Positive electrode material, method for manufacturing positive electrode material, and secondary battery

By depositing a crystalline composite metal oxide using a deep eutectic solvent on secondary battery cathode materials, the high electrical resistance and heat-related issues are addressed, resulting in improved high-rate characteristics and cycle stability.

WO2024204204A1PCT designated stage expired Publication Date: 2024-10-03SHINSHU UNIVERSITY +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011958
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing secondary battery cathode materials with titanium or niobium oxide coatings have high electrical resistance, limiting high-rate characteristics and cycle stability due to amorphous surfaces, which hinder electron flow and increase heat-related deterioration.

Method used

A crystalline composite metal oxide, such as titanium and niobium oxide, is deposited on the surface of the cathode active material using a deep eutectic solvent, reducing electrical resistivity and enhancing crystallinity, allowing improved electron and ion mobility.

Benefits of technology

The approach results in enhanced high-rate characteristics and cycle stability by reducing electrical resistance and suppressing heat-induced deterioration, leading to increased battery capacity and prolonged cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011958_03102024_PF_FP_ABST
    Figure JP2024011958_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A positive electrode material for secondary batteries that has exceptional high rate characteristics and cycle characteristics, the positive electrode material containing a positive electrode active material 10 and a crystalline metal oxide 20 that is attached to part of the surface of the positive electrode active material 10.
Need to check novelty before this filing date? Find Prior Art

Description

Cathode material, method for producing the cathode material, and secondary battery

[0001] The present invention relates to a cathode material for a secondary battery, a method for producing the cathode material, and a secondary battery including the cathode material.

[0002] 2. Description of the Related Art Secondary batteries such as lithium ion secondary batteries are lightweight and have high energy density, and are therefore used as power sources for personal computers, mobile terminals, and the like, and for driving vehicles.

[0003] Various materials have been investigated for the cathode materials used in secondary batteries from the viewpoints of increasing capacity and functionality. For example, Patent Document 1 discloses a cathode material in which a titanium-containing oxide is attached to the surface of a lithium-containing transition metal oxide, which is a cathode active material, and then the resultant is sintered. It is described that this improves the charging characteristics of lithium-ion secondary batteries at a high depth of charge.

[0004] Patent Document 2 discloses a cathode material in which niobium oxide or titanium oxide is made to be present on the surface of a lithium nickel composite oxide, which is a cathode active material, and then the resulting material is fired, and describes that this improves the thermal stability of lithium ion secondary batteries.

[0005] JP 2009-224307 A Japanese Patent No. 3835412 A

[0006] In the positive electrode material disclosed in Patent Document 1, the surface of a lithium-containing transition metal oxide is coated with a sintered titanium-containing oxide, thereby modifying the interface between the positive electrode material and the non-aqueous electrolyte, thereby accelerating the lithium ion migration reaction and improving the charging characteristics over a wide range of charge depths.

[0007] Furthermore, in the cathode material disclosed in Patent Document 2, the material coating the surface of the lithium nickel composite oxide is niobium oxide or titanium oxide, which has a melting point equal to or higher than the firing temperature. This allows the niobium or titanium oxide obtained by firing to be stably present on the surface of the lithium nickel composite oxide, thereby obtaining a cathode material with high thermal stability.

[0008] However, in the cathode materials disclosed in Patent Documents 1 and 2, the titanium-containing oxide or titanium or niobium oxide coating the surface of the cathode active material is formed by sintering or firing, making it amorphous and resulting in high electrical resistance. Therefore, even if the surface of the cathode active material is coated with a titanium-containing oxide or titanium or niobium oxide, the electrical resistance at the surface of the cathode active material cannot be reduced. Therefore, a large amount of electrons cannot flow during charge and discharge, making it difficult to improve high-rate performance. For the same reason, it is also difficult to suppress deterioration of the cathode active material due to heat generation during charge and discharge, making it difficult to improve cycle performance.

[0009] The present invention has been made in view of the above points, and a main object of the present invention is to provide a positive electrode material for a secondary battery having excellent high-rate characteristics and cycle characteristics, and a method for producing the same.

[0010] The cathode material according to the present invention is a cathode material for a secondary battery, and includes a cathode active material and a crystalline metal oxide attached to a portion of the surface of the cathode active material.

[0011] In a preferred embodiment, the metal oxide is a composite oxide containing multiple types of metals.

[0012] In a preferred embodiment, the metal oxide is a composite oxide containing titanium and a transition metal other than titanium.

[0013] In a preferred embodiment, the transition metal other than titanium is any one of niobium, tantalum, zirconia, molybdenum, and tungsten.

[0014] In a preferred embodiment, the metal oxide is a composite oxide of titanium and niobium.

[0015] The method for producing a cathode material according to the present invention is a method for producing a cathode material for a secondary battery, and includes the steps of kneading a powder of a cathode active material and a powder of a metal oxide in a deep eutectic solvent to obtain a kneaded mixture, and heating the kneaded mixture to precipitate a crystalline metal oxide on a portion of the surface of the cathode active material.

[0016] In a preferred embodiment, the metal oxide powder contains powders of multiple types of metal oxides, and the metal oxide precipitated on part of the surface of the positive electrode active material is a composite oxide of each metal in the multiple types of metal oxides.

[0017] In a preferred embodiment, the metal oxide powder contains a titanium oxide powder and a powder of an oxide of a transition metal other than titanium, and the metal oxide precipitated on a portion of the surface of the positive electrode active material is a composite oxide containing titanium and the transition metal other than titanium.

[0018] In a preferred embodiment, the oxide of a transition metal other than titanium is any one of niobium oxide, tantalum oxide, zirconia oxide, molybdenum oxide, and tungsten oxide.

[0019] According to the present invention, it is possible to provide a positive electrode material for a secondary battery having excellent high-rate characteristics and cycle characteristics, and a method for producing the same.

[0020] 2A is a photograph taken with a scanning electron microscope of the surface of a positive electrode active material after heating a kneaded mixture obtained by kneading a positive electrode active material, titanium oxide, and niobium oxide in a deep eutectic solvent. FIG. 2B is a photograph taken with a TEM of a precipitate attached to the surface of a positive electrode active material. FIG. 2C is a photograph showing an enlarged view of the area indicated by arrow A in FIG. 2A. FIG. 2D is a graph showing the battery capacity of a lithium ion secondary battery in an example. FIG. 2E is a graph showing the cycle characteristics of a lithium ion secondary battery in an example. FIG. 2F is a graph showing the battery capacity of a lithium ion secondary battery produced by changing the ratio of titanium oxide and niobium oxide to the positive electrode active material.

[0021] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the present invention is not limited to the following embodiments.

[0022] The cathode material in this embodiment is a cathode material for a secondary battery, and includes a cathode active material and a crystalline metal oxide attached to a portion of the surface of the cathode active material. Typically, a cathode for a secondary battery is manufactured by mixing this cathode material, a conductive material such as carbon, and a binder such as PVDF (polyvinylidene fluoride) in an organic solvent to form a slurry cathode mixture, and then applying this cathode mixture to a cathode current collector such as aluminum foil.

[0023] The secondary battery includes a lithium ion secondary battery, a lithium sulfur secondary battery, etc. For example, the positive electrode active material of a lithium ion secondary battery is LiCoO 2 , LiNiO 2 , LiNi 0.8 Co 0.2 O 2 , LiMn 2 O 4 The positive electrode active material is preferably made of two or more types of positive electrode active materials having different particle sizes. A positive electrode active material having a small particle size can be formed, for example, by using a flux method.

[0024] The metal oxide attached to the surface of the positive electrode active material is made of a material that has crystallinity and low electrical resistivity. 5 Ω cm or less is preferable. This reduces the electrical resistance on the surface of the positive electrode active material, allowing a large amount of electrons to flow during charge and discharge, resulting in improved high-rate characteristics. In addition, deterioration of the positive electrode active material due to heat generation during charge and discharge can be suppressed, thereby improving cycle characteristics.

[0025] It is preferable that the interface in contact with the metal oxide positive electrode active material be in an amorphous state. Typically, the crystal lattice of a positive electrode active material changes to an amorphous state due to oxidation-reduction reactions accompanying charge and discharge, or contraction due to reaction heat. Therefore, if the interface in contact with the metal oxide positive electrode active material is in a crystalline state, lattice mismatch occurs, resulting in poor ion and electron mobility. Therefore, by making the interface in contact with the metal oxide positive electrode active material amorphous, the mobility of ions and electrons can be improved. This can further improve high-rate performance.

[0026] The metal oxide is deposited in a crystalline state on the surface of the positive electrode active material using a deep eutectic solvent, which will be described later, resulting in a metal oxide with low electrical resistivity being attached to the surface of the positive electrode active material.

[0027] As shown in Fig. 1, the metal oxide 20 is attached to a portion of the surface of the positive electrode active material 10. Here, Fig. 1 is a photograph of the surface of the positive electrode active material 10 taken with a scanning electron microscope. Note that if the proportion of the metal oxide 20 attached to the surface of the positive electrode active material 10 is too high, this is undesirable because it may hinder the migration of lithium ions from the positive electrode active material 10 and result in a decrease in capacity. Here, "attached" refers to a state in which the positive electrode active material and the metal oxide are in stable contact, and includes cases in which they are chemically bonded and physically in close contact.

[0028] The metal oxide may be a composite oxide containing multiple metals. The metal oxide may be, for example, a composite oxide containing titanium and a transition metal other than titanium. Such a composite oxide is precipitated on the surface of the positive electrode active material in a crystalline state using a deep eutectic solvent. Examples of transition metals other than titanium include niobium, tantalum, zirconia, molybdenum, and tungsten.

[0029] Next, a method for producing a cathode material for a secondary battery in this embodiment will be described.

[0030] The method for producing a cathode material in this embodiment includes the steps of kneading a powder of a cathode active material and a powder of a metal oxide in a deep eutectic solvent to obtain a kneaded mixture, and heating the obtained kneaded mixture to precipitate a crystalline metal oxide on a portion of the surface of the cathode active material. Hereinafter, an example of the metal oxide adhered to the surface of the cathode active material will be described, taking a composite oxide containing titanium and a transition metal other than titanium as an example.

[0031] First, a powder of a positive electrode active material, a powder of titanium oxide, and a powder of an oxide of a transition metal other than titanium, such as niobium oxide, tantalum oxide, zirconia oxide, molybdenum oxide, or tungsten oxide, are kneaded in a deep eutectic solvent to obtain a kneaded mixture.

[0032] Here, a "deep eutectic solvent" refers to a compound formed by a mixture of a hydrogen bond donor compound and a hydrogen bond acceptor compound, whose melting point is significantly lowered by the eutectic and which becomes liquid at around room temperature. Examples of hydrogen bond donor compounds that can be used include urea, acetamide, and ethylene glycol. Examples of hydrogen bond acceptor compounds that can be used include choline chloride and N-ethyl-2-hydroxy-N.

[0033] Next, the kneaded mixture obtained by the kneading is heated to precipitate a composite oxide containing titanium and a transition metal other than titanium on a part of the surface of the positive electrode active material. The kneaded mixture can be heated, for example, by placing the deep eutectic solvent kneaded with the positive electrode active material powder or the like in a tubular furnace and flowing nitrogen through the tubular furnace.

[0034] The kneaded mixture is preferably heated to a temperature equal to or higher than the temperature at which the deep eutectic solvent thermally decomposes. This causes the deep eutectic solvent to evaporate, and a composite oxide of titanium oxide and a transition metal other than titanium is precipitated in a crystalline state on the surface of the positive electrode active material. As a result, a positive electrode material is obtained in which a crystalline metal oxide is attached to a portion of the surface of the positive electrode active material.

[0035] Furthermore, since the deep eutectic solvent is still at a high temperature after the composite oxide of titanium oxide and a transition metal other than titanium is precipitated on the surface of the positive electrode active material, the precipitated composite oxide chemically reacts with the positive electrode active material, and the interface of the composite oxide in contact with the positive electrode active material becomes amorphous.

[0036] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0037] <Production of Cathode Material> 1.0 g of a powder of a cathode active material (lithium iron phosphate (LFP)), 0.004 g of a powder of titanium oxide, and 0.001 g of a powder of niobium oxide were kneaded in 0.01 g of a deep eutectic solvent (a mixture of choline chloride and urea) for 30 minutes.

[0038] Next, the kneaded mixture was placed in a tubular furnace and heated at 800°C for 3 hours while flowing nitrogen at a flow rate of 0.5 L / min. The thermal decomposition temperature of the deep eutectic solvent is approximately 400°C, but the heating temperature was set higher at 800°C in order to quickly evaporate the deep eutectic solvent and reduce the residue of the deep eutectic solvent.

[0039] <Observation of Precipitates on the Surface of the Positive Electrode Active Material> Figure 1 is a photograph taken with an SEM (scanning electron microscope) of the surface of the positive electrode active material after heating the kneaded material. As shown in Figure 1, a precipitate 20 was observed adhering to the surface of the positive electrode active material 10. Elemental analysis using SEM-EDX (scanning electron microscope-energy dispersive X-ray spectroscopy) confirmed that this precipitate 20 is a substance containing titanium and niobium, and it is presumed to be a composite oxide of titanium and niobium. It can be seen that this precipitate 20 is adhering to the surface of the positive electrode active material 10 in surface contact.

[0040] Fig. 2A is a photograph taken with a TEM (transmission electron microscope) of a precipitate (a composite oxide of titanium and niobium) 20 attached to the surface of positive electrode active material 10, and Fig. 2B is a photograph showing an enlargement of the area indicated by arrow A in Fig. 2A. As shown in Fig. 2B, it was confirmed that precipitate 20 attached to the surface of positive electrode active material 10 has regularly aligned crystals and is crystalline.

[0041] <Preparation of Lithium Ion Secondary Battery> The cathode material prepared by the above method, a conductive material (acetylene black), and a binder (PVDF) were mixed in a weight ratio of 90:5:5 in an organic solvent (N-methyl-pyrrolidone (NMP)) to prepare a slurry cathode mixture.

[0042] This positive electrode mixture was applied to an aluminum foil, dried at 120° C., and then pressed together with the aluminum foil to prepare a positive electrode plate.

[0043] The negative electrode plate was made of lithium metal foil.

[0044] A positive electrode plate and a negative electrode plate were wound with a separator interposed therebetween to prepare an electrode body, and this electrode body was housed in a battery case together with a non-aqueous electrolyte solution to prepare a lithium ion secondary battery (hereinafter referred to as the "lithium ion secondary battery of the example").

[0045] For comparison, a lithium ion secondary battery (hereinafter referred to as the comparative lithium ion secondary battery) was fabricated in the same manner as above using a positive electrode active material that had not been treated to have a metal oxide (a composite oxide of titanium and niobium) adhered to its surface.

[0046] <Measurement of Battery Capacity> The fabricated lithium ion secondary battery was subjected to three charge / discharge cycles at a charge / discharge rate of 0.05 C to 5 C, and the battery capacity [mAh / g] was measured.

[0047] FIG. 3 is a graph showing the measurement results of battery capacity, where the graph indicated by circles shows the battery capacity of the lithium ion secondary battery of the example, and the graph indicated by squares shows the battery capacity of the lithium ion secondary battery of the comparative example.

[0048] As shown in Figure 3, the battery capacity of the lithium-ion secondary battery of the Example is larger than that of the lithium-ion secondary battery of the Comparative Example. In particular, the difference in battery capacity becomes more significant as the current during charging and discharging increases, indicating improved high-rate characteristics. This is thought to be because the metal oxide (composite oxide of titanium and niobium) attached to the surface of the positive electrode active material has a low electrical resistivity, which reduces the electrical resistance on the surface of the positive electrode active material, allowing a large amount of electrons to flow during charging and discharging.

[0049] <Measurement of Cycle Characteristics> The produced lithium ion secondary battery was repeatedly charged and discharged at a charge and discharge rate of 1 C to measure the change in discharge capacity [mAh / g], thereby measuring the cycle characteristics.

[0050] FIG. 4 is a graph showing the measurement results of the cycle characteristics, in which the graph indicated by arrow A shows the cycle characteristics of the lithium ion secondary battery of the example, and the graph indicated by arrow B shows the cycle characteristics of the lithium ion secondary battery of the comparative example.

[0051] 4, the cycle characteristics of the lithium-ion secondary battery of the Example are improved by more than twice the number of cycles at which the discharge capacity starts to decrease compared to the cycle characteristics of the lithium-ion secondary battery of the Comparative Example. This is thought to be because the metal oxide (composite oxide of titanium and niobium) attached to the surface of the positive electrode active material has low electrical resistivity, which reduces the electrical resistance on the surface of the positive electrode active material, thereby making it possible to suppress deterioration of the positive electrode active material due to heat generation during charge and discharge.

[0052] <Ratio of Metal Oxide (Titanium and Niobium Composite Oxide) to Positive Electrode Active Material> Positive electrode materials were prepared by changing the ratio of titanium oxide and niobium oxide to the positive electrode active material as shown in Table 1 below, and lithium ion secondary batteries were prepared by the same method as above.

[0053]

[0054] 5 is a graph showing the results of measuring the battery capacity of lithium-ion secondary batteries fabricated with different ratios (wt%) of titanium oxide and niobium oxide to the positive electrode active material. The horizontal axis shows the ratio of the total mass of titanium oxide and niobium oxide to the mass of the positive electrode active material. The graph indicated by arrows A, B, C, D, and E shows the change in battery capacity when the charge / discharge rates are 0.05 C, 0.5 C, 1.0 C, 2.0 C, and 5.0 C, respectively.

[0055] 5, when the total mass of titanium oxide and niobium oxide is in the range of 0.2 to 0.7 wt % relative to the mass of the positive electrode active material, the battery capacity of the lithium-ion secondary battery is increased relative to the battery capacity of the comparative lithium-ion secondary battery at all charge / discharge rates. In particular, when the charge / discharge rate is 5.0 C, the increase in battery capacity is significant, and it is clear that the high-rate characteristics are improved.

[0056] Note that when the ratio of the total mass of titanium oxide and niobium oxide to the total mass of the positive electrode active material was less than 0.2 wt%, no increase in battery capacity was observed. This is thought to be because the amount of metal oxide (titanium and niobium composite oxide) attached to the surface of the positive electrode active material was small, and therefore did not reduce the electrical resistance on the surface of the positive electrode active material. Furthermore, when the ratio of the total mass of titanium oxide and niobium oxide to the mass of the positive electrode active material exceeded 0.7 wt%, the battery capacity was found to be lower than that of the comparative lithium-ion secondary battery. This is thought to be because when the ratio of metal oxide (titanium and niobium composite oxide) attached to the surface of the positive electrode active material was too high, the migration of lithium ions from the positive electrode active material was hindered, resulting in a decrease in battery capacity.

[0057] Although the present invention has been described above with reference to preferred embodiments, these descriptions are not limiting and various modifications are possible. For example, when a crystalline titanium and niobium composite oxide is deposited on the surface of a positive electrode active material using a deep eutectic solvent, the ratio (mass ratio) of titanium oxide to niobium oxide can be changed to deposit the crystalline titanium and niobium composite oxide. In this case, the electrical resistivity of the deposited titanium and niobium composite oxide is 10 5 The ratio (mass ratio) of titanium oxide to niobium oxide may be set so that the resistivity is Ω·cm or less.

[0058] The metal oxide powder kneaded with the positive electrode active material powder in the deep eutectic solvent may contain powders of multiple metal oxides. In this case, the metal oxide precipitated on a portion of the surface of the positive electrode active material is a composite oxide of each metal in the multiple metal oxides.

[0059] Furthermore, the positive electrode mixture containing the positive electrode material of this embodiment can be used in a secondary battery including a positive electrode plate in which a positive electrode mixture is formed on a positive electrode current collector.

[0060] Furthermore, the metal oxide does not necessarily have to have a crystalline structure.

[0061] 10 Positive electrode active material 20 Precipitate (metal oxide)

Claims

1. A positive electrode material for a secondary battery, comprising: a positive electrode active material; and a crystalline metal oxide attached to a portion of a surface of the positive electrode active material.

2. The positive electrode material according to claim 1, wherein the metal oxide is a composite oxide containing multiple types of metals.

3. The positive electrode material according to claim 2, wherein the metal oxide is a composite oxide containing titanium and a transition metal other than titanium.

4. The positive electrode material according to claim 3, wherein the transition metal other than titanium is any one of niobium, tantalum, zirconia, molybdenum, and tungsten.

5. The positive electrode material according to claim 3, wherein the metal oxide is a composite oxide of titanium and niobium.

6. The positive electrode material according to claim 1, wherein the positive electrode active material is made of two or more types of positive electrode active material having different particle sizes.

7. The positive electrode material according to claim 1, wherein the interface of said metal oxide with said positive electrode active material is in an amorphous state.

8. A method for producing a positive electrode material for a secondary battery, comprising: kneading a powder of a positive electrode active material and a powder of a metal oxide in a deep eutectic solvent to obtain a kneaded mixture; and heating the kneaded mixture to precipitate a crystalline metal oxide on a portion of a surface of the positive electrode active material.

9. The method for producing a positive electrode material according to claim 8, wherein the metal oxide powder contains powders of multiple types of metal oxides, and the metal oxide precipitated on a portion of the surface of the positive electrode active material is a composite oxide of each metal in the multiple types of metal oxides.

10. The method for producing a positive electrode material according to claim 8, wherein the metal oxide powder comprises a powder of titanium oxide and a powder of an oxide of a transition metal other than titanium, and the metal oxide precipitated on a portion of the surface of the positive electrode active material is a composite oxide containing titanium and a transition metal other than titanium.

11. The method for producing a positive electrode material according to claim 10, wherein the oxide of a transition metal other than titanium is any one of niobium oxide, tantalum oxide, zirconia oxide, molybdenum oxide, and tungsten oxide.

12. The method for producing a positive electrode material according to claim 11, wherein the oxide of a transition metal other than titanium is niobium oxide, and the total mass of the titanium oxide powder and the niobium oxide powder is in the range of 0.2 to 0.7 wt % relative to the mass of the positive electrode active material powder.

13. The method for producing a positive electrode material according to claim 12, wherein the crystalline composite oxide precipitated on a portion of the surface of the positive electrode active material is a composite oxide of titanium and niobium.

14. A secondary battery comprising a positive electrode plate in which a positive electrode mixture is formed on a positive electrode current collector, the positive electrode mixture comprising the positive electrode material according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Lithium composite oxide, positive electrode active material for lithium secondary battery and lithium secondary battery comprising the same

    JP2020029396A

  • Metal air battery

    JP2021111574A

  • Electrode body for all-solid-state batteries, and method for producing same

    WO2019103008A1