Resin molding composition, resin molded article, and housing

The thermoplastic resin composition with scaly glass particles and band-shaped glass fibers addresses warping and anisotropy issues in molded products, enhancing dimensional accuracy and strength for electronic component housings.

WO2024203941A1PCT designated stage expired Publication Date: 2024-10-03PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011462
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Molded products made from thermoplastic resin compositions often warp due to anisotropy caused by resin flow during injection molding, leading to dimensional inaccuracies and strength issues.

Method used

A thermoplastic resin composition incorporating scaly glass particles with a specific particle diameter to thickness ratio and band-shaped glass fibers with a defined aspect ratio, which reduces molding shrinkage rates and linear expansion coefficients, minimizing anisotropy and enhancing dimensional accuracy and strength.

Benefits of technology

The composition achieves improved dimensional accuracy and high strength in molded products by reducing anisotropy and molding shrinkage rates, making it suitable for housing electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011462_03102024_PF_FP_ABST
    Figure JP2024011462_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides: a resin molding composition that can provide moldings with an improved dimensional accuracy and can impart high strength to moldings; a resin molded article; and a housing. A resin molding composition according to the present disclosure comprises: a thermoplastic resin (A); scale-shaped glass particles (B) having a value of 100-400 for the ratio a / t of the average particle diameter a, which is the particle diameter at a cumulative value of 50% in the volume-based particle size distribution measured by laser diffraction scattering, to the average thickness t; and band-shaped glass fibers (C) having an aspect ratio of 1.5-5.0.
Need to check novelty before this filing date? Find Prior Art

Description

Molding resin composition, resin molded body, and housing

[0001] The present disclosure relates to a molding resin composition, a resin molded body, and a housing, and more particularly to a molding resin composition, a resin molded body that is a molded product of the molding resin composition, and a housing used to house electronic components.

[0002] Thermoplastic resins are relatively easy to process, and therefore can be used to produce molded articles by, for example, heating, melting, and molding the resin. For example, thermoplastic polyester resins are molded to produce molded articles such as housings and parts.

[0003] Patent Document 1 discloses a thermoplastic resin composition for laser welding containing a polyester resin (A), an epoxy resin (B), an inorganic filler (C), and short glass fibers (D) having an average fiber length of 100 μm or less. It also describes that this thermoplastic resin composition preferably contains 10 to 50 mass % of long glass fibers (E) having an average fiber length of 1 mm or more.

[0004] JP 2010-24396 A

[0005] An object of the present disclosure is to provide a molding resin composition, a resin molded article, and a housing that can improve the dimensional accuracy of molded articles and impart high strength to the molded articles.

[0006] A molding resin composition according to one embodiment of the present disclosure contains a thermoplastic resin (A), scaly glass particles (B) having a ratio a / t of 100 or more and 400 or less of an average particle diameter a, which is the particle diameter at 50% of the cumulative total in a volume-based particle size distribution measured by a laser diffraction scattering method, to an average thickness t, and ribbon-shaped glass fibers (C) having an aspect ratio of 1.5 or more and 5.0 or less.

[0007] A resin molded article according to one aspect of the present disclosure is a molded article obtained by molding the molding resin composition.

[0008] A housing according to an aspect of the present disclosure is used to house an electronic component. The housing includes the resin molded article.

[0009] Fig. 1A is a schematic perspective view showing an example of a housing according to one embodiment of the present invention. Fig. 1B is a cross-sectional view taken along line X-X in Fig. 1A. Fig. 2 is a schematic perspective view showing an example of the shape of scaly glass particles. Fig. 3 is a schematic perspective view showing an example of the shape of ribbon-shaped glass fibers.

[0010] 1. Overview First, the background to the configuration of the present disclosure will be described.

[0011] Molded articles are obtained from resin compositions containing thermoplastic resins, for example, by injection molding. To improve the strength of the molded articles, reinforcing materials such as fillers are blended into the resin compositions. For example, Patent Document 1 proposes the combined use of short glass fibers and long glass fibers.

[0012] However, according to the inventors' own investigations, molded articles made from resin compositions containing thermoplastic resins sometimes warp, resulting in deviations in the dimensions of the molded articles from the desired values. After detailed investigations into the cause of this, the inventors discovered that the warpage is caused by anisotropy of the molded articles due to resin flow during injection molding of the resin composition. Resin flow causes an orientation phenomenon in which the longitudinal direction of glass fibers in the resin composition aligns with the resin flow direction. This results in anisotropy in the molded articles, in which the mold shrinkage rate and linear expansion coefficient differ greatly between the resin flow direction and the direction perpendicular to the resin flow direction. This anisotropy causes warpage of the molded articles. The mold shrinkage rate refers to the shrinkage rate of a molded article that shrinks due to cooling when the resin composition is molded in the mold. Therefore, the inventors conducted extensive research to achieve both improved dimensional accuracy and high strength in molded articles, and have completed the molding resin composition of the present disclosure.

[0013] That is, the molding resin composition of this embodiment contains a thermoplastic resin (A), scaly glass particles (B), and ribbon-shaped glass fibers (C). When the average thickness of the scaly glass particles (B) is t and the average particle diameter of the scaly glass particles (B) is a, the ratio represented by a / t is 100 or more and 400 or less. The average particle diameter is the particle diameter at 50% cumulative in a volume-based particle size distribution measured by a laser diffraction scattering method, i.e., the median diameter. The aspect ratio of the ribbon-shaped glass fiber (C) is 1.5 or more and 5.0 or less. The aspect ratio of the ribbon-shaped glass fiber (C) is a value represented by w / d, where d is the average minor axis of a cross section perpendicular to the longitudinal direction of the ribbon-shaped glass fiber (C) and w is the average major axis of this cross section. Thus, the molding resin composition of this embodiment can achieve excellent dimensional accuracy in molded articles and can impart high strength to the molded articles. Specifically, the molding resin composition contains both scaly glass particles (B) having a ratio a / t of the average particle diameter to the average thickness of 100 to 400 and band-shaped glass fibers (C) having an aspect ratio of 1.5 to 5.0. This allows the molding resin composition to have a reduced molding shrinkage and linear expansion coefficient in a direction perpendicular to the resin flow direction when molded. This reduces the anisotropy of the molding shrinkage and linear expansion coefficient in the molded product. The molding resin composition of this embodiment therefore allows the molded product to have excellent dimensional accuracy and improved strength.

[0014] 2. Details The molding resin composition, resin molded body, and housing of this embodiment will be described in detail below, with reference to the drawings as necessary. However, the embodiment described below is merely one of various embodiments of the present disclosure. The following embodiment can be modified in various ways depending on the design as long as the object of the present disclosure is achieved. Furthermore, each figure is a schematic diagram, and the ratios of the sizes and thicknesses of the components in each figure do not necessarily reflect the actual dimensional ratios.

[0015] [Molding Resin Composition] As described above, the molding resin composition of this embodiment contains a thermoplastic resin (A), glass flake particles (B), and ribbon-shaped glass fibers (C).

[0016] Components that can be contained in the molding resin composition of this embodiment will be specifically described.

[0017] <Thermoplastic Resin> The thermoplastic resin (A) can be any compound having appropriate thermoplastic properties, and examples thereof include polyester resins.

[0018] The polyester resin may contain a crystalline component. In the present disclosure, a crystalline component refers to a resin having a crystalline portion in which molecular chains are regularly arranged at or below the crystallization temperature, or a resin having a melting point. The polyester resin may contain an amorphous component that does not have crystallinity.

[0019] The polyester resin preferably contains at least one compound (polymer) selected from the group consisting of polybutylene terephthalate-based resins, polyethylene terephthalate-based resins, and polyethylene naphthalate-based resins.

[0020] The thermoplastic resin (A) preferably contains at least one of a polybutylene terephthalate resin (A1) and a polyethylene terephthalate resin (A2), and preferably contains both a polybutylene terephthalate resin (A1) and a polyethylene terephthalate resin (A2). When the thermoplastic resin (A) contains a polybutylene terephthalate resin (A1), the flowability of the molding resin composition during molding can be improved. When the molding resin composition contains a polyethylene terephthalate resin (A2) in addition to the polybutylene terephthalate resin (A1), the molding shrinkage of the molding resin composition can be maintained low because the crystallization rate of the polybutylene terephthalate resin (A1) is relatively fast, while the crystallization rate of the polyethylene terephthalate resin (A2) is relatively slow. Therefore, by including a molding resin composition containing a polybutylene terephthalate resin (A1) and a polyethylene terephthalate resin (A2), dimensional accuracy can be further improved.

[0021] When the thermoplastic resin (A) contains both a polybutylene terephthalate resin (A1) and a polyethylene terephthalate resin (A2), the mass ratio of the polybutylene terephthalate resin (A1) to the polyethylene terephthalate resin (A2) ((A1) / (A2)) is preferably within a range of 51 / 49 to 90 / 10, which can further reduce the molding shrinkage of the molding resin composition.

[0022] Examples of the polybutylene terephthalate resin (A1) include a polymer obtained by polymerizing, by a polymerization method such as polycondensation reaction, a reactive mixture containing a copolymerizable component (also referred to as a first copolymerizable component) containing terephthalic acid or an ester-forming derivative thereof and a copolymerizable component (also referred to as a second copolymerizable component) containing 1,4-butanediol or an ester-forming derivative thereof.

[0023] The first copolymerizable component is not limited to the above and may further include an appropriate polycarboxylic acid component. The second copolymerizable component is not limited to the above and may further include an appropriate polyol component. Examples of the polycarboxylic acid component include at least one compound selected from the group consisting of isophthalic acid, naphthalenedicarboxylic acid, adipic acid, sebacic acid, dodecanedioic acid, and oxalic acid. Examples of the polyol component include at least one compound selected from the group consisting of ethylene glycol, propylene glycol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, polyethylene glycol, poly-1,3-propylene glycol, and polytetramethylene glycol.

[0024] Specific examples of the polybutylene terephthalate resin (A1) include at least one polymer selected from the group consisting of polybutylene terephthalate (PBT), polybutylene (terephthalate / isophthalate), polybutylene (terephthalate / adipate), polybutylene (terephthalate / sebacate), polybutylene (terephthalate / decanedicarboxylate), polybutylene (terephthalate / naphthalate), and poly(butylene / ethylene) terephthalate. In the above, " / " means a copolymer; for example, "polybutylene (A / B)" is a polycondensate of 1,4-butanediol with A and B.

[0025] Examples of the polyethylene terephthalate resin (A2) include polymers obtained by a polymerization method such as polycondensation of a reactive mixture containing terephthalic acid or an ester-forming derivative thereof and ethylene glycol or an ester-forming derivative thereof. Other copolymerization components may be used as copolymerization components within the scope of the copolymerization that does not impair the properties of the polyethylene terephthalate resin (A2). Examples of such other copolymerization components include those similar to the copolymerization components (first copolymerization component and second copolymerization component) in the polybutylene terephthalate resin (A1).

[0026] The ratio of the thermoplastic resin (A) to the total solid content of the molding resin composition is preferably 35% by mass or more and 85% by mass or less. When the ratio of the thermoplastic resin (A) to the total solid content of the molding resin composition is 35% by mass or more, the flowability of the molding resin composition can be maintained well when molding. Furthermore, when the ratio of the thermoplastic resin (A) to the total solid content of the molding resin composition is 85% by mass or less, the high strength of the molded product of the molding resin composition can be maintained well. In the present disclosure, the "total solid content of the molding resin composition" refers to the total amount of components that may be contained in the molding resin composition, excluding volatile components. The ratio of the thermoplastic resin (A) to the total solid content of the molding resin composition is more preferably 60% by mass or more, and even more preferably 65% ​​by mass or more. The ratio of the thermoplastic resin (A) to the total solid content of the molding resin composition is more preferably 80% by mass or less, and even more preferably 75% by mass or less.

[0027] (Scaly Glass Particles) The molding resin composition contains scaly glass particles (B).

[0028] In the present disclosure, the term "scaly glass particles" refers to a flat glass filler material. For example, as shown in FIG. 2, the scaly glass particles (B) have a polygonal shape in a planar view, and have a thickness of, for example, t x , particle diameter is a x The particle diameters in FIG. 2 are shown merely for convenience.

[0029] The shape of the scaly glass particles (D) in a plan view may be a polygonal shape such as a triangle or a rectangle, or may be a circular shape, an elliptical shape, a sector shape, etc. The scaly glass particles (B) may have a flat shape and a layer structure.

[0030] The aspect ratio a / t of the scaly glass particles (B) of this embodiment, which is the ratio of the average particle diameter to the average thickness, where t is the average thickness and a is the average particle diameter, is 100 or more and 400 or less. When the molding resin composition contains scaly glass particles (B) satisfying the above ratio a / t, the scaly glass particles (B) having a relatively large surface area and a flat shape can be stacked in the molding resin composition. This can reduce the molding shrinkage of the molded product in the flow direction (parallel direction) and perpendicular direction of the molding resin composition during molding. Furthermore, the scaly glass particles (B) can also reduce the linear expansion coefficient of the molded product in the parallel direction and perpendicular direction. Therefore, the molded product is less likely to exhibit anisotropy.

[0031] The average particle size of the scaly glass particles (B) is the cumulative 50% particle size (D50) in the volume-based particle size distribution measured by the laser diffraction scattering method as described above. The average thickness of the scaly glass particles (B) is the arithmetic mean value of the thicknesses of three or more particles arbitrarily selected from the scaly glass particles (B) measured using a scanning electron microscope (SEM).

[0032] The average particle size of the scaly glass particles (B) is preferably 100 μm or more and 300 μm or less. If the average particle size of the scaly glass particles (B) is within the above range, the molding shrinkage rate in the parallel and perpendicular directions of the molded product can be further reduced. The average particle size of the scaly glass particles (B) is more preferably 110 μm or more, and even more preferably 130 μm or more. The average particle size of the scaly glass particles (B) is more preferably 200 μm or less, and even more preferably 180 μm or less.

[0033] The average thickness of the scaly glass particles (B) is preferably 0.3 μm or more and 1.5 μm or less. In this case, anisotropy of the molded product is less likely to occur. The average thickness of the scaly glass particles (B) is more preferably 0.1 μm or more, and even more preferably 0.5 μm or more. Furthermore, the average thickness of the scaly glass particles (B) is more preferably 1.2 μm or less, and even more preferably 0.8 μm or less.

[0034] In this embodiment, the scaly glass particles (B) have anisotropy, but the anisotropy is sufficiently smaller than that of fibrous components such as scaly glass particles, cylindrical glass fibers, or ribbon-shaped glass fibers not satisfying the a / t ratio of the present disclosure, or inorganic fillers not satisfying the w / d ratio of the present disclosure. Therefore, the scaly glass particles (B) particularly contribute to improving the dimensional accuracy when molding a molding resin composition, and can maintain good strength of the molded product. The anisotropy of the scaly glass particles (B) here refers to the difference in orientation characteristics between the parallel direction parallel to the longitudinal direction and the perpendicular direction perpendicular thereto. The smaller the difference in orientation characteristics between the parallel direction and the perpendicular direction, the lower the anisotropy.

[0035] The proportion of the scaly glass particles (B) relative to the total solid content of the molding resin composition is preferably 10% by mass or more and 40% by mass or less. When the proportion is 10% by mass or more, the molding resin composition can maintain dimensional accuracy during molding, and the strength of the resin molding 1 can be further increased. When the proportion is 40% by mass or less, the dimensional accuracy of the molding resin composition during molding can be further increased. The proportion of the scaly glass particles (B) is more preferably 15% by mass or more, and even more preferably 20% by mass or more. Furthermore, the proportion of the scaly glass particles (B) is more preferably 35% by mass or less, and even more preferably 30% by mass or less.

[0036] The material of the scaly glass particles (B) is not particularly limited, but the material of the scaly glass particles (B) includes, for example, at least one selected from the group consisting of E glass, A glass, and C glass. In particular, the material of the scaly glass particles (B) preferably includes E glass.

[0037] (Strip-Shaped Glass Fiber) In this embodiment, the molding resin composition contains a strip-shaped glass fiber (C).

[0038] The "strip-shaped glass fiber" in the present disclosure refers to a glass fibrous filler material having a flattened cylindrical shape. The flattened cylindrical shape is, for example, a cylindrical shape crushed in one direction. Therefore, the strip-shaped glass fiber (C) is distinguished from the cylindrical glass fiber. As shown in FIG. 3, an example of the strip-shaped glass fiber (C) is a fiber having a cross section perpendicular to the longitudinal direction that has a flattened circular shape, and a minor axis of, for example, d x, the major axis is longer than the minor axis, x , and has a minor diameter, a major diameter, and a fiber length, where L is the fiber length.

[0039] In this embodiment, the aspect ratio of the band-shaped glass fiber (C) is 1.5 or more and 5.0 or less. By containing the band-shaped glass fiber (C) satisfying the above aspect ratio, the molding resin composition can contribute to reducing the molding shrinkage rate in the parallel and perpendicular directions of the molded product. In addition, the band-shaped glass fiber (C) can also reduce the linear expansion coefficient of the molded product of the molding resin composition. And, by blending the band-shaped glass fiber (C) together with the above-mentioned scaly glass particles (B), it can also contribute to improving the physical properties of the molded product, particularly improving the mechanical strength.

[0040] The average minor axis and the average major axis of the cross section perpendicular to the longitudinal direction of the ribbon-shaped glass fiber (C) can be obtained, for example, by measuring as follows. An SEM image of the ribbon-shaped glass fiber (C) is measured at a magnification of 800 times under the condition of an acceleration voltage of 15 kV using a scanning electron microscope. The minor axis and the major axis of each of 50 fibers in the ribbon-shaped glass fiber (C) are measured. The arithmetic mean values ​​of the minor axes and the arithmetic mean values ​​of the major axes are the average minor axis and the average major axis of the ribbon-shaped glass fiber (C), respectively. The ribbon-shaped glass fiber (C) is distinguished from cylindrical glass fibers. Note that the cross section of the cylindrical glass fiber perpendicular to the longitudinal direction of the fiber has a substantially circular shape, and the aspect ratio of this cross section is about 1.0. In this embodiment, the ribbon-shaped glass fiber (C) may have anisotropy, but the anisotropy is sufficiently smaller than that of cylindrical glass fibers, ribbon-shaped glass fibers not satisfying the aspect ratio of the present disclosure, fibrous glass components such as inorganic fillers, etc. Therefore, the strip-shaped glass fiber (C) can particularly contribute to improving the dimensional accuracy of the molded product when molding the molding resin composition, and can improve the strength of the molded product. Note that the anisotropy of the strip-shaped glass fiber (C) here refers to the difference in orientation characteristics between the parallel direction parallel to the longitudinal direction of the strip-shaped glass fiber (C) and the vertical direction perpendicular thereto. The smaller the difference in orientation characteristics between the parallel direction and the vertical direction, the lower the anisotropy can be said to be.

[0041] The average minor axis of the cross section perpendicular to the longitudinal direction of the strip-shaped glass fiber (C) is preferably 3 μm or more and 15 μm or less. In this case, the anisotropy of the molded product is less likely to occur, so the dimensional accuracy of the molded product can be further improved, and the strength of the molded product can be further improved. The average major axis of the cross section perpendicular to the longitudinal direction of the strip-shaped glass fiber (C) is not particularly limited as long as it satisfies the above aspect ratio.

[0042] The fiber length of the strip-shaped glass fiber (C) in the molding resin composition is preferably 150 μm or more and 300 μm or less. In this case, the dimensional accuracy of the molding resin composition can be maintained well, and the strength of the molded product can be further improved. The fiber length of the strip-shaped glass fiber (C) refers to the longitudinal length (length 1 in FIG. 3). Note that the "fiber length of the strip-shaped glass fiber (C)" here refers to the fiber length of the strip-shaped glass fiber (C) in the molding resin composition when the molding resin composition is prepared, and is different from the dimension of the strip-shaped glass fiber (C) as a raw material before preparing the molding resin composition. The fiber length of the strip-shaped glass fiber as a raw material before preparing the molding resin composition is, for example, 1.0 mm or more and 5.0 mm or less.

[0043] The proportion of the strip-shaped glass fiber (C) relative to the total solid content of the molding resin composition is preferably 5% by mass or more and 20% by mass or less. When the proportion of the strip-shaped glass fiber (C) is 5% by mass or more, the dimensional accuracy of the molding resin composition can be maintained at a good level, and when it is 20% by mass or less, the mechanical strength of the resin molding 1 can be further increased. The proportion of the strip-shaped glass fiber (C) is more preferably 7% by mass or more. The proportion of the strip-shaped glass fiber (C) is more preferably 15% by mass or less.

[0044] <Epoxy Compound> The molding resin composition preferably further contains an epoxy compound (D). The epoxy compound (D) reacts with a portion of the thermoplastic resin (A) in the molding resin composition, thereby imparting hydrolysis resistance to the molding resin composition and its molded article. For example, when the thermoplastic resin (A) contains a polyester resin, prolonged exposure to high-temperature water, high-temperature and high humidity, or an alkaline environment may hydrolyze the ester groups of the polyester resin. The epoxy compound (D) of this embodiment has at least two epoxy groups per molecule. The epoxy compound (D) preferably has an epoxy equivalent of 150 g / eq. or more and 250 g / eq. or less. When the molding resin composition contains the epoxy compound (D), if the epoxy equivalent of the epoxy compound (D) is 150 g / eq. or more, the reaction between the thermoplastic resin (A) and the epoxy resin (B) can be appropriately suppressed when the components of the molding resin composition are kneaded. Therefore, the viscosity of the molding resin composition is prevented from increasing excessively, and good flowability of the molding resin composition can be ensured. Furthermore, when the epoxy equivalent of the epoxy compound (D) is 250 g / eq. or less, even if the thermoplastic resin (A) in the molding resin composition contains a component that is easily hydrolyzed, hydrolysis of the thermoplastic resin (A) can be prevented.

[0045] Examples of the epoxy compound (D) include at least one resin selected from the group consisting of bisphenol epoxy resins, novolac epoxy resins, alicyclic epoxy resins, glycidyl ethers, glycidyl esters, glycidyl amines, and heterocyclic epoxy resins. Specific examples of bisphenol epoxy resins include bisphenol A epoxy resins, bisphenol F epoxy resins, and bisphenol S epoxy resins. Examples of novolac epoxy resins include phenol novolac epoxy resins, cresol novolac epoxy resins such as o-cresol novolac epoxy resins, bisphenol A novolac epoxy resins, and dicyclopentadiene novolac epoxy resins. Examples of alicyclic epoxy resins include 3,4-epoxy-6-methylcyclohexylmethyl-3,4-epoxy-6-methylcyclohexanecarboxylate, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, and 1-epoxyethyl-3,4-epoxycyclohexane. Examples of glycidyl esters include phthalic acid diglycidyl ester, tetrahydrophthalic acid diglycidyl ester, and dimer acid glycidyl ester. Examples of glycidyl amines include tetraglycidyldiaminodiphenylmethane, triglycidyl p-aminophenol, and N,N-diglycidylaniline. Examples of heterocyclic epoxy resins include 1,3-diglycidyl-5,5-dimethylhydantoin and triglycidyl isocyanurate. The epoxy compound (D) may be at least one compound selected from the group consisting of the above. The epoxy compound (D) preferably contains a cresol novolac epoxy resin, and more preferably contains an o-cresol novolac epoxy resin. In this case, the hydrolysis resistance of the resin molded body 1 produced from the molding resin composition can be further improved.

[0046] The epoxy compound (D) may contain an epoxy analogue other than those mentioned above, so long as it has two or more epoxy groups in one molecule and an epoxy equivalent of 150 g / eq. or more and 250 g / eq. or less. For example, the epoxy compound (D) may contain a compound having at least one oxetane group in one molecule.

[0047] The proportion of the epoxy compound (D) relative to the total solid content of the molding resin composition is preferably 0.5% by mass or more and 7% by mass or less, which can satisfactorily improve the flowability of the molding resin composition during molding.

[0048] The proportion of the epoxy compound (D) relative to the total solid content of the molding resin composition is preferably 0.5% by mass or more, and even more preferably 1% by mass or more, and more preferably 5% by mass or less, and even more preferably 2% by mass or less.

[0049] (Other Components) The molding resin composition may contain other components, such as additives, as long as the addition does not depart from the scope of the present disclosure. Examples of the additives include inorganic fillers, mold release agents, thickeners, antifoaming agents, heat stabilizers, antioxidants, lubricants, and UV stabilizers.

[0050] The inorganic filler can further improve the mechanical strength of the resin molded body 1 produced from the molding resin composition. In the present disclosure, the inorganic filler is distinguished from the above-mentioned scaly glass particles (B) and ribbon-shaped glass fibers (C). That is, the inorganic filler does not include the scaly glass particles (B) and ribbon-shaped glass fibers (C). Materials for the inorganic filler include, for example, inorganic oxides, inorganic hydroxides, inorganic nitrides, and inorganic carbides. Specific examples of inorganic filler materials include at least one of talc, aluminum hydroxide, alumina (aluminum oxide), silica, mica, clay, wollastonite, titanium oxide, barium titanate, silicon nitride, aluminum nitride, boron nitride, silicon carbide, zirconium carbide, and magnesium hydroxide.

[0051] The form of the inorganic filler is not particularly limited as long as it does not deviate from the object of the present disclosure, and the inorganic filler may be, for example, in powder form or granular form.

[0052] When the molding resin composition contains an inorganic filler, the proportion of the inorganic filler relative to the total solid content of the molding resin composition is, for example, 0.5% by mass or more and 5% by mass or less.

[0053] Examples of the release agent include fatty acids such as stearic acid, montanic acid, and myristic acid, metal salts of fatty acids such as zinc stearate and calcium stearate, surfactants such as phosphate esters, carnauba wax, and polyethylene wax.

[0054] Examples of the thickener include an oxide or hydroxide of at least one divalent metal selected from the group consisting of magnesium, calcium, zinc, and strontium, and an acrylic polymer.

[0055] The antifoaming agent may be, for example, a silicone-based antifoaming agent, and specifically, there are oil-type, solution-type, powder-type, emulsion-type, and the like.

[0056] The method for preparing the molding resin composition is not particularly limited, but it can be prepared, for example, as follows.

[0057] First, a mixture is prepared by adding the thermoplastic resin (A), the epoxy compound (D) if necessary, and appropriate additives to a container and mixing them. Mixing can be performed using a mixer such as a tumbler mixer or a Henschel mixer, or a blender. The mixing time is not particularly limited as long as the components are mixed uniformly, and may be any appropriate time. Next, the mixture is kneaded while being heated using an appropriate device. Examples of devices for kneading include a twin-screw extrusion kneader, a kneader, a roll, a disperser, an azihomogenizer, a planetary mixer, and a crusher.

[0058] Subsequently, the mixture is melted, and the scaly glass particles (B), the ribbon-shaped glass fibers (C), and, if necessary, appropriate additives are added to the molten mixture, and the mixture is further kneaded to obtain a kneaded product. The kneading temperature can be appropriately adjusted depending on the composition of the molding resin composition, etc. The kneading temperature can be, for example, 220°C or higher and 280°C or lower. The kneading time is not particularly limited as long as the molding resin composition can be kneaded uniformly.

[0059] The kneaded mixture is then cooled to an appropriate temperature to solidify, thereby obtaining a molding resin composition.

[0060] The molding resin composition may be cut into pellets using an appropriate pelletizing device such as a pelletizer. In this case, the size of the molding resin composition pellets is not particularly limited, but may be, for example, 2 mm or more and 4 mm or less. In this way, a molding resin composition in pellet form can be obtained.

[0061] [Resin Molded Body and Housing] In this embodiment, the resin molded body 1 can be produced by molding the molding resin composition prepared above. In other words, the resin molded body 1 is a molded article containing the molding resin composition described above. The resin molded body 1 is produced, for example, by heating and melting the molding resin composition to form it.

[0062] As described above, the resin molded body 1 contains the molding resin composition, and therefore the molded resin molded body 1 can have excellent dimensional accuracy and high strength. The resin molded body 1 can be used to house electronic components and the like that require high dimensional accuracy. Therefore, the molding resin composition and the resin molded body 1 can be used as a housing 10 that houses electronic components and the like. Specifically, the resin molded body 1 can be used as a housing 10 that seals electrical circuits and the like in electronic components such as semiconductor devices 100, including electronic control components such as engine control units (ECUs) and sensors. However, the uses of the resin molded body and the housing are not limited to these.

[0063] To produce the resin molded body 1, a moldable resin composition can be molded into an appropriate shape by, for example, injection molding to obtain the resin molded body 1. Specific examples of injection molding methods include high-speed injection molding and injection compression molding. High-speed injection molding and injection compression molding have excellent moldability. The conditions for injection molding may be adjusted appropriately depending on the composition and physical properties of the moldable resin composition, and the resin molded body 1 to be produced.

[0064] The injection compression molding method can be carried out by any suitable operation, for example, by injecting a molten molding resin composition into the injection molding mold while the mold is opened slightly wider than the thickness dimension of the resin molding 1 to be produced, thereby filling the thin-walled portion with the molding resin composition, and then closing the mold, thereby producing a resin molding 1 having the desired shape.

[0065] The housing 10 of this embodiment will be described using a specific example, but the housing is not limited to the uses described below.

[0066] The resin molded body 1 of this embodiment can be used as the entire container for placing and sealing a device such as a semiconductor device 100 inside, or as a housing 10, which is a portion of the container. For example, as shown in FIGS. 1A and 1B , the housing 10 has a housing main body 11 including, for example, the resin molded body 1, and a lid 12. The housing main body 11 and the lid 12 can include molded articles of a molding resin composition. That is, both the housing main body 11 and the lid 12 can be the resin molded body 1. The housing main body 11 has a recess. The housing 10 shields the internal space from the outside. In the housing 10, the housing main body 11 functions as a main body having a recess, and the lid 12 functions as a lid that closes the recess in the housing main body 11. When the recess in the housing main body 11 is closed by the lid 12, the space surrounded by the inner surface of the recess and the lid becomes the internal space. The semiconductor device 100 or the like can be placed in the internal space. 1A and 1B , as a specific example, a semiconductor device 100 is disposed in the internal space of a housing 10 produced by overlapping and welding a lid portion 12 to a housing body portion 11. The semiconductor device 100 includes a substrate 120, a mounted component 130, and a sealing material 140. The substrate 120 includes conductor wiring 121. The mounted component 130 includes a bump electrode 131, which is mounted to the substrate 120 via solder 132 on the conductor wiring 121. The sealing material 140 seals at least a portion of the gap between the substrate 120 and the mounted component 130. The housing 10 can be produced by, for example, appropriately bonding together molded components (in the above example, the housing body portion 11 and the lid portion 12) produced from a molding resin composition. While it has been described above that housing 10 has housing body 11 and lid 12, and that housing body 11 and lid 12 are resin molded bodies 1 made from a molding resin composition, housing 10 may, for example, consist of housing body 11 only, or may consist of housing body 11 and a lid member (not shown) different from lid 12. Furthermore, the members arranged inside housing 10 are not limited to electronic devices such as semiconductor device 100, and may be appropriate members depending on the purpose.

[0067] [Physical properties of molding resin composition] The molding shrinkage of the molding resin composition in the parallel and perpendicular directions is preferably 0.8% or less. The molding shrinkage of the molding resin composition is more preferably 0.6% or less, and even more preferably 0.5% or less. There is no particular lower limit for the molding shrinkage of the molding resin composition. The molding shrinkage can be measured and calculated based on the method described in the Examples "(3-1) Mold shrinkage and anisotropy" below.

[0068] The anisotropy of the resin molded body 1 with respect to molding shrinkage is preferably 0.2 or less. This can make it possible to make thermoplastic resin molded articles less susceptible to warping. That is, the dimensional accuracy of molded articles produced from the molding resin composition can be further improved. The anisotropy of the resin molded body 1 with respect to molding shrinkage is more preferably less than 0.2, and ideally, the anisotropy of the resin molded body 1 is 0. In the present disclosure, the anisotropy of molding shrinkage can be calculated from a value calculated from the molding shrinkage of the resin molded body 1 measured in accordance with ISO 294-4. Specifically, a flat plate-shaped resin molded body 1 is produced, and the molding shrinkage of the resin molded body 1 is measured in each of the perpendicular and parallel directions to obtain the molding shrinkage of the perpendicular direction and the molding shrinkage of the parallel direction. The value (absolute value) calculated from the difference between these molding shrinkages is defined as the anisotropy with respect to molding shrinkage. In this case, the parallel direction is a direction parallel to the longitudinal direction of the resin molded body 1 , and the vertical direction is a direction perpendicular to the parallel direction and the thickness direction of the resin molded body 1 .

[0069] The linear expansion coefficient of the molding resin composition in the parallel direction in the temperature range of 90°C to 120°C is preferably less than 100 ppm / °C. The linear expansion coefficient of the molding resin composition in the perpendicular direction in the temperature range of 90°C to 120°C is preferably more than 50 ppm / °C and not more than 100 ppm / °C. The linear expansion coefficient in this embodiment can be measured by the method described in "(3-2) Linear expansion coefficient and anisotropy" in the Examples below. In this disclosure, the linear expansion coefficient at the above temperatures is specified for evaluating the linear expansion coefficient.

[0070] The anisotropy of the linear expansion coefficient of the resin molded body 1 is preferably less than 120. In this case, warping of the thermoplastic resin molded body can be reduced. That is, the dimensional accuracy of the molded body produced from the molding resin composition can be further improved. In the present disclosure, the anisotropy of the linear expansion coefficient is obtained by measuring the linear expansion coefficient in the above-mentioned perpendicular and parallel directions in a temperature range of 90°C to 120°C to obtain the linear expansion coefficient in the perpendicular direction and the linear expansion coefficient in the parallel direction, and defining the value (absolute value) calculated from the difference between these linear expansion coefficients as the anisotropy. The anisotropy of the linear expansion coefficient of the resin molded body 1 is more preferably 120 or less, and even more preferably 70 or less. In this case, the parallel direction is the direction parallel to the longitudinal direction of the resin molded body 1, and the perpendicular direction is the direction perpendicular to the parallel direction and the thickness direction of the resin molded body 1.

[0071] The flexural strength of the molded article of the molding resin composition is preferably greater than 120 MPa. In this case, the molded article of the molding resin composition has excellent mechanical strength. The flexural strength of the molded article of the molding resin composition is more preferably 150 MPa or more, and even more preferably 170 MPa or more. The flexural strength is obtained by measuring a test piece of the dumbbell molded article using a universal testing machine (autograph) in accordance with ISO 527-1 and ISO 27-2. The specific measurement method can be measured by the method described in Example "(3-3) Flexural Strength" below.

[0072] The flexural modulus of the molded article of the molding resin composition is preferably greater than 6.0 GPa. In this case, the molded article of the molding resin composition has excellent mechanical strength. The flexural modulus of the molded article of the molding resin composition is more preferably 8.0 GPa or more, and even more preferably 10.0 GPa or more. The flexural modulus is obtained by measuring a test piece of a dumbbell molded article using a universal testing machine (autograph) in accordance with ISO 527-1 and ISO 527-2. Specific measurement methods can be described in the "(3-4) flexural modulus" section of the Examples below.

[0073] The deflection temperature under load of a molded article of the molding resin composition is preferably greater than 150°C. In this case, the molded article of the molding resin composition has excellent heat resistance. The deflection temperature under load of the molding resin composition is more preferably 160°C or higher, even more preferably 170°C or higher, and even more preferably 190°C or higher. The deflection temperature under load is obtained by measuring a test piece using a heat distortion tester in accordance with ISO 75-2. A specific measurement method can be described in the example "(3-5) Deflection Temperature under Load" below.

[0074] 3. Summary As is apparent from the above embodiments, the present disclosure includes the following aspects.

[0075] The molding resin composition of the first embodiment contains a thermoplastic resin (A), scaly glass particles (B) having a ratio a / t of 100 or more and 400 or less of an average particle diameter a, which is the particle diameter at 50% of the cumulative total in a volume-based particle size distribution measured by a laser diffraction scattering method, to an average thickness t, and strip-shaped glass fibers (C) having an aspect ratio of 1.5 or more and 5.0 or less.

[0076] According to this embodiment, the dimensional accuracy of the molded product can be improved, and high strength can be imparted to the molded product.

[0077] In a second aspect, in the first aspect, the average particle diameter is 100 μm or more and 300 μm or less, and the average thickness is 0.3 μm or more and 1.5 μm or less.

[0078] According to this embodiment, the molding shrinkage rate of the molded product in the flow direction (parallel direction) and the perpendicular direction when molding the molding resin composition can be further reduced, making it more difficult for the molded product to become anisotropic.

[0079] In a third aspect, in the first or second aspect, the fiber length of the strip-shaped glass fiber (C) is 150 μm or more and 300 μm or less.

[0080] According to this embodiment, the dimensional accuracy of the molded product can be maintained at a good level, and the strength of the molded product can be further improved.

[0081] In a fourth aspect, in any one of the first to third aspects, the average minor axis of the cross section of the strip-shaped glass fiber (C) perpendicular to the longitudinal direction is 3 μm or more and 15 μm or less.

[0082] According to this embodiment, the molded product can be made less likely to have anisotropy, the dimensional accuracy of the molded product can be improved, and the strength of the molded product can be improved.

[0083] In a fifth aspect, in any one of the first to fourth aspects, the proportion of the thermoplastic resin (A) relative to the total solid content of the molding resin composition is 35% by mass or more and 85% by mass or less.

[0084] According to this embodiment, the dimensional accuracy of the molded product can be maintained well, and the high strength of the molded product can be maintained well.

[0085] In a sixth aspect, in any one of the first to fifth aspects, the proportion of the scaly glass particles (B) relative to the total solid content of the molding resin composition is 10% by mass or more and 40% by mass or less.

[0086] According to this embodiment, the dimensional accuracy of the molded product can be maintained and the strength of the molded product can be further increased. In this case, the dimensional accuracy of the molded product can be further increased.

[0087] In a seventh aspect, in any one of the first to sixth aspects, the proportion of the band-shaped glass fiber (C) to the total amount of solids in the molding resin composition is 5% by mass or more and 20% by mass or less.

[0088] According to this embodiment, the dimensional accuracy of the molded product can be maintained at a good level, and the mechanical strength of the molded product can be further increased.

[0089] In an eighth aspect, in any one of the first to seventh aspects, the thermoplastic resin (A) contains a polybutylene terephthalate-based resin (A1) and a polyethylene terephthalate-based resin (A2), and the mass ratio (A1 / A2) of the polybutylene terephthalate-based resin (A1) to the polyethylene terephthalate-based resin (A2) is within a range of 51 / 49 to 90 / 10.

[0090] According to this embodiment, the molding shrinkage rate of the molded product can be further reduced.

[0091] In a ninth aspect, in any one of the first to eighth aspects, an epoxy compound (D) is further contained. The epoxy compound (D) has two or more epoxy groups in one molecule and has an epoxy equivalent of 150 g / eq. or more and 250 g / eq. or less.

[0092] According to this embodiment, the viscosity of the molding resin composition can be prevented from increasing excessively, and good flowability can be ensured. Furthermore, even if the thermoplastic resin (A) in the molding resin composition contains a component that is easily hydrolyzed, hydrolysis of the thermoplastic resin (A) can be prevented.

[0093] In a tenth aspect, the proportion of the epoxy compound (D) relative to the total amount of solids in the molding resin composition is 0.5% by mass or more and 7% by mass or less.

[0094] According to this embodiment, the flowability of the molding resin composition during molding can be improved favorably.

[0095] The resin molded article (1) of the eleventh aspect is a molded article obtained by molding the molding resin composition of any one of the first to tenth aspects.

[0096] According to this embodiment, a resin molded product (1) having excellent dimensional accuracy and high strength can be obtained.

[0097] The housing (10) of the twelfth aspect is used to house an electronic component. The housing (10) includes the resin molded article (1) of the eleventh aspect.

[0098] According to this embodiment, a housing (10) having excellent dimensional accuracy and high strength can be obtained.

[0099] The present disclosure will be described in more detail below with reference to examples. However, the present disclosure is not limited to the following examples, and various modifications can be made depending on the design as long as the object of the present disclosure is achieved.

[0100] (1) Preparation of Molding Resin Composition First, the components shown in the composition column of Table 1 were prepared. In Examples 1 to 4, a "thermoplastic resin" and an "epoxy compound" were mixed in a blender, and then "scaly glass particles" and "strip-shaped glass fibers" were added in the amounts (parts by mass) shown in Table 1. The mixture was kneaded in a twin-screw extrusion kneader with the cylinder temperature heated to 260°C to prepare a kneaded product. In Reference Example 1, no "strip-shaped glass fibers" were added, and in Comparative Examples 1 to 4, no "scaly glass particles" were added. In Comparative Example 5, only "glass beads" were added instead of the "scaly glass particles" and "strip-shaped glass fibers," and in Comparative Example 6, "fused crushed silica" was added. In Comparative Example 7, "glass beads" were added instead of the "scaly glass particles," and in Comparative Example 8, "fused crushed silica" was added. In Reference Example 1 and Comparative Examples 1 to 8, kneaded materials were prepared by kneading using a twin-screw extrusion kneader with a cylinder temperature heated to 260° C., as in Examples 1 to 4. In this way, molding resin compositions of the Examples, Reference Examples, and Comparative Examples were obtained.

[0101] The details of the components shown in the composition column in the table are as follows. The values ​​shown in the table represent parts by mass, except for "A1 / A2," which indicates the ratio of polyester resin 1 (A1) to polyester resin (A2). - Polyester Resins - Polyester Resin 1 (A1): Polybutylene terephthalate (PBT) resin (manufactured by Chang Chun Plastics Co. Ltd., product name PBT 1200-211M). - Polyester Resin 2 (A2): Polyethylene terephthalate (PET) resin (manufactured by FAR EASTERN NEW CENTURY CORPORATION, product name CRB-B21). - Glass flake particles - Glass flake particle 1: Product of Nippon Sheet Glass Co., Ltd., product name MEG160FY-M01 (E glass, average thickness (t): 0.7 μm, average particle diameter (a): 160 μm, ratio a / t = 229) - Glass strip - Glass fiber strip 1: Product of Nitto Boseki Co., Ltd., product name CSG 3PL-830 (average minor diameter (d): 8.8 μm, average major diameter (w): 21.8 μm, ratio w / d = 2.5). - Glass fiber strip 2: Product of Nitto Boseki Co., Ltd., product name CSG 3PA-830S (average minor diameter (d): 6.9 μm, average major diameter (w): 26.8 μm, ratio w / d = 3.9). - Cylindrical glass fiber - Cylindrical glass fiber 1: Manufactured by Asahi Fiberglass Co., Ltd. Product name MF06JB1-20 (average minor axis (d): 10 μm, average major axis (w): 10 μm, ratio w / d = 1). - Cylindrical glass fiber 2: Manufactured by Nippon Electric Glass Co., Ltd. Product name ECS03 T-187 (average minor axis (d): 13 μm, average major axis (w): 13 μm, ratio w / d = 1). - Glass beads - Glass beads 1: Manufactured by Potters Ballotini Co., Ltd. Product name EGB731CV-PN. - Fused crushed silica - Fused crushed silica 1: Manufactured by Fumitec Co., Ltd. Product name FMT-15. - Epoxy compound - Epoxy compound 1: o-cresol novolac epoxy resin (epoxy equivalent 210 g / eq.). - Lubricant - Oxidized polyethylene wax 1: Clariant Chemicals Co., Ltd. Product name Licowax PED522. - Talc - Talc 1: Takehara Chemical Industry Co., Ltd. Product name TT Talc.

[0102] (2) Preparation of molded article of resin composition The molding resin composition (kneaded product) of (1) was cooled in water and then cut into pellets of about 2 to 4 mm using a pelletizer, thereby obtaining pellets of the molding resin composition.

[0103] The pellets of the molding resin composition were then dried in a thermostatic oven at 140° C. for 4 hours. The moisture content of the resulting dried product was 0.2% or less.

[0104] Next, a test piece (specimen) was produced using an 80t injection molding machine (ES-1000 manufactured by Nissei Plastic Industrial Co., Ltd.). The injection molding conditions were a cylinder temperature of 260°C and a mold temperature of 80°C. As a result, a test piece (specimen) of a resin molded body (60mm x 60mm x 1mmt) and a dumbbell test piece (173mm in total length, 8mm in parallel portion length, 10mm in parallel portion width, and 4mm in thickness) were obtained.

[0105] (3) Evaluation (3-1) Mold shrinkage and anisotropy The mold shrinkage in the perpendicular and parallel directions was measured for a 60 mm x 60 mm x 2 mm thick test piece in accordance with ISO-294-4. The obtained values ​​are shown in Table 1-2. The obtained mold shrinkage in the perpendicular direction and the parallel direction were evaluated according to the following criteria: A: The mold shrinkage is 0.5% or less. B: The mold shrinkage is more than 0.5% and less than 0.8%. C: The mold shrinkage is 0.8% or more.

[0106] The difference (absolute value) between the molding shrinkage rates in the perpendicular and parallel directions was defined as anisotropy, and the anisotropy was evaluated according to the following criteria: A: Anisotropy is 0.2 or less. B: Anisotropy is greater than 0.2 and less than 0.5. C: Anisotropy is 0.5 or more.

[0107] (3-2) Linear Expansion Coefficient and Anisotropy Dumbbell test specimens were prepared from the molded product of the molding resin composition prepared in (2) and cut to a width of 4 mm, length of 10 mm, and thickness of 4 mm for test measurement. Each prepared test specimen was subjected to the TMA method using a thermal analyzer (Model TMA7100, manufactured by Hitachi High-Tech Science Corporation) at a heating rate of 5°C / min and a measurement temperature of 10 to 140°C, and the linear expansion coefficients (CTE) in the horizontal and vertical directions were calculated under a load of 5 g (compression mode) in the temperature range of 90°C to 120°C. The linear expansion coefficients obtained are shown in Table 1-2. The linear expansion coefficients in the horizontal and vertical directions were evaluated according to the following criteria: A: The linear expansion coefficient was 50 ppm / °C or less. B: The linear expansion coefficient was greater than 50 ppm / °C and less than 100 ppm / °C. C: The linear expansion coefficient is 100 ppm / °C or more.

[0108] The anisotropy during heating was defined as the difference (absolute value) between the linear expansion coefficient in the perpendicular direction and the linear expansion coefficient in the parallel direction, and was evaluated according to the following criteria: A: Anisotropy is 70 or less. B: Anisotropy is more than 70 and less than 120. C: Anisotropy is 120 or more.

[0109] (3-3) Flexural Strength Dumbbell test specimens were prepared from the molded product of the molding resin composition prepared in (2), and the flexural strength was measured in accordance with ISO-527-1, 2 using a universal testing machine (autograph). The dimensions of the dumbbell test specimen were a total length of 173 mm, a parallel portion length of 80 mm, a parallel portion width of 10 mm, and a thickness of 4 mm. The measurement results obtained are shown in Table 1-2. Based on the measurement results, the flexural strength of the molded product was evaluated according to the following criteria: A: The flexural strength was 170 MPa or more. B: The flexural strength was greater than 120 MPa and less than 170 MPa. C: The flexural strength was 120 MPa or less.

[0110] (3-4) Flexural Modulus Dumbbell test pieces were prepared from the molded product of the molding resin composition prepared in (2), and the flexural modulus was measured using a universal testing machine (autograph) in accordance with ISO-527-1 and 2. The measurement results are shown in Table 1-2. Based on the measurement results, the flexural strength of the molded product was evaluated according to the following criteria. The measurement conditions were the same as in (3-3) above. A: The flexural modulus was 8.0 GPa or more. B: The flexural modulus was greater than 6.0 GPa and less than 8.0 GPa. C: The flexural modulus was 6.0 GPa or less.

[0111] (3-5) Deflection Temperature Under Load Test specimens were prepared from the molded product of the molding resin composition prepared in (2), and the deflection temperature under load was measured using a heat distortion tester in accordance with ISO-75-2. The dimensions of the test specimen were a total length of 80 mm, a width of 10 mm, and a thickness of 4 mm. The measurement conditions were a measurement temperature of 23 to 250°C (heating rate of 120°C / h) and a bending stress of 1.80 MPa. The measurement results obtained are shown in Table 1-2. Based on the measurement results, the tensile strength of the molded product was evaluated according to the following criteria: A: The deflection temperature under load was 180°C or higher. B: The deflection temperature under load was greater than 150°C and less than 180°C. C: The deflection temperature under load was 150°C or lower.

[0112]

[0113]

[0114] 1 resin molded body 10 housing

Claims

1. A molding resin composition comprising: a thermoplastic resin (A); scaly glass particles (B) having a ratio a / t of 100 or more and 400 or less of an average particle diameter a, which is the particle diameter at 50% of the cumulative diameter in a volume-based particle size distribution measured by a laser diffraction scattering method, to an average thickness t; and band-shaped glass fibers (C) having an aspect ratio of 1.5 or more and 5.0 or less.

2. The molding resin composition according to claim 1, wherein the average particle size is 100 μm or more and 300 μm or less, and the average thickness is 0.3 μm or more and 1.5 μm or less.

3. The molding resin composition according to claim 1, wherein the fiber length of the band-shaped glass fiber (C) is 150 μm or more and 300 μm or less.

4. The molding resin composition according to claim 1, wherein the average short diameter of the cross section perpendicular to the longitudinal direction of the band-shaped glass fiber (C) is 3 μm or more and 15 μm or less.

5. The molding resin composition according to claim 1, wherein the proportion of said thermoplastic resin (A) relative to the total solid content of said molding resin composition is 35% by mass or more and 85% by mass or less.

6. The molding resin composition according to claim 1, wherein the proportion of said scaly glass particles (B) relative to the total solid content of said molding resin composition is 10% by mass or more and 40% by mass or less.

7. The molding resin composition according to claim 1, wherein the proportion of said band-shaped glass fiber (C) relative to the total solid content of said molding resin composition is 5 mass % or more and 20 mass % or less.

8. The molding resin composition according to claim 1, wherein the thermoplastic resin (A) contains a polybutylene terephthalate-based resin (A1) and a polyethylene terephthalate-based resin (A2), and the mass ratio (A1 / A2) of the polybutylene terephthalate-based resin (A1) to the polyethylene terephthalate-based resin (A2) is within a range of 51 / 49 to 90 / 10.

9. The molding resin composition according to claim 1, further comprising an epoxy compound (D), which has two or more epoxy groups in one molecule and has an epoxy equivalent of 150 g / eq. or more and 250 g / eq. or less.

10. The molding resin composition according to claim 9, wherein the ratio of the epoxy compound (D) to the total solid content of the molding resin composition is 0.5% by mass or more and 7% by mass or less.

11. A resin molded product obtained by molding the molding resin composition according to any one of claims 1 to 10.

12. A housing used to house an electronic component, the housing comprising the resin molded article according to claim 11.

Citation Information

Patent Citations

  • Thermoplastic polyester resin composition

    JP2010150534A

  • Glass-reinforced resin composition

    JP2010275413A

  • Glass-reinforced resin composition

    JP2012207075A

  • Polycarbonate resin composition

    WO2019073818A1