Wavelength-selective retardation plate and optical element
The wavelength-selective retardation plate with strategically designed wave plates and liquid crystal alignment minimizes phase differences across incident angles, addressing color misalignment and enabling miniaturization in AR and VR glasses by ensuring consistent diffraction of light across wavelengths.
Patent Information
- Application Number
- PCT/JP2024/011895
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
In optical devices such as AR and VR glasses, wavelength-selective retardation plates face challenges in minimizing the phase difference between light incident from the front direction and oblique directions, leading to color misalignment issues due to varying diffraction angles based on wavelength, which complicates the miniaturization and thinning of diffraction elements.
A wavelength-selective retardation plate configuration with multiple wave plates having different slow axis directions and Nz factors between 0.3 and 0.7, utilizing optically anisotropic layers with rod-like and discotic liquid crystal compounds, and a liquid crystal alignment pattern that rotates continuously, compensates for refractive index differences to minimize phase differences across different incident angles.
This configuration ensures that light of different wavelengths is diffracted in nearly the same direction, reducing color misalignment and enabling the miniaturization of optical elements while maintaining desired diffraction performance.
Smart Images

Figure JP2024011895_03102024_PF_FP_ABST
Abstract
Description
Wavelength-selective retardation plate, optical element
[0001] The present invention relates to a wavelength-selective retardation plate and an optical element.
[0002] Optical elements that control the direction of light are used in many optical devices and optical systems. For example, optical elements that control the direction of light are used in various optical devices, such as head-mounted displays (HMDs) such as AR (Augmented Reality) glasses, VR (Virtual Reality) glasses, and MR (Mixed Reality) glasses, which superimpose virtual images and various information on an actually viewed scene, head-up displays (HUDs), backlights of liquid crystal display devices, projectors, beam steering, and sensors for detecting objects and measuring the distance to objects. As an example, in VR glasses, an image displayed on a display (optical engine) is magnified by a lens-based optical system, and the light emitted from the display is focused at the position of the user's eyes, allowing the user to view the virtual image. It is known that VR glasses use a diffraction element (including a hologram) as a lens-based magnifying optical system, and the diffraction element diffracts light emitted from a display to focus the light toward the user's eyes (see Patent Documents 1 and 2). Furthermore, AR glasses, for example, display an image displayed by a display (optical engine) by entering one end of a light guide plate, propagating therethrough, and emitting it from the other end, thereby superimposing a virtual image on the scene the user is actually viewing. AR glasses use a diffraction element to diffract (refract) light from the display (projected light) and cause it to enter one end of the light guide plate. This allows the light to be introduced into the light guide plate at an angle and propagate within the light guide plate. The light propagating through the light guide plate is then diffracted by the diffraction element at the other end of the light guide plate and emitted from the light guide plate toward the user's viewing position.
[0003] The diffraction angle of light by a diffraction element varies depending on the wavelength of the light. That is, the traveling direction of light diffracted by a diffraction element differs depending on the wavelength of the light. Therefore, when light of different wavelengths is diffracted by a single diffraction element, for example, in a color image consisting of red, green, and blue images, the positions of the red, green, and blue images will differ, resulting in so-called color shift.
[0004] In order to eliminate color shift, it is conceivable to use a wavelength-selective retardation plate to adjust the traveling direction of light depending on the wavelength, as disclosed in, for example, Non-Patent Document 1. Non-Patent Document 1 discloses that stacking a λ plate and a 2λ plate so that their slow axes form a specific angle functions as a wavelength-selective retardation plate. Non-Patent Document 1 also discloses that the wavelength-selective retardation plate can be used in a wavelength-selective beam splitter or beam combiner.
[0005] International Publication No. 2021 / 150510 International Publication No. 2022 / 045167
[0006] GD Sharp, JR Birge, Retarder stack Technology for Color Manipulation, SID 1999 DIGEST, pp.1072-1075
[0007] In recent years, there has been a demand for further miniaturization and thinning of VR glasses and AR glasses. To achieve further miniaturization and thinning, optical path designs may be used in which light is incident on the diffraction element from a direction inclined (oblique) from the front direction and diffracted. With such optical path designs, light incident on the diffraction element from the front direction and light incident on the diffraction element from an oblique direction must be diffracted in desired directions. Furthermore, to achieve further miniaturization and thinning, regions with large diffraction angles of light in the diffraction element may be provided. With such optical path designs, diffracted light travels obliquely within the diffraction element. Therefore, when using a wavelength-selective retardation plate as described above, light is incident on the wavelength-selective retardation plate from an oblique direction. The present inventors have studied the wavelength-selective retardation plate described in Non-Patent Document 1 and found that there is a large difference in phase difference between light incident from the front direction and light incident from an oblique direction. If the difference in the phase difference is large, the diffraction direction may not be as desired when a wavelength-selective retardation plate and a diffraction element are used in combination. Therefore, it has been desired to reduce the difference in the phase difference.
[0008] Therefore, an object of the present invention is to provide a wavelength-selective retardation plate that has a small difference between the phase difference occurring when light is incident from the front direction and the phase difference occurring when light is incident from an oblique direction, and to provide an optical element using the wavelength-selective retardation plate.
[0009] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. That is, they have found that the above problems can be solved by the following configuration.
[0010] [1] A wavelength-selective retardation plate having a plurality of wave plates, wherein the wavelength-selective retardation plate changes the phase of polarized light in a first wavelength range but does not change the phase of polarized light in a second wavelength range different from the first wavelength range, the plurality of wave plates have different slow axis orientations, and the plurality of wave plates each have an Nz factor of more than 0.3 and less than 0.7. [2] The wavelength-selective retardation plate according to [1], wherein each of the plurality of wave plates includes at least an optically anisotropic layer A having an Nz factor of more than 0.5 and an optically anisotropic layer B having an Nz factor of less than 0.5, and the angle between the in-plane slow axis of the optically anisotropic layer A and the in-plane slow axis of the optically anisotropic layer B is 45° or less. [3] The wavelength-selective retardation plate according to [2], wherein the optically anisotropic layer A is formed using a composition containing a rod-shaped liquid crystal compound, and the optically anisotropic layer B is formed using a composition containing a discotic liquid crystal compound. [4] The wavelength-selective retardation plate according to [2] or [3], wherein at least one of the optically anisotropic layer A and the optically anisotropic layer B is a layer formed by fixing the alignment direction of a twisted liquid crystal compound. [5] An optical element comprising: a plurality of optically anisotropic layers formed using a composition containing a liquid crystal compound, the layers having a liquid crystal orientation pattern in which the orientation of the optical axis derived from the liquid crystal compound changes while continuously rotating along at least one direction in a plane; and a wavelength-selective retardation plate according to any one of [1] to [4], disposed between at least a pair of the plurality of optically anisotropic layers, wherein the rotation directions of the orientations of the optical axes in the adjacent two optically anisotropic layers are opposite to each other; the first wavelength region includes wavelengths longer than those in the second wavelength region; the wavelength-selective retardation plate converts circularly polarized light in the first wavelength region into circularly polarized light having an opposite rotation direction, without changing the phase of circularly polarized light in the second wavelength region; and wherein, in the liquid crystal orientation pattern, when the length of a 180° rotation of the orientation of the optical axis in the one direction in which the orientation of the optical axis changes while continuously rotating is defined as one period, the length of one period of at least one of the optically anisotropic layers is different from that of the other optically anisotropic layers.
[0011] According to the present invention, it is possible to provide a wavelength-selective retardation plate that has a small difference between the phase difference occurring when light is incident from the front direction and the phase difference occurring when light is incident from an oblique direction.The present invention also provides an optical element using the wavelength-selective retardation plate.
[0012] 14 is a schematic diagram of a wavelength-selective retardation plate of the present invention; FIG. 15 is a diagram showing the relationship between the slow axis orientations of the wave plates in the wavelength-selective retardation plate of the present invention; FIG. 16 is a diagram conceptually showing an example of an optical element of the present invention; FIG. 17 is a diagram conceptually showing an optically anisotropic layer of the optical element shown in FIG. 3; FIG. 18 is a plan view of the optically anisotropic layer of the optical element shown in FIG. 3; FIG. 19 is a conceptual diagram showing the function of the optically anisotropic layer of the optical element shown in FIG. 3; FIG. 19 is a conceptual diagram showing the function of the optical element shown in FIG. 3; FIG. 20 is a conceptual diagram showing the function of the optical element shown in FIG. 21; FIG. 22 is a diagram conceptually showing another example of the optical element of the present invention; FIG. 23 is a conceptual diagram showing the function of the optical element shown in FIG. 22; FIG. 24 is a diagram conceptually showing an example of an exposure apparatus for exposing an alignment film of the optical element shown in FIG. 3; FIG. 25 is a plan view of another example of the optically anisotropic layer of the optical element of the present invention; FIG. 26 is a diagram conceptually showing an example of an exposure apparatus for exposing an alignment film that forms the optically anisotropic layer shown in FIG. 14; FIG. 2 is a diagram conceptually illustrating another example of the optically anisotropic layer of the optical element of the present invention.
[0013] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.
[0014] The following describes the meaning of each description in this specification. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this specification, "same" is intended to include a margin of error generally accepted in the technical field. Furthermore, in this specification, when terms such as "all," "all," and "entirely," are used, in addition to the case of 100%, they are intended to include a margin of error generally accepted in the technical field, for example, 99% or more, 95% or more, or 90% or more.
[0015] In this specification, visible light refers to electromagnetic waves with wavelengths visible to the human eye, and refers to light in the wavelength range of 380 to 780 nm. Invisible light refers to light in wavelength ranges less than 380 nm and greater than 780 nm. Furthermore, although not limited thereto, visible light includes light in the wavelength range of 420 to 490 nm as blue light, light in the wavelength range of 495 to 570 nm as green light, and light in the wavelength range of 620 to 750 nm as red light.
[0016] In this specification, Re(λ) represents the in-plane retardation at a wavelength λ. Unless otherwise specified, the wavelength λ is 550 nm. In this specification, Re(λ) is a value measured at a wavelength λ using an AxoScan (manufactured by Axometrics). By inputting the average refractive index ((nx + ny + nz) / 3) and film thickness (d (μm)) into AxoScan, the following slow axis direction (°) is calculated: Re(λ) = R0(λ) Rth(λ) = ((nx + ny) / 2 - nz) × d Note that R0(λ) is displayed as a numerical value calculated by AxoScan, but it means Re(λ). Furthermore, nx represents the refractive index in the in-plane slow axis direction, ny represents the refractive index in the in-plane direction perpendicular to the in-plane slow axis, and nz represents the refractive index in the thickness direction. In addition, in this specification, the Nz factor is a value given by Nz = (nx - nz) / (nx - ny), where nx is the refractive index in the in-plane slow axis direction, ny is the refractive index in the direction perpendicular to the in-plane slow axis, and nz is the refractive index in the thickness direction, all measured by AxoScan.
[0017] [Wavelength-Selective Retardation Plate] The wavelength-selective retardation plate of the present invention includes a plurality of wave plates. Each of the plurality of wave plates has a different slow axis orientation, and each of the plurality of wave plates has an Nz factor greater than 0.3 and less than 0.7. The wavelength-selective retardation plate of the present invention changes the phase of polarized light in a first wavelength range, but does not change the phase of polarized light in a second wavelength range different from the first wavelength range. The principle behind this is explained below. The refractive index of materials typically used in wave plates varies depending on wavelength. Therefore, the phase difference imparted by a wave plate is given by the product of the refractive index difference and the thickness of the wave plate. Therefore, in a wave plate, the phase difference imparted to light of each wavelength varies depending on the wavelength of the incident light. In other words, when polarized light (white light) with a specific phase is incident on a wave plate, the wave plate can be considered an optical element that changes the polarized light of the white light into a polarization state in which the phase differs depending on the wavelength. Therefore, by using wave plates as optical elements (taps) and stacking multiple wave plates with different slow axis orientations, the wave plate stack can function as a finite impulse response filter. That is, when polarized light (white light) of a specific phase is incident on the wave plate stack, the wave plate stack can function as a wavelength-selective retardation plate that changes the phase of polarized light in a specific wavelength range and does not change the phase of polarized light in other wavelength ranges. It should be understood by those skilled in the art that a finite impulse response filter can function as a filter exhibiting a desired response by adjusting and combining the response characteristics (optical characteristics) of the taps (optical elements). Details of the above principle are also described in the above-mentioned non-patent document 1. Specific examples and modified examples of wavelength-selective retardation plates will be described in detail later.
[0018] Furthermore, the mechanism by which the wavelength-selective retardation plate of the present invention reduces the difference between the phase difference occurring when light is incident from the front direction and the phase difference occurring when light is incident from an oblique direction is not entirely clear, but the inventors speculate as follows. When light is incident from a direction perpendicular to the surface of the wave plate (the front direction), the incident light generates a phase difference due to the refractive index difference in the in-plane direction. On the other hand, when light is incident from a direction tilted from the perpendicular direction to the surface of the wave plate (the oblique direction), the refractive index difference in the in-plane direction may change depending on the azimuth angle of the incident light. Here, the Nz factors of the multiple wave plates used in the wavelength-selective retardation plate of the present invention are each greater than 0.3 and less than 0.7. When the Nz factor of the wave plate is within the above range, it is possible to compensate for the change in the refractive index difference in the in-plane direction even for light incident from an oblique direction, and to impart the same refractive index difference as when light is incident from the front direction. As a result, it is believed that the difference between the phase difference occurring when light is incident from the front direction and the phase difference occurring when light is incident from an oblique direction is reduced.
[0019] An example of a wavelength-selective retardation plate of the present invention will be described with reference to the drawings. Fig. 1 shows a schematic diagram of a wavelength-selective retardation plate 100, which is an example of the wavelength-selective retardation plate of the present invention. The wavelength-selective retardation plate 100 has a first wave plate 112, a second wave plate 114, and a third wave plate 116, in this order. The in-plane slow axis direction of the first wave plate 112 is a first in-plane slow axis direction D1, the in-plane slow axis direction of the second wave plate 114 is a second in-plane slow axis direction D2, and the in-plane slow axis direction of the third wave plate 116 is a third in-plane slow axis direction D3. Here, the Re(725) of the first wave plate 112 at a wavelength of 725 nm is 725 nm, the Re(725) of the second wave plate 114 is 1450 nm, and the Re(725) of the third wave plate 116 is 1450 nm. The Nz factors of the first wave plate 112, the second wave plate 114, and the third wave plate 116 are each 0.5 at a wavelength of 550 nm. The first wave plate 112, the second wave plate 114, and the third wave plate 116 each have an Re(450) / Re(550) of 1.09, and are made of a normal dispersion material.
[0020] The wavelength-selective retardation plate 100 changes the phase of polarized light in a first wavelength range for linearly polarized light P incident from the first wave plate 112 side, while not changing the phase of polarized light in a second wavelength range different from the first wavelength range. The vibration direction DP of the incident linearly polarized light P is the left-right direction on the paper. FIG. 2 shows the azimuth relationship between the first in-plane slow axis direction D1, the second in-plane slow axis direction D2, the third in-plane slow axis direction D3, and the vibration direction DP when the wavelength-selective retardation plate 100 is viewed from the third wave plate 116 side. The first in-plane slow axis direction D1 is rotated 45° clockwise with respect to the vibration direction DP. The second in-plane slow axis direction D2 is rotated 77° counterclockwise with respect to the vibration direction DP. The third in-plane slow axis direction D3 is rotated 80° clockwise with respect to the vibration direction DP.
[0021] By stacking wave plates made of materials with the above optical properties in the above-described orientation relationship, a wavelength-selective retardation plate can be realized that, based on the above-described principle, changes the phase of polarization in a first wavelength range (the wavelength range of green light in the illustrated example) of linearly polarized light P incident from the first wave plate 112 side, while not changing the phase of polarization in a second wavelength range (the wavelength range of red light and blue light in the illustrated example) different from the first wavelength range. Furthermore, since the Nz factors of the first wave plate 112, the second wave plate 114, and the third wave plate 116 are each 0.5, it is possible to compensate for changes in the phase difference of light incident from an oblique direction. As a result, based on the above-described principle, it is believed that the difference between the phase difference occurring when light is incident from the front direction and the phase difference occurring when light is incident from an oblique direction is reduced. The wavelength-selective retardation plate 100 shown in FIG. 1 is an example of a wavelength-selective retardation plate of the present invention, and the wavelength-selective retardation plate of the present invention may also be in the form shown later.
[0022] The characteristics of the wavelength-selective retardation plate of the present invention and the configuration used in the wavelength-selective retardation plate of the present invention will be described below.
[0023] <First Wavelength Range and Second Wavelength Range> The wavelength-selective retardation plate of the present invention changes the phase of polarized light in a first wavelength range, but does not change the phase of polarized light in a second wavelength range different from the first wavelength range. The first wavelength range in which the phase of polarized light changes can be appropriately adjusted depending on the application in which the wavelength-selective retardation plate is used. In particular, it is preferable that at least a portion of the first wavelength range falls within the visible light range (380 to 780 nm). Note that the first wavelength range can be adjusted by the optical characteristics of the wavelength plate used, as described below. Furthermore, the phase difference of polarized light changed in the first wavelength range can be appropriately adjusted depending on the application in which the wavelength-selective retardation plate is used. In particular, it is preferable that the phase difference of polarized light changed in the first wavelength range is λ / 2. That is, when incident light is linearly polarized, it is preferable that in the first wavelength range, the light is converted into linearly polarized light in a direction perpendicular to the polarization direction of the linearly polarized light of the incident light, and that in the second wavelength range, the polarization direction of the linearly polarized light of the incident light is not converted.
[0024] In this specification, the first wavelength range and the second wavelength range are defined as follows. Hereinafter, a method for determining the first wavelength range and the second wavelength range when the phase difference of the polarized light to be changed in the first wavelength range is λ / 2 will be described. A laminate is produced by arranging a pair of linear polarizers in a crossed Nicol configuration and disposing the wavelength-selective retardation plate of the present invention between the linear polarizers. Unpolarized white light (wavelength range: 420 to 670 nm) is irradiated onto the laminate from a direction perpendicular to the surface of the linear polarizer. When producing the laminate, the angle between the transmission axis direction of the linear polarizer on the side irradiated with white light and the in-plane slow axis direction of the wavelength-selective retardation plate on the side irradiated with white light is adjusted to have an azimuth relationship of 45°. If the in-plane slow axis direction of the wavelength-selective retardation plate on the side irradiated with white light is known in advance, that direction may be used. At this time, the transmission spectrum of the laminate is obtained using a spectrophotometer on the side opposite to the side irradiated with white light. Furthermore, a transmission spectrum is obtained when the two linear polarizers are arranged so that their absorption axes are parallel and the white light is irradiated. Here, when the light intensity at each wavelength in the transmission spectrum of the two linear polarizers arranged so that their absorption axes are parallel is set to 100%, the wavelength range in the transmission spectrum of the laminate in which the transmittance at each wavelength is 80% or more is defined as the first wavelength range. A wavelength range different from the first wavelength range is defined as the second wavelength range. Even if the in-plane slow axis direction of the wavelength-selective retardation plate on the side irradiated with white light is unknown, the transmission spectrum of the laminate can be obtained by gradually rotating only the stacking direction of the wavelength-selective retardation plate to obtain a transmission spectrum, which shows minimum and maximum transmittance values, and the transmission spectrum of the laminate can be measured in the stacking direction in which the difference between the maximum and minimum transmittance values in the transmission spectrum is largest.
[0025] In the above-described embodiment, the phase difference of the polarized light changed in the first wavelength range is λ / 2, but the phase difference can be adjusted appropriately depending on the application, and the phase difference of the polarized light changed in the first wavelength range may be λ / 4. That is, when the incident light is linearly polarized, the linearly polarized light of the incident light is converted to circularly polarized light in the first wavelength range, and the polarization state of the linearly polarized light of the incident light is not changed in the second wavelength range. When the phase difference of the polarized light changed in the first wavelength range is λ / 4, the first wavelength range is determined in the same manner as described above. Note that when the phase difference of the polarized light changed in the first wavelength range is λ / 4, the first wavelength range is defined as the wavelength range in which the transmittance at each wavelength in the transmission spectrum of the laminate is 40 to 60% when the light intensity at each wavelength in the transmission spectrum of two linear polarizers arranged with their absorption axes parallel to each other is 100%.
[0026] <Wave Plate> The multiple wave plates used in the wavelength-selective retardation plate of the present invention each have a different slow axis orientation, and the Nz factors of the multiple wave plates are each greater than 0.3 and less than 0.7. That is, the multiple wave plates of the present invention are stacked so that the slow axis orientations are different. Here, the Nz factor of each wave plate is a value at the average wavelength between the upper and lower wavelength limits of the first wavelength range. For example, when the first wavelength range is λa to λb nm, the Nz factor of each wave plate is a value at (λa + λb) / 2. The Nz factors of the multiple wave plates are preferably greater than 0.4 and less than 0.6. Note that when multiple first wavelength ranges are observed, the average wavelength of each observed first wavelength range is first determined, and the Nz factor of the wave plate is determined at each average wavelength for wavelengths in the visible light range. When a plurality of first wavelength ranges are observed, the above-mentioned "Nz factor of the wave plate is greater than 0.3 and less than 0.7" means that at least one of the Nz factors at the average wavelength of each of the observed first wavelength ranges is greater than 0.3 and less than 0.7. Note that the Nz factor at the average wavelength of each of the observed first wavelength ranges is preferably greater than 0.3 and less than 0.7.
[0027] The wave plate is not particularly limited as long as it has the above-mentioned Nz factor and exhibits the function of a wavelength-selective retardation plate when combined with other wave plates. The wave plate may be composed of a single layer or multiple layers. In particular, in terms of ease of adjusting the Nz factor, it is preferable that the wave plate includes an optically anisotropic layer A having an Nz factor greater than 0.5 and an optically anisotropic layer B having an Nz factor less than 0.5. Note that when the wave plate is composed of multiple layers, the Nz factor of the wave plate may be calculated by determining the refractive index in each direction of the entire wave plate, or may be calculated from the Nz factor of each layer constituting the wave plate and the thickness of each layer constituting the wave plate. For example, when a wave plate is composed of a layer X having an Nz factor of z1 and a layer Y having an Nz factor of z2, and the thickness of layer X is d1 and the thickness of layer 1 is d2, the Nz factor Nza of the wave plate can be calculated by the following formula: (Formula) Nza=z1×d1 / (d1+d2)+z2×d2 / (d1+d2) That is, when the wave plate includes an optically anisotropic layer A and an optically anisotropic layer B, the Nz factors of the optically anisotropic layer A and the optically anisotropic layer B and the thickness of each layer may be adjusted so that the Nz factor of the wave plate is greater than 0.3 and less than 0.7. In the above preferred embodiment, the angle formed between the in-plane slow axis of the optically anisotropic layer A and the in-plane slow axis of the optically anisotropic layer B is preferably 45° or less, more preferably 20° or less, and even more preferably 5° or less. In the above preferred embodiment, the angle formed between the in-plane slow axis of the optically anisotropic layer A and the in-plane slow axis of the optically anisotropic layer B may be 0°.
[0028] Furthermore, at least one of the plurality of wave plates used in the wavelength-selective retardation plate of the present invention preferably exhibits forward wavelength dispersion (normal dispersion), which is a characteristic in which the refractive index increases as the wavelength becomes shorter. In particular, it is preferable that all of the plurality of wave plates used in the wavelength-selective retardation plate of the present invention exhibit forward wavelength dispersion. In the above-described embodiment, the forward wavelength dispersion is preferably exhibited in the visible light region. The widths of the first wavelength region and the second wavelength region can be controlled, for example, by the optical characteristics of the wave plate (e.g., the dispersion characteristics of the wave plate).
[0029] The thickness of the wave plate can be adjusted appropriately, but is preferably 0.5 to 1000 μm, more preferably 1 to 100 μm.
[0030] The following describes the optically anisotropic layer A and the optically anisotropic layer B. In addition, later, an embodiment in which the wave plate is composed of a single layer (optically anisotropic layer C) will also be described.
[0031] (Optically Anisotropic Layer A) The optically anisotropic layer A used in a preferred embodiment of the retardation plate is an optically anisotropic layer having an Nz factor of more than 0.5. Examples of the optically anisotropic layer having an Nz factor of more than 0.5 include a stretched film and a layer formed using a composition containing a rod-like liquid crystal compound, and a layer formed using a composition containing a rod-like liquid crystal compound is preferred.
[0032] The layer formed using a composition containing a rod-shaped liquid crystal compound is preferably, for example, a layer in which horizontally aligned rod-shaped liquid crystal compounds are fixed. A layer in which horizontally aligned rod-shaped liquid crystal compounds are fixed typically corresponds to a so-called positive A plate. The state in which the rod-shaped liquid crystal compounds are horizontally aligned refers to the state in which the long axis of the rod-shaped liquid crystal compounds is parallel to the main surface of the optically anisotropic layer A. Strict parallelism is not required, and the angle between the long axis of the rod-shaped liquid crystal compounds and the main surface of the optically anisotropic layer A is preferably in the range of 0±20°, more preferably 0±10°. In this specification, the "fixed" state refers to a state in which the alignment of the liquid crystal compounds is maintained. Specifically, typically, the layer is preferably in a temperature range of 0 to 50°C, or, under more severe conditions, in the temperature range of −30 to 70°C, in which the layer has no fluidity and can stably maintain the fixed alignment without any change in the alignment due to an external field or external force.
[0033] Furthermore, when the refractive index in the in-plane slow axis direction is nx, the refractive index in the in-plane direction perpendicular to the slow axis is ny, and the refractive index in the thickness direction is nz, the positive A plate satisfies the relationship of formula (A1). Formula (A1) nx>ny≒nz Note that the above "≒" encompasses not only the case where the two are completely identical, but also the case where the two are substantially identical. For example, "substantially the same" includes "ny≒nz" when (ny-nz)×d is -10 to 10 nm, preferably -5 to 5 nm, and also includes "nx≒nz" when (nx-nz)×d is -10 to 10 nm, preferably -5 to 5 nm. Note that in (ny-nz)×d, d is the layer thickness.
[0034] The optically anisotropic layer A may also be a layer formed by fixing the orientation direction of rod-shaped liquid crystal compounds that are twisted around a certain axis. Even in the case of the optically anisotropic layer A having the above-described configuration, it is possible to determine the nx, ny, and nz values by the above-described method.
[0035] Known compounds can be used as the rod-shaped liquid crystal compound. Examples of the rod-shaped liquid crystal compound include the compounds described in claim 1 of JP-A-11-513019 and in paragraphs 0026 to 0098 of JP-A-2005-289980. Rod-shaped liquid crystal compounds exemplified in the section on optical elements described below may also be used.
[0036] The rod-shaped liquid crystal compound may have a polymerizable group. In this specification, the type of the polymerizable group is not particularly limited, and a functional group capable of undergoing an addition polymerization reaction is preferred, a polymerizable ethylenically unsaturated group or a ring-polymerizable group is more preferred, and a (meth)acryloyl group, a vinyl group, a styryl group, or an allyl group is still more preferred.
[0037] The Nz factor of the optically anisotropic layer A is more than 0.5, and preferably 0.8 or more. There is no particular upper limit to the Nz factor of the optically anisotropic layer A, but it is usually 10 or less, and often 5 or less. When the optically anisotropic layer A contains a rod-like liquid crystal compound, the Nz factor of the optically anisotropic layer A is often 0.8 to 1.2.
[0038] (Optically Anisotropic Layer B) The optically anisotropic layer B used in a preferred embodiment of the retardation plate is an optically anisotropic layer having an Nz factor of less than 0.5. Examples of optically anisotropic layers having an Nz factor of less than 0.5 include layers formed using a composition containing a discotic liquid crystal compound, and a layer formed by fixing a discotic liquid crystal compound in which the discotic liquid crystal compound is vertically aligned is preferred. A layer formed by fixing a rod-shaped liquid crystal compound in which the discotic liquid crystal compound is vertically aligned usually corresponds to a so-called negative A plate. The state in which the discotic liquid crystal compound is vertically aligned means that the discotic plane of the discotic liquid crystal compound and the main surface of the optically anisotropic layer B are perpendicular to each other. Strict perpendicularity is not required, and the angle between the discotic plane of the discotic liquid crystal compound and the main surface of the optically anisotropic layer B is preferably in the range of 90±20°, more preferably 90±10°.
[0039] Furthermore, when the refractive index in the in-plane slow axis direction is nx, the refractive index in the in-plane direction perpendicular to the slow axis is ny, and the refractive index in the thickness direction is nz, the negative A plate satisfies the relationship of formula (A2). Formula (A2) ny<nx≒nz Note that the above "≒" encompasses not only the case where the two are completely identical, but also the case where the two are substantially identical. For example, "substantially the same" includes "ny≒nz" when (ny-nz)×d is -10 to 10 nm, preferably -5 to 5 nm, and also includes "nx≒nz" when (nx-nz)×d is -10 to 10 nm, preferably -5 to 5 nm. Note that in (ny-nz)×d, d is the layer thickness.
[0040] The optically anisotropic layer B may also be a layer formed by fixing the alignment direction of a discotic liquid crystal compound that is twisted around a certain axis. Even in the case of the optically anisotropic layer B having the above-described configuration, it is possible to determine the nx, ny, and nz values by the above-described method.
[0041] Known compounds can be used as the discotic liquid crystal compound. Examples of the discotic liquid crystal compound include the compounds described in paragraphs 0020 to 0067 of JP-A No. 2007-108732 and paragraphs 0013 to 0108 of JP-A No. 2010-244038. Furthermore, discotic liquid crystal compounds exemplified in the section on optical elements described below may also be used. The discotic liquid crystal compound may have a polymerizable group. Preferred examples of the polymerizable group include the same polymerizable groups as those of rod-shaped liquid crystal compounds.
[0042] The Nz factor of the optically anisotropic layer B is less than 0.5, and preferably 0.2 or less. There is no particular lower limit to the Nz factor of the optically anisotropic layer B, but it is usually -10 or more, and often -5 or more. When the optically anisotropic layer B contains a discotic liquid crystal compound, the Nz factor of the optically anisotropic layer B is often -0.2 to 0.2.
[0043] (Optically Anisotropic Layer C) As described above, the wave plate may be composed of a single layer. Such a wave plate preferably comprises an optically anisotropic layer C that is a B plate having a positive Rth. The Nz factor of the optically anisotropic layer C is greater than 0.3 and less than 0.7. In addition, when the refractive index in the in-plane slow axis direction is nx, the refractive index in the direction perpendicular to the in-plane slow axis is ny, and the refractive index in the thickness direction is nz, the B plate having a positive Rth satisfies the relationship of formula (B2). Formula (B2) (nx+ny) / 2<nz
[0044] A B plate having a positive Rth can be obtained by a known method, for example, by stretching a film, for example, as described in JP-A-5-157911, JP-A-2006-072309, or JP-A-2007-298960, by laminating a shrinkable film on one or both sides of a polymer film, and then stretching the film by heating in the thickness (nz) direction.
[0045] <Combination of Wave Plates> The wavelength-selective retardation plate of the present invention is formed by stacking the above-described wave plates so that their slow axis orientations are different. The optical properties of the wave plates and the lamination method thereof can be appropriately selected so as to change the phase of polarized light in a first wavelength range while not changing the phase of polarized light in a second wavelength range different from the first wavelength range, and those skilled in the art can design them according to the above-described principles. For example, when the average wavelength between the upper and lower limit wavelengths of the desired second wavelength range is λ2, the in-plane retardation of the wave plate is preferably λ2±200 nm, more preferably λ2±100 nm, and even more preferably λ2±50 nm at the above average wavelength λ2. Furthermore, for example, with regard to a combination of preferred in-plane slow axes of wave plates, it is preferable to combine, for example, the wave plates shown in Table 1 below so that the in-plane slow axis directions thereof are at the angles shown in Table 1. In Table 1, λ2 represents the value of the average wavelength between the upper and lower limit wavelengths of the desired second wavelength range. The angles listed in Table 1 below are angles of the slow axis azimuth relative to the vibration direction of the incident linearly polarized light, and when viewed from the side opposite to the incident side of the incident linearly polarized light, clockwise are represented as negative values and counterclockwise are represented as positive values. Furthermore, when each angle listed in Table 1 below is θn, the angles listed may be θn±5°, and θn±3° is preferred. A configuration in which the positive and negative signs of the angle values listed in the table below are respectively reversed is also preferably used. Furthermore, a configuration in which the angle values are respectively obtained by adding 90° to the angles listed in the table below is also preferably used. Furthermore, in Table 1 below, the wave plate on the side where linearly polarized light is incident is referred to as the first plate.
[0046]
[0047] The average wavelength of the first wavelength range can be adjusted by adjusting the average wavelength (λ2) of the second wavelength range. The wavelength ranges of the second wavelength range and the first wavelength range can be adjusted by adjusting the optical characteristics of the wave plate used and the angle of the slow axis orientation.
[0048] <Other Layers> The wavelength-selective retardation plate of the present invention may have other layers in addition to the above-described configuration, such as a λ / 4 plate, a support, and an attachment layer.
[0049] When the wavelength-selective retardation plate of the present invention is used as a wavelength-selective retardation plate for circularly polarized light, it is preferable that the wavelength-selective retardation plate has a λ / 4 plate as another layer. In the above embodiment, it is preferable that a λ / 4 plate be provided on both one surface and the other surface of the wavelength-selective retardation plate. A known λ / 4 plate can be used as the λ / 4 plate. Various retardation plates can be used, such as a polymer, a cured layer of a liquid crystal compound, and a structural birefringence layer. It is preferable that the λ / 4 plate has reverse dispersion. The reverse dispersion of the λ / 4 plate allows it to accommodate incident light with a wide wavelength range. It is also preferable that the λ / 4 plate is formed by stacking multiple retardation plates and using a retardation layer that effectively functions as a λ / 4 plate. For example, the λ / 4 plate described in International Publication No. 2013 / 137464, which is a broadband λ / 4 plate formed by combining a λ / 2 plate and a λ / 4 plate, can accommodate incident light with a wide wavelength range and can be preferably used.
[0050] When the wavelength-selective retardation plate of the present invention has a λ / 4 plate, it is preferable to adjust the orientations of the λ / 4 plate and the wavelength-selective retardation plate so that, when circularly polarized light is polarization-converted into linearly polarized light by the λ / 4 plate, the vibration direction of the polarization-converted linearly polarized light is the same as the vibration direction of the incident linearly polarized light in the above-mentioned embodiment.
[0051] The support is not particularly limited as long as it can maintain the wavelength-selective retardation plate, and known supports can be used. Various sheet-like materials (films, plate-like materials) can be used as the support. A transparent support is preferred. Examples of the transparent support include inorganic transparent supports such as glass, and organic transparent supports such as resin films. Examples of resin films include polyacrylic resin films such as polymethyl methacrylate, cellulose resin films such as cellulose triacetate, cycloolefin polymer films (e.g., trade name "Arton" manufactured by JSR Corporation, trade name "Zeonor" manufactured by Nippon Zeon Co., Ltd.), polyethylene terephthalate (PET), polycarbonate, and polyvinyl chloride. The thickness of the support is preferably 1 to 1000 μm, more preferably 3 to 250 μm, and even more preferably 5 to 150 μm.
[0052] The laminating layer is used when laminating wave plates to each other or a wave plate to another layer (e.g., a λ / 4 plate and a support). The laminating layer may be a layer made of an adhesive that has fluidity when laminating and then becomes solid, a layer made of a pressure-sensitive adhesive that is a soft gel-like (rubber-like) solid when laminating and does not change to a gel-like state after lamination, or a layer made of a material that has the characteristics of both an adhesive and a pressure-sensitive adhesive. Therefore, the laminating layer may be any known material used for laminating sheet-like objects in optical devices, optical elements, etc., such as an optically clear adhesive (OCA), an optically clear double-sided tape, or an ultraviolet-curable resin.
[0053] [Optical Element] The optical element of the present invention comprises a plurality of optically anisotropic layers formed using a composition containing a liquid crystal compound, each having a liquid crystal orientation pattern in which the orientation of the optical axis derived from the liquid crystal compound changes while continuously rotating along at least one in-plane direction. The optical element of the present invention also comprises the wavelength-selective retardation plate described above disposed between at least one pair of the plurality of optically anisotropic layers. Here, the rotation directions of the orientations of the optical axes of the adjacent two optically anisotropic layers are opposite to each other. The first wavelength range includes wavelengths longer than those in the second wavelength range, and the wavelength-selective retardation plate converts circularly polarized light in the first wavelength range into circularly polarized light with an opposite rotation direction, without changing the phase of circularly polarized light in the second wavelength range. Furthermore, in the liquid crystal orientation pattern, when the length of a 180° rotation of the orientation of the optical axis in the one direction in which the orientation of the optical axis changes while continuously rotating is defined as one period, the length of the one period of at least one of the optically anisotropic layers is different from that of the other optically anisotropic layers.
[0054] The optical element of the present invention has a small wavelength dependency of the refraction angle of incident and transmitted light, and can emit light of different wavelengths incident from the same direction in almost the same direction.
[0055] An example of the optical element of the present invention is shown in Figure 3. The optical element 10 shown in Figure 3 includes a first optically anisotropic member 12, a second optically anisotropic member 14, and a wavelength-selective retardation plate 18G disposed between the first optically anisotropic member 12 and the second optically anisotropic member 14. As described above, the optical element of the present invention includes an optically anisotropic layer formed using a composition containing a liquid crystal compound and having a predetermined liquid crystal orientation pattern in which the optical axis derived from the liquid crystal compound rotates, arranged in the thickness direction. The first optically anisotropic member 12 includes a support 20, an alignment film 24A, and a first optically anisotropic layer 26A. The second optically anisotropic member 14 includes a support 20, an alignment film 24B, and a second optically anisotropic layer 26B. In the optical element of the present invention, as described above, the wavelength-selective retardation plate converts circularly polarized light in a specific wavelength range (first wavelength range) into circularly polarized light in the opposite rotation direction, and transmits (passes through) light in the other second wavelength range as is. In the illustrated optical element 10, the wavelength-selective retardation plate 18G converts the rotation direction of the circularly polarized light of the green light into the opposite rotation direction, and transmits the other light as circularly polarized light of the same rotation direction.
[0056] Although not shown in the figure, the first optically anisotropic member 12 and the wavelength-selective retardation plate 18G, and the wavelength-selective retardation plate 18G and the second optically anisotropic member 14 are bonded together by a bonding layer provided between the layers. The same bonding layer as that described in the section on the wavelength-selective retardation plate can be used for the bonding layer. The optical element of the present invention may be constructed by stacking the first optically anisotropic member 12, the wavelength-selective retardation plate 18G, and the second optically anisotropic member 14 and holding them with a frame or a jig. The optical element of the present invention is not limited to the illustrated example in which the first optically anisotropic member 12, the wavelength-selective retardation plate 18G, and the second optically anisotropic member 14 are stacked in close contact with each other; a configuration in which one or more of these members are arranged at a distance from each other may also be used.
[0057] Furthermore, although the illustrated optical element 10 has a support 20 for each optically anisotropic member, the optical element of the present invention does not necessarily need to have a support 20 for each optically anisotropic member. For example, the optical element of the present invention may have a configuration in which a wavelength-selective retardation plate 18G is formed on the surface of the second optically anisotropic member 14 (second optically anisotropic layer 26B), an alignment film 24A is formed thereon, and a first optically anisotropic layer 26A is formed thereon. Alternatively, the optical element of the present invention may be configured from the above configuration by peeling off the support 20 of the second optically anisotropic member 14, leaving only the wavelength-selective retardation plate, alignment film, and optically anisotropic layer, or by peeling off the alignment film as well, leaving only the wavelength-selective retardation plate and optically anisotropic layer.
[0058] That is, the optical element of the present invention has an arrangement of a plurality of optically anisotropic layers, a wavelength-selective retardation plate between at least one pair of adjacent optically anisotropic layers, and the optically anisotropic layers have a liquid crystal orientation pattern in which the direction of the optical axis derived from the liquid crystal compound rotates in one direction, and further, various layer configurations can be used as long as the liquid crystal orientation pattern of at least one optically anisotropic layer has a different period as described below.
[0059] <Optical Anisotropic Member> The optical element 10 of the present invention includes a wavelength-selective retardation plate 18G provided between a first optical anisotropic member 12 and a second optical anisotropic member 14. As described above, the first optical anisotropic member 12 includes a support 20, an alignment film 24A, and a first optical anisotropic layer 26A. The second optical anisotropic member 14 includes a support 20, an alignment film 24B, and a second optical anisotropic layer 26B.
[0060] (Support) In the first optically anisotropic member 12 and the second optically anisotropic member 14, the support 20 supports the alignment films 24A and 24B, as well as the first optically anisotropic layer 26A and the second optically anisotropic layer 26B. In the following description, when it is not necessary to distinguish between the alignment films 24A and 24B, the alignment films 24A and 24B will also be collectively referred to as "alignment films." Furthermore, in the following description, when it is not necessary to distinguish between the first optically anisotropic layer 26A and the second optically anisotropic layer 26B, the first optically anisotropic layer 26A and the second optically anisotropic layer 26B will also be collectively referred to as "optically anisotropic layers."
[0061] As long as it can support the alignment film and the optically anisotropic layer, various sheet-like materials (films, plates) can be used as the support 20. The supports described above can be used as the support 20.
[0062] (Alignment film) In the first optically anisotropic member 12, an alignment film 24A is formed on the surface of the support 20. In the second optically anisotropic member 14, an alignment film 24B is formed on the surface of the support 20. The alignment film 24A is an alignment film for orienting the liquid crystal compound 30 in a predetermined liquid crystal alignment pattern when forming the first optically anisotropic layer 26A of the first optically anisotropic member 12. The alignment film 24B is an alignment film for orienting the liquid crystal compound 30 in a predetermined liquid crystal alignment pattern when forming the second optically anisotropic layer 26B of the second optically anisotropic member 14.
[0063] As will be described later, in the optical element 10 of the present invention, the optically anisotropic layer has a liquid crystal orientation pattern in which the orientation of the optical axis 30A (see FIG. 5 ) derived from the liquid crystal compound 30 changes while continuously rotating along one in-plane direction (the direction of the arrow X described later). Therefore, the orientation film of each optically anisotropic member is formed so that the optically anisotropic layer can form this liquid crystal orientation pattern. In the optical element of the present invention, when the length of a 180° rotation of the orientation of the optical axis 30A in one direction in which the orientation of the optical axis 30A changes while continuously rotating in the liquid crystal orientation pattern is defined as one period (optical axis rotation period), at least one optically anisotropic layer has a liquid crystal orientation pattern whose length differs from that of the other optically anisotropic layers. In the optical element 10 shown in FIG. 3 , one period (one period Λ) of the liquid crystal orientation pattern in the first optically anisotropic layer 26A is A ) is one period (one period Λ) of the liquid crystal alignment pattern in the second optically anisotropic layer 26B. B ) is shorter than
[0064] In the following description, "the orientation of the optical axis 30A rotates" may also be simply referred to as "the optical axis 30A rotates."
[0065] Various known alignment films can be used, including, for example, a rubbed film made of an organic compound such as a polymer, an obliquely evaporated film of an inorganic compound, a film having microgrooves, and a film formed by accumulating LB (Langmuir-Blodgett) films made of organic compounds such as ω-tricosanoic acid, dioctadecylmethylammonium chloride, and methyl stearate by the Langmuir-Blodgett method.
[0066] An alignment film formed by rubbing treatment can be formed by rubbing the surface of the polymer layer several times in a certain direction with paper or cloth. Preferred examples of materials used for the alignment film include polyimide, polyvinyl alcohol, polymers having polymerizable groups described in JP-A-9-152509, and materials used to form alignment films described in JP-A-2005-97377, JP-A-2005-99228, and JP-A-2005-128503.
[0067] In the optical element 10 of the present invention, the alignment film is preferably a so-called photo-alignment film obtained by irradiating a photo-alignable material with polarized or non-polarized light. That is, in the optical element 10 of the present invention, the alignment film is preferably a photo-alignment film formed by applying a photo-alignment material onto the support 20. Irradiation with polarized light can be performed on the photo-alignment film from a vertical direction or an oblique direction, and irradiation with non-polarized light can be performed on the photo-alignment film from an oblique direction.
[0068] Examples of photo-alignment materials that can be used in the photo-alignment film of the present invention include those disclosed in JP-A-2006-285197, JP-A-2007-76839, JP-A-2007-138138, JP-A-2007-94071, JP-A-2007-121721, JP-A-2007-140465, JP-A-2007-156439, and JP-A-2007-160466. azo compounds described in JP-A-07-133184, JP-A-2009-109831, Japanese Patent No. 3883848 and Japanese Patent No. 4151746, aromatic ester compounds described in JP-A-2002-229039, maleimides having photo-alignable units described in JP-A-2002-265541 and JP-A-2002-317013, and / or alkenyl-substituted nadimide compounds, photocrosslinkable silane derivatives described in Japanese Patent Nos. 4205195 and 4205198, photocrosslinkable polyimides, photocrosslinkable polyamides, and photocrosslinkable esters described in JP-T-2003-520878, JP-T-2004-529220, and JP-T-4162850, and photodimerizable compounds described in JP-A-9-118717, JP-A-10-506420, JP-A-2003-505561, WO 2010 / 150748, JP-A-2013-177561, and JP-A-2014-12823, in particular cinnamate compounds, chalcone compounds, and coumarin compounds, are exemplified as preferred examples. Among these, azo compounds, photocrosslinkable polyimides, photocrosslinkable polyamides, photocrosslinkable esters, cinnamate compounds, and chalcone compounds are preferably used.
[0069] There is no limitation on the thickness of the alignment film, and it may be set appropriately depending on the material of which the alignment film is formed so as to obtain the necessary alignment function. The thickness of the alignment film is preferably 0.01 to 5 μm, and more preferably 0.05 to 2 μm.
[0070] There is no limitation on the method for forming the alignment film, and various known methods can be used depending on the material for forming the alignment film. One example is a method in which an alignment film is applied to the surface of the support 20, dried, and then exposed to laser light to form an alignment pattern.
[0071] An example of an exposure device for forming an alignment pattern by exposing an alignment film is conceptually shown in Fig. 13. Note that, although the example shown in Fig. 13 illustrates exposure of the alignment film 24A of the first optical anisotropic member 12, an alignment pattern can also be formed in the alignment film 24B of the second optical anisotropic member 14 in the same manner using the same exposure device.
[0072] The exposure device 60 shown in Figure 13 includes a light source 64 equipped with a laser 62, a λ / 2 plate (not shown) that changes the polarization direction of laser light M emitted by the laser 62, a beam splitter 68 that splits the laser light M emitted by the laser 62 and passing through the λ / 2 plate (not shown) into two beams MA and MB, and mirrors 70A and 70B and λ / 4 plates 72A and 72B that are respectively arranged on the optical paths of the two split beams MA and MB. Although not shown, the light source 64 includes a polarizing plate and emits linearly polarized light P0. The λ / 4 plates 72A and 72B have optical axes that are orthogonal to each other. The λ / 4 plate 72A splits the linearly polarized light P0 0 (ray MA) is polarized by right-handed circular polarization P R The λ / 4 plate 72B is a linearly polarized light P 0 (Light ray MB) is polarized by left-handed circular polarization P L are converted to , respectively.
[0073] The support 20 having the alignment film 24A before the alignment pattern is formed is placed in an exposure unit, and two light beams MA and MB are caused to intersect and interfere on the alignment film 24A, and the alignment film 24A is irradiated with the interference light to expose it. This interference causes the polarization state of the light irradiated on the alignment film 24A to periodically change in the form of interference fringes. This results in an alignment pattern in which the alignment state periodically changes on the alignment film 24A. In the exposure device 60, the period of the alignment pattern can be adjusted by changing the crossing angle α of the two light beams MA and MB. That is, in the exposure device 60, by adjusting the crossing angle α, the length of one period (one period Λ) in which the optical axis 30A originating from the liquid crystal compound 30 rotates 180° in one direction of the rotation of the optical axis 30A can be adjusted. By forming an optically anisotropic layer on an alignment film having such an alignment pattern in which the alignment state changes periodically, it is possible to form a first optically anisotropic layer 26A having a liquid crystal alignment pattern in which the optic axis 30A derived from the liquid crystal compound 30 rotates continuously in one direction, as will be described later. In addition, by rotating the optic axes of the λ / 4 plates 72A and 72B by 90° each, the rotation direction of the optic axis 30A can be reversed.
[0074] In the optical element of the present invention, the alignment film is provided as a preferred embodiment but is not an essential component. For example, by forming an alignment pattern on the support 20 by a method of rubbing the support 20 or a method of processing the support 20 with laser light or the like, it is possible to configure the first optically anisotropic layer 26A etc. to have a liquid crystal alignment pattern in which the direction of the optic axis 30A derived from the liquid crystal compound 30 changes while continuously rotating along at least one direction in the plane.
[0075] <<Optical Anisotropic Layer>> In the first optically anisotropic member 12, a first optically anisotropic layer 26A is formed on the surface of the alignment film 24A. In the second optically anisotropic member 14, a second optically anisotropic layer 26B is formed on the surface of the alignment film 24B. Note that in FIG. 3 (and FIGS. 6 to 8 described below), in order to simplify the drawings and clearly show the configuration of the optical element 10, both the first optically anisotropic layer 26A and the second optically anisotropic layer 26B only show the liquid crystal compound 30 (liquid crystal compound molecules) on the surface of the alignment film. However, as conceptually shown in FIG. 4 exemplarily illustrating the first optically anisotropic layer 26A, the first optically anisotropic layer 26A and the second optically anisotropic layer 26B have a structure in which aligned liquid crystal compounds 30 are stacked, similar to an optically anisotropic layer formed using a composition containing a typical liquid crystal compound.
[0076] As described above, in the optical element 10 of the present invention, the optically anisotropic layers (first optically anisotropic layer 26A and second optically anisotropic layer 26B) are formed using a composition containing a liquid crystal compound. When the in-plane retardation value of the optically anisotropic layer is set to λ / 2, the optically anisotropic layer functions as a general λ / 2 plate, that is, imparts a phase difference of half the wavelength, i.e., 180°, to two orthogonal linearly polarized components contained in light incident on the optically anisotropic layer.
[0077] The optically anisotropic layer has a liquid crystal orientation pattern in which the direction of the optical axis derived from the liquid crystal compound changes while continuously rotating in one direction indicated by arrow X within the plane of the optically anisotropic layer. The optical axis 30A derived from the liquid crystal compound 30 is the axis along which the refractive index of the liquid crystal compound 30 is highest, i.e., the slow axis. For example, if the liquid crystal compound 30 is a rod-shaped liquid crystal compound, the optical axis 30A is aligned along the long axis direction of the rod shape. In the following description, the "one direction indicated by arrow X" will also be referred to simply as the "arrow X direction." In the following description, the optical axis 30A derived from the liquid crystal compound 30 will also be referred to as the "optical axis 30A of the liquid crystal compound 30" or "optical axis 30A." In the optically anisotropic layer, the liquid crystal compound 30 is two-dimensionally aligned in a plane parallel to the arrow X direction and the Y direction perpendicular to the arrow X direction. In FIGS. 3 and 4 and FIGS. 6 to 8, which will be described later, the Y direction is perpendicular to the paper surface.
[0078] FIG. 5 conceptually shows a plan view of the first optically anisotropic layer 26A. The plan view is a view of the optical element 10 in FIG. 3 as seen from above, i.e., a view of the optical element 10 as seen in the thickness direction (i.e., the stacking direction of each layer (film)). In other words, a view of the first optically anisotropic layer 26A as seen from a direction perpendicular to the main surface. Furthermore, in FIG. 5, in order to clearly show the configuration of the optical element 10 of the present invention, only the liquid crystal compound 30 on the surface of the alignment film 24A is shown, as in FIG. 3. However, as described above, the first optically anisotropic layer 26A has a structure in which the liquid crystal compound 30 is stacked in the thickness direction, starting from the liquid crystal compound 30 on the surface of the alignment film 24A, as shown in FIG. 4.
[0079] 5, the first optically anisotropic layer 26A is described as a representative example, but the second optically anisotropic layer 26B basically has the same configuration and functions and effects, except for the length of one period (one period Λ) of the liquid crystal alignment pattern, which will be described later. The rotation directions of the optical axis 30A are opposite between the first optically anisotropic layer 26A and the second optically anisotropic layer 26B. That is, when the rotation direction of the optical axis 30A in the first optically anisotropic layer 26A is clockwise, the rotation direction of the optical axis 30A in the second optically anisotropic layer is counterclockwise.
[0080] The first optically anisotropic layer 26A has a liquid crystal alignment pattern in which the orientation of the optical axis 30A derived from the liquid crystal compound 30 changes while continuously rotating along the direction of arrow X within the plane of the first optically anisotropic layer 26A. The phrase "the orientation of the optical axis 30A of the liquid crystal compound 30 changes while continuously rotating in the direction of arrow X (a predetermined direction)" specifically means that the angle formed between the optical axis 30A of the liquid crystal compound 30 aligned along the direction of arrow X and the direction of arrow X varies depending on the position in the direction of arrow X, and the angle formed between the optical axis 30A and the direction of arrow X sequentially changes along the direction of arrow X from θ to θ+180° or θ−180°. The difference in angle between the optical axes 30A of the liquid crystal compounds 30 adjacent to each other in the direction of arrow X is preferably 45° or less, more preferably 15° or less, and even more preferably a smaller angle.
[0081] On the other hand, the liquid crystal compounds 30 forming the first optically anisotropic layer 26A are arranged at equal intervals in the Y direction perpendicular to the direction of the arrow X, i.e., in the Y direction perpendicular to the direction in which the optical axes 30A continuously rotate. In other words, among the liquid crystal compounds 30 forming the first optically anisotropic layer 26A, the liquid crystal compounds 30 aligned in the Y direction have the same angle between the direction of the optical axes 30A and the direction of the arrow X.
[0082] In the optical element 10 of the present invention, in the liquid crystal orientation pattern of the liquid crystal compound 30, the length (distance) over which the optical axis 30A of the liquid crystal compound 30 rotates 180° in the direction of arrow X, in which the orientation of the optical axis 30A continuously changes in plane, is defined as the length Λ of one period in the liquid crystal orientation pattern. In other words, the length of one period in the liquid crystal orientation pattern is defined as the distance from the angle θ between the optical axis 30A of the liquid crystal compound 30 and the direction of arrow X to the angle θ + 180°. That is, the length Λ of one period is defined as the distance between the centers in the direction of arrow X of two liquid crystal compounds 30 that have the same angle with the direction of arrow X. Specifically, as shown in FIG. 5 , the length Λ of one period is defined as the distance between the centers in the direction of arrow X of two liquid crystal compounds 30 whose optical axes 30A coincide with the direction of arrow X. In the following description, this length Λ of one period is also referred to as "one period Λ." In the following description, in order to distinguish one period Λ in each optically anisotropic layer, one period Λ in the first optically anisotropic layer 26A will be referred to as "Λ A ", one period Λ in the second optically anisotropic layer 26B is "Λ B In the optical element 10 of the present invention, the liquid crystal alignment pattern of the optically anisotropic layer repeats this one period Λ in the direction of arrow X, that is, in one direction in which the direction of the optical axis 30A changes by continuously rotating.
[0083] As described above, in the optically anisotropic layer, the liquid crystal compounds aligned in the Y direction have the same angle between their optical axes 30A and the direction of arrow X (one direction in which the optical axes of the liquid crystal compounds 30 rotate). A region in which the liquid crystal compounds 30, with the same angle between their optical axes 30A and the direction of arrow X, are arranged in the Y direction, is referred to as region R. In this case, the in-plane retardation (Re) value in each region R is preferably half the wavelength, i.e., λ / 2. These in-plane retardations are calculated by the product of the refractive index difference Δn associated with the refractive index anisotropy of region R and the thickness of the optically anisotropic layer. Here, the refractive index difference associated with the refractive index anisotropy of region R in the optically anisotropic layer is a refractive index difference defined by the difference between the refractive index in the direction of the slow axis in the plane of region R and the refractive index in the direction perpendicular to the direction of the slow axis. That is, the refractive index difference Δn due to the refractive index anisotropy of region R is equal to the difference between the refractive index of liquid crystal compound 30 in the direction of optical axis 30A and the refractive index of liquid crystal compound 30 in the direction perpendicular to optical axis 30A in the plane of region R. In other words, the refractive index difference Δn is equal to the refractive index difference of the liquid crystal compound.
[0084] When circularly polarized light is incident on such optically anisotropic layers (first optically anisotropic layer 26A and second optically anisotropic layer 26B), the light is refracted and the direction of the circularly polarized light is converted. This action is conceptually shown in FIG. 6, exemplifying the first optically anisotropic layer 26A. It is assumed that the product of the refractive index difference of the liquid crystal compound and the thickness of the optically anisotropic layer in the first optically anisotropic layer 26A is λ / 2. As shown in FIG. 6, when the product of the refractive index difference of the liquid crystal compound in the first optically anisotropic layer 26A and the thickness of the optically anisotropic layer is λ / 2, left-handed circularly polarized incident light L 1 When incident, the incident light L 1 is given a phase difference of 180° by passing through the first optically anisotropic layer 26A, and becomes the transmitted light L 2 is converted to right-handed circularly polarized light.
[0085] On the other hand, as conceptually shown in FIG. 7, when the product of the refractive index difference of the liquid crystal compound of the first optically anisotropic layer 26A and the thickness of the optically anisotropic layer is λ / 2, right-handed circularly polarized incident light L 4 When incident, the incident light L 4is given a phase difference of 180° by passing through the first optically anisotropic layer 26A, and becomes the left-handed circularly polarized transmitted light L 5 is converted to
[0086] In the first optically anisotropic layer 26A, the in-plane retardation value of the plurality of regions R is preferably a half wavelength. The in-plane retardation Re(550) of the plurality of regions R of the first optically anisotropic layer 26A for incident light having a wavelength of 550 nm is expressed as Re(550)=Δn 550 ×d is preferably within the range defined by the following formula (1): 550 is the refractive index difference due to the refractive index anisotropy of the region R when the wavelength of incident light is 550 nm, and d is the thickness of the first optically anisotropic layer 26A. 550 ×d≦350 nm (1) That is, the in-plane retardation Re(550) of the plurality of regions R of the first optically anisotropic layer 26A=Δn 550 When ×d satisfies the formula (1), a sufficient amount of the circularly polarized component of the light incident on the first optically anisotropic layer 26A can be converted into circularly polarized light traveling in a direction inclined forward or backward with respect to the direction of the arrow X. In-plane retardation Re(550)=Δn 550 ×d is 225 nm≦Δn 550 ×d≦340 nm is more preferable, and 250 nm≦Δn 550 It is more preferable that ×d≦330 nm. The above formula (1) is a range for incident light having a wavelength of 550 nm, but the in-plane retardation Re(λ) of the plurality of regions R of the optically anisotropic layer for incident light having a wavelength of λ nm is λ ×d is preferably within the range defined by the following formula (1-2), and can be set appropriately: 0.7 λnm≦Δn λ ×d≦1.3λnm...(1-2)
[0087] Furthermore, the in-plane retardation values of the regions R in the first optically anisotropic layer 26A may be outside the range of the above formula (1). 550 ×d<200 nm or 350 nm<Δn 550×d, it is possible to separate light into light traveling in the same direction as the incident light and light traveling in a direction different from the incident light. 550 When ×d approaches 0 nm or 550 nm, the component of light traveling in the same direction as the incident light increases, and the component of light traveling in a direction different from the incident light decreases.
[0088] Furthermore, the in-plane retardation Re(450) of each region R of the first optically anisotropic layer 26A for incident light having a wavelength of 450 nm is expressed as Re(450)=Δn 450 ×d and the in-plane retardation Re(550)=Δn of each region R of the first optically anisotropic layer 26A for incident light having a wavelength of 550 nm. 550 ×d preferably satisfies the following formula (2): 450 is the refractive index difference associated with the refractive index anisotropy of the region R when the wavelength of the incident light is 450 nm. (Δn 450 × d) / (Δn 550 ×d)<1.0 (2) Formula (2) indicates that the liquid crystal compound 30 contained in the first optically anisotropic layer 26A has reverse dispersion. That is, when formula (2) is satisfied, the first optically anisotropic layer 26A can accommodate incident light over a wide wavelength range.
[0089] Here, by changing one period Λ of the liquid crystal alignment pattern formed in the first optically anisotropic layer 26A, the transmitted light L 2 and L 5 Specifically, the shorter the period Λ of the liquid crystal alignment pattern, the stronger the interference between the lights passing through the adjacent liquid crystal compounds 30, and therefore the angle of refraction of the transmitted light L 2 and L 5 In addition, the incident light L 1 and L 4 Transmitted light L 2 and L 5 The angle of refraction of the incident light L 1 and L 4 (Transmitted light L 2 and L 5) . Specifically, the longer the wavelength of the incident light, the greater the refraction of the transmitted light. That is, when the incident light is red, green, and blue, the red light is refracted the most and the blue light is refracted the least. Furthermore, by reversing the rotation direction of the optical axis 30A of the liquid crystal compound 30, which rotates along the direction of arrow X, the refraction direction of the transmitted light can be reversed.
[0090] The optically anisotropic layer is composed of a cured layer of a liquid crystal composition containing a rod-shaped or discotic liquid crystal compound, and has a liquid crystal alignment pattern in which the optical axis of the rod-shaped or discotic liquid crystal compound is aligned as described above. An alignment film is formed on a support 20, and a liquid crystal composition is applied to the alignment film and cured to obtain an optically anisotropic layer composed of a cured layer of the liquid crystal composition. While the optically anisotropic layer functions as a so-called λ / 2 plate, the present invention also includes an embodiment in which a laminate integrally comprising the support 20 and the alignment film functions as a λ / 2 plate. The liquid crystal composition for forming the optically anisotropic layer contains a rod-shaped or discotic liquid crystal compound, and may further contain other components such as a leveling agent, an alignment control agent, a polymerization initiator, and an alignment aid.
[0091] Furthermore, the optically anisotropic layer preferably has a broadband with respect to the wavelength of incident light, and is preferably constructed using a liquid crystal material whose birefringence exhibits reverse dispersion. It is also preferable to impart a twist component to the liquid crystal composition or to laminate different retardation layers, thereby making the optically anisotropic layer substantially broadband with respect to the wavelength of incident light. For example, JP 2014-089476 A discloses a method for realizing a broadband patterned λ / 2 plate by laminating two layers of liquid crystal with different twist directions in an optically anisotropic layer, and this method can be preferably used in the present invention.
[0092] Rod-shaped liquid crystal compounds include azomethines, azoxys, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexanecarboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, and alkenylcyclohexylbenzonitriles. Not only low-molecular-weight liquid crystal molecules such as those mentioned above, but also polymeric liquid crystal molecules can be used.
[0093] It is more preferable to fix the alignment of the rod-shaped liquid crystal compound by polymerization. Examples of polymerizable rod-shaped liquid crystal compounds include those described in Makromol. Chem. , Vol. 190, p. 2255 (1989), Advanced Materials Vol. 5, p. 107 (1993), U.S. Patent Nos. 4,683,327, 5,622,648, 5,770,107, WO 95 / 22586, 95 / 24455, 97 / 00600, 98 / 23580, 98 / 52905, JP-A-1-272551, JP-A-6-16616, JP-A-7-110469, JP-A-11-80081, and compounds described in Japanese Patent Application No. 2001-64627 can be used. Furthermore, as the rod-shaped liquid crystal compound, for example, those described in JP-A-11-513019 and JP-A-2007-279688 can also be preferably used.
[0094] Discotic Liquid Crystal Compound: As the discotic liquid crystal compound, for example, those described in JP-A Nos. 2007-108732 and 2010-244038 can be preferably used. When a discotic liquid crystal compound is used in the optically anisotropic layer, the liquid crystal compound 30 stands up in the thickness direction in the optically anisotropic layer, and the optic axis 30A derived from the liquid crystal compound is defined as an axis perpendicular to the disc surface, i.e., a so-called fast axis (see FIG. 17 ).
[0095] <Wavelength-Selective Retardation Plate> The optical element 10 of the present invention includes a wavelength-selective retardation plate 18G provided between the first optically anisotropic member 12 and the second optically anisotropic member 14. In the optical element of the present invention, the wavelength-selective retardation plate is a member that converts circularly polarized light in a specific wavelength range into circularly polarized light having an opposite rotation direction. In the optical element of the present invention, a preferred embodiment is one in which, in addition to the wavelength-selective retardation plate described above, λ / 4 plates are provided on both sides of the wavelength-selective retardation plate. In the optical element shown in the figure, the wavelength-selective retardation plate 18G selectively converts circularly polarized green light into circularly polarized light having an opposite rotation direction, converting right-handed circularly polarized green light into left-handed circularly polarized green light and converting left-handed circularly polarized green light into right-handed circularly polarized green light, while transmitting (passing through) other light while maintaining the rotation direction.
[0096] In other words, a wavelength-selective retardation plate shifts the phase by π only in a specific wavelength range. Such a wavelength-selective retardation plate can also be called, for example, a λ / 2 plate that acts only in a specific wavelength range. Wavelength-selective retardation plates are as described above.
[0097] <Function of Optical Element> As described above, an optically anisotropic layer formed using a composition containing a liquid crystal compound and having a liquid crystal orientation pattern in which the direction of the optical axis 30A rotates along the direction of arrow X refracts circularly polarized light, but the angle of refraction varies depending on the wavelength of the light. Specifically, the longer the wavelength of light, the greater the angle of refraction. Therefore, for example, when incident light is red, green, and blue light, red light is refracted the most and blue light is refracted the least. Therefore, for example, in an AR glass light guide plate, if an optical element made of an optically anisotropic layer having the above-mentioned liquid crystal orientation pattern in which the direction of the optical axis 30A rotates is used as a diffraction element for light entering and exiting the light guide plate, the transmission directions of red light, green light, and blue light will differ in a full-color image, resulting in an image with so-called color shift, in which the red image, green image, and blue image do not match. Here, color misalignment can be eliminated by providing a light guide plate corresponding to each of the red, green, and blue images and stacking three light guide plates, as described in, for example, Bernard C. Kress et al., Towards the Ultimate Mixed Reality Experience: HoloLens Display Architecture Choices, SID 2017 DIGEST, pp. 127-131. However, this configuration makes the light guide plates thick and heavy overall, and also makes the configuration complicated.
[0098] In contrast, the optical element of the present invention has an arrangement of multiple optically anisotropic layers, and a wavelength-selective retardation plate between at least one pair of adjacent optically anisotropic layers among the arranged optically anisotropic layers. Furthermore, the optically anisotropic layers have a liquid crystal orientation pattern in which the orientation of the optical axis derived from the liquid crystal compound rotates in one direction, and the period of the liquid crystal orientation pattern of at least one optically anisotropic layer is different from that of the other optically anisotropic layers. With such an optical element of the present invention, the wavelength dependence of the refraction angle of light is significantly reduced, and light of different wavelengths can be refracted in approximately the same direction and transmitted and emitted. Therefore, by using the optical element of the present invention (e.g., optical element 32 described below) as a diffraction element that introduces light into a light guide plate and / or a diffraction element that outputs light from the light guide plate in, for example, AR glasses, a single light guide plate can propagate red, green, and blue images without causing color shift, thereby displaying appropriate images to the user.
[0099] The operation of the optical element 10 will be described in detail below with reference to the conceptual diagrams in Figures 8 and 9. In the optical element of the present invention, the optical operation is basically achieved only by the optically anisotropic layer and the wavelength-selective retardation plate. Therefore, in order to simplify the drawings and clearly show the configuration and effects, Figure 8 (and Figure 11 , which will be described later) shows only the first optically anisotropic layer 26A and the second optically anisotropic layer 26B of the first optically anisotropic member 12 and the second optically anisotropic member 14, respectively, and the illustrated members are spaced apart in the arrangement direction.
[0100] As described above, the optical element 10 includes a wavelength-selective retardation plate 18G disposed between the first optically anisotropic member 12 having the first optically anisotropic layer 26A and the second optically anisotropic member 14 having the second optically anisotropic layer 26B, which reverses the rotation direction of circularly polarized green light. The optical element 10, as an example, refracts and transmits incident light, for example, circularly polarized blue light and circularly polarized green light. While the incident light in FIG. 8 is right-handed circularly polarized light, the same effect can be achieved if the incident light is left-handed circularly polarized light, except that the direction of refraction is reversed.
[0101] In the optical element 10, right-handed circularly polarized green light G Rand right-handed circularly polarized blue light B R (Incident light L in FIG. 7 4 When the left-handed circularly polarized light G 1L and left-handed circularly polarized blue light B 1L (Transmitted light L in FIG. 7 5 As described above, the angle of refraction by the first optically anisotropic layer 26A is larger for green light having a longer wavelength, and therefore, as shown in FIG. 9, the angle of refraction for the incident light is the angle θ G1 The angle θ of blue light (B) B1 Furthermore, one period Λ of the optically anisotropic layer is larger than one period Λ of the first optically anisotropic layer 26A. A is shorter, the angle of refraction of each ray is larger than when it passes through the second optically anisotropic layer 26B.
[0102] Left-handed circularly polarized green light G transmitted through the first optically anisotropic layer 26A 1L and left-handed circularly polarized blue light B 1L Then, the left-handed circularly polarized light G of the green light is incident on the wavelength-selective retardation plate 18G. As described above, the wavelength-selective retardation plate 18G converts only the circularly polarized light of the green light into circularly polarized light of the opposite rotation direction, and transmits (straight passes through) the other light while maintaining the rotation direction. 1L and left-handed circularly polarized blue light B 1L is incident on the wavelength selective retardation plate 18G and passes through it, and is converted into left-handed circularly polarized blue light B 1L On the other hand, left-handed circularly polarized green light G 1L is right-handed circularly polarized green light G 1R is converted to
[0103] Right-handed circularly polarized green light G transmitted through the wavelength-selective retardation plate 18G 1R and left-handed circularly polarized blue light B 1L The right-handed circularly polarized green light G that has entered the second optically anisotropic layer 26B is then incident on the second optically anisotropic layer 26B. 1R and left-handed circularly polarized blue light B 1L is similarly refracted and converted into left-handed circularly polarized green light G2L and right-handed circularly polarized blue light B 2R and is emitted.
[0104] Here, right-handed circularly polarized green light G 1R and left-handed circularly polarized blue light B 1L As described above, the first optically anisotropic layer 26A and the second optically anisotropic layer 26B have opposite rotation directions of the optical axes 30A of the liquid crystal compounds 30. Therefore, as shown in FIGS. 8 and 9, left-handed circularly polarized light B of blue light is rotated in the opposite direction. 2L is further refracted in the direction opposite to the arrow X direction, and as shown on the left side of FIG. 9, the incident light (right-handed circularly polarized blue light B R ) with respect to the angle θ B2 On the other hand, right-handed circularly polarized green light G 1R 9, the left-handed circularly polarized light G of the green light is refracted in the direction of arrow X in the second optically anisotropic layer 26B, in the opposite direction to that of the first optically anisotropic layer 26A. 2L is the incident light (right-handed circularly polarized green light G R ) with the first angle θ G1 Left-handed circularly polarized blue light B 2L Angle θ B2 Almost the same as the angle θ G2 It is emitted at.
[0105] As described above, in the optical element 10 of the present invention, green light, which has a long wavelength and is highly refracted by the optically anisotropic layer, is refracted in the direction opposite to the arrow X by the first optically anisotropic layer 26A, and then refracted in the direction of arrow X by the second optically anisotropic layer 26B so as to return the refraction. In contrast, blue light, which has a short wavelength and is less refracted by the optically anisotropic layer, is refracted in the direction opposite to the arrow X by both the first optically anisotropic layer 26A and the second optically anisotropic layer 26B. That is, in the optical element 10, depending on the magnitude of refraction by the optically anisotropic layer due to wavelength, long-wavelength light, which is highly refracted, is refracted the first time, and then refracted in the opposite direction the second time to return the refraction. In contrast, short-wavelength light, which is less refracted, is refracted the second time in the same direction as the first time. As a result, the refraction angle θ of the green light with respect to the incident light isG2 and the angle of refraction of blue light θ B2 Therefore, according to the optical element 10 of the present invention, the incident blue light and green light can be refracted at approximately the same angle and emitted in approximately the same direction.
[0106] As described above, the angle of light refracted by the first optically anisotropic layer 26A and the second optically anisotropic layer 26B increases as the wavelength of the light increases. Furthermore, the angle of light refracted by the first optically anisotropic layer 26A and the second optically anisotropic layer 26B increases as the period Λ of the optic axis 30A rotating by 180° along the direction of the arrow X in the liquid crystal alignment pattern decreases. In the optical element 10, as shown in FIG. 3, for example, the period Λ of the liquid crystal alignment pattern in the first optically anisotropic layer 26A increases. A is one period Λ of the liquid crystal alignment pattern in the second optically anisotropic layer 26B. B That is, the first optically anisotropic layer 26A on the light incident side refracts light more strongly. Therefore, by adjusting one period Λ of the liquid crystal orientation pattern for the wavelength of light of interest, it is possible to suitably make the emission directions of light of different wavelengths the same.
[0107] When light of two wavelength ranges is targeted as in the illustrated optical element 10, the design wavelength of the long wavelength light is λa and the design wavelength of the short wavelength light is λb (λa>λb), and one period of the liquid crystal orientation pattern in the first optically anisotropic layer is Λ 1 , one period of the liquid crystal alignment pattern in the second optically anisotropic layer is represented by Λ 2 In this case, the following equation Λ 2 = [(λa+λb) / (λa-λb)]Λ 1 When the following expression is satisfied, the emission directions of light in the two wavelength ranges can be made to be substantially the same. In this expression, either the first optically anisotropic layer 26A or the second optically anisotropic layer 26B may be the first layer. Taking this into consideration, in the present invention, it is preferable that the optical element 10 intended for light of two wavelengths (wavelength ranges) satisfies the following expression: 0.6*{[(λa+λb) / (λa-λb)]Λ 1 ≦Λ 2 ≦3.0*{[(λa+λb) / (λa−λb)]Λ1} This makes it possible to make the wavelength dependency of refraction extremely small, and to make the emission directions of light in the two wavelength ranges approximately the same. Furthermore, in the present invention, it is more preferable that the optical element 10 intended for light of two wavelengths (wavelength ranges) satisfies the following formula: 0.7*{[(λa+λb) / (λa-λb)]Λ 1 ≦Λ 2 ≦1.8*{[(λa+λb) / (λa−λb)]Λ 1} It is more preferable that the following formula is satisfied: 0.8*{[(λa+λb) / (λa-λb)]Λ 1 ≦Λ 2 ≦1.3*{[(λa+λb) / (λa−λb)]Λ 1} It is particularly preferable that the following formula is satisfied: 0.9*{[(λa+λb) / (λa-λb)]Λ 1 ≦Λ 2 ≦1.15*{[(λa+λb) / (λa−λb)]Λ 1}
[0108] [Second Aspect of Optical Element] The optical element 10 described above is intended for light in two wavelength ranges (design wavelengths), namely, green light and blue light. However, the optical element of the present invention is not limited to this, and may be intended for light in three or more wavelength ranges, and may refract and emit incident light.
[0109] An example is shown in Figure 10. Note that the optical element 32 shown in Figure 10 uses many of the same components as the optical element 10 shown in Figure 1, so the same components are denoted by the same reference numerals, and the following description will mainly focus on the different parts. The optical element 32 shown in Figure 10 has a third optical anisotropic member 16 and a wavelength-selective retardation plate 18R in addition to the first optical anisotropic member 12, second optical anisotropic member 14, and wavelength-selective retardation plate 18G of the optical element 10 described above.
[0110] The third optically anisotropic member 16 has a configuration similar to that of the first optically anisotropic member 12, etc., and includes a support 20, an alignment film 24C, and a third optically anisotropic layer 26C. The alignment film 24C and the third optically anisotropic layer 26C are similar to the alignment film 24A and the first optically anisotropic layer 26A described above, except for a different period Λ. The wavelength-selective retardation plate 18R selectively converts circularly polarized red light into circularly polarized light with the opposite rotation direction, converting right-handed circularly polarized red light into left-handed circularly polarized red light and converting left-handed circularly polarized red light into right-handed circularly polarized red light, while allowing all other light to pass through as is.
[0111] In the optical element 32, the first optically anisotropic layer 26A and the third optically anisotropic layer 26C have the same rotation direction of the optical axis 30A of the liquid crystal compound 30 along the direction of arrow X, while the second optically anisotropic layer 26B has the opposite rotation direction of the optical axis 30A of the liquid crystal compound 30 along the direction of arrow X to that of the other two optically anisotropic layers. In the optical element 32, one period Λ in the direction of arrow X, in which the optical axis 30A of the liquid crystal compound 30 rotates by 180° in the liquid crystal orientation pattern, is equal to one period Λ of the first optically anisotropic layer 26A. A is the shortest, and one period Λ of the second optically anisotropic layer 26B is B is the longest. The optical element 32 has the first optically anisotropic member 12 side as the light incident side. That is, in the optical element 32, the first optically anisotropic layer 26A on the light incident side refracts light the most. Furthermore, the optical element 32 has a wavelength-selective retardation plate 18R disposed between the first optically anisotropic member 12 (first optically anisotropic layer 26A) and the second optically anisotropic member 14 (second optically anisotropic layer 26B) that selectively converts the rotation direction of circularly polarized light of red light. Furthermore, the optical element 32 has a wavelength-selective retardation plate 18G disposed between the second optically anisotropic member 14 and the third optically anisotropic member 16 (third optically anisotropic layer 26C) that selectively converts the rotation direction of circularly polarized light of green light.
[0112] The operation of the optical element 32 will be described in detail below with reference to Figures 11 and 12. The optical element 10 refracts and transmits incident light, for example, circularly polarized red light, circularly polarized green light, and circularly polarized blue light, in a predetermined direction. As in Figure 8 above, the incident light in Figure 11 is right-handed circularly polarized light, but the operation and effect are the same even if the incident light is left-handed circularly polarized light, except that the direction of refraction is reversed.
[0113] In the optical element 10, right-handed circularly polarized red light R R , right-handed circularly polarized green light G R and right-handed circularly polarized blue light B R (Incident light L in FIG. 7 4 When the left-handed circularly polarized light R 1L , left-handed circularly polarized green light G 1L and left-handed circularly polarized blue light B 1L (Transmitted light L in FIG. 7 5 As described above, the angle of refraction by the first optically anisotropic layer 26A is largest for red light, which has the longest wavelength, and smallest for blue light, which has the shortest wavelength. Therefore, the angle of refraction of the incident light is, as shown in FIG. 12, the angle θ R1 is the largest, and the angle θ of green light (G) G1 is in the middle, and the angle θ of blue light (B) B1 The period Λ of the optically anisotropic layer is the smallest. A is shortest, the angle of refraction of each ray is largest when it passes through the first optically anisotropic layer 26A.
[0114] Left-handed circularly polarized red light R transmitted through the first optically anisotropic layer 26A 1L , left-handed circularly polarized green light G 1L and left-handed circularly polarized blue light B 1L Next, the left-handed circularly polarized light R of the red light is incident on the wavelength-selective retardation plate 18R. As described above, the wavelength-selective retardation plate 18R converts only the circularly polarized light of the red light into circularly polarized light of the opposite rotation direction, and transmits the other light as it is. 1L , left-handed circularly polarized green light G 1Land left-handed circularly polarized blue light B 1L is incident on the wavelength selective retardation plate 18R and passes through it, and is converted into left-handed circularly polarized green light G 1L and left-handed circularly polarized blue light B 1L On the other hand, left-handed circularly polarized red light R 1L is right-handed circularly polarized red light R 1R is converted to
[0115] Right-handed circularly polarized red light R transmitted through the wavelength-selective retardation plate 18R 1R , left-handed circularly polarized green light G 1L and left-handed circularly polarized blue light B 1L The right-handed circularly polarized red light R then enters the second optically anisotropic layer 26B. 1R , left-handed circularly polarized green light G 1L and left-handed circularly polarized blue light B 1L is similarly refracted and converted into circularly polarized light of the opposite rotation direction, resulting in left-handed circularly polarized red light R 2L , right-handed circularly polarized green light G 2R and right-handed circularly polarized blue light B 2R and is emitted.
[0116] Here, both the green light and the blue light incident on the second optically anisotropic layer 26B are left-handed circularly polarized light. In contrast, the red light incident on the second optically anisotropic layer 26B is right-handed circularly polarized light whose circular polarization direction is different from that of the green light and the blue light, having been converted by the wavelength-selective retardation plate 18R. As described above, the first optically anisotropic layer 26A and the second optically anisotropic layer 26B have opposite rotation directions of the optical axes 30A of the liquid crystal compounds 30. Therefore, as shown in Figures 11 and 12, the left-handed circularly polarized light G of the green light incident on the second optically anisotropic layer 26B 2L and left-handed circularly polarized blue light B 2L is further refracted in the direction opposite to the arrow X direction, and as shown in FIG. 12, the incident light (right-handed circularly polarized green light G R and right-handed circularly polarized blue light B R ) with respect to the angle θ G2 and angle θ B2 On the other hand, the right-handed circularly polarized light R of red light, which is incident on the second optically anisotropic layer 26B and has the opposite direction to the circularly polarized light R of red light, is emitted. 1R12, is refracted in the direction of arrow X in the opposite direction to the first optically anisotropic layer 26A, so as to be returned to the left-handed circularly polarized light R 2L is the incident light (right-handed circularly polarized red light R R ) with respect to the angle θ R1 Angle θ is smaller than R2 The period Λ of the optically anisotropic layer is equal to the period Λ of the second optically anisotropic layer 26B. B Since the angle of refraction of each ray is the smallest when it passes through the second optically anisotropic layer 26B, the angle of refraction of each ray is the smallest when it passes through the second optically anisotropic layer 26B.
[0117] Left-handed circularly polarized red light R transmitted through the second optically anisotropic layer 26B 2L , right-handed circularly polarized green light G 2R and right-handed circularly polarized blue light B 2R Next, the left-handed circularly polarized light R of the red light is incident on the wavelength-selective retardation plate 18G. As described above, the wavelength-selective retardation plate 18G converts only the circularly polarized light of the green light into circularly polarized light of the opposite rotation direction, and transmits the other light as it is. 2L , right-handed circularly polarized green light G 2R and right-handed circularly polarized blue light B 2R is incident on the wavelength selective retardation plate 18G and passes through it, and is converted into left-handed circularly polarized red light R 2L and right-handed circularly polarized blue light B 2R On the other hand, right-handed circularly polarized green light G 2R is left-handed circularly polarized green light G 2L is converted to
[0118] Left-handed circularly polarized red light R transmitted through the wavelength-selective retardation plate 18G 2L , left-handed circularly polarized green light G 2L and right-handed circularly polarized blue light B 2R The left-handed circularly polarized red light R that has entered the third optically anisotropic layer 26C is then incident on the third optically anisotropic layer 26C. 2L , left-handed circularly polarized green light G 2L and right-handed circularly polarized blue light B 2R is similarly refracted and converted into circularly polarized light of the opposite rotation direction, resulting in right-handed circularly polarized red light R 3R , right-handed circularly polarized green light G 3Rand left-handed circularly polarized blue light B 3L and is emitted.
[0119] Here, the blue light incident on the third optical anisotropic layer 26C is right-handed circularly polarized blue light B 2R In addition, since the direction of circular polarization of the red light has been converted by the wavelength selective retardation plate 18R in advance, the red light incident on the third optically anisotropic layer 26C is left-handed circularly polarized red light R, which has a different direction of circular polarization from that of the blue light. 2L Furthermore, the green light incident on the third optically anisotropic layer 26C is converted into left-handed circularly polarized green light G, the direction of which has been converted by the wavelength-selective retardation plate 18G. 2L That is, the blue light incident on the third optically anisotropic layer 26C is right-handed circularly polarized light, and the red and green lights are left-handed circularly polarized light whose circular polarization direction has been converted by the wavelength-selective retardation plate. As described above, the second and third optically anisotropic layers 26B and 26C have opposite rotation directions of the optical axes 30A of the liquid crystal compounds 30.
[0120] Therefore, as shown in FIGS. 11 and 12, the right-handed circularly polarized light B of blue light incident on the third optically anisotropic layer 26C 2R is further refracted in the direction opposite to the arrow X direction, and as shown in FIG. 12, the incident light (right-handed circularly polarized blue light B R ) with respect to the angle θ B3 In contrast, the left-handed circularly polarized red light R 2L When the light is incident on the third optically anisotropic layer 26C, it is further refracted so as to return in the direction of the arrow X. As a result, the right-handed circularly polarized red light R 3R is the incident light (right-handed circularly polarized red light R R ) with respect to the angle θ R2 Angle θ is smaller than R3 Similarly, green light, which has the opposite circular polarization to blue light, is emitted as left-handed circularly polarized light G. 2L When the light enters the third optically anisotropic layer 26C, it is refracted in the direction of arrow X, as shown in the center of FIG. 11. As a result, right-handed circularly polarized green light G 3R is the incident light (right-handed circularly polarized green light G R) with respect to the angle θ G2 Angle θ is smaller than G3 It is emitted at.
[0121] That is, in the optical element 32, red light, which has the longest wavelength and is refracted most by the optically anisotropic layers, is refracted in the direction opposite to the arrow X direction by the first optically anisotropic layer 26A, and then refracted twice in the opposite arrow X direction by the second optically anisotropic layer 26B and the third optically anisotropic layer 26C. Green light, which has the second longest wavelength and is refracted second most by the optically anisotropic layers, is refracted in the direction opposite to the arrow X direction by the first optically anisotropic layer 26A and the second optically anisotropic layer 26B, and then refracted once in the opposite arrow X direction by the third optically anisotropic layer 26C. Blue light, which has the shortest wavelength and is refracted least by the optically anisotropic layers, is refracted three times in the opposite arrow X direction by the first optically anisotropic layer 26A, the second optically anisotropic layer 26B, and the third optically anisotropic layer 26C. In this way, the optical element 32 of the present invention first refracts all light rays largely in the same direction, and then, depending on the magnitude of refraction by the optically anisotropic layer depending on the wavelength, refracts the light rays with the longest wavelengths the greatest number of times in a direction opposite to the initial refraction, reduces the number of times of refraction in the direction opposite to the initial refraction as the wavelength becomes shorter, and minimizes the number of times of refraction in the direction opposite to the initial refraction for the light rays with the shortest wavelengths. This allows the refraction angle θ of the red light with respect to the incident light to be adjusted. R3 and the angle of refraction of green light θ G3 and the angle of refraction of blue light θ B3 Therefore, the optical element 32 of the present invention can refract the incident red, blue, and green light at approximately the same angles and emit them in approximately the same direction.
[0122] When light of three wavelength ranges is targeted as in the illustrated optical element 32, the design wavelength of the longest wavelength light is λa, the design wavelength of the intermediate wavelength light is λb, and the design wavelength of the shortest wavelength light is λc (λa>λb>λc), and one period of the liquid crystal orientation pattern in the first optically anisotropic layer is Λ. 1 , one period of the liquid crystal alignment pattern in the second optically anisotropic layer is represented by Λ 2, one period of the liquid crystal alignment pattern in the third optically anisotropic layer is represented by Λ 3 Then, the following two equations Λ 2 = [(λa+λc)λb / (λa-λb)λc]Λ 1 , Λ 3 = [(λa+λc)λb / (λb-λc)λa]Λ 1 When the following expression is satisfied, the emission directions of light in the two wavelength ranges can be made to be approximately the same. In this expression, either the first optically anisotropic layer 26A or the third optically anisotropic layer 26C may be the first layer. Taking this into consideration, in the present invention, in the optical element 32 intended for light of three wavelengths (wavelength ranges), it is preferable to satisfy at least one of the following two expressions, and more preferably to satisfy both: 0.6*{[(λa+λc)λb / (λa-λb)λc]Λ 1 ≦Λ 2 ≦3.0*{[(λa+λc)λb / (λa−λb)λc]Λ 1} 0.6*{[(λa+λc)λb / (λb-λc)λa]Λ 1 ≦Λ 3 ≦3.0*{[(λa+λc)λb / (λb−λc)λa]Λ 1} This makes it possible to make the wavelength dependency of refraction extremely small and make the emission directions of light in the two wavelength ranges approximately the same. Furthermore, in the present invention, it is more preferable that the optical element 32 intended for light of three wavelengths (wavelength ranges) satisfies the following two formulas: 0.7*{[(λa+λc)λb / (λa-λb)λc]Λ 1 ≦Λ 2 ≦1.8*{[(λa+λc)λb / (λa−λb)λc]Λ 1} 0.7*{[(λa+λc)λb / (λb-λc)λa]Λ 1 ≦Λ 3 ≦1.8*{[(λa+λc)λb / (λb−λc)λa]Λ 1} It is more preferable that the following two formulas are satisfied: 0.8*{[(λa+λc)λb / (λa-λb)λc]Λ 1 ≦Λ 2 ≦1.3*{[(λa+λc)λb / (λa−λb)λc]Λ 1} 0.8*{[(λa+λc)λb / (λb-λc)λa]Λ 1 ≦Λ 3 ≦1.3*{[(λa+λc)λb / (λb−λc)λa]Λ 1 It is particularly preferable that the following two formulas are satisfied: 0.9*{[(λa+λc)λb / (λa-λb)λc]Λ 1 ≦Λ 2 ≦1.15*{[(λa+λc)λb / (λa−λb)λc]Λ 1} 0.9*{[(λa+λc)λb / (λb-λc)λa]Λ 1 ≦Λ 3 ≦1.15*{[(λa+λc)λb / (λb−λc)λa]Λ 1}
[0123] In the optical element of the present invention, as described above, a plurality of optically anisotropic layers are arranged, and according to the wavelength of light, the longer the wavelength of light that is refracted by the optically anisotropic layers, the more times the light is refracted in the opposite direction to the first optically anisotropic layer, so that light of different wavelengths can be refracted at approximately the same angle and emitted in approximately the same direction. Therefore, in the optical element of the present invention, when there are a plurality of wavelength-converting retardation layers, it is preferable that the wavelength range of the light that converts circularly polarized light into the opposite rotation direction gradually becomes shorter in the arrangement direction of the optically anisotropic layers, as in the optical element 32 shown in Figures 10 and 11.
[0124] Furthermore, in the optical element of the present invention, it is easier to control the refraction of each light beam and make the refraction of each light beam uniform by increasing the refraction by the initial optically anisotropic layer, gradually refracting the light beams in the same direction thereafter, and then gradually returning the refraction to the opposite direction. Considering this point, as with the optical element 32 shown in Figures 10 and 11, it is preferable that the period Λ of the liquid crystal orientation pattern of the optically anisotropic layer located at the end of the alignment direction is shortest. In other words, it is preferable that the refraction by the optically anisotropic layer located at the end of the alignment direction is maximized. Note that in the optical element of the present invention, the period Λ of the liquid crystal orientation pattern of the optically anisotropic layer may be configured to gradually increase in the alignment direction of the optically anisotropic layer. Alternatively, the period Λ of the liquid crystal orientation pattern of the optically anisotropic layer may vary irregularly in the alignment direction of the optically anisotropic layer, for example, by providing an optically anisotropic layer having an intermediate period Λ of the liquid crystal orientation pattern between an optically anisotropic layer having the largest period Λ of the liquid crystal orientation pattern and an optically anisotropic layer having the smallest period Λ of the liquid crystal orientation pattern, as in the optical element 32 shown in Figures 10 and 11. That is, in the optical element of the present invention, the period Λ of the liquid crystal orientation pattern of each optically anisotropic layer may be set appropriately depending on the wavelength of light and the refractive index of the optically anisotropic layer.
[0125] In the optical element of the present invention, when multiple wavelength-converting retardation layers are included, the optically anisotropic layers and the wavelength-converting retardation layers are basically arranged alternately, as in the optical element 32 shown in Figures 10 and 11. In this case, it is preferable that the number of wavelength-converting retardation layers is one less than the number of optically anisotropic layers. However, the present invention is not limited thereto. For example, multiple optically anisotropic layers may be arranged in succession, and light refracted continuously by the multiple optically anisotropic layers may be incident on the wavelength-converting retardation layer. Furthermore, multiple wavelength-converting retardation layers may be arranged between two optically anisotropic layers. However, when multiple wavelength-converting retardation layers that convert circularly polarized light in the same wavelength range into circularly polarized light with opposite rotation directions are arranged between two optically anisotropic layers, it is preferable that the number of wavelength-converting retardation layers be an odd number.
[0126] In the optical element of the present invention, optically anisotropic layers may exist in which the period Λ of the liquid crystal alignment pattern is the same, but it is preferable that the period Λ of the liquid crystal alignment pattern is different in all optically anisotropic layers in order to easily make the refraction of light in a plurality of wavelength ranges, i.e., the emission angle, uniform.
[0127] In the optical element of the present invention, there is no limitation on one period Λ in the alignment pattern of the optically anisotropic layer, and it may be set appropriately depending on the application of the optical element, etc.
[0128] The optical element of the present invention may have a wavelength-selective retardation plate that selectively converts circularly polarized light of the shortest design wavelength into circularly polarized light with the opposite rotation direction. For example, a third wavelength-selective retardation plate B that selectively converts circularly polarized light of blue light into circularly polarized light with the opposite rotation direction may be disposed after the third optically anisotropic layer 26C (downstream in the light traveling direction). As described above, the third wavelength-selective retardation plate B converts only circularly polarized light of blue light into circularly polarized light with the opposite rotation direction, and transmits other light as it is. Therefore, right-handed circularly polarized light R of red light 3R , right-handed circularly polarized green light G 3R and left-handed circularly polarized blue light B 3L is incident on the third wavelength selective retardation plate B and passes through it, and is converted into right-handed circularly polarized red light R 3R and right-handed circularly polarized green light G 3R On the other hand, left-handed circularly polarized blue light B 3L is right-handed circularly polarized blue light B 3R As a result, the circularly polarized blue, green, and red light emitted from the optical element can be converted into circularly polarized light with the same rotation direction.
[0129] Here, the optical element of the present invention is suitably used, for example, in AR glasses as a diffraction element that refracts light displayed by a display and introduces it into a light guide plate, and as a diffraction element that refracts light propagating through the light guide plate and emits it from the light guide plate to a user's observation position. In particular, the optical element 32 capable of displaying full-color images is suitably used as a diffraction element in AR glasses. In this case, in order to achieve total reflection of light in the light guide plate, it is necessary to refract the light at a relatively large angle relative to the incident light and introduce it into the light guide plate. Furthermore, in order to reliably emit light that has propagated through the light guide plate, it is necessary to refract the light at a relatively large angle relative to the incident light. Furthermore, as described above, the angle of light transmission through the optically anisotropic layer can be increased by shortening the period Λ of the liquid crystal orientation pattern.
[0130] In consideration of this point, one period Λ of the liquid crystal alignment pattern of the optically anisotropic layer is preferably 50 μm or less, more preferably 10 μm or less, and even more preferably 3 μm or less. In consideration of the accuracy of the liquid crystal alignment pattern, one period Λ of the liquid crystal alignment pattern of the optically anisotropic layer is preferably 0.1 μm or more.
[0131] 3 to 12, the optical axis 30A of the liquid crystal compound 30 in the liquid crystal alignment pattern of the optically anisotropic layer continuously rotates only along the direction of the arrow X. However, the present invention is not limited to this, and various configurations can be used as long as the optical axis 30A of the liquid crystal compound 30 in the optically anisotropic layer continuously rotates along one direction.
[0132] One example is an optically anisotropic layer 34 having a liquid crystal orientation pattern that is a concentric pattern from the inside to the outside, in which the direction of the optical axis of the liquid crystal compound 30 changes while continuously rotating, as conceptually shown in the plan view of Fig. 14. In other words, the liquid crystal orientation pattern of the optically anisotropic layer 34 shown in Fig. 14 is a liquid crystal orientation pattern in which the direction of the optical axis of the liquid crystal compound 30 changes while continuously rotating is provided radially from the center of the optically anisotropic layer 34.
[0133] 14 also shows only the liquid crystal compound 30 on the surface of the alignment film, as in FIG. 6 . However, as described above, the optically anisotropic layer 34 has a structure in which the liquid crystal compound 30 is stacked starting from the liquid crystal compound 30 on the surface of the alignment film, as shown in FIG. 4 . Furthermore, although only one optically anisotropic layer 34 is shown in FIG. 14 , the optical element of the present invention has a plurality of optically anisotropic layers, and a wavelength-selective retardation plate is provided between at least one pair of optically anisotropic layers, as described above. Therefore, even when an optically anisotropic layer having such a concentric liquid crystal alignment pattern is provided, the optical element has a configuration in which a first optically anisotropic layer, a wavelength-selective retardation plate that converts circularly polarized light of red light, a second optically anisotropic layer, a wavelength-selective retardation plate that converts circularly polarized light of green light, and a third optically anisotropic layer are arranged, as in the optical element 32 shown in FIG. 10 .
[0134] In the optically anisotropic layer 34 shown in FIG. 14 , the optical axis (not shown) of the liquid crystal compound 30 is the longitudinal direction of the liquid crystal compound 30. In the optically anisotropic layer 34, the direction of the optical axis of the liquid crystal compound 30 changes while continuously rotating along a number of directions from the center of the optically anisotropic layer 34 toward the outside, for example, the direction indicated by arrow A1, the direction indicated by arrow A2, the direction indicated by arrow A3, etc. Circularly polarized light incident on the optically anisotropic layer 34 having this liquid crystal orientation pattern undergoes a change in absolute phase in each of the local regions where the optical axis direction of the liquid crystal compound 30 differs. At this time, the amount of change in each absolute phase differs depending on the direction of the optical axis of the liquid crystal compound 30 into which the circularly polarized light is incident.
[0135] The optically anisotropic layer 34 having such a concentric liquid crystal orientation pattern, i.e., a liquid crystal orientation pattern in which the optical axis changes by continuously rotating radially, can transmit incident light as divergent or convergent light depending on the direction of rotation of the optical axis of the liquid crystal compound 30 and the direction of the incident circularly polarized light. In other words, by making the liquid crystal orientation pattern of the optically anisotropic layer concentric, the optical element of the present invention can function as, for example, a convex lens or a concave lens.
[0136] Here, when the liquid crystal orientation pattern of the optically anisotropic layer is concentric and the optical element functions as a convex lens, it is preferable to gradually shorten one period Λ, in which the optical axis rotates 180°, from the center of the optically anisotropic layer 34 toward the outside in one direction in which the optical axis continuously rotates. As described above, the angle of refraction of light with respect to the incident direction increases as one period Λ of the liquid crystal orientation pattern becomes shorter. Therefore, by gradually shortening one period Λ of the liquid crystal orientation pattern from the center of the optically anisotropic layer 34 toward the outside in one direction in which the optical axis continuously rotates, the light focusing power of the optically anisotropic layer 34 can be further improved, and the performance as a convex lens can be improved.
[0137] In the present invention, depending on the application of the optical element, for example, when it is used as a concave lens, it is preferable to rotate one period Λ, in which the optical axis rotates by 180°, from the center of the optically anisotropic layer 34 in the opposite direction to the direction in which the optical axis continuously rotates, and gradually shorten the period Λ from the center of the optically anisotropic layer 34 toward the outside in one direction. As described above, the angle of refraction of light with respect to the incident direction increases as the period Λ in the liquid crystal orientation pattern becomes shorter. Therefore, by gradually shortening one period Λ in the liquid crystal orientation pattern from the center of the optically anisotropic layer 34 toward the outside in one direction in which the optical axis continuously rotates, the light divergence power of the optically anisotropic layer 34 can be further improved, and the performance as a concave lens can be improved.
[0138] In the present invention, it is also preferable to reverse the rotation direction of the incident circularly polarized light, for example, when the optical element is a concave lens.
[0139] In the present invention, when the optical element is used as a convex lens or a concave lens, it is preferable that the following formula be satisfied: Φ(r)=(π / λ)[(r 2 +f 2 ) 1/2 -f] where r is the distance from the center of the concentric circle and is expressed by the following formula: r = (x 2 +y 2 ) 1/2x and y represent the position in the plane, and (x, y) = (0, 0) represents the center of the concentric circle. Φ(r) represents the angle of the optical axis at the distance r from the center, λ represents the wavelength, and f represents the designed focal length.
[0140] Conversely, in the present invention, the period Λ of the concentric liquid crystal orientation pattern may be gradually increased from the center of the optically anisotropic layer 34 outward in one direction in which the optical axis continuously rotates. Furthermore, depending on the application of the optical element, for example, when it is desired to provide a light intensity distribution in the transmitted light, a configuration may be used in which, rather than gradually changing the period Λ in one direction in which the optical axis continuously rotates, there are regions in which the period Λ varies in part in one direction in which the optical axis continuously rotates. In addition, the optical element of the present invention may have an optically anisotropic layer in which the period Λ is uniform throughout and an optically anisotropic layer in which the period Λ varies in part. This point also applies to a configuration in which the optical axis continuously rotates in only one direction, as shown in FIG. 3, which will be described later.
[0141] 15 conceptually shows an example of an exposure device for forming such a concentric alignment pattern on an alignment film (e.g., alignment film 24A, alignment film 24B, and alignment film 24C). Exposure device 80 includes a light source 84 equipped with a laser 82, a polarizing beam splitter 86 that splits laser light M from laser 82 into S-polarized light MS and P-polarized light MP, a mirror 90A arranged in the optical path of the P-polarized light MP, a mirror 90B arranged in the optical path of the S-polarized light MS, a lens 92 arranged in the optical path of the S-polarized light MS, a polarizing beam splitter 94, and a λ / 4 plate 96.
[0142] The P-polarized light MP split by the polarizing beam splitter 86 is reflected by a mirror 90A and enters a polarizing beam splitter 94. On the other hand, the S-polarized light MS split by the polarizing beam splitter 86 is reflected by a mirror 90B, collected by a lens 92, and enters the polarizing beam splitter 94. The P-polarized light MP and the S-polarized light MS are combined by the polarizing beam splitter 94 and converted into right- and left-circularly polarized light according to the polarization direction by a λ / 4 plate 96, and then enter the alignment film 24 on the support 20. Here, due to interference between the right- and left-circularly polarized light, the polarization state of the light irradiated onto the alignment film 24 changes periodically in the form of interference fringes. Because the crossing angle between the left- and right-circularly polarized light changes from the inside to the outside of the concentric circles, an exposure pattern whose pitch changes from the inside to the outside is obtained. This results in a concentric alignment pattern in the alignment film 24 in which the alignment state changes periodically.
[0143] In this exposure device 80, one period Λ of the liquid crystal orientation pattern in which the optical axis of the liquid crystal compound 30 continuously rotates 180° along one direction can be controlled by changing the refractive power of the lens 92 (the F-number of the lens 92), the focal length of the lens 92, and the distance between the lens 92 and the orientation film 24. Furthermore, by adjusting the refractive power of the lens 92 (the F-number of the lens 92), the length Λ of one period of the liquid crystal orientation pattern can be changed in one direction in which the optical axis continuously rotates. Specifically, the length Λ of one period of the liquid crystal orientation pattern in one direction in which the optical axis continuously rotates can be changed by adjusting the spread angle of the light expanded by the lens 92, which interferes with the parallel light. More specifically, when the refractive power of the lens 92 is weakened, the light approaches parallel light, so the length Λ of one period of the liquid crystal orientation pattern gradually shortens from the inside to the outside, and the F-number increases. Conversely, when the refractive power of the lens 92 is increased, the length Λ of one period of the liquid crystal alignment pattern suddenly decreases from the inside to the outside, and the F-number decreases.
[0144] In this way, the configuration in which the period Λ of the optical axis, which rotates 180°, is changed in one direction in which the optical axis continuously rotates, can also be used in the configuration in which the optical axis 30A of the liquid crystal compound 30 continuously rotates and changes only in one direction, the direction of the arrow X, as shown in Figures 3 to 12. For example, by gradually shortening the period Λ of the liquid crystal orientation pattern in the direction of the arrow X, an optical element that transmits light in a condensing manner can be obtained. Furthermore, by reversing the direction in which the optical axis rotates 180° in the liquid crystal orientation pattern, an optical element that transmits light in a diffusive manner only in the direction of the arrow X can be obtained. Note that an optical element that transmits light in a diffusive manner only in the direction of the arrow X can also be obtained by reversing the rotation direction of the incident circularly polarized light. Furthermore, depending on the application of the optical element, for example, when it is desired to provide a light intensity distribution in the transmitted light, a configuration in which the period Λ is partially different in the direction of the arrow X rather than gradually changing the period Λ in the direction of the arrow X can also be used. For example, as a method for partially changing one period Λ, a method of patterning a photo-alignment film by scanning exposure while arbitrarily changing the polarization direction of focused laser light can be used.
[0145] The optical element of the present invention can be used in various applications that transmit light in a direction different from the incident direction, such as an optical path changing member in an optical device, a light focusing element, a light diffusing element in a predetermined direction, and a diffraction element.
[0146] As a preferred example, as conceptually shown in FIG. 16 , the optical element 32 may be provided at a distance from the light guide plate 42. This diffractive element guides light (projected image) emitted by the display 40 into the light guide plate 42 at an angle sufficient for total reflection, and then emits the light propagating through the light guide plate 42 from the light guide plate 42 to a viewing position for a user U wearing the AR glasses. While FIG. 16 illustrates the optical element 32 shown in FIG. 10 as a full-color image, the optical element 10 shown in FIG. 3 may also be suitably used when displaying a two-color image with AR glasses. As mentioned above, the optical element of the present invention has a small angle dependency of the refraction angle during transmission, allowing red, green, and blue light emitted by the display 40 to be refracted in the same direction. Therefore, even when a single light guide plate 42 propagates red, green, and blue images, a full-color image without color shift can be emitted from the light guide plate to a viewing position for a user U wearing the AR glasses. Therefore, by using the optical element of the present invention, the light guide plate of the AR glass can be made thinner and lighter overall, and the configuration of the AR glass can be simplified. Note that the light guide element of the present invention is not limited to a configuration in which two optical elements of the present invention are provided spaced apart from each other on a light guide plate 42 as shown in Figure 16, and may be configured such that only one optical element of the present invention is provided on a light guide plate for introducing light into the light guide plate 42 or for extracting light from the light guide plate 42.
[0147] In the above examples, the optical element of the present invention is used as an optical element having two or three optically anisotropic layers, which transmits and refracts two colors of light, green light and blue light, or three colors of light, red light, green light, and blue light. However, the present invention is not limited to this, and various configurations can be used. For example, the optical element of the present invention may have three optically anisotropic layers and two wavelength-selective retardation plates, as in FIG. 1, and transmits and refracts two colors selected from red light, green light, and blue light, as well as infrared light or ultraviolet light. Alternatively, the optical element of the present invention may have four or five (or six or more) optically anisotropic layers and three or four (the number of optically anisotropic layers minus one) wavelength-selective retardation plates, and transmits and refracts infrared light and / or ultraviolet light in addition to red light, green light, and blue light. Alternatively, the optical element of the present invention may have two optically anisotropic layers and one wavelength-selective retardation plate, as in Fig. 1, and may be configured to transmit and refract red light and blue light or red light and green light, or to refract and transmit one color selected from red light, green light, and blue light, and infrared light or ultraviolet light, or to refract and transmit infrared light and / or ultraviolet light.
[0148] The present invention will be described in more detail below with reference to examples. The materials, amounts used, ratios, treatment details, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the examples shown below.
[0149] Comparative Example 1 <Preparation of Wavelength-Selective Retardation Plate> (Support) A glass substrate was prepared as a support.
[0150] (Formation of Orientation Film) The following coating solution for forming an alignment film was applied to a support by spin coating. The support on which the coating film of the coating solution for forming an alignment film had been formed was dried on a hot plate at 60° C. for 60 seconds to form an alignment film.
[0151] Coating liquid for forming alignment film ----------------------------------- Photoalignment material A 1.00 parts by mass Water 16.00 parts by mass Butoxyethanol 42.00 parts by mass Propylene glycol monomethyl ether 42.00 parts by mass ---------------------------------------------------
[0152] -Photo alignment material A-
[0153] (Exposure of Alignment Film) The resulting alignment film was exposed to polarized ultraviolet light (50 mJ / cm 2 , using an ultra-high pressure mercury lamp) to form an alignment film P-1.
[0154] (Preparation of Wave Plate A1) The following composition A-1 was prepared as a rod-like liquid crystal composition for forming a wave plate.
[0155] Composition A-1 ----------------------------------- Rod-like liquid crystal compound L-1 100.00 parts by mass Photopolymerization initiator B 1.00 part by mass Surfactant F1 (listed below) 0.057 parts by mass Surfactant F2 (listed below) 0.143 parts by mass Methyl ethyl ketone 161.5 parts by mass Cyclohexanone 28.5 parts by mass
[0156] Rod-shaped liquid crystal compound L-1
[0157] Photopolymerization initiator B
[0158] Surfactant F1
[0159] Surfactant F2
[0160]
[0161] The wave plate was formed by applying the above composition A-1 onto the alignment film P-1. The applied coating film was heated on a hot plate at 110°C. Thereafter, it was heated at 100°C under a low-oxygen atmosphere (100 ppm or less) with an illuminance of 80 mW / cm. 2 , irradiation amount 500mJ / cm 2 The alignment of the rod-shaped liquid crystal compound was fixed by curing the film by irradiating it with light from a metal halide lamp. Waveplate A1 was thus obtained. The Re(725) of the obtained waveplate A1 at a wavelength λ=725 nm was 725 nm. The Nz factor of the produced waveplate A1 was 1.0 at 550 nm. The Re(725) was measured using an Axoscan manufactured by Axometrix, and the Nz factor was measured by changing the angle of incidence by ±40° (in 5° increments) in a plane parallel to the slow axis and fast axis of the waveplate.
[0162] (Preparation of Wave Plate A2) Wave plate A2 was obtained in the same manner as in preparation of wave plate A1, except that the film thickness of the coating film of composition A-1 was changed. The Re(725) of the obtained wave plate A2 at a wavelength λ=725 nm was 1450 nm. The Nz factor of the prepared wave plate A2 was 1.0 at 550 nm.
[0163] Waveplate A1 and waveplate A2 were laminated to form the layer configuration shown in Table 2 below. Furthermore, during lamination, the support and alignment film were peeled off, and then the layers were laminated sequentially. This resulted in the production of a first wavelength-selective retardation plate that converts linearly polarized green light into orthogonal linearly polarized light and does not change the phase of linearly polarized light in other wavelength ranges. The angles shown in Table 1 below are the angles of the slow axis azimuth relative to the vibration direction of the incident linearly polarized light, and when viewed from the side opposite to the side onto which the linearly polarized light is incident, clockwise are represented as negative values and counterclockwise are represented as positive values. This also applies to tables showing the configurations of wavelength-selective retardation plates in the following examples and comparative examples.
[0164]
[0165] [Example 1] <Preparation of Wavelength-Selective Retardation Plate> (Formation of Alignment Film) An alignment film P-1 was formed on a support in the same manner as in Comparative Example 1. (Preparation of Waveplate B1) An optically anisotropic layer B1-1 was prepared in the same manner as in the preparation of the waveplate A1 in Comparative Example 1, except that the film thickness of the coating film of the rod-shaped liquid crystal compound was adjusted. The Re(725) of the obtained optically anisotropic layer B1-1 at a wavelength λ of 725 nm was 362.5 nm. The Nz factor of the prepared optically anisotropic layer B1-1 was 1.0 at 550 nm.
[0166] Further, as a discotic liquid crystal composition for forming the wave plate B1, the following composition B-1 was prepared.
[0167] Composition B-1 ------------------------------------------------ 80 parts by mass of the following discotic liquid crystal (A) 20 parts by mass of the following discotic liquid crystal (B) Polymerizable monomer E1 10 parts by mass Surfactant F4 0.3 parts by mass Photopolymerization initiator (Irgacure 907, manufactured by BASF) 3 parts by mass Methyl ethyl ketone 290 parts by mass Cyclohexanone 50 parts by mass
[0168] Discotic liquid crystal (A)
[0169] Discotic liquid crystal (B)
[0170] Polymerizable Monomer E1
[0171] Surfactant F4 (The symbol assigned to each repeating unit indicates the content of each repeating unit by mass.)
[0172] The wave plate B1 was formed by applying the composition B-1 to the optically anisotropic layer B1-1. Specifically, the surface of the optically anisotropic layer B1-1 was subjected to a discharge of 150 W·min / m 2After corona treatment, Composition B-1 was applied to the corona-treated surface. The coating film was then dried at 70°C for 2 minutes, and after the solvent was evaporated, the coating film was heat-aged at 115°C for 3 minutes. Thereafter, the coating film was kept at 45°C and irradiated with ultraviolet light (300 mJ / cm) using a metal halide lamp under a nitrogen atmosphere. 2 ) and cured to fix the alignment of the discotic liquid crystal compound. Waveplate B1 was thus obtained. The obtained waveplate B1 had an Re(725) of 725 nm at a wavelength λ of 725 nm. The fabricated waveplate B1 also had an Nz factor of 0.5 at 550 nm. The optically anisotropic layer B1-2 formed on the optically anisotropic layer B1-1 using composition B-1 containing a discotic liquid crystal compound had an Re(725) of 362.5 nm at a wavelength λ of 725 nm. The fabricated optically anisotropic layer B1-2 also had an Nz factor of 0 at 550 nm.
[0173] (Preparation of Waveplate B2) An optically anisotropic layer B2-1 formed from a rod-shaped liquid crystal compound, an optically anisotropic layer B2-2 formed from a discotic liquid crystal compound, and a laminate thereof, a waveplate B2, were obtained in the same manner as in preparation of waveplate B1, except that the thicknesses of the coating films of the rod-shaped liquid crystal compound and the discotic liquid crystal compound were changed. The obtained optically anisotropic layer B2-1 had an Re(725) of 725 nm at a wavelength λ of 725 nm. The prepared optically anisotropic layer B2-1 also had an Nz factor of 1.0 at 550 nm. The obtained optically anisotropic layer B2-2 had an Re(725) of 725 nm at a wavelength λ of 725 nm. The prepared optically anisotropic layer B2-2 also had an Nz factor of 0. The obtained waveplate B2 had an Re(725) of 1450 nm at a wavelength λ of 725 nm. The Nz factor of the fabricated wavelength B2 was 0.5 at 550 nm.
[0174] Waveplate B1 and waveplate B2 were laminated to have the layer configuration shown in Table 3 below. Furthermore, during lamination, the support and alignment film were peeled off, and then the layers were laminated in order. This produced a second wavelength-selective retardation plate that converts linearly polarized green light into orthogonal linearly polarized light, while leaving the phase of linearly polarized light in other wavelength ranges unchanged.
[0175]
[0176] Comparative Example 2 <Preparation of Wavelength-Selective Retardation Plate> Wave plates C1 and C2 were prepared in the same manner as in Comparative Example 1, except that the thickness of the coating film of the rod-like liquid crystal compound was adjusted.
[0177] The Re(490) of the obtained wave plate C1 at a wavelength λ of 490 nm was 490 nm. The Nz factor of the produced wave plate C1 was 1.0 at 650 nm.
[0178] The Re(490) of the obtained wave plate C2 at a wavelength λ of 490 nm was 980 nm. The Nz factor of the produced wave plate C2 was 1.0 at 650 nm.
[0179] Waveplate C1 and waveplate C2 were laminated to have the layer configuration shown in Table 4 below. Furthermore, during lamination, the support and alignment film were peeled off, and then the layers were laminated in order. This produced a third wavelength-selective retardation plate that converts linearly polarized red light into orthogonal linearly polarized light and does not change the phase of linearly polarized light in other wavelength ranges.
[0180]
[0181] Example 2 Preparation of Wavelength-Selective Retardation Plate Optically anisotropic layers D1-1 and D1-2 were prepared in the same manner as in Example 1, except that the thicknesses of the coating films of the rod-shaped liquid crystal compound and the discotic liquid crystal compound were adjusted, thereby obtaining a wave plate D1. Optically anisotropic layers D2-1 and D2-2 were prepared in the same manner as in Example 1, thereby obtaining a wave plate D2.
[0182] The resulting optically anisotropic layer D1-1 had an Re(490) of 245 nm at a wavelength λ of 490 nm. The Nz factor of the produced optically anisotropic layer D1-1 was 1.0 at 650 nm. The resulting optically anisotropic layer D1-2 had an Re(490) of 245 nm at a wavelength λ of 490 nm. The Nz factor of the produced optically anisotropic layer D1-2 was 0 at 650 nm. The resulting waveplate D1 had an Re(490) of 490 nm at a wavelength λ of 490 nm. The Nz factor of the produced waveplate D1 was 0.5 at 650 nm.
[0183] The resulting optically anisotropic layer D2-1 had an Re(490) of 490 nm at a wavelength λ of 490 nm. The Nz factor of the produced optically anisotropic layer D2-1 was 1.0 at 650 nm. The resulting optically anisotropic layer D2-2 had an Re(490) of 490 nm at a wavelength λ of 490 nm. The Nz factor of the produced optically anisotropic layer D2-2 was 0 at 650 nm. The resulting waveplate D2 had an Re(490) of 980 nm at a wavelength λ of 490 nm. The Nz factor of the produced waveplate D2 was 0.5 at 650 nm.
[0184] Wave plate D1 and wave plate D2 were laminated to have the layer configuration shown in Table 5 below. Furthermore, during lamination, the support and alignment film were peeled off, and then the layers were laminated in order. This produced a fourth wavelength-selective retardation plate that converts linearly polarized light of red light into orthogonal linearly polarized light and does not change the phase of linearly polarized light in other wavelength ranges.
[0185]
[0186] [Comparative Example 3] <Preparation of Wavelength-Selective Retardation Plate> The wave plates A1 and A2 prepared in Comparative Example 1 were laminated to obtain the layer configuration shown in Table 6 below. Furthermore, during lamination, the support and alignment film were peeled off, and then the layers were laminated in order. This produced a fifth wavelength-selective retardation plate that converts linearly polarized light of green light into orthogonal linearly polarized light, without changing the phase of linearly polarized light in other wavelength ranges.
[0187]
[0188] [Example 3] <Preparation of Wavelength-Selective Retardation Plate> The wave plates B1 and B2 prepared in Example 1 were laminated to form the layer configuration shown in Table 7 below. Furthermore, during lamination, the support and alignment film were peeled off, and then the layers were laminated in order. In this way, a sixth wavelength-selective retardation plate was prepared, which converts linearly polarized light of green light into orthogonal linearly polarized light, without changing the phase of linearly polarized light in other wavelength ranges.
[0189]
[0190] [Comparative Example 4] <Preparation of Wavelength-Selective Retardation Plate> The wave plates C1 and C2 prepared in Comparative Example 2 were laminated to obtain the layer configuration shown in Table 8 below. Furthermore, during lamination, the support and alignment film were peeled off, and then the layers were laminated in order. In this way, a seventh wavelength-selective retardation plate was prepared, which converts linearly polarized light of red light into orthogonal linearly polarized light, without changing the phase of linearly polarized light in other wavelength ranges.
[0191]
[0192] [Example 4] <Preparation of Wavelength-Selective Retardation Plate> The wave plates D1 and D2 prepared in Example 2 were laminated to have the layer configuration shown in Table 9 below. Furthermore, during lamination, the support and alignment film were peeled off, and then the layers were laminated in order. In this way, an eighth wavelength-selective retardation plate was prepared, which converts linearly polarized light of red light into orthogonal linearly polarized light, without changing the phase of linearly polarized light in other wavelength ranges.
[0193]
[0194] [Evaluation of Wavelength-Selective Retardation Plate] The wavelength-selective retardation plates of the examples and comparative examples were sandwiched between two linear polarizers to evaluate their retardation characteristics with respect to linearly polarized light. The two linear polarizers were arranged so that their transmission axes were perpendicular to each other, and linearly polarized light at an azimuth angle of 0° was incident on the first retardation layer of the wavelength-selective retardation plate. In this arrangement, unpolarized light was first incident from the front (at an angle of 0° relative to the normal) of the wavelength-selective retardation plate placed between the linear polarizers, and the light intensity of the emitted light was measured with a photodetector. Furthermore, the orientation of only the wavelength-selective retardation plate placed between the linear polarizers was adjusted so that linearly polarized light was incident on the wavelength-selective retardation plate at an azimuth angle of 0° and a polar angle of 40°. Similarly, the light intensity of the emitted light was measured with a photodetector. When the light intensity of light emitted from the wavelength-selective retardation plate disposed between the above-mentioned linear polarizers is Iout, and the light intensity of light emitted when the transmission axes of the two linear polarizers are arranged parallel to each other and the wavelength-selective retardation plate is removed is Ipara, the transmittance was calculated from the following formula: Transmittance = Iout / Ipara For light of a certain wavelength, the higher the transmittance, the more the wavelength-selective retardation plate functions as a λ / 2 retardation plate, and the lower the transmittance, the less it functions as a λ / 2 retardation plate.
[0195] Light having wavelengths of 450 nm, 532 nm, and 650 nm was incident on the wavelength-selective retardation plates produced in Comparative Examples 1 to 4 and Examples 1 to 4, and the transmittance (phase difference characteristics with respect to linearly polarized light) at each wavelength was evaluated. When light was incident from the front, the wavelength-selective retardation plates of Comparative Example 1 and Example 1 had high transmittance (≧80%) at a wavelength of 532 nm and had equivalent λ / 2 retardation function. Furthermore, the transmittance was low (≦10%) at wavelengths of 450 nm and 650 nm, and they had almost no retardation function. That is, it was confirmed that the wavelength-selective retardation plates of Comparative Example 1 and Example 1 functioned as wavelength-selective retardation plates when light was incident from the front direction. When light was incident at a polar angle of 40°, the wavelength-selective retardation plate of Example 1 had high transmittance at a wavelength of 532 nm and had excellent λ / 2 retardation function compared to the wavelength-selective retardation plate of Comparative Example 1. Furthermore, for wavelengths of 450 nm and 650 nm, the wavelength-selective retardation plate of Example 1 had lower transmittance and better wavelength selectivity than the wavelength-selective retardation plate of Comparative Example 1. That is, it was confirmed that the wavelength-selective retardation plate of Example 1 had a small difference between the phase difference occurring when light was incident from the front direction and the phase difference occurring when light was incident from an oblique direction.
[0196] When light was incident from the front, the wavelength-selective retardation plates of Comparative Example 2 and Example 2 had high transmittance (≧80%) at a wavelength of 650 nm and had equivalent λ / 2 retardation function. Furthermore, at wavelengths of 450 nm and 532 nm, the transmittance was low (≦10%) and they had almost no retardation function. That is, it was confirmed that the wavelength-selective retardation plates of Comparative Example 1 and Example 1 function as wavelength-selective retardation plates when light was incident from the front. When light was incident at an oblique angle of 40°, the wavelength-selective retardation plate of Example 2 had a higher transmittance at a wavelength of 650 nm and an excellent λ / 2 retardation function compared to the wavelength-selective retardation plate of Comparative Example 2. Furthermore, at wavelengths of 450 nm and 532 nm, the wavelength-selective retardation plate of Example 2 had a lower transmittance and excellent wavelength selectivity compared to the wavelength-selective retardation plate of Comparative Example 2. That is, it was confirmed that the wavelength-selective retardation plate of Example 2 has a small difference between the phase difference occurring when light is incident from the front direction and the phase difference occurring when light is incident from an oblique direction.
[0197] The wavelength-selective retardation plates of Comparative Example 3 and Example 3 had high transmittance (≧80%) at a wavelength of 532 nm and equivalent λ / 2 retardation function when light was incident from the front. Furthermore, they had low transmittance (≦10%) at wavelengths of 450 nm and 650 nm, and had almost no retardation function. That is, it was confirmed that the wavelength-selective retardation plates of Comparative Example 3 and Example 3 function as wavelength-selective retardation plates when light was incident from the front. When light was incident at an oblique angle of 40°, the wavelength-selective retardation plate of Example 3 had a higher transmittance at a wavelength of 532 nm and an excellent λ / 2 retardation function compared to the wavelength-selective retardation plate of Comparative Example 3. Furthermore, at wavelengths of 450 nm and 650 nm, the wavelength-selective retardation plate of Example 3 had a lower transmittance and excellent wavelength selectivity compared to the wavelength-selective retardation plate of Comparative Example 3. That is, it was confirmed that the wavelength-selective retardation plate of Example 3 had a small difference between the phase difference occurring when light was incident from the front direction and the phase difference occurring when light was incident from an oblique direction. Furthermore, the transmittance spectra (wavelengths of 400 nm to 700 nm) of the wavelength-selective retardation plates produced in Examples 1 and 3 were measured when light was incident from the front. The wavelength-selective retardation plate of Example 3 had a higher transmittance for green light (wavelengths of 500 nm to 570 nm) than the wavelength-selective retardation plate of Example 1, and thus had a superior λ / 2 retardation function.
[0198] The wavelength-selective retardation plates produced in Comparative Example 4 and Example 4 had high transmittance (≧80%) at a wavelength of 650 nm and equivalent λ / 2 retardation function when light was incident from the front. Furthermore, they had low transmittance (≦10%) at wavelengths of 450 nm and 532 nm, and exhibited almost no retardation function. That is, it was confirmed that the wavelength-selective retardation plates of Comparative Example 4 and Example 4 function as wavelength-selective retardation plates when light was incident from the front. When light was incident at an oblique angle of 40°, the wavelength-selective retardation plate of Example 4 had a higher transmittance at a wavelength of 650 nm than Comparative Example 4 and exhibited excellent λ / 2 retardation function. Furthermore, the wavelength-selective retardation plate of Example 4 had a lower transmittance at wavelengths of 450 nm and 532 nm than Comparative Example 4 and exhibited excellent wavelength selectivity. That is, it was confirmed that the wavelength-selective retardation plate of Example 4 had a small difference between the retardation generated when light was incident from the front and the retardation generated when light was incident from an oblique direction. Furthermore, the transmittance spectra (wavelengths of 400 nm to 700 nm) were measured for the wavelength-selective retardation plates of Examples 2 and 4 when light was incident from the front. The wavelength-selective retardation plate of Example 4 had a higher transmittance for red light (wavelengths of 620 nm to 690 nm) than Example 2, and had an excellent λ / 2 retardation function.
[0199] Comparative Example 11 Preparation of Wavelength-Selective Retardation Plate for Circularly Polarized Light (Preparation of λ / 4 Plate) The following composition C-1 was prepared as a liquid crystal composition for forming a λ / 4 plate.
[0200] Composition C-1 ----------------------------------- Liquid crystal compound L-2 42.00 parts by mass Liquid crystal compound L-3 42.00 parts by mass Liquid crystal compound L-4 16.00 parts by mass Polymerization initiator PI-1 0.50 parts by mass Surfactant G-1 0.20 parts by mass Methyl ethyl ketone 176.00 parts by mass Cyclopentanone 44.00 parts by mass ---------------------------------------------------
[0201] Liquid crystal compound L-2
[0202] Liquid crystal compound L-3
[0203] Liquid crystal compound L-4
[0204] Polymerization initiator PI-1
[0205] Surfactant G-1 (The symbol assigned to each repeating unit indicates the content of each repeating unit by mass.)
[0206] An optically anisotropic layer QA in which the alignment direction of the reverse dispersion liquid crystal compound was fixed was formed by the following procedure. The optically anisotropic layer QA was formed by applying the above composition C-1 onto the above alignment film P-1. The applied coating was heated to 100°C on a hot plate, then cooled to 65°C, and then irradiated with ultraviolet light of 365 nm wavelength at 500 mJ / cm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with an irradiation dose of 1000 nm, thereby fixing the alignment of the liquid crystal compound. Thus, an optically anisotropic layer QA was obtained. The resulting optically anisotropic layer QA had an Re(550) of 138 nm and an Re(450) / Re(550) ratio of 0.86.
[0207] Furthermore, a layer in which the alignment direction of a reverse dispersion liquid crystal compound was fixed was formed as an optically anisotropic layer QC by the following procedure. The optically anisotropic layer QC was formed by coating the following composition D-1 on the optically anisotropic layer QA. The coated film was heated to 70°C on a hot plate, then cooled to 65°C, and then irradiated with ultraviolet light of 365 nm wavelength at 500 mJ / cm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with an irradiation dose of 1000 nm to fix the alignment of the liquid crystal compound. This resulted in a λ / 4 plate. The retardation Rth(550) in the thickness direction of the obtained optically anisotropic layer QC was −69 nm.
[0208] Composition D-1 ----------------------------------- 34.00 parts by mass of liquid crystal compound L-1 below 44.00 parts by mass of liquid crystal compound L-2 above 22.00 parts by mass of liquid crystal compound L-3 above 1.50 parts by mass of polymerization initiator PI-1 above 0.40 parts by mass of surfactant T-2 below 0.20 parts by mass of surfactant T-3 below 0.50 parts by mass of compound S-1 below 14.00 parts by mass of compound M-1 below 248.00 parts by mass ------------------------------------------------
[0209] Liquid crystal compound L-1
[0210] Surfactant T-2
[0211] Surfactant T-3
[0212] Compound S-1
[0213] Compound M-1
[0214] The above-prepared λ / 4 plate, the third wavelength-selective retardation plate prepared in Comparative Example 2, and the first wavelength-selective retardation plate prepared in Comparative Example 1 were laminated together to form the layer structures shown in Tables 10 and 11 below. Furthermore, during lamination, the support and the alignment film were peeled off, and then the layers were laminated sequentially. This resulted in the wavelength-selective retardation plate R1, which converts circularly polarized light of red light into circularly polarized light with the opposite rotation direction, without changing the phase of circularly polarized light in other wavelength ranges, and the wavelength-selective retardation plate G1, which converts circularly polarized light of green light into the opposite circularly polarized light, without changing the phase of circularly polarized light in other wavelength ranges.
[0215]
[0216]
[0217] <Preparation of First Optically Anisotropic Member> (Formation of Alignment Film) An alignment film was formed on a support in the same manner as in Comparative Example 1. The alignment film was exposed to light in the following manner.
[0218] (Exposure of Alignment Film) The alignment film was exposed using the exposure device shown in Figure 15 to form an alignment film PG-1 having an alignment pattern. In the exposure device, a laser emitting laser light with a wavelength of 355 nm was used. The exposure amount by the interference light was 1000 mJ / cm 2 It was decided.
[0219] (Formation of Optically Anisotropic Layer) The following composition E-1 was prepared as a liquid crystal composition for forming the first optically anisotropic layer.
[0220] Composition E-1 --------------------------------------------------- Liquid crystal compound L-1 above: 10.00 parts by mass Liquid crystal compound L-5 below: 90.00 parts by mass Chiral agent C1: 0.69 parts by mass Polymerization initiator (Irgacure OXE01, manufactured by BASF): 1.00 part by mass Surfactant F2 above: 0.30 parts by mass Methyl ethyl ketone: 550.00 parts by mass Cyclopentanone: 550.00 parts by mass
[0221] Liquid crystal compound L-5
[0222] Chiral agent C1
[0223] The optically anisotropic layer was formed by applying composition E-1 in multiple layers onto the alignment film PG-1. Multilayer application refers to the process of first applying composition E-1 as a first layer onto the alignment film, heating it, and then curing it with UV light to form a liquid crystal fixation layer, and then repeatedly applying layers from the second layer onwards onto the liquid crystal fixation layer, and similarly heating it and curing it with UV light. By forming the optically anisotropic layer by multilayer application, the alignment direction of the alignment film is reflected from the bottom surface to the top surface of the optically anisotropic layer, even if the total thickness of the optically anisotropic layer is large.
[0224] First, the first layer was formed by applying the above composition E-1 onto the alignment film PG-1, heating the coating to 80°C on a hot plate, and then irradiating ultraviolet light of 365 nm wavelength at 300 mJ / cm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with an irradiation amount of 1000 ppm, thereby fixing the orientation of the liquid crystal compound and forming a liquid crystal fixing layer.
[0225] The second and subsequent layers were coated on top of the liquid crystal fixing layer, and then heated and cured with ultraviolet light under the same conditions as above to form a liquid crystal fixing layer. In this way, coating was repeated until the desired total thickness was reached, forming an optically anisotropic layer and producing a liquid crystal diffraction element.
[0226] The complex refractive index Δn of the cured layer of liquid crystal composition E-1 was determined by measuring the retardation value and film thickness of the liquid crystal fixed layer (cured layer) obtained by applying liquid crystal composition E-1 to a separately prepared support with an alignment film for retardation measurement, aligning the director of the liquid crystal compound horizontally to the substrate, and then irradiating the layer with ultraviolet light to fix the layer. Δn can be calculated by dividing the retardation value by the film thickness. The retardation value was measured at the desired wavelength using an Axoscan manufactured by Axometrix, and the film thickness was measured using a scanning electron microscope.
[0227] The optically anisotropic layer is finally formed by 550 It was confirmed by a polarizing microscope that the thickness (Re(550)) was 150 nm and that a periodic alignment surface was formed. In the liquid crystal alignment pattern of this optically anisotropic layer, one period in which the optical axis of the liquid crystal compound rotated by 180° was 0.8 μm. In addition, in this optically anisotropic layer, the twist angle of the liquid crystal compound in the thickness direction was 83°. Hereinafter, unless otherwise specified, "Δn 550 Measurements such as "×d" were carried out in the same manner.
[0228] As a liquid crystal composition for forming the second optically anisotropic layer, the following composition E-2 was prepared.
[0229] Composition E-2 ------------------------------------------------------------------- Liquid crystal compound L-1 10.00 parts by mass Liquid crystal compound L-5 90.00 parts by mass Chiral agent C1 0.03 parts by mass Polymerization initiator (Irgacure OXE01, manufactured by BASF) 1.00 part by mass Surfactant F2 0.30 parts by mass Methyl ethyl ketone 550.00 parts by mass Cyclopentanone 550.00 parts by mass
[0230] A second optically anisotropic layer was formed in the same manner as the first optically anisotropic layer, except that composition E-2 was used and the thickness of the optically anisotropic layer was adjusted.
[0231] The optically anisotropic layer is finally formed by 550 It was confirmed by a polarizing microscope that the thickness (Re(550)) of the liquid crystal layer was 335 nm and that a periodic alignment surface was formed. In the liquid crystal alignment pattern of this optically anisotropic layer, one period in which the optical axis of the liquid crystal compound rotated by 180° was 0.8 μm. In addition, in this optically anisotropic layer, the twist angle of the liquid crystal compound in the thickness direction was 8°.
[0232] As a liquid crystal composition for forming the third optically anisotropic layer, the following composition E-3 was prepared.
[0233] Composition E-3 --------------------------------------------------- Liquid crystal compound L-1 10.00 parts by mass Liquid crystal compound L-5 90.00 parts by mass Chiral agent C2 below 0.60 parts by mass Polymerization initiator (Irgacure OXE01, manufactured by BASF) 1.00 part by mass Surfactant F2 above 0.30 parts by mass Methyl ethyl ketone 550.00 parts by mass Cyclopentanone 550.00 parts by mass
[0234] A third optically anisotropic layer was formed in the same manner as the first optically anisotropic layer, except that composition E-3 was used and the thickness of the optically anisotropic layer was adjusted.
[0235] The optically anisotropic layer is finally formed by 550It was confirmed using a polarizing microscope that the thickness (Re(550)) was 170 nm and that a periodic alignment surface was formed. In the liquid crystal alignment pattern of this optically anisotropic layer, one period in which the optical axis of the liquid crystal compound rotated by 180° was 0.8 μm. In addition, in this optically anisotropic layer, the twist angle of the liquid crystal compound in the thickness direction was -78°. In this way, a first optically anisotropic member including a first liquid crystal diffraction element A1 was produced.
[0236] Chiral agent C2
[0237] <Preparation of Second Optically Anisotropic Member> (Formation of Alignment Film) An alignment film was formed in the same manner as in Comparative Example 1. The alignment film was exposed to light in the following manner.
[0238] (Exposure of Alignment Film) The alignment film was exposed using the exposure device shown in Figure 15 to form an alignment film PG-2 having an alignment pattern. In the exposure device, a laser emitting laser light with a wavelength of 355 nm was used. The exposure amount by the interference light was 1000 mJ / cm 2 It was decided.
[0239] A second optically anisotropic member including a second liquid crystal diffraction element A2 was produced in the same manner as the first liquid crystal diffraction element A1, except that the alignment film PG-2 was used, and each optically anisotropic layer was adjusted to have the following phase difference.
[0240] In the second liquid crystal diffraction element A2 thus fabricated, the Δn 550 × The thickness (Re(550)) is 150 nm, the twist angle of the liquid crystal compound in the thickness direction is 83°, and the Δn 550 × The thickness (Re(550)) is 335 nm, the twist angle of the liquid crystal compound in the thickness direction is 8°, and the Δn 550 The thickness (Re(550)) was 170 nm, and the twist angle of the liquid crystal compound in the thickness direction was -78°. In the liquid crystal alignment pattern of the optically anisotropic layer of this liquid crystal diffraction element, one period in which the optical axis of the liquid crystal compound rotates by 180° was 10.0 μm.
[0241] <Preparation of Third Optically Anisotropic Member> (Formation of Alignment Film) An alignment film was formed on a support in the same manner as in Comparative Example 1. The alignment film was exposed to light in the following manner.
[0242] (Exposure of Alignment Film) The alignment film was exposed using the exposure device shown in Figure 15 to form an alignment film PG-3 having an alignment pattern. In the exposure device, a laser emitting laser light with a wavelength of 355 nm was used. The exposure amount by the interference light was 1000 mJ / cm 2 It was decided.
[0243] A third optically anisotropic member including a third liquid crystal diffraction element A3 was produced in the same manner as the first liquid crystal diffraction element A1, except that the alignment film PG-3 was used, and each optically anisotropic layer was adjusted to have the following phase difference.
[0244] In the third liquid crystal diffraction element A3 thus fabricated, the Δn 550 × The thickness (Re(550)) is 150 nm, the twist angle of the liquid crystal compound in the thickness direction is 83°, and the Δn 550 × The thickness (Re(550)) is 335 nm, the twist angle of the liquid crystal compound in the thickness direction is 8°, and the Δn 550 The thickness (Re(550)) was 170 nm, and the twist angle of the liquid crystal compound in the thickness direction was -78°. In the liquid crystal alignment pattern of the optically anisotropic layer of this liquid crystal diffraction element, one period in which the optical axis of the liquid crystal compound rotates by 180° was 8.9 μm.
[0245] The wavelength-selective retardation plate and the liquid crystal diffraction element prepared above were laminated to form the layer structure shown in Table 12. Furthermore, during lamination, the support and the alignment film were peeled off from the optically anisotropic member, and then the layers were laminated in order. In this way, a liquid crystal diffraction element (optical element) having wavelength selectivity was prepared.
[0246]
[0247] [Example 11] <Preparation of wavelength-selective retardation plate for circularly polarized light> The λ / 4 plate prepared in Comparative Example 11 and the wavelength-selective retardation plates prepared in Examples 2 and 1 were laminated to obtain the layer configurations shown in Tables 13 and 14 below. Furthermore, during lamination, the support and the alignment film were peeled off, and then the plates were laminated sequentially. This resulted in the preparation of wavelength-selective retardation plate R2, which converts circularly polarized light of red light into circularly polarized light with an opposite rotation direction, without changing the phase of circularly polarized light in other wavelength ranges, and wavelength-selective retardation plate G2, which converts circularly polarized light of green light into the opposite circularly polarized light, without changing the phase of circularly polarized light in other wavelength ranges.
[0248]
[0249]
[0250] The wavelength-selective retardation plate prepared above and the liquid crystal diffraction element prepared in Comparative Example 11 were laminated to obtain the layer structure shown in Table 15 below. Furthermore, during lamination, the support and alignment film were peeled off from each optically anisotropic member, and then the layers were laminated in order. In this way, a liquid crystal diffraction element (optical element) having wavelength selectivity was produced.
[0251]
[0252] Comparative Example 12: <Preparation of Wavelength-Selective Retardation Plate for Circularly Polarized Light>
[0253] The λ / 4 plate prepared in Comparative Example 11 and the wavelength-selective retardation plates prepared in Comparative Examples 4 and 3 were laminated to obtain the layer configurations shown in Tables 16 and 17 below. Furthermore, during lamination, the support and the alignment film were peeled off, and then the plates were laminated sequentially. This resulted in the preparation of wavelength-selective retardation plate R3, which converts circularly polarized light of red light into circularly polarized light with the opposite rotation direction, without changing the phase of circularly polarized light in other wavelength ranges, and wavelength-selective retardation plate G3, which converts circularly polarized light of green light into the opposite circularly polarized light, without changing the phase of circularly polarized light in other wavelength ranges.
[0254]
[0255]
[0256] The wavelength-selective retardation plate prepared above and the liquid crystal diffraction element prepared in Comparative Example 11 were laminated to form the layer structure shown in Table 18 below. Furthermore, during lamination, the support and alignment film were peeled off from each optically anisotropic member, and then the layers were laminated in order. In this way, a liquid crystal diffraction element (optical element) having wavelength selectivity was produced.
[0257]
[0258] [Example 12] <Preparation of wavelength-selective retardation plate for circularly polarized light> The λ / 4 plate prepared in Comparative Example 11 and the wavelength-selective retardation plates prepared in Examples 4 and 3 were laminated to obtain the layer configurations shown in Tables 19 and 20 below. Furthermore, during lamination, the support and the alignment film were peeled off, and then the plates were laminated sequentially. This resulted in the preparation of wavelength-selective retardation plate R4, which converts circularly polarized light of red light into circularly polarized light with an opposite rotation direction, without changing the phase of circularly polarized light in other wavelength ranges, and wavelength-selective retardation plate G4, which converts circularly polarized light of green light into the opposite circularly polarized light, without changing the phase of circularly polarized light in other wavelength ranges.
[0259]
[0260]
[0261] The wavelength-selective retardation plate prepared above and the liquid crystal diffraction element prepared in Comparative Example 11 were laminated to obtain the layer structure shown in Table 21 below. Furthermore, during lamination, the support and alignment film were peeled off from each optically anisotropic member, and then the layers were laminated in order. In this way, a liquid crystal diffraction element (optical element) having wavelength selectivity was produced.
[0262]
[0263] [Evaluation of Wavelength-Selective Liquid Crystal Diffraction Element] When light was incident on the fabricated wavelength-selective liquid crystal diffractive element from the front (at an angle of 0° relative to the normal), the angle and light intensity of the transmitted diffracted light relative to the incident light were measured for red, green, and blue light. The angle of the transmitted diffracted light was the angle of the transmitted diffracted light relative to the incident light when the incident direction of the incident light was set to 0°. Specifically, laser light having output center wavelengths of red light (635 nm), green light (532 nm), and blue light (450 nm) was incident perpendicularly to the fabricated optical element from a position 10 cm away from the normal direction, and the transmitted diffracted light was captured on a screen placed 100 cm away to calculate the transmission angle. In addition, the light intensity of the transmitted diffracted light at each wavelength was measured using a photodetector. In this example, the design wavelength λa of the longest wavelength light was 635 nm, the design wavelength λb of the intermediate wavelength light was 532 nm, and the design wavelength λc of the shortest wavelength light was 450 nm. The laser light was perpendicularly incident on the circular polarizer B, the circular polarizer G, and the circular polarizer R corresponding to each wavelength, and was converted into circularly polarized light, which was then incident on the fabricated optical element and evaluated. ave and the maximum transmission angle θ of red light, green light, and blue light. max and the minimum transmission angle θ min From this, the wavelength dependency PE [%] of the diffraction angle of the transmitted diffracted light was calculated by the following formula. The smaller the PE, the lower the wavelength dependency of the diffraction angle of the transmitted diffracted light. PE [%] = [(θ max -θ min ) / θ ave ]×100 Based on the calculated PE, the wavelength dependency of the diffraction angle of the transmitted diffracted light was evaluated according to the following criteria: AA: PE is 5% or less; A: PE is more than 5% and 10% or less; B: PE is more than 10% and 20% or less; C: PE is more than 20% and 30% or less; D: PE is more than 30%
[0264] The wavelength dependence of the diffraction of transmitted diffracted light of the wavelength-selective liquid crystal diffraction elements prepared in Comparative Example 11, Comparative Example 12, Example 11, and Example 12 was evaluated as AA. On the other hand, compared to the wavelength-selective liquid crystal diffraction element of Comparative Example 11, the wavelength-selective liquid crystal diffraction element of Example 11 had a higher light intensity of transmitted diffracted light at any wavelength of 450 nm, 532 nm, and 635 nm. Furthermore, compared to the wavelength-selective liquid crystal diffraction element of Comparative Example 12, the wavelength-selective liquid crystal diffraction element of Example 12 had a higher light intensity of transmitted diffracted light at any wavelength of 450 nm, 532 nm, and 635 nm. In the above evaluation, since diffraction occurs inside the wavelength-selective liquid crystal diffraction element and the direction of light travel changes, the diffracted light is incident from an oblique direction with respect to the normal direction of the surface of the wavelength-selective retardation plate in the wavelength-selective liquid crystal diffraction element. Therefore, the fact that the light intensity of the transmitted diffracted light is large as described above indicates that even if the diffracted light is incident on the wavelength-selective retardation plate from an oblique direction, a designed phase difference is generated and the amount of diffracted light in a desired direction increases.
[0265] [Comparative Example 21]
[0266] <Preparation of First Optically Anisotropic Member> (Formation of Alignment Film) An alignment film was formed on a support in the same manner as in Comparative Example 1. The alignment film was exposed to light in the following manner.
[0267] (Exposure of Alignment Film) The alignment film was exposed using the exposure device shown in Figure 15 to form an alignment film PL-1 having a concentric alignment pattern. In the exposure device, a laser emitting laser light with a wavelength of 355 nm was used. The exposure dose by the interference light was 1000 mJ / cm. 2 It was decided.
[0268] A first optically anisotropic member including the first liquid crystal diffraction element LA1 was produced in the same manner as the first liquid crystal diffraction element A1, except that the alignment film PL-1 was used.
[0269] In the first liquid crystal diffraction element LA1 thus fabricated, the Δn 550 × The thickness (Re(550)) is 150 nm, the twist angle of the liquid crystal compound in the thickness direction is 83°, and the Δn 550× The thickness (Re(550)) is 335 nm, the twist angle of the liquid crystal compound in the thickness direction is 8°, and the Δn 550 The thickness (Re(550)) was 170 nm, and the twist angle of the liquid crystal compound in the thickness direction was -78°. In the liquid crystal orientation pattern of the optically anisotropic layer of this liquid crystal diffraction element, the period in which the optical axis of the liquid crystal compound rotated by 180° was 1.9 μm at a distance of 5 mm from the center, 1.0 μm at a distance of 10 mm from the center, and 0.8 μm at a distance of 15 mm from the center, resulting in a liquid crystal orientation pattern in which the period became shorter outward.
[0270] <Preparation of Second Optically Anisotropic Member> (Formation of Alignment Film) An alignment film was formed on a support in the same manner as in Comparative Example 1. The alignment film was exposed to light in the following manner.
[0271] (Exposure of Alignment Film) The alignment film was exposed using the exposure device shown in Figure 15 to form an alignment film PL-2 having a concentric alignment pattern. In the exposure device, a laser emitting laser light with a wavelength of 355 nm was used. The exposure dose by the interference light was 1000 mJ / cm. 2 It was decided.
[0272] A second optically anisotropic member including a second liquid crystal diffraction element LA2 was produced in the same manner as the first liquid crystal diffraction element A1, except that the alignment film PL-2 was used.
[0273] In the second liquid crystal diffraction element LA2 thus fabricated, the Δn 550 × The thickness (Re(550)) is 150 nm, the twist angle of the liquid crystal compound in the thickness direction is 83°, and the Δn 550 × The thickness (Re(550)) is 335 nm, the twist angle of the liquid crystal compound in the thickness direction is 8°, and the Δn 550The thickness (Re(550)) was 170 nm, and the twist angle of the liquid crystal compound in the thickness direction was -78°. In the liquid crystal orientation pattern of the optically anisotropic layer of this liquid crystal diffraction element, the period in which the optical axis of the liquid crystal compound rotates by 180° was 23.4 μm at a distance of 5 mm from the center, 13.0 μm at a distance of 10 mm from the center, and 10.0 μm at a distance of 15 mm from the center, resulting in a liquid crystal orientation pattern in which the period became shorter outward.
[0274] <Preparation of third optically anisotropic member> (Formation of alignment film) An alignment film was formed in the same manner as in Comparative Example 1. The alignment film was formed on a support. The alignment film was exposed to light in the following manner.
[0275] (Exposure of Alignment Film) The alignment film was exposed using the exposure device shown in Figure 15 to form an alignment film PL-3 having a concentric alignment pattern. In the exposure device, a laser emitting laser light with a wavelength of 355 nm was used. The exposure dose by the interference light was 1000 mJ / cm. 2 It was decided.
[0276] A third optically anisotropic member including a third liquid crystal diffraction element LA3 was produced in the same manner as the first liquid crystal diffraction element A1, except that an alignment film PL-3 was used.
[0277] In the third liquid crystal diffraction element LA3 thus fabricated, the Δn 550 × The thickness (Re(550)) is 150 nm, the twist angle of the liquid crystal compound in the thickness direction is 83°, and the Δn 550 × The thickness (Re(550)) is 335 nm, the twist angle of the liquid crystal compound in the thickness direction is 8°, and the Δn 550 The thickness (Re(550)) was 170 nm, and the twist angle of the liquid crystal compound in the thickness direction was -78°. In the liquid crystal orientation pattern of the optically anisotropic layer of this liquid crystal diffraction element, the period in which the optical axis of the liquid crystal compound rotates by 180° was 20.8 μm at a distance of 5 mm from the center, 11.6 μm at a distance of 10 mm from the center, and 8.9 μm at a distance of 15 mm from the center, resulting in a liquid crystal orientation pattern in which the period became shorter outward.
[0278] The wavelength-selective retardation plate prepared in Comparative Example 11 and the liquid crystal diffraction element prepared above were laminated to obtain the layer structure shown in Table 22 below. Furthermore, during lamination, the support and alignment film were peeled off from each optically anisotropic member, and then the layers were laminated in order. In this way, a liquid crystal diffraction element (optical element) having wavelength selectivity was produced.
[0279]
[0280] [Example 21] The wavelength-selective retardation plate prepared in Example 11 and the liquid crystal diffraction element prepared in Comparative Example 21 were laminated to obtain the layer structure shown in Table 23 below. Furthermore, when laminating each, the support and alignment film were peeled off from the optically anisotropic member, and then the layers were laminated in order. In this way, a liquid crystal diffraction element (optical element) having wavelength selectivity was produced.
[0281]
[0282] [Comparative Example 22] The wavelength-selective retardation plate prepared in Comparative Example 12 and the liquid crystal diffraction element prepared in Comparative Example 21 were laminated to obtain the layer structure shown in Table 24 below. Furthermore, during lamination, the support and alignment film were peeled off from the optically anisotropic member, and then the layers were laminated in order. In this way, a liquid crystal diffraction element (optical element) having wavelength selectivity was produced.
[0283]
[0284] [Example 22] The wavelength-selective retardation plate prepared in Example 12 and the liquid crystal diffraction element prepared in Comparative Example 21 were laminated to obtain the layer structure shown in Table 25 below. Furthermore, during lamination, the support and alignment film were peeled off from each optically anisotropic member, and then laminated in order. In this way, a liquid crystal diffraction element (optical element) having wavelength selectivity was produced.
[0285] [Evaluation of Wavelength-Selective Liquid Crystal Diffraction Element] When light was incident on the fabricated wavelength-selective liquid crystal diffraction element from the front (at an angle of 0° relative to the normal), the angle and light intensity of the transmitted diffracted light relative to the incident light were measured for red, green, and blue light. The angle of the transmitted diffracted light is the angle of the transmitted diffracted light relative to the incident light when the incident direction of the incident light is 0°. The angle of the transmitted diffracted light was measured in the same manner as the measurement for the wavelength-selective liquid crystal diffraction element described above, and the wavelength dependence PE [%] was calculated. In this example, the design wavelength λa of the longest wavelength light was 635 nm, the design wavelength λb of the intermediate wavelength light was 532 nm, and the design wavelength λc of the shortest wavelength light was 450 nm. The evaluation was also performed by incident laser light at distances of 5 mm, 10 mm, and 15 mm from the center of the wavelength-selective diffraction element. Based on the calculated PE, the wavelength dependence of the diffraction angle of the transmitted diffracted light was evaluated according to the following criteria. AA: PE is 5% or less. A: PE is more than 5% and less than 10%. B: PE is more than 10% and less than 20%. C: PE is more than 20% and less than 30%. D: PE is more than 30%.
[0286] The wavelength dependency of the diffraction of the transmitted diffracted light of the wavelength-selective liquid crystal diffraction elements prepared in Comparative Example 21, Comparative Example 22, Example 21, and Example 22 was evaluated as AA. On the other hand, compared to the wavelength-selective liquid crystal diffraction element of Comparative Example 21, the wavelength-selective liquid crystal diffraction element of Example 21, particularly at positions 10 mm and 15 mm away from the center of the liquid crystal diffraction element, obtained a high light intensity of the transmitted diffracted light at any wavelength of 450 nm, 532 nm, and 635 nm. Furthermore, compared to the wavelength-selective liquid crystal diffraction element of Comparative Example 22, the wavelength-selective liquid crystal diffraction element of Example 22, particularly at positions 10 mm and 15 mm away from the center of the liquid crystal diffraction element, obtained a high light intensity of the transmitted diffracted light at any wavelength of 450 nm, 532 nm, and 635 nm. In the above evaluation, diffraction occurs inside the wavelength-selective liquid crystal diffraction element, changing the direction of light propagation, and the diffracted light is incident from an oblique direction with respect to the normal direction to the surface of the wavelength-selective retardation plate in the wavelength-selective liquid crystal diffraction element. Therefore, the fact that the light intensity of the transmitted diffracted light is high as described above indicates that even if the diffracted light is incident on the wavelength-selective retardation plate from an oblique direction, the designed phase difference is generated and the amount of diffracted light in the desired direction is increased.
[0287] REFERENCE SIGNS LIST 10 Optical element 12 First optically anisotropic member 14 Second optically anisotropic member 16 Third optically anisotropic member 18G, 18R, 100 Wavelength-selective retardation plate 20 Support 24A, 24B, 24C Alignment film 26A First optically anisotropic layer 26B Second optically anisotropic layer 26C Third optically anisotropic layer 30 Liquid crystal compound 30A Optical axis 34 Optically anisotropic layer 40 Display 42 Light guide plate 60, 80 Exposure device 62, 82 Laser 64, 84 Light source 68 Beam splitter 70A, 70B, 90A, 90B Mirror 72A, 72B, 96 λ / 4 plate 86, 94 Polarizing beam splitter 92 Lens 112 First wave plate 114 Second wave plate 116 Third wave plate D1 First in-plane slow axis direction D2 Second in-plane slow axis direction D3 Third in-plane slow axis direction B R , B 2R Right-handed circularly polarized blue light G R , G1R , G 2R , G 3R Right-handed circularly polarized green light R R , R 1R , R 3R Right-handed circularly polarized red light B 1L , B 3L Left-handed circularly polarized blue light G 1L , G 2L Left-handed circularly polarized green light R 1L , R 2L Left circularly polarized red light M Laser light MA, MB Light MP P polarized light MS S polarized light P O Linear polarized light P R Right circular polarization P L Left circularly polarized light Q1, Q2 Absolute phase E1, E2 Equiphase surface U User
Claims
1. A wavelength-selective retardation plate having a plurality of wave plates, wherein the wavelength-selective retardation plate changes the phase of polarized light in a first wavelength range and does not change the phase of polarized light in a second wavelength range different from the first wavelength range, the plurality of wave plates each have a different slow axis orientation, and the Nz factors of the plurality of wave plates are each greater than 0.3 and less than 0.
7.
2. The wavelength-selective retardation plate according to claim 1, wherein each of the plurality of wave plates includes at least an optically anisotropic layer A having an Nz factor of greater than 0.5 and an optically anisotropic layer B having an Nz factor of less than 0.5, and the angle between the in-plane slow axis of the optically anisotropic layer A and the in-plane slow axis of the optically anisotropic layer B is 45° or less.
3. The wavelength-selective retardation plate according to claim 2, wherein the optically anisotropic layer A is formed using a composition containing a rod-shaped liquid crystal compound, and the optically anisotropic layer B is formed using a composition containing a discotic liquid crystal compound.
4. The wavelength-selective retardation plate according to claim 2, wherein at least one of said optically anisotropic layer A and said optically anisotropic layer B is a layer in which the alignment direction of a twisted liquid crystal compound is fixed.
5. An optical element comprising: a plurality of optically anisotropic layers formed using a composition containing a liquid crystal compound, the layers having a liquid crystal orientation pattern in which the orientation of the optical axis derived from the liquid crystal compound changes while rotating continuously along at least one direction in a plane; and a wavelength-selective retardation plate according to any one of claims 1 to 4, disposed between at least a pair of the plurality of optically anisotropic layers; wherein the rotation directions of the orientation of the optical axis in the two adjacent optically anisotropic layers are opposite to each other; the first wavelength region includes wavelengths longer than the wavelengths in the second wavelength region; the wavelength-selective retardation plate converts circularly polarized light in the first wavelength region into circularly polarized light having an opposite rotation direction, without changing the phase of the circularly polarized light in the second wavelength region; and wherein, in the liquid crystal orientation pattern, when the length of the orientation of the optical axis rotating 180° in the one direction in which the orientation of the optical axis changes while rotating continuously is defined as one period, at least one of the optically anisotropic layers has a length of one period different from that of the other optically anisotropic layers.
Citation Information
Patent Citations
Liquid crystal display element
JP2006337676A
Liquid crystal display device
JP2007163894A
Wide-angle compensation of uniaxial retarder stacks
JP2020528159A
Optical member and image display device
WO2021106766A1