Method and apparatus for producing fiber-integrated material

The method of boiling, beating, and molding recovered fibers with a water-based adhesive addresses the limitations of current recycling methods, producing high-strength, design-enhanced fiber aggregate materials that can be effectively reused in diverse applications, aligning with sustainable development goals.

WO2024203837A1PCT designated stage expired Publication Date: 2024-10-03BEERO INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011272
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current methods for recycling textile waste into fiber aggregate materials face challenges such as limited applications, insufficient strength, and inability to effectively utilize design properties, leading to wastage and inefficient reuse of fibers.

Method used

A method involving boiling, beating, and mixing recovered fibers with a water-based adhesive, followed by hot pressing and molding to create a laminate material with polishing, which enhances the strength and design quality of the fiber aggregate material.

Benefits of technology

Enables the effective reuse of discarded textiles to produce high-strength, design-rich fiber aggregate materials suitable for various applications, aligning with sustainable development goals by reducing waste and promoting social and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011272_03102024_PF_FP_ABST
    Figure JP2024011272_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a method and an apparatus for producing a fiber-integrated material which is very strong and has favorable design properties from a recovered fiber product. Provided is a method for producing a fiber-integrated material which is characterized by comprising: a step for extracting a fibrous material by immersing a recovered fiber product in a resin adhesive, and stewing and beating the immersed recovered fiber product; a step for creating a fiber-integrated material by mixing an aqueous adhesive into the extracted fibrous material; a step for hot-pressing and molding the fiber-integrated material; and a step for polishing the molded fiber-integrated material.
Need to check novelty before this filing date? Find Prior Art

Description

Method and apparatus for producing fiber-assembly material

[0001] The present invention relates to a method and an apparatus for manufacturing fiber-based materials such as plywood and laminated lumber using fiber cloth, and more specifically, to a method and an apparatus for manufacturing fiber-based materials for building materials and flooring materials by reusing fiber cloth that would otherwise be discarded.

[0002] In recent years, various types of clothing, such as work uniforms, have been mass-produced and discarded, but no method has been established for effectively reusing such textile products. Furthermore, scraps of textile fabric are generated when uniforms are manufactured, but no method has been established for effectively reusing such scraps.

[0003] Traditionally, textile waste (rags) from clothing and other materials has been incinerated, except for being recycled into rags and pile. The rags obtained by unraveling woven fabric retain their fibrous properties, except for the fact that the fiber length has been shortened by cutting. From the perspective of recycling, it is preferable to reuse the rags from textiles included in general waste. Furthermore, when clothing is rag-recycled and reconstituted into clothing, 40 to 50 percent of the fibers are discarded because they cannot be spun into yarn due to the shortened fiber length, which is not ideal recycling.

[0004] Patent Document 1 discloses a method for manufacturing a fiberboard, specifically, a method for manufacturing a fiberboard by reusing fiber products and fiber cloths that were scheduled to be discarded (hereinafter referred to as "recycled fiber products"). However, since the applications for which the fiberboard can be used are limited, it cannot be said that the fiberboard is being used effectively.

[0005] On the other hand, it is problematic if the material is simply easy to process; it is desirable for the fiber aggregate to have a certain degree of strength. In this regard, Patent Document 2 provides some suggestions, although it is a technology other than fiber cloth, but it is difficult to transfer the technology to fiber products using a simple method. In order to reuse fiber products and have them adopted in many products for a wide range of uses, it is desirable to be able to utilize the design properties of fiber products.

[0006] Patent Document 3 discloses a fiberboard made from recycled fiber-recycled materials that can be used as a greening material on which plants such as moss can be cultivated. However, the fiberboard in Patent Document 3 does not have enough strength to be used as a building material, and so its use as a greening material has traditionally been limited to that of such a material.

[0007] Japanese Patent Application Laid-Open No. 2005-254695 Japanese Patent Application Laid-Open No. 2004-25857 Japanese Patent Application Laid-Open No. 2009-148950

[0008] According to one aspect of the present invention, an object is to provide a method and an apparatus for producing a fiber-filled material having high strength and a high designability from recovered fiber products.

[0009] According to one aspect of the present invention, there is provided a method for producing a fiber cloth, comprising the steps of: boiling and beating recovered fiber products to extract fibrous material; mixing the extracted fibrous material with an aqueous adhesive and immersing the adhesive; hot pressing and molding the immersed material into an aggregate; and polishing the molded aggregate.

[0010] According to one aspect of the present invention, clothing and the like that would otherwise be discarded can be recovered and used to manufacture new products, thereby enabling the effective reuse of recovered textile products.

[0011] Furthermore, it is possible to produce a highly designable fiber-collected material that makes use of the texture of the recycled fiber products.

[0012] Furthermore, from the perspective of the Sustainable Development Goals (SDGs), it is possible to provide products that have a positive impact on society, such as the global environment and local communities (so-called social good).

[0013] Other objects, features and advantages of the present invention will become apparent from the following description of the preferred embodiments of the present invention taken in conjunction with the accompanying drawings.

[0014] FIG. 1 is a flowchart showing a manufacturing process for a fiber-assembly material according to an embodiment of the present invention. FIG. 2 is a flowchart showing a manufacturing process for materials such as building materials and flooring materials according to an embodiment of the present invention. FIG. 3 shows a press using a mold for mass-producing a fiber-assembly material (denim resin board) according to an embodiment of the present invention. FIG. 4 shows a fiber-assembly material (denim resin board) with a three-layer structure according to an embodiment of the present invention. FIG. 5 shows a fiber-assembly material (denim resin board) with a three-layer structure according to another embodiment of the present invention. FIG. 6 shows a fiber-assembly material (denim resin board) according to yet another embodiment of the present invention. FIG. 7 shows test results for an embodiment of the present invention. FIG. 8 shows test results for an embodiment of the present invention. FIG. 9 shows supplementary diagrams for the test results of FIG. 8.

[0015] FIG. 1 is a flow chart showing a process for manufacturing a fibrous material according to an embodiment of the present invention.

[0016] In S1010, uniforms and other clothing that were scheduled to be discarded (hereinafter referred to as "recovered textile products") are defatted. Here, "recovered textile products" refers to recovered textile secondary processed products made from woven, knitted, and nonwoven fabrics, such as used clothing, towels, wrapping cloths, and curtains, from ordinary households, that is, rags that have been disintegrated and turned into fibers. In addition to rags, cutting waste and fiber waste (waste fibers) generated in the spinning process, knitting and weaving process, nonwoven fabric manufacturing process, and sewing process can also be used as recovered textile products.

[0017] Examples of fibers used in this embodiment include natural fibers and chemical fibers. Natural fibers include, for example, dietary fibers such as cotton and hemp, and animal fibers such as wool and silk. Chemical fibers include, for example, synthetic fibers such as nylon, and recycled fibers such as rayon. In a preferred embodiment of this embodiment, denim is used as the recycled fiber product.

[0018] Reclaimed wool refers to fibers that are made by collecting unwanted products and cutting scraps such as wool and cotton, putting them through a de-pilling machine or a de-pilling machine, and returning them to a cotton-like state.

[0019] In S1010, the depilated denim fibers are immersed in a resin adhesive. An example of the blending ratio is 80% denim fiber and 20% resin adhesive (1000 g of denim fiber, 200 g of resin adhesive). It is also possible to replace about 10% of the denim fiber with hemp (manufactured for the purpose of Japanese paper manufacturing). The use of hemp increases the rigidity of the fiber-assembly material produced in this example.

[0020] Here, when the amount of resin adhesive was kept roughly constant (200 g to 300 g), the amount of semi-wool denim fiber mixed in was examined, and the following results were obtained.

[0021] Less than 500g: The finished product will be too soft and will not harden (it is too light to be manufactured).

[0022] 500g to 800g: The product hardens, but the material becomes too soft, causing dents and cracks when dropped. This creates a manufacturing problem.

[0023] 800g to 1,300g: This is the appropriate value. In other words, there are no problems with the manufacturing process or the finish.

[0024] 1,300g or more: This is the appropriate value, but the manufacturing cost increases. It is fine for furniture and other decorative materials, but as a building material it deviates significantly from the market price. In other words, there are no manufacturing problems, but there are problems with costs, etc.

[0025] The above results are summarized in Table 1.

[0026]

[0027] In S1020, the recovered fibers are boiled. For example, the recovered fibers are placed in a boiling alkaline solution (approximately 100°C) and boiled for about 15 minutes. Examples of alkaline solutions include lime (calcium hydroxide), soda ash (sodium carbonate), or caustic soda (sodium hydroxide). By adjusting the boiling time, the amount of non-fibrous material remaining in the fibers can be changed, allowing the quality and texture of the fibers to be optimized. The boiling process removes oil from the recovered fibers and expands them, resulting in a more fibrous (softer) fiber.

[0028] In S1030, the recovered fibers are further processed by beating or refining. "Beat" refers to a process in which the recovered fibers are beaten with a club, hammer, or other beating machine to loosen the recovered fibers so that they can be easily dispersed into single fibers in water. In this embodiment, "beating" refers to at least breaking down the recovered fibers from a fabric state (i.e., a woven or knitted state) into a fibrous state, specifically reducing the average fiber length to 10 mm or less, preferably 5 mm or less. "Beating" refers to a process in which the single fibers constituting the recovered fibers are ground in water between blades (rotary blades in the case of a refiner, and a combination of a rotary blade and a fixed blade in the case of a beater) using a beating machine such as a beater or refiner.

[0029] In this example, the recovered fibers were boiled and then beaten or refined. However, in other examples, other treatments may be carried out in addition to boiling, refining, and refining. For example, bleaching and dusting may be carried out as necessary.

[0030] In S1040, a binder is mixed with the de-piled fiber and stirred. This strengthens the bonds between the denim fibers and creates the texture of Japanese paper. In particular, when a collection material is made from recovered denim fiber dyed with indigo (indigo blue), it is possible to obtain a collection material that takes advantage of the strength of denim threads in addition to the texture and feel of denim.

[0031] Empirically, the amount of binder mixed in is approximately 20% of the total volume (mass). If the binder ratio is too low, the strength of the aggregate will be weakened, and if there is too much binder, the design will be impaired. The binder material here is, for example, an aqueous adhesive containing vinyl acetate resin, which has adhesive properties such as wood glue. The aqueous adhesive can be solidified by evaporating the water contained in the aqueous adhesive through a process such as heat pressing, which will be described later.

[0032] Furthermore, the denim on the laminated surface may be mixed with an adhesive such as Selectibond. The main component of the adhesive that can be used in this example is urethane, which has good coating properties and excellent water and heat resistance, but adhesives containing components that can be expected to have similar effects may also be used.

[0033] Another example of a material that may be further mixed is PLA (Polylactic Acid) resin. PLA resin is a plastic material derived from plants such as starch found in corn and potatoes. While this manufacturing method, which uses a water-based adhesive, offers reasonable price and functionality, it poses the risk of swelling when submerged in water, making it unsuitable for outdoor use. Therefore, when manufacturing composite materials intended for building materials such as flooring (for outdoor use or in locations subject to flooding), a water-resistant resin, such as epoxy resin, can be used.

[0034] In S1050, the liquid resin produced in S1040 is poured into a mold and heat-pressed and molded to create a fiber-assembly material. In this example, heat pressing allows the assembly to be pressed using a flat mold. Heating conditions are determined appropriately depending on the type of fiber and binder, but heating may be performed at a temperature above the melting point of the aqueous adhesive used as the binder, preferably 10 to 30 degrees higher than the melting point of the aqueous resin. The heating time is approximately 50 to 70 minutes for a 300mm square flooring material, for example. While a temperature sufficient to melt the aqueous adhesive is sufficient, an unnecessarily high temperature can cause fiber degradation or melting. For example, for a 300mm square flooring material, a mold with dimensions of approximately 300 x 300 mm and a thickness of 15 mm can be used after molding. A mold with a size of 910 x 1820 mm can also be used to fit standard sizes such as plywood.

[0035] In the step S1050 of hot pressing and molding, a plurality of hot pressing and molding means may be used to produce a plurality of sheets of fiber-assembly material at once.

[0036] After the heat press molding, the laminate is cooled to a predetermined temperature in the cooling step S1060. The cooling method is not particularly limited. Since the heat press molding is performed by pressing with a concave-convex mold, the laminate solidifies in the same shape by cooling as it is, and therefore the pressed shape can be maintained even at room temperature.

[0037] In S1070, the hot-pressed and molded fiber aggregate is sanded using any abrasive material (grinder, sandpaper, etc.). The surface of the aggregate can be made smooth by sanding. Then, by sanding the painted upper surface, the surface of the aggregate can be made wet and glossy.

[0038] The fiber aggregate material that has been hot-pressed and molded in this embodiment can be given a variety of finishes, such as a finish that is simply polished, a finish that is polished and then painted to give it a glossy finish, or a finish that is lightly scraped with a metal brush to restore the unevenness of the material and then painted with a glossy finish.

[0039] Furthermore, if the heat-pressed and molded aggregate has a warp that is greater than a certain tolerance (for example, 2 mm), it may be polished to fit within the tolerance. Furthermore, the unevenness created by peeling off the surface during polishing may be used to create a texture.

[0040] The following describes alternative or additional steps to S1070. For example, all or part of the following steps (a) to (d) may be incorporated into the steps of this embodiment.

[0041] (a) The surface that has hardened by natural drying is polished.

[0042] (b) After applying an undercoat such as a sealer and letting it dry, another sealer is applied and dried. This process is repeated twice. In other words, by applying the sealer and drying it multiple times, not only can a thick coating be formed, but it can also be easily sanded after drying.

[0043] (c) Allow to dry thoroughly before sanding.

[0044] (d) After applying and drying a 5-minute water-based urethane matte, another 5-minute water-based urethane matte is applied and dried. In this example, a 5-minute water-based urethane matte is used simply to preserve the denim's color and texture without overly suppressing the gloss. Alternatives that offer similar effects may also be used. For example, the polished surface may be impregnated with resin for a finishing touch, which can accelerate the hardening of the surface in (e) described below. Examples of resins used in this example include Selecty and Kigatame. Selecty can harden currently available sheet-shaped cotton (cotton fibers flattened into a sheet). Kigatame can be applied as a finishing touch after hardening with Selecty, thereby hardening and enhancing the texture.

[0045] (e) The surface is hardened. Specifically, after (d), the strength is increased by repeating the (a) surface polishing process and (d) coating process. In this way, by repeating the process, the surface strength can be adjusted, and it is possible to create a finish suitable for different uses such as flooring and wall materials.

[0046] 2 is a flowchart showing a manufacturing process for materials such as building materials and flooring materials according to one embodiment of the present invention. More specifically, the flowchart shows a process for manufacturing building materials (flooring materials) from the fiber-integrated materials manufactured by the manufacturing process of FIG.

[0047] In step S2010, the surface of the produced fiber-assembly material is polished. Before the surface polishing, the fiber-assembly material may be cut into a size required for a building material (flooring material).

[0048] In S2020, the surface-polished fiber lumber is glossed (a wood hardener is applied to give it a glossy finish). Furthermore, wood hardener, i.e., by applying lacquer or synthetic resin to the cell walls inside the wood, the rigidity of the wood can be strengthened.

[0049] In S2030, tongue and groove processing (processing of uneven surfaces on the sides) is performed. Tongue and groove processing is a wood processing method used to join flooring and edge boards, and tongue and groove refers to the uneven processing on the side of the board. Generally, the convex part of the protrusion is called the male tongue and the concave part is called the female tongue.

[0050] In S2040, the entire surface is coated with a urethane paint.

[0051] By the above-described manufacturing process, a building material (flooring material) can be manufactured.

[0052] FIG. 3 shows a press machine using a die for mass production of fiber-reinforced material (denim resin board) according to one embodiment of the present invention.

[0053] By using the press of this embodiment, it is possible to press multiple layers of fiber aggregates with different thicknesses, preventing the formation of separate layers in the molded product. The maximum pressure of the press is 150 T. The press of this embodiment can press resin by sandwiching it between the upper and lower press dies, each of which is wired with an electric heating pipe. Pressing multiple resin boards at once enables mass production. A three-layer fiber aggregate (denim resin board) manufactured using such a press is shown in Figure 4.

[0054] 4 shows a three-layered fiberboard (denim resin board) according to one embodiment of the present invention. The fiberboard of this embodiment has a length (thickness) x width x height of T*300*300 mm, and a product thickness of T10 mm, T12 mm, T15 mm, or T20 mm.

[0055] The fiber-reinforced material (denim resin board) according to one embodiment of the present invention has a three-layer structure consisting of an upper layer, a middle layer, and a lower layer, and is specifically composed of an upper denim felt surface, a middle felt (miscellaneous felt), and a lower denim felt surface. Here, the miscellaneous felt is, for example, a general-purpose felt made from miscellaneous cotton, and is highly absorbent, thermoplastic (melts when heated and hardens when cooled), and highly processable.

[0056] The denim resin of this embodiment can be used for furniture (tops, seats, etc.) and small items, and an example of the specifications for this is as follows.

[0057] Hardness equivalent to walnut (air-dry specific gravity 0.63) Repeated impact test (55 kg weight is evenly applied, raised approximately 50 mm, and then dropped. This operation is repeated 8,000 times at a rate of 20 times per minute) Static strength test (1,300 N force is applied 10 times for 10 seconds) Heat resistance (heat resistant up to 80°) Waterproof (waterproof) UV test (no discoloration, etc.)

[0058] Although blue is shown as an example of the color of the denim in FIG. 4, it may be a color other than blue.

[0059] Figure 5 shows a three-layered fiber assembly (denim resin board) according to another embodiment of the present invention. The fiber assembly (denim resin board) according to one embodiment of the present invention has a three-layered structure consisting of an upper layer, a middle layer, and a lower layer. Specifically, it is composed of an (upper) denim felt surface, a middle felt (denim felt), and a (lower) denim felt surface. The middle felt of the fiber assembly (denim resin board) in Figure 5 is a felt manufactured by the manufacturing method described with reference to Figures 1 to 4, and the upper and lower felts may be general-purpose felts. In other words, the upper and lower felts may have different mechanical and functional performance requirements compared to the middle felt.

[0060] Fig. 6 shows a fiber-assembly material (denim resin board) according to yet another embodiment of the present invention. The fiber-assembly material (denim resin board) of this embodiment may use felt manufactured by the manufacturing method as described with reference to Figs. 1 to 4, for example.

[0061] Since the fiber aggregate of this example is composed of multiple layers, the rigidity of the fiber aggregate of this example can be determined by whether or not layer separation occurs during a rigidity test. Here, a rigidity (hardening) test for the three-layer fiber aggregate of this example will be described. The rigidity test for this example was performed by immersing the material in water at a temperature of 40 to 60°C after hot press molding and leaving it in a constant temperature bath (set at 50°C). The material was then removed from the constant temperature bath and left at room temperature for 61 hours. The weight was measured after leaving it for 67 hours. The test results are shown in Figure 7.

[0062] Furthermore, after the above measurements, the same fiber-assembly material was left for two weeks, and the state of water evaporation from the fiber-assembly material immersed in warm water was checked. The test results are shown in Figure 8. Figure 9 is a supplementary diagram of the test results in Figure 8.

[0063] Considering the above test results, it is thought that increasing the denim fiber ratio (amount) increases the water absorption rate (amount), which not only increases rigidity but also prevents layer separation. Furthermore, as the water absorption rate of the denim fiber increases, the change in thickness of the fiber-assembled material becomes small, and after a certain period of time, the moisture in the material is released to the outside, returning it to its original dry state (original thickness). Therefore, even when the fiber-assembled material of this example is used for furniture, etc., it can prevent product deterioration due to indoor humidity, etc.

[0064] Although the embodiments of the present invention have been described above, various alternatives, modifications, and variations are possible for those skilled in the art based on the above description, and the present invention includes the various alternatives, modifications, and variations described above within the scope of the present invention.

Claims

1. A method for producing a fiber material comprising the steps of: immersing a recycled fiber product in a resin adhesive, boiling and beating the immersed recycled fiber product to extract fiber matter; mixing the extracted fiber matter with an aqueous adhesive to produce a fiber material; hot pressing and molding the fiber material; and polishing the molded fiber material.

2. The method according to claim 1, characterized in that the blend ratio when the recycled fiber product is immersed in the resin adhesive is 80% recycled fiber product and 20% resin adhesive.

3. The method according to claim 2, wherein the amount of recycled fiber material mixed is 800 g to 1,300 g.

4. A method for producing building materials or flooring materials from the fiber aggregate produced according to claim 1, comprising the steps of: polishing the surface of the fiber aggregate; glossing the surface-polished fiber aggregate; tongue-and-groove the gloss-processed fiber aggregate; and applying a urethane coating to the entire surface of the tongue-and-groove fiber aggregate, wherein the surface polishing step and the coating step are repeated to produce a building material or flooring material.

5. The method according to claim 1, further comprising the steps of: after the polishing step, polishing the surface that has been naturally dried and hardened; applying an undercoat paint such as a sealer and drying it, then applying the sealer again and drying it; drying and then polishing; applying a 5-minute water-based urethane matte finish, drying it, then applying a 5-minute water-based urethane matte finish again and drying it; and hardening the surface.

6. A layered structured integrated material manufactured by pressing three layers, an upper layer, a middle layer, and a lower layer, the upper layer and the lower layer being fiber integrated materials manufactured as described in claim 1, and the middle layer being miscellaneous felt. The layered structured integrated material described in any one of claims 1 to 5.

7. A laminated material having a layered structure manufactured by pressing three layers, namely an upper layer, a middle layer, and a lower layer, characterized in that at least one of the upper layer, the middle layer, and the lower layer is a fiber laminated material manufactured as described in claim 1.

8. A fiber assembly manufactured according to claim 1.

9. The method of claim 2, wherein approximately 10% of said recycled fiber product is comprised of hemp.

Citation Information

Patent Citations

  • Manufacturing method of fiberboard and its manufacturing apparatus

    JP2005254695A

  • Method for manufacturing for fiber board

    JP2011126258A

  • Recycled board manufacturing method and recycled board

    WO2022254576A1