Honeycomb structure
The honeycomb structure with a varying catalyst distribution and configuration addresses the energy efficiency and methane conversion rate issues in methanation reactions by managing temperature and catalyst distribution, resulting in improved energy savings and methane production efficiency.
Patent Information
- Application Number
- PCT/JP2024/011126
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
The methanation reaction for converting carbon dioxide into methane faces challenges with energy efficiency and methane conversion rate due to temperature control issues and catalyst degradation, especially when the reaction temperature exceeds 450°C, leading to insufficient methane production.
A honeycomb structure with a varying amount of methanation reaction catalyst supported on its surface, increasing towards the downstream side, and having a thin and thick portion configuration to manage temperature and catalyst distribution, utilizing Ni as an active component with a cerium oxide carrier, effectively controlling the reaction and suppressing hot spots.
This configuration enhances energy savings and improves the methane conversion rate while extending the catalyst's lifespan by stabilizing the reaction and utilizing reaction heat efficiently.
Smart Images

Figure JP2024011126_03102024_PF_FP_ABST
Abstract
Description
Honeycomb structure
[0001] The present invention relates to a honeycomb structure.
[0002] In recent years, from the viewpoint of reducing environmental impact, the recovery of carbon dioxide and its reuse as a raw material for carbon compounds have been considered. For example, methanation, in which carbon dioxide is reacted with hydrogen to convert it into methane, has been proposed (see, for example, Patent Document 1). In such methanation, a raw material gas containing carbon dioxide and hydrogen is supplied to a reactor heated to a predetermined temperature to cause a methanation reaction. However, since the methanation reaction is an exothermic reaction, the temperature rises in the reactor section where the methanation reaction occurs. However, the chemical equilibrium of the methanation reaction at atmospheric pressure drops above 450°C. Therefore, unless the reaction and temperature are appropriately controlled depending on the location of the reactor, the methane conversion rate may be insufficient.
[0003] Japanese Patent Application Laid-Open No. 2015-196619
[0004] A primary object of the present invention is to provide a honeycomb structure capable of producing methane with energy savings and an excellent methane conversion rate.
[0005] [1] A honeycomb structure according to one embodiment of the present invention includes a honeycomb substrate and a catalyst layer. The honeycomb substrate has partition walls defining a plurality of cells. The cells include gas channels. The catalyst layer includes a methanation catalyst for methanating carbon dioxide by reacting it with hydrogen. The catalyst layer is provided on the surface of the partition walls so as to face the gas channels. The catalyst layer has a gradient in the amount of methanation catalyst supported per unit area of the partition walls in the direction of passage of a fluid through the gas channels. [2] In the honeycomb structure described in [1] above, the amount of methanation catalyst supported may increase toward the downstream side in the passage direction. [3] In the honeycomb structure described in [2] above, the catalyst layer may have a first end portion that is an upstream end portion in the passage direction and a second end portion that is a downstream end portion in the passage direction. When the entire length of the catalytic layer in the passage direction is taken as 100% and the first end of the catalytic layer is taken as 0%, the amount of the methanation reaction catalyst supported in the catalytic layer in a range of 0% to 10% may be less than the amount of the methanation reaction catalyst supported in the catalytic layer in a range of 50% to 100%. [4] In the honeycomb structure described in [2] or [3] above, when the entire length of the catalytic layer in the passage direction is taken as 100% and the first end of the catalytic layer is taken as 0%, the thickness of the catalytic layer at a position of 50% may be greater than the thickness of the catalytic layer at a position of 5%. [5] In the honeycomb structure described in [4] above, the catalytic layer may include a thin portion and a thick portion in that order in the passage direction. [6] In the honeycomb structure described in any of [1] to [5] above, the methanation reaction catalyst may include Ni as an active component and a cerium oxide support supporting Ni.
[0006] According to an embodiment of the present invention, a honeycomb structure capable of producing methane with low energy consumption and an excellent methane conversion rate can be realized.
[0007] Fig. 1 is a schematic perspective view of a honeycomb structure according to one embodiment of the present invention, Fig. 2 is a schematic cross-sectional view of the honeycomb structure of Fig. 1, and Fig. 3 is a schematic cross-sectional view of a honeycomb structure according to another embodiment of the present invention.
[0008] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In addition, in order to clarify the description, the drawings may show the width, thickness, shape, etc. of each part more schematically than in the embodiment, but these are merely examples and do not limit the interpretation of the present invention.
[0009] A. Overview of Honeycomb Structure FIG. 1 is a schematic perspective view of a honeycomb structure according to one embodiment of the present invention; FIG. 2 is a schematic cross-sectional view of the honeycomb structure of FIG. 1. The honeycomb structure 100 of the illustrated example includes a honeycomb substrate 1 and a catalyst layer 2. The honeycomb substrate 1 includes partition walls 12 that define a plurality of cells 13. The cells 13 include gas flow channels 14. The catalyst layer 2 contains a methanation catalyst for methanating carbon dioxide with hydrogen. The catalyst layer 2 is provided on the surface of the partition walls 12 so as to face the gas flow channels 14. The catalyst layer 2 has a gradient in the amount of methanation catalyst supported (hereinafter referred to as catalyst supported amount) per unit area of the partition walls 12 in the direction of passage of a fluid through the gas flow channels 14 (hereinafter referred to as the passage direction). According to this configuration, the catalyst layer, which varies in catalyst loading amount in the direction of passage, is provided on the surface of the partition walls of the honeycomb substrate. Therefore, when a raw gas containing at least carbon dioxide and hydrogen is passed through the gas flow path and supplied to the catalyst layer, the carbon dioxide and hydrogen can be appropriately brought into contact with the methanation catalyst according to the composition of the raw gas. Therefore, the reaction and temperature control depending on the location of the honeycomb structure can be appropriately adjusted without increasing the complexity and / or size of the methanation production equipment, and the methanation reaction shown in the following formula (1) can be smoothly carried out. Because the methanation reaction (1) is an exothermic reaction, the generated heat (reaction heat) can be effectively utilized to promote the chemical reaction. As a result, methane can be produced with low energy consumption and at an excellent methane conversion rate. 2 +4H 2 →CH 4 +2H 2 O...(1)
[0010] In one embodiment, the catalyst loading amount increases toward the downstream side in the direction of passage. The catalyst loading amount may increase continuously or stepwise toward the downstream side in the direction of passage. As will be described in detail later, the feed gas may contain oxygen in addition to carbon dioxide and hydrogen. In this case, when the feed gas is supplied to the catalyst layer and the hydrogen and oxygen come into contact with the methanation reaction catalyst, a combustion reaction shown in the following formula (2) may proceed. Since the combustion reaction (2) is an exothermic reaction, the generated reaction heat can be effectively used to proceed with the methanation reaction (1). O 2 +2H 2 →2H 2 O...(2) Meanwhile, the combustion reaction (2) has a higher reaction rate than the methanation reaction (1), and may proceed preferentially in the upstream portion of the catalyst layer in the direction of passage. This may result in the formation of localized high-temperature areas (hot spots) in the upstream portion of the catalyst layer in the direction of passage. The formation of hot spots may result in a decrease in methane conversion and / or deterioration of the methanation catalyst. In contrast, in one embodiment, the catalyst loading increases toward the downstream side in the direction of passage, thereby suppressing the formation of hot spots in the upstream portion of the catalyst layer and allowing the methanation reaction (1) to proceed sufficiently in the downstream portion of the catalyst layer. This may result in an improvement in methane conversion and a longer life for the methanation catalyst.
[0011] The catalyst layer 2 typically has a first end 2a and a second end 2b (see FIG. 2). The first end 2a is the upstream end in the passage direction, and the second end 2b is the downstream end in the passage direction. In one embodiment, when the total length of the catalyst layer 2 in the passage direction is 100% and the first end 2a of the catalyst layer 2 is 0%, the catalyst loading amount in the range of 0% to 10% of the catalyst layer 2 is less than the catalyst loading amount in the range of 50% to 100% of the catalyst layer 2. Therefore, the formation of hot spots in the upstream portion (range of 0% to 10%) of the catalyst layer can be stably suppressed.
[0012] The catalyst loading amount in the range of 0% to 10% of the catalyst layer 2 is, for example, 1.0 mg / mm 2~6.0 mg / mm 2 and preferably 2.0 mg / mm 2 ~5.0 mg / mm 2 When the catalyst loading is within this range, the methanation reaction (1) and the combustion reaction (2) can proceed in a balanced manner in the upstream portion of the catalyst layer, thereby stably achieving energy savings and improving the methane conversion rate.
[0013] The catalyst loading amount in the range of 50% to 100% of the catalyst layer 2 is, for example, 5.0 mg / mm 2 ~20 mg / mm 2 and preferably 6.0 mg / mm 2 ~16 mg / mm 2 When the catalyst loading is within this range, the methanation reaction (1) can proceed more smoothly in the downstream portion of the catalyst layer, and the methane conversion rate can be further improved.
[0014] The catalyst loading amount in the catalyst layer 2 in the range of more than 10% to less than 50% (hereinafter referred to as 10% to 50%) can be arbitrarily and appropriately adjusted depending on the application. The catalyst loading amount in the range of 10% to 50% in the catalyst layer 2 may be, for example, the same as the catalyst loading amount in the range of 0% to 10% described above, or may be the same as the catalyst loading amount in the range of 50% to 100% described above. The catalyst loading amount in the range of 10% to 50% in the catalyst layer 2 is specifically 1.0 mg / mm 2 ~20 mg / mm 2 and preferably 2.0 mg / mm 2 ~16 mg / mm 2 is.
[0015] The concentration of the catalyst loading in the catalyst layer 2 can be achieved by any appropriate configuration. For example, the thickness of the catalyst layer 2 may be adjusted while the content ratio of the methanation reaction catalyst in the catalyst layer 2 is kept substantially constant, or the thickness of the catalyst layer 2 may be kept substantially constant while the content ratio of the methanation reaction catalyst in the catalyst layer 2 is adjusted.
[0016] In one embodiment, the thickness of the catalytic layer 2 is appropriately adjusted while the methanation reaction catalyst content in the catalytic layer 2 is kept substantially constant in the passage direction. Typically, when the total length of the catalytic layer 2 in the passage direction is 100% and the first end 2 a of the catalytic layer 2 is 0%, the thickness of the catalytic layer 2 at a position of 50% is greater than the thickness of the catalytic layer 2 at a position of 5%. The thickness of the catalytic layer 2 at a position of 50% is, for example, 1.2 times or more, preferably 1.5 times or more, and more preferably 2.0 times or more, the thickness of the catalytic layer 2 at a position of 5%. On the other hand, the thickness of the catalytic layer 2 at a position of 50% is, for example, 5.0 times or less, preferably 4.0 times or less, the thickness of the catalytic layer 2 at a position of 5%. When the thickness of the catalytic layer at a position of 50% is within this range, the methane conversion rate can be further improved.
[0017] In the illustrated example, the catalyst layer 2 includes a thin portion 21 and a thick portion 22 in this order in the passage direction. The thin portion 21 is located upstream of the thick portion 22 in the passage direction. The thick portion 22 is located downstream of the thin portion 21 in the passage direction. Typically, the thin portion 21 is located in at least a range of 0% to 10% of the catalyst layer 2, and the thick portion 22 is located in at least a range of 50% to 100% of the catalyst layer 2. A portion of the catalyst layer 2 between 10% and 50% (hereinafter referred to as 10% to 50%) may be either the thin portion 21 or the thick portion 22. In other words, the range of the thin portion 21 in the catalyst layer 2 is 0% to (50-α)%, and the range of the thick portion 22 in the catalyst layer 2 is (50-α)% to 100%. Here, α is, for example, 0 to 45, for example, 0 to 40, for example, 0 to 30, for example, 0 to 20, or for example, 0 to 10.
[0018] The range of the thin portion 21 in the catalyst layer 2 is, for example, 0% to 10% of the catalyst layer 2, or for example, 0% to 5% of the catalyst layer 2. The thin portion 21 is thinner than the thick portion 22. The thickness of the thin portion 21 is, for example, 1 μm to 20 μm, and preferably 5 μm to 15 μm. The range of the thick portion 22 in the catalyst layer 2 is, for example, 50% to 100% of the catalyst layer 2, or for example, 20% to 100% of the catalyst layer 2, or for example, 10% to 100% of the catalyst layer 2, or for example, 5% to 100% of the catalyst layer 2. The thickness of the thick portion 22 is, for example, 10 μm to 80 μm, preferably 20 μm to 50 μm, and more preferably 25 μm to 35 μm. The range of the thickness ratio of the thick portion 22 to the thin portion 21 is, for example, the same as the range of the thickness ratio of the 50% position to the 5% position in the catalyst layer 2 described above.
[0019] In one embodiment, the content of the methanation catalyst in the catalyst layer 2 is substantially constant throughout the entire catalyst layer 2. The content of the methanation catalyst in the catalyst layer 2 is, for example, 50 mass% or more, preferably 70 mass% or more, more preferably 80 mass% or more, and even more preferably 90 mass% or more. On the other hand, the upper limit of the content of the methanation catalyst in the catalyst layer 2 is typically 100 mass%. When the content of the methanation catalyst in the catalyst layer is within this range, the methanation reaction can be promoted more stably.
[0020] As shown in Fig. 3, the honeycomb structure 100 may be divided into a plurality of blocks 3 in the passage direction. The honeycomb structure 100 includes a first block 3a and a second block 3b. The first block 3a is located upstream of the second block 3b in the passage direction. Thin portions 21 are provided on the surfaces of the partition walls 12 in the first block 3a. Thick portions 22 are provided on the surfaces of the partition walls 12 in the second block 3b. This also allows the catalyst layer 2 to have a varying catalyst loading amount in the passage direction.
[0021] B. Details of the Honeycomb Substrate As shown in FIGS. 1 and 2 , the honeycomb substrate 1 typically has a flow-through honeycomb structure. The honeycomb substrate 1 may have any suitable shape (overall shape). Examples of the shape of the honeycomb substrate 1 include a cylindrical shape with a circular bottom, an elliptical cylindrical shape with an elliptical bottom, a rectangular prism with a polygonal bottom, and a cylindrical shape with an irregular bottom. In one embodiment, the honeycomb substrate 1 has a cylindrical shape. The outer diameter and length of the honeycomb substrate 1 can be appropriately set depending on the purpose. Although not shown, the honeycomb substrate 1 may have a hollow region at the center in a cross section perpendicular to the longitudinal direction.
[0022] In the illustrated example, the honeycomb substrate 1 includes an outer peripheral wall 11 and partition walls 12 located inside the outer peripheral wall 11. The outer peripheral wall 11 and the partition walls 12 may be formed integrally or separately. In the illustrated example, the outer peripheral wall 11 and the partition walls 12 are formed integrally.
[0023] The outer peripheral wall 11 has a cylindrical shape. The thickness of the outer peripheral wall 11 can be appropriately set depending on the application of the honeycomb structure. The thickness of the outer peripheral wall 11 can be, for example, 1 mm to 10 mm, or can be, for example, 2 mm to 8 mm.
[0024] As described above, the partition walls 12 define a plurality of cells 13. The cells 13 extend in the longitudinal direction (axial direction) of the honeycomb substrate 1 from the first end face 1a (inlet end face) to the second end face 1b (outlet end face) of the honeycomb substrate 1 (see FIG. 2). The cells 13 have any appropriate shape in a cross section perpendicular to the longitudinal direction of the honeycomb structure 1. Examples of the cross-sectional shape of the cells include a triangle, a rectangle, a pentagon, a polygon having hexagons or more, a circle, and an ellipse. The cross-sectional shapes and sizes of the cells may all be the same, or at least some of them may be different. Among such cross-sectional shapes of the cells, a rectangle is preferred, and a square or rectangle is more preferred.
[0025] The cell density of the honeycomb substrate 1 is, for example, 100 cpsi or more, preferably 300 cpsi or more. On the other hand, the upper limit of the cell density of the honeycomb substrate 1 is typically 1000 cpsi. When the cell density is in this range, carbon dioxide and hydrogen can be brought into contact with the catalyst layer more efficiently. In this specification, the "cell density of the honeycomb substrate" means the cell density of the cross section in the length direction (direction in which the cells extend) of the honeycomb substrate, and "cpsi" refers to the cell density of 6.4516 cm of the cross section. 2 This refers to the number of cells per square inch.
[0026] As will be described in detail later, gas flow channels 14 are formed inside the cells 13. The gas flow channels 14 are spaces formed inside the cells 13, and extend from the first end face 1a (inlet end face) to the second end face 1b (outlet end face) in the same manner as the cells 13. The cross-sectional shape of the gas flow channels 14 may be the same as that of the cells 13 described above, preferably a quadrangle, and more preferably a square or rectangle. The cross-sectional shapes and sizes of the gas flow channels 14 may all be the same, or at least some may be different.
[0027] In the illustrated example, the partition walls 12 have first partition walls 12a and second partition walls 12b that are perpendicular to each other, and the first partition walls 12a and the second partition walls 12b define a plurality of cells 13. The cross-sectional shape of the cells 13 is quadrangular except for the portions where the first partition walls 12a and the second partition walls 12b contact the outer peripheral wall 11. The configuration of the partition walls is not limited to the above-described partition walls 12. The partition walls may have first partition walls extending in the radial direction and second partition walls extending in the circumferential direction, which define a plurality of cells.
[0028] The thickness of the partition walls 12 can be set arbitrarily and appropriately. The thickness of the partition walls 12 is typically thinner than the thickness of the peripheral wall 11. The thickness of the partition walls 12 is, for example, 0.0127 mm (0.5 mil) or more, preferably 0.0254 mm (1.0 mil) or more. On the other hand, the thickness of the partition walls 12 is, for example, 0.508 mm (20 mil) or less, preferably 0.254 (10 mil) mm or less, more preferably 0.2032 (8.0 mil) mm or less, and even more preferably 0.127 (5.0 mil) mm or less. When the thickness of the partition walls is in this range, the mechanical strength of the honeycomb structure can be sufficient, and the cell density can be adjusted to the above-mentioned range. The thickness of the partition walls is measured, for example, by cross-sectional observation using a scanning electron microscope (SEM).
[0029] The partition walls 12 typically have a plurality of pores. The average pore diameter in the partition walls 12 can be set appropriately depending on the purpose. The average pore diameter in the partition walls 12 is, for example, 1 μm or more, and preferably 5 μm or more. On the other hand, the average pore diameter in the partition walls 12 is, for example, 20 μm or less, and preferably 15 μm or less. The average pore diameter is measured by, for example, mercury porosimetry. The porosity in the partition walls 12 can be set appropriately depending on the purpose. The porosity in the partition walls 12 is, for example, 15% or more, and preferably 30% or more. On the other hand, the porosity in the partition walls 12 is, for example, 60% or less, preferably 55% or less, and more preferably 50% or less. The porosity is measured by, for example, mercury porosimetry. When the average pore diameter and / or the porosity in the partition walls 12 are within such ranges, the catalyst loading amount in the partition walls can be improved.
[0030] The density of the partition walls 12 can be appropriately set depending on the purpose. The density of the partition walls 12 is, for example, 1.7 g / cm 3 ~2.8g / cm 3 and preferably 1.8 g / cm 3 ~2.6g / cm 3 The density is measured by, for example, mercury intrusion porosimetry.
[0031] Examples of materials that can be used to form the honeycomb substrate 1 include ceramic materials, such as zirconia-based materials, alumina-titanium carbide-based composite materials, Si-SiC-based composite materials, aluminum nitride, aluminum oxide, silicon nitride, silicon carbide, zirconia, cordierite, and mullite.
[0032] These ceramic materials can be used alone or in combination. Among these ceramic materials, ceramic materials having heat resistance and oxidation resistance are preferred, and cordierite and Si-SiC composite materials are more preferred.
[0033] C. Details of the Catalyst Layer The catalyst layer 2 is formed on the surface of the partition wall 12. In the honeycomb structure 1, the gas flow passage 14 is formed in a portion of the cross section of the cell 13 where the catalyst layer 2 is not formed (typically the central portion). The catalyst layer 2 may be formed on the entire inner surface of the partition wall 12 (i.e., so as to surround the gas flow passage 14) as in the illustrated example, or may be formed on a part of the surface of the partition wall. When the catalyst layer 2 is formed on the entire inner surface of the partition wall 12, the methane conversion rate can be stably improved. Note that the first end 2a of the catalyst layer 2 typically faces the first end face 1a of the honeycomb substrate 1, and the second end 2b of the catalyst layer 2 typically faces the second end face 1b of the honeycomb substrate 1.
[0034] As described above, the catalyst layer 2 contains a methanation catalyst. A methanation catalyst typically contains an active component and a carrier supporting the active component. The active component can promote the methanation reaction represented by formula (1) above. Examples of the active component include metal elements, more specifically, alkali metal elements such as K and Na; platinum group elements such as Ir, Ru, and Rh; alkaline earth metal elements such as Ca; and Ni. The metal elements may be contained in the methanation catalyst singly or in combination. These metal elements may be contained in the methanation catalyst in a metallic state, as a metal salt, or as an oxide. Among these metal elements, Ni is preferred, and Ni in a metallic state is more preferred.
[0035] Examples of the carrier include metal oxides, and more specifically, oxides of rare earth elements such as cerium oxide and yttrium oxide; zirconium oxide; aluminum oxide; silicon oxide; and magnesium oxide. The carriers can be contained in the methanation reaction catalyst alone or in combination. Among these carriers, oxides of rare earth elements are preferred, and cerium oxide is more preferred. The content of the active component is, for example, 0.01 to 50 parts by mass, and preferably 1 to 20 parts by mass, relative to 100 parts by mass of the carrier. When the content of the active component is within this range, the methanation reaction can be stably promoted.
[0036] The methanation catalyst may have any appropriate shape. The methanation catalyst is typically in the form of particles. Hereinafter, the particulate methanation catalyst may be referred to as catalyst particles. In one embodiment, the catalyst layer 2 contains aggregates of a plurality of catalyst particles. The aggregates of a plurality of catalyst particles may form mesopores in the catalyst layer 2. The catalyst layer 2 may contain other components (for example, a binder) in addition to the methanation catalyst. A representative example of the binder is an inorganic binder, and more specifically, Al 2 O 3 , SiO 2 , ZrO 2 Examples include:
[0037] The average pore diameter of the catalyst layer 2 is, for example, 0.2 μm to 10 μm, and preferably 1.0 μm to 5.0 μm. The BET specific surface area of the catalyst layer 2 is, for example, 10 m 2 / g to 300m 2 / g, preferably 50m 2 / g to 200m 2 / g, more preferably 80m 2 / g~150m 2 / g.
[0038] D. Manufacturing Method of Honeycomb Structure Next, a description will be given of a manufacturing method of the honeycomb structure 100. In one embodiment, the manufacturing method of the honeycomb structure 100 includes a step of preparing a honeycomb substrate 1; and a step of forming a catalyst layer 2 on the partition walls 12 of the honeycomb substrate 1.
[0039] The honeycomb substrate 1 is produced, for example, by the following method: First, a binder and water or an organic solvent are added as needed to a material powder containing the above-described ceramic material, and the resulting mixture is kneaded to form a clay. The clay is then molded (typically by extrusion molding) into a desired shape, dried, and then fired as needed.
[0040] Next, the catalyst layer 2 is formed on the partition wall 12. The method for forming the catalyst layer 2 is not particularly limited, and any appropriate method may be adopted. In one embodiment, the step of forming the catalyst layer 2 includes, in order, a step of preparing catalyst particles, a step of preparing a catalyst slurry in which the catalyst particles are dispersed, and a step of applying the catalyst slurry to the surfaces of the partition wall 12.
[0041] In the process of preparing catalyst particles, for example, a carrier dispersion liquid in which the above-mentioned metal oxide (carrier) particles (hereinafter referred to as metal oxide particles) are dispersed, and a metal salt solution in which the above-mentioned metal element (active component) salt (hereinafter referred to as metal salt) is dissolved are prepared.
[0042] To prepare a carrier dispersion, metal oxide particles are added to a dispersion medium and stirred. The primary particle diameter of the metal oxide particles is, for example, 5 nm to 200 nm. The amount of metal oxide particles added is, for example, 0.5 parts by mass to 25 parts by mass per 100 parts by mass of the dispersion medium. Any appropriate solvent that does not dissolve metal oxide particles can be used as the dispersion medium. Examples of the dispersion medium include water and alcohols. The dispersion medium can be used alone or in combination. Of the dispersion mediums, water is preferred.
[0043] To prepare the metal salt solution, a metal salt is added to a solvent and stirred. Examples of metal salts include nitrates, chlorides, and bromides, preferably nitrates, and more preferably nickel nitrate. The metal salts can be used alone or in combination. The amount of metal salt added is, for example, 1.0 to 30 parts by mass per 100 parts by mass of the solvent. Examples of solvents include those similar to the dispersion medium described above. The solvents can be used alone or in combination. Among the solvents, preferably, the same dispersion medium as used in the carrier dispersion liquid is used.
[0044] Next, the metal salt solution is added to the carrier dispersion and stirred. This prepares a mixed solution of the carrier dispersion and the metal salt solution. The mixing ratio of the carrier dispersion and the metal salt solution can be adjusted arbitrarily and appropriately so that the content of the metal element (active component) in the produced methanation catalyst falls within the above-mentioned range.
[0045] Next, the mixed liquid is heated while stirring to evaporate the dispersion medium and solvent. This results in a solid. The solid is then heated. The heating temperature of the solid is, for example, 300°C to 700°C, preferably 400°C to 600°C. The heating time of the solid is, for example, 0.5 hours to 8 hours, preferably 2 hours to 4 hours. The heating of the solid may be carried out in the atmosphere or in a reducing atmosphere (typically a hydrogen atmosphere). The heating of the solid is preferably carried out in the atmosphere. This results in the preparation of methanation reaction catalyst particles (catalyst particles). The primary particle diameter of the catalyst particles is, for example, 5 nm to 80 nm.
[0046] In the step of preparing the catalyst slurry, catalyst particles are added to a dispersion medium and stirred. Any appropriate solvent that does not dissolve the catalyst particles can be used as the dispersion medium. Examples of the dispersion medium include water and alcohols. The dispersion medium can be used alone or in combination. Among the dispersion mediums, water is preferred. As a result, the catalyst particles are dispersed in the dispersion medium to prepare the catalyst slurry. The content of the catalyst particles in the catalyst slurry is, for example, 3.0% by mass to 30% by mass, and preferably 5.0% by mass to 20% by mass. When the content of the catalyst particles in the catalyst slurry is within this range, the catalyst slurry can be smoothly applied to the partition walls, and a catalyst layer can be stably formed.
[0047] Next, in the step of applying the catalyst slurry to the surfaces of the partition walls 12, the catalyst slurry is applied onto the partition walls 12 of the honeycomb substrate 1 by any appropriate method.
[0048] In one embodiment, the honeycomb substrate 1 is immersed in the catalyst slurry multiple times by changing the immersion portion of the honeycomb substrate 1. For example, first, the entire honeycomb substrate 1 is immersed in the catalyst slurry. Then, the honeycomb substrate 1 is pulled out of the catalyst slurry. As a result, the catalyst slurry is applied to the surfaces of the partition walls 12. Then, the coating of the catalyst slurry formed on the partition walls 12 is dried at any appropriate heating temperature as necessary. As a result, a first layer is formed on the surfaces of the partition walls 12. Next, the honeycomb substrate 1 on which the first layer has been formed is moved along the length direction of the honeycomb substrate 1, and is immersed in the catalyst slurry from the second end face 1b to any appropriate intermediate portion (specifically, the portion between the first end face 1a and the second end face 1b). Then, the honeycomb substrate 1 is pulled out of the catalyst slurry. As a result, the catalyst slurry is applied to the portions of the first layer corresponding to the thick portions 22, and the catalyst slurry is not applied to the portions corresponding to the thin portions 21. Thereafter, the coating of the catalyst slurry formed on the first layer is dried at any appropriate heating temperature, as necessary. In this way, a second layer is formed on the surface of the first layer. Furthermore, the above-described immersion and drying are repeated, as necessary. As a result of the above, a catalyst layer having the thin portions 21 and the thick portions 22 can be formed on the partition walls 12.
[0049] In another embodiment, the honeycomb substrate 1 is immersed in the catalyst slurry multiple times in the same orientation. For example, first, the honeycomb substrate 1 is moved along its length and immersed in the catalyst slurry from the second end face 1b to the first end face 1a. The honeycomb substrate 1 is then lifted out of the catalyst slurry. This allows the catalyst slurry to be applied to the surfaces of the partition walls 12. Next, the honeycomb substrate 1 is typically positioned so that the second end face 1b of the honeycomb substrate 1 faces downward and the first end face 1a of the honeycomb substrate 1 faces upward, and is dried at any appropriate heating temperature. This forms a first layer on the surfaces of the partition walls 12. The thickness of the first layer can increase from the first end face 1a side toward the second end face 1b side. Next, the honeycomb substrate 1 on which the first layer has been formed is moved along its length and again immersed in the catalyst slurry from the second end face 1b to the first end face 1a. Then, typically, the catalyst layer 2 is dried in the same manner as above to form a second layer on the surface of the first layer. The immersion and drying are repeated as necessary. As a result, the catalyst layer 2 having a thickness that continuously increases from the first end face 1 a toward the second end face 1 b can be formed on the partition wall 12.
[0050] 3, a plurality of honeycomb-shaped substrates 1 may be prepared, and the catalyst slurry may be applied by any appropriate method to the partition walls 12 of each of the plurality of honeycomb-shaped substrates 1. The thickness of the catalyst layer 2 formed on the partition walls 12 of each honeycomb-shaped substrate 1 can be adjusted by appropriately changing the number of times the catalyst slurry is applied and dried. This allows the first block 3a, in which the thin-walled portions 21 are formed on the partition walls 12, and the second block 3b, in which the thick-walled portions 22 are formed on the partition walls 12, to be prepared separately.
[0051] In this way, a honeycomb structure 100 including the honeycomb substrate 1 and the catalyst layer 2 is manufactured. The honeycomb structure 100 is subjected to a reduction treatment as needed. This can reduce the active components contained in the catalyst layer to a metallic state. In the reduction treatment, H 2The honeycomb structure is heat-treated in an atmosphere at a heating temperature of, for example, 300 to 600° C., and preferably 400 to 500° C. The heating time is, for example, 0.1 to 8 hours, and preferably 0.5 to 2 hours.
[0052] E. Methane Production Apparatus and Methane Production Method The above-described honeycomb structure 100 is a honeycomb structure for a methanation reaction, and can be suitably used in a methane production apparatus that produces methane by reacting carbon dioxide with hydrogen. The methane production apparatus includes at least the above-described honeycomb structure 100. The methane production apparatus may include any appropriate configuration in addition to the honeycomb structure 100. In the methane production apparatus including the honeycomb structure 100, methane can be produced by supplying a raw material gas containing carbon dioxide and hydrogen to the catalyst layer 2 of the honeycomb structure 100.
[0053] In one embodiment, the honeycomb structure 100 is heated to a predetermined methanation reaction initiation temperature, and a raw material gas containing carbon dioxide and hydrogen is supplied to the gas flow passages 14 of the honeycomb structure 100. The methanation reaction initiation temperature is, for example, 200°C to 300°C. As a result, the raw material gas is supplied to the catalyst layer 2 at the methanation reaction initiation temperature, and the methanation reaction of the above formula (1) is initiated.
[0054] The carbon dioxide content in the feed gas is, for example, 1.0 vol% to 20 vol%, preferably 5.0 vol% to 15 vol%. The hydrogen content in the feed gas is, for example, 4.0 vol% to 80 vol%, preferably 20 vol% to 60 vol%. In one embodiment, the feed gas contains oxygen in addition to carbon dioxide and hydrogen. When the feed gas contains oxygen, the combustion reaction represented by formula (2) above can proceed when hydrogen and oxygen come into contact with the methanation reaction catalyst. The oxygen content in the feed gas is, for example, 0.5 vol% to 10 vol%, preferably 1.0 vol% to 5.0 vol%. Furthermore, the feed gas may contain nitrogen as the balance. Any appropriate value can be adopted for the flow rate of such a feed gas. The flow rate of the feed gas is, for example, 500 mL / min to 15,000 mL / min.
[0055] When the raw material gas is supplied to the catalyst layer 2 at the methanation reaction initiation temperature and the methanation reaction of formula (1) begins, the methanation reaction can be continued by utilizing the reaction heat. Therefore, external heating of the honeycomb structure 100 may be stopped. In a state in which external heating of the honeycomb structure 100 is stopped, the honeycomb structure 100 can be maintained at, for example, 300°C to 500°C by the reaction heat. In other words, by using the honeycomb structure 100, automated methanation can be performed. Therefore, energy conservation in methane production can be achieved. Furthermore, since the honeycomb structure 100 can be maintained at a temperature suitable for the methanation reaction without providing a heat insulating material for the honeycomb structure 100, a methane production apparatus can be designed to be compact.
[0056] As a result, a methane-containing gas is continuously discharged from the gas flow passages 14 of the honeycomb structure 100. The methane-containing gas contains at least methane. The methane-containing gas may also contain raw material gas that remains unreacted. In such methane production, since the catalyst layer 2 has the above-mentioned concentration of catalyst loading, methane can be produced with an excellent methane conversion rate. The methane conversion rate is, for example, 65% or more, preferably 70% or more, more preferably 75% or more, and even more preferably 80% or more. On the other hand, the methane conversion rate is, for example, 100% or less, or, for example, 90% or less.
[0057] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these examples.
[0058] Example 1 Preparation of Honeycomb Substrate A clay containing cordierite was extruded and then dried to prepare the honeycomb substrate shown in FIG. 1 . The honeycomb substrate had a cylindrical shape with a diameter of 20 mm and a length of 50 mm. The honeycomb substrate included partition walls defining a plurality of cells and an outer peripheral wall surrounding the partition walls. The cross-sectional shape of the cells was rectangular. The cell density of the honeycomb substrate was 300 cpsi, the partition wall thickness was 0.0254 mm, the average pore diameter of the partition walls was 20 μm, and the porosity of the partition walls was 50%. Preparation of Methanation Reaction Catalyst Cerium (IV) oxide particles (manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd.) were introduced into distilled water and then stirred under reduced pressure at room temperature (23°C) for 12 hours. This resulted in a dispersion of metal oxide particles. Additionally, nickel (II) nitrate hexahydrate was dissolved in distilled water to obtain a nickel nitrate aqueous solution. The nickel nitrate aqueous solution was then added to the dispersion of metal oxide particles and stirred at room temperature (23°C) for 2 hours. The mixture of the dispersion and the aqueous solution was then heated to 80°C while stirring to evaporate the water. The remaining solid was then heated at 500°C for 3 hours. This resulted in methanation reaction catalyst particles (hereinafter referred to as catalyst particles). The catalyst particles contained nickel oxide (NiO) and cerium (IV) oxide supporting nickel oxide (NiO). The Ni content in the methanation reaction catalyst particles was 10 parts by mass per 100 parts by mass of cerium oxide. <<Preparation of Catalyst Layer>> The obtained catalyst particles were dispersed in distilled water to prepare a catalyst slurry. The catalyst slurry contained 10% by mass of catalyst particles. Next, the entire honeycomb substrate prepared above was immersed in the catalyst slurry for 5 seconds under normal pressure (0.1 MPa) and room temperature (23°C). Thereafter, the honeycomb substrate was pulled out of the catalyst slurry. In this way, the catalyst slurry was applied to the surfaces of the partition walls. Thereafter, the catalyst slurry applied to the surfaces of the partition walls was heated at 100°C for 120 minutes and dried. The above immersion and drying were repeated three times. In this way, a first layer was formed on the surfaces of the partition walls. Next, the honeycomb substrate on which the first layer was formed was arranged so that the length direction of the honeycomb substrate was approximately parallel to the vertical direction and the second end face faced the liquid surface of the catalyst slurry.The honeycomb substrate was then moved downward and immersed in the catalyst slurry from the second end face of the honeycomb substrate to a predetermined intermediate position for 5 seconds under the above conditions. With the honeycomb substrate immersed in the catalyst slurry to the intermediate position, the first end face of the honeycomb substrate was positioned vertically away from the liquid surface of the catalyst slurry. The honeycomb substrate was then lifted out of the catalyst slurry. This coated the catalyst slurry onto the surface of the first layer. The catalyst slurry coated onto the surface of the first layer was then heated at 100°C for 120 minutes and dried. The above immersion and drying process was repeated seven times. This formed a second layer on the surface of the first layer. This resulted in the formation of a catalyst layer having a thin portion (first layer) and thick portions (first and second layers). The catalyst layer contained aggregates of catalyst particles. When the total length of the catalytic layer is 100% and the first end of the catalytic layer is 0%, the thin portion was provided over 0% to 10% of the catalytic layer, and the thick portion was provided over 10% to 100% of the catalytic layer. The thickness of the catalytic layer at the 5% position (i.e., the thin portion), the thickness of the catalytic layer at the 50% position (i.e., the thick portion), and the catalyst loading amount in each of the thin portion and the thick portion are shown in Table 1. In this way, a honeycomb structure including a honeycomb substrate and a catalytic layer was manufactured.
[0059] Comparative Example 1 A honeycomb substrate and a catalyst slurry were prepared in the same manner as in Example 1. The honeycomb substrate was then positioned so that the length direction of the honeycomb substrate was approximately parallel to the vertical direction and the second end face faced the liquid surface of the catalyst slurry. The honeycomb substrate was then moved downward, and the honeycomb substrate was immersed in the catalyst slurry from the second end face to the first end face in the same manner as described above. The honeycomb substrate was then lifted out of the catalyst slurry. This coated the catalyst slurry onto the partition wall surfaces. The catalyst slurry coated onto the partition wall surfaces was then heated and dried in the same manner as described above. This formed a first layer on the partition wall surfaces. The honeycomb substrate with the first layer formed thereon was then turned over and positioned so that the first end face faced the liquid surface of the catalyst slurry. The honeycomb substrate was then moved downward, and the honeycomb substrate was immersed in the catalyst slurry from the first end face to the second end face in the same manner as described above. The honeycomb substrate was then lifted out of the catalyst slurry. This coated the catalyst slurry onto the surface of the first layer. The catalyst slurry coated onto the surface of the first layer was then heated and dried in the same manner as above. This formed a second layer onto the surface of the first layer. The above immersion and drying process was repeated seven times. This resulted in the formation of a catalyst layer with a substantially uniform thickness throughout, and a honeycomb structure was manufactured. The thickness of the catalyst layer at the 5% position, the thickness at the 50% position, and the catalyst loading amount are shown in Table 1.
[0060] <Automethanation Test> The honeycomb structures obtained in the examples and comparative examples were inserted into a reaction tube with an inner diameter of 21 mm. As a pretreatment for the reaction, the honeycomb structures were heated to 500°C using an electric furnace installed around the outer periphery of the reaction tube, and hydrogen gas was introduced into the reaction tube for reduction. The temperature of the electric furnace was then lowered to 200°C, and a mixed gas consisting of 10% by volume of carbon dioxide, 3% by volume of oxygen, 46% by volume of hydrogen, and the remainder of nitrogen was introduced into the reaction tube as a raw material gas. The flow rate of the raw material gas introduced into the reaction tube was set to 1,000 mL / min. As a result, the raw material gas passed through each gas flow channel provided in the honeycomb structure, and methane-containing gas flowed out of the reaction tube. While the raw material gas was flowing into the reaction tube, the set temperature of the electric furnace was gradually lowered, and finally, heating by the electric furnace was stopped. The temperature of the first end of the catalyst layer after heating by the electric furnace was stopped was measured using a thermocouple. The results are shown in Table 1. The concentrations of carbon dioxide and methane in the methane-containing gas flowing out of the reaction tube after the heating of the electric furnace was stopped were measured using a gas chromatograph-thermal conductivity detector (GC-TCD). Based on the measurement results, the conversion rate (%) of carbon dioxide to methane was calculated using the following formula (I). The results are shown in Table 1. Methane conversion rate (%) = (amount of methane contained in methane-containing gas (volume %) / amount of carbon dioxide contained in feed gas (volume %)) × 100 (I)
[0061]
[0062] <Evaluation> As shown in Table 1, when the catalyst layer has a gradient in the amount of methanation reaction catalyst supported in the direction of passage of the fluid in the gas flow channel (particularly, the supported amount is relatively small in the upstream portion and relatively large in the downstream portion), it is found that the methane conversion rate can be significantly improved.
[0063] The honeycomb structure according to the embodiment of the present invention can be suitably used in a methane production apparatus that produces methane by reacting carbon dioxide with hydrogen.
[0064] REFERENCE SIGNS LIST 1 honeycomb substrate 12 partition wall 13 cell 14 gas flow channel 2 catalyst layer 2a first end of catalyst layer 2b second end of catalyst layer 21 thin portion 22 thick portion 100 honeycomb structure
Claims
1. A honeycomb structure comprising: a honeycomb substrate having partition walls defining a plurality of cells including gas flow paths; and a catalyst layer including a methanation reaction catalyst for reacting carbon dioxide with hydrogen to produce methanation, the catalyst layer being provided on a surface of the partition wall so as to face the gas flow paths, wherein the catalyst layer has a gradient in the amount of the methanation reaction catalyst supported per unit area of the partition wall in the passage direction of a fluid in the gas flow paths.
2. The honeycomb structure according to claim 1, wherein the amount of the methanation reaction catalyst carried increases toward the downstream side in the passing direction.
3. The honeycomb structure according to claim 2, wherein the catalyst layer has a first end which is an upstream end in the passing direction and a second end which is a downstream end in the passing direction, and when the total length of the catalyst layer in the passing direction is 100% and the first end of the catalyst layer is 0%, the amount of the methanation reaction catalyst supported in a range of 0% to 10% of the catalyst layer is less than the amount of the methanation reaction catalyst supported in a range of 50% to 100% of the catalyst layer.
4. A honeycomb structure as described in claim 2, wherein when the total length of the catalyst layer in the passing direction is 100% and the first end of the catalyst layer is 0%, the thickness of the catalyst layer at a 50% position is greater than the thickness of the catalyst layer at a 5% position.
5. The honeycomb structure according to claim 4, wherein the catalyst layer includes a thin portion and a thick portion in that order in the passing direction.
6. The honeycomb structure according to any one of claims 1 to 5, wherein the methanation reaction catalyst contains Ni as an active component and a cerium oxide carrier supporting Ni.
Citation Information
Patent Citations
Carbon dioxide fixation system
JP2015196619A
Articles for removing carbon monoxide
JP2005538019A
Co2 methanation catalyst and carbon dioxide reduction method using the same
JP2019155227A
Method for manufacturing methane and manufacturing system
JP2020033280A
Catalyst reaction device
JP2020093216A