Resist polymer, photosensitive resin composition, interlayer insulating film, and polymer production method.
A resist polymer with specific structural units and a photosensitive resin composition address the thermomechanical property deficiencies of conventional alkali-soluble resins, offering improved heat resistance, moisture resistance, and thermomechanical performance for interlayer insulating films.
Patent Information
- Application Number
- PCT/JP2024/010945
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-19
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional alkali-soluble resins used in resist applications lack sufficient thermomechanical properties, particularly moisture resistance and a low coefficient of linear expansion, which are essential for interlayer insulating films in semiconductors.
A resist polymer comprising structural units derived from maleimide, aromatic, and acid group-containing monomers, with a specific imide equivalent weight and limited primary hydroxyl group content, combined with a photosensitive resin composition for improved photocurability, alkali solubility, heat resistance, and thermomechanical properties.
The polymer and resin composition provide a cured product with enhanced heat resistance, moisture resistance, and thermomechanical properties, suitable for interlayer insulating films and other applications requiring these properties.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Resist polymer, photosensitive resin composition, interlayer insulating film, and method for producing polymer
[0001] The present disclosure relates to a resist polymer, a photosensitive resin composition, an interlayer insulating film, and a method for producing the polymer. More specifically, the present disclosure relates to a resist polymer, a photosensitive resin composition, an interlayer insulating film, and a method for producing the polymer, which are excellent in heat resistance, alkali solubility, and photocurability, as well as in thermomechanical properties and moisture resistance.
[0002] The application of alkali-soluble resins and photosensitive resin compositions to various applications, such as various optical members and electric / electronic devices, including color filters, inks, printing plates, printed wiring boards, semiconductor devices, photoresists, organic insulating films, and organic protective films used in liquid crystal displays and solid-state imaging devices, has been extensively studied, and resins and resin compositions having excellent properties required for each application have been developed.
[0003] In recent years, optical components and electrical and electronic devices have become smaller, thinner, and more energy-efficient, and this has led to demands for higher performance in the various components used in them. To meet such demands, research is being conducted into alkali-soluble resins with even better properties.
[0004] Resins used in resist applications require properties such as photocurability, alkali solubility, and heat resistance, and alkali-soluble resins for resists that are excellent in such properties have been developed to date. For example, Patent Document 1 describes a maleimide copolymer obtained by polymerizing monomer components including an N-substituted maleimide monomer, an aromatic vinyl monomer, and an unsaturated monocarboxylic acid monomer, as a polymer that is excellent in heat resistance, flow thermal stability, and alkali solubility.
[0005] Furthermore, for example, Patent Document 2 describes a polymer obtained by polymerizing an N-substituted maleimide monomer, an ether dimer, vinyl toluene, and a monomer having an acid group as essential components, as a polymer that has excellent heat resistance, can reduce gas generation upon heating, and has a high dissolution rate in organic solvents and alkalis.
[0006] Furthermore, for example, Patent Document 3 describes a curable resin composition containing a radical polymerizable polymer having a structure obtained by reacting a carboxyl group in a polymer that is a base polymer with a monomer having a functional group that can react with the carboxyl group, the radical polymerizable polymer containing, as essential units, a structural unit derived from a maleimide-based monomer, a structural unit derived from an unsaturated carboxylic acid monomer that does not have an ester bond, and a structural unit derived from a monomer that has a hydroxyl group.
[0007] JP 2002-30119 A JP 2009-40999 A JP 2019-174761 A
[0008] However, conventional alkali-soluble resins have not yet been fully studied in terms of their thermomechanical properties such as moisture resistance and low linear expansion coefficient. When a resin composition containing an alkali-soluble resin is used as an interlayer insulating film material for a semiconductor, moisture resistance and a low linear expansion coefficient are required to ensure good adhesion to the substrate.
[0009] The present disclosure has been made in view of the above-described current situation, and aims to provide a resist polymer and a photosensitive resin composition that are excellent in photocurability, alkali solubility, and heat resistance, as well as in thermomechanical properties and moisture resistance.
[0010] The present inventors have conducted extensive research into alkali-soluble resins and found that the glass transition temperature of a polymer can be increased and the linear expansion coefficient can be reduced by including a large amount of structural units derived from maleimide monomers, i.e., by reducing the imide equivalent of the polymer. They also found that the polarity of the polymer can be reduced and the moisture resistance can be improved by including an aromatic ring in the polymer or reducing the amount of primary hydroxyl groups in the polymer. They then discovered that a polymer having three specific structural units, a specific range of the content of structural units derived from primary hydroxyl group-containing monomers, and a specific range of imide equivalent can provide a cured product that has excellent photocurability, alkali solubility, heat resistance, and moisture resistance, a low linear expansion coefficient, and excellent thermomechanical properties, and thus have arrived at the present disclosure.
[0011] That is, the present disclosure provides the following aspects. [1] A resist polymer comprising structural units (A) derived from a maleimide monomer, structural units (B) derived from an aromatic monomer, and structural units (C) derived from an acid group-containing monomer, wherein the content of structural units (D) derived from a primary hydroxyl group-containing monomer is less than 5 mass% relative to 100 mass% of all structural units in the polymer, and the polymer has an imide equivalent of 670 g / equivalent or less. [2] The resist polymer according to [1] above, wherein the polymer has an ester bond equivalent of 500 g / equivalent or more. [3] The resist polymer according to [1] or [2] above, wherein the polymer further comprises a structural unit (E) having a polymerizable double bond in a side chain. [4] The resist polymer according to [3] above, wherein the structural unit (E) comprises a structural unit represented by the following general formula (1):
[0012] (In the formula, R 1 and R 2 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. 3 represents a trivalent hydrocarbon group having 1 to 10 carbon atoms.) [5] The resist polymer according to any one of the above [1] to [4], wherein the structural unit (B) derived from an aromatic monomer includes a structural unit represented by the following general formula (2):
[0013] (In the formula, R 4 ~R 9are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms.) [6] A resist polymer according to any one of [1] to [5] above, wherein the polymer has a weight average molecular weight of 20,000 or less. [7] A photosensitive resin composition comprising the resist polymer according to any one of [1] to [6] above and an organic solvent. [8] The photosensitive resin composition according to [7] above, wherein the photosensitive resin composition comprises a thermal crosslinking agent. [9] An interlayer insulating film comprising a cured product of the photosensitive resin composition according to [7] or [8] above.
[10] A method for producing a polymer, comprising a step of polymerizing a monomer component containing, based on 100% by mass of the monomer component, 35 to 60% by mass of a maleimide-based monomer (a), 10 to 60% by mass of an aromatic-based monomer (b), and 5 to 30% by mass of an acid group-containing monomer (c), and a content of a primary hydroxyl group-containing monomer (d) of less than 5% by mass, in the presence of a solvent, wherein the solvent contains an ester-based solvent.
[0014] The resist polymer and photosensitive resin composition according to the present disclosure have excellent photocurability and alkali solubility, and can provide a cured product that is excellent in heat resistance, moisture resistance, and thermomechanical properties. The resist polymer and photosensitive resin composition according to the present disclosure are suitable for various applications such as interlayer insulating films.
[0015] The present disclosure will be described in detail below. It should be noted that a combination of two or more of the individual preferred embodiments of the present disclosure described below is also a preferred embodiment of the present disclosure. In this specification, "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid," and "(meth)acrylate" means "acrylate and / or methacrylate."
[0016] 1. Resist Polymer The present disclosure relates to a resist polymer comprising structural units (A) derived from a maleimide monomer, structural units (B) derived from an aromatic monomer, and structural units (C) derived from an acid group-containing monomer, wherein the content of structural units (D) derived from a primary hydroxyl group-containing monomer is less than 5 mass% relative to 100 mass% of all structural units in the polymer, and the imide equivalent of the polymer is 670 g / equivalent or less.
[0017] The resist polymer of the present disclosure has excellent photocurability and alkali solubility, and can provide a cured product with excellent heat resistance, moisture resistance, and thermomechanical properties. The resist polymer of the present disclosure exhibits such effects because it contains structural units derived from maleimide monomers and has an imide equivalent weight of a certain amount or less, i.e., the amount of structural units derived from maleimide monomers is a certain amount or more, thereby improving the heat resistance of the polymer and providing a low linear expansion coefficient; it contains structural units derived from aromatic monomers and has a certain amount or less of primary hydroxyl groups, thereby reducing hydrophilicity and improving moisture resistance; and it also contains structural units derived from acid group-containing monomers, thereby providing alkali solubility.
[0018] Each structural unit constituting the resist polymer of the present disclosure will be described. In this specification, the term "structural unit" refers to a repeating (structural) unit derived from a monomer constituting the polymer.
[0019] Structural Unit (A) The resist polymer of the present disclosure has a structural unit (A) derived from a maleimide monomer. By including the structural unit (A), it is possible to improve heat resistance and thermomechanical properties.
[0020] Examples of the structural unit (A) include a structural unit represented by the following general formula (3).
[0021] (In the formula, R 10 represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms.
[0022] The above R 10 The hydrocarbon group represented by the formula (I) may be linear or cyclic, and may be saturated or unsaturated. Among these, a cyclic unsaturated hydrocarbon group is preferred, and an aromatic hydrocarbon group is more preferred, in view of good properties of the cured product.
[0023] Examples of the chain saturated hydrocarbon group include alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, a sec-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a hexyl group, a 2-methylpentyl group, a heptyl group, a 2-methylhexyl group, a 2,2-dimethylpentyl group, a 3-ethylpentyl group, an octyl group, a methylheptyl group, a dimethylhexyl group, a nonyl group, and a decyl group.
[0024] Examples of the chain unsaturated hydrocarbon group include a vinyl group, an n-propenyl group, an isopropenyl group, a 1-butenyl group, a 1-pentenyl group, a 2-methyl-1-butenyl group, and a 1-hexenyl group.
[0025] Examples of the cyclic saturated hydrocarbon group include cycloalkyl groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a norbornyl group, and an adamantyl group.
[0026] Examples of cyclic unsaturated hydrocarbon groups include cycloalkenyl groups such as cyclopropenyl, cyclobutenyl, cyclopentenyl, and cyclohexenyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; and aromatic hydrocarbon groups such as aralkyl groups such as benzyl, phenethyl, and phenylpropyl.
[0027] The number of carbon atoms in the hydrocarbon group is preferably 1 to 15, more preferably 1 to 10, and even more preferably 6 to 7, in terms of good heat resistance and moisture resistance.
[0028] In the hydrocarbon group, at least one of the hydrogen atoms constituting the hydrocarbon group may be substituted with a halogen atom, a hydroxyl group, an alkyl group, or the like.
[0029] The polymer having the structural unit (A) can be obtained by polymerizing a monomer component containing a maleimide-based monomer (a). Examples of the maleimide-based monomer (a) include maleimide and N-substituted maleimide, and N-substituted maleimide is preferred because of its good heat resistance and moisture resistance.
[0030] Examples of the N-substituted maleimide include N-cyclohexylmaleimide, N-phenylmaleimide, N-methylmaleimide, N-ethylmaleimide, N-isopropylmaleimide, N-t-butylmaleimide, N-dodecylmaleimide, N-benzylmaleimide, and N-naphthylmaleimide, and one or more of these can be used. Among these, N-phenylmaleimide and N-benzylmaleimide are preferred, and N-benzylmaleimide is more preferred, in terms of good heat resistance and moisture resistance.
[0031] Examples of the N-phenylmaleimide include phenylmaleimide; alkyl-substituted phenylmaleimides such as p-methylphenylmaleimide and p-butylphenylmaleimide; phenolic hydroxyl group-substituted phenylmaleimides such as p-hydroxyphenylmaleimide; and halogen-substituted phenylmaleimides such as o-chlorophenylmaleimide, o-dichlorophenylmaleimide and p-dichlorophenylmaleimide.
[0032] Examples of the N-benzylmaleimide include benzylmaleimide; alkyl-substituted benzylmaleimides such as p-methylbenzylmaleimide and p-butylbenzylmaleimide; phenolic hydroxyl group-substituted benzylmaleimides such as p-hydroxybenzylmaleimide; and halogen-substituted benzylmaleimides such as o-chlorobenzylmaleimide, o-dichlorobenzylmaleimide and p-dichlorobenzylmaleimide.
[0033] The resist polymer may have only one type of the structural unit (A), or may have two or more types.
[0034] The content of the structural unit (A) is preferably 35 to 60% by mass, relative to 100% by mass of all structural units in the resist polymer, in order to provide sufficient heat resistance and moisture resistance. In order to achieve a good balance between heat resistance and alkaline developability, the content of the structural unit (A) is more preferably 40 to 55% by mass, and even more preferably 45 to 50% by mass, relative to 100% by mass of all structural units in the polymer.
[0035] Structural Unit (B) The resist polymer of the present disclosure contains a structural unit (B) derived from an aromatic monomer. By including the structural unit (B), it is possible to improve moisture resistance and heat resistance.
[0036] The polymer containing the structural unit (B) can be obtained by polymerizing a monomer component containing an aromatic monomer (b). Examples of the aromatic monomer (b) include compounds having an aromatic group and a polymerizable functional group.
[0037] Examples of the polymerizable functional group include groups having a polymerizable double bond, such as a (meth)acryloyl group, a vinyl group, an allyl group, a methallyl group, etc. Among these, a (meth)acryloyl group is preferred in terms of high polymerizability, versatility, and supply stability.
[0038] Examples of the aromatic group include aryl groups such as a phenyl group, an o-tolyl group, an m-tolyl group, a p-tolyl group, a 2,3-xylyl group, a 2,4-xylyl group, a 2,5-xylyl group, a 2,6-xylyl group, a 3,4-xylyl group, a 3,5-xylyl group, and a 1-naphthyl group, and aralkyl groups such as a benzyl group.
[0039] Specific examples of the aromatic monomer (b) include styrene, vinyltoluene, α-methylstyrene, methoxystyrene, etc. Among these, styrene and vinyltoluene are preferred in terms of good heat resistance and moisture resistance, and vinyltoluene is more preferred in terms of excellent electrical insulation and developability.
[0040] The structural unit (B) is preferably a structural unit represented by the following general formula (2): The structural unit represented by general formula (2) has a structure in which an aromatic ring is directly connected to the main chain, and therefore is less susceptible to thermal decomposition and has better heat resistance.
[0041] (In the formula, R 4 ~R 9 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms.
[0042] In the above general formula (2), R 4 ~R 9are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. 4 ~R 9 The hydrocarbon group represented by the above-mentioned R 10 Among these, saturated hydrocarbon groups are preferred, and alkyl groups are more preferred, in terms of good heat resistance and moisture resistance.
[0043] R 4 is preferably a hydrogen atom or a methyl group.
[0044] R 5 ~R 9 The hydrocarbon groups represented by the formula (I) may be the same or different and are preferably saturated hydrocarbon groups having 1 to 10 carbon atoms, more preferably alkyl groups having 1 to 5 carbon atoms, and even more preferably alkyl groups having 1 to 3 carbon atoms.
[0045] The resist polymer may have only one type of the structural unit (B), or may have two or more types.
[0046] The content of the structural unit (B) is preferably 10 to 60% by mass relative to 100% by mass of all structural units in the resist polymer, in order to provide sufficient heat resistance and moisture resistance. In order to achieve a good balance between heat resistance and alkaline developability, the content of the structural unit (B) is more preferably 20 to 50% by mass, and even more preferably 30 to 40% by mass relative to 100% by mass of all structural units in the polymer.
[0047] Structural Unit (C) The resist polymer contains a structural unit (C) derived from an acid group-containing monomer. By containing the structural unit (C), the resist polymer becomes alkali-soluble.
[0048] The polymer containing the structural unit (C) can be obtained by polymerizing a monomer component containing an acid group-containing monomer (c). Examples of the acid group-containing monomer include compounds having an acid group and a polymerizable functional group.
[0049] Examples of the polymerizable functional group include the same groups as those having a polymerizable double bond described above, and among these, a (meth)acryloyl group is preferred.
[0050] Examples of the acid group include functional groups that undergo a neutralization reaction with alkaline water, such as a carboxyl group, a phenolic hydroxyl group, a carboxylic anhydride group, a phosphoric acid group, a sulfonic acid group, etc. Among these, a carboxyl group is preferred.
[0051] Examples of the acid group-containing monomer include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, cinnamic acid, and vinylbenzoic acid; unsaturated polycarboxylic acids such as maleic acid, fumaric acid, itaconic acid, citraconic acid, and mesaconic acid; long-chain unsaturated monocarboxylic acids in which the unsaturated group and the carboxyl group are chain-extended, such as β-carboxyethyl (meth)acrylate, mono(2-acryloyloxyethyl) succinate, and mono(2-methacryloyloxyethyl) succinate; unsaturated acid anhydrides such as maleic anhydride and itaconic anhydride; and phosphate group-containing unsaturated compounds such as Light Ester P-1M (manufactured by Kyoeisha Chemical Co., Ltd.). Among these, carboxylic acid monomers (unsaturated monocarboxylic acids, unsaturated polycarboxylic acids, long-chain unsaturated monocarboxylic acids, and unsaturated acid anhydrides) are preferred from the standpoints of versatility, availability, and the like. In terms of reactivity, alkali solubility, etc., the acid group-containing monomer is more preferably an unsaturated monocarboxylic acid, and even more preferably (meth)acrylic acid.
[0052] The structural unit (C) is preferably a structural unit represented by the following general formula (4).
[0053] (In the formula, R 11 represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms.
[0054] In the above general formula (4), R 11 The hydrocarbon group represented by the above-mentioned R 10 Among the hydrocarbon groups represented by the formula (I), the hydrocarbon groups having 1 to 6 carbon atoms are exemplified, but among them, saturated hydrocarbon groups are preferred, and alkyl groups are more preferred, in terms of good heat resistance and moisture resistance. 11 is preferably a hydrogen atom or a methyl group.
[0055] The resist polymer may have only one type of the structural unit (C), or may have two or more types.
[0056] The content of the structural unit (C) is preferably 5 to 30% by mass, more preferably 10 to 25% by mass, and even more preferably 15 to 20% by mass, relative to 100% by mass of all structural units in the resist polymer, in order to achieve a good balance between heat resistance, moisture resistance, and the like while exhibiting good alkali developability.
[0057] Structural Unit (D) The resist polymer of the present disclosure may further include a structural unit (D) derived from a primary hydroxyl group-containing monomer, but the content thereof is less than 5% by mass relative to 100% by mass of all structural units in the resist polymer. In the resist polymer of the present disclosure, if the content of the structural unit (D) is 5% by mass or more relative to 100% by mass of all structural units in the polymer, the hydrophilicity of the polymer increases, and the moisture resistance of the cured product may decrease, resulting in impaired physical properties. In order to further improve moisture resistance, the content of the structural unit (D) is preferably 4.5% by mass or less, more preferably 4% by mass or less, even more preferably 3.5% by mass or less, and particularly preferably 2.5% by mass or less, relative to 100% by mass of all structural units in the polymer.
[0058] The polymer having the structural unit (D) can be obtained by polymerizing a monomer component containing a primary hydroxyl group-containing monomer (d). Examples of the primary hydroxyl group-containing monomer include compounds having a primary hydroxyl group and a polymerizable functional group.
[0059] Examples of the polymerizable functional group include the same groups as those having a polymerizable double bond described above, and among these, a (meth)acryloyl group is preferred.
[0060] Examples of the primary hydroxyl group-containing monomer (d) include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2,3-hydroxypropyl (meth)acrylate; and hydroxyalkyl (meth)acrylamides such as 2-hydroxymethyl (meth)acrylamide, 2-hydroxyethyl (meth)acrylamide, 2-hydroxypropyl (meth)acrylamide, 3-hydroxypropyl (meth)acrylamide, 4-hydroxybutyl (meth)acrylamide, hydroxypivalyl (meth)acrylamide, 5-hydroxypentyl (meth)acrylamide, and 6-hydroxyhexyl (meth)acrylamide.
[0061] Structural Unit (E) The resist polymer of the present disclosure may further include a structural unit (E) having a polymerizable double bond in a side chain. By including the structural unit (E), photocurability can be improved.
[0062] Examples of the polymerizable double bond include the same as those mentioned above, and among these, a (meth)acryloyl group is preferred.
[0063] The structural unit (E) can be obtained, for example, by polymerizing a monomer component containing an acid group-containing monomer to obtain a base polymer having the structural unit (C), and then reacting the acid group of the obtained base polymer with a compound having an epoxy group and a polymerizable double bond to introduce a polymerizable double bond into the side chain; or by polymerizing a monomer component containing an epoxy group-containing monomer to obtain a base polymer, and then reacting the epoxy group of the obtained base polymer with an acid group-containing monomer to introduce a polymerizable double bond into the side chain.
[0064] The compound having an epoxy group and a polymerizable double bond includes an epoxy group-containing monomer, such as those described in the structural unit (F) below.
[0065] The structural unit (E) is preferably a structural unit represented by the following general formula (1).
[0066]
[0067] (In the formula, R 1 and R 2 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. 3 represents a trivalent hydrocarbon group having 1 to 10 carbon atoms.
[0068] In the above general formula (1), R 1 and R 2 The hydrocarbon group having 1 to 6 carbon atoms represented by the formula (I) is the same as the above-mentioned R 10 Among the hydrocarbon groups represented by the formula (I), those having 1 to 6 carbon atoms are preferred. Among these, saturated hydrocarbon groups are preferred, and alkyl groups are more preferred. 1 and R 2 is preferably a hydrogen atom or a methyl group.
[0069] R 3 The trivalent hydrocarbon group represented by the formula (I) is preferably a trivalent saturated hydrocarbon group. The number of carbon atoms in the trivalent hydrocarbon group is preferably 1 to 20, more preferably 2 to 10, and even more preferably 3 to 7.
[0070] R 3 Examples of the trivalent hydrocarbon group represented by the formula (I) include the following.
[0071]
[0072] The resist polymer may have only one type of the structural unit (E), or may have two or more types.
[0073] The resist polymer may further include a structural unit (F) other than the structural units (A) to (E) described above. Examples of the structural unit (F) include structural units derived from the following monomers: Methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, n-amyl (meth)acrylate, s-amyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, tridecyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecanyl (meth)acrylate, cyclohexyl (meth)acrylate, (Meth)acrylic acid ester monomers such as dicyclopentanyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, 1,4-dioxaspiro[4,5]dec-2-ylmethacrylic acid, (meth)acryloylmorpholine, 4-(meth)acryloyloxymethyl-2-methyl-2-ethyl-1,3-dioxolane, 4-(meth)acryloyloxymethyl-2-methyl-2-isobutyl-1,3-dioxolane, 4-(meth)acryloyloxymethyl-2-methyl-2-cyclohexyl-1,3-dioxolane, and 4-(meth)acryloyloxymethyl-2,2-dimethyl-1,3-dioxolane; Epoxy group-containing monomers such as glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, β-ethylglycidyl (meth)acrylate, vinylbenzyl glycidyl ether, allyl glycidyl ether, (3,4-epoxycyclohexyl)methyl (meth)acrylate, and vinylcyclohexene oxide; (meth)acrylamides such as N,N-dimethyl(meth)acrylamide and N-methylol(meth)acrylamide;Macromonomers having a (meth)acryloyl group at one end of the polymer molecular chain, such as polystyrene, polymethyl (meth)acrylate, polyethylene oxide, polypropylene oxide, polysiloxane, polycaprolactone, and polycaprolactam; conjugated dienes such as 1,3-butadiene, isoprene, and chloroprene; vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl benzoate; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, 2-ethylhexyl vinyl ether, n-nonyl vinyl ether, lauryl vinyl ether, cyclohexyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, methoxyethoxyethyl vinyl ether, methoxypolyethylene glycol vinyl ether, 2-hydroxyethyl vinyl ether, and 4-hydroxybutyl vinyl ether; N-vinyl compounds such as N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylimidazole, N-vinylmorpholine, and N-vinylacetamide; Unsaturated isocyanates such as isocyanatoethyl (meth)acrylate and allyl isocyanate; etc.;
[0074] The resist polymer may have only one type of the structural unit (F), or may have two or more types.
[0075] In terms of good photocurability, the content of the structural unit (F) is preferably 3 to 30% by mass, more preferably 5 to 25% by mass, and even more preferably 7 to 20% by mass, relative to 100% by mass of all structural units in the resist polymer.
[0076] The resist polymer has an imide equivalent of 670 g / equivalent or less. When the imide equivalent is within this range, heat resistance and thermomechanical properties can be further improved. The imide equivalent is preferably 300 to 650 g / equivalent, more preferably 350 to 600 g / equivalent, and even more preferably 400 to 550 g / equivalent, in order to achieve a good balance between heat resistance, alkaline developability, and the like. The imide equivalent can be determined by dividing the mass (g) of the solids content of the polymer solution by the amount (mol) of imide groups in the polymer.
[0077] The resist polymer preferably has an ester bond equivalent of 500 g / equivalent or more. When the ester bond equivalent is within the above-mentioned range, heat resistance can be further improved. From the viewpoint of achieving a good balance between heat resistance, photocurability, alkali developability, and the like, the ester bond equivalent is more preferably 600 to 10,000 g / equivalent, even more preferably 650 to 5,000 g / equivalent, and particularly preferably 700 to 3,000 g / equivalent. The ester bond equivalent can be determined by dividing the mass (g) of the solid content of the polymer solution by the ester bond amount (mol) of the polymer.
[0078] In order to achieve a good balance between heat resistance, alkaline developability, etc., the weight average molecular weight of the resist polymer is preferably 20,000 or less, more preferably 2,000 to 18,000, even more preferably 3,000 to 15,000, and still more preferably 4,000 to 10,000. The weight average molecular weight is a value obtained by measurement using gel permeation chromatography (GPC) in accordance with the method described in the Examples.
[0079] The resist polymer preferably has an acid value of 80 to 200 mgKOH / g. When the acid value is within the above range, good alkaline developability is likely to be exhibited. The acid value is more preferably 90 to 180 mgKOH / g, and even more preferably 100 to 150 mgKOH / g, in that the exposed area is less likely to be corroded by an alkaline developer. The acid value is a value obtained by measurement using a neutralization titration method using a KOH solution, and specifically, a value obtained by measurement using the method described in the Examples.
[0080] When the resist polymer has a polymerizable double bond in a side chain, the double bond equivalent of the polymer is preferably 800 to 5000 g / equivalent, more preferably 900 to 4000 g / equivalent, and even more preferably 1000 to 3000 g / equivalent.
[0081] The double bond equivalent can be calculated by dividing the mass (g) of the polymer solid content by the amount of double bonds (mol) of the polymer. The double bond here refers to a double bond having radical polymerizability. That is, a polymerizable double bond represented by a (meth)acryloyl group, for example, a double bond generated by adding tetrahydrophthalic anhydride to a hydroxyl group is not included in the calculation of the double bond equivalent because it has no reactivity. The amount of double bonds of the polymer is 1 It can be determined by H-NMR measurement or iodometric titration.
[0082] <Method for Producing Resist Polymer> The method for producing the resist polymer is not particularly limited as long as it is a method that can polymerize monomer components to obtain a desired polymer, and known polymerization methods can be used.
[0083] The method for polymerizing the monomer components is not particularly limited, and commonly used techniques such as bulk polymerization, solution polymerization, and emulsion polymerization can be used. Among these, solution polymerization is preferred because it is industrially advantageous and allows for easy structural adjustment, such as molecular weight. Furthermore, the polymerization mechanism of the monomer components can be based on polymerization methods such as radical polymerization, anionic polymerization, cationic polymerization, and coordination polymerization, but because of its industrial advantages, polymerization methods based on radical polymerization mechanisms are preferred. Furthermore, the molecular weight of the polymer obtained by polymerizing the monomer components can be controlled by appropriately adjusting the amount and type of polymerization initiator, the polymerization temperature, and the type and amount of chain transfer agent.
[0084] Examples of the polymerization initiator include organic peroxides such as di-t-butyl peroxide and t-butylperoxy-2-ethylhexanoate, and azo compounds such as 2,2'-azobis(isobutyronitrile) and dimethyl 2,2'-azobis(2-methylpropionate), which are commonly used as polymerization initiators. These may be used alone or in combination of two or more.
[0085] Examples of the chain transfer agent include compounds having a mercapto group, such as alkyl mercaptans such as n-dodecyl mercaptan, mercaptocarboxylic acids such as 3-mercaptopropionic acid and mercaptoacetic acid, mercaptocarboxylic acid esters such as methyl mercaptoacetate, and hydroxyl group-containing mercaptans such as 1-mercaptoethanol, 1-mercapto-1,1-methanediol, 1-mercapto-1,1-ethanediol, 3-mercapto-1,2-propanediol, 2-mercapto-1,2-propanediol, 2-mercapto-2-methyl-1,3-propanediol, 2-mercapto-2-ethyl-1,3-propanediol, 1-mercapto-2,2-propanediol, 2-mercaptoethyl-2-methyl-1,3-propanediol, and 2-mercaptoethyl-2-ethyl-1,3-propanediol, which are commonly used as chain transfer agents. These may be used alone or in combination of two or more. The amount of these added can be appropriately determined using a known method. Among them, the chain transfer agent preferably contains at least one selected from the group consisting of the hydroxyl group-containing mercaptans and the mercaptocarboxylic acids, and more preferably contains the hydroxyl group-containing mercaptans and the mercaptocarboxylic acids.
[0086] By using the above-mentioned hydroxyl group-containing mercaptans, the polymer molecules are thought to have hydroxyl groups at their terminals, and while maintaining good alkaline developability, the degree of freedom of movement of the terminals is reduced due to interactions (hydrogen bonds) caused by the hydroxyl groups, thereby improving the thermomechanical properties of the cured product obtained by curing the polymer. The above-mentioned hydroxyl group-containing mercaptans are more preferably mercaptans having multiple hydroxyl groups. The number of hydroxyl groups in the above-mentioned hydroxyl group-containing mercaptans per molecule is preferably 2 to 7, more preferably 2 to 5, and even more preferably 2 to 3.
[0087] Examples of solvents used in the polymerization include ether solvents such as tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, and diethylene glycol dimethyl ether; ketone solvents such as acetone and methyl ethyl ketone; ester solvents such as ethyl acetate, butyl acetate, propylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate; aromatic hydrocarbon solvents such as toluene, xylene, and ethylbenzene; chloroform; dimethyl sulfoxide; and dimethyl carbonate. These solvents may be used alone or in combination of two or more. Among these, it is preferable to include an ester solvent in view of the good solubility of the imide monomer and the resist polymer obtained by polymerization.
[0088] The polymerization solvent preferably contains 10 to 100% by mass, more preferably 50 to 100% by mass, and even more preferably 80 to 100% by mass of the ester solvent, based on 100% by mass of the total polymerization solvent.
[0089] Regarding polymerization conditions, the polymerization temperature may be appropriately set depending on the type and amount of the monomers used, the type and amount of the polymerization initiator, etc., and is, for example, preferably 50 to 130° C., more preferably 60 to 120° C. Similarly, the polymerization time can also be appropriately set and is, for example, preferably 1 to 5 hours, more preferably 2 to 4 hours.
[0090] The method for producing the resist polymer preferably includes a step (1) of polymerizing, in the presence of a solvent, a monomer component that contains a maleimide monomer (a), an aromatic monomer (b), and an acid group-containing monomer (c), and that contains less than 5 mass % of a primary hydroxyl group-containing monomer (d).
[0091] The monomer component preferably contains, based on 100% by mass of the monomer component, 35 to 60% by mass of a maleimide monomer (a), 10 to 60% by mass of an aromatic monomer (b), and 5 to 30% by mass of an acid group-containing monomer (c), and the content of the primary hydroxyl group-containing monomer (d) is less than 5% by mass.
[0092] The monomer component more preferably contains, based on 100% by mass of the monomer component, 40 to 55% by mass of a maleimide monomer (a), 20 to 50% by mass of an aromatic monomer (b), and 10 to 25% by mass of an acid group-containing monomer (c), with the content of the primary hydroxyl group-containing monomer (d) being less than 4% by mass; and even more preferably, based on 100% by mass of the monomer component, 45 to 50% by mass of a maleimide monomer (a), 30 to 40% by mass of an aromatic monomer (b), and 15 to 20% by mass of an acid group-containing monomer (c), with the content of the primary hydroxyl group-containing monomer (d) being less than 3.5% by mass.
[0093] Examples of the maleimide-based monomer (a), aromatic-based monomer (b), acid group-containing monomer (c), and primary hydroxyl group-containing monomer (d) include the same monomers as those described above.
[0094] When the resist polymer has the structural unit (E), it is preferable to further include a step (2) of using the polymer obtained in the step (1) as a base polymer and subsequently reacting this base polymer with an epoxy group-containing monomer, whereby a polymerizable double bond is introduced into a side chain of the base polymer by reacting an acid group of the base polymer with an epoxy group of the epoxy group-containing monomer.
[0095] The epoxy group-containing monomer may be any of those listed above. The amount of the epoxy group-containing monomer relative to the base polymer is not particularly limited, and may be appropriately adjusted so that the content of the structural unit (E) falls within the desired range.
[0096] In the reaction step (2), commonly used additives such as a polymerization inhibitor, a reaction catalyst, etc. may be used. The amount of the additive added may be adjusted appropriately.
[0097] Examples of the polymerization inhibitor include benzoquinone, hydroquinones (e.g., hydroquinone, hydroquinone monomethyl ether, p-tert-butylhydroquinone, p-benzoquinone, etc.), phenols (e.g., 2,6-di-t-butyl-4-methylphenol, 6-t-butyl-2,4-dimethylphenol, 2,2'-methylenebis(4-methyl-6-t-butylphenol)), catechols (e.g., p-tert-butylcatechol, etc.), amines (e.g., N,N-diethylhydroxylamine, etc.), 1,1-diphenyl-2-picrylhydrazyl, tri-p-nitrophenylmethyl, phenothiazine, piperidine 1-oxyls (e.g., 2,2,6,6-tetramethylpiperidine 1-oxyl, etc.), oxygen, and the like.
[0098] Examples of the reaction catalyst include tertiary amines such as triethylamine, tertiary phosphines such as triphenylphosphine, lithium chloride, quaternary ammonium salts, quaternary phosphonium salts, etc. Among these, tertiary amines and tertiary phosphines are preferred in terms of increasing the electrical insulation properties of the cured product.
[0099] In the above reaction step (2), the reaction temperature is not particularly limited, but is preferably 90 to 140° C., more preferably 100 to 130° C., and even more preferably 110 to 120° C. The reaction time is also not particularly limited, but is preferably 2 to 20 hours, more preferably 3 to 15 hours, and even more preferably 5 to 10 hours.
[0100] The method for producing the resist polymer may include other steps in addition to the steps described above. Examples of other steps include an aging step, a neutralization step, a step of deactivating the polymerization initiator or chain transfer agent, a dilution step, a drying step, a concentration step, and a purification step. These steps can be carried out by known methods.
[0101] The present disclosure also provides a method for producing a polymer as described above, which includes a step of polymerizing a monomer component containing, based on 100% by mass of the monomer component, 35 to 60% by mass of a maleimide monomer (a), 10 to 60% by mass of an aromatic monomer (b), and 5 to 30% by mass of an acid group-containing monomer (c), with a primary hydroxyl group-containing monomer (d) content of less than 5% by mass, in the presence of a solvent, wherein the solvent includes an ester solvent. The polymerization step is preferably carried out in the presence of a polymerization initiator and a chain transfer agent in addition to the solvent.
[0102] 2. Photosensitive Resin Composition The resist polymer of the present disclosure can be combined with an organic solvent to form a photosensitive resin composition. Such a photosensitive resin composition containing the resist polymer and an organic solvent also constitutes part of the present disclosure. Because the photosensitive resin composition of the present disclosure contains the resist polymer, it can provide a cured product that has excellent photocurability and alkali solubility, as well as excellent heat resistance, moisture resistance, and thermomechanical properties.
[0103] In the photosensitive resin composition, the content of the resist polymer is not particularly limited and may be appropriately set depending on the application, the blending of other components, etc. For example, it is preferably 5 to 90 mass%, more preferably 10 to 85 mass%, and even more preferably 15 to 80 mass%, relative to 100 mass% of the total solid content of the photosensitive resin composition. In this specification, the "total solid content" means the total amount of components that form a cured product (excluding solvents and the like that volatilize during the formation of a cured product).
[0104] The organic solvent is not particularly limited and may be appropriately selected depending on the purpose and application. Examples thereof include the above-mentioned polymerization solvents and other known solvents.
[0105] The content of the organic solvent is not particularly limited and may be adjusted appropriately depending on the application of the photosensitive resin composition, and is preferably 10 to 90% by mass, more preferably 15 to 85% by mass, and even more preferably 20 to 80% by mass relative to 100% by mass of the solid content (total amount) of the photosensitive resin composition.
[0106] The photosensitive resin composition preferably further contains a thermal crosslinking agent, which increases the crosslink density of the cured product, thereby further improving the moisture resistance, heat resistance, and thermomechanical properties.
[0107] The thermal crosslinking agent is preferably a compound having a group capable of reacting with an acid group such as a carboxyl group, and examples thereof include epoxy compounds, melamine compounds, oxazoline compounds, etc. Among these, epoxy compounds are preferred in terms of excellent photocurability and resolution during image formation.
[0108] The content of the thermal crosslinking agent is not particularly limited and may be adjusted appropriately depending on the application of the photosensitive resin composition, etc., but is, for example, preferably 1 to 40 mass %, more preferably 1.5 to 35 mass %, and even more preferably 2 to 30 mass %, relative to 100 mass % of the solid content (total amount) of the photosensitive resin composition.
[0109] The photosensitive resin composition preferably further contains a photopolymerization initiator and a polymerizable compound. The photopolymerization initiator is preferably a radically polymerizable photopolymerization initiator. Specific examples of the photopolymerization initiator include aminoketone compounds such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one ("IRGACURE907", manufactured by BASF), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1-one ("IRGACURE369", manufactured by BASF), and 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one ("IRGACURE379", manufactured by BASF); 2,2-dimethoxy-1,2-diphenylethan-1-one ("IRGACURE651", manufactured by BASF), and phenylglyoxylic acid methyl ester ("DAROCURE benzyl ketal compounds such as 1-hydroxy-cyclohexyl-phenyl-ketone ("IRGACURE184", manufactured by BASF), 2-hydroxy-2-methyl-1-phenyl-propan-1-one ("DAROCUR1173", manufactured by BASF), 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one ("IRGACURE2959", manufactured by BASF), 2-hydroxy -1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propan-1-one ("IRGACURE 127", manufactured by BASF Corporation), [1-hydroxy-cyclohexyl-phenyl-ketone + benzophenone] ("IRGACURE 500", manufactured by BASF Corporation), and other hydroketone compounds; as well as other alkylphenone compounds exemplified in paragraphs
[0084] to
[0086] of JP-A No. 2013-227485;1,2-Octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime) ("OXE01", manufactured by BASF), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) ("OXE02", manufactured by BASF), 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], ethanone ("OXE03", manufactured by BASF), 1-[9-ethyl Examples of the compound include oxime ester compounds such as [-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-,1-(O-acetyloxime) ("OXE04", manufactured by BASF); benzophenone compounds; benzoin compounds; thioxanthone compounds; halomethylated triazine compounds; halomethylated oxadiazole compounds; biimidazole compounds; titanocene compounds; benzoic acid ester compounds; acridine compounds; and phosphine oxide compounds. These compounds may be used alone or in combination of two or more.
[0110] The content of the photopolymerization initiator is not particularly limited as long as it is within a range in which the effects of the present disclosure are exhibited, and may be set as appropriate. For example, the content is preferably 0.5 to 30 mass%, more preferably 0.7 to 25 mass%, and even more preferably 1 to 20 mass%, relative to 100 mass% of the total solid content of the photosensitive resin composition of the present disclosure.
[0111] The polymerizable compound is a low molecular weight compound having a polymerizable unsaturated bond (also referred to as a polymerizable unsaturated group) that can be polymerized by irradiation with active energy rays such as free radicals, electromagnetic waves (e.g., infrared rays, ultraviolet rays, X-rays, etc.), and electron beams, and examples thereof include monofunctional compounds having one polymerizable unsaturated group in the molecule and polyfunctional compounds having two or more polymerizable unsaturated groups.
[0112] Examples of the monofunctional compound include N-substituted maleimide monomers, (meth)acrylic acid esters, (meth)acrylamides, unsaturated monocarboxylic acids, unsaturated polycarboxylic acids, unsaturated monocarboxylic acids in which the unsaturated group and the carboxyl group are chain-extended, unsaturated acid anhydrides, aromatic vinyls, conjugated dienes, vinyl esters, vinyl ethers, N-vinyl compounds, unsaturated isocyanates, etc. Furthermore, monomers having an active methylene group or an active methine group can also be used.
[0113] Examples of the polyfunctional compound include the following compounds.bifunctional (meth)acrylate compounds such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, bisphenol A alkylene oxide di(meth)acrylate, and bisphenol F alkylene oxide di(meth)acrylate; Trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, ethylene oxide-added trimethylolpropane tri(meth)acrylate, ethylene oxide-added ditrimethylolpropane tetra(meth)acrylate, ethylene oxide-added pentaerythritol tetra(meth)acrylate, ethylene oxide-added dipentaerythritol hexa(meth)acrylate, propylene oxide-added trimethylolpropane tri(meth)acrylate, propylene oxide-added ditrimethylolpropane tetra(meth)acrylate, propylene oxide-added pentaerythritol tetra(meth)acrylate, propylene oxide-added dipentaerythritol hexa(meth)acrylate, ε-caprolactone-added trimethylolpropane tri(meth)acrylate, ε-caprolactone-added ditrimethylolpropane tetra(meth)acrylate, ε-caprolactone-added pentaerythritol tetra(meth)acrylate, ε-caprolactone-added dipentaerythritol hexa(meth)acrylate, dipentaerythritol pentaacrylate succinic acid-modified product, pentaerythritol triacrylate succinic acid-modified product, dipentaerythritol pentaacrylate phthalic acid-modified product, pentaerythritol triacrylate phthalic acid-modified product, and the following formula (6):
[0114]
[0115] polyfunctional (meth)acrylate compounds having three or more functional groups, such as modified dipentaerythritol hexaacrylate represented by the formula: polyfunctional vinyl ethers such as ethylene glycol divinyl ether, diethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, butylene glycol divinyl ether, hexanediol divinyl ether, bisphenol A alkylene oxide divinyl ether, bisphenol F alkylene oxide divinyl ether, trimethylolpropane trivinyl ether, ditrimethylolpropane tetravinyl ether, glycerin trivinyl ether, pentaerythritol tetravinyl ether, dipentaerythritol pentavinyl ether, dipentaerythritol hexavinyl ether, ethylene oxide-added trimethylolpropane trivinyl ether, ethylene oxide-added ditrimethylolpropane tetravinyl ether, ethylene oxide-added pentaerythritol tetravinyl ether, and ethylene oxide-added dipentaerythritol hexavinyl ether;
[0116] vinyl ether group-containing (meth)acrylic acid esters such as 2-vinyloxyethyl (meth)acrylate, 3-vinyloxypropyl (meth)acrylate, 1-methyl-2-vinyloxyethyl (meth)acrylate, 2-vinyloxypropyl (meth)acrylate, 4-vinyloxybutyl (meth)acrylate, 4-vinyloxycyclohexyl (meth)acrylate, 5-vinyloxypentyl (meth)acrylate, 6-vinyloxyhexyl (meth)acrylate, 4-vinyloxymethylcyclohexylmethyl (meth)acrylate, p-vinyloxymethylphenylmethyl (meth)acrylate, 2-(vinyloxyethoxy)ethyl (meth)acrylate, and 2-(vinyloxyethoxyethoxyethoxy)ethyl (meth)acrylate;
[0117] polyfunctional allyl ethers such as ethylene glycol diallyl ether, diethylene glycol diallyl ether, polyethylene glycol diallyl ether, propylene glycol diallyl ether, butylene glycol diallyl ether, hexanediol diallyl ether, bisphenol A alkylene oxide diallyl ether, bisphenol F alkylene oxide diallyl ether, trimethylolpropane triallyl ether, ditrimethylolpropane tetraallyl ether, glycerin triallyl ether, pentaerythritol tetraallyl ether, dipentaerythritol pentaallyl ether, dipentaerythritol hexaallyl ether, ethylene oxide-added trimethylolpropane triallyl ether, ethylene oxide-added ditrimethylolpropane tetraallyl ether, ethylene oxide-added pentaerythritol tetraallyl ether, and ethylene oxide-added dipentaerythritol hexaallyl ether;
[0118] Allyl group-containing (meth)acrylic acid esters such as allyl (meth)acrylate; polyfunctional (meth)acryloyl group-containing isocyanurates such as tri(acryloyloxyethyl)isocyanurate, tri(methacryloyloxyethyl)isocyanurate, alkylene oxide-added tri(acryloyloxyethyl)isocyanurate, and alkylene oxide-added tri(methacryloyloxyethyl)isocyanurate; polyfunctional allyl group-containing isocyanurates such as triallyl isocyanurate; polyfunctional urethane (meth)acrylates obtained by reacting polyfunctional isocyanates such as tolylene diisocyanate, isophorone diisocyanate, and xylylene diisocyanate with hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; polyfunctional aromatic vinyls such as divinylbenzene; etc. These polymerizable compounds may be used alone or in combination of two or more.
[0119] The content of the polymerizable compound is not particularly limited as long as it is within a range in which the effects of the present disclosure are exhibited, and may be set as appropriate. For example, the content is preferably 5 to 80 mass%, more preferably 7 to 70 mass%, and even more preferably 9 to 50 mass%, relative to 100 mass% of the total solid content of the photosensitive resin composition.
[0120] In addition to the above-mentioned components, the photosensitive resin composition may contain other components as necessary. Examples of the other components include colorants (pigments, dyes); dispersants; heat resistance improvers; leveling agents; development aids; inorganic fine particles such as silica fine particles and zirconia fine particles; silane-based, aluminum-based, and titanium-based coupling agents; thermosetting resins such as phenolic resins and polyvinylphenols; curing aids such as polyfunctional thiol compounds; plasticizers; polymerization inhibitors; ultraviolet absorbers; antioxidants; matting agents; antifoaming agents; antistatic agents; slip agents; surface modifiers; thixotropic agents; thixotropic aids; quinone diazide compounds; polyhydric phenol compounds; cationically polymerizable compounds; acid generators; and the like. These may be used alone or in combination of two or more. These other components may be appropriately selected from known compounds, and the amount used may also be appropriately determined.
[0121] <Preparation of Photosensitive Resin Composition> The method for preparing the photosensitive resin composition of the present disclosure is not particularly limited and may be a known method, for example, a method in which the above-mentioned components are mixed and dispersed using various mixers or dispersers. The mixing and dispersion step is not particularly limited and may be performed by a known method. In addition, other steps that are usually performed may be further included. When the photosensitive resin composition contains a colorant, it is preferable to prepare it through a known step such as a colorant dispersion treatment step.
[0122] <Cured Product> The cured product obtained by curing the photosensitive resin composition of the present disclosure has excellent heat resistance, moisture resistance, and thermomechanical properties.
[0123] The method for obtaining the cured product is not particularly limited, and any known method may be used. For example, the photosensitive resin composition described above may be applied to a substrate or molded, and then cured by drying, heating, or irradiating with energy rays such as ultraviolet rays, or a combination of these, to obtain a cured product.
[0124] Alternatively, the photosensitive resin composition may be applied to a substrate by a known method, the applied product may be dried as needed to form a coating film, and the coating film may then be exposed to light through a photomask. After exposure, the unexposed portion may be dissolved in an aqueous alkaline solution for alkaline development, and the resulting solution may be washed as needed, followed by heating (post-curing), thereby obtaining a cured product. The coating, drying, exposure, alkaline development, and heating may be performed by known techniques.
[0125] When the cured product is a cured film, the film thickness is preferably 0.5 to 10 μm, more preferably 0.7 to 7 μm, and even more preferably 1 to 5 μm, in order to be able to exhibit good heat resistance and thermomechanical properties.
[0126] The resist polymer and photosensitive resin composition of the present disclosure are excellent in photocurability and alkali solubility, and can provide cured products that are excellent in heat resistance, moisture resistance, and thermomechanical properties. Therefore, they are suitable for use in resist applications that require photocurability, alkali solubility, heat resistance, moisture resistance, or thermomechanical properties.
[0127] Specific preferred applications of the resist polymer and photosensitive resin composition of the present disclosure include, for example, applications in components of various optical members and electrical and electronic devices, such as color filters, black matrices, photospacers, black column spacers, inks, printing plates, printed wiring boards, semiconductor elements, photoresists, films, and organic insulating films (interlayer insulating films) used in liquid crystal, organic electroluminescent, quantum dot, and micro LED liquid crystal displays, solid-state imaging devices, touch panel displays, millimeter-wave antennas, etc. Among these, applications in interlayer insulating films are preferred because of their good thermomechanical properties.
[0128] The interlayer insulating film is, for example, an insulating film formed between a TFT array element and a transparent conductive film forming a pixel electrode in a TFT active matrix substrate used in a liquid crystal display device in order to protect the TFT array element, or an insulating film formed between a semiconductor chip and a wiring layer, etc. Such an interlayer insulating film made of a cured product of the above-mentioned photosensitive resin composition also constitutes one aspect of the present disclosure.
[0129] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples. Unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass."
[0130] In the examples, various physical properties were measured as follows. <Acid Value> Approximately 3 g of each polymer solution was weighed out and dissolved in a mixed solvent of 90 g of acetone and 10 g of water. The solution was titrated using a 0.1 N aqueous solution of KOH as a titrant. The titration was performed using an automatic titrator (product name: COM-555, manufactured by Hiranuma Sangyo Co., Ltd.), and the acid value per 1 g of solids (mg KOH / g) was determined from the acid value of the polymer solution and the solids content of the polymer solution. The solids content of the polymer solution was determined as follows. That is, approximately 1 g of the polymer solution was weighed out in an aluminum cup, dissolved by adding approximately 3 g of acetone, and then allowed to dry naturally at room temperature. The solution was then dried at 160°C for 1.5 hours using a vacuum dryer (manufactured by EYELA, product name: VOS-301SD), allowed to cool in a desiccator, and its mass was measured. The solids content (% by mass) of the polymer solution was calculated from the amount of mass loss.
[0131] <Double bond equivalent (g / equivalent)> The double bond equivalent was determined by dividing the mass (g) of the solid content of the polymer solution by the double bond amount (mol) of the polymer. The double bond amount was determined by dividing the mass of the compound having a polymerizable double bond used to introduce the polymerizable double bond by the molecular weight.
[0132] <Ester bond equivalent (g / equivalent)> The ester bond equivalent was determined by dividing the mass (g) of the solid content of the polymer solution by the amount of ester bonds (mol) of the polymer. The amount of ester bonds was determined as the sum of the mass of a compound having an ester bond among the monomers used in polymer synthesis divided by its molecular weight, and, in the case where an ester bond is generated in the polymerizable double bond introduction reaction, the mass of a compound having a polymerizable double bond used in the introduction of the polymerizable double bond divided by its molecular weight.
[0133] <Imide equivalent (g / equivalent)> The imide equivalent was determined by dividing the mass (g) of the solid content of the polymer solution by the amount (mol) of imide groups in the polymer. The amount of imide groups was determined by dividing the mass of the compound having an imide group among the monomers used in polymer synthesis by the molecular weight.
[0134] <Weight Average Molecular Weight> The weight average molecular weight was measured by GPC (gel permeation chromatography) using polystyrene as a standard substance and tetrahydrofuran as an eluent with an HLC-8220GPC (manufactured by Tosoh Corporation).
[0135] <Thermal decomposition resistance> A solution prepared by adding 4 g of tetrahydrofuran to 2 g of each polymer solution was added dropwise to 60 g of hexane, and the precipitated polymer was separated, removed, and vacuum dried overnight at 40°C. 10 mg of the obtained polymer powder was weighed, and the temperature at which the weight decreased by 5% under a nitrogen atmosphere was measured using a thermogravimetric analyzer TGA-50 (manufactured by Shimadzu Corporation). The higher the 5% weight loss temperature, the higher the thermal decomposition resistance.
[0136] <Alkali Solubility> 30% dipentaerythritol hexaacrylate (DPHA) and 5% photopolymerization initiator (Irgacure 907, manufactured by BASF) were added to the solid content of each polymer solution, and propylene glycol monomethyl ether acetate (PGMEA) was added to the mixture so that the resin solid content was 30%. The resulting solution was applied to a copper plate (50 mm long x 50 mm wide) by spin coating, dried at 80°C for 30 minutes, and then cooled to room temperature to prepare a test plate for evaluation on which a 4 μm thick coating film was formed. The prepared test plate was immersed in a 1% by mass aqueous sodium carbonate solution at 30°C for 30 seconds or 60 seconds, and the degree of dissolved residue on the coating film was visually observed to evaluate alkali solubility.
[0137] <Photocurability> The test plate for evaluating alkali solubility obtained above was subjected to a photoirradiation of 2 J / cm 2 After irradiation with light, the sample was immersed in a 1% by mass aqueous solution of sodium carbonate at 30° C. for 60 seconds. If no whitening or erosion of the coating film was observed, the sample was evaluated as "good."
[0138] <Moisture Resistance (Adhesion After PCT Treatment)> Moisture resistance was evaluated by a peel test after PCT (pressure cooker test) treatment. First, a dried coating film was formed in the same manner as in the evaluation of photocurability, and then irradiated with light to obtain a cured product. This was heated at 150°C for 1 hour to prepare a test substrate, which was then heated at 120°C under water vapor pressure for 6 hours. The cured film after heating was subjected to a cross-cut test in accordance with JIS K 5600-5-6:1999 and evaluated according to the following criteria. ⊚: Corresponds to Class 0 in the evaluation criteria of JIS K 5600-5-6:1999. ◯: Corresponds to Class 1 in the evaluation criteria of JIS K 5600-5-6:1999. Δ: Corresponds to Class 2 in the evaluation criteria of JIS K 5600-5-6:1999. ×: Corresponds to Class 3 in the evaluation criteria of JIS K 5600-5-6:1999. In addition, the cross-cut test carried out in the same manner before the PCT treatment was rated as ⊚ in all cases.
[0139] Thermomechanical Properties (TMA) Thermosetting resin compositions were prepared by blending 828EL (a bisphenol A epoxy resin manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight 186, with equimolar ratios of the polymer's carboxyl groups and the epoxy resin's epoxy groups) and triphenylphosphine into each polymer solution in the proportions shown in Table 2. The resulting thermosetting resin compositions were applied to a polyethylene terephthalate film to a dry thickness of approximately 80 μm, dried at 90°C for 30 minutes, cured at 180°C for 1 hour, and then cooled. The peeled cured coating film was then cut into 5 mm wide pieces to serve as measurement samples. Using a Bruker AXS TMA 4000 thermomechanical analyzer (manufactured by Bruker AXS Co., Ltd.), thermal analysis was performed in tension mode with a chuck distance of 20 mm. The thermomechanical properties were evaluated based on the glass transition temperature (Tg) and the average linear expansion coefficient α (50-150 ppm / °C) from 50 to 150°C.
[0140] Synthesis Example 1 (Example 1) 100 g of propylene glycol monomethyl ether acetate (PGMEA) was charged into a separable flask equipped with a condenser as a reaction vessel, and after purging with nitrogen, the temperature was raised to 90°C. Meanwhile, 45 g of N-benzylmaleimide, 18.8 g of acrylic acid, 2 g of t-butylperoxy-2-ethylhexanoate, and 144 g of PGMEA were mixed in dropping vessel 1. Furthermore, 36.2 g of vinyltoluene (m- and p-60:40 mixture) and 5 g of 3-mercaptopropionic acid were mixed in dropping vessel 2. While maintaining the reaction temperature at 90°C, the mixture was added dropwise from dropping vessels 1 and 2 to the reaction vessel at a constant rate over 4.0 hours. After completion of the dropwise addition, the temperature was maintained at 90°C for 30 minutes, after which 1.5 g of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued for an additional 30 minutes at 90°C. The reaction temperature was then raised to 115°C, and the reaction was continued for 1.5 hours, followed by cooling to room temperature to obtain polymer solution A-1. The properties of the obtained polymer, as well as the evaluation results of the 5% weight loss temperature, alkali solubility, photocurability, and moisture resistance (adhesion after PCT treatment) are shown in Table 1.
[0141] Synthesis Example 2 (Example 2) 100 g of propylene glycol monomethyl ether acetate (PGMEA) was charged into a separable flask equipped with a condenser as a reaction vessel, and after purging with nitrogen, the temperature was raised to 90°C. Meanwhile, 45 g of N-benzylmaleimide, 18.8 g of acrylic acid, 2 g of t-butylperoxy-2-ethylhexanoate, and 144 g of PGMEA were mixed in dropping vessel 1. Furthermore, 36.2 g of vinyltoluene (m- and p-60:40 mixture) and 5 g of 3-mercaptopropionic acid were mixed in dropping vessel 2. While maintaining the reaction temperature at 90°C, the mixture was added dropwise from dropping vessels 1 and 2 to the reaction vessel at a constant rate over 4.0 hours. After completion of the dropwise addition, the temperature was maintained at 90°C for 30 minutes, after which 1.5 g of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued for an additional 30 minutes at 90°C. Thereafter, the reaction temperature was raised to 115 ° C., and the reaction was continued for 1.5 hours. After cooling to room temperature, 9.5 g of glycidyl methacrylate, 0.3 g of Antage W-400 (manufactured by Kawaguchi Chemical Industry Co., Ltd.) as a polymerization inhibitor, and 0.2 g of triethylamine as a catalyst were added, and the temperature was raised to 110 ° C. while bubbling a nitrogen-air mixed gas adjusted to an oxygen concentration of 7%, and the reaction was carried out for 2 hours. Thereafter, the temperature was raised to 115 ° C. and the reaction was carried out for 5 hours to complete the reaction, and the reaction was cooled to room temperature, and polymer solution A-2 was obtained. The characteristic values of the obtained polymer, 5% weight loss temperature, alkali solubility, photocurability, and moisture resistance (adhesion after PCT treatment) are shown in Table 1.
[0142] Synthesis Example 3 (Example 3) 100 g of propylene glycol monomethyl ether acetate (PGMEA) was charged into a separable flask equipped with a condenser as a reaction vessel, and after purging with nitrogen, the temperature was raised to 90°C. Meanwhile, 50 g of N-benzylmaleimide, 18.8 g of acrylic acid, 4 g of t-butylperoxy-2-ethylhexanoate, and 141 g of PGMEA were mixed in dropping vessel 1. Furthermore, 31.2 g of vinyltoluene (a 60:40 mixture of m- and p-) was charged in dropping vessel 2. While maintaining the reaction temperature at 90°C, the mixture was added dropwise from dropping vessels 1 and 2 to the reaction vessel at a constant rate over 4.0 hours. After completion of the dropwise addition, the temperature was maintained at 90°C for 30 minutes, after which 3 g of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued for an additional 30 minutes at 90°C. Thereafter, the reaction temperature was raised to 115 ° C., and the reaction was continued for 1.5 hours. After cooling to room temperature, 9.5 g of glycidyl methacrylate, 0.3 g of Antage W-400 (manufactured by Kawaguchi Chemical Industry Co., Ltd.) as a polymerization inhibitor, and 0.2 g of triethylamine as a catalyst were added, and the temperature was raised to 110 ° C. while bubbling a nitrogen-air mixed gas adjusted to an oxygen concentration of 7%, and the reaction was carried out for 2 hours. Thereafter, the temperature was raised to 115 ° C. and the reaction was carried out for 5 hours to complete the reaction, and the reaction was cooled to room temperature, and polymer solution A-3 was obtained. The characteristic values of the obtained resin, 5% weight loss temperature, alkali solubility, photocuring property, and moisture resistance (adhesion after PCT treatment) are shown in Table 1.
[0143] Polymer solution A-4 was obtained by the same procedure as in Synthesis Example 2, except that N-phenylmaleimide was used instead of N-benzylmaleimide. The properties of the obtained resin, as well as the evaluation results of the 5% weight loss temperature, alkali solubility, photocurability, and moisture resistance (adhesion after PCT treatment) are shown in Table 1.
[0144] Polymer solution A-5 was obtained by the same procedure as in Synthesis Example 2, except that styrene was used instead of vinyltoluene. The properties of the obtained resin, as well as the evaluation results of the 5% weight loss temperature, alkali solubility, photocurability, and moisture resistance (adhesion after PCT treatment) are shown in Table 1.
[0145] Polymer solution A-6 was obtained by carrying out the same operation as in Synthesis Example 2, except that the 36.2 g of vinyltoluene in Synthesis Example 2 was replaced with a mixture of 33.2 g of vinyltoluene and 3 g of 2-hydroxyethyl methacrylate. The characteristic values of the obtained resin, and the results of evaluation of various properties such as 5% weight loss temperature, alkali solubility, photocurability, and moisture resistance (adhesion after PCT treatment) are shown in Table 1.
[0146] Synthesis Example 7 (Example 7) 100 g of PGMEA was charged into a separable flask equipped with a condenser as a reaction vessel, and after purging with nitrogen, the temperature was raised to 90°C. Meanwhile, 35 g of N-benzylmaleimide, 24 g of acrylic acid, 2 g of t-butylperoxy-2-ethylhexanoate, and 144 g of PGMEA were mixed in dropping vessel 1. Furthermore, 41 g of vinyltoluene (m- and p-60:40 mixture) and 5 g of 3-mercaptopropionic acid were mixed in dropping vessel 2. While maintaining the reaction temperature at 90°C, the mixture was added dropwise from dropping vessels 1 and 2 to the reaction vessel at a constant rate over 4.0 hours. After completion of the dropwise addition, the mixture was maintained at 90°C for 30 minutes, after which 1.5 g of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued for an additional 30 minutes at 90°C. Thereafter, the reaction temperature was raised to 115 ° C., and the reaction was continued for 1.5 hours. After cooling to room temperature, 17.4 g of glycidyl methacrylate, 0.3 g of Antage W-400 (manufactured by Kawaguchi Chemical Industry Co., Ltd.) as a polymerization inhibitor, and 0.2 g of triethylamine as a catalyst were added, and the temperature was raised to 110 ° C. while bubbling a nitrogen-air mixed gas adjusted to an oxygen concentration of 7%, and the reaction was carried out for 2 hours. Thereafter, the temperature was raised to 115 ° C. and the reaction was carried out for 9 hours to complete the reaction, and the reaction was cooled to room temperature to obtain polymer solution A-7. The characteristic values of the obtained resin, 5% weight loss temperature, alkali solubility, photocurability, and moisture resistance (adhesion after PCT treatment) are shown in Table 1.
[0147] Synthesis Example 8 (Example 8) 100 g of propylene glycol monomethyl ether acetate (PGMEA) was charged into a separable flask equipped with a condenser as a reaction vessel, and after purging with nitrogen, the vessel was heated to 90°C. Meanwhile, 45 g of N-benzylmaleimide, 20 g of acrylic acid, 2 g of t-butylperoxy-2-ethylhexanoate, and 144 g of PGMEA were mixed in dropping vessel 1. Furthermore, 35 g of vinyltoluene (m- and p-60:40 mixture), 2.2 g of 3-mercaptopropionic acid, and 1.1 g of 3-mercapto-1,2-propanediol were mixed in dropping vessel 2. While maintaining the reaction temperature at 90°C, the mixture was added dropwise from dropping vessels 1 and 2 to the reaction vessel at a constant rate over 4.0 hours. After the dropwise addition was completed, the mixture was maintained at 90°C for 30 minutes, after which 0.6 g of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued at 90°C for another 30 minutes. The reaction temperature was then raised to 115°C, and the reaction was continued for 1.5 hours. After cooling to room temperature, 9.5 g of glycidyl methacrylate, 0.3 g of Antage W-400 (manufactured by Kawaguchi Chemical Industry Co., Ltd.) as a polymerization inhibitor, and 0.2 g of triethylamine as a catalyst were added, and the temperature was raised to 110°C while bubbling a nitrogen-air mixed gas adjusted to an oxygen concentration of 7%, and the reaction was carried out for 2 hours. The temperature was then raised to 115°C, and the reaction was carried out for 5 hours to complete the reaction, and the mixture was cooled to room temperature to obtain Polymer Solution A-8. The characteristic values of the obtained polymer, 5% weight loss temperature, alkali solubility, photocurability, and moisture resistance (adhesion after PCT treatment) were evaluated, and the results are shown in Table 1.
[0148] Comparative Polymer Solution B-1 was obtained by carrying out the same procedure as in Synthesis Example 1, except that the amounts of N-benzylmaleimide and vinyltoluene (a 60:40 mixture of m- and p-) were changed to 25 g and 56.2 g, respectively. The properties of the obtained resin, as well as the evaluation results of the 5% weight loss temperature, alkali solubility, photocurability, and moisture resistance (adhesion after PCT treatment), are shown in Table 1.
[0149] Comparative Polymer Solution B-2 was obtained by the same procedure as in Synthesis Example 2, except that the amount of N-benzylmaleimide was 30 g and the amount of vinyltoluene (a 40:60 mixture of m- and p-) was 51.2 g. The properties of the obtained resin, as well as the evaluation results of the 5% weight loss temperature, alkali solubility, photocurability, and moisture resistance (adhesion after PCT treatment) are shown in Table 1.
[0150] Synthesis Example 11 (Comparative Example 3) 100 g of PGMEA was charged into a separable flask equipped with a condenser as a reaction vessel, and after purging with nitrogen, the temperature was raised to 90°C. Meanwhile, 30 g of N-benzylmaleimide, 24 g of acrylic acid, 2 g of t-butylperoxy-2-ethylhexanoate, and 144 g of PGMEA were mixed in dropping vessel 1. Furthermore, 46 g of vinyltoluene (m- and p-60:40 mixture) and 5 g of 3-mercaptopropionic acid were mixed in dropping vessel 2. While maintaining the reaction temperature at 90°C, the mixture was added dropwise from dropping vessels 1 and 2 to the reaction vessel at a constant rate over 4.0 hours. After completion of the dropwise addition, the temperature was maintained at 90°C for 30 minutes, after which 1.5 g of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued for an additional 30 minutes at 90°C. Thereafter, the reaction temperature was raised to 115 ° C., and the reaction was continued for 1.5 hours. After cooling to room temperature, 17.4 g of glycidyl methacrylate, 0.3 g of Antage W-400 (manufactured by Kawaguchi Chemical Industry Co., Ltd.) as a polymerization inhibitor, and 0.2 g of triethylamine as a catalyst were added, and the temperature was raised to 110 ° C. while bubbling a nitrogen-air mixed gas adjusted to an oxygen concentration of 7%, and the reaction was carried out for 2 hours. Thereafter, the temperature was raised to 115 ° C. and the reaction was carried out for 9 hours to complete the reaction, and the reaction was cooled to room temperature to obtain a comparative polymer solution B-3. The characteristic values of the obtained resin, 5% weight loss temperature, alkali solubility, photocurability, and moisture resistance (adhesion after PCT treatment) are shown in Table 1.
[0151] Comparative Polymer Solution B-4 was obtained by carrying out the same procedure as in Synthesis Example 2, except that the 36.2 g of vinyltoluene used in Synthesis Example 2 was replaced with a mixture of 31.2 g of vinyltoluene and 5 g of 2-hydroxyethyl methacrylate. The properties of the obtained resin, as well as the evaluation results of the 5% weight loss temperature, alkali solubility, photocurability, and moisture resistance (adhesion after PCT treatment), are shown in Table 1.
[0152] (Examples 9 to 16, Comparative Examples 5 to 8) The results of thermomechanical property (TMA) measurements are shown in Table 2. The values A-1 to A-8 and B-1 to B-4 in Table 2 are the resin solid content.
[0153]
[0154]
[0155] As shown in Tables 1 and 2, the polymers of the examples, which contain structural units derived from maleimide-based monomers, structural units derived from aromatic-based monomers, and structural units derived from acid group-containing monomers, have an imide equivalent of 670 g / equivalent or less, and have a content of structural units derived from primary hydroxyl group-containing monomers of less than 5% by mass, were confirmed to be excellent in all of photocurability, alkali solubility, heat resistance, moisture resistance, and thermomechanical properties.
[0156] Among the polymers of the examples, polymers (A-1) to (A-3), which used N-benzylmaleimide and vinyltoluene without using 2-hydroxyethyl methacrylate and had a low imide equivalent, showed better results. Furthermore, polymer (A-8), which used 3-mercapto-1,2-propanediol, a hydroxyl group-containing mercaptan, as a chain transfer agent, showed improved heat resistance and thermomechanical properties while maintaining good alkaline developability.
[0157] On the other hand, the comparative polymers (B-1) to (B-4) that did not satisfy at least one of the above conditions resulted in poor moisture resistance and thermomechanical properties. It is believed that the high imide equivalent polymers (B-1) to (B-3) had a high linear expansion coefficient of the cured film, which increased the difference in the linear expansion coefficient between the cured film and the substrate, resulting in a weak interface and reduced adhesion. It is believed that the polymer (B-4) containing 5% by mass or more of 2-hydroxyethyl methacrylate had high hydrophilicity, low heat resistance, and low moisture resistance, resulting in reduced adhesion.
[0158] The polymers of the present disclosure and resin compositions containing the polymers have excellent photocurability and alkali solubility, and therefore can be suitably used as resist polymers or photosensitive resin compositions. Furthermore, they also have excellent heat resistance, moisture resistance, and thermomechanical properties (low linear expansion coefficient), and therefore can be suitably used as interlayer insulating film materials, etc.
Claims
1. A polymer for resist comprising structural units (A) derived from a maleimide monomer, structural units (B) derived from an aromatic monomer, and structural units (C) derived from an acid group-containing monomer, wherein the content of structural units (D) derived from a primary hydroxyl group-containing monomer is less than 5% by mass relative to 100% by mass of all structural units of the polymer, and the imide equivalent of the polymer is 670 g / equivalent or less.
2. The resist polymer according to claim 1, wherein the ester bond equivalent of said polymer is 500 g / equivalent or more.
3. The resist polymer according to claim 1 or 2, further comprising a structural unit (E) having a polymerizable double bond in a side chain.
4. The resist polymer according to claim 3, wherein the structural unit (E) contains a structural unit represented by the following general formula (1): (In the formula, R 1 and R 2 are the same or different and each represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. 3 represents a trivalent hydrocarbon group having 1 to 10 carbon atoms.
5. A resist polymer according to any one of claims 1 to 4, characterized in that the structural unit (B) derived from an aromatic monomer contains a structural unit represented by the following general formula (2): (In the formula, R 4 ~R 9 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms.
6. A resist polymer according to any one of claims 1 to 5, characterized in that the weight average molecular weight is 20,000 or less.
7. A photosensitive resin composition comprising the resist polymer according to any one of claims 1 to 6 and an organic solvent.
8. The photosensitive resin composition according to claim 7, further comprising a thermal crosslinking agent.
9. An interlayer insulating film comprising a cured product of the photosensitive resin composition according to claim 7 or 8.
10. A method for producing a polymer, comprising a step of polymerizing a monomer component containing, based on 100% by mass of the monomer component, 35 to 60% by mass of a maleimide monomer (a), 10 to 60% by mass of an aromatic monomer (b), and 5 to 30% by mass of an acid group-containing monomer (c), and containing less than 5% by mass of a primary hydroxyl group-containing monomer (d), in the presence of a solvent, wherein the solvent contains an ester solvent.
Citation Information
Patent Citations
Ionizing radiation-curable resin composition for color filter, color filter and liquid crystal panel
JP2003215322A
Negative photosensitive resin composition
JP2007279728A
Positive radiation-sensitive resin composition, interlayer insulating film and method for forming the same
JP2011191344A
Transfer film, electrode protective film, laminate, capacitive input device, and method for producing touch panel
WO2019130750A1