Resist underlayer film forming composition
The resist underlayer film forming composition, utilizing a glycoluril compound and aromatic compounds, addresses the bending issue in semiconductor manufacturing by achieving high film density and hardness, thereby improving stress resistance and lithography performance.
Patent Information
- Application Number
- PCT/JP2024/012012
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-03
AI Technical Summary
Semiconductor manufacturing processes face challenges with resist underlayer films that bend after etching spin-on carbon (SOC) processing, requiring materials with high hardness and density to prevent bending and improve stress resistance during etching.
A resist underlayer film forming composition is developed using a polymer synthesized from a glycoluril compound and an aromatic compound with phenolic hydroxyl groups, combined with a solvent, and optionally including crosslinking agents, acid generators, and surfactants, to achieve high film density and hardness through π-π stacking and hydrogen bonding.
The composition forms a resist underlayer film with high hardness and density, enhancing stress resistance during etching and improving lithography performance by preventing film bending and promoting excellent photoresist patterns with higher dry etching speed.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Resist underlayer film-forming composition
[0001] The present invention relates to a resist underlayer film-forming composition suitable for lithography in semiconductor substrate processing, a resist underlayer film obtained from the resist underlayer film-forming composition, a method for forming a resist pattern using the resist underlayer film-forming composition, and a method for manufacturing a semiconductor device using the composition.
[0002] In recent years, semiconductor manufacturing processes have progressed rapidly, and in hybrid processes, materials are bending after etching spin-on carbon (SOC). Therefore, there is a demand for materials that do not bend even when SOC is etched. Accordingly, there is also a strong demand for resist underlayer films with high hardness. The present invention has advanced the development of film materials with high film hardness.
[0003] Improving film density also improves film hardness. Higher film density and film hardness improve stress resistance during etching, resulting in a film material that is less likely to bend. The inventors of the present application have discovered that, in order to increase film density, high film density and high hardness can be achieved by synthesizing a polymer by polymerizing monomers with rigid, linear skeletons in two dimensions (planar structure) and then stacking them in three dimensions through π-π stacking or hydrogen bonding, and by synthesizing a polymer containing hydroxyl groups with thermally crosslinkable sites.
[0004] Specifically, they found that a polymer of a glycoluril compound having a substituent and a reactive comonomer having a phenolic hydroxyl group exhibited high film density and high hardness.
[0005] It has been reported that a glycoluril compound is contained in an antireflective film-forming composition for use in the lithography process of manufacturing semiconductor devices, and that an antireflective film formed from the antireflective film-forming composition effectively absorbs reflected light from a substrate when irradiating light with wavelengths of 248 nm, 193 nm, 157 nm, etc. is used for microfabrication, does not intermix with a photoresist layer, provides an excellent photoresist pattern, and has a higher dry etching rate than a photoresist (see Patent Document 1).
[0006] It has also been reported that an antireflective film formed from a coating composition containing a polymer obtainable by reacting a glycoluril compound with at least one reactive compound containing at least one hydroxyl group and / or at least one acid group has the characteristic of suppressing reflection from the substrate even in exposure to light of a short wavelength and protecting the lithography performance of the photoresist (see Patent Document 2).
[0007] However, although Patent Documents 1 and 2 mention the formation of a high-density, high-hardness film, they do not provide any proof of this.
[0008] JP 2004-126161 A Japanese Patent No. 5613950 A
[0009] With the rapid progress of semiconductor manufacturing processes, there is a strong demand for higher quality and improved properties of resist underlayer films. Resist underlayer films are required to have high density, hardness, and resistance to bending after etching. The present invention provides a resist underlayer film-forming composition having these properties, a resist underlayer film obtained from the resist underlayer film-forming composition, a method for forming a resist pattern using the resist underlayer film-forming composition, and a method for manufacturing a semiconductor device using the composition.
[0010] The present invention solves the above-mentioned problems. Specifically, the present invention encompasses the following: A first aspect of the present invention relates to a resist underlayer film-forming composition comprising a polymer obtained by reacting a glycoluril compound with an aromatic compound having at least one phenolic hydroxyl group, and a solvent, wherein the polymer has a nitrogen content of less than 10 mass%. A second aspect of the present invention relates to the resist underlayer film-forming composition according to the first aspect, wherein the polymer has a carbon content of 80% or less. A third aspect of the present invention relates to the resist underlayer film-forming composition according to the first aspect, wherein the glycoluril compound is a glycoluril compound substituted with at least one substituent, and the substituent is at least one substituent selected from the group consisting of alkylol groups having 1 to 12 carbon atoms, alkoxyalkyl groups having 2 to 12 carbon atoms, and alkenyloxyalkyl groups having 3 to 12 carbon atoms. A fourth aspect of the present invention relates to the resist underlayer film-forming composition according to the first aspect, wherein the glycoluril compound is selected from the group consisting of tetramethylol glycoluril, tetrabutoxymethyl glycoluril, tetramethoxymethyl glycoluril, partially methylolated glycoluril, dimethoxymethyl glycoluril, monomethyl ether of dimethylol glycoluril or dimethyl ether of dimethylol glycoluril, trimethyl ether of tetramethylol glycoluril, tetramethyl ether of tetramethylol glycoluril, tetraethoxymethyl glycoluril, tetrapropoxymethyl glycoluril, tetraamyloxymethyl glycoluril, tetrahexoxymethyl glycoluril, and mixtures thereof. A fifth aspect of the present invention relates to the resist underlayer film-forming composition according to the first aspect, wherein the glycoluril compound is a glycoluril compound substituted with at least a methoxymethyl group. A sixth aspect of the present invention relates to the resist underlayer film-forming composition according to the first aspect, wherein the aromatic compound having a phenolic hydroxyl group is selected from the following compounds: A seventh aspect of the present invention relates to the resist underlayer film-forming composition according to the first aspect, wherein the solvent has a boiling point of 160°C or higher. An eighth aspect of the present invention relates to the resist underlayer film-forming composition according to the first aspect, further comprising a crosslinking agent. A ninth aspect of the present invention relates to the resist underlayer film-forming composition according to the eighth aspect, wherein the crosslinking agent is an aminoplast crosslinking agent or an aminoplast crosslinking agent and a phenoplast crosslinking agent. A tenth aspect of the present invention relates to the resist underlayer film-forming composition according to the first aspect, further comprising a surfactant. An eleventh aspect of the present invention relates to the resist underlayer film-forming composition according to the first aspect, further comprising an acid and / or a salt thereof and / or an acid generator. A twelfth aspect of the present invention relates to a resist underlayer film that is a baked product of a coating film comprising the composition according to any one of the first to eleventh aspects. A thirteenth aspect of the present invention relates to a method for forming a resist pattern used in semiconductor manufacturing, comprising the steps of applying the resist underlayer film-forming composition according to any one of the first to eleventh aspects onto a semiconductor substrate and baking the composition to form a resist underlayer film, forming a resist film on the resist underlayer film, and forming a resist pattern on the resist film by irradiating with light or an electron beam and developing. A fourteenth aspect of the present invention relates to a method for manufacturing a semiconductor device, comprising the steps of applying the resist underlayer film-forming composition according to any one of the first to eleventh aspects onto a semiconductor substrate and baking the composition to form a resist underlayer film, forming a resist film on the resist underlayer film, forming a resist pattern on the resist film, etching the resist underlayer film using the resist pattern, and processing a semiconductor substrate using the patterned resist underlayer film. A fifteenth aspect of the present invention relates to the method for manufacturing a semiconductor device according to the fourteenth aspect, wherein a resist pattern is formed on the resist film by irradiating with light or an electron beam and developing. A sixteenth aspect of the present invention relates to the method for manufacturing a semiconductor device according to the fourteenth aspect, wherein the resist pattern is formed on the resist film by a nanoimprint method or a self-assembled film.A 17th aspect of the present invention relates to a method for manufacturing a semiconductor device, comprising the steps of applying the resist underlayer film-forming composition according to any one of the first to eleventh aspects onto a semiconductor substrate and baking the composition to form a resist underlayer film, forming a hard mask on the resist underlayer film, further forming a resist film on the hard mask, forming a resist pattern on the resist film, etching the hard mask using the resist pattern, etching the resist underlayer film using the patterned hard mask, and processing a semiconductor substrate using the patterned resist underlayer film. An 18th aspect of the present invention relates to the method for manufacturing a semiconductor device according to the 17th aspect, in which the hard mask is formed by applying a composition containing an inorganic substance or by vapor deposition of a composition containing an inorganic substance. A 19th aspect of the present invention relates to the method for manufacturing a semiconductor device according to the 17th aspect, in which a resist pattern is formed on the resist film by irradiation with light or an electron beam and development. A 20th aspect of the present invention relates to the method for manufacturing a semiconductor device according to the 17th aspect, in which the resist pattern is formed on the resist film by a nanoimprint method or a self-assembled film. A 21st aspect of the present invention relates to a method for manufacturing a semiconductor device, including the steps of applying the resist underlayer film-forming composition according to any one of the first to 11th aspects onto a semiconductor substrate and baking the composition to form a resist underlayer film, forming a hard mask on the resist underlayer film, further forming a resist film on the hard mask, forming a resist pattern on the resist film, etching the hard mask using the resist pattern, etching the resist underlayer film using the patterned hard mask, removing the hard mask, and processing a semiconductor substrate using the patterned resist underlayer film. A 22nd aspect of the present invention relates to the method for manufacturing a semiconductor device according to the 21st aspect, in which the hard mask is formed by applying a composition containing an inorganic substance or by vapor deposition of a composition containing an inorganic substance. A 23rd aspect of the present invention relates to the method for manufacturing a semiconductor device according to the 21st aspect, in which a resist pattern is formed on the resist film by irradiating with light or an electron beam and developing.A 24th aspect of the present invention relates to the method for manufacturing a semiconductor device according to the 21st aspect, wherein the formation of a resist pattern on the resist film is carried out by a nanoimprint method or a self-assembled film. A 25th aspect of the present invention relates to the method for manufacturing a semiconductor device according to the 21st aspect, wherein the removal of the hard mask is carried out by etching or an alkaline chemical solution. A 26th aspect of the present invention relates to a method for manufacturing a semiconductor device, comprising the steps of: applying the resist underlayer film-forming composition according to any one of the first to 11th aspects onto a semiconductor substrate and baking the composition to form a resist underlayer film; forming a hard mask on the resist underlayer film; further forming a resist film on the hard mask; forming a resist pattern on the resist film; etching the hard mask using the resist pattern; etching the resist underlayer film using the patterned hard mask; removing the hard mask; forming a vapor-deposited film (spacer) on the resist underlayer film after hard mask removal; processing the vapor-deposited film (spacer) by etching; removing the patterned resist underlayer film to leave the patterned vapor-deposited film (spacer); and processing the semiconductor substrate using the patterned vapor-deposited film (spacer). A 27th aspect of the present invention relates to the method for manufacturing a semiconductor device according to the 26th aspect, wherein the hard mask is formed by applying a composition containing an inorganic substance or vapor-depositing a composition containing an inorganic substance. The 28th aspect of the present invention relates to the method for manufacturing a semiconductor device according to the 26th aspect, wherein a resist pattern is formed on the resist film by irradiation with light or an electron beam and development. The 29th aspect of the present invention relates to the method for manufacturing a semiconductor device according to the 26th aspect, wherein the resist pattern is formed on the resist film by a nanoimprint method or a self-assembled monolayer. The 30th aspect of the present invention relates to the method for manufacturing a semiconductor device according to the 26th aspect, wherein the hard mask is removed by either etching or an alkaline chemical solution.
[0011] The resist underlayer film-forming composition of the present invention has a small free volume in the two-dimensional direction and a coplanar structure. Furthermore, by synthesizing a polymer that is stacked in the three-dimensional direction by hydrogen bonding or the like, a resist underlayer film with high film density can be formed. Furthermore, by synthesizing a polymer containing a hydroxyl group with a thermally crosslinkable moiety, a resist underlayer film with even higher hardness can be achieved. Such resist underlayer films with high film density and high hardness can be widely applied to diverse semiconductor manufacturing processes.
[0012] The resist underlayer film-forming composition of the present invention is characterized by comprising a polymer obtained by reacting a glycoluril compound with an aromatic compound having at least one phenolic hydroxyl group, and a solvent. It may further comprise, as desired, a crosslinking agent, an acid generator, or a surfactant. Each component will be described in detail below.
[0013] <Glycoluril Compound> The glycoluril compound of the present invention is preferably a glycoluril compound substituted with at least one type of substituent. The glycoluril compound of the present invention may be a single type of glycoluril compound or may be used as a mixture.
[0014] Examples of the substituent include an alkylol group having 1 to 12 carbon atoms, an alkoxyalkyl group having 2 to 12 carbon atoms, and an alkenyloxyalkyl group having 3 to 12 carbon atoms.
[0015] Alkylol groups having 1 to 12 carbon atoms are preferred, such as methylol, butyrol, and ethylol. Alkoxyalkyl groups having 2 to 12 carbon atoms are preferred, such as methoxymethyl, ethoxymethyl, propoxymethyl, butoxymethyl, pentyloxymethyl, hexoxymethyl, methoxyethyl, ethoxyethyl, propoxyethyl, butoxyethyl, methoxypropyl, ethoxypropyl, propoxypropyl, butoxypropyl, methoxybutyl, ethoxybutyl, propoxybutyl, and butoxybutyl. Alkenyloxyalkyl groups having 3 to 12 carbon atoms are preferred, such as vinyloxymethyl, vinyloxyethyl, vinyloxypropyl, allyloxymethyl, allyloxyethyl, and allyloxypropyl.
[0016] Glycoluril compounds substituted with these substituents are preferred and are selected from the group consisting of tetramethylol glycoluril, tetrabutoxymethyl glycoluril, tetramethoxymethyl glycoluril, partially methylolated glycoluril, dimethoxymethyl glycoluril, monomethyl ether of dimethylol glycoluril or dimethyl ether of dimethylol glycoluril, trimethyl ether of tetramethylol glycoluril, tetramethyl ether of tetramethylol glycoluril, tetraethoxymethyl glycoluril, tetrapropoxymethyl glycoluril, tetraamyloxymethyl glycoluril, tetrahexoxymethyl glycoluril, and mixtures thereof.
[0017] <Aromatic Compound Having a Phenolic Hydroxyl Group> The aromatic compound having a phenolic hydroxyl group is selected from the following compounds.
[0018]
[0019] Preferably, the aromatic compound having a phenolic hydroxyl group is selected from the following compositions:
[0020] <Production of Polymer> The polymer obtained by the reaction of a glycoluril compound with an aromatic compound having a phenolic hydroxyl group can be prepared by a known method, for example, by condensing a glycoluril compound with an aromatic compound having a phenolic hydroxyl group.
[0021] The glycoluril compound and the aromatic compound having a phenolic hydroxyl group may be used alone or in combination of two or more. In this condensation reaction, the aromatic compound having a phenolic hydroxyl group can be used in a ratio of 0.1 to 10 moles, preferably 0.1 to 2 moles, per mole of the glycoluril compound. Preferably, the nitrogen content of the polymer is less than 10% by mass. More preferably, the carbon content of the polymer is 80% or less.
[0022] The condensation reaction can be carried out without a solvent, but is usually carried out using a solvent. The solvent is not particularly limited as long as it can dissolve the reaction substrates and does not inhibit the reaction. Examples of the solvent include ethers such as 1,2-dimethoxyethane, diethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, tetrahydrofuran, and dioxane. Furthermore, if the catalyst used is a liquid, such as formic acid, it can also serve as a solvent. The condensation reaction temperature is usually 40°C to 200°C, preferably 80°C to 180°C. The reaction time varies depending on the reaction temperature, but is usually 5 minutes to 50 hours, preferably 5 minutes to 24 hours.
[0023] The weight average molecular weight of the polymer according to one embodiment of the present invention is usually 500 to 100,000, preferably 600 to 50,000, 700 to 10,000, or 800 to 8,000.
[0024] The resist underlayer film-forming composition according to one embodiment of the present invention contains a solvent. The solvent is not particularly limited as long as it can dissolve the polymer obtained by the reaction of a glycoluril compound with an aromatic compound having a phenolic hydroxyl group, and other optional components that are added as needed.
[0025] Examples of the solvent include methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, methyl isobutyl carbinol, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monobutyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, and ethylene glycol. monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, propylene glycol monomethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol dipropyl ether, propylene glycol dibutyl ether, ethyl lactate, propyl lactate, isopropyl lactate, butyl lactate, isobutyl lactate, methyl formate, ethyl formate, propyl formate, isopropyl formate, butyl formate, isobutyl formate, amyl formate, isoamyl formate, methyl acetate, ethyl acetate, amyl acetate, isoamyl acetate, hexyl acetate, methyl propionate, ethyl propionate, propyl propionate,Isopropyl propionate, butyl propionate, isobutyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, isopropyl butyrate, butyl butyrate, isobutyl butyrate, ethyl hydroxyacetate, methyl 2-hydroxy-2-methylpropionate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxy-2-methylpropionate, methyl 2-hydroxy-3-methylbutyrate, ethyl methoxyacetate, ethyl ethoxyacetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-methoxybutyl Examples of suitable solvents include acetate, 3-methoxypropyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, 3-methyl-3-methoxybutyl butyrate, methyl acetoacetate, toluene, xylene, methyl ethyl ketone, methyl propyl ketone, methyl butyl ketone, 2-heptanone, 3-heptanone, 4-heptanone, N,N-dimethylformamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpyrrolidone, 4-methyl-2-pentanol, and γ-butyrolactone. These solvents can be used alone or in combination of two or more.
[0026] In addition, a solvent having a boiling point of 160° C. or higher can be included in combination with a solvent having a boiling point of less than 160° C. As such a high-boiling point solvent, for example, the following compounds described in WO 2018 / 131562 (A1) can be preferably used. [R in formula (i)] 1 , R 2 and R 3 each represents a hydrogen atom, an oxygen atom, a sulfur atom, or an alkyl group having 1 to 20 carbon atoms which may be interrupted by an amide bond, and may be the same or different from each other and may be bonded to each other to form a ring structure.
[0027] Alternatively, 1,6-diacetoxyhexane (boiling point 260 ° C.), tripropylene glycol monomethyl ether (boiling point 242 ° C.), and various other high-boiling solvents described in paragraph 0082 of JP-A-2021-84974 can be preferably used.
[0028] Alternatively, dipropylene glycol monomethyl ether acetate (boiling point 213°C), diethylene glycol monoethyl ether acetate (boiling point 217°C), diethylene glycol monobutyl ether acetate (boiling point 247°C), dipropylene glycol dimethyl ether (boiling point 171°C), dipropylene glycol monomethyl ether (boiling point 187°C), dipropylene glycol monobutyl ether (boiling point 231°C), tripropylene glycol monomethyl ether (boiling point 242°C), γ-butyrolactone (boiling point 204°C), benzyl alcohol (boiling point 205°C), propylene carbonate (boiling point 242°C), tetraethylene glycol dimethyl ether (boiling point 275°C), 1,6-diacetoxyhexane (boiling point 260°C), dipropylene glycol (boiling point 230°C), 1, 3-butylene glycol diacetate (boiling point 232° C.) and various other high boiling point solvents described in paragraphs 0023 to 0031 of the publication can be preferably used.
[0029] <Acid and / or Salt Thereof and / or Acid Generator> The resist underlayer film forming composition, which is one embodiment of the present invention, may contain an acid and / or a salt thereof and / or an acid generator.
[0030] Examples of the acid include p-toluenesulfonic acid, trifluoromethanesulfonic acid, salicylic acid, 5-sulfosalicylic acid, 4-phenolsulfonic acid, camphorsulfonic acid, 4-chlorobenzenesulfonic acid, benzenedisulfonic acid, 1-naphthalenesulfonic acid, citric acid, benzoic acid, hydroxybenzoic acid, and naphthalenecarboxylic acid.
[0031] The salt may be a salt of the above-mentioned acid, and is not limited thereto, but ammonia derivative salts such as trimethylamine salts and triethylamine salts, pyridine derivative salts, morpholine derivative salts, etc. may be suitably used.
[0032] The amount of the acid and / or salt thereof to be used is usually 0.0001 to 20% by mass, preferably 0.0005 to 10% by mass, and more preferably 0.01 to 5% by mass, based on the total solid content.
[0033] Examples of the acid generator include a thermal acid generator and a photoacid generator.
[0034] Examples of the thermal acid generator include 2,4,4,6-tetrabromocyclohexadienone, benzoin tosylate, 2-nitrobenzyl tosylate, K-PURE (registered trademark) CXC-1612, CXC-1614, TAG-2172, TAG-2179, TAG-2678, TAG2689, and TAG2700 (manufactured by King Industries), and SI-45, SI-60, SI-80, SI-100, SI-110, and SI-150 (manufactured by Sanshin Chemical Industry Co., Ltd.), and other organic sulfonic acid alkyl esters.
[0035] Photoacid generators generate acid when the resist is exposed to light. This allows the acidity of the underlayer film to be adjusted. This is one way to match the acidity of the underlayer film to that of the upper layer resist. Adjusting the acidity of the underlayer film also allows for adjustment of the pattern shape of the upper layer resist.
[0036] Examples of the photoacid generator contained in the resist underlayer film-forming composition of the present invention include onium salt compounds, sulfonimide compounds, and disulfonyldiazomethane compounds.
[0037] Examples of the onium salt compound include iodonium salt compounds such as diphenyliodonium hexafluorophosphate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium nonafluoro-normal butanesulfonate, diphenyliodonium perfluoro-normal octanesulfonate, diphenyliodonium camphorsulfonate, bis(4-tert-butylphenyl)iodonium camphorsulfonate, and bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate, as well as sulfonium salt compounds such as triphenylsulfonium hexafluoroantimonate, triphenylsulfonium nonafluoro-normal butanesulfonate, triphenylsulfonium camphorsulfonate, and triphenylsulfonium trifluoromethanesulfonate.
[0038] Examples of the sulfonimide compound include N-(trifluoromethanesulfonyloxy)succinimide, N-(nonafluoronormalbutanesulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, and N-(trifluoromethanesulfonyloxy)naphthalimide.
[0039] Examples of the disulfonyldiazomethane compound include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane, bis(2,4-dimethylbenzenesulfonyl)diazomethane, and methylsulfonyl-p-toluenesulfonyldiazomethane.
[0040] The acid generator may be used alone or in combination of two or more thereof. When an acid generator is used, the proportion thereof is 0.01 to 10 parts by mass, or 0.1 to 8 parts by mass, or 0.5 to 5 parts by mass, relative to 100 parts by mass of the solid content of the resist underlayer film-forming composition.
[0041] <Other Optional Components> The resist underlayer film-forming composition of one embodiment of the present invention may contain, in addition to the above, a crosslinking agent, a surfactant, a light absorber, a rheology modifier, an adhesion aid, a curing catalyst, and the like, as needed.
[0042] <Crosslinking Agent> Typical crosslinking agents include aminoplast crosslinking agents and phenoplast crosslinking agents. As the crosslinking agent, a crosslinking agent with high heat resistance can be used. As a crosslinking agent with high heat resistance, a compound containing a crosslink-forming substituent having an aromatic ring (e.g., a benzene ring or a naphthalene ring) in the molecule can be preferably used.
[0043] Aminoplast crosslinking agents include highly alkylated, alkoxylated, or alkoxyalkylated melamine, benzoguanamine, glycoluril, urea, and polymers thereof. Crosslinking agents having at least two crosslink-forming substituents are preferred, including compounds such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea, and methoxymethylated thiourea. Condensates of these compounds can also be used.
[0044] Preferably, it is at least one selected from the group consisting of tetramethoxymethyl glycoluril and hexamethoxymethyl melamine.
[0045] Some specific examples are as follows:
[0046] Phenoplast crosslinking agents include highly alkylated, alkoxylated, or alkoxyalkylated aromatics, their polymers, and the like. Preferred crosslinking agents have at least two crosslink-forming substituents per molecule, such as 2,6-dihydroxymethyl-4-methylphenol, 2,4-dihydroxymethyl-6-methylphenol, bis(2-hydroxy-3-hydroxymethyl-5-methylphenyl)methane, bis(4-hydroxy-3-hydroxymethyl-5-methylphenyl)methane, 2,2-bis(4-hydroxy-3,5-dihydroxymethylphenyl)propane, bis(3-formyl-4-hydroxyphenyl)methane, bis(4-hydroxy-2,5-dimethylphenyl)formylmethane, and α,α-bis(4-hydroxy-2,5-dimethylphenyl)-4-formyltoluene. Condensates of these compounds can also be used.
[0047] In addition to the above, other examples of such compounds include compounds having a partial structure of the following formula (4) and polymers or oligomers having a repeating unit of the following formula (5).
[0048] The above R 11 , R 12 , R 13 , and R 14 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and the above-mentioned examples of these alkyl groups can be used. n1 is an integer of 1 to 4, n2 is an integer of 1 to (5-n1), and (n1+n2) is an integer of 2 to 5. n3 is an integer of 1 to 4, n4 is an integer of 0 to (4-n3), and (n3+n4) is an integer of 1 to 4. Oligomers and polymers having a repeating unit structure number of 2 to 100, or 2 to 50, can be used.
[0049] Some specific examples are as follows:
[0050] The crosslinking agents, such as aminoplast crosslinking agents and phenoplast crosslinking agents, may be used alone or in combination of two or more. For example, only an aminoplast crosslinking agent may be used, or both an aminoplast crosslinking agent and a phenoplast crosslinking agent may be used. The aminoplast crosslinking agent may be produced by a method known per se or a method equivalent thereto, or a commercially available product may be used. The amount of the crosslinking agent, such as an aminoplast crosslinking agent or a phenoplast crosslinking agent, used varies depending on the coating solvent used, the base substrate used, the required solution viscosity, the required film shape, etc., but is 0.001% by mass or more, 0.01% by mass or more, 0.05% by mass or more, 0.5% by mass or more, or 1.0% by mass or more, and 80% by mass or less, 50% by mass or less, 40% by mass or less, 20% by mass or less, or 10% by mass or less, based on the total solids content of the resist underlayer film-forming composition of the present invention.
[0051] <Surfactant> The resist underlayer film forming composition according to the present invention can contain a surfactant in order to prevent pinholes, striations, and the like from occurring and to further improve coatability against surface irregularities.
[0052] Examples of surfactants include nonionic surfactants such as polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkylaryl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether; polyoxyethylene-polyoxypropylene block copolymers; sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate; and polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate. Examples of suitable surfactants include fluorosurfactants such as EFTOP EF301, EF303, and EF352 (trade names, manufactured by Tochem Products Co., Ltd.), Megafac F171, F173, R-30, and R-40 (trade names, manufactured by Dainippon Ink Co., Ltd.), Fluorad FC430 and FC431 (trade names, manufactured by Sumitomo 3M Limited), and Asahiguard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (trade names, manufactured by Asahi Glass Co., Ltd.); and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.).
[0053] The amount of these surfactants to be added is usually 2.0 mass % or less, and preferably 1.0 mass % or less, based on the total solid content of the resist underlayer film-forming composition of the present invention. These surfactants may be added alone or in combination of two or more.
[0054] <Other Additives> Examples of light absorbing agents include commercially available light absorbing agents described in "Technology and Market of Industrial Dyes" (CMC Publishing) and "Dye Handbook" (edited by the Society of Organic Synthetic Chemistry), such as C.I. Disperse Yellow 1, 3, 4, 5, 7, 8, 13, 23, 31, 49, 50, 51, 54, 60, 64, 66, 68, 79, 82, 88, 90, 93, 102, 114, and 124; C.I. Disperse Orange 1, 5, 13, 25, 29, 30, 31, 44, 57, 72, and 73; C.I. C.I. Disperse Red 1, 5, 7, 13, 17, 19, 43, 50, 54, 58, 65, 72, 73, 88, 117, 137, 143, 199, and 210; C.I. Disperse Violet 43; C.I. Disperse Blue 96; C.I. Fluorescent Brightening Agent 112, 135, and 163; C.I. Solvent Orange 2 and 45; C.I. Solvent Red 1, 3, 8, 23, 24, 25, 27, and 49; C.I. Pigment Green 10; C.I. Pigment Brown 2, etc. can be suitably used. The light-absorbing agent is usually blended in an amount of 10% by mass or less, and preferably 5% by mass or less, based on the total solid content of the resist underlayer film-forming composition according to the present invention.
[0055] The rheology modifier is added primarily to improve the fluidity of the resist underlayer film-forming composition, particularly in the baking step, to improve the film thickness uniformity of the resist underlayer film and the ability of the resist underlayer film-forming composition to fill holes. Specific examples include phthalic acid derivatives such as dimethyl phthalate, diethyl phthalate, diisobutyl phthalate, dihexyl phthalate, and butyl isodecyl phthalate; adipic acid derivatives such as di-n-butyl adipate, diisobutyl adipate, diisooctyl adipate, and octyldecyl adipate; maleic acid derivatives such as di(n-butyl) maleate, diethyl maleate, and dinonyl maleate; oleic acid derivatives such as methyl oleate, butyl oleate, and tetrahydrofurfuryl oleate; and stearic acid derivatives such as n-butyl stearate and glyceryl stearate. These rheology modifiers are typically incorporated in an amount of less than 30% by mass based on the total solids content of the resist underlayer film-forming composition of the present invention.
[0056] The adhesion promoter is added mainly for the purpose of improving the adhesion between the substrate or resist and the resist underlayer film-forming composition, and particularly to prevent peeling of the resist during development. Specific examples include chlorosilanes such as trimethylchlorosilane, dimethylvinylchlorosilane, methyldiphenylchlorosilane, and chloromethyldimethylchlorosilane; alkoxysilanes such as trimethylmethoxysilane, dimethyldiethoxysilane, methyldimethoxysilane, dimethylvinylethoxysilane, diphenyldimethoxysilane, and phenyltriethoxysilane; silazanes such as hexamethyldisilazane, N,N'-bis(trimethylsilyl)urea, dimethyltrimethylsilylamine, and trimethylsilylimidazole; vinyltrichlorosilane; Examples of the adhesion aid include silanes such as silane, γ-chloropropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and γ-glycidoxypropyltrimethoxysilane; heterocyclic compounds such as benzotriazole, benzimidazole, indazole, imidazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, urazole, thiouracil, mercaptoimidazole, and mercaptopyrimidine; and ureas such as 1,1-dimethylurea and 1,3-dimethylurea, or thiourea compounds. These adhesion aids are blended in an amount of usually less than 5% by mass, and preferably less than 2% by mass, based on the total solids content of the resist underlayer film-forming composition of the present invention.
[0057] The curing catalyst is effective for curing the film. Specific examples include, but are not limited to, sulfonium salt compounds such as triphenylsulfonium nitrate, triphenylsulfonium maleate, triphenylsulfonium trifluoroacetate, triphenylsulfonium hydrochloride, and triphenylsulfonium acetate.
[0058] The resist underlayer film-forming composition according to the present invention has a solids content of 0.1 to 70% by mass, or 0.1 to 60% by mass. The solids content is the content of all components of the resist underlayer film-forming composition excluding the solvent. The solids content may contain a crosslinkable resin in an amount of 1 to 99.9% by mass, or 50 to 99.9% by mass, or 50 to 95% by mass, or 50 to 90% by mass.
[0059] <Resist Underlayer Film> The resist underlayer film can be formed, for example, as follows using the resist underlayer film-forming composition according to the present invention.
[0060] Substrates used in the manufacture of semiconductor devices (e.g., silicon wafer substrates, silicon dioxide coated substrates (SiO 2 The resist underlayer film-forming composition according to one embodiment of the present invention is applied onto a substrate (e.g., a silicon nitride substrate (SiN substrate), a silicon oxynitride substrate (SiON substrate), a titanium nitride substrate (TiN substrate), a tungsten substrate (W substrate), a glass substrate, an ITO substrate, a polyimide substrate, or a substrate coated with a low dielectric constant material (low-k material)) by a suitable application method such as a spinner or coater, and then baked using a heating means such as a hot plate to form a resist underlayer film. Baking conditions are appropriately selected from a baking temperature of 80°C to 800°C and a baking time of 0.3 to 60 minutes. Preferably, the baking temperature is 150°C to 400°C and the baking time is 0.5 to 2 minutes. Air may be used as the atmospheric gas during baking, or an inert gas such as nitrogen or argon can also be used. In one embodiment, it is particularly preferred that the oxygen concentration is 1% or less. Here, the thickness of the formed underlayer film is, for example, 10 to 1000 nm, 20 to 500 nm, 30 to 400 nm, or 50 to 300 nm. Furthermore, if a quartz substrate is used as the substrate, a replica of a quartz imprint mold (mold replica) can be produced.
[0061] Furthermore, an adhesion layer and / or a silicon-containing layer containing 99% by mass or less, or 50% by mass or less of Si can be formed by coating or vapor deposition on the resist underlayer film according to one embodiment of the present invention. For example, an adhesion layer as described in JP-A-2013-202982 or JP-A-5827180, a silicon-containing resist underlayer film (inorganic resist underlayer film)-forming composition as described in WO 2009 / 104552 (A1) can be formed by spin coating, or a Si-based inorganic material film can be formed by CVD or the like.
[0062] Furthermore, by applying the resist underlayer film-forming composition of one embodiment of the present invention to a semiconductor substrate having a portion with a step and a portion without a step (a so-called stepped substrate) and baking it, the step between the portion with a step and the portion without a step can be reduced.
[0063] <Method for Forming a Resist Pattern> A method for forming a resist pattern used in manufacturing a semiconductor device includes the steps of applying the resist underlayer film-forming composition according to the present invention onto a substrate used in manufacturing the semiconductor device and baking the composition to form a resist underlayer film, forming a resist film on the resist underlayer film, and forming a resist pattern on the resist film by irradiating the resist film with light or an electron beam and developing the resist pattern.
[0064] <Method for manufacturing a semiconductor device> (i) A method for manufacturing a semiconductor device according to one aspect of the present invention includes the steps of: applying a resist underlayer film-forming composition according to one aspect of the present invention onto a semiconductor substrate and baking the composition to form a resist underlayer film; forming a resist film on the resist underlayer film; forming a resist pattern on the resist film by irradiating with light or an electron beam and developing the resist film; etching and patterning the resist underlayer film using the resist pattern; and processing a semiconductor substrate using the patterned resist underlayer film.
[0065] (ii) A method for manufacturing a semiconductor device according to one aspect of the present invention includes the steps of: applying a resist underlayer film-forming composition according to one aspect of the present invention onto a semiconductor substrate and baking the composition to form a resist underlayer film; forming a hard mask on the resist underlayer film; further forming a resist film on the hard mask; forming a resist pattern on the resist film by irradiating with light or an electron beam and developing; etching and patterning the hard mask using the resist pattern; etching and patterning the resist underlayer film using the patterned hard mask; and processing a semiconductor substrate using the patterned resist underlayer film.
[0066] (iii) A method for manufacturing a semiconductor device according to one aspect of the present invention includes the steps of: applying a resist underlayer film-forming composition according to one aspect of the present invention onto a semiconductor substrate and baking the composition to form a resist underlayer film; forming a hard mask on the resist underlayer film; further forming a resist film on the hard mask; forming a resist pattern on the resist film by irradiating with light or an electron beam and developing; etching and patterning the hard mask using the resist pattern; etching and patterning the resist underlayer film using the patterned hard mask; removing the hard mask; and processing a semiconductor substrate using the patterned resist underlayer film.
[0067] (iv) A method for producing a semiconductor device according to one embodiment of the present invention includes the steps of: applying a resist underlayer film-forming composition according to one embodiment of the present invention onto a semiconductor substrate and baking the composition to form a resist underlayer film; forming a hard mask on the resist underlayer film; further forming a resist film on the hard mask; forming a resist pattern on the resist film by irradiating with light or an electron beam and developing; etching and patterning the hard mask using the resist pattern; etching and patterning the resist underlayer film using the etched hard mask; removing the hard mask; forming a vapor-deposited film (spacer) on the resist underlayer film after hard mask removal; processing the vapor-deposited film (spacer) by etching; removing the patterned resist underlayer film to leave the patterned vapor-deposited film (spacer); and processing a semiconductor substrate using the patterned vapor-deposited film (spacer). A semiconductor substrate can be processed using the production methods (i) to (iv) above.
[0068] The step of forming a resist underlayer film using the resist underlayer film forming composition of one embodiment of the present invention is as described above in the <Resist underlayer film> section.
[0069] A hard mask such as a silicon-containing film may be formed as a second resist underlayer film on the resist underlayer film formed in the above steps, and a resist pattern may be formed thereon [(ii) to (iv) above].
[0070] The hard mask may be a coating film of a composition containing an inorganic substance, or a vapor-deposited film of an inorganic substance formed by a vapor deposition method such as CVD or PVD, and may be a SiON film, a SiN film, or a SiO 2 An example is a membrane.
[0071] Furthermore, an anti-reflective coating (BARC) may be formed on this hard mask, or a resist shape correction film without anti-reflective properties may be formed.
[0072] In the step of forming the resist pattern, exposure is performed through a mask (reticle) for forming a predetermined pattern or by direct writing. Examples of exposure sources that can be used include g-line, i-line, KrF excimer laser, ArF excimer laser, EUV, and electron beam. After exposure, post-exposure baking is performed as needed. The resist is then developed with a developer (e.g., a 2.38% by mass aqueous solution of tetramethylammonium hydroxide), and then rinsed with a rinse solution or pure water to remove the used developer. Post-baking is then performed to dry the resist pattern and enhance adhesion to the underlayer.
[0073] The etching step performed after the formation of the resist pattern is performed by dry etching.
[0074] The resist film may be patterned by a nanoimprinting method or a self-assembled film method. In the nanoimprinting method, a resist composition is molded using a patterned mold that is transparent to irradiated light. In the self-assembled film method, a pattern is formed using a self-assembled film that naturally forms a regular structure on the nanometer order, such as a diblock polymer (e.g., polystyrene-polymethyl methacrylate).
[0075] In the nanoimprint method, before applying the curable composition that will form the resist film, a silicon-containing layer (hard mask layer) may be optionally formed on the resist underlayer film by coating or vapor deposition, and further an adhesion layer may be formed on the resist underlayer film or the silicon-containing layer (hard mask layer) by coating or vapor deposition, and the curable composition that will form the resist film may be applied on the adhesion layer.
[0076] The following gases are used for processing the hard mask (silicon-containing layer), resist underlayer film, and substrate: CF 4 , CHF 3 , C.H. 2 F 2 , C.H. 3 F, C 4 F 6 , C 4 F 8 , O 2 , N2 O, NO 2 , He, H 2 These gases may be used alone or in combination of two or more. Furthermore, these gases may be mixed with argon, nitrogen, carbon dioxide, carbonyl sulfide, sulfur dioxide, neon, or nitrogen trifluoride.
[0077] In addition, wet etching may be performed to simplify the process and reduce damage to the processed substrate. This leads to suppression of fluctuations in processing dimensions and reduction of pattern roughness, making it possible to process the substrate with high yield. Therefore, in steps (iii) to (iv), the hard mask can be removed using either etching or an alkaline chemical solution. In particular, when an alkaline chemical solution is used, there are no restrictions on the components, but it is preferable that the alkaline component contains the following:
[0078] Examples of the alkaline component include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, methyltripropylammonium hydroxide, methyltributylammonium hydroxide, ethyltrimethylammonium hydroxide, dimethyldiethylammonium hydroxide, benzyltrimethylammonium hydroxide, hexadecyltrimethylammonium hydroxide, and (2-hydroxyethyl)trimethylammonium hydroxide, monoethanolamine, diethanolamine, triethanolamine, 2-(2-aminoethoxy)ethanol, N,N-dimethylethanolamine, N,N-diethylethanolamine, N , N-dibutylethanolamine, N-methylethanolamine, N-ethylethanolamine, N-butylethanolamine, N-methyldiethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, tetrahydrofurfurylamine, N-(2-aminoethyl)piperazine, 1,8-diazabicyclo[5.4.0]undecene-7, 1,4-diazabicyclo[2.2.2]octane, hydroxyethylpiperazine, piperazine, 2-methylpiperazine, trans-2,5-dimethylpiperazine, cis-2,6-dimethylpiperazine, 2-piperidinemethanol, cyclohexylamine, 1,5-diazabicyclo[4.3.0]nonene-5, etc. Furthermore, particularly from the viewpoint of handling, tetramethylammonium hydroxide and tetraethylammonium hydroxide are particularly preferred, and an inorganic base may be used in combination with the quaternary ammonium hydroxide. As the inorganic base, alkali metal hydroxides such as potassium hydroxide, sodium hydroxide, rubidium hydroxide, etc. are preferred, with potassium hydroxide being more preferred.
[0079] The present invention will be explained in more detail below with reference to Synthesis Examples, Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0080] [Synthesis of Polymer] The weight-average molecular weights shown in the synthesis examples below in this specification are the results of measurement by gel permeation chromatography (hereinafter abbreviated as GPC in this specification). A GPC device (HLC-8320GPC) manufactured by Tosoh Corporation was used for the measurement, and the measurement conditions etc. are as follows. GPC column: TSKgel Super H-RC, TSKgel Super Multipore HZ-N, TSKgel Super Multipore HZ-N (manufactured by Tosoh Corporation) Column temperature: 40°C Solvent: tetrahydrofuran (Kanto Chemical, for high performance liquid chromatography) Standard sample: polystyrene (manufactured by Shodex)
[0081] Synthesis Example 1 Synthesis of Polymer (1) (PL-LI / PGA = 100 / 100) A 200 mL three-neck flask equipped with a stirrer and a condenser was charged with 15.00 g (47.12 mmol) of tetramethoxymethyl glycoluril (POWDERLINK 1174, manufactured by Mitsui Cytec Co., Ltd.), 5.94 g (47.12 mmol) of phloroglucinol (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.02 g (0.24 mmol) of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 83.75 g of propylene glycol monomethyl ether. The temperature was raised to 50°C and the mixture was stirred at 50°C for 9 hours. After the reaction was stopped, the mixture was added dropwise to 732 g of water to precipitate a polymer. The resulting precipitate was filtered, washed with 183 mL of water three times, and vacuum dried to obtain a polymer. The molecular weight of this polymer was measured by GPC (standard polystyrene equivalent) and found to have a weight average molecular weight (Mw) of 1,413, with a yield of 58.4%. This polymer has a repeating unit structure represented by the following formula (1). The obtained polymer was diluted with propylene glycol monomethyl ether to a solids concentration of 30%, and cation exchange resin and anion exchange resin in amounts equal to the solids amount were added, followed by stirring for 4 hours. The ion exchange resin was filtered to obtain a polymer solution.
[0082] Synthesis Example 2 Synthesis of Polymer (2) (PL-LI / THPE = 100 / 100) A 100 mL three-neck flask equipped with a stirrer and a condenser was charged with 5.00 g (15.71 mmol) of tetramethoxymethyl glycoluril (POWDERLINK 1174, manufactured by Mitsui Cytec Co., Ltd.), 4.81 g (15.71 mmol) of 1,1,1-tris(4-hydroxyphenyl)ethane (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.0075 g (0.08 mmol) of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 39.24 g of propylene glycol monomethyl ether, and the mixture was heated to 50° C. and stirred at 50° C. for 6 hours. After quenching the reaction, the mixture was added dropwise to 392 g of a mixed solvent of methanol (Kanto Chemical, special grade) and water (5 / 5) to precipitate the polymer. The resulting precipitate was filtered off, and the filter cake was washed three times with 98 mL of a methanol / water (5 / 5) mixed solvent and vacuum dried to obtain a polymer. The molecular weight of this polymer was measured by GPC (standard polystyrene equivalent), and the weight average molecular weight (Mw) was 850, with a yield of 50.9%. This polymer has a repeating unit structure represented by the following formula (2). The resulting polymer was diluted with propylene glycol monomethyl ether to a solids concentration of 30%, and cation exchange resin and anion exchange resin in amounts equal to the solids amount were added, followed by stirring for 4 hours. The ion exchange resin was filtered to obtain a polymer solution.
[0083] Synthesis Example 3 Synthesis of Polymer (3) (PL-LI / BHPF = 100 / 100) A 100 mL three-neck flask equipped with a stirrer and a condenser was charged with 5.00 g (15.71 mmol) of tetramethoxymethyl glycoluril (POWDERLINK 1174, manufactured by Mitsui Cytec Co., Ltd.), 5.50 g (15.71 mmol) of 9,9-bis(4-hydroxyphenyl)fluorene (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.0075 g (0.08 mmol) of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 42.01 g of propylene glycol monomethyl ether, and the mixture was heated to 50° C. and stirred at 50° C. for 6 hours. After quenching the reaction, the mixture was added dropwise to 410 g of a mixed solvent of methanol (Kanto Chemical, special grade) and water (5 / 5) to precipitate the polymer. The resulting precipitate was filtered off, and the filter cake was washed three times with 105 mL of a methanol / water (5 / 5) mixed solvent, followed by vacuum drying to obtain a polymer. The molecular weight of this polymer was measured by GPC (standard polystyrene equivalent), revealing a weight average molecular weight (Mw) of 2125 and a yield of 64.4%. This polymer has a repeating unit structure represented by the following formula (3). The resulting polymer was diluted with propylene glycol monomethyl ether to a solids concentration of 30%, and cation exchange resin and anion exchange resin in amounts equal to the solids amount were added, followed by stirring for 4 hours. The ion exchange resin was filtered off to obtain a polymer solution.
[0084] Comparative Synthesis Example 1 Synthesis of Polymer (S1) (PL-LI / Styrene Glycol = 100 / 100) 5.00 g (15.71 mmol) of tetramethoxymethyl glycoluril (POWDERLINK 1174, manufactured by Mitsui Cytec Co., Ltd.), 2.17 g (15.71 mmol) of styrene glycol (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.0299 g (0.16 mmol) of para-toluenesulfonic acid monohydrate (manufactured by Tokyo Chemical Industry Co., Ltd.), and 28.65 g of propylene glycol monomethyl ether acetate were placed in a 100 mL three-neck flask equipped with a stirrer and a condenser, and the mixture was heated to 85°C and stirred at 85°C for 4 hours. After the reaction was stopped, cation exchange resin and anion exchange resin in amounts equal to the solid content were added to the resulting reaction solution, and the mixture was stirred for 4 hours. The ion exchange resin was filtered off to obtain a polymer solution. The weight average molecular weight (Mw) measured by GPC in terms of standard polystyrene was 3489. When the molecular weight of this polymer was measured by GPC (in terms of standard polystyrene), the weight average molecular weight (Mw) was 1218, and the polymer had a repeating unit structure represented by the following formula (6):
[0085] Comparative Synthesis Example 2 Synthesis of Polymer (S2) (PL-LI / 1,4-butanediol = 100 / 100) 5.00 g (15.71 mmol) of tetramethoxymethyl glycoluril (POWDERLINK 1174, manufactured by Mitsui Cytec Co., Ltd.), 1.41 g (15.71 mmol) of 1,4-butanediol (manufactured by Tokyo Chemical Industry Co., Ltd.), 1.49 g (7.85 mmol) of para-toluenesulfonic acid monohydrate (manufactured by Tokyo Chemical Industry Co., Ltd.), and 24.17 g of propylene glycol monomethyl ether acetate were placed in a 100 mL three-neck flask equipped with a stirrer and a condenser, and the mixture was heated to 85°C and stirred at 70°C for 5 hours. After the reaction was stopped, cation exchange resin and anion exchange resin in amounts equal to the solid content were added to the resulting reaction solution, and the mixture was stirred for 4 hours. The ion exchange resin was filtered off to obtain a polymer solution. The molecular weight of this polymer was measured by GPC (standard polystyrene equivalent) and found to have a weight average molecular weight (Mw) of 995, and the polymer had a repeating unit structure represented by the following formula (7).
[0086] <Preparation of Resist Underlayer Film> Polymers (1) to (3) and (S1) to (S2), a crosslinker [tetramethoxymethyl glycoluril], an acid catalyst [p-toluenesulfonic acid], a solvent [propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), and Megafac R-40 (manufactured by DIC Corporation) as a surfactant] were mixed in the weight proportions shown in Table 4 below (the weight proportions of the crosslinker, acid generator, and surfactant are shown when the weight of the polymer is taken as 100; for the solvents, the weight proportions of each solvent are shown when the total solvent weight is taken as 100), and the mixture was filtered through a 0.1 μm polytetrafluoroethylene microfilter to prepare resist underlayer film materials (Examples 1 to 3, Comparative Examples 1 and 2).
[0087] [Hardness Measurement] The resist underlayer film-forming compositions prepared in Examples 1 to 3 and Comparative Examples 1 and 2 were each applied onto a silicon wafer using a spinner. The wafer was then baked on a hot plate at 400°C for 90 seconds to form a resist underlayer film (film thickness 0.2 µm). A nanoindentation test was performed using a nanoindenter manufactured by Toyo Corporation to measure the hardness of the resist underlayer film. The results are shown in Table 1. The resist underlayer films formed from the resist underlayer film-forming compositions prepared in Examples 1 to 3 had higher hardness than the resist underlayer films formed from the resist underlayer film-forming compositions prepared in Comparative Examples 1 and 2.
[0088] [Measurement of Film Density] Each of the resist underlayer film-forming compositions prepared in Examples 1 to 3 and Comparative Examples 1 and 2 was applied onto a silicon wafer using a spinner. The coating was then baked on a hot plate at 400°C for 90 seconds to form a resist underlayer film (film thickness: 0.2 µm). XRR measurement was performed using a D8 DISCOVER manufactured by Bruker AXS to measure the film density of the resist underlayer film. The results are shown in Table 2. The resist underlayer films formed from the resist underlayer film-forming compositions prepared in Examples 1 to 3 had higher film densities than the resist underlayer films formed from the resist underlayer film-forming compositions prepared in Comparative Examples 1 and 2.
Claims
1. A resist underlayer film-forming composition comprising a polymer obtained by reacting a glycoluril compound with an aromatic compound having at least one phenolic hydroxyl group, and a solvent, wherein the nitrogen content of the polymer is less than 10 mass%.
2. The resist underlayer film forming composition according to claim 1, wherein the carbon content of the polymer is 80% or less.
3. The resist underlayer film forming composition according to claim 1, wherein the glycoluril compound is a glycoluril compound substituted with at least one type of substituent, and the substituent is at least one type of substituent selected from the group consisting of an alkylol group having 1 to 12 carbon atoms, an alkoxyalkyl group having 2 to 12 carbon atoms, and an alkenyloxyalkyl group having 3 to 12 carbon atoms.
4. The resist underlayer film forming composition according to claim 1, wherein the glycoluril compound is selected from the group consisting of tetramethylol glycoluril, tetrabutoxymethyl glycoluril, tetramethoxymethyl glycoluril, partially methylolated glycoluril, dimethoxymethyl glycoluril, monomethyl ether of dimethylol glycoluril or dimethyl ether of dimethylol glycoluril, trimethyl ether of tetramethylol glycoluril, tetramethyl ether of tetramethylol glycoluril, tetraethoxymethyl glycoluril, tetrapropoxymethyl glycoluril, tetraamyloxymethyl glycoluril, tetrahexoxymethyl glycoluril, and mixtures thereof.
5. The resist underlayer film forming composition according to claim 1, wherein the glycoluril compound is a glycoluril compound substituted with at least a methoxymethyl group.
6. The resist underlayer film forming composition according to claim 1, wherein the aromatic compound having a phenolic hydroxyl group is selected from the following compounds:
7. The resist underlayer film forming composition according to claim 1, wherein the solvent has a boiling point of 160°C or higher.
8. The resist underlayer film forming composition according to claim 1, further comprising a crosslinking agent.
9. The resist underlayer film forming composition according to claim 8, wherein the crosslinking agent is an aminoplast crosslinking agent or an aminoplast crosslinking agent and a phenoplast crosslinking agent.
10. The resist underlayer film forming composition according to claim 1, further comprising a surfactant.
11. The resist underlayer film forming composition according to claim 1, further comprising an acid and / or a salt thereof and / or an acid generator.
12. A resist underlayer film which is a fired product of a coating film made of the composition according to any one of claims 1 to 11.
13. A method for forming a resist pattern used in the manufacture of semiconductors, comprising the steps of: applying the resist underlayer film forming composition according to any one of claims 1 to 11 onto a semiconductor substrate and baking the composition to form a resist underlayer film; forming a resist film on the resist underlayer film; and forming a resist pattern on the resist film by irradiating the resist film with light or an electron beam and developing the resist pattern.
14. A method for manufacturing a semiconductor device, comprising the steps of: applying the resist underlayer film forming composition according to any one of claims 1 to 11 onto a semiconductor substrate and baking the composition to form a resist underlayer film; forming a resist film on the resist underlayer film; forming a resist pattern on the resist film; etching the resist underlayer film using the resist pattern; and processing a semiconductor substrate using the patterned resist underlayer film.
15. The method for producing a semiconductor device according to claim 14, further comprising the step of forming a resist pattern on the resist film by irradiating the resist film with light or an electron beam and developing the resist film.
16. The method for manufacturing a semiconductor device according to claim 14, wherein the resist pattern is formed on the resist film by a nanoimprint method or a self-assembled film.
17. A method for manufacturing a semiconductor device, comprising the steps of: applying a resist underlayer film forming composition according to any one of claims 1 to 11 onto a semiconductor substrate and baking the composition to form a resist underlayer film; forming a hard mask on the resist underlayer film; further forming a resist film on the hard mask; forming a resist pattern on the resist film; etching the hard mask with the resist pattern; etching the resist underlayer film with the patterned hard mask; and processing a semiconductor substrate with the patterned resist underlayer film.
18. The method for manufacturing a semiconductor device according to claim 17, wherein the hard mask is formed by coating a composition containing an inorganic substance or by vapor deposition of a composition containing an inorganic substance.
19. The method for producing a semiconductor device according to claim 17, further comprising the step of forming a resist pattern on the resist film by irradiating the resist film with light or an electron beam and developing the resist film.
20. The method for manufacturing a semiconductor device according to claim 17, wherein the resist pattern is formed on the resist film by a nanoimprint method or a self-assembled film.
21. A method for manufacturing a semiconductor device, comprising the steps of: applying a resist underlayer film forming composition according to any one of claims 1 to 11 onto a semiconductor substrate and baking the composition to form a resist underlayer film; forming a hard mask on the resist underlayer film; further forming a resist film on the hard mask; forming a resist pattern on the resist film; etching the hard mask using the resist pattern; etching the resist underlayer film using the patterned hard mask; removing the hard mask; and processing a semiconductor substrate using the patterned resist underlayer film.
22. The method for manufacturing a semiconductor device according to claim 21, wherein the hard mask is formed by coating a composition containing an inorganic substance or by vapor deposition of a composition containing an inorganic substance.
23. The method for producing a semiconductor device according to claim 21, further comprising forming a resist pattern on the resist film by irradiation with light or an electron beam and development.
24. The method for manufacturing a semiconductor device according to claim 21, wherein the resist pattern is formed on the resist film by a nanoimprint method or a self-assembled film.
25. The method for manufacturing a semiconductor device according to claim 21, wherein the hard mask is removed by either etching or an alkaline chemical solution.
26. A method for manufacturing a semiconductor device, comprising the steps of: applying a resist underlayer film forming composition according to any one of claims 1 to 11 onto a semiconductor substrate and baking the composition to form a resist underlayer film; forming a hard mask on the resist underlayer film; further forming a resist film on the hard mask; forming a resist pattern on the resist film; etching the hard mask with the resist pattern; etching the resist underlayer film with the patterned hard mask; removing the hard mask; forming a vapor-deposited film (spacer) on the resist underlayer film after removing the hard mask; processing the vapor-deposited film (spacer) by etching; removing the patterned resist underlayer film to leave the patterned vapor-deposited film (spacer); and processing a semiconductor substrate with the patterned vapor-deposited film (spacer).
27. The method for producing a semiconductor device according to claim 26, wherein the hard mask is formed by coating a composition containing an inorganic substance or by vapor deposition of a composition containing an inorganic substance.
28. The method for producing a semiconductor device according to claim 26, further comprising forming a resist pattern on the resist film by irradiating the resist film with light or an electron beam and developing the resist film.
29. The method for manufacturing a semiconductor device according to claim 26, wherein the resist pattern is formed on the resist film by a nanoimprint method or a self-assembled film.
30. The method for manufacturing a semiconductor device according to claim 26, wherein the hard mask is removed by either etching or an alkaline chemical solution.
Citation Information
Patent Citations
Lower layer film composition for imprinting, and pattern forming method using the same
JP2013202982A
Resist underlayer film-forming composition for semiconductor, resist underlayer film, method for forming resist underlayer film, and method for manufacturing patterned substrate
JP2019020701A
Material for forming organic film, patterning process, and polymer
JP2021084974A
Anti-reflective coating composition for photoresists
JP5613950B2
Curable composition for imprinting, composition for adhesion to substrates, and semiconductor device using the same
JP5827180B2
Cited By
Underlayer film material for self-assembled materials
WO2026164053A1