Steel sheet and method for manufacturing steel sheet

The optimization of a steel plate's decarburized layer and annealing process addresses the bendability and strength challenges of high-strength steel plates with Si and Mn additions, achieving effective plating adhesion and weight reduction for vehicle bodies.

WO2024203606A1PCT designated stage expired Publication Date: 2024-10-03KOBE STEEL LTD

Patent Information

Application Number
PCT/JP2024/010716
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-19
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

High-strength steel plates with added Si and Mn face challenges in bendability due to surface oxidation, leading to poor plating adhesion and unplated areas, and existing methods do not adequately address the need for both high strength and excellent bendability in vehicle body materials.

Method used

A steel plate with a controlled decarburized layer, where the carbon concentration gradient is optimized within specific ranges near the surface, combined with an annealing process involving oxidation and reduction treatments at controlled oxygen concentrations and dew points, to enhance both strength and bendability.

Benefits of technology

The approach results in a steel plate with high tensile strength (980 MPa or more) and excellent bendability, as evidenced by reduced carbon concentration near the surface and controlled decarburization, enabling effective plating adhesion and weight reduction in vehicle bodies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010716_03102024_PF_FP_ABST
    Figure JP2024010716_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A steel sheet in which a position in the sheet thickness direction where the carbon concentration (mass%) is 50% of the bulk carbon concentration is in a region of at least 0.20% of the sheet thickness from the surface of the steel sheet, and a position in the sheet thickness direction where the carbon concentration (mass%) is 90% of the bulk carbon concentration is in a region of no more than 8.0% of the sheet thickness from the surface of the steel sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Steel plate and method for manufacturing the same

[0001] The present disclosure relates to a steel sheet and a method for manufacturing the steel sheet, and more particularly to a high-tensile steel sheet having excellent bendability and a method for manufacturing the steel sheet.

[0002] There has been a demand for improved occupant safety in vehicles, and for this purpose, the strength of vehicle body materials has been improved. On the other hand, against the backdrop of worsening issues such as global warming, there has been an accelerating movement to improve automobile fuel efficiency. It is known that reducing the weight of vehicle bodies is an effective way to improve fuel efficiency.

[0003] The addition of Si and Mn is effective in increasing the strength of steel sheets to achieve vehicle body weight reduction. However, during continuous annealing, Si and Mn oxidize even in a reducing atmosphere in which Fe oxidation does not occur, and oxides of Si and Mn are formed on the outermost surface of the steel sheet. The oxides of Si and Mn reduce the wettability between molten zinc and the base steel sheet during, for example, a zinc-based plating process, so steel sheets to which Si and Mn have been added have problems such as frequent bare spots or poor plating adhesion.

[0004] In response to the above-mentioned problems, Patent Document 1 discloses a method for producing a high-strength hot-dip galvanized steel sheet that is excellent in coating adhesion, workability, and fatigue resistance, in which the steel sheet is treated with O 2 Concentration 1000 ppm by volume or more, H 2 The mixture is heated at a temperature of 400 to 750°C in an atmosphere with an O concentration of 1000 ppm by volume or more, and then 2 Concentration less than 1000 ppm by volume, H 2 An oxidation treatment is performed by heating at a temperature of 600 to 850°C in an atmosphere with an O concentration of 1000 volume ppm or more, and then in a heating zone, H 2 Concentration is 5 to 30% by volume, H 2 O concentration is 10 to 1000 volume ppm, the remainder is N 2 and inevitable impurities in an atmosphere, the temperature is increased to 650 to 900°C at a rate of 0.1°C / sec or more, and then the 2 Concentration is 5 to 30% by volume, H 2 O concentration is 500 to 5000 volume ppm, the remainder is N 2and unavoidable impurities, the temperature change in the soaking zone is within ±20° C., and reduction annealing is performed by soaking for 10 to 300 seconds.

[0005] Japanese Patent Application Laid-Open No. 2017-166057

[0006] When manufacturing automotive parts, steel sheets are sometimes bent to form part shapes. However, high-strength steel sheets, for example, having a strength of 980 MPa or more, or even 1180 MPa or more, are difficult to be bent satisfactorily to form the desired part shape, i.e., it is difficult to ensure excellent bendability. Patent Document 1 does not address the issue of improving the bendability of plated steel sheets. The present disclosure has been made in view of the above circumstances, and its purpose is to provide a steel sheet that is high in strength, can contribute to weight reduction of a vehicle body, and exhibits excellent bendability, and a method for easily manufacturing the steel sheet.

[0007] A first aspect of the present invention is a steel sheet in which, in the sheet thickness direction, the position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is in a region that is 0.20% or more of the sheet thickness from the steel sheet surface, and the position where the carbon concentration (mass %) is 90% of the bulk carbon concentration is in a region that is 8.0% or less of the sheet thickness from the steel sheet surface.

[0008] Aspect 2 of the present invention is a steel sheet having a maximum carbon concentration (mass%) in a region from the surface of the steel sheet to 20 μm in the sheet thickness direction of less than 70% of the bulk carbon concentration, and a surface decarburization amount per mm of sheet thickness on one side of the steel sheet of 0.045 mol / m 2 The steel sheet according to aspect 1, which is as follows:

[0009] A third aspect of the present invention is the steel sheet according to the first or second aspect, which has a tensile strength of 980 MPa or more.

[0010] A fourth aspect of the present invention is the steel sheet according to any one of the first to third aspects, wherein the chemical composition satisfies the following: C: 0.08% by mass or more and 0.30% by mass or less; Si: more than 0.5% by mass and 3.0% by mass or less; Mn: 1.5% by mass or more and 3.0% by mass or less; Cr: 0% by mass or more and 1.0% by mass or less; P: more than 0.1% by mass or less; S: more than 0.05% by mass or less; Al: more than 0% by mass and 1.0% by mass or less; and N: more than 0.01% by mass or less, with the balance being Fe and inevitable impurities.

[0011] A fifth aspect of the present invention is a method for producing a steel sheet, comprising an annealing step of performing an oxidation treatment under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C, followed by a reduction treatment, wherein the reduction treatment includes a first reduction treatment having a dew point of −35 to −15°C, followed by a second reduction treatment having a dew point of −25 to 0°C, which is higher than the dew point of the first reduction treatment.

[0012] A sixth aspect of the present invention is the method for producing a steel sheet according to the fifth aspect, wherein the temperature achieved in the first reduction treatment and the second reduction treatment is 800 to 920°C.

[0013] According to the present disclosure, it is possible to provide a steel sheet that has high strength, can contribute to reducing the weight of a vehicle body, and exhibits excellent bendability, and a method for manufacturing the steel sheet.

[0014] FIG. 1-1 is a graph showing the relationship between the dew point at the center of the soaking zone during the second reduction treatment and R / t. FIG. 1-2 is another graph showing the relationship between the dew point at the center of the soaking zone during the second reduction treatment and R / t. FIG. 2-1 is a graph showing the relationship between the dew point at the center of the soaking zone during the second reduction treatment and tensile strength TS. FIG. 2-2 is another graph showing the relationship between the dew point at the center of the soaking zone during the second reduction treatment and tensile strength TS. FIG. 3 is a diagram showing an example of a carbon concentration profile obtained in an example. FIG. 4-1 is a graph showing the relationship between R / t and the position where the carbon concentration (mass%) in the thickness direction is 50% of the bulk carbon concentration. FIG. 4-2 is another graph showing the relationship between R / t and the position where the carbon concentration (mass%) in the thickness direction is 50% of the bulk carbon concentration. FIG. 5-1 is a graph showing the relationship between tensile strength TS and the position where the carbon concentration (mass%) in the thickness direction is 90% of the bulk carbon concentration. Figure 5-2 is another graph showing the relationship between the position where the carbon concentration (mass%) in the sheet thickness direction is 90% of the bulk carbon concentration and tensile strength TS. Figure 6-1 is a graph showing the relationship between the ratio of the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm to the bulk carbon concentration and R / t. Figure 6-2 is another graph showing the relationship between the ratio of the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm to the bulk carbon concentration and R / t. Figure 7-1 is a graph showing the relationship between the amount of surface decarburization per 1 mm of sheet thickness and tensile strength TS. Figure 7-2 is another graph showing the relationship between the amount of surface decarburization per 1 mm of sheet thickness and tensile strength TS.

[0015] The present inventors have conducted extensive research to obtain a steel sheet that exhibits excellent bendability in bending despite its high strength. As a result, they have found that by providing a decarburized layer within a predetermined range in the surface layer of the steel sheet, excellent bendability can be obtained while maintaining high strength. They have also found that a decarburized layer within a predetermined range that can achieve both high strength and excellent bendability can be formed in the surface layer of the steel sheet by controlling the conditions for annealing the steel sheet (original sheet). Hereinafter, the steel sheet of this embodiment will first be described.

[0016] [Steel Plate] (Decarburized Layer at Surface of Steel Plate) The steel plate according to this embodiment has the following characteristics: (I) In the plate thickness direction, the position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is in a region of 0.20% or more of the plate thickness from the surface of the steel plate, and the position where the carbon concentration (mass %) is 90% of the bulk carbon concentration is in a region of 8.0% or less of the plate thickness from the surface of the steel plate.

[0017] In the steel sheet according to this embodiment, the position in the sheet thickness direction where the carbon concentration (mass %) is 50% of the bulk carbon concentration is located in a region of 0.20% or more of the sheet thickness from the surface of the steel sheet. This position relates to the thickness of the decarburized layer that contributes to bendability. By ensuring that this position is located in a region of 0.20% or more of the sheet thickness from the surface of the steel sheet and that the decarburized layer has a thickness of at least a certain level that contributes to bendability, it is possible to reliably exhibit excellent bendability in bending. The position where the carbon concentration (mass %) is 50% of the bulk carbon concentration may be located in a region of at least 0.5%, or even at least 1.0%, of the sheet thickness from the surface of the steel sheet.

[0018] Furthermore, in the steel sheet according to this embodiment, the position in the sheet thickness direction where the carbon concentration (mass%) is 90% of the bulk carbon concentration is located in a region of 8.0% or less of the sheet thickness from the surface of the steel sheet. Increasing the thickness of the decarburized layer improves bendability, but tends to reduce strength. However, the inventors have conducted studies and found that if the position where the carbon concentration (mass%) is 90% of the bulk carbon concentration is located in a region of 8.0% or less of the sheet thickness from the surface of the steel sheet, the reduction in strength can be sufficiently suppressed. The position where the carbon concentration (mass%) is 90% of the bulk carbon concentration may be located in a region of 6.0% or less of the sheet thickness from the surface of the steel sheet.

[0019] The steel plate according to this embodiment has the following characteristics: (II) the maximum carbon concentration (mass%) in a region from the surface of the steel plate to 20 μm in the plate thickness direction is less than 70% of the bulk carbon concentration; and (II) the amount of surface decarburization per mm of plate thickness on one side of the steel plate is 0.045 mol / m 2 or less, preferably 0.035 mol / m 2 Also the following:

[0020] The present inventors examined conventional steel sheets and first found that a region with a significantly high carbon concentration exists in the surface layer of the steel sheet, and that this is the cause of deterioration in bendability. Then, as described below, they investigated the manufacturing conditions of the steel sheet and found that excellent bendability can be easily obtained by promoting decarburization in the surface layer of the steel sheet and suppressing the carbon concentration in the surface layer of the steel sheet. Specifically, they found that excellent bendability can be easily obtained by suppressing the maximum carbon concentration (mass %) in the region from the surface of the steel sheet to 20 μm in the thickness direction to less than 70% of the bulk carbon concentration. The maximum carbon concentration is preferably 65% ​​or less of the bulk carbon concentration, and more preferably 60% or less of the bulk carbon concentration.

[0021] In addition, the steel plate according to this embodiment has a surface decarburization amount of 0.045 mol / m per 1 mm of plate thickness on one side of the steel plate. 2 or less, preferably 0.035 mol / m 2 By suppressing the surface decarburization amount per mm of plate thickness to 0.030 mol / m or less, a high strength of 980 MPa or more, particularly 1180 MPa or more, can be ensured. 2 More preferably, it is 0.025 mol / m or less. 2 The following is the result.

[0022] From the viewpoint of achieving both high strength and excellent bendability, the steel sheet according to this embodiment only needs to satisfy at least one of the above (I) and (II), and preferably satisfies the above (I), and more preferably satisfies both the above (I) and (II).

[0023] The "steel sheet surface" refers to the surface of the steel sheet in the case of a steel sheet obtained by annealing a cold-rolled steel sheet, and to the position of the interface between the coating layer and the base steel sheet in the case of a plated steel sheet. In the case of a zinc-based coating, for example, the position of the interface between the coating layer and the base steel sheet refers to the point where Zn constituting the coating layer is no longer detected (the Zn analysis value is 0) when Zn is analyzed from the surface of the coating layer in the thickness direction of the coating layer by GD-OES as performed in the examples described below, and this point is defined as the starting point of the distance (depth) from the steel sheet surface.

[0024] The steel sheet according to this embodiment exhibits excellent bendability in bending despite its high strength. For example, the strength may be a tensile strength TS of 980 MPa or more, preferably 1180 MPa or more. Furthermore, when subjected to a bending test shown in the examples described later, the steel sheet according to this embodiment exhibits excellent bendability with a limit R / t of less than 2.5.

[0025] The thickness of the steel sheet according to this embodiment is not limited, and can be, for example, 0.4 mm or more and 4 mm or less (in the case of a plated steel sheet, the thickness of the base steel sheet).

[0026] (Composition of Steel Sheet) To achieve high strength, the steel sheet according to this embodiment may have a composition in which the Si content exceeds 0.5 mass %, for example. The Si content is more preferably 1.0 mass % or more, even more preferably 1.1 mass % or more, and even more preferably 1.2 mass % or more. The upper limit of the Si content may be, for example, 3.0 mass %.

[0027] In one preferred embodiment, the steel sheet has a chemical composition that satisfies the following: C: 0.08% by mass or more and 0.30% by mass or less, Si: more than 0.5% by mass and 3.0% by mass or less, Mn: 1.5% by mass or more and 3.0% by mass or less, Cr: 0% by mass or more and 1.0% by mass or less, P: more than 0.1% by mass or less, S: more than 0.05% by mass or less, Al: more than 0% by mass and 1.0% by mass or less, and N: more than 0.01% by mass or less, with the balance being Fe and inevitable impurities. Each element will be described below.

[0028] [C: Preferably 0.08% by mass or more, 0.30% by mass or less] C is an element effective in improving the strength of steel sheets. When included in steel together with Si, and optionally with Mn, C is a particularly effective strengthening element for ensuring a final tensile strength of 980 MPa or more, or even 1180 MPa or more. Furthermore, C is also an element necessary for ensuring retained austenite and improving workability. To effectively exert this effect, the C content is preferably 0.08% by mass or more, more preferably 0.11% by mass or more, and even more preferably 0.13% by mass or more. While a high C content is preferable from the viewpoint of ensuring the strength of the steel sheet, excessive C content may deteriorate corrosion resistance, spot weldability, and workability. Therefore, the C content is preferably 0.30% by mass or less, more preferably 0.25% by mass or less, and even more preferably 0.23% by mass or less.

[0029] [Mn: Preferably 1.5% by mass or more, and 3.0% by mass or less] Like Si, Mn is an inexpensive strengthening element for steel and is effective in improving the strength of steel sheets. Mn, when contained in steel together with Si and, if necessary, C, is a particularly effective strengthening element for ensuring a final tensile strength of 980 MPa or more, and even 1180 MPa or more. Furthermore, Mn stabilizes austenite and contributes to improving the workability of steel sheets by generating retained austenite. To effectively exert this effect, the Mn content is preferably 1.5% by mass or more, more preferably 1.8% by mass or more, and even more preferably 2.0% by mass or more. However, if the Mn content is too high, the ductility of the steel sheet may decrease, adversely affecting the workability of the steel sheet and further reducing the weldability of the steel sheet. From these viewpoints, the Mn content is preferably 3.0% by mass or less, more preferably 2.8% by mass or less, and even more preferably 2.7% by mass or less.

[0030] [Si: More than 0.5 mass% and 3.0 mass% or less] Si is an inexpensive steel strengthening element that does not significantly affect the workability of steel sheets. Furthermore, Si is an element that can suppress the decomposition of retained austenite, which is useful for improving the workability of steel sheets, and the formation of carbides. To effectively exert this effect, the Si content is more than 0.5 mass%, preferably 1.0 mass% or more, more preferably 1.1 mass% or more, and even more preferably 1.2 mass% or more. While there is no particular upper limit for the Si content, if the Si content is too high, the solid solution strengthening effect of Si may become significant, increasing the rolling load. Furthermore, Si scale may be generated during hot rolling, resulting in surface defects of the steel sheet. Therefore, from the viewpoint of, for example, manufacturing stability, the Si content is preferably 3.0 mass% or less, more preferably 2.7 mass% or less, and even more preferably 2.5 mass% or less.

[0031] [Cr: Preferably 0% by mass or more and 1.0% by mass or less] Cr is an element effective in improving the strength of steel sheet. Furthermore, Cr improves the corrosion resistance of steel sheet and has the effect of suppressing hydrogen generation due to corrosion of steel sheet. Specifically, Cr has the effect of promoting the formation of iron oxide (α-FeOOH). Iron oxide is said to be thermodynamically stable and protective among rusts formed in the atmosphere. By promoting the formation of such rust, the penetration of generated hydrogen into the steel sheet can be suppressed, and hydrogen-assisted cracking can be sufficiently suppressed even when the steel sheet is used in a severe corrosive environment, for example, in the presence of chlorides. Furthermore, Cr, like B and Ti, is an element effective in improving the delayed fracture resistance of steel sheet. Therefore, Cr can be contained in an amount that does not affect the strength and workability, such as elongation, of the steel sheet. Although the Cr content may be 0% by mass, to effectively exert these effects, the Cr content is preferably more than 0% by mass, more preferably 0.003% by mass or more, and even more preferably 0.01% by mass or more. On the other hand, if the Cr content is excessive, there is a risk that the workability of the steel sheet, such as elongation, may deteriorate. Therefore, the Cr content is preferably 1.0 mass% or less, more preferably 0.8 mass% or less, and even more preferably 0.6 mass% or less.

[0032] [P: preferably more than 0 mass% and 0.1 mass% or less] P is an element that is inevitably present as an impurity element. If the P content is excessive, it may deteriorate weldability. Therefore, the P content is preferably suppressed to 0.1 mass% or less, more preferably 0.08 mass% or less, and even more preferably 0.05 mass% or less.

[0033] [S: preferably more than 0 mass% and 0.05 mass% or less] S is an element that is inevitably present as an impurity element. Usually, steel inevitably contains about 0.0005 mass% of S. Excessive S content may form sulfide-based inclusions, promote hydrogen absorption in a corrosive environment, deteriorate the delayed fracture resistance of the steel sheet, and deteriorate the weldability and workability of the steel sheet. Therefore, the S content is preferably suppressed to 0.05 mass% or less, more preferably 0.01 mass% or less, and even more preferably 0.005 mass% or less.

[0034] [Al: preferably more than 0 mass% and 1.0 mass% or less] Al is an element that has a deoxidizing effect. To effectively exert this effect, the Al content is preferably more than 0 mass%, more preferably 0.005 mass% or more, and even more preferably 0.02 mass% or more. If the Al content is excessive, inclusions such as alumina may increase, which may deteriorate the workability of the steel sheet. Therefore, the Al content is preferably 1.0 mass% or less, more preferably 0.8 mass% or less, and even more preferably 0.5 mass% or less.

[0035] [N: preferably more than 0 mass% and 0.01 mass% or less] N is an element that is inevitably present as an impurity element. If the N content is excessive, nitrides may be formed, which may deteriorate the workability of the steel sheet. In particular, when the steel sheet contains B to improve hardenability, N combines with B to form BN precipitates, which inhibits the hardenability-improving effect of B. Therefore, the N content is preferably suppressed to 0.01 mass% or less, more preferably 0.008 mass% or less, and even more preferably 0.005 mass% or less.

[0036] [Balance] The balance is Fe and inevitable impurities. The inevitable impurities include trace elements (e.g., As, Sb, Sn, etc.) that are introduced depending on the conditions of raw materials, materials, manufacturing equipment, etc. The aforementioned P, S, and N are generally preferable as their contents are lower, so they can also be considered inevitable impurities. However, the present disclosure can easily achieve its effects by suppressing the contents of these elements to a specific range, and therefore defines them as above. For this reason, in this specification, the "unavoidable impurities" that constitute the balance are a concept that excludes elements whose composition ranges are specified.

[0037] In addition to the above components, other well-known optional components may also be contained to the extent that they do not impair strength or sufficient bendability. Optional components include Cu, Ni, Ti, Nb, V, and B. These optional components are described below.

[0038] [Cu: preferably more than 0 mass% and 1.0 mass% or less] Like Cr, Cu is an element that is effective in improving the strength of the steel sheet and has the effect of suppressing hydrogen generation due to corrosion of the steel sheet, thereby improving the corrosion resistance of the steel sheet. Like Cr, Cu has the effect of promoting the formation of iron oxide. To effectively exert these effects, the Cu content is preferably more than 0 mass%, more preferably 0.003 mass% or more, and even more preferably 0.05 mass% or more. Furthermore, from the viewpoint of the workability of the steel sheet, the Cu content is preferably 1.0 mass% or less, more preferably 0.8 mass% or less, and even more preferably 0.5 mass% or less.

[0039] [Ni: preferably more than 0 mass% and 1.0 mass% or less] Like Cr and Cu, Ni is an element that is effective in improving the strength of a steel sheet and has the effect of suppressing hydrogen generation due to corrosion of the steel sheet, thereby improving the corrosion resistance of the steel sheet. Like Cr and Cu, Ni also has the effect of promoting the formation of iron oxide. To effectively exert these effects, the Ni content is preferably more than 0 mass%, more preferably 0.003 mass% or more, and even more preferably 0.05 mass% or more. Furthermore, from the viewpoint of ensuring the workability of the steel sheet, the Ni content is preferably 1.0 mass% or less, more preferably 0.8 mass% or less, and even more preferably 0.5 mass% or less.

[0040] [Ti: Preferably More than 0 Mass % and Not More than 0.15 Mass %] Like Cr, Cu, and Ni, Ti is an element that is effective in improving the strength of a steel sheet and has the effect of suppressing hydrogen generation due to corrosion of the steel sheet, thereby improving the corrosion resistance of the steel sheet. Like Cr, Cu, and Ni, Ti also has the effect of promoting the formation of iron oxide. Like B and Cr, Ti is also an element that is effective in improving the delayed fracture resistance of the steel sheet, so it can be contained in an amount that does not affect the strength and workability, such as elongation, of the steel sheet. To effectively exert these effects, the Ti content is preferably more than 0 mass %, more preferably 0.003 mass % or more, and even more preferably 0.05 mass % or more. Furthermore, from the viewpoint of ensuring the workability of the steel sheet, the Ti content is preferably 0.15 mass % or less, more preferably 0.12 mass % or less, and even more preferably 0.10 mass % or less.

[0041] [Nb: preferably more than 0 mass% and 0.15 mass% or less] Nb is an element that is effective in improving the strength of steel sheet and also acts to refine austenite grains after quenching, thereby improving the toughness of the steel sheet. To effectively exert this effect, the Nb content is preferably more than 0 mass%, more preferably 0.003 mass% or more, and even more preferably 0.005 mass% or more. On the other hand, an excessive Nb content may generate a large amount of carbides, nitrides, or carbonitrides, which may deteriorate the workability or delayed fracture resistance of the steel sheet. Therefore, the Nb content is preferably 0.15 mass% or less, more preferably 0.12 mass% or less, and even more preferably 0.10 mass% or less.

[0042] [V: preferably more than 0 mass% and 0.15 mass% or less] Like Nb, V is an element that is effective in improving the strength of steel sheet and also refines austenite grains after quenching, thereby improving the toughness of the steel sheet. To effectively exert this effect, the V content is preferably more than 0 mass%, more preferably 0.003 mass% or more, and even more preferably 0.005 mass% or more. On the other hand, an excessive V content, like Nb, may form large amounts of carbides, nitrides, or carbonitrides, which may deteriorate the workability or delayed fracture resistance of the steel sheet. Therefore, the V content is preferably 0.15 mass% or less, more preferably 0.12 mass% or less, and even more preferably 0.10 mass% or less.

[0043] [B: preferably more than 0 mass% and 0.005 mass% or less] B is an element useful for improving the hardenability and weldability of steel sheets. Like Ti and Cr, B is also effective in improving the delayed fracture resistance of steel sheets. Therefore, B can be added in an amount that does not affect the strength and workability, such as elongation, of the steel sheets. To effectively exert these effects, the B content is preferably more than 0 mass%, more preferably 0.0002 mass% or more, even more preferably 0.0003 mass% or more, and particularly preferably 0.0004 mass% or more. On the other hand, if the B content is excessive, these effects may saturate, and ductility may decrease, resulting in poor workability. Therefore, the B content is preferably 0.005 mass% or less, more preferably 0.004 mass% or less, and even more preferably 0.003 mass% or less.

[0044] Examples of the steel sheet include cold-rolled steel sheets and plated steel sheets. The type of plated steel sheet is not limited, and may be, for example, a zinc-based plated steel sheet that is coated with a zinc-based plating such as Al-Zn plating, Ni-Zn plating, Fe-Zn plating, Cr-Zn plating, or Mg-Zn plating. Specific examples of the zinc-based plated steel sheet include hot-dip galvanized steel sheets (GI), galvannealed steel sheets (GA), and electrogalvanized steel sheets (EG).

[0045] [Method for Manufacturing Steel Sheet] Next, a method for manufacturing a high-strength steel sheet according to the present disclosure, particularly a method for manufacturing a steel sheet with good galvanizability, will be described.

[0046] The method for manufacturing a steel sheet according to this embodiment includes an annealing step in which an oxidation treatment is performed under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C, followed by a reduction treatment, and the reduction treatment includes a first reduction treatment in which the dew point is −35 to −15°C, followed by a second reduction treatment in which the dew point is −25 to 0°C, which is higher than the dew point of the first reduction treatment.

[0047] Oxidation treatment of the surface of a steel sheet forms an Fe oxide layer on the surface of the steel sheet. Subsequently, reduction treatment is performed in a reducing atmosphere to form a decarburized layer on the surface of the steel sheet while forming a reduced Fe layer that can be used to favorably form, for example, a coating layer. Adding water vapor throughout the entire reduction treatment can result in excessive decarburization, potentially reducing strength. On the other hand, if a high dew point is used in the first half of the reduction treatment, decarburization occurs once, but carbon re-diffuses (re-carburizes) in the decarburized region in the second half of the reduction treatment, resulting in poor bendability. Therefore, the inventors conducted research and found that by performing the oxidation treatment as described above, while defining the dew point ranges for the first and second reduction treatments in the reduction treatment, and setting the dew point for the second reduction treatment higher than that for the first reduction treatment, it is possible to easily ensure the decarburized state of the surface layer of the steel sheet, which achieves both high strength and excellent bendability. The oxidation treatment and reduction treatment are described below.

[0048] (Oxidation Treatment) Oxidation treatment is carried out under conditions of an oxygen concentration of 0.1 to 2%. Although the oxidation treatment can be carried out under conditions of an oxygen concentration of 0.0%, it is preferable to set the oxygen concentration to 0.1% or more in order to obtain a plated steel sheet from the viewpoint of obtaining an excellent plating appearance. The oxygen concentration is more preferably 0.15% or more, and even more preferably 0.20% or more. On the other hand, if the oxygen concentration is too high, excessive oxidation can easily cause oxide scale to adhere to the rolls inside the furnace, resulting in indentation marks on the steel sheet, a defect known as pickup. To prevent the occurrence of such a defect, the oxygen concentration is set to 2% or less. The oxygen concentration is preferably 1.7% or less, and more preferably 1.5% or less. The concentrations of elements other than oxygen are not particularly limited, and for example, CO 2 , N 2 , H 2 For example, the oxidation treatment is carried out in a direct fired furnace (DFF) type annealing furnace or the like, in a combustion gas such as coke oven gas (COG) or liquefied petroleum gas (LPG), to remove unburned O 2 The treatment can be carried out in a gas atmosphere with a controlled concentration.

[0049] The oxidation treatment is carried out under the condition of an ultimate temperature of 650 to 750°C. For example, heating may be carried out in an oxidation heating zone in a DFF type annealing furnace to an ultimate temperature range of 650 to 750°C. By achieving an ultimate temperature of 750°C or less, the SiO 2 on the surface of the steel sheet in the vicinity of the width direction edges can be reduced. 2 As a result, for example, when the steel sheet according to this embodiment is a plated steel sheet, good plating adhesion can be obtained.

[0050] In this specification, the "ultimate temperature" during heating in oxidation treatment means the maximum ultimate sheet temperature of the steel sheet that is heated and controlled in the oxidation heating zone.

[0051] The temperature reached in the oxidation treatment is preferably 730°C or lower, more preferably 720°C or lower, and even more preferably 700°C or lower. On the other hand, the steel sheet temperature in the oxidation treatment is set to 650°C or higher from the viewpoint of forming an Fe oxide layer in the above gas atmosphere. The steel sheet temperature in the oxidation treatment is preferably 670°C or higher.

[0052] The temperature rise time in the oxidation treatment is not particularly limited, and may be adjusted so that an excessively long time does not result in the formation of a fayalite layer, which may adversely affect platability, for example. Specifically, the temperature rise time in the oxidation treatment may be appropriately adjusted in consideration of the hot rolling conditions (particularly the coiling temperature), the annealing conditions before pickling, the pickling conditions, and the steel sheet temperature during heating in the oxidation treatment. For example, the temperature rise time in the oxidation treatment is preferably 10 seconds or more, more preferably 15 seconds or more. Furthermore, for example, the temperature rise time in the oxidation treatment is preferably 120 seconds or less, more preferably 90 seconds or less. Note that, although the above description deals with the case where the oxidation treatment is performed while the temperature is being raised, the mode of the oxidation treatment is not limited thereto, and the oxidation treatment may also be performed by, for example, raising the temperature to the target temperature and maintaining the target temperature.

[0053] (Reduction Treatment) The reduction treatment forms a desired decarburized layer on the surface of the steel sheet. Furthermore, when the steel sheet is a plated steel sheet, for example, a reduced Fe layer capable of forming a good plated layer is formed. In the manufacturing method according to this embodiment, the reduction treatment is performed by first performing a first reduction treatment with a dew point of −35 to −15°C, followed by a second reduction treatment with a dew point of −25 to 0°C, which is higher than the dew point of the first reduction treatment. The first and second reduction treatments are described below. (First Reduction Treatment) In the first reduction treatment, the dew point is set to a range of −35 to −15°C. If the dew point exceeds −15°C, decarburization tends to proceed more than necessary, resulting in a decrease in strength. Furthermore, the reduction treatment becomes difficult to proceed, and iron oxide produced in the oxidation treatment adheres to the rolls, easily causing a defect known as pickup, which causes indentations in the steel sheet. Therefore, the dew point is set to −15°C or lower. The dew point is preferably −20°C or lower. On the other hand, from the viewpoint of suppressing the need for additional equipment and costs, the dew point in the first reduction treatment is set to −35° C. or higher, and preferably −30° C. or higher.

[0054] The dew point may be within the above range in the atmosphere at the center of the front stage of the reduction zone where the first reduction treatment is performed. The dew point in the first reduction treatment and the second reduction treatment described below can be controlled, for example, by introducing water vapor gas and mixing it with the atmospheric gas in the furnace, or by bubbling the atmospheric gas to mix water vapor therein.

[0055] The atmosphere of the first reduction treatment satisfies the above dew point and contains N 2 , H 2 , CO, H 2 O, O 2 and other unavoidable impurities. In the first reduction treatment, after the temperature of the steel sheet reaches 800°C in the atmosphere, the steel sheet is held in a temperature range of 800 to 920°C for, for example, 60 to 240 seconds. The "holding" includes not only a constant temperature but also a temperature change within the temperature range.

[0056] (Second Reduction Treatment) Next, the dew point of the second reduction treatment will be described. Figures 1-1 (Nos. 1 to 16) and 1-2 (Nos. 17 to 22) are graphs created using examples described later, showing the relationship between the dew point at the center of the soaking zone during the second reduction treatment and R / t. As shown by the arrows in Figures 1-1 and 1-2, in order to achieve excellent bendability with an R / t of less than 2.5, it is necessary to set the dew point at −25°C or higher during the second reduction treatment. Figures 2-1 (Nos. 1 to 16) and 2-2 (Nos. 17 to 22) are also graphs created using examples described later, showing the relationship between the dew point at the center of the soaking zone during the second reduction treatment and tensile strength TS. It can be seen from Figures 2-1 and 2-2 that by setting the dew point at 0°C or lower, high tensile strength TS of 980 MPa or higher, or even 1180 MPa or higher, can be ensured. The dew point in the second reduction treatment is preferably −15° C. or lower.

[0057] The atmosphere of the second reduction treatment satisfies the above dew point and contains N 2 , H 2 , CO, H 2 O, O 2 In the second reduction treatment, the steel sheet is held in the atmosphere at a temperature range of 800 to 920°C for, for example, 60 to 240 seconds. The "holding" includes not only a constant temperature but also a temperature change within the temperature range.

[0058] The first reduction treatment and the second reduction treatment may be performed in separate atmospheres having different dew points as described above, and the specific embodiment is not limited thereto. For example, a reduction furnace for performing each of the first reduction treatment and the second reduction treatment may be provided. In addition, when the steel sheet is a plated steel sheet, a partition wall having an opening area ratio of 20% or less may be provided midway in the reduction zone of the continuous hot-dip galvanizing line to separate the first reduction treatment from the second reduction treatment.

[0059] Between the first reduction treatment and the second reduction treatment, it is permissible to insert, for example, a holding step in which at least one of the conditions (dew point, heating temperature) of the first reduction treatment is maintained, or a cooling step in which the steel sheet is cooled to a temperature between the heating temperature of the first reduction treatment and room temperature, as long as this does not adversely affect the decarburization state of the steel sheet according to this embodiment. Preferably, the second reduction treatment is performed subsequent to the first reduction treatment.

[0060] The oxidation treatment and reduction treatment may be carried out using any known single or multiple pieces of equipment. Preferably, from the viewpoints of production efficiency, cost, and quality maintenance, a continuous hot-dip galvanizing line (CGL) is used. By using a continuous hot-dip galvanizing line, oxidation treatment and reduction treatment by an oxidation-reduction method, and hot-dip galvanizing treatment and alloying treatment when producing, for example, a galvanized steel sheet as a steel sheet, can be carried out continuously in a single production line. More specifically, oxidation treatment and reduction treatment by an oxidation-reduction method can be carried out, for example, using an annealing furnace in a DFF-type continuous hot-dip galvanizing line. The oxidation treatment can be carried out, for example, in the heating zone of a DFF-type annealing furnace, as described above. The reduction treatment can be carried out, for example, in the soaking zone of a DFF-type annealing furnace.

[0061] The method for producing the steel sheet (base sheet) to be annealed is not particularly limited. The steel sheet (base sheet) to be annealed can be obtained by melting and casting steel in a conventional manner to obtain a steel slab, and then subjecting the steel slab to a rolling step (hot rolling or cold rolling) in a conventional manner.

[0062] The manufacturing method according to this embodiment is only required to include the annealing step, and other steps are not limited. The steel sheet according to this embodiment may be a cold-rolled steel sheet that has been annealed without undergoing any post-annealing steps. Alternatively, after annealing, a plating step, such as a hot-dip galvanizing step and / or an alloying step, may be performed to obtain the steel sheet according to this embodiment, for example, a hot-dip galvanized steel sheet (GI) or an alloyed hot-dip galvanized steel sheet (GA). Alternatively, an electrogalvanizing step may be performed to obtain the steel sheet according to this embodiment, for example, an electrogalvanized steel sheet (EG).

[0063] The method for forming a zinc plating layer on the surface of the annealed steel sheet is not particularly limited, and any known method can be used as appropriate. For example, the base material after the annealing step can be immersed in a plating bath. When immersing in the plating bath, for example, gas wiping or the like can be used to reduce the plating deposition weight to, for example, 20 g / m 2 More than 200g / m 2 It is preferable to suppress it to the following level.

[0064] The plating bath can be, for example, a binary or higher alloy plating containing Zn, such as Al—Zn plating, Fe—Zn plating, Ni—Zn plating, Cr—Zn plating, and Mg—Zn plating.

[0065] The plating may be performed by impregnating the material using a plating bath containing components other than zinc at a concentration of, for example, 0.01% by mass to 0.5% by mass at a temperature of, for example, 300°C to 600°C for, for example, 1 second to 30 seconds. The alloying treatment is also not particularly limited, and any known method may be used as appropriate. For example, the alloying treatment may be performed by reheating the material at an alloying temperature of 470°C to 600°C for 1 second to 100 seconds.

[0066] The present disclosure will be described in more detail below with reference to examples. The present disclosure is not limited to the following examples, and can be implemented by making appropriate modifications within the scope of the above-mentioned and below-mentioned aims, and all such modifications are included in the technical scope of the present disclosure.

[0067] As the annealing samples, Nos. 1 to 11 were prepared, each of which had a bulk carbon concentration, i.e., a C content of the steel sheet (base sheet) of 0.22 mass%, a Si content of 1.7 mass%, a Mn content of 2.0 mass%, a Cr content of 0.5 mass%, an Al content of 0.04 mass%, and the balance being Fe and inevitable impurities (note that "unavoidable impurities" here includes P, S, and N in amounts within the above-mentioned ranges), a ferrite+pearlite structure, and a strength of 700 to 800 MPa. For Nos. 12 to 16, base plates were prepared that had a bulk carbon concentration of 0.13 mass% (0.13 mass% C), a Si content of 0.9 mass%, a Mn content of 2.3 mass%, a Cr content of 0.57 mass%, an Al content of 0.02 mass%, and the balance being Fe and inevitable impurities (note that "unavoidable impurities" here includes P, S, and N in amounts within the ranges mentioned above), a structure of ferrite and pearlite, and a strength of 700 to 800 MPa. For Nos. 17 to 22, base plates were prepared having a bulk carbon concentration of 0.21% by mass (0.21% by mass C), a Si content of 1.8% by mass, a Mn content of 2.3% by mass, an Al content of 0.45% by mass, and the balance being Fe and inevitable impurities (note that "unavoidable impurities" here includes P, S, and N in amounts within the ranges described above), a structure of ferrite and pearlite, and a strength of 600 to 700 MPa.

[0068] The annealing sample was subjected to oxidation treatment and reduction treatment using an actual machine. Specifically, oxidation treatment was performed at the oxygen concentration and ultimate temperature shown in Table 1, and then a first reduction treatment (heating zone) and a second reduction treatment (soaking zone) shown in Table 1 were performed in this order under the conditions (ultimate temperature, dew point) shown in Table 1. The conditions for the "first reduction zone" in Table 1 indicate the conditions for the first reduction treatment, and the conditions for the "second reduction zone" indicate the conditions for the second reduction treatment.

[0069] The steel sheet after the second reduction treatment was cooled to 460°C and then immersed in an Al-Zn plating bath containing 0.08 to 0.13 mass% of Al (Al is effective Al%, plating bath temperature is 460 to 480°C) to perform galvanization. The coating weight was 40 g / m by gas wiping. 2 90g / m or more 2The conditions were controlled as follows, and then alloying treatment was carried out at 480 to 490°C for 20 to 30 seconds to obtain galvannealed steel sheets.

[0070]

[0071] The obtained galvannealed steel sheets were evaluated as follows.

[0072] [Means for Measuring Decarburization Behavior: Measurement of Carbon Profile by GD-OES] As described below, carbon profile measurement was carried out by GD-OES (Glow Discharge Optical Emission Spectrometry) to examine the decarburization behavior.

[0073] (Sample Preparation) Materials measuring 50 mm x 40 mm x thickness or 30 mm x 30 mm x thickness were collected. They were then degreased as per usual methods to prepare samples. Using these samples, the mass % concentration of each element was measured using GD-OES under the following conditions.

[0074] (Measurement conditions) Equipment used: Marcus-type radio frequency glow discharge optical emission surface analyzer (rf-GD-OES) GD-Profiler 2 manufactured by HORIBA, Ltd. Sputtering method: normal sputtering Measurement range: φ4 mm Type of gas: Ar Elements to be analyzed: B, C, O, Al, Si, Ti, Cr, Mn, Fe, Zn, P, S, N (In this example, the evaluation was performed on these elements, but if elements other than those listed above are contained in, for example, the plating layer or steel sheet, the elements other than those listed above will also be analyzed.)

[0075] (Measurement Method) GD-OES measurements were carried out on the plated surface of the sample up to a depth of 150 μm in the thickness direction.

[0076] (Analysis Method) Since the sputtering rate of the above-mentioned device is almost constant, the sputtering crater depth of the sample was measured after the analysis was completed, and the value (sputtering depth) was plotted on the horizontal axis.

[0077] The details of the calibration curve method for converting the measured emission intensity of each element into a concentration are shown below. i (g / sec) and luminescence intensity Ii The relationship between W and W is expressed by the following formula (1) using the slope a and intercept b of the calibration curve. i = aI i + b Formula (1) Sputter weight W of the element i per unit time i is the concentration C i (wt.%), density ρ (g / cm 3 ), and for a reference sample with a known sputtering rate Δd (cm / sec), the sputtering area S (cm 2 ) and is calculated using the following formula (2): i =C i ×ρ×Δd×S...Formula (2)

[0078] W i Using two or more reference samples with known emission intensities I i The slope a and intercept b of the above formula (1) were determined, and a calibration curve was created with the horizontal axis representing the emission intensity and the vertical axis representing the spatter weight. The reference samples used are shown in Table 2 below. Using the created calibration curve, the spatter weight was determined from the emission intensity of each target element, and the weight ratio was used to convert it into a concentration. The calibration curve used to convert the O concentration was 2 Correction was performed using the formula so that the concentration ratio of Si to O became 1:2.

[0079]

[0080] The carbon analysis results were used to obtain carbon profiles. An example is shown in Figure 3. Figure 3 shows Comparative Example No. 2 and Inventive Example No. 10. In Figure 3, the carbon profiles of both materials have a carbon concentration peak within the surface layer of 20 µm (specifically, in the internal oxide layer). However, while the carbon concentration in the Comparative Example is higher than the bulk carbon concentration, the carbon concentration in the Inventive Example is kept sufficiently lower than the bulk carbon concentration. Since the bulk carbon concentration of the sample used in this example was 0.22 mass%, the upper limit of the maximum carbon concentration (mass%) (vertical axis) in the region from the steel sheet surface to 20 µm is 0.22 mass% x 70% = 0.15 mass%.

[0081] From the obtained carbon concentration profile in the sheet thickness direction, the position where the carbon concentration (mass%) was 50% of the bulk carbon concentration, the position where the carbon concentration (mass%) was 90% of the bulk carbon concentration, and the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm were determined. Note that the bulk carbon concentration was corrected for analysis so that the carbon concentration at a sufficiently deep position (120 to 150 μm) measured by GD-OES was the value obtained by conventional steel analysis. For example, if the steel analysis value was 0.22% and the GD-OES analysis value was 0.25%, the GD-OES analysis value was multiplied by 0.22 / 0.25 and used for analysis.

[0082] The amount of surface decarburization per 1 mm of sheet thickness on one side of the steel sheet was determined as follows. First, the amount of desorbed carbon was determined from the difference between the bulk carbon concentration and the carbon concentration profile of the steel sheet (after decarburization). 2 For a steel plate, the volume of iron in the decarburized part (m 3 ) x density (specific gravity) of iron (7.87 x 10 6 g / m 3 The total amount of decarburization was calculated by multiplying the ratio of decarburized carbon in the iron of the decarburized portion by the atomic weight of carbon (g / mol). The total amount of decarburization was then divided by the plate thickness to obtain the surface layer decarburization amount (mol / m) per 1 mm of plate thickness on one side of the steel plate. 2 ) was sought.

[0083] [Evaluation of limit bending property (R / t)] The bendability of the steel sheet was evaluated by the following procedure. Test pieces with a width of 40 mm and a length of 100 mm, with the major axis perpendicular to the rolling direction, were prepared, and a bending test was performed using the V-block method in accordance with JIS Z 2248:2014. In the bending test, the bending radius was varied from 0 to 7 mm to determine the minimum bending radius at which the material could be bent without breaking. This was taken as the limit bending radius R (mm), and the ratio of limit bending radius R (mm) to sheet thickness t (mm) was calculated. A ratio of limit bending radius R (mm) to sheet thickness t (mm) of less than 2.5 was evaluated as having excellent bendability, and a ratio of 2.5 or more was evaluated as having poor bendability.

[0084] [Measurement of TS (Tensile Strength)] TS (tensile strength) was measured by taking a JIS No. 5 tensile test piece from the steel plate so that the direction perpendicular to the rolling direction of the steel plate was the longitudinal direction, according to the method specified in JIS Z 2241: 2011. A TS (tensile strength) of 980 MPa or more was evaluated as high strength (preferably 1180 MPa or more was even higher strength), and a TS of less than 980 MPa was evaluated as poor strength.

[0085] [Evaluation of platability] The appearance of the plated steel sheet samples was visually observed. If adhesion of dross due to the presence of selective oxides of Si and Mn, which have an adverse effect on plating formation, was observed, the plateability was evaluated as poor (×), and if no adhesion was observed, the plateability was evaluated as excellent (◯). The results are shown in Table 3.

[0086]

[0087] Based on the results of Table 3, graphs showing the relationship between the position where the carbon concentration (mass%) in the thickness direction is 50% of the bulk carbon concentration and R / t are shown in Figure 4-1 (Nos. 1 to 16) and Figure 4-2 (Nos. 17 to 22). From Figures 4-1 and 4-2, it can be seen that in order to achieve excellent bendability with an R / t of less than 2.5, as indicated by the arrows in the figures, it is sufficient to ensure that the position where the carbon concentration (mass%) in the thickness direction is 50% of the bulk carbon concentration is in a region that is 0.20% or more of the thickness from the steel sheet surface.

[0088] Based on the results of Table 3, graphs showing the relationship between the position where the carbon concentration (mass%) in the sheet thickness direction is 90% of the bulk carbon concentration and the tensile strength TS are shown in Figure 5-1 (Nos. 1 to 16) and Figure 5-2 (Nos. 17 to 22). Figures 5-1 and 5-2 show that if the position where the carbon concentration (mass%) in the sheet thickness direction is 90% of the bulk carbon concentration is in a region 8.0% or less of the sheet thickness from the steel sheet surface, a high strength of tensile strength TS of 980 MPa or more, preferably 1180 MPa or more can be ensured.

[0089] Based on the results of Table 3 above, graphs showing the relationship between R / t and the ratio of the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm deep, relative to the bulk carbon concentration, are shown in Figure 6-1 (Nos. 1 to 16) and Figure 6-2 (Nos. 17 to 22). Figures 6-1 and 6-2 show that, in order to achieve excellent bendability with an R / t of less than 2.5, as indicated by the arrows in the figures, it is preferable to set the ratio of the maximum carbon concentration (mass%) in the region from the steel sheet surface to 20 μm deep, relative to the bulk carbon concentration, to less than 70%.

[0090] Based on the results of Table 3, graphs showing the relationship between the amount of surface decarburization per mm of plate thickness on one side of the steel plate and the tensile strength TS are shown in Figure 7-1 (Nos. 1 to 16) and Figure 7-2 (Nos. 17 to 22). From Figures 7-1 and 7-2, it can be seen that the amount of surface decarburization per mm of plate thickness was 0.045 mol / m 2 or less, preferably 0.035 mol / m 2 It can be seen that if the tensile strength TS is 980 MPa or more, preferably 1180 MPa or more, a high strength can be ensured if the tensile strength TS is 0.028 mol / m or less. 2 By setting the above to the above, a higher tensile strength TS of 1200 MPa or more can be achieved.

[0091] In Table 3, Nos. 1 to 4 and 22 did not have the surface layer of the steel sheet defined in this embodiment and were poor in bendability. Nos. 5 to 21 had the surface layer of the steel sheet defined in this embodiment and were able to achieve both high strength and excellent bendability. It can be seen that, in order to ensure the steel sheet properties of high strength, excellent bendability, and also excellent galvanizability, it is advisable to perform oxidation treatment under specified conditions in the manufacturing process, as in Nos. 9 to 21.

[0092] The disclosure of this specification may include the following aspects. Aspect 1 of the present invention is a steel sheet in which, in the sheet thickness direction, the position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is in a region from the steel sheet surface to 0.20% or more of the sheet thickness, and the position where the carbon concentration (mass %) is 90% of the bulk carbon concentration is in a region from the steel sheet surface to 8.0% or less of the sheet thickness. Aspect 2 of the present invention is a steel sheet in which the maximum carbon concentration (mass %) in a region from the steel sheet surface to 20 μm in the sheet thickness direction is less than 70% of the bulk carbon concentration, and the amount of surface decarburization per mm of sheet thickness on one side of the steel sheet is 0.035 mol / m 2 Aspect 3 of the present invention is the steel sheet according to Aspect 1, wherein the tensile strength is 1180 MPa or more. Aspect 4 of the present invention is the steel sheet according to any one of Aspects 1 to 3, wherein the chemical composition satisfies the following: C: 0.08% by mass or more and 0.30% by mass or less, Si: more than 0.5% by mass and 3.0% by mass or less, Mn: 1.5% by mass or more and 3.0% by mass or less, Cr: more than 0% by mass and 1.0% by mass or less, P: more than 0% by mass and 0.1% by mass or less, S: more than 0% by mass and 0.05% by mass or less, Al: more than 0% by mass and 1.0% by mass or less, and N: more than 0% by mass and 0.01% by mass or less, with the balance being Fe and unavoidable impurities. Aspect 5 of the present invention is a method for producing a steel sheet, comprising an annealing step of performing an oxidation treatment under conditions of an oxygen concentration of 0.1 to 2% and an ultimate temperature of 650 to 750°C, followed by a reduction treatment, wherein the reduction treatment includes a first reduction treatment having a dew point of -35 to -15°C, followed by a second reduction treatment having a dew point of -25 to 0°C, which is higher than that of the first reduction treatment. Aspect 6 of the present invention is the method for producing a steel sheet according to Aspect 5, wherein the ultimate temperatures in the first reduction treatment and the second reduction treatment are 800 to 920°C.

[0093] This application claims priority to Japanese Patent Application No. 2023-056165, filed on March 30, 2023, and Japanese Patent Application No. 2024-022770, filed on February 19, 2024. Japanese Patent Application Nos. 2023-056165 and 2024-022770 are incorporated herein by reference.

Claims

1. A steel plate in which, in the plate thickness direction, the position where the carbon concentration (mass %) is 50% of the bulk carbon concentration is in an area 0.20% or more of the plate thickness from the steel plate surface, and the position where the carbon concentration (mass %) is 90% of the bulk carbon concentration is in an area 8.0% or less of the plate thickness from the steel plate surface.

2. The maximum carbon concentration (mass%) in the region from the steel plate surface to 20 μm in the plate thickness direction is less than 70% of the bulk carbon concentration, and the amount of surface decarburization per 1 mm of plate thickness on one side of the steel plate is 0.045 mol / m 2 The steel sheet according to claim 1 , wherein:

3. The steel plate according to claim 1 or 2, having a tensile strength of 980 MPa or more.

4. A steel plate according to claim 1 or 2, the chemical composition of which is: C: 0.08 mass% or more and 0.30 mass% or less; Si: more than 0.5 mass% and 3.0 mass% or less; Mn: 1.5 mass% or more and 3.0 mass% or less; Cr: 0 mass% or more and 1.0 mass% or less; P: more than 0 mass% and 0.1 mass% or less; S: more than 0 mass% and 0.05 mass% or less; Al: more than 0 mass% and 1.0 mass% or less; and N: more than 0 mass% and 0.01 mass% or less, with the balance being Fe and unavoidable impurities.

5. A method for manufacturing a steel sheet, comprising an annealing process in which an oxidation treatment is performed under conditions of an oxygen concentration of 0.1-2% and an ultimate temperature of 650-750°C, followed by a reduction treatment, the reduction treatment including a first reduction treatment having a dew point of -35--15°C, followed by a second reduction treatment having a dew point of -25-0°C, which is higher than that of the first reduction treatment.

6. The method for manufacturing a steel sheet according to claim 5, wherein the temperature achieved in the first reduction treatment and the second reduction treatment is 800 to 920°C.

Citation Information

Patent Citations

  • Method of manufacturing high-strength hot-dip galvanized steel plate

    JP2017166057A

  • Planter

    JP2023056165A

  • Composition for preventing, improving or treating chronic kidney disease

    JP2024022770A

  • Steel sheet for can excellent in aging resistance and baking hardenability and its production

    JP1999199991A

  • Method for manufacturing a press-hardened coated steel part and a pre-coated steel sheet enabling the manufacture of such part

    JP2016504488A

Cited By

  • Steel sheet and plated steel sheet

    WO2026004485A1