Fatty acid-treated zinc oxide particles, method for producing same, and dispersion and cosmetic having same blended therein
The surface treatment of zinc oxide particles with fatty acid salts at elevated temperatures in a slurry process addresses the challenges of precipitation and thickening, achieving stable, water-repellent dispersions with improved dispersibility and performance.
Patent Information
- Application Number
- PCT/JP2024/011810
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Fatty acid-treated zinc oxide particles face challenges such as precipitation, thickening, and inferior performance due to the formation of fatty acid soap and unreacted free fatty acids, making it difficult to achieve stable, highly concentrated dispersions with sufficient water repellency.
A method involving the surface treatment of zinc oxide particles with fatty acid salts at temperatures above the melting point of the fatty acid, using a slurry process without drying, to ensure proper bonding and minimize unreacted fatty acids and agglomeration, resulting in particles with improved dispersibility and stability.
The method produces zinc oxide particles with excellent dispersibility and stability, maintaining low viscosity even at high concentrations, and providing effective water repellency without the need for silicone or alkoxysilane treatments.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Fatty acid-treated zinc oxide particles, their production method, and dispersions and cosmetics containing the same
[0001] The present invention relates to fatty acid-treated zinc oxide particles, a method for producing the same, and a dispersion and a cosmetic composition containing the same.
[0002] Titanium dioxide particles and zinc oxide particles have traditionally been used as UV scattering agents in sunscreen cosmetics and other products due to their high UV blocking properties and transparency. These powders have hydrophilic surfaces in their untreated state, which can be easily washed away by sweat or rain. For this reason, they are often used after undergoing a water-repellent treatment on their particle surfaces, particularly in cosmetics.
[0003] Silicone treatment and alkoxysilane treatment are commonly used as such water-repellent treatments, but in recent years, silicone-treated products have tended to be avoided, and as an alternative, zinc oxide treated with a fatty acid, which is a naturally occurring component, has been sought (e.g., Patent Documents 1 and 2).
[0004] However, when fatty acid treatment is performed, problems occur such as a decrease in performance due to the formation of a fatty acid soap consisting of zinc ions dissolved in water and fatty acids, thickening due to the presence of unreacted free fatty acids, or precipitation of solids, etc. Therefore, it is difficult to stably obtain a high-concentration dispersion, and its performance is inferior to that of silicone-treated or alkoxysilane-treated zinc oxide, so fatty acid-treated zinc oxide is not widely distributed on the market.
[0005] JP 2016-196381 A JP 2021-083334 A
[0006] In view of the above, an object of the present invention is to provide fatty acid-treated zinc oxide particles that have excellent dispersibility, do not show excessive thickening even when blended at high concentrations, and can give dispersions with excellent stability over time.
[0007] The present invention relates to a compound having a peak at 1350-1500 cm in an FT-IR spectrum measured using an attenuated total reflectance (ATR) method. -1 The maximum absorbance (I 1 ) for 1500-1600 cm -1 The maximum absorbance (I2 ) ratio (I 2 / I 1 ) is 0.8 to 1.2, and -1 The maximum absorbance (I 4 ) for 1700-1720 cm -1 The maximum absorbance (I 3 ) ratio (I 3 / I 4 The fatty acid-treated zinc oxide particles are characterized in that the saturation coefficient (S) of the fatty acid-treated zinc oxide particles is 1.2 or less, the primary particle size is 0.1 μm or less as measured by a transmission electron microscope, and the powder is dispersed in isopropyl alcohol by irradiating the powder with ultrasonic waves at a rated output of 600 W and a vibration amplitude of 100% for 1 minute at room temperature, and the volume-based mode diameter of the dispersion obtained by laser diffraction scattering is 0.30 μm or less. The fatty acid is preferably at least one selected from the group consisting of stearic acid, isostearic acid, and palmitic acid.
[0008] The present invention also relates to a method for producing fatty acid-treated zinc oxide particles, comprising the steps of (1) repulping zinc oxide particles (raw material) in a dispersion medium to prepare a slurry, (2) neutralizing a fatty acid with a base to obtain an aqueous fatty acid salt solution, and (3) adding the obtained aqueous fatty acid salt solution to the zinc oxide slurry for surface treatment, wherein the raw material zinc oxide particles are obtained by a production method including a step of aging fine zinc oxide particles in water containing a dissolved zinc salt, and are subjected to step (1) without a drying step, and steps (2) and (3) are carried out at a temperature equal to or higher than the melting point of the fatty acid. The above-mentioned zinc oxide particles (raw material) are preferably dispersed by placing the powder in a 0.0025% by mass aqueous sodium hexametaphosphate solution and irradiating it with ultrasonic waves at a rated output of 600 W and a vibration amplitude of 100% using an ultrasonic homogenizer at room temperature for 3 minutes, and the resulting dispersion has a median diameter of 0.30 μm or less as measured by a laser diffraction scattering method. The present invention also relates to a dispersion containing the above-mentioned fatty acid-treated zinc oxide particles. The present invention also relates to a cosmetic preparation containing the above-mentioned fatty acid-treated zinc oxide particles.
[0009] The present invention provides a fatty acid-treated zinc oxide having sufficient water repellency and a low environmental impact. Furthermore, by using the fatty acid-treated zinc oxide particles of the present invention, a dispersion and a cosmetic composition having excellent dispersibility and stability over time can be obtained.
[0010] 1 is a diagram showing an FT-IR spectrum of a fatty acid-treated zinc oxide particle obtained in an example. 2 is a diagram showing an FT-IR spectrum of a fatty acid-treated zinc oxide particle obtained in a comparative example. 3 is a schematic diagram illustrating a method for measuring the primary particle diameter of a fatty acid-treated zinc oxide particle of the present invention.
[0011] The present invention will be described in detail below.
[0012] (Fatty Acid-Treated Zinc Oxide Particles) The fatty acid-treated zinc oxide particles of the present invention can suppress thickening of the dispersion even when incorporated at a high concentration, and can produce a dispersion with excellent stability over time. To achieve this effect, it is believed that the following three conditions must be met: (1) The amount of fatty acid zinc (fatty acid soap) produced must be suppressed. (2) The amount of unreacted fatty acid remaining must be suppressed. (3) The particles are easily dispersible.
[0013] The various problems described above are believed to be caused by fatty acid zinc, unreacted fatty acid, and agglomerated particles, and therefore the object of the present invention can be achieved by reducing these components.
[0014] When the treatment with fatty acid in the present invention is performed, it is preferable to obtain treated particles in which fatty acid is bound to the surface of zinc oxide particles. On the other hand, free fatty acid zinc produces undesirable effects. It is thought that free fatty acid zinc is produced when zinc oxide reacts with water to generate zinc ions, which then react with fatty acid to become fatty acid zinc. Therefore, in the present invention, the surface treatment process is adjusted to prevent such reactions as much as possible.
[0015] Furthermore, if unreacted fatty acid remains, this also has a negative effect on performance, so it is desirable to avoid the production of excess fatty acid.
[0016] Furthermore, if particles aggregate, they will break down during dispersion, leaving untreated surfaces, which is thought to result in thickening when blended at high concentrations.Easily dispersible particles do not aggregate and are uniformly treated, so they do not thicken even when blended at high concentrations, making it possible to obtain a low-viscosity dispersion.
[0017] The fatty acid-treated zinc oxide particles of the present invention satisfy the above (1) and (2), and therefore the IR peak intensity derived from the fatty acid zinc or fatty acid is smaller than the IR peak intensity of zinc oxide particles that have not been subjected to a suitable surface treatment. This is referred to as (I 2 / I 1 ) and (I 3 / I 4 ) is expressed as a parameter.
[0018] The fatty acid-treated zinc oxide particles of the present invention have a wavelength of 1350-1500 cm in the FT-IR spectrum measured using an attenuated total reflectance (ATR) method. -1 The maximum absorbance (I 1 ) for 1500-1600 cm -1 The maximum absorbance (I 2 ) ratio (I 2 / I 1 ) is 0.8 to 1.2, and 1750-1800 cm -1 The maximum absorbance (I 4 ) for 1700-1720 cm -1 The maximum absorbance (I 3 ) ratio (I 3 / I 4 The ratio (I) is 1.2 or less. 2 / I 1 ) absorbance I 1 The value is 1350-1500 cm -1 Detected in CH 3 Symmetric bending vibration, COO - Symmetric stretching vibration, CH 3 The absorbance of the maximum peak of any of the asymmetric bending vibrations, absorbance I 2 The value is 1500-1600 cm -1 COO -The ratio (I 2 / I 1 When the value of the ratio (I) is between 0.8 and 1.2, it means that the fatty acid is bonded to the zinc oxide surface, and when it is greater than 1.2, it means that free fatty acid zinc is precipitated. When the ratio is less than 0.8, it means that the fatty acid is not sufficiently bonded to the zinc oxide surface, and a large amount of unreacted fatty acid is present. 2 / I 1 The lower limit of ) is preferably 0.9, and the upper limit is preferably 1.1.
[0019] The fatty acid-treated zinc oxide particles of the present invention further have a viscosity of 1750-1800 cm -1 The maximum absorbance (I 4 ) for 1700-1720 cm -1 The maximum absorbance (I 3 ) ratio (I 3 / I 4 The absorbance I is 1.2 or less. 3 The value is 1700-1720 cm -1 The absorbance of the C═O stretching vibration peak detected at 4 The value is 1750-1800 cm -1 This is the absorbance value of the peaks of the C=O stretching vibration of four-membered rings, five-membered rings, and acid anhydrides, which are detected in the present manufacturing process. Since there are no substances corresponding to four-membered rings, five-membered rings, or acid anhydrides, no peaks are detected. Therefore, I 3 / I 4 If the value of I exceeds 1.2, it means that unreacted fatty acid remains. 3 / I 4 ) is preferably 1.1 or less, and although there is no particular lower limit, it is preferably 0.8 or more.
[0020] Furthermore, since the fatty acid-treated zinc oxide particles of the present invention satisfy the above-mentioned (3), the particle size distribution in weak dispersion is close to the primary particle size, which is expressed in the present invention by a parameter called the mode diameter. The fatty acid-treated zinc oxide particles of the present invention are characterized in that the primary particle size measured from a transmission electron microscope photograph is 0.1 μm or less, and the powder is placed in isopropyl alcohol and irradiated with ultrasonic waves at a rated output of 600 W and a vibration amplitude of 100% for 1 minute at room temperature to form a dispersion, which has a volume-based mode diameter of 0.30 μm or less as measured by a laser diffraction scattering method.
[0021] Specifically, the primary particle diameter in the present invention is a particle diameter (μm) defined as the unidirectional diameter (the distance between two parallel lines in a fixed direction sandwiching a particle as shown in FIG. 3 ; measurement was performed in a fixed direction for particles of any shape in the image) in a field of view of 2,000 to 50,000 times magnification in a photograph taken with a transmission electron microscope JEM-1200EX II (manufactured by JEOL Ltd.), and is calculated by measuring the unidirectional diameters of 250 primary particles in the TEM photograph and calculating the average value of their cumulative distribution. The primary particle diameter is more preferably 0.005 μm or more and less than 0.1 μm.
[0022] The mode diameter in the present invention was specifically determined by the following method: 0.1 g of the fatty acid-treated zinc oxide particles was placed in 50 ml of isopropyl alcohol, and an ultrasonic homogenizer US-600E (manufactured by Nippon Seiki Seisakusho, rated output 600 W) was used to irradiate the particles with ultrasonic waves at 100% vibration amplitude for 1 minute at room temperature to prepare a slurry, and the volumetric mode diameter was measured using a laser diffraction / scattering particle size distribution analyzer LA-960S (manufactured by Horiba, Ltd.). Another feature of the fatty acid-treated zinc oxide particles of the present invention is that they have extremely high dispersibility, and therefore can be sufficiently dispersed simply by applying a weak ultrasonic impact. It is more preferable that the mode diameter be 0.20 μm or less.
[0023] The fatty acid-treated zinc oxide particles of the present invention have a surface treatment layer made of a fatty acid on the surface. As a water-repellent surface treatment agent, a fatty acid with high environmental adaptability is most desirable. Note that the surface treatment here refers to a water-repellent treatment for reducing the affinity of the zinc oxide particle surface for water, and surface treatment using a material that is easily soluble in water or dispersible in water after treatment does not fall under the category of "water-repellent treatment" in the present invention.
[0024] The fatty acid used in the present invention preferably has strong water repellency. Compounds that chemically bond with inorganic powders are preferred, but even compounds that physically adsorb can achieve some degree of effectiveness. The fatty acid is preferably a higher fatty acid having 10 to 30 carbon atoms, as this can further improve the dispersibility of zinc oxide particles in the dispersion. Specifically, at least one selected from saturated fatty acids such as stearic acid, isostearic acid, myristic acid, lauric acid, and palmitic acid, and unsaturated fatty acids such as oleic acid is preferred. Among these, stearic acid, palmitic acid, and isostearic acid are preferred, as they have a particularly simple structure, are inexpensive, highly stable, and have strong water repellency. Furthermore, to create a treatment agent with a lower environmental impact, it is preferable to use a plant-derived fatty acid.
[0025] The fatty acid-treated zinc oxide particles of the present invention may also be obtained by coating the particle surfaces of the raw zinc oxide particles with another inorganic compound. That is, the zinc oxide particles may be surface-treated with another inorganic compound and then further surface-treated with a fatty acid. Known inorganic surface treatment materials can be used as the coating material, and for example, the zinc oxide particles may be coated with one or more oxides or hydroxides of Al, Si, Zr, Sn, etc.
[0026] Zinc oxide particles, which are the active ingredient, release zinc ions over time, which can disrupt the emulsion system when incorporated into cosmetics. In addition, the surface catalytic activity of zinc oxide poses the problem of denaturing other ingredients. However, coating with an inorganic compound can prevent the zinc ions from leaking out, and for such applications (e.g., cosmetics), coating with an inorganic compound is preferred.
[0027] In particular, it is preferable to use a material that has been surface-treated with one or both of aluminum hydroxide and hydrous silica, as this is harmless to the environment and the human body and has a high activity suppression effect.
[0028] The coating amount of the inorganic surface treatment material is preferably 1 to 30% by mass relative to the zinc oxide. Within this range, sufficient activity suppression is achieved and the effect on the properties of the zinc oxide is small. The lower limit is more preferably 3% by mass. The upper limit is more preferably 20% by mass.
[0029] The surface treatment method with the inorganic surface treatment material is not particularly limited, and can be carried out by a well-known general method.
[0030] The fatty acid-treated zinc oxide particles of the present invention preferably have an apparent density of 0.5 g / ml or more. An apparent density of 0.5 g / ml or more is preferable in that the bulk of the powder is reduced, which reduces the amount of dust generated and facilitates packing into packaging containers, allowing for large quantities of powder to be transported. It is also preferable in that the powder is easier to handle, for example, allowing it to be mixed with other components in a container with a smaller volume. The apparent density is more preferably 0.6 g / ml or more. The higher the apparent density, the smaller the bulk of the powder. The apparent density can be measured by the method described in JIS K 5101-12-1, Pigment Test Method - Apparent Density or Apparent Specific Volume (Static Method).
[0031] The fatty acid-treated zinc oxide particles of the present invention have a BET specific surface area of 25 m 2 / g or less. 2 If the specific surface area exceeds 1 / g, the particle size becomes small and aggregation tends to occur. The BET specific surface area can be measured by the method described in the Examples.
[0032] The carbon content in the fatty acid-treated zinc oxide particles of the present invention is preferably 0.5% by mass or more and less than 8.0% by mass. If the carbon content is less than 0.5% by mass, there is a risk that the particles will not exhibit a sufficient water-repellent effect. If the carbon content is 8.0% by mass or more, there is a risk that the purity of the zinc oxide will decrease, resulting in a decrease in performance, and addition of an excessive amount may lead to the precipitation of free fatty acid zinc. More preferably, the carbon content is 1.0% by mass or more and less than 7.0% by mass. The carbon content can be measured by the method described in the Examples.
[0033] (Method for producing fatty acid-treated zinc oxide particles) The method for producing the fatty acid-treated zinc oxide particles of the present invention is not particularly limited, but may include, for example, a method for producing fatty acid-treated zinc oxide particles, which includes a step (1) of repulping zinc oxide particles as raw material in a dispersion medium to prepare a slurry, a step (2) of neutralizing the fatty acid with a base to obtain an aqueous fatty acid salt solution, and a step (3) of adding the obtained aqueous fatty acid salt solution to the zinc oxide slurry to perform a surface treatment, wherein the zinc oxide particles as raw material are obtained by a production method including a step of aging fine zinc oxide particles in water in which a zinc salt has been dissolved, and are subjected to step (1) without a drying step, and the steps (2) and (3) are carried out at a temperature equal to or higher than the melting point of the fatty acid. Such a production method also constitutes one aspect of the present invention.
[0034] The step (1) is a step of preparing a slurry by repulping zinc oxide particles as raw materials in a dispersion medium. In the production method of the present invention, preparing a slurry of zinc oxide particles in step (1) is an important step. That is, the method is characterized in that the fatty acid coating is formed when the zinc oxide particles are in a dispersed slurry state, rather than in a dry, aggregated state.
[0035] Here, the zinc oxide particles used as the raw material in step (1) are those that have undergone a synthesis reaction in an aqueous medium, and are used to prepare a slurry directly without undergoing a drying step. That is, it is preferable that there is no step of drying the particles between the particle production step and the fatty acid treatment step. In this way, aggregation between particles is suppressed, and surface treatment of the aggregated particles is not required, thereby achieving the excellent dispersion performance described above.
[0036] In step (1), each zinc oxide particle is surface-treated, and thus water repellency can be efficiently imparted without the need for an excessive amount of fatty acid coating. In step (1), the zinc oxide particle slurry is not limited, but preferably contains zinc oxide particles in the range of 10 to 1000 g / L, for example.
[0037] The method for preparing the slurry is not particularly limited, and for example, zinc oxide particles obtained in a zinc oxide particle production process are filtered, then added to water without drying, and dispersed for 10 to 30 minutes at 5 to 30° C. to obtain a uniform slurry with a zinc oxide particle concentration of 10 to 1,000 g / L. The dispersion medium is not particularly limited, and for example, alcohols such as isopropanol or organic solvents can be used, but water is preferably used from the standpoints of safety and production costs.
[0038] The above-mentioned step (2) is a step of neutralizing a fatty acid with a base to obtain an aqueous fatty acid salt solution, and is carried out at a temperature above the melting point of the fatty acid. From a manufacturing standpoint, the concentration of the above-mentioned fatty acid salt aqueous solution is preferably 15 wt% or less, more preferably 10 wt% or less. Therefore, the above-mentioned temperature is preferably a temperature at which the solubility of the fatty acid salt in water is 10 wt% or more. The above-mentioned neutralization preferably uses a commonly used base such as caustic soda (sodium hydroxide) or caustic potash (potassium hydroxide). Since the above-mentioned melting point and solubility are determined by the composition of the fatty acid used, the temperature of step (2) may vary. For example, when stearic acid is used as the fatty acid, the melting point of stearic acid is 70°C, so the step should be carried out at 70°C or higher. Furthermore, when caustic soda is used as the base, the solubility of sodium stearate in water is 3 wt% at 70°C and 10 wt% at 75°C, so a temperature of 75°C or higher is more preferable.
[0039] The step (2) is preferably carried out with stirring. Stirring allows the fatty acid and fatty acid salt to be more thoroughly melted and dissolved. The stirring means in the step (2) is not particularly limited, but examples thereof include stirring with a stirring blade, shaking, stirring with a mixer, and stirring with a stirrer.
[0040] The above step (3) is a step of adding the obtained aqueous fatty acid salt solution to the zinc oxide slurry to perform surface treatment. In the surface treatment step, it is preferable to add the aqueous fatty acid salt solution to the zinc oxide particle slurry obtained in step (1) and then stir the mixture. Stirring makes it easier for the fatty acid to be uniformly adsorbed onto the zinc oxide particles, allowing the surface treatment to be performed more efficiently. The stirring time is not particularly limited, but is preferably 5 minutes or more. The stirring means is not particularly limited, but examples include stirring with a stirring blade, shaking stirring, stirring with a mixer, and stirring with a stirrer.
[0041] Like step (2), step (3) of the surface treatment step is also carried out at a temperature equal to or higher than the melting point of the fatty acid, and more preferably at a temperature at which the solubility of the fatty acid salt in water is 10 wt % or higher. In steps (2) and (3), the fatty acid is reacted with zinc oxide in a liquid state rather than a solid state, thereby enabling uniform surface treatment. If the temperature in steps (2) and (3) is lower than the melting point of the fatty acid, the reaction between the fatty acid and fatty acid salt and zinc oxide may be insufficient. In this case, insufficient reaction includes a state in which the fatty acid and fatty acid salt remain solid and are not uniformly chemically bonded to or physically adsorbed on the zinc oxide. If the zinc oxide is not uniformly treated, the ratio (I 2 / I 1 ) and ratio (I 3 / I 4 Even if the amount of the fatty acid salt in the aqueous solution of the zinc oxide is within the range of the present invention, problems such as aggregation of untreated portions and difficulty in adsorbing the dispersant to portions with an excessive amount of treatment may occur during the preparation of the dispersion, resulting in increased viscosity. In the above step (3), it is preferable to heat both the aqueous fatty acid salt solution and the zinc oxide slurry to a temperature equal to or higher than the melting point of the fatty acid.
[0042] The step (3) is a step of adding an aqueous solution of fatty acid salt, and it is preferable to add the fatty acid so that the amount of added fatty acid is 1.0% by mass or more relative to the zinc oxide particles. If the amount added is less than 1.0% by mass, there is a risk of insufficient water repellency. It is more preferably 1.5% by mass or more. Furthermore, the amount added is preferably 10% by mass or less. If the amount added exceeds 10% by mass, simple fatty acid zinc remains that cannot be bonded to the zinc oxide surface even when the drying step is carried out at a temperature equal to or higher than the melting points of the fatty acid and fatty acid zinc. As a result, the ratio (I 2 / I 1 ) may fall outside the range of the present invention. The amount added is more preferably 8 mass % or less.
[0043] After the surface treatment step is completed, the resulting slurry is aged for 0.5 to several tens of hours while continuing to stir, thereby forming a fatty acid coating on the surface of the zinc oxide particles. During the aging step, small amounts of other components may be added within a range that does not impair the effects of the present invention. For example, a dispersant or the like may also be added.
[0044] The aging is preferably carried out at 45 to 110° C. In particular, the aging time can be 0.5 to 24 hours. Since zinc oxide particles that have been subjected to uniform treatment can be obtained depending on conditions such as the aging temperature, aging time, and zinc oxide concentration, it is preferable to appropriately set these conditions depending on the type and amount of fatty acid added.
[0045] The fatty acid-treated zinc oxide particles thus obtained may be subjected to post-treatments such as pH adjustment, filtration, and water washing, as necessary. In the pH adjustment step, the pH of the aged slurry is preferably adjusted to 6 to 10, more preferably 7 to 8. Commonly used acids such as sulfuric acid and hydrochloric acid are preferably used as the neutralizing agent, and zinc salts such as zinc sulfate and zinc chloride may also be used. The method for producing fatty acid-treated zinc oxide particles of the present invention preferably further includes a drying step. Drying is preferably carried out at a temperature above the melting point of the fatty acid, more preferably above the melting point of the fatty acid zinc. Drying at a temperature above the melting points of the fatty acid and the fatty acid zinc melts the remaining fatty acid and excess precipitated fatty acid zinc, allowing them to chemically bond to the zinc oxide surface. For example, when stearic acid is used as the fatty acid, drying is preferably carried out at a temperature above the melting point of stearic acid (70°C) and more preferably above the melting point of zinc stearate (120°C).
[0046] The heating temperature in the drying step is not particularly limited, but it is preferable that the surface treatment is not followed by a calcination step in which the surface is heated at 300°C or higher. By doing so, the particle size and shape of the zinc oxide particles as the raw material can be maintained, and the effects of the present invention as described above can be particularly suitably obtained. Furthermore, it is preferable to carry out a pulverization step as necessary after the drying step. An example of dry pulverization is an atomizer.
[0047] Although the zinc oxide particles used as the raw material are not particularly limited, it is preferable to use those having high dispersibility in themselves, since this will also increase the dispersibility of the resulting fatty acid-treated zinc oxide particles. In particular, it is preferable to use zinc oxide particles having a median diameter of 0.30 μm or less, as measured by a laser diffraction scattering method, in a dispersion obtained by irradiating an ultrasonic homogenizer with ultrasonic waves at a rated output of 600 W and a vibration amplitude of 100% at room temperature for 3 minutes in a 0.0025 mass % aqueous solution of sodium hexametaphosphate.
[0048] As described above, by subjecting zinc oxide particles with excellent dispersibility to fatty acid treatment, a uniform fatty acid coating layer is formed on each particle, and the resulting fatty acid-treated zinc oxide particles also have excellent dispersibility, so that they can be dispersed with a weak impact when blended into cosmetics, etc. On the other hand, when no impact is applied, aggregated particles can be formed with a moderate cohesive force, resulting in good handleability.
[0049] The shape of the zinc oxide particles as the raw material is not particularly limited, but a plate shape is preferred in terms of improving the feel of the resulting fatty acid-treated zinc oxide particles when used and their ability to shield against UV rays, etc. For example, the primary particle diameter is preferably less than 0.1 μm, the aspect ratio is preferably less than 2.5, and the oil absorption / BET specific surface area is preferably 1.5 ml / 100 m. 2 The oil absorption / BET specific surface area (ml / 100 m) is preferably less than or equal to 1. 2 ) is the value of oil absorption (ml / 100g) and BET specific surface area (m 2 / g), and the smaller this value, the lower the oil absorption per unit area of the particle surface, the less the particles aggregate, and the higher the particle independence and dispersibility. Examples of such zinc oxide raw material particles include those obtained by a production method including a step of aging fine zinc oxide particles having a primary particle diameter of 0.005 μm or more and 0.05 μm or less in water containing a dissolved zinc salt. Specifically, it is preferable to use, for example, zinc oxide particles disclosed in International Publication No. 2012 / 147888.
[0050] WO 2012 / 147888 discloses a method for obtaining zinc oxide particles with excellent dispersibility by a production method including a step of aging fine zinc oxide particles in water containing a dissolved zinc salt. After producing zinc oxide particles in water by such a method, it is preferable to perform surface treatment as described above without filtering and drying. This allows surface treatment of zinc oxide particles with little aggregation, thereby achieving the object of the present invention.
[0051] The primary particle size is less than 0.1 μm, the aspect ratio is less than 2.5, and the oil absorption / BET specific surface area is 1.5 ml / 100 m by the manufacturing method described in WO 2012 / 147888. 2 It is particularly preferable to obtain zinc oxide particles characterized by the following: such zinc oxide particles are used as a raw material.
[0052] The fatty acid-treated zinc oxide particles of the present invention may further be subjected to other surface treatments as necessary. The surface treatments are not particularly limited, and examples thereof include known treatment methods such as inorganic surface treatments for forming inorganic oxide layers such as silica layers, alumina layers, zirconia layers, and titania layers, and various other surface treatments. Furthermore, multiple types of surface treatments may be performed sequentially.
[0053] More specifically, the surface treatment may be performed with a surface treatment agent selected from an organic aluminum compound, an organic titanium compound, a polyhydric alcohol, or an alkanolamine. The amount of such a surface treatment agent used can be appropriately determined depending on the particle size of the zinc oxide particles.
[0054] The fatty acid-treated zinc oxide particles of the present invention may be dispersed in water or an oil solution to form a dispersion, and such dispersions are also included in the present invention.
[0055] (Dispersion, Cosmetic) The dispersion of the present invention preferably contains the fatty acid-treated zinc oxide particles of the present invention in a proportion of 40 to 80 mass % of the total amount of the dispersion. The lower limit is more preferably 45 mass %, and even more preferably 50 mass %. Because the fatty acid-treated zinc oxide particles have the effects described above, even in this relatively high blending range, the dispersibility is good, the viscosity of the dispersion is low, and the viscosity is maintained over time.
[0056] The dispersion of the present invention preferably further contains polyhydroxystearic acid. This compound functions as a dispersant, and the inclusion of this compound is preferred in that the fatty acid-treated zinc oxide particles are well dispersed in the solvent. The use of polyhydroxystearic acid is particularly preferred in that good dispersion can be achieved even with a small amount, and that the fatty acid-treated zinc oxide particles having a water-repellent surface treatment layer are less likely to be washed away by water during use.
[0057] The hydroxyl group of hydroxystearic acid is preferably bonded to the carbon at position 12, and the degree of polymerization of hydroxystearic acid is preferably 3 to 12, more preferably 4 to 8. Commercially available products include Salacos HS-6C (manufactured by Nisshin Oillio Co., Ltd.) and ARLACEL P-100 (manufactured by Uniqema Co., Ltd.).
[0058] The blending amount of the polyhydroxystearic acid in the dispersion is preferably 0.1 to 10% by mass. The lower limit is more preferably 1% by mass, and the upper limit is even more preferably 7% by mass or less. This ratio is particularly preferred in that it increases the solvent content and provides high compatibility with formulations when blended into cosmetics.
[0059] The dispersion of the present invention preferably contains an oil as a medium for dispersing the fatty acid-treated zinc oxide particles. The oil is not particularly limited, but from the standpoint of environmental impact, an oil that does not have a polysiloxane skeleton is preferred, and liquid oils that are liquid at room temperature (15 to 25°C) are preferred from the standpoint of dispersibility. Examples include ester oils, fruit oils, and other fats and oils. Of these, ester oils and fruit oils are preferred because they are easy to use in cosmetics. Specific examples include the following, and one or more of these can be used.
[0060] Examples of the ester oils include ethylhexyl palmitate, isopropyl isostearate, ethyl oleate, octyldodecyl oleate, octyldodecyl myristate, diisostearyl malate, glyceryl tricaprylate, isooctyl isononanoate, isotridecyl isononanoate, isononyl isononanoate, ethylhexyl isononanoate, propylene glycol dicaprate, neopentylene glycol dicaprate, neopentylene glycol diethylhexanoate, cetyl ethylhexanoate, glyceryl tri-2-ethylhexanoate, jojoba oil, isopropyl myristate, isopropyl palmitate, isotridecyl isononanoate, polyglyceryl diisostearate, diglyceryl triisostearate, glyceryl tribehenate, hexa(hydroxystearic acid / stearic acid) dipentaerythrityl hydroxystearate / rosinate, neopentyl glycol dioctanoate, cholesteryl isostearate, cholesteryl hydroxystearate, cholesteryl stearate, cholesteryl lanolinate, phytosteryl oleate, di(cholesteryl-behenyl-octyldodecyl) N-lauroyl-L-glutamate, di(phytosteryl-2-octyldodecyl) N-lauroyl-L-glutamate, and the like.
[0061] Examples of the fruit oil include olive fruit oil, lily of the valley fruit oil, fennel fruit oil, caraway fruit oil, pepper fruit oil, coriander fruit oil, juniper oil, vanilla fruit oil, bergamot fruit oil, and lemon fruit oil.
[0062] Examples of the other oils and fats include safflower oil, soybean oil, evening primrose oil, grape seed oil, rosehip oil, coconut oil, almond oil, sesame oil, wheat germ oil, corn oil, cottonseed oil, avocado oil, camellia oil, persic oil, castor oil, peanut oil, hazelnut oil, macadamia nut oil, medfoam oil, cacao butter, shea butter, Japan wax, coconut oil, palm oil, palm kernel oil, beef tallow, horse tallow, mink oil, milk fat, egg yolk oil, turtle oil, Japan wax, and camellia oil.
[0063] The blending amount of the oil agent in the dispersion is preferably 5 to 60% by mass. This ratio is advantageous in that it facilitates compatibility with the oil when blended into cosmetics, etc. The lower limit is more preferably 10% by mass, and the upper limit is more preferably 55% by mass.
[0064] In addition to the above components, the dispersion of the present invention may contain preservatives, pH adjusters, pure water, etc., depending on the purpose.
[0065] The dispersion of the present invention preferably has an initial viscosity of 1,500 mPa·s or less, more preferably 1,000 mPa·s or less, as measured by the following evaluation method. Within this range, the viscosity is low and beads can be easily separated after dispersion.
[0066] Method for evaluating initial viscosity: 8 ml of the dispersion immediately after production was placed in a 9 ml screw bottle, and rotated at 12 rpm using a B-type viscometer (Tokyo Keiki, TVB-10) with a rotor No. 4, and the viscosity (25°C) was measured 60 seconds after the start of rotation.
[0067] Furthermore, the dispersion of the present invention preferably has a viscosity after 7 days of 2,000 mPa s or less, more preferably 1,800 mPa s or less, as measured by the following evaluation method. Within this range, the viscosity is not too high, and the dispersion is easy to remove from a container and handle.
[0068] Method for evaluating viscosity over time: 8 ml of the dispersion immediately after production was placed in a 9 ml screw bottle and stored in a 40°C thermostatic chamber for 7 days. The dispersion was then rotated at 12 rpm using a B-type viscometer (TVB-10 manufactured by Tokyo Keiki) with a rotor No. 4, and the viscosity (25°C) was measured 60 seconds after the start of rotation.
[0069] The method for producing the dispersion of the present invention is not particularly limited. Specifically, for example, the dispersion can be obtained by using the fatty acid-treated zinc oxide particles, dispersant, and solvent as raw materials, and mixing and stirring them with other components.
[0070] The dispersion of the present invention is preferably an oil-based dispersion that is substantially free of water. Furthermore, the content of components other than the fatty acid-treated zinc oxide particles, dispersant, and solvent is preferably 1% by mass or less, more preferably 0.5% by mass or less. Furthermore, the dispersion may consist of only the fatty acid-treated zinc oxide particles, dispersant, and solvent. The dispersion of the present invention can be used, in particular, as a raw material for producing cosmetics. Therefore, in order to avoid formulation limitations, it is preferable that the dispersion contain as few components other than those described above as possible.
[0071] The dispersion of the present invention may contain inorganic particles other than zinc oxide. The inorganic particles that can be used in combination are not particularly limited, but examples include titanium dioxide. In particular, when titanium dioxide is used in combination with zinc oxide, the problem of thickening tends to become more pronounced, so the effects of the present invention become more pronounced when used in combination with titanium dioxide. When zinc oxide is used as an ultraviolet screening agent in ultraviolet protective cosmetics, titanium dioxide particles with a different ultraviolet screening range may be used in combination, and the present invention is also useful in such cases.
[0072] In the present invention, the titanium dioxide particles used in combination are not particularly limited, but it is preferable to use titanium dioxide particles that have been surface-treated with a fatty acid. The amount of fatty acid coated on the titanium dioxide particles is preferably 4.0 to 8.5 mass% relative to the titanium dioxide particles. Examples of the fatty acid include the same fatty acids as those used for zinc oxide. As with zinc oxide particles, it is preferable to treat the titanium dioxide particles with aluminum hydroxide or hydrous silicic acid, and then with a fatty acid.
[0073] The surface treatment of titanium dioxide particles can be carried out by a conventionally known method or by the same method as that used for treating zinc oxide particles described above.
[0074] It is preferable to use titanium dioxide particles having an average primary particle diameter of 200 nm or less. If the average primary particle diameter of titanium dioxide particles exceeds 200 nm, the hiding power is high, the particles become white, and the transparency is low. The lower limit of the average primary particle diameter of titanium dioxide particles is not particularly limited, but is usually 5 nm. The average primary particle diameter of titanium dioxide particles is calculated by measuring the particle diameters of 200 randomly selected particles under an electron microscope and averaging the particle diameters.
[0075] The shape of titanium dioxide particles is not particularly limited, and any shape such as spherical, rod-like, needle-like, spindle-like, or plate-like can be used. Regarding the average primary particle diameter in the case of shapes other than spherical, the average diameter is defined as the average length of the minor axis in the case of rod-like, needle-like, or spindle-like particles, and as the average diagonal length of the surface in the case of plate-like particles. The major axis diameter / minor axis diameter (aspect ratio) of the titanium dioxide particles is preferably 9 or less. The aspect ratio of titanium dioxide particles is calculated as the average value of the major axis diameter / minor axis diameter of 200 particles randomly selected under an electron microscope.
[0076] When inorganic particles other than zinc oxide, such as titanium dioxide, are used, the total amount of the fatty acid-treated zinc oxide particles and the inorganic particles other than zinc oxide, such as titanium dioxide, is preferably 40 to 70 mass % of the total amount of the dispersion. When inorganic particles other than zinc oxide, such as titanium dioxide, are used, the inorganic particles may be blended within a range that does not impede the object of the present invention, and for example, the blending amount of the inorganic particles other than zinc oxide, such as titanium dioxide, is preferably no more than twice the mass of the zinc oxide.
[0077] The dispersion of the present invention is preferably a non-silicone dispersion. Non-silicone dispersion means that it does not substantially contain silicone-based materials, and preferably does not substantially contain silicone-based oils, silicone-based surfactants, or inorganic particles surface-treated with silicone-based surface treatment agents. The content of silicone-based materials is preferably 1% by mass or less, more preferably 0.5% by mass or less, of the total amount of the dispersion.
[0078] The dispersion of the present invention is suitable for use in cosmetics. The cosmetics are not particularly limited, but can be blended into cosmetics for external application to the skin or hair, such as skin care products, hair products, makeup products, and UV protection products. The product form is also not particularly limited, but can be in the form of an emulsion, cream, solid, paste, gel, multi-layered, mousse, spray, or the like.
[0079] The cosmetic of the present invention may contain any aqueous and oily components that can be used in the cosmetic field. The aqueous and oily components are not particularly limited, and examples include oils, surfactants, humectants, higher alcohols, sequestering agents, water-soluble natural, semi-synthetic, and synthetic polymers, water-soluble and oil-soluble polymers, organic UV filters, and various extracts. If necessary, the cosmetic may also contain various powders, such as inorganic and organic pigments, inorganic and organic clay mineral powders, inorganic and organic pigments treated with metal soaps or silicones, coloring agents such as organic dyes, and other pharmaceutical ingredients, such as preservatives, antioxidants, coloring agents, thickeners, emulsifying thickeners, pH adjusters, fragrances, cooling agents, antiperspirants, disinfectants, skin activators, anti-inflammatory agents, whitening agents, and film-forming agents. Specifically, the desired cosmetic can be produced by conventional methods by blending one or more of the ingredients listed below. The amounts of these ingredients are not particularly limited as long as they do not impair the effects of the present invention. Furthermore, inorganic powders of ultraviolet scattering agents such as titanium dioxide and cerium oxide may be used to the extent that the object of the present invention is not impaired. The cosmetic composition of the present invention may be formulated as a non-silicone-based composition, or may be formulated to contain silicone-based materials such as silicone-based oils such as methylsilicone and methylphenylsilicone, depending on the purpose.
[0080] The oils are not particularly limited, and examples thereof include avocado oil, camellia oil, turtle oil, macadamia nut oil, corn oil, mink oil, olive oil, rapeseed oil, egg yolk oil, sesame oil, persic oil, wheat germ oil, camellia oil, castor oil, linseed oil, safflower oil, cottonseed oil, perilla oil, soybean oil, peanut oil, tea seed oil, kaya oil, rice bran oil, Chinese tung oil, Japanese tung oil, jojoba oil, germ oil, triglycerin, glycerin trioctanoate, glycerin triisopalmitate, cacao butter, coconut oil, horse tallow, hydrogenated coconut oil, palm oil, beef tallow, mutton tallow, hydrogenated beef tallow, palm kernel oil, lard, beef bone fat, Japan wax kernel oil, hydrogenated oil, beef trotter fat, Japan wax, hydrogenated castor oil, beeswax, candelilla wax, cotton wax, carnauba wax, bayberry wax, and bayberry wax. Examples of suitable waxes include bottle wax, spermaceti wax, montan wax, bran wax, lanolin, kapok wax, lanolin acetate, liquid lanolin, sugarcane wax, lanolin fatty acid isopropyl, hexyl laurate, reduced lanolin, jojoba wax, hard lanolin, shellac wax, POE lanolin alcohol ether, POE lanolin alcohol acetate, POE cholesterol ether, lanolin fatty acid polyethylene glycol, POE hydrogenated lanolin alcohol ether, liquid paraffin, ozokerite, pristane, paraffin, ceresin, squalene, petrolatum, microcrystalline wax, propylene glycol dicaprate, ethylhexyl palmitate, and isotridecyl isononanoate.
[0081] The surfactant is not particularly limited, and examples thereof include lipophilic nonionic surfactants, hydrophilic nonionic surfactants, and other surfactants. The lipophilic nonionic surfactant is not particularly limited, and examples thereof include sorbitan fatty acid esters such as sorbitan monooleate, sorbitan monoisostearate, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan sesquioleate, sorbitan trioleate, diglycerol sorbitan penta-2-ethylhexylate, and diglycerol sorbitan tetra-2-ethylhexylate; glycerin polyglycerin fatty acids such as glycerin monocottonseed oil fatty acid, glycerin monoerucate, glycerin sesquioleate, glycerin monostearate, α,α'-oleic acid pyroglutamate, and glycerin monostearate malate; propylene glycol fatty acid esters such as propylene glycol monostearate; hydrogenated castor oil derivatives; and glycerin alkyl ethers.
[0082] The hydrophilic nonionic surfactant is not particularly limited, and examples thereof include POE sorbitan fatty acid esters (e.g., polysorbate 60) such as POE sorbitan monooleate, POE sorbitan monostearate, and POE sorbitan tetraoleate; POE sorbitan fatty acid esters such as POE sorbitan monolaurate, POE sorbitan monooleate, POE sorbitan pentaoleate, and POE sorbit monostearate; POE glycerin monostearate, POE glycerin monoisostearate, and POE glycerin triisostearate; POE glycerin fatty acid esters such as stearate, POE fatty acid esters such as POE monooleate, POE distearate, POE dioleate, and ethylene glycol distearate, POE alkyl ethers such as POE lauryl ether, POE oleyl ether, POE stearyl ether, POE behenyl ether, POE 2-octyldodecyl ether, and POE cholestanol ether, and POE alkyl phenyl ethers such as POE octylphenyl ether, POE nonylphenyl ether, and POE dinonylphenyl ether. POE-POP alkyl ethers such as POE-POP cetyl ether, POE-POP 2-decyltetradecyl ether, POE-POP monobutyl ether, POE-POP hydrogenated lanolin, POE-POP glycerin ether, tetraPOE-tetraPOP ethylenediamine condensates such as Tetronic, POE castor oil, POE hydrogenated castor oil, POE hydrogenated castor oil monoisostearate, POE hydrogenated castor oil triisostearate, POE hydrogenated castor oil monopyroglutamic acid monoisostearyl phosphate diesters, POE castor oil derivatives such as POE hydrogenated castor oil maleic acid, POE beeswax / lanolin derivatives such as POE sorbitol beeswax, alkanolamides such as coconut oil fatty acid diethanolamide, lauric acid monoethanolamide, fatty acid isopropanolamide, POE propylene glycol fatty acid esters, POE alkylamines, POE fatty acid amides, sucrose fatty acid esters, POE nonylphenyl formaldehyde condensates, alkylethoxydimethylamine oxide, trioleyl phosphate, and the like.
[0083] Examples of the other surfactants include anionic surfactants such as fatty acid soaps, higher alkyl sulfate ester salts, POE triethanolamine lauryl sulfate, and alkyl ether sulfate ester salts; cationic surfactants such as alkyltrimethylammonium salts, alkylpyridinium salts, alkyl quaternary ammonium salts, alkyldimethylbenzylammonium salts, POE alkylamines, alkylamine salts, and polyamine fatty acid derivatives; and amphoteric surfactants such as imidazoline-based amphoteric surfactants and betaine-based surfactants, which may be blended within a range that does not cause problems in terms of stability and skin irritation.
[0084] The moisturizer is not particularly limited, and examples thereof include xylitol, sorbitol, maltitol, chondroitin sulfate, hyaluronic acid, mucoitin sulfate, caronic acid, atelocollagen, cholesteryl-12-hydroxystearate, sodium lactate, bile salts, dl-pyrrolidone carboxylate, short-chain soluble collagen, diglycerin (EO)PO adduct, Rosa robur extract, yarrow extract, melilot extract, and the like.
[0085] The higher alcohol is not particularly limited, and examples thereof include straight-chain alcohols such as lauryl alcohol, cetyl alcohol, stearyl alcohol, behenyl alcohol, myristyl alcohol, oleyl alcohol, and cetostearyl alcohol; and branched-chain alcohols such as monostearyl glycerin ether (batyl alcohol), 2-decyltetradecynol, lanolin alcohol, cholesterol, phytosterol, hexyldodecanol, isostearyl alcohol, and octyldodecanol.
[0086] The sequestering agent is not particularly limited, and examples thereof include 1-hydroxyethane-1,1-diphosphonic acid, 1-hydroxyethane-1,1-diphosphonic acid tetrasodium salt, sodium citrate, sodium polyphosphate, sodium metaphosphate, gluconic acid, phosphoric acid, citric acid, ascorbic acid, succinic acid, and edetic acid.
[0087] The natural water-soluble polymer is not particularly limited, and examples thereof include plant-based polymers such as gum arabic, tragacanth gum, galactan, guar gum, carob gum, karaya gum, carrageenan, pectin, agar, quince seed (marmelo), algae colloid (cassowia extract), starch (rice, corn, potato, wheat), and glycyrrhizic acid; microbial-based polymers such as xanthan gum, dextran, succinoglucan, and pullulan; and animal-based polymers such as collagen, casein, albumin, and gelatin.
[0088] The semi-synthetic water-soluble polymer is not particularly limited, and examples thereof include starch-based polymers such as carboxymethyl starch and methylhydroxypropyl starch; cellulose-based polymers such as methyl cellulose, nitrocellulose, ethyl cellulose, methylhydroxypropyl cellulose, hydroxyethyl cellulose, sodium cellulose sulfate, hydroxypropyl cellulose, sodium carboxymethyl cellulose (CMC), crystalline cellulose and cellulose powder; and alginic acid-based polymers such as sodium alginate and propylene glycol alginate.
[0089] The synthetic water-soluble polymer is not particularly limited, and examples thereof include vinyl polymers such as polyvinyl alcohol, polyvinyl methyl ether, and polyvinylpyrrolidone; polyoxyethylene polymers such as polyethylene glycol 20,000, 40,000, and 60,000; polyoxyethylene-polyoxypropylene copolymer polymers; acrylic polymers such as sodium polyacrylate, polyethyl acrylate, and polyacrylamide; polyethyleneimine; and cationic polymers.
[0090] The inorganic water-soluble polymer is not particularly limited, and examples thereof include bentonite, AlMg silicate (veegum), laponite, hectorite, and silicic anhydride.
[0091] The organic ultraviolet screening agent is not particularly limited, and examples thereof include benzoic acid-based ultraviolet screening agents such as para-aminobenzoic acid (hereinafter abbreviated as PABA), PABA monoglycerin ester, N,N-dipropoxy PABA ethyl ester, N,N-diethoxy PABA ethyl ester, N,N-dimethyl PABA ethyl ester, and N,N-dimethyl PABA butyl ester; anthranilic acid-based ultraviolet screening agents such as homomenthyl-N-acetylanthranilate; amyl salicylate, menthyl salicylate, homomenthyl salicylate, and the like. salicylic acid-based ultraviolet screening agents such as ethylhexyl p-methoxycinnamate, octyl cinnamate, phenyl salicylate, benzyl salicylate, and p-isopropanol phenyl salicylate; ethylhexyl p-methoxycinnamate, octyl cinnamate, ethyl-4-isopropyl cinnamate, methyl-2,5-diisopropyl cinnamate, ethyl-2,4-diisopropyl cinnamate, methyl-2,4-diisopropyl cinnamate, propyl-p-methoxycinnamate, isopropyl-p-methoxycinnamate, isoamyl cinnamic acid-based ultraviolet screening agents such as 2-methyl-p-methoxycinnamate, 2-ethoxyethyl-p-methoxycinnamate, cyclohexyl-p-methoxycinnamate, ethyl-α-cyano-β-phenylcinnamate, 2-ethylhexyl-α-cyano-β-phenylcinnamate, and glyceryl mono-2-ethylhexanoyl-di-para-methoxycinnamate; 2,4-dihydroxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, and 2,2'-dihydroxy-4,4'-dimethoxybenzophenone; benzophenone-based ultraviolet screening agents such as benzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-4'-methylbenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonate, 4-phenylbenzophenone, 2-ethylhexyl-4'-phenyl-benzophenone-2-carboxylate, 2-hydroxy-4-n-octoxybenzophenone, and 4-hydroxy-3-carboxybenzophenone;Examples include 3-(4'-methylbenzylidene)-d,l-camphor, 3-benzylidene-d,l-camphor, urocanic acid, urocanic acid ethyl ester, 2-phenyl-5-methylbenzoxazole, 2,2'-hydroxy-5-methylphenylbenzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, dibenzalazine, dianisoylmethane, 4-methoxy-4'-t-butyldibenzoylmethane, 5-(3,3-dimethyl-2-norbornylidene)-3-pentan-2-one, and the like;
[0092] The various extracts are not particularly limited, and examples thereof include houttuynia cordata extract, phellodendron bark extract, melilot extract, dead nettle extract, licorice extract, peony extract, soapwort extract, loofah extract, cinchona extract, saxifrage extract, sophora flavescens extract, watercress extract, fennel extract, primrose extract, rose extract, rehmannia root extract, lemon extract, lithospermum root extract, aloe extract, calamus root extract, eucalyptus extract, horsetail extract, sage extract, thyme extract, tea extract, seaweed extract, cucumber extract, clove extract, raspberry extract, melissa extract, carrot extract, horse chestnut extract, peach extract, peach leaf extract, mulberry extract, knettleflower extract, witch hazel extract, placenta extract, thymus extract, silk extract, and licorice extract.
[0093] Examples of the various powders include luster pigments such as red iron oxide, yellow iron oxide, black iron oxide, titanium mica, iron oxide-coated titanium mica, and titanium oxide-coated glass flakes; inorganic powders such as mica, talc, kaolin, sericite, titanium dioxide, and silica; and organic powders such as polyethylene powder, nylon powder, cross-linked polystyrene, cellulose powder, and silicone powder. Preferably, in order to improve sensory properties and cosmetic durability, part or all of the powder components may be treated with a substance such as silicones, fluorine compounds, metal soaps, oils, and acyl glutamates by a known method to make them water-repellent.
[0094] Other pharmaceutical ingredients are not particularly limited, and examples include vitamins such as vitamin A oil, retinol, retinol palmitate, inositol, pyridoxine hydrochloride, benzyl nicotinate, nicotinamide, DL-α-tocopherol nicotinate, magnesium ascorbyl phosphate, 2-O-α-D-glucopyranosyl-L-ascorbic acid, vitamin D2 (ergocaciferol), dl-α-tocopherol, dl-α-tocopherol acetate, pantothenic acid, and biotin; hormones such as estradiol and ethinyl estradiol; amino acids such as arginine, aspartic acid, cystine, cysteine, methionine, serine, leucine, and tryptophan; anti-inflammatory agents such as allantoin and azulene, whitening agents such as arbutin, and astringents such as tannic acid.
[0095] The cosmetic of the present invention is not particularly limited in its manufacturing method, and may be manufactured by a manufacturing method appropriate for the form of the cosmetic. Specifically, for example, the cosmetic can be obtained by mixing the dispersion of the present invention with other components.
[0096] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" are "% by mass" and "parts by mass" without any particular limitation.
[0097] (Production Example of Raw Zinc Oxide Cake) 80 g of FINEX-50 (manufactured by Sakai Chemical Industry Co., Ltd., primary particle size: 0.020 μm) was repulped in 1200 ml of an aqueous zinc acetate solution having a zinc acetate concentration of 0.135 mol / L to prepare a slurry. Subsequently, the slurry was heated to 70°C over 42 minutes while stirring, and aged at 70°C for 2 hours while stirring. After aging, the slurry was filtered and washed with water. Subsequently, the obtained solid was repulped in 3 liters of water to prepare a slurry, which was heated to 95°C while stirring, and heated and washed at 95°C for 60 minutes while stirring. After heating and washing, the slurry was filtered and washed with water to obtain a zinc oxide cake.
[0098] Example 1: 30 g of zinc oxide pure content was weighed out from the zinc oxide cake obtained in the Production Example and repulped in pure water to a powder concentration of 100 g / L to prepare a zinc oxide slurry. 0.45 g of 30% caustic soda was added to the pure water and heated to 90°C. Then, 0.9 g (3.0% based on zinc oxide) of stearic acid (Fujifilm Wako Pure Chemical Industries, Ltd., stearic acid, plant-derived) was added to obtain a sodium stearate aqueous solution. The sodium stearate aqueous solution (90°C) was added to the zinc oxide slurry heated to 90°C, and the mixture was aged for 2 hours while maintaining the temperature at 90°C. After aging, the mixture was cooled to 70°C, adjusted to pH 7.0 with sulfuric acid, filtered, washed with water, and dried at 120°C for 16 hours to obtain stearic acid-treated zinc oxide particles. The physical properties of the resulting particles and the coating were evaluated and are shown in Table 1. The melting point of stearic acid is 70°C.
[0099] (Example 2) Stearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that 0.3 g of 30% caustic soda was added to pure water, the mixture was heated to 90°C, and then 0.6 g of stearic acid (2.0% based on zinc oxide) was added to obtain an aqueous sodium stearate solution, and the mixture was filtered, washed with water, and then dried at 80°C.
[0100] (Example 3) Isostearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that stearic acid was replaced with isostearic acid (isostearic acid (mixture of isomers) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) The melting point of isostearic acid is 7°C.
[0101] Example 4 Palmitic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that palmitic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of stearic acid. The melting point of palmitic acid is 64°C.
[0102] Comparative Example 1 Stearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that they were dried at 80° C. for 16 hours.
[0103] Comparative Example 2 Stearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that the amount of 30% caustic soda was 1.5 g and the amount of stearic acid was 3.0 g (10.0% based on the zinc oxide).
[0104] (Comparative Example 3) Zinc oxide powder was obtained by drying the zinc oxide cake obtained in Production Example at 120°C for 16 hours. 30 g of the obtained zinc oxide powder was placed in a plastic bag, and 1.2 g (4.0% based on the zinc oxide) of stearic acid was added and mixed, followed by heat treatment in a dryer at 120°C for 16 hours to obtain stearic acid-treated zinc oxide particles.
[0105] Comparative Example 4 Stearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that the zinc oxide cake obtained in Production Example was changed to FINEX-30 (manufactured by Sakai Chemical Industry Co., Ltd., average particle size 35 nm), the amount of 30% caustic soda was changed to 0.6 g, and the amount of stearic acid was changed to 1.2 g (4.0% based on zinc oxide).
[0106] Comparative Example 5 Stearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that 0.45 g of 30% caustic soda was added to the zinc oxide slurry, the mixture was heated to 40°C, 0.9 g of stearic acid (3.0% based on the zinc oxide) was added, and the mixture was aged for 2 hours while maintaining the temperature at 40°C.
[0107] Comparative Example 6 Isostearic acid-treated zinc oxide particles were obtained in the same manner as in Comparative Example 2, except that stearic acid was changed to isostearic acid.
[0108] (Evaluation Method 1) Composition of Obtained Particles The composition of the obtained particles shown in Table 1 is the result of analysis using an X-ray diffractometer Ultima III (manufactured by Rigaku Corporation) equipped with a copper tube.
[0109] (Evaluation Method 2) Primary Particle Diameter The primary particle diameter in this specification is calculated as the average particle diameter of 250 particles randomly selected from a 20,000 to 50,000-fold field of view in a photograph taken with a transmission electron microscope JEM-1200EX II (manufactured by JEOL Ltd.) by measuring the particle diameters of the 250 particles.
[0110] (Evaluation Method 3) BET Specific Surface Area The BET specific surface area (m 2 / g) is a value measured using a fully automatic BET specific surface area measuring device Macsorb Model HM-1200 (manufactured by Mountech Co., Ltd.).
[0111] (Evaluation Method 4) Carbon Content The carbon contents in Table 1 are values measured using a carbon amount measuring device, CARBON ANALYZER EMIA-110 (manufactured by Horiba Ltd.).
[0112] (Evaluation Method 5) Mode Diameter In this specification, the mode diameter is a value measured using a laser diffraction / scattering particle size distribution analyzer LA-960S (manufactured by Horiba, Ltd.). 0.1 g of zinc oxide particles from each of the Examples and Comparative Examples was placed in 50 ml of isopropyl alcohol, and the slurry was ultrasonically dispersed for 1 minute using an ultrasonic homogenizer US-600E (manufactured by Nippon Seiki Seisakusho, Ltd.). The measurement was performed on a volume basis, with the refractive index of the zinc oxide from each of the Examples and Comparative Examples being 2.00 and the refractive index of isopropyl alcohol being 1.378. When the mode diameter of the slurry ultrasonically dispersed for 1 minute is 0.30 μm or less, this means that many particles close to the primary particle size are present even with weak dispersion, and therefore the dispersibility is high. When the mode diameter exceeds 0.30 μm, this means that the particles are strongly agglomerated and the dispersibility is low.
[0113] (Evaluation Method 6) Water Repellency 80 mL of distilled water was placed in a 100 mL beaker, 0.2 g of fatty acid-treated zinc oxide particles was floated on it, and the mixture was stirred 10 times with a spatula. The water was visually inspected for turbidity and evaluated according to the following evaluation criteria: ◯: Water was clear and not turbid; △: Water was slightly turbid and semi-transparent; ×: Water was cloudy
[0114] (Evaluation Method 7) Apparent Density: Measured by the method described in JIS K 5101-12-1 Pigment Test Methods - Apparent Density or Apparent Specific Volume (Static Method).
[0115] (Evaluation Method 8) FT-IR The FT-IR spectra in Figures 1 and 2 were measured using a Fourier transform infrared spectrophotometer FT-IR Nicolet iS 10 (manufactured by Thermo Fisher Scientific) under the following conditions: detector: DTGS KBr, resolution: 4 cm -1 The measurement was performed with 16 scans. The attached equipment was a single-reflection horizontal ATR Smart iTR, the plate (IRE) used was a diamond crystal, and the angle of incidence was 45°. The absorbance I 1 The value is 1350-1500 cm -1 Detected in CH3 Symmetric bending vibration, COO - Symmetric stretching vibration, CH 3 The absorbance of the maximum peak of any of the asymmetric bending vibrations, absorbance I 2 The value is 1500-1600 cm -1 COO - This is the absorbance value of the maximum peak of the antisymmetric stretching vibration. 2 / I 1 When the absorbance I is between 0.8 and 1.2, it means that the fatty acid is bonded to the zinc oxide surface, when it is greater than 1.2, it means that free fatty acid Zn is precipitated, and when it is less than 0.8, it means that the fatty acid is not sufficiently bonded to the zinc oxide surface. 3 The value is 1700-1720 cm -1 The absorbance of the C═O stretching vibration peak detected at 4 The value is 1750-1800 cm -1 This is the absorbance value of the peaks of the C=O stretching vibration of four-membered rings, five-membered rings, and acid anhydrides, which are detected in the present manufacturing process. Since there are no substances corresponding to four-membered rings, five-membered rings, or acid anhydrides, no peaks are detected. Therefore, I 3 / I 4 If the value is greater than 1.2, it means that unreacted fatty acid remains.
[0116] (Examples 5 to 8 and Comparative Examples 7 to 12) Dispersions of fatty acid-treated zinc oxide particles having the compositions shown in Table 2 were prepared by the manufacturing method described below, and each sample was evaluated for "initial viscosity," "viscosity after 40°C," and "stability over time." The results are also shown in Table 2. (Manufacturing Method) The fatty acid-treated zinc oxide particles of the Examples and Comparative Examples, polyhydroxystearic acid (Salacos HS-6C, manufactured by Nisshin Oillio Co., Ltd.), and isotridecyl isononanoate (Salacos 913, manufactured by Nisshin Oillio Co., Ltd.) were placed in a mayonnaise jar in the proportions shown in Table 2, along with zirconia beads (0.5 mm, manufactured by Toray Industries, Inc.) in an amount twice the total amount of the components. The mixture was thoroughly stirred, and then fixed to a paint conditioner (manufactured by RED DEVIL Co., Ltd.) and vibrated for 60 minutes to produce a dispersion. The evaluation results of the physical properties of the resulting dispersions are shown in Table 2.
[0117] (Initial Viscosity) After dispersion, the dispersion was placed in a 9 ml screw bottle, and the viscosity (25°C) was measured 60 seconds after the start of rotation at 12 rpm using a B-type viscometer (manufactured by Tokyo Keiki) with a rotor No. 4.
[0118] (Viscosity over time at 40°C) The dispersion was placed in a 9 ml screw bottle and stored in a thermostatic chamber at 40°C for 7 days, and the viscosity was measured 60 seconds after the start of rotation at 12 rpm using a B-type viscometer (manufactured by Tokyo Keiki) with a rotor No. 4.
[0119] (Stability over time) After storage for 7 days in a 40°C thermostatic chamber, the state was evaluated according to the following criteria: ⊚: no settling and viscosity less than 1000 mPa·s ◯: no settling and viscosity 1000 mPa·s or more and less than 2000 mPa·s △: no settling and viscosity 2000 mPa·s or more and less than 3000 mPa·s ×: settling occurred or viscosity 3000 mPa·s or more
[0120]
[0121]
[0122] Table 1 shows that the fatty acid-treated zinc oxide particles of the examples have excellent dispersibility and sufficient water repellency. Furthermore, Table 2 shows that there was no significant increase in the initial viscosity or viscosity over time, indicating that the particles also have excellent stability.
[0123] Example 9 (Sunscreen O / W Cream) A sunscreen O / W cream was prepared using the ingredients shown in Table 3 below and by the following manufacturing method. (Manufacturing Method) (1) Components 1 to 6 were mixed uniformly and dissolved by heating. (2) Components 7 to 12 were mixed uniformly and heated. (3) Components (1) above was added to components (2) above to emulsify, and the mixture was cooled to obtain a sunscreen O / W cream.
[0124] (Note 1) (Sodium acrylate / sodium acryloyldimethyltaurate) copolymer: SIMULGEL EG QD (manufactured by SEPPIC) (Note 2) Plant-derived cellulose (2% aq): RHEOCRYSTA C-2SP (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.)
[0125] The sunscreen O / W cream of Example 9 obtained as described above was stable without changing over time, and in terms of feel during use, it spread smoothly and well on the skin upon application, left no sticky or squeaky feeling on the skin after application, was highly transparent, and was an organic UV absorber-free sunscreen O / W cream with excellent durability of sunscreen effect.
[0126] The dispersion of the present invention can be suitably used by being blended into cosmetics.
Claims
1. In the FT-IR spectrum measured using the attenuated total reflection method (ATR method), -1 The maximum absorbance (I 1 ) at 1500-1600 cm -1 The maximum absorbance (I 2 ) ratio (I 2 / I 1 ) is 0.8 to 1.2, and -1 The maximum absorbance (I 4 ) 1700-1720 cm -1 The maximum absorbance (I 3 ) ratio (I 3 / I 4 ) is 1.2 or less, the primary particle diameter as measured by a transmission electron microscope is 0.1 μm or less, and the powder is placed in isopropyl alcohol, and the powder is dispersed by irradiating it with ultrasonic waves at a rated output of 600 W and a vibration amplitude of 100% for 1 minute at room temperature, and the mode diameter on a volume basis as measured by a laser diffraction scattering method of the dispersion liquid is 0.30 μm or less.
2. The zinc oxide particles treated with a fatty acid according to claim 1, wherein the fatty acid is at least one selected from the group consisting of stearic acid, isostearic acid, and palmitic acid.
3. A method for producing fatty acid-treated zinc oxide particles, comprising the steps of: (1) repulping zinc oxide particles as raw material in a dispersion medium to prepare a slurry; (2) neutralizing a fatty acid with a base to obtain an aqueous fatty acid salt solution; and (3) adding the obtained aqueous fatty acid salt solution to the zinc oxide slurry for surface treatment, wherein the zinc oxide particles as raw material are obtained by a production method including a step of maturing fine zinc oxide particles in water containing dissolved zinc salt, and are subjected to step (1) without a drying step, and steps (2) and (3) are carried out at a temperature equal to or higher than the melting point of the fatty acid.
4. A method for producing fatty acid-treated zinc oxide particles as described in claim 3, in which the raw material zinc oxide particles are dispersed by placing the powder in a 0.0025 mass% aqueous solution of sodium hexametaphosphate and irradiating it with ultrasound at a rated output of 600 W and a vibration amplitude of 100% using an ultrasonic homogenizer for 3 minutes at room temperature, and the median diameter of the dispersion measured by laser diffraction scattering method is 0.30 μm or less.
5. A dispersion comprising the fatty acid-treated zinc oxide particles according to claim 1 or 2.
6. A cosmetic preparation comprising the fatty acid-treated zinc oxide particles according to claim 1 or 2.
Citation Information
Patent Citations
Production method of surface-coated zinc oxide particle
JP2016196381A
Seedling transplanter
JP2021083334A
Zinc oxide particles, production method for same, cosmetic material, heat-dissipating filler, heat-dissipating resin composition, heat-dissipating grease, and heat-dissipating coating composition
WO2012147888A1
Ultrafine, particulate zinc oxide silicone dispersion, its production and ultraviolet screening cosmetic
JP2000191489A
sunscreen composition