction of the plated steel sheet, and TS min is the minimum value of the tensile strength at the five locations, and the five locations are, in the sheet width direction, two locations at positions W / 10 to W / 8 from both ends toward the center, two locations at positions W / 4 from both ends toward the center, and one location in the center, where W is the sheet width.
[0010] A second aspect of the present invention is the plated steel sheet according to the first aspect, further comprising at least one selected from the group consisting of Nb: more than 0 mass % and not more than 0.20 mass % and V: more than 0 mass % and not more than 0.50 mass %.
[0011] A third aspect of the present invention is the plated steel sheet according to the first or second aspect, further comprising at least one element selected from the group consisting of Ni: more than 0 mass % and not more than 2.0 mass %, Cr: more than 0 mass % and not more than 2.0 mass %, and Mo: more than 0 mass % and not more than 0.50 mass %.
[0012] A fourth aspect of the present invention is the plated steel sheet according to any one of the first to third aspects, further comprising: B: more than 0 mass % and not more than 0.0050 mass %.
[0013] A fifth aspect of the present invention is the plated steel sheet according to any one of the first to fourth aspects, further comprising at least one selected from the group consisting of Mg: more than 0% by mass and not more than 0.040% by mass, REM: more than 0% by mass and not more than 0.040% by mass, and Ca: more than 0% by mass and not more than 0.040% by mass.
[0014] A sixth aspect of the present invention is the plated steel sheet according to any one of the first to fifth aspects, wherein, in the sheet thickness direction, a position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is in a region that is 0.2% or more of the sheet thickness from the surface of the steel sheet.
[0015] A seventh aspect of the present invention is the plated steel sheet according to any one of the first to sixth aspects, wherein a maximum carbon concentration (mass%) in a region extending from the surface of the steel sheet to 20 μm in the sheet thickness direction is less than 70% of the bulk carbon concentration.
[0016] Aspect 8 of the present invention is a process for obtaining a rolled sheet by hot rolling a steel having the chemical composition according to any one of Aspects 1 to 5; a first heating process for heating the rolled sheet to a first heating temperature of 850°C or more and 910°C or less; a process for holding the rolled sheet at the first heating temperature after the first heating process for 5 to 1800 seconds; a first cooling process for cooling the rolled sheet to a first cooling stop temperature of 350°C to 750°C after the holding process; and a retention process for holding the rolled sheet after the first cooling process from the first cooling stop temperature to a second cooling start temperature of 350°C to the first cooling stop temperature at an average cooling rate of 10°C / second or less which is slower than that of the first cooling process, for a time in the temperature range from the first cooling stop temperature to the second cooling start temperature of 20 to 300 seconds. The method for producing a plated steel sheet according to any one of Aspects 1 to 7 includes, after the residence step, a second cooling step of cooling from the second cooling start temperature to a second cooling stop temperature of 100 to 300°C at an average cooling rate that is faster than that of the residence step; a second heating step of heating to a second heating temperature of 300 to 500°C after the second cooling step; a step of holding the steel sheet at the second heating temperature for 300 to 1800 seconds after the second heating step to obtain a steel sheet; and a step of forming a plating layer on the steel sheet.
[0017] A ninth aspect of the present invention is the production method according to Aspect 8, further comprising, after the step of obtaining the rolled plate, performing an oxidation treatment under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C, and the holding step includes reduction treatments including a first reduction treatment having a dew point of -35 to -15°C, followed by a second reduction treatment having a dew point of -25 to 0°C, which is higher than the dew point of the first reduction treatment.
[0018] According to an embodiment of the present invention, it is possible to provide a plated steel sheet that has high strength, can contribute to weight reduction of a vehicle body, has a predetermined yield ratio and high formability, and has reduced variation in tensile strength in the sheet width direction, and a manufacturing method thereof.
[0019] FIG. 1 is a diagram showing an example of a carbon concentration profile obtained in an example.
[0020] The present inventors have conducted investigations from various angles in order to realize a plated steel sheet that has high strength (tensile strength TS of 980 MPa or more), can contribute to weight reduction of a vehicle body, has a predetermined yield ratio YR (0.55 to 0.75), and high formability (elongation EL of 19% or more, hole expansion ratio λ of 20% or more), and in which variation in tensile strength in the sheet width direction is suppressed.
[0021] Usually, in order to sufficiently introduce soft ferrite and the like, it is effective to perform annealing after the hot rolling step (hereinafter also referred to as "first heating") at a relatively low temperature.
[0022] The present inventors have found that when soft ferrite and the like are introduced by conventional methods as described above, the metallographic structure and the like in the steel sheet become non-uniform, which can result in variations in tensile strength in the sheet width direction. Therefore, the present inventors have found that by adjusting the composition to a predetermined level (particularly by adding a predetermined amount of Al, which can contribute to the formation of ferrite and upper bainite), annealing the steel sheet after rolling at a high temperature of 850°C or higher to eliminate post-rolling distortion and the like, and then allowing the steel sheet to dwell (or be held) at a predetermined temperature range during subsequent cooling, it is possible to achieve a predetermined metallographic structure containing a sufficient amount of ferrite and the like, thereby obtaining a plated steel sheet having high strength (high tensile strength), a predetermined yield ratio, and high formability, and in which variations in tensile strength in the sheet width direction are suppressed. Details of each requirement specified in the embodiments of the present invention are described below.
[0023] <1. Plated Steel Sheet> A plated steel sheet according to an embodiment of the present invention includes a steel sheet and a plating layer disposed on the surface of the steel sheet. The plating layer may be a zinc-based plating layer such as a hot-dip galvanized layer, a galvannealed hot-dip galvanized layer, or an electrogalvanized layer, or an aluminum plating layer such as a hot-dip aluminum plating layer. The zinc-based plating layer may be a zinc-based alloy plating layer such as zinc-Ni, zinc-Fe, or zinc-Al. The plating layer may be formed on at least one surface (e.g., the rolled surface) of the steel sheet, or may be formed on both opposing surfaces, or may be formed on the entire surface of the steel sheet. Specific examples of plated steel sheets including the zinc-based plating layer include hot-dip galvanized steel sheets (GI), galvannealed hot-dip galvanized steel sheets (GA), and electrogalvanized steel sheets (EG).
[0024] 2. Chemical Composition of Steel Sheet Included in Plated Steel Sheet> The steel sheet included in the plated steel sheet according to an embodiment of the present invention (which may be, for example, the portion of the plated steel sheet excluding the plating layer) preferably contains 0.150 to 0.300 mass% C, 0.80 to 2.20 mass% Si, 1.60 to 2.80 mass% Mn, 0.300 to 0.800 mass% Al, 0.010 to 0.050 mass% Ti, 0.050 mass% or less (including 0 mass%) of P, 0.0100 mass% or less (including 0 mass%) of S, and 0.0100 mass% or less (including 0 mass%) of N, with the balance being iron and inevitable impurities. Each component will be described in detail below.
[0025] (C: 0.150 to 0.300 mass%) C is an element effective for obtaining a desired structure such as retained austenite (hereinafter also referred to as "residual γ") and improving properties such as tensile strength TS and elongation EL. To achieve this effect, the C content is 0.150 mass% or more, preferably 0.170 mass% or more, more preferably 0.180 mass% or more, and even more preferably 0.200 mass% or more. On the other hand, if the C content is excessive, MA (martensite-austenite constituent) and residual γ become coarse, the hole expandability λ decreases, and weldability is also adversely affected. Therefore, the C content is 0.300 mass% or less, preferably 0.280 mass% or less, more preferably 0.260 mass% or less, and even more preferably 0.250 mass% or less.
[0026] (Si: 0.80 to 2.20 mass%) Si suppresses the precipitation of cementite and promotes the formation of residual γ. To achieve this effect, the Si content is 0.80 mass% or more, preferably 0.90 mass% or more, more preferably 1.00 mass% or more, and even more preferably 1.20 mass% or more. On the other hand, if the Si content is excessive, MA and residual γ become coarse, reducing the hole expansion ratio λ and also reducing weldability. Therefore, the Si content is 2.20 mass% or less, preferably 2.10 mass% or less, and more preferably 2.00 mass% or less.
[0027] (Mn: 1.60 to 2.80% by mass) Mn is an element that contributes to improving the strength of steel sheets through solid solution strengthening and is necessary for ensuring high strength. To achieve this effect, the Mn content is set to 1.60% by mass or more, preferably 1.80% by mass or more, and more preferably 2.00% by mass or more. On the other hand, if the Mn content is excessive, the formation of ferrite and upper bainite is suppressed during the manufacturing process, making it impossible to sufficiently introduce a soft structure that contributes to improving ductility, and as a result, high elongation (EL) cannot be achieved. Therefore, the Mn content is set to 2.80% by mass or less, preferably 2.70% by mass or less, more preferably 2.60% by mass or less, and even more preferably 2.50% by mass or less.
[0028] (Al: 0.300 to 0.800 mass%) Al has the effect of promoting the formation of ferrite and upper bainite, and is an important element for ensuring the desired area ratios of ferrite and upper bainite during short-term retention in a predetermined temperature range described below. To achieve this effect, the Al content is set to 0.300 mass% or more, preferably 0.350 mass% or more, and more preferably 0.400 mass% or more. On the other hand, if the Al content is excessive, it may become difficult to eliminate heterogeneity in the structure resulting from the manufacturing process, which may result in variations in strength within the steel sheet. For this reason, the Al content is set to 0.800 mass% or less, preferably 0.750 mass% or less, and more preferably 0.700 mass% or less.
[0029] (Ti: 0.010 to 0.050 mass%) Ti is an element that exhibits the effects of precipitation strengthening and refining the metal structure, and contributes to increasing the strength of the steel sheet. To exhibit this effect, the Ti content is set to 0.010 mass% or more, preferably 0.015 mass% or more, and more preferably 0.020 mass% or more. On the other hand, if the Ti content is excessive, Ti carbonitrides will precipitate in excess, reducing the workability of the steel sheet. Therefore, the Ti content is set to 0.050 mass% or less, preferably 0.045 mass% or less, and more preferably 0.040 mass% or less.
[0030] (P: 0.050% by mass or less (including 0% by mass)) P is an element that is inevitably present as an impurity element. If the P content is excessive, the elongation EL and the hole expansion ratio λ decrease. Therefore, the P content is set to 0.050% by mass or less, and preferably 0.030% by mass or less. In this specification, "including 0% by mass" means that it includes embodiments in which it is not intentionally added, that is, cases in which the content is below the unavoidable impurity level (it does not exclude cases in which it is intentionally added).
[0031] (S: 0.0100% by mass or less (including 0% by mass)) S is an element that is inevitably present as an impurity element. If the S content is excessive, sulfide-based inclusions such as MnS are formed, which become the starting points for cracks and reduce the hole expansion ratio λ. Therefore, the S content is set to 0.0100% by mass or less, and preferably 0.0050% by mass or less.
[0032] (N: 0.0100% by mass or less (including 0% by mass)) N is an element that is inevitably present as an impurity element. If the N content is excessive, coarse nitrides are formed, which causes deterioration of bendability and hole expandability and the occurrence of blowholes during welding. For this reason, the N content is set to 0.0100% by mass or less. Note that reducing the N content is costly, and attempting to reduce it to less than 0.0005% by mass results in a significant increase in costs. For this reason, it is preferable that the lower limit of the N content is set to 0.0005% by mass or more.
[0033] The steel sheet included in the plated steel sheet according to the embodiment of the present invention preferably has the above-described chemical composition, with the balance being iron and inevitable impurities in one embodiment of the present invention. Elements introduced due to the conditions of raw materials, materials, manufacturing facilities, etc. are permitted as inevitable impurities. Note that, for example, P, S, and N, which are typically present in smaller amounts, are considered inevitable impurities, but their composition ranges are separately specified as described above. Therefore, in this specification, the term "unavoidable impurities" constituting the balance refers to elements excluding those whose composition ranges are separately specified.
[0034] In a preferred embodiment of the present invention, in addition to the above elements, it is also effective to further contain, as necessary, (a) at least one selected from the group consisting of Nb: more than 0% by mass and 0.20% by mass or less and V: more than 0% by mass and 0.50% by mass or less; (b) at least one selected from the group consisting of Ni: more than 0% by mass and 2.0% by mass or less, Cr: more than 0% by mass and 2.0% by mass or less, and Mo: more than 0.50% by mass or less; (c) B: more than 0% by mass and 0.0050% by mass; and (d) at least one selected from the group consisting of Mg: more than 0% by mass and 0.040% by mass or less, REM: more than 0.040% by mass or less, and Ca: more than 0% by mass and 0.040% by mass or less. The properties of the plated steel sheet are further improved depending on the type of element contained.
[0035] (a) At least one selected from the group consisting of Nb: more than 0 mass% and 0.20 mass% or less and V: more than 0 mass% and 0.50 mass% or less) Nb is an element that exerts the effects of precipitation strengthening and refining the metal structure, and contributes to improving the strength of the steel sheet. Therefore, the Nb content is preferably more than 0 mass%. This effect increases as the Nb content increases, and the Nb content is more preferably 0.005 mass% or more, and even more preferably 0.010 mass% or more. On the other hand, if the Nb content is excessive, Nb carbonitrides may be excessively precipitated, which may reduce the workability of the steel sheet. Therefore, the Nb content is preferably 0.20 mass% or less, more preferably 0.10 mass% or less, and even more preferably 0.060 mass% or less. Like Nb, V is an element that exerts the effects of precipitation strengthening and refining the metal structure, and contributes to improving the strength of the steel sheet. Therefore, the V content is preferably more than 0 mass%. This effect increases as the V content increases, and the V content is more preferably 0.010 mass% or more, and even more preferably 0.020 mass% or more. On the other hand, if the V content is excessive, excessive precipitation of V carbonitrides may occur, which may reduce the workability of the steel sheet. Therefore, the V content is preferably 0.50 mass% or less, more preferably 0.40 mass% or less, even more preferably 0.30 mass% or less, and even more preferably 0.10 mass% or less.
[0036] (b) At least one selected from the group consisting of Ni: more than 0 mass% and 2.0 mass% or less, Cr: more than 0 mass% and 2.0 mass% or less, and Mo: more than 0 mass% and 0.50 mass% or less) Ni contributes to improving the strength of the steel sheet and is an element effective for stabilizing residual γ and ensuring a desired amount of residual γ. Therefore, the Ni content is preferably more than 0 mass%. This effect increases as the Ni content increases, and the Ni content is more preferably 0.001 mass% or more, and even more preferably 0.01 mass% or more. On the other hand, an excessive Ni content may reduce manufacturability during hot rolling. Therefore, the Ni content is preferably 2.0 mass% or less, and more preferably 1.0 mass% or less. Cr, like Ni, contributes to improving the strength of the steel sheet and is an element effective for stabilizing residual γ and ensuring a desired amount of residual γ. Therefore, the Cr content is preferably more than 0 mass%. This effect increases as the Cr content increases, and the Cr content is more preferably 0.001% by mass or more, and even more preferably 0.02% by mass or more. On the other hand, an excessive Cr content reduces manufacturability during hot rolling. Therefore, the Cr content is preferably 2.0% by mass or less, and more preferably 1.0% by mass or less. Like Ni and Cr, Mo contributes to improving the strength of the steel sheet and is an effective element for stabilizing residual γ and ensuring a desired amount of residual γ. Therefore, the Mo content is preferably greater than 0% by mass. This effect increases as the Mo content increases, and the Mo content is more preferably 0.001% by mass or more, and even more preferably 0.01% by mass or more. On the other hand, an excessive Mo content may reduce manufacturability during hot rolling. Therefore, the Mo content is preferably 0.50% by mass or less, and more preferably 0.20% by mass or less. Ni, Cr and Mo may be contained either singly or in combination of two or three of them.
[0037] (c) B: More than 0 mass% and 0.0050 mass% or less) B is an element that is effective in suppressing excessive ferrite transformation by increasing hardenability. Therefore, the B content is preferably more than 0 mass%. This effect increases as the B content increases, and the B content is more preferably 0.0001 mass% or more, even more preferably 0.0003 mass% or more, and even more preferably 0.0005 mass% or more. However, if the B content is excessive, the hardenability increases excessively, which may make it difficult to introduce ferrite and upper bainite during cooling. Therefore, the B content is preferably 0.0050 mass% or less, more preferably 0.0030 mass% or less, and even more preferably 0.0020 mass% or less.
[0038] (d) At least one selected from the group consisting of Mg: more than 0% by mass and 0.040% by mass or less, REM: more than 0% by mass and 0.040% by mass or less, and Ca: more than 0% by mass and 0.040% by mass or less) Mg, REM (rare earth elements), and Ca form fine oxides and / or sulfides and suppress a decrease in hole expandability due to coarse oxides and / or sulfides. Therefore, the contents of Mg, REM, and Ca are preferably each more than 0% by mass. This effect increases as their contents increase, but the contents of Mg, REM, and Ca are more preferably 0.0005% by mass or more, and even more preferably 0.0010% by mass or more. However, if the contents of Mg, REM, and Ca are excessive, the oxides and / or sulfides may become coarse, resulting in a decrease in hole expandability. Therefore, the contents of Mg, REM, and Ca are each preferably 0.040% by mass or less, and more preferably 0.010% by mass or less. Note that REM includes 17 elements in total, including Sc, Y, and the lanthanoid series rare earth elements from La (atomic number 15) to Lu (atomic number 71), and the REM content means the total amount of these 17 elements.
[0039] 3. Metallographic Structure of Steel Sheet Included in Plated Steel Sheet> The metallographic structure of the steel sheet included in the plated steel sheet according to the embodiment of the present invention has a total of 30 to 70 area % of ferrite and upper bainite, 10 to 45 area % of tempered martensite, 5 to 35 area % of MA, and 5 to 20 volume % of retained austenite. Each structure will be described below.
[0040] (The total area percentage of ferrite and upper bainite is 30 to 70%.) Ferrite and upper bainite are important structures for improving workability (especially elongation (EL)). Therefore, the total area percentage of ferrite and upper bainite is 30% or more, preferably 35% or more, and more preferably 40% or more. On the other hand, since both ferrite and upper bainite have low strength, an excessive total area percentage of ferrite and upper bainite reduces the tensile strength (TS) and yield stress (YS). Therefore, the total area percentage of ferrite and upper bainite is 70% or less, preferably 65% or less, and more preferably 60% or less. The area percentages of ferrite and upper bainite can be determined by observing a nital-etched steel sheet with a scanning electron microscope (SEM) and measuring the black areas not containing carbides using a point counting method or the like.
[0041] (Tempered martensite is 10 to 45 area %) Tempered martensite is an important metal structure for ensuring the desired tensile strength TS and yield ratio YR. For this reason, the tempered martensite content is 10 area % or more, preferably 15 area % or more, more preferably 18 area % or more, and even more preferably 20 area % or more. On the other hand, if the tempered martensite content is excessive, the elongation EL decreases. For this reason, the tempered martensite content is 45 area % or less, preferably 40 area % or less, and more preferably 35 area % or less. The area fraction of tempered martensite can be determined as the region excluding ferrite, upper bainite, MA, and the remaining structure including pearlite and cementite.
[0042] (MA is 5 to 35 area %) MA is a composite structure of fresh martensite and residual γ. Since MA contains residual γ, increasing the amount of MA is effective in improving workability such as elongation (EL). For this reason, the MA content is set to 5 area % or more, preferably 7 area % or more, and more preferably 10 area % or more. However, since very hard fresh martensite is also contained in MA, increasing the MA content increases the interface between fresh martensite and other structures, and the hole expansion ratio λ decreases. Therefore, the MA content is set to 35 area % or less, preferably 30 area % or less, and more preferably 25 area % or less. The area ratio of MA can be determined by observing a nital-etched steel sheet with an SEM and measuring the gray areas that do not contain carbides using the point counting method.
[0043] (Residual austenite is 5 to 20% by volume) Residual γ causes the TRIP (Transformation Induced Plasticity) phenomenon, in which the residual γ transforms into martensite during press working, etc., contributing to improved elongation (EL). Because martensite formed by the TRIP phenomenon has high hardness, residual γ is an effective structure for improving tensile strength (TS) and elongation (EL). To achieve the desired strength and workability, the residual γ content is 5% by volume or more, preferably 6% by volume or more, more preferably 8% by volume or more, and even more preferably 10% by volume or more. On the other hand, because residual γ is a structure with a low yield ratio, the volume fraction of residual γ to ensure the desired yield ratio is 20% by volume or less, preferably 19% by volume or less, more preferably 18% by volume or less, and even more preferably 16% by volume or less. The volume fraction of residual γ can be measured, for example, by X-ray diffraction. In this method, for example, a portion of the steel sheet from the surface to ¼ of the thickness of the steel sheet is removed by mechanical polishing, chemical polishing, etc., and an X-ray diffraction pattern is obtained from the exposed surface using Co-Kα radiation as characteristic X-rays. The volume fraction of retained γ can then be measured from the integrated intensity ratio of the diffraction peaks of the body-centered cubic lattice (bcc) phase to the body-centered tetragonal (bct) and face-centered cubic lattice (fcc).
[0044] The remaining structure of the metal structure includes pearlite, cementite, etc. The remaining structure may be contained in a total amount of 10 area % or less.
[0045] 4. Mechanical Properties of Plated Steel Sheet The plated steel sheet according to this embodiment can exhibit high strength (high tensile strength), a predetermined yield ratio, and high formability (high elongation and high hole expansion ratio). In this specification, a high-strength plated steel sheet is one having a tensile strength TS of 980 MPa or more, specifically, one that satisfies the following formula (2): TS min ≧980 MPa (2) In formula (2), TS minis the minimum value of the tensile strength at five different locations in the width direction of the plated steel sheet, and the five locations are two locations in the width direction, where W is the sheet width, from both ends toward the center at positions W / 10 to W / 8, two locations at positions W / 4 from both ends toward the center, and one location in the center. The predetermined yield ratio YR is 0.55 to 0.75. It is believed that achieving the above tensile strength and yield ratio ensures sufficient collision safety when applied to, for example, automobile bodies. Furthermore, in this specification, a plated steel sheet with high formability is defined as one having an elongation EL of 19% or more and a hole expansion ratio λ of 20% or more. The left side of the above formula (2) is preferably 990 MPa or more, more preferably 1000 MPa or more. The yield ratio is preferably 0.57 to 0.72. The elongation EL is preferably 20% or more, more preferably 21% or more. The hole expansion ratio λ is preferably 23% or more, more preferably 25% or more, and even more preferably 30% or more. Furthermore, the yield stress YS is preferably 550 MPa or more in order to ensure collision safety, more preferably 570 MPa or more, and even more preferably 600 MPa or more.
[0046] Furthermore, the plated steel sheet according to this embodiment has reduced variation in tensile strength in the sheet width direction (i.e., the direction perpendicular to the rolling direction and the sheet thickness direction), and specifically satisfies the following formula (1): TS max -TS min <20 MPa (1) In formula (1), TS max is the maximum value of the tensile strength at five different points in the width direction of the plated steel sheet (i.e., the direction perpendicular to the rolling direction and the thickness direction), and TS min is the minimum value of the tensile strength at the five locations, and the five locations are, in the sheet width direction, two locations at positions W / 10 to W / 8 from both ends toward the center, where W is the sheet width, two locations at positions W / 4 from both ends toward the center, and one location in the center. It is preferable that the left side of the above formula (1) is 18 MPa or less.
[0047] The thickness of the steel sheet included in the plated steel sheet according to this embodiment is not particularly limited. The thickness of the steel sheet included in the plated steel sheet according to this embodiment may be, for example, 0.8 mm or more and 2.3 mm or less. The coating weight of the plated steel sheet according to this embodiment is not particularly limited, and may be, for example, 10 to 100 g / m per side. 2 The width W of the plated steel sheet according to this embodiment (i.e., the length in the direction perpendicular to the rolling direction and the sheet thickness direction) is not particularly limited, but may be, for example, 800 mm or more and 1200 mm or less.
[0048] <5. Decarburized Layer in the Surface of Steel Sheet Contained in Plated Steel Sheet> In the plated steel sheet according to this embodiment, (I) in the sheet thickness direction, the position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is preferably located in a region of 0.2% or more of the sheet thickness from the surface of the steel sheet. This position relates to the thickness of the decarburized layer that contributes to bendability. By ensuring that this position is located in a region of 0.2% or more of the sheet thickness from the surface of the steel sheet and that the decarburized layer that contributes to bendability has a certain thickness or more, it is possible to reliably exhibit excellent bendability in bending. The position where the carbon concentration (mass %) is 50% of the bulk carbon concentration may be located in a region of 0.5% or more, or even 1.0% or more of the sheet thickness from the surface of the steel sheet.
[0049] The steel sheet included in the plated steel sheet according to this embodiment preferably has the following characteristics: (II) the maximum carbon concentration (mass %) in the region from the surface of the steel sheet to 20 μm in the thickness direction is less than 70% of the bulk carbon concentration. The inventors examined steel sheets included in conventional plated steel sheets and first found that a region with a significantly high carbon concentration exists in the surface layer of the steel sheet, and that this is the cause of deterioration in bendability. Then, as described below, they investigated the manufacturing conditions of the steel sheet and found that excellent bendability can be obtained by promoting decarburization in the surface layer of the steel sheet to suppress the carbon concentration in the surface layer of the steel sheet. Specifically, they found that excellent bendability can be obtained by suppressing the maximum carbon concentration (mass %) in the region from the surface of the steel sheet to 20 μm in the thickness direction to less than 70% of the bulk carbon concentration. The maximum carbon concentration is preferably 65% or less of the bulk carbon concentration, and more preferably 60% or less of the bulk carbon concentration.
[0050] From the viewpoint of exhibiting excellent bendability, the plated steel sheet according to the present embodiment preferably satisfies at least one of the above (I) and (II), and more preferably satisfies both of the above (I) and (II).
[0051] The "surface of the steel sheet" refers to the position of the interface between the plating layer and the steel sheet. In the case of a zinc-based plating, for example, the position of the interface between the plating layer and the steel sheet refers to the point at which Zn constituting the plating layer is no longer detected (the Zn analysis value is 0) when Zn is analyzed from the surface of the plating layer in the thickness direction of the plating layer by GD-OES, as measured in the examples described later, and this point is defined as the starting point of the distance (depth) from the steel sheet surface.
[0052] The plated steel sheet according to this embodiment exhibits high strength (high tensile strength), a predetermined yield ratio, and high formability (high elongation and high hole expansion ratio), satisfies the above formula (1), and further, when subjected to a bending test shown in the examples described later, can exhibit excellent bendability with a limit R / t of 2.0 or less.
[0053] 6. Method for manufacturing plated steel sheet A method for manufacturing a plated steel sheet according to an embodiment of the present invention includes: (A) a step of hot rolling a steel having the above-described chemical composition to obtain a rolled sheet; (B) a first heating step of heating the rolled sheet to a first heating temperature of 850°C or more and 910°C or less; (C) a step of holding the rolled sheet at the first heating temperature after the first heating step for 5 to 1800 seconds; (D) a first cooling step of cooling the rolled sheet to a first cooling stop temperature of 350°C to 750°C after the holding step; and (E) a retention step after the first cooling step of retaining the sheet from the first cooling stop temperature to a second cooling start temperature of 350°C to the first cooling stop temperature at an average cooling rate of 10°C / second or less that is slower than that of the first cooling step, and for a time of 20 to 300 seconds in the temperature range from the first cooling stop temperature to the second cooling start temperature. (F) after the holding step, a second cooling step of cooling from the second cooling start temperature to a second cooling stop temperature of 100 to 300°C at an average cooling rate faster than that of the holding step, (G) after the second cooling step, a second heating step of heating to a second heating temperature of 300 to 500°C, (H) after the second heating step, a step of holding at the second heating temperature for 300 to 1800 seconds to obtain a steel sheet, and (I) a step of forming a coating layer on the steel sheet. Each step will be described in detail below.
[0054] (A) Step of Obtaining Rolled Plate Steel having the above-described composition is melted and cast by a conventional method, and the steel (steel slab) is subjected to a conventional hot rolling process to obtain a rolled plate. As an example, a steel (steel slab) having the above-described composition cast by a continuous casting method, an ingot method, a thin slab casting method, or the like may be reheated to about 1150 to 1300°C, hot rolled to a finish rolling temperature of about 850 to 950°C, and then coiled at about 500 to 700°C to obtain a rolled plate.
[0055] If necessary, the rolled plate may be pickled by a conventional method to remove surface scale, and if necessary, the rolled plate may be further subjected to cold rolling by a conventional method.
[0056] (B) First Heating Step: The rolled sheet is heated to a first heating temperature of 850°C or higher and 910°C or lower. If the first heating temperature is lower than 850°C, the reverse transformation to austenite is insufficient, and a processed structure containing strain due to rolling remains, resulting in strength variations in the width direction of the plated steel sheet. Therefore, the first heating temperature is set to 850°C or higher, preferably 860°C or higher, and more preferably 870°C or higher. On the other hand, if the first heating temperature exceeds 910°C, the grain size becomes coarse, which may result in a decrease in the amount of ferrite and upper bainite transformed during the cooling step (which may result in an excessive area fraction of tempered martensite) and a decrease in workability such as the hole expansion ratio. Therefore, the first heating temperature is set to 910°C or lower, preferably 900°C or lower. The heating rate is not particularly limited, and the temperature may be increased at any heating rate. For example, the temperature may be increased from room temperature to the first heating temperature at an average heating rate of 1°C / s or higher and 100°C / s or lower.
[0057] (C) Step of Holding at First Heating Temperature The rolled sheet is held at the first heating temperature for 5 to 1800 seconds. If the holding time is less than 5 seconds, the reverse transformation to austenite is insufficient, the worked structure cannot be fully resolved, and strength variations occur in the width direction of the plated steel sheet. Therefore, the holding time is 5 seconds or more, preferably 10 seconds or more, and more preferably 20 seconds or more. On the other hand, if the holding time exceeds 1800 seconds, not only will productivity decrease, but the crystal grains of the steel sheet structure may become coarse, which may also result in a decrease in workability such as the hole expansion ratio λ. Therefore, the holding time is 1800 seconds or less, preferably 1500 seconds or less, and more preferably 1000 seconds or less.
[0058] After step (A), an oxidation treatment is preferably performed under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C (hereinafter also referred to as "step (B1)"). Step (C) preferably includes a first reduction treatment in which the dew point is -35 to -15°C, followed by a second reduction treatment in which the dew point is -25 to 0°C, which is higher than the dew point of the first reduction treatment (hereinafter also referred to as "step (C1)"). For example, the oxidation treatment in step (B1) may be performed after step (A) and before step (B), or may be performed during the temperature increase to the first heating temperature in step (B) (i.e., step (B) may include the oxidation treatment in step (B1)). The reduction treatment in step (C1) may be performed during the holding at the first heating temperature in step (C).
[0059] By subjecting the surface of a steel sheet to an oxidation treatment in step (B1), an Fe oxide layer can be formed on the surface of the steel sheet. Subsequently, by performing a reduction treatment in step (C1) in a reducing atmosphere, a decarburized layer can be formed on the surface of the steel sheet, while a reduced Fe layer capable of favorably forming, for example, a coating layer can be formed. The inventors have conducted studies and found that by performing the oxidation treatment as described above and specifying the dew point ranges of the first and second reduction treatments in the reduction treatment, and by setting the dew point of the second reduction treatment higher than that of the first reduction treatment, it is possible to easily ensure the decarburized state of the surface layer of the steel sheet described above, which allows for high tensile strength, a predetermined yield ratio, high elongation, high hole expansion ratio, and excellent bendability. Each step of the oxidation treatment and the reduction treatment will be described below.
[0060] (B1) Oxidation Treatment The oxidation treatment is preferably carried out under conditions of an oxygen concentration of 0.1 to 2%. From the viewpoint of obtaining an excellent coating appearance, the oxygen concentration is preferably 0.1% or more, more preferably 0.15% or more, and even more preferably 0.2% or more. On the other hand, if the oxygen concentration is too high, excessive oxidation can easily cause oxide scale to adhere to the rolls in the furnace, resulting in the occurrence of indentation marks on the steel sheet, a defect known as pickup. From the viewpoint of suppressing the occurrence of such defects, the oxygen concentration is preferably 2% or less, more preferably 1.7% or less, and even more preferably 1.5% or less. The concentrations of elements other than oxygen are not particularly limited. For example, CO2 , N 2 , H 2 For example, the oxidation treatment is carried out in a direct fired furnace (DFF) type annealing furnace or the like, in a combustion gas such as coke oven gas (COG) or liquefied petroleum gas (LPG), to remove unburned O and other unavoidable impurities. 2 The oxidation treatment can be carried out in a gas atmosphere with a controlled concentration. The oxidation treatment is preferably carried out under the condition of an ultimate temperature of 650 to 750°C. For example, heating can be carried out in an oxidation heating zone in a DFF type annealing furnace to an ultimate temperature of 650 to 750°C. By achieving an ultimate temperature of 750°C or less, the SiO 2 This can suppress the reaction between the FeO and the steel sheet caused by the oxidation treatment, thereby improving the adhesion between the steel sheet and the plating layer.
[0061] In this specification, the "ultimate temperature" during heating in the oxidation treatment step means the maximum ultimate sheet temperature of the rolled sheet that is heated and controlled in the oxidation heating zone.
[0062] The temperature reached in the oxidation treatment is more preferably 730°C or lower, even more preferably 720°C or lower, and even more preferably 700°C or lower. On the other hand, from the viewpoint of forming an Fe oxide layer in the gas atmosphere, the steel sheet temperature in the oxidation treatment is preferably 650°C or higher. The steel sheet temperature in the oxidation treatment is more preferably 670°C or higher.
[0063] The temperature rise time in the oxidation treatment is not particularly limited, and may be adjusted so as not to form a fayalite layer, which would adversely affect platability, if the oxidation treatment is too long. Specifically, the temperature rise time in the oxidation treatment may be appropriately adjusted taking into consideration the hot rolling conditions (particularly the coiling temperature), the annealing conditions before pickling, the pickling conditions, and the steel sheet temperature during heating in the oxidation treatment. For example, the temperature rise time in the oxidation treatment is preferably 10 seconds or more, more preferably 15 seconds or more. Furthermore, for example, the temperature rise time in the oxidation treatment is preferably 120 seconds or less, more preferably 90 seconds or less. Note that, although the above description has been given of the case where the oxidation treatment is performed while the temperature is being raised, the mode of the oxidation treatment is not limited thereto, and the oxidation treatment may be performed by, for example, raising the temperature to the target temperature and maintaining the target temperature.
[0064] (C1) Reduction Treatment In the reduction treatment, a decarburized layer is formed on the surface layer of the steel sheet, while a reduced Fe layer that can favorably form a plating layer is formed. In the manufacturing method according to this embodiment, the reduction treatment preferably includes a first reduction treatment in which the dew point is −35 to −15° C., followed by a second reduction treatment in which the dew point is −25 to 0° C., which is higher than the dew point in the first reduction treatment. The first reduction treatment and the second reduction treatment will be described below.
[0065] (C1a) First Reduction Treatment In the first reduction treatment, the dew point is preferably set in the range of -35 to -15°C. If the dew point exceeds -15°C, decarburization is likely to proceed more than necessary, which may result in a decrease in strength. In addition, the reduction treatment becomes difficult to proceed, and a defect called pickup is likely to occur, in which iron oxide produced in the oxidation treatment adheres to the rolls and causes pressure scratches on the steel sheet. Therefore, the dew point is preferably set to -15°C or lower. A dew point of -20°C or lower is more preferable. On the other hand, from the viewpoint of suppressing the need for additional equipment and costs, the dew point in the first reduction treatment is preferably set to -35°C or higher. A dew point of -30°C or higher is more preferable.
[0066] The dew point may be within the above range in the atmosphere at the center of the front stage of the reduction zone where the first reduction treatment is performed. The dew point in the first reduction treatment and the second reduction treatment described below can be controlled, for example, by introducing water vapor gas and mixing it with the atmospheric gas in the furnace, or by bubbling the atmospheric gas to mix water vapor therein.
[0067] The atmosphere of the first reduction treatment satisfies the above dew point and contains N 2 , H 2 , CO, H 2 O, O 2 and other unavoidable impurities. In the first reduction treatment, after the steel sheet reaches a temperature of 850°C in the atmosphere, the steel sheet is heated in a temperature range of 850 to 910°C for, for example, 60 to 240 seconds. The "holding" mentioned above includes not only a constant temperature but also a case where the temperature fluctuates within the temperature range.
[0068] (C1b) Second reduction treatment Next, the dew point in the second reduction treatment will be described. In order to achieve excellent bendability with an R / t of less than 2.0, the dew point in the second reduction treatment is preferably −25° C. or higher. On the other hand, the upper limit of the dew point in the second reduction treatment is preferably 0° C. or lower in order to exhibit higher strength. The dew point in the second reduction treatment is more preferably −15° C. or lower.
[0069] The atmosphere of the second reduction treatment satisfies the above dew point and contains N 2 , H 2 , CO, H 2 O, O 2 and other unavoidable impurities. In the second reduction treatment, the steel sheet is heated in the above atmosphere in a temperature range in which the steel sheet reaches a temperature of 850 to 910°C for, for example, 60 to 240 seconds. The "holding" mentioned above includes not only a constant temperature but also a case in which the temperature fluctuates within the above temperature range.
[0070] The first reduction treatment and the second reduction treatment may be performed in separate atmospheres having different dew points as described above, and the specific embodiment is not limited thereto. For example, a reduction furnace for performing each of the first reduction treatment and the second reduction treatment may be provided. In addition, when the steel sheet is a plated steel sheet, a partition wall having an opening area ratio of 20% or less may be provided midway in the reduction zone of the continuous hot-dip galvanizing line to separate the first reduction treatment from the second reduction treatment.
[0071] Between the first reduction treatment and the second reduction treatment, it is permissible to insert a step such as a holding step for maintaining at least one of the conditions (dew point, etc.) of the first reduction treatment, as long as this step does not adversely affect the decarburization state of the steel sheet according to this embodiment. Preferably, the second reduction treatment is performed subsequent to the first reduction treatment.
[0072] The oxidation treatment and reduction treatment may be carried out using any known single or multiple pieces of equipment. Preferably, from the viewpoints of production efficiency, cost, and quality maintenance, a continuous hot-dip galvanizing line (CGL) is used. By using a continuous hot-dip galvanizing line, oxidation treatment and reduction treatment by an oxidation-reduction method, and hot-dip galvanizing treatment and alloying treatment when producing, for example, a galvanized steel sheet as a steel sheet, can be carried out continuously in a single production line. More specifically, oxidation treatment and reduction treatment by an oxidation-reduction method can be carried out, for example, using an annealing furnace in a DFF-type continuous hot-dip galvanizing line. The oxidation treatment can be carried out, for example, in a heating zone in a DFF-type annealing furnace, as shown in the front vertical direction. The reduction treatment can be carried out, for example, in a soaking zone in a DFF-type annealing furnace.
[0073] (D) First Cooling Step After step (C), the steel is cooled to a first cooling stop temperature of 350°C to 750°C. If the first cooling stop temperature is less than 350°C, the ferrite and upper bainite cannot be sufficiently transformed (as a result, the area ratio of tempered martensite may become excessive), and the desired workability (high elongation EL, etc.) cannot be achieved. For this reason, the first cooling stop temperature is set to 350°C or higher, preferably 360°C or higher, and more preferably 370°C or higher. On the other hand, if the first cooling stop temperature exceeds 750°C, the transformation of ferrite and upper bainite does not occur, and the desired workability cannot be achieved. For this reason, the first cooling stop temperature is set to 750°C or lower, preferably 720°C or lower, and more preferably 700°C or lower.
[0074] The cooling rate from the first heating temperature to the first cooling stop temperature is not particularly limited, and the average cooling rate may be, for example, 1° C. / sec or more and 50° C. / sec or less.
[0075] (E) Dwelling Step After step (D), the steel is cooled from the first cooling stop temperature to a second cooling start temperature of 350°C to the first cooling stop temperature at an average cooling rate of 10°C / second or less, which is slower than that in step (D), and the time in the temperature range from the first cooling stop temperature to the second cooling start temperature is set to 20 to 300 seconds. Steps (D) and (E) can promote the transformation of ferrite and upper bainite.
[0076] If the average cooling rate from the first cooling stop temperature to the second cooling start temperature (350°C to the first cooling stop temperature) exceeds 10°C / sec or is equal to or greater than that in step (E), the ferrite and upper bainite cannot be sufficiently transformed, and the desired workability cannot be achieved. Therefore, the average cooling rate is 10°C / sec or less, preferably 8°C / sec or less, more preferably 5°C / sec or less, and even more preferably 3°C / sec or less. Note that if the second cooling start temperature is the first cooling stop temperature, the average cooling rate is 0°C / sec.
[0077] If the time in the temperature range from the first cooling stop temperature to the second cooling start temperature is less than 20 seconds, the ferrite and upper bainite cannot be sufficiently transformed, and the desired workability cannot be achieved. Therefore, the time is set to 20 seconds or more, preferably 25 seconds or more, and more preferably 30 seconds or more. On the other hand, if the time exceeds 300 seconds, ferrite and upper bainite are excessively formed, making it difficult to ensure a tensile strength of 980 MPa or more. Therefore, the time is set to 300 seconds or less, preferably 200 seconds or less, more preferably 150 seconds or less, and even more preferably 100 seconds or less.
[0078] (F) Second Cooling Step After step (E), the steel is cooled from the second cooling start temperature to a second cooling stop temperature of 100 to 300° C. at an average cooling rate faster than that in step (E). This causes martensitic transformation to proceed, and tempered martensite is formed by carrying out the second heating step (tempering) described below.
[0079] If the second cooling stop temperature is less than 100°C, martensitic transformation will proceed excessively, making it impossible to ensure the desired amount of retained γ, and resulting in reduced workability. Therefore, the second cooling stop temperature is set to 100°C or higher, preferably 120°C or higher, and more preferably 140°C or higher. On the other hand, if the second cooling stop temperature exceeds 300°C, the desired amount of martensite will not be ensured, and the yield stress YS (and yield ratio YR) will decrease. Therefore, the second cooling stop temperature is set to 300°C or lower, preferably 250°C or lower, and more preferably 200°C or lower.
[0080] From the viewpoint of productivity, the cooling rate from the second cooling start temperature to the second cooling stop temperature is set to an average cooling rate faster than that in step (E). The average cooling rate may be, for example, 1°C / sec or more and 50°C / sec or less.
[0081] In this step, after cooling is stopped, the temperature may be held for a certain period of time, or the second heating step described below may be carried out without holding the temperature. Even if the holding time at the second cooling stop temperature is long, the properties are hardly affected, but from the viewpoint of productivity, it is preferable to set the holding time to, for example, 600 seconds or less.
[0082] (G) Second Heating Step After step (F), the steel is heated to a second heating temperature of 300 to 500°C. This step and the holding step (H) described below temper the martensite, and also transform a portion of the untransformed austenite into bainite. As a result, C is concentrated in the untransformed austenite, stabilizing it and leaving it as retained γ.
[0083] If the second heating temperature is less than 300°C, the bainite formed with the tempered martensite becomes excessively hard, resulting in reduced workability. Therefore, the second heating temperature is set to 300°C or higher, preferably 320°C or higher, and more preferably 340°C or higher. On the other hand, if the second heating temperature exceeds 500°C, the bainite formed with the tempered martensite becomes excessively soft, resulting in reduced tensile strength TS. Therefore, the second heating temperature is set to 500°C or lower, preferably 480°C or lower, and more preferably 450°C or lower.
[0084] The heating rate from the second cooling stop temperature of 300°C or less to the second heating temperature is not particularly limited, and may be, for example, 1°C / sec or more and 100°C / sec or less as an average heating rate.
[0085] (H) Step of holding at the second heating temperature for 300 to 1800 seconds to obtain a steel sheet. After step (G), the steel sheet is held at the second heating temperature for 300 to 1800 seconds to obtain a steel sheet included in the plated steel sheet according to this embodiment. If the holding time is less than 300 seconds, the bainite transformation does not proceed sufficiently, resulting in insufficient C enrichment in the untransformed γ and a decrease in the amount of residual γ. Therefore, the holding time is set to 300 seconds or more, preferably 350 seconds or more, and more preferably 400 seconds or more. On the other hand, if the holding time exceeds 1800 seconds, there is little effect on the mechanical properties, but productivity decreases. Therefore, the holding time is set to 1800 seconds or less, preferably 1200 seconds or less, and more preferably 600 seconds or less.
[0086] (I) Step of forming a plating layer on the steel sheet The above-mentioned plating layer is formed on the surface of the steel sheet. The conditions for forming the plating layer are not particularly limited, and a conventional plating process can be adopted. For example, when forming a hot-dip galvanized layer, the hot-dip galvanizing process may be performed by immersing the steel sheet in a hot-dip galvanizing bath at a temperature of 300°C or higher and 550°C or lower. The plating time may be appropriately adjusted so as to ensure the desired coating weight, and is preferably, for example, 1 to 10 seconds.
[0087] For alloying hot-dip galvanizing, an alloying treatment may be performed after the above-mentioned hot-dip galvanizing. The alloying treatment temperature is not particularly limited, but if the alloying treatment temperature is too low, alloying does not proceed sufficiently, so it is preferably 450°C or higher, more preferably 460°C or higher, and even more preferably 480°C or higher. However, if the alloying treatment temperature is too high, alloying proceeds excessively, resulting in an excessive Fe concentration in the coating layer and deterioration of coating adhesion. From this perspective, the alloying treatment temperature is preferably 550°C or lower, more preferably 540°C or lower, and even more preferably 530°C or lower. The alloying treatment time is not particularly limited, and may be adjusted so that the hot-dip galvanizing is alloyed. The alloying treatment time is, for example, 10 to 60 seconds.
[0088] The method for manufacturing a plated steel sheet according to an embodiment of the present invention may include other steps without departing from the scope of the present disclosure.
[0089] The following examples are provided to more specifically describe the embodiments of the present invention. The embodiments of the present invention are not limited to the following examples, and may be modified as appropriate within the scope of the above-described and below-described aims, and all such modifications are within the technical scope of the embodiments of the present invention.
[0090] Steel having the chemical composition shown in Table 1 was cast, cooled to room temperature after casting, and then heated to 1200 to 1350°C. Thereafter, hot rolling including rough rolling at a temperature of 1100°C or higher and finish rolling at a temperature of 920°C or higher was performed, followed by cooling after finish rolling and coiling at a temperature of 600°C or higher to obtain a rolled plate. This rolled plate was pickled to remove surface scale, and then cold rolled at a rolling ratio of 40 to 50% to obtain a plate thickness of 1.0 to 1.6 mm.
[0091]
[0092] The rolled steel sheets were subjected to the above-described step (B1) and steps (B) to (I) under the conditions shown in Table 2 to obtain plated steel sheets of Test Nos. 1 to 10 (however, for Test Nos. 8 to 10, as described below, the steel sheets were not plated, and only the temperature history of step (I) for forming a plating layer was given). In Table 2, "-" indicates that the data was not measured. Although not shown in Table 2, in Test Nos. 1 to 10, step (B1) was performed during the temperature rise to the first heating temperature in step (B), the oxygen concentration at each temperature reached was 0.1 to 2%, and the temperature rise time in the oxidation treatment was 10 seconds or more and 120 seconds or less. The heating times (holding times) of the first reduction treatment (step (C1a)) and the second reduction treatment (step (C1b)) were each 60 seconds or more. In addition, in step (E), the steel sheet was held at the first cooling stop temperature (i.e., the first cooling stop temperature and the second cooling start temperature were equivalent), and the "time in the temperature range from the first cooling stop temperature to the second cooling start temperature" corresponded to the holding time at the first cooling stop temperature, and the average cooling rate from the first cooling stop temperature to the second cooling start temperature was 0°C / sec. In step (F), the steel sheet was cooled to the second cooling stop temperature at an average cooling rate faster than that in step (E). In step (I), the steel sheet was immersed in a hot-dip galvanizing bath at 300°C to 550°C (galvanizing time: 1 to 10 seconds) and then subjected to an alloying treatment, with the alloying treatment time being 10 to 60 seconds. In Tests Nos. 8 to 10, only the temperature history was applied to step (I). Specifically, the steel sheet was heated to 300°C to 550°C and held there for 1 to 10 seconds, and then held at the "alloying treatment temperature" shown in Table 2 for 10 to 60 seconds.
[0093]
[0094] The plated steel sheets of Test Nos. 1 to 10 described above were subjected to the following evaluations.
[0095] <Metal Structure Evaluation> For the plated steel sheets of Test Nos. 1 to 10, test specimens were taken from the end toward the center in the sheet width direction (perpendicular to the rolling direction and sheet thickness direction) so as to include a position of W (sheet width) / 4. A cross section parallel to the rolling direction and sheet width direction and located 1 / 4 of the sheet thickness from the steel sheet surface of the plated steel sheet was exposed from the test specimen by nital etching. The cross section was observed using an SEM, and the sum of the area fraction of ferrite and the area fraction of upper bainite, the area fraction of tempered martensite, and the area fraction of MA were determined using the above-mentioned method. Furthermore, an X-ray diffraction pattern was obtained from the cross section using Co-Kα radiation as characteristic X-rays, and the volume fraction of retained γ was determined using the above-mentioned method. Regarding the remaining structure, no structures other than pearlite and cementite were observed, and the total amount of the remaining structure was 10 area % or less.
[0096] <Means for Measuring Decarburization Behavior: Measurement of Carbon Profile by GD-OES> As described below, carbon profile was measured by GD-OES (Glow Discharge Optical Emission Spectrometry) to examine the decarburization behavior.
[0097] (Sample Preparation) Materials measuring 50 mm x 40 mm x thickness or 30 mm x 30 mm x thickness were collected. They were then degreased as per usual methods to prepare samples. Using these samples, the mass % concentration of each element was measured using GD-OES under the following conditions.
[0098] (Measurement conditions) Equipment used: Marcus-type radio frequency glow discharge optical emission surface analyzer (rf-GD-OES) GD-Profiler 2 manufactured by HORIBA, Ltd. Sputtering method: normal sputtering Measurement range: φ4 mm Type of gas: Ar Elements to be analyzed: B, C, O, Al, Si, Ti, Cr, Mn, Fe, Zn, P, S, N (In this example, the evaluation was performed on these elements, but if elements other than those mentioned above are contained in, for example, the plating layer and / or the steel sheet, the elements other than those mentioned above will also be analyzed.)
[0099] (Measurement Method) GD-OES measurements were carried out on the plated surface of the sample up to a depth of 150 μm in the thickness direction.
[0100] (Analysis Method) Since the sputtering rate of the above-mentioned device is almost constant, the sputtering crater depth of the sample was measured after the analysis was completed, and the value (sputtering depth) was plotted on the horizontal axis.
[0101] The details of the calibration curve method for converting the measured emission intensity of each element into a concentration are shown below.
[0102] Sputter weight W of element i per unit time i (g / sec) and luminescence intensity I i The relationship between W and W is expressed by the following formula (3) using the slope a and intercept b of the calibration curve. i = aI i + b Equation (3) Sputter weight W of the element i per unit time i is the concentration C i (wt.%), density ρ (g / cm 3 ), and for a reference sample with a known sputtering rate Δd (cm / sec), the sputtering area S (cm 2 ) and is calculated using the following formula (4): i =C i ×ρ×Δd×S...Formula (4)
[0103] W i Using two or more reference samples with known emission intensities I i The slope a and intercept b of the above formula (3) were determined, and a calibration curve was created with the horizontal axis representing the emission intensity and the vertical axis representing the spatter weight. The reference materials used are shown in Table 3 below. Using the created calibration curve, the spatter weight was determined from the emission intensity of each target element, and the weight ratio was used to convert it into a concentration. The calibration curve used to convert the O concentration was 2 Correction was performed using the formula so that the concentration ratio of Si to O became 1:2.
[0104]
[0105] The carbon analysis results were used to obtain carbon profiles, an example of which is shown in Figure 1. Figure 1 shows the carbon profiles of Test No. 5 and Test No. 7. In Figure 1, the carbon profiles of all materials have a carbon concentration peak within the surface layer of 20 μm (specifically, in the internal oxide layer), but it can be seen that in Test No. 7, the carbon concentration is higher than the bulk carbon concentration, whereas in Test No. 5, the carbon concentration is kept sufficiently lower than the bulk carbon concentration.
[0106] From the obtained carbon concentration profile in the sheet thickness direction, the position where the carbon concentration (mass%) was 50% of the bulk carbon concentration and the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm were determined. Note that the bulk carbon concentration was corrected for analysis so that the carbon concentration at a sufficiently deep position (120 to 150 μm) measured by GD-OES was the value obtained by conventional steel analysis. For example, if the steel analysis value was 0.22% and the GD-OES analysis value was 0.25%, the GD-OES analysis value was multiplied by 0.22 / 0.25 and used for analysis.
[0107] <Evaluation of tensile strength, yield stress, yield ratio, elongation, and tensile strength variations in the sheet width direction> JIS No. 5 test pieces (plate-shaped test pieces) were taken so that the sheet width direction in a plane parallel to the cold-rolled rolling surface of the steel sheet was the longitudinal direction of the test piece. Regarding the sampling positions, where the sheet width is W, test pieces were taken from five locations in the sheet width direction: two locations at W / 8 from both ends toward the center, two locations at W / 4 from both ends toward the center, and one location in the center. Using the test pieces, a tensile test was performed in accordance with JIS Z 2241:2011 to measure the tensile strength TS, yield stress YS, and elongation EL. The yield ratio YR was calculated as YS / TS. The minimum tensile strength TS of the five locations was minExamples where the yield ratio YS was 980 MPa or more were evaluated as sufficient, and examples where it was less than 980 MPa were evaluated as insufficient. Examples where the yield ratio YS was 0.55 to 0.75 were evaluated as sufficient, and examples where it was outside the range of 0.55 to 0.75 were evaluated as insufficient. Examples where the elongation EL was 19% or more were evaluated as sufficient, and examples where it was less than 19% were evaluated as insufficient. Note that for each physical property value other than tensile strength, the value measured using a test specimen taken from one location in the sheet width direction, which was W / 4 from both ends toward the center, was used.
[0108] <Hole Expanding Ratio Evaluation> For Test Nos. 1 to 10, a hole expanding test specified in JIS Z 2256:2010 was performed to measure the hole expanding ratio λ. Examples in which the hole expanding ratio λ was 20% or more were evaluated as sufficient, and examples in which the hole expanding ratio λ was less than 20% were evaluated as insufficient.
[0109] <Evaluation of Limit Bendability (R / t)> The bendability of Test Nos. 1 to 10 was evaluated according to the following procedure. Test pieces with a width of 40 mm and a length of 100 mm were prepared with the major axis in the sheet width direction, and a bending test was performed using the V-block method in accordance with JIS Z 2248:2014. The bending radius was varied from 0 to 7 mm to determine the minimum bending radius at which the material could be bent without breaking. This was taken as the limit bending radius R (mm), and the ratio of limit bending radius R (mm) to sheet thickness t (mm) was calculated. Examples where the limit bending radius R (mm) / sheet thickness t (mm) was 2.0 or less were evaluated as having excellent bendability, and examples where the ratio exceeded 2.0 were evaluated as having poor bendability.
[0110] The results are shown in Table 4. In Table 4, "-" indicates that the measurement was not performed. In Table 4, "F+UB" is the sum of the area fractions of ferrite and upper bainite, "M" is the area fraction of tempered martensite, "MA" is the area fraction of MA, "residual γ" is the volume fraction of retained austenite, and "maximum carbon concentration in surface layer" is the maximum carbon concentration (mass%) in a region from the surface of the steel sheet to 20 μm in the sheet thickness direction.
[0111]
[0112] The results in Table 4 can be considered as follows. Test Nos. 1 to 4 in Table 4 all satisfied the requirements defined in the embodiments of the present invention, exhibiting high strength, a predetermined yield ratio, and high workability, and also satisfying formula (1). Test Nos. 1 to 4 also satisfied the requirements for excellent bendability (satisfying at least one of the above-mentioned (I) and (II)), and were excellent in bendability. On the other hand, Test Nos. 5 to 7 in Table 4 all did not satisfy the requirements defined in the embodiments of the present invention, and were insufficient in the evaluation of the strength, yield ratio, workability, and / or tensile strength variations in the sheet width direction.
[0113] In Test No. 5, the first heating temperature in step (B) was less than 850°C, so the variation in tensile strength in the sheet width direction was large. However, Test No. 5 met the requirements for exhibiting excellent bendability (satisfying at least one of the above-mentioned (I) and (II)), and was excellent in bendability.
[0114] In Test No. 6, the first heating temperature was above 910°C, so the total of ferrite and upper bainite was less than 30 area % and tempered martensite was more than 45 area %, resulting in a yield ratio YR of more than 0.75. However, Test No. 6 met the requirements for exhibiting excellent bendability (satisfying at least one of the above-mentioned (I) and (II)), and was therefore excellent in bendability.
[0115] In Test No. 7, the first heating temperature in step (B) was less than 850°C, resulting in a large variation in tensile strength in the sheet width direction. Furthermore, the dew point in step (C1b) was less than -25°C and lower than the dew point in step (C1a), which did not satisfy the requirements for excellent bendability (satisfying at least one of the above-mentioned (I) and (II)), resulting in poor bendability.
[0116] In Test No. 8, the C content exceeded 0.300% by mass, the Al content was less than 0.300% by mass, and the first heating temperature in step (B) exceeded 910°C, so the total of ferrite and upper bainite was less than 30% by area, tempered martensite was more than 45% by area, and MA was less than 5% by area, resulting in a yield ratio YR of more than 0.75 and an elongation EL of less than 19%.
[0117] In Test No. 9, the Ti content was less than 0.010% by mass, the first cooling stop temperature in step (D) was less than 350°C, and the holding time in the second heating in step (H) was less than 300 seconds, so the total of ferrite and upper bainite was less than 30 area %, tempered martensite was more than 45 area %, and MA was less than 5 area %, and the yield ratio YR was more than 0.75 and the elongation EL was less than 19%.
[0118] In Test No. 10, the first heating temperature in step (B) was above 910°C and the second cooling stop temperature in step (F) was above 300°C, so the tempered martensite was less than 10 area% and the MA was more than 35 area%, and the yield ratio YR was less than 0.55, the elongation EL was less than 19%, and the hole expansion ratio λ was less than 20%.
[0119] This application claims priority from Japanese Patent Application No. 2023-056191, filed March 30, 2023, and Japanese Patent Application No. 2024-022772, filed February 19, 2024. Japanese Patent Application Nos. 2023-056191 and 2024-022772 are incorporated herein by reference.
Claims
1. A plated steel sheet comprising a steel sheet and a plating layer disposed on a surface of the steel sheet, the plated steel sheet satisfying the following formulas (1) and (2), wherein the steel sheet contained in the plated steel sheet has a component composition consisting of: C: 0.150 to 0.300 mass%, Si: 0.80 to 2.20 mass%, Mn: 1.60 to 2.80 mass%, Al: 0.300 to 0.800 mass%, Ti: 0.010 to 0.050 mass%, P: 0.050 mass% or less (including 0 mass%), S: 0.0100 mass% or less (including 0 mass%), N: 0.0100 mass% or less (including 0 mass%), and the balance: iron and unavoidable impurities; and A plated steel sheet having a metal structure in which the total of ferrite and upper bainite is 30 to 70 area %, tempered martensite is 10 to 45 area %, MA is 5 to 35 area %, and retained austenite is 5 to 20 volume %. max -TS min <20MPa...(1) TS min ≧980 MPa (2) In the formulas (1) and (2), TS max is the maximum value of the tensile strength at five different points in the sheet width direction of the plated steel sheet, and TS min is the minimum value of the tensile strength at the five locations, and the five locations are, in the sheet width direction, two locations at positions W / 10 to W / 8 from both ends toward the center, two locations at positions W / 4 from both ends toward the center, and one location in the center, where W is the sheet width.
2. The plated steel sheet according to claim 1, further comprising at least one selected from the group consisting of Nb: more than 0 mass% and not more than 0.20 mass% and V: more than 0 mass% and not more than 0.50 mass%.
3. The plated steel sheet according to claim 1, further comprising at least one selected from the group consisting of Ni: more than 0 mass% and not more than 2.0 mass%, Cr: more than 0 mass% and not more than 2.0 mass%, and Mo: more than 0 mass% and not more than 0.50 mass%.
4. The plated steel sheet according to claim 1, further comprising B: more than 0 mass% and not more than 0.0050 mass%.
5. The plated steel sheet according to claim 1, further comprising at least one selected from the group consisting of Mg: more than 0 mass% and not more than 0.040 mass%, REM: more than 0 mass% and not more than 0.040 mass%, and Ca: more than 0 mass% and not more than 0.040 mass%.
6. The plated steel sheet according to claim 1, wherein in the sheet thickness direction, a position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is located in a region that is 0.2% or more of the sheet thickness from the surface of the steel sheet.
7. The plated steel sheet according to claim 1, wherein the maximum carbon concentration (mass%) in a region extending from the surface of the steel sheet to 20 μm in the sheet thickness direction is less than 70% of the bulk carbon concentration.
8. A process for obtaining a rolled plate by hot rolling a steel having a chemical composition according to any one of claims 1 to 5; a first heating process for heating the rolled plate to a first heating temperature of 850°C or more and 910°C or less; a process for holding the plate at the first heating temperature for 5 to 1800 seconds after the first heating process; a first cooling process for cooling the plate to a first cooling stop temperature of 350°C to 750°C after the holding process; a retention process for holding the plate from the first cooling stop temperature to a second cooling start temperature which is 350°C to the first cooling stop temperature at an average cooling rate of 10°C / sec or less and slower than that of the first cooling process after the first cooling process, and for a time in the temperature range from the first cooling stop temperature to the second cooling start temperature of 20 to 300 seconds after the retention process; and a second cooling process for cooling the plate from the second cooling start temperature to a second cooling stop temperature of 100 to 300°C at an average cooling rate faster than that of the retention process after the retention process.
8. The method for producing a plated steel sheet according to claim 1, comprising: a second heating step of heating to a second heating temperature of 300 to 500° C. after the second cooling step; a step of holding the steel sheet at the second heating temperature for 300 to 1800 seconds after the second heating step to obtain a steel sheet; and a step of forming a plating layer on the steel sheet.
9. The method of claim 8, further comprising, after the step of obtaining the rolled plate, performing an oxidation treatment under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C, and the holding step includes performing a first reduction treatment having a dew point of -35 to -15°C, and then a second reduction treatment having a dew point of -25 to 0°C, which is higher than that of the first reduction treatment.
Citation Information
Patent Citations
HIGH STRENGTH COLD ROLLED STEEL SHEET EXCELLENT IN PROCESSABILITY AND COLLISION CHARACTERISTICS AND HAVING TENSILE STRENGTH OF 980 MPa OR MORE, AND MANUFACTURING METHOD THEREFOR
JP2016194139A
Method for installing duct in centralized type air conditioning system and duct used for the same
JP2023056191A
Learning data generation system, estimation system, learning data generation method, estimation method, and program
JP2024022772A
Hot rolled steel sheet for cold rolled steel sheet or for hot-dip galvanized steel sheet and method of producing the same
JP2016089235A
Tempered coated steel sheet with very good formability and method for producing same
JP2020509202A