Rare earth bonded magnet

The rare earth bonded magnet with isotropic Nd-Fe-B powder and cured epoxy resin addresses mechanical and electrical challenges, enhancing strength and resistance without compromising magnetic properties, thus improving motor performance.

WO2024203793A1PCT designated stage expired Publication Date: 2024-10-03MINEBEAMITSUMI INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011184
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-16
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Rare earth bonded magnets used in high-speed motors face challenges in mechanical strength and electrical resistance, leading to potential damage and inefficiency, with existing solutions increasing weight and complexity while compromising magnetic properties.

Method used

A rare earth bonded magnet composed of isotropic Nd-Fe-B magnet powder and a cured epoxy resin with a specific weight ratio, achieving high radial crushing strength and electrical resistivity without significant magnetic property degradation, through optimized powder production and resin content.

Benefits of technology

The solution enhances mechanical strength and electrical resistance of rare earth bonded magnets, preventing damage and improving motor efficiency while maintaining magnetic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011184_03102024_PF_FP_ABST
    Figure JP2024011184_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This rare earth bonded magnet comprises a rare earth magnet powder and a cured product of a thermosetting resin, wherein: the rare earth magnet powder is an isotropic Nd-Fe-B-based magnet powder; the thermosetting resin is an epoxy resin; the content of the cured product in 100 wt% of the rare earth bonded magnet is more than 5 wt% but not more than 6.5 wt%; and the rare earth bonded magnet has a porosity of less than 5%, a radial crushing strength of not less than 60 MPa, and an electric resistivity of not less than 100 μΩ・m.
Need to check novelty before this filing date? Find Prior Art

Description

rare earth bonded magnet

[0001] The present invention relates to a rare earth bonded magnet.

[0002] In recent years, rare earth permanent magnets have been used in a wide range of fields, including rotating machinery such as motors, general home appliances, audio equipment, medical equipment, and general industrial machinery, due to their excellent magnetic properties. Rare earth bonded magnets, obtained from rare earth magnetic powder and a binder (resin) that binds the powder, offer a high degree of freedom in shape, contributing to the miniaturization and high performance of the above-mentioned machinery. One proposed rare earth bonded magnet is one that combines Nd—Fe—B magnetic powder with a thermosetting epoxy resin binder (see, for example, Patent Document 1).

[0003] In the rare earth bonded magnet of Patent Document 1, Nd-Fe-B quenched magnet powder is used as the rare earth magnet powder, and epoxy resin is used as the binder resin, with approximately 2.5 wt % of epoxy resin mixed in.

[0004] Furthermore, when a rare earth bonded magnet is incorporated into a motor that rotates at high speed, a large centrifugal force acts on the rotor to which the rare earth bonded magnet is attached, which can cause the rare earth bonded magnet to break and fly apart.As a means to prevent this from happening, a configuration has been proposed in which a protective cover made of reinforced plastic is provided on the rare earth bonded magnet (see, for example, Patent Document 2).

[0005] JP-A No. 6-314605 JP-A No. 8-107641

[0006] If a protective cover made of reinforced plastic as described in Patent Document 2 is provided on a rare earth bonded magnet as described in Patent Document 1, it is possible to prevent the rare earth bonded magnet from flying off, but this increases the weight of the rotor, increasing inertia, and the number of parts and the number of installation steps, which increases costs, etc. For this reason, it is necessary to increase the mechanical strength (radial crushing strength) of the rare earth bonded magnet.

[0007] Furthermore, compared to rare earth sintered magnets, rare earth bonded magnets have the advantage of high electrical resistance due to the presence of insulating resin between the magnetic powder particles. However, when a rare earth bonded magnet containing conventional Nd—Fe—B magnetic powder and 2 wt% to 3 wt% resin is incorporated into a high-speed motor, the electrical resistance is not necessarily high, resulting in increased eddy current loss and reduced motor efficiency. For this reason, it is necessary to increase the electrical resistance.

[0008] As described above, in a configuration in which a rare earth bonded magnet containing a thermosetting resin is used in a motor that rotates at high speed, there is room for further improvement over the rare earth bonded magnet.

[0009] Therefore, an object of the present invention is to provide a rare earth bonded magnet that has high radial crushing strength and electrical resistance without causing a significant decrease in the magnetic properties of the rare earth bonded magnet.

[0010] In order to solve the above-mentioned problems and achieve the object, a rare earth bonded magnet according to one embodiment of the present invention is a rare earth bonded magnet comprising rare earth magnet powder and a cured resin of a thermosetting resin, wherein the rare earth magnet powder is an isotropic Nd—Fe—B based magnet powder, the thermosetting resin is an epoxy resin, the cured resin is contained in an amount of more than 5 wt % and not more than 6.5 wt % based on 100 wt % of the rare earth bonded magnet, and the rare earth bonded magnet has a porosity of less than 5%, a radial crushing strength of 60 MPa or more, and an electrical resistivity of 100 μΩ·m or more.

[0011] According to one aspect of the present invention, a rare earth bonded magnet having high radial crushing strength and electrical resistance can be obtained without causing a significant decrease in the magnetic properties of the rare earth bonded magnet.

[0012] FIG. 1 is a diagram showing the ratios (Vol %) of rare earth magnet powder, cured thermosetting resin, and voids in a rare earth magnet bond.

[0013] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to these embodiments. Furthermore, the components in the following embodiments include those that are easily replaceable by those skilled in the art, or those that are substantially the same.

[0014] <Embodiment 1> The rare earth bonded magnet of embodiment 1 includes a rare earth magnet powder and a cured resin of a thermosetting resin. The rare earth magnet powder is an isotropic Nd (neodymium)-Fe (iron)-B (boron) based magnet powder. Examples of isotropic Nd—Fe—B based magnet powder include MQP-14-12 (product name), MQP-8-5 (product name), MQP-10-8.5HD (product name), MQP-11-8 (product name), and MQP12-8HD (product name) manufactured by Magnequench Corporation.

[0015] Alternatively, for example, Nd—Fe—B magnet powder produced by a rapid cooling method may be used. Specifically, an Nd—Fe—B alloy is melted by high-frequency induction heating under reduced pressure or in an argon atmosphere. The molten alloy is then sprayed onto a rotating copper roll and rapidly cooled (rapidly cooled) to produce ribbon-shaped thin strips. The thin strips are then broken into pieces, for example, several millimeters to several tens of millimeters in size, and pulverized using a grinder or the like to obtain powder. The pulverized powder is then classified using a sieve with a specified mesh and then heat-treated to produce rare earth magnet powder. This rare earth magnet powder is magnetically isotropic because the easy axes of magnetization of the crystal grains are not aligned in a single direction.

[0016] The rare earth magnet powder preferably has a particle size in the range of 45 μm or more and less than 175 μm. Alternatively, the rare earth magnet powder may have a particle size in the range of 45 μm or more and less than 75 μm, or may have a particle size in the range of 75 μm or more and less than 175 μm. Such particle size ranges can be adjusted by classification using a sieve with a specified mesh.

[0017] The cured thermosetting resin contained in the rare earth bonded magnet of embodiment 1 is specifically a cured epoxy resin, that is, the thermosetting resin is an epoxy resin.

[0018] The cured resin is contained in an amount of more than 5% by weight and not more than 6.5% by weight of the rare earth bonded magnet. The rare earth magnet powder is contained in an amount of 93.5% by weight or more and less than 95% by weight. In the rare earth bonded magnet of embodiment 1, it is preferable that the rare earth magnet powder and the cured thermosetting resin are uniformly mixed. Conventionally, when producing bonded magnets using thermosetting resins, the binder ratio is used in an amount of 2% by weight or more and not more than 3% by weight.

[0019] The rare earth bonded magnet of embodiment 1 has a porosity of less than 5%. As such, the rare earth bonded magnet of embodiment 1 contains the above-mentioned amount of cured thermosetting resin, resulting in a low porosity and high radial crushing strength. In other words, the rare earth bonded magnet of embodiment 1 has a radial crushing strength of 60 MPa or more. Furthermore, because the rare earth bonded magnet of embodiment 1 has a low porosity and a relatively high volume fraction occupied by rare earth magnetic powder, deterioration of magnetic properties is also suppressed.

[0020] Furthermore, the rare earth bonded magnet of embodiment 1 contains the above amount of cured thermosetting resin, and therefore has high electrical resistance. That is, the rare earth bonded magnet of embodiment 1 has an electrical resistivity of 100 μΩ·m or more.

[0021] The rare earth bonded magnet of embodiment 1 can be produced, for example, as follows. First, the rare earth magnet powder and the components that make up the cured resin in the rare earth bonded magnet (the raw material components of the cured resin) are mixed in a predetermined ratio to produce a compound. The ratio of the rare earth magnet powder to the raw material components of the cured resin is considered to be the same as the ratio of the rare earth magnet powder to the cured resin in the produced rare earth bonded magnet. The raw material components of the cured resin include a thermosetting resin binder (e.g., epoxy resin) and a curing agent. Furthermore, a small amount of a lubricant (e.g., calcium stearate) may be added when producing the compound. Specifically, the lubricant may be added in an amount of 0.02 wt % or more but less than 0.5 wt % based on the total weight of the rare earth magnet powder and the raw material components of the cured resin (100 wt %).

[0022] Next, the compound is filled into the cavity of a mold and compressed under a predetermined pressure to produce a green body. The green body is then removed from the mold and placed in an oven, where it is thermally cured at a predetermined temperature for a predetermined time to produce a cured body (thermoset body) containing the rare earth magnet powder and the cured resin. It is also preferable to apply a rust prevention measure to the surface of the cured body to prevent oxidation. Known methods of rust prevention, such as electrocoating and spray coating, can be used. In this way, the rare earth bonded magnet of embodiment 1 is obtained.

[0023] <Embodiment 2> One of the objectives of embodiment 2 is to prevent a significant decrease in the magnetic properties of the rare earth bonded magnet even when the rare earth magnetic powder is small.

[0024] To solve the above-mentioned problems and achieve the object, the rare earth bonded magnet according to the second embodiment is a rare earth bonded magnet containing a rare earth magnetic powder and a cured thermosetting resin, wherein the rare earth magnetic powder is an isotropic Nd—Fe—B magnetic powder, the thermosetting resin is an epoxy resin, the cured resin is contained in an amount of more than 5% by weight and not more than 6.5% by weight based on 100% by weight of the rare earth bonded magnet, the particle size of the rare earth magnetic powder is 45 μm or less, and the surface of the rare earth magnetic powder is coated with a compound containing phosphorus. In the second embodiment, as in the first embodiment, the rare earth bonded magnet preferably has a porosity of less than 5%, a ring strength of 60 MPa or more, and an electrical resistivity of 100 μΩ·m or more.

[0025] By subjecting rare earth magnet powder to phosphate treatment after pulverization, oxidation degradation of the magnet powder can be prevented, which prevents a significant deterioration in the magnetic properties of the rare earth bonded magnet.

[0026] Furthermore, when the above-mentioned phosphate treatment is performed, even if the particle size of the rare earth magnet powder is greater than 0 μm and less than 45 μm, it is possible to provide a rare earth bonded magnet without preventing a significant deterioration in the magnetic properties of the rare earth bonded magnet.

[0027] Furthermore, the rare earth magnet powder is not limited to Nd—Fe—B quenched magnetic powder, but may also be isotropic Sm—Fe—N, anisotropic Sm—Fe—N, anisotropic Nd—Fe—B magnetic powder (product name d-HDDR), or SmCo magnetic powder (pulverized anisotropic magnetic powder).

[0028] Furthermore, the thermosetting resin may be a conductive epoxy resin. In this case, in the process of electrodeposition coating, in which a current is passed through the magnet to apply a conductive epoxy resin for rust prevention, the magnet itself is conductive, so the electrodeposition coating adheres easily and the film-forming properties of the electrodeposition coating can be improved. The manufacturing methods for the rare earth magnet powder, the cured resin of the thermosetting resin, and the rare earth bonded magnet are the same as those of embodiment 1, except as described above.

[0029] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these examples. The following examples correspond to embodiment 1.

[0030] [Example] <Preparation of Rare Earth Bonded Magnet> Isotropic Nd—Fe—B based magnet powder was used as the rare earth magnet powder. MQP-14-12 (product name) manufactured by Magnequench was prepared as the isotropic Nd—Fe—B based magnet powder. The particle size of MQP-14-12 was classified into two groups: 75 μm or more and less than 150 μm, and 45 μm or more and less than 75 μm. The classification was carried out using a sieve with a specified mesh. Next, for each of the two groups, the isotropic Nd—Fe—B based magnet powder was mixed with raw material components of a cured resin (manufactured by Pernoc, model number XW2310) containing an epoxy resin binder and a curing agent at a specified blending ratio to prepare a compound. Here, the blending ratio of the raw material components of the cured resin was 2.5 wt % for the cured resin and 97.5 wt % for the rare earth magnet powder, with the total weight being 100 wt %. Furthermore, compounds were also prepared in the following cases: 5 wt % for the cured resin and 95 wt % for the rare earth magnet powder; 5.5 wt % for the cured resin and 94.5 wt % for the rare earth magnet powder; 6 wt % for the cured resin and 94 wt % for the rare earth magnet powder; 6.5 wt % for the cured resin and 93.5 wt % for the rare earth magnet powder; and 7.5 wt % for the cured resin and 92.5 wt % for the rare earth magnet powder. The compounds were prepared by mixing the raw material components of the cured resin dissolved in a solvent with the rare earth magnet powder, evaporating the solvent, and then crushing and classifying the mixture. The compounds were all prepared with the same particle size, and the fluidity conditions for filling into the mold cavity were the same. Next, the compounds were filled into the mold cavity and pressed under a predetermined pressure (molding pressure: surface pressure 5 ton / cm 2) was added and compressed to produce a green body. The green body was cylindrical with a diameter of 10 mm and a height of 7 mm. Next, the green body was removed from the mold and placed in an oven where it was thermally cured at a predetermined temperature (150°C) for a predetermined time to produce a cured body (thermosetting body). The cured body was cylindrical with a diameter of 10 mm and a height of 7 mm. As shown, no difference in size was observed between the green body and the cured body. Next, a rust prevention measure (specifically, electrocoating) was applied to the surface of the cured body to prevent oxidation. In this way, rare earth bonded magnets (Samples 1 to 12) containing rare earth magnet powder and a cured resin of a thermosetting resin were produced. Here, Samples 3 to 5 and 9 to 11 are examples, and Samples 1, 2, 6, 7, 8, and 12 are comparative examples.

[0031] <Evaluation Method> (Porosity) The porosity was calculated from the apparent density relative to the true density. The evaluation criteria are as follows: ○: Porosity is less than 5%. △: Porosity is 5% or more but less than 15%. ×: Porosity is 15% or more.

[0032] (Radial crushing strength) The radial crushing strength was measured in accordance with JIS Z2507. The evaluation criteria are as follows: ⊚: The radial crushing strength is 100 MPa or more. ◯: The radial crushing strength is 60 MPa or more and less than 100 MPa. Δ: The radial crushing strength is 50 MPa or more and less than 60 MPa. ×: The radial crushing strength is less than 50 MPa.

[0033] (Electrical Resistivity) Electrical resistivity was measured using a four-point probe method. The magnet sample had a diameter of 10 mm and a height of 7 mm, and the average electrical resistivity was calculated for N5 evaluations. The evaluation criteria are as follows: ◎: Electrical resistivity is 100 μΩ·m or more. ○: Electrical resistivity is 10 μΩ·m or more but less than 100 μΩ·m. △: Electrical resistivity is less than 10 μΩ·m.

[0034] (Overall Evaluation) An overall evaluation was performed on Samples 1 to 12. The evaluation criteria are as follows: ∘: The evaluation results for both radial crushing strength and electrical resistivity are ⊚. ×: Other than the above. The evaluation results for Samples 1 to 12 are shown in Tables 1 and 2 below. In Table 1, "45-75" for magnetic powder particle size (μm) indicates that the particle size of the isotropic Nd—Fe—B based magnetic powder is in the range of 45 μm or more and less than 75 μm. In Table 2, "75-150" for magnetic powder particle size (μm) indicates that the particle size of the isotropic Nd—Fe—B based magnetic powder is in the range of 75 μm or more and less than 150 μm.

[0035]

[0036] Table 1 shows samples 1 to 6, which are rare earth bonded magnets with isotropic Nd—Fe—B magnetic powder particle sizes ranging from 45 μm to less than 75 μm. Sample 1, in which the raw material component content of the cured resin was 2.5 wt %, had a porosity of 15% or more, and both the radial crushing strength and electrical resistance (surface resistivity) were rated Fair. This is because the raw material component content of the cured resin was approximately the same as that of conventional rare earth bonded magnets. Sample 6, in which the raw material component content of the cured resin was 7.5 wt %, had some of the binder leaking out of the cavity, posing a manufacturing problem, and was therefore not rated. This is because the raw material component content of the cured resin was too high. Samples 3 to 5, other than the samples with raw material component content of 2.5 wt %, 5 wt %, and 7.5 wt %, were rated Excellent in all categories. Therefore, the overall rating of Samples 3 to 5 shown in Table 1 is Fair. The results in Table 1 show that as the porosity in a rare earth bonded magnet decreases, the radial crushing strength and electrical resistivity increase. In the working examples, Samples 3 to 5, both the radial crushing strength and electrical resistivity can be increased. Compared to Sample 1 (Comparative Example), in which the amount of raw material components in the cured resin is 2.5% by weight, Samples 3 to 5 have an increased amount of raw material components in the cured resin, resulting in a slight decrease in the magnetic powder filling ratio. However, this is only a slight decrease compared to the magnetic properties of the rare earth bonded magnet of Sample 1 (Comparative Example), and it has been confirmed that magnetic properties comparable to those of the rare earth bonded magnet of Sample 1 (Comparative Example) can be obtained.

[0037]

[0038] Table 2 shows the evaluations of samples 7 to 12, which are rare earth bonded magnets with isotropic Nd—Fe—B magnetic powder particle sizes ranging from 75 μm to less than 150 μm. Sample 7, in which the raw material component content of the cured resin was 2.5 wt %, had a porosity of 15% or more, and both the radial crushing strength and electrical resistivity were rated as fair. This is because the raw material component content of the cured resin was approximately the same as that of conventional rare earth bonded magnets. Sample 12, in which the raw material component content of the cured resin was 7.5 wt %, had some of the binder leaking out of the cavity, which posed a manufacturing problem, and was therefore not evaluated. This is because the raw material component content of the cured resin was too high. Samples 9 to 11, other than the samples with raw material component content of 2.5 wt %, 5 wt %, and 7.5 wt %, were rated as excellent in all categories. Therefore, the overall evaluation of samples 9 to 11 shown in Table 2 is rated as excellent. The results in Table 2 show that as the porosity in a rare earth bonded magnet decreases, the radial crushing strength and electrical resistivity increase. In the practical examples, Samples 9 to 11, both the radial crushing strength and electrical resistivity can be increased. Compared to Sample 7 (Comparative Example), which has a conventional amount of raw material components of 2.5% by weight of the cured resin, Samples 9 to 11 have an increased amount of raw material components of the cured resin, resulting in a slight decrease in the magnetic powder filling ratio. However, this is only a slight decrease compared to the magnetic properties of the rare earth bonded magnet of Sample 7 (Comparative Example), and it has been confirmed that magnetic properties comparable to those of the rare earth bonded magnet of Sample 7 (Comparative Example) can be obtained.

[0039] FIG. 1 shows the ratio (Vol%) of rare earth magnet powder, cured thermosetting resin, and voids in a rare earth magnet bond. Specifically, it shows samples 1 to 6. It can be seen that samples 3 to 5 have a reduced void ratio, resulting in higher radial crushing strength. It can also be seen that samples 3 to 5 have almost no reduction in the ratio of rare earth magnet powder, suppressing the deterioration of magnetic properties. The void ratio was calculated as follows. Magnetic powder density 7.6 [g / cm 3 ], resin specific gravity 0.92 [g / cm 3 The true density of the prototype magnet was calculated from the volume ratio of magnetic powder to resin in the true density, and the remainder was taken as the porosity.

Claims

1. A rare earth bonded magnet comprising rare earth magnet powder and a cured thermosetting resin, wherein the rare earth magnet powder is isotropic Nd-Fe-B magnet powder, the thermosetting resin is epoxy resin, the cured resin is contained in an amount of more than 5% by weight and not more than 6.5% by weight based on 100% by weight of the rare earth bonded magnet, and the rare earth bonded magnet has a porosity of less than 5%, a radial crushing strength of 60 MPa or more, and an electrical resistivity of 100 μΩ・m or more.

2. A rare earth bonded magnet comprising rare earth magnet powder and a hardened thermosetting resin, wherein the thermosetting resin is an epoxy resin, the hardened resin is contained in an amount of more than 5% by weight and not more than 6.5% by weight per 100% by weight of the rare earth bonded magnet, the particle size of the rare earth magnet powder is 45 μm or less, and the surface of the rare earth magnet powder is coated with a compound containing phosphorus.

3. The rare earth bonded magnet according to claim 2, wherein the rare earth magnet powder is an isotropic Nd-Fe-B system magnet powder.

4. The rare earth bonded magnet according to claim 2, wherein the rare earth magnet powder is anisotropic Nd-Fe-B system magnet powder.

5. The rare earth bonded magnet according to claim 2, wherein the rare earth magnetic powder is an isotropic Sm-Fe-N magnetic powder.

6. The rare earth bonded magnet according to claim 2, wherein the rare earth magnet powder is anisotropic Sm-Fe-N system magnet powder.

7. The rare earth bonded magnet according to claim 2, wherein the rare earth magnet powder is anisotropic SmCo-based magnet powder.

8. The rare earth bonded magnet according to claim 2, wherein the epoxy resin is electrically conductive.

Citation Information

Patent Citations

  • Method for plating bond magnet

    JP1992276095A

  • Coating and coated product

    JP1996170192A

  • Rare-earth bonded magnet, composition for rare-earth bonded magnet and manufacture of rare-earth bonded magnet

    JP1997232132A

  • High weather resistant magnet powder, its manufacturing method and bonded magnet using the same

    JP2003217915A

  • Iron-based magnet alloy powder including rare earth element, method for manufacturing the same, rare earth composition for bond magnet, and rare earth magnet

    JP2018081969A