Fast-curing high-toughness soft paint powder coating and preparation method thereof

By using specific resins and toughening agent combinations in powder coatings, combined with silane coupling agent treatment and alumina to prevent agglomeration, the problems of long curing time and poor flexibility of powder coatings are solved, and rapid curing and efficient spraying are achieved to ensure coating. The stability and bending resistance of the layer during metal processing.

CN118956239AInactive Publication Date: 2024-11-15SHANDONG AIYUE POWDER COATING CO LTD +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411441343.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing powder coatings have a long curing time at high temperatures and have poor flexibility and adhesion, resulting in low spraying efficiency and prone to coating cracking and damage during metal processing.

Method used

It adopts a combination of end hydroxyl and end carboxylic polyester resins, glycerin resins, toughening agents, high toughness polyester resins and other materials, and through specific esterification reactions and silane coupling agent treatment, it forms high toughness and good bonding properties. Combined with alumina to prevent agglomeration, a rapid curing, high toughness, lacquer powder coating is prepared.

Benefits of technology

It achieves rapid curing at 240°C, improves spraying efficiency and bending resistance of the coating, avoids cracking and damage of the coating during metal processing, and meets the requirements of efficient spraying and processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a fast-curing high-toughness soft paint powder coating and a preparation method thereof, and relates to the technical field of powder coatings. Comprising hydroxyl-terminated polyester resin, carboxyl-terminated polyester resin, glycoluril resin, a flexibilizer, an acrylate leveling agent, a polyester curing agent TGIC, hydroxyl polyester resin, high-toughness polyester resin, isocyanate and the like. The fast-curing high-toughness mein paint powder coating is sprayed on coil steel, can effectively replace a liquid coating to reduce emission of VOC (volatile organic compound), can be cured at 240 DEG C within 90 seconds, is high in curing speed, meets the requirement on the spraying speed of an existing coil material, and is good in bending resistance of a coating film. And meanwhile, a cured paint film is free of obvious cracking in an OT bending test, a sprayed finished product is qualified in a 1T bending test 12 months later, and the problem that in the prior art, a color-coated sheet cannot be processed in the later period of powder spraying is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder coatings, in particular to a fast-curing high-toughness lacquer powder coating and a preparation method thereof. Background Art

[0002] Since powder coatings do not contain organic solvents, they have the advantages of saving resources, reducing environmental pollution, and 100% utilization rate. At present, the thermal baking curing process of ordinary powder coatings on the market is about 200°C for curing for 10 to 20 minutes, but the coil spraying efficiency is high and the speed is fast, and the curing time is basically about 90 seconds. Therefore, the curing conditions of existing powder coatings seriously affect the spraying efficiency of coils. At the same time, the finished color steel plate sprayed with coils needs to be bent in the later stage, but the existing powder coatings have poor bending performance, and the surface itself is uneven, with "ridges" and "valleys" surface effects. In addition, due to the low flexibility and poor adhesion of existing powder coatings, the coating is very easy to crack and break during the bending, extension, stamping, stretching and other processing of metals.

[0003] Therefore, there is an urgent need to develop a fast-curing, high-toughness lacquer powder coating that can cure quickly at high temperatures, has high flexibility and good adhesion, and will not cause cracking or damage to the coating during processing. Summary of the invention

[0004] To solve the above problems, the purpose of the present invention is to provide a fast-curing high-toughness lacquer powder coating and a preparation method thereof.

[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions: A fast-curing high-toughness lacquer powder coating comprises the following raw materials, measured in parts by weight: 40-50 parts of hydroxyl-terminated and carboxyl-terminated polyester resins, 2-5 parts of glycoluril resins, 1-3 parts of toughening agents, 0.1-0.4 parts of benzoin, 0.6-1 parts of acrylate leveling agents, 0.3-0.6 parts of amine-blocked sulfonates, 4.5-5 parts of polyester curing agent TGIC, 0.6-1 parts of colorants, 3.5-4 parts of fillers, 15-20 parts of hydroxyl polyester resins, 15-20 parts of high-toughness polyester resins and 4-5 parts of isocyanates.

[0006] Preferably, 0.1 to 0.5 parts of aluminum oxide is also included. The addition of aluminum oxide can prevent the powder coating from agglomerating during storage.

[0007] Preferably, the acid value of the hydroxyl-terminated and carboxyl-terminated polyester resin is 30-40 mgKOH / g, and the hydroxyl value is 20-30 mgKOH / g.

[0008] Preferably, the hydroxyl-terminated and carboxyl-terminated polyester resins are prepared according to the following steps: Remove moisture from phthalic acid and diol respectively and set aside; In parts by weight, phthalic acid, diol and stannous octoate are added to a reaction kettle, nitrogen is introduced, the temperature is raised to 105-115° C. for heat preservation and reaction, a vacuum pump and a condenser are turned on during the reaction to remove water vapor generated by the reaction and promote the reaction, and the hydroxyl value and acid value of the reaction liquid are detected after the reaction for 1.5-2 hours. When the hydroxyl value of the reaction liquid is 20-30 mgKOH / g and the acid value is 30-40 mgKOH / g, a polymerization inhibitor is added, the temperature is lowered to 25-35° C., the material is discharged, and crushed with a crusher to obtain a hydroxyl-terminated and carboxyl-terminated polyester resin; The mass ratio of phthalic acid, diol, stannous octoate and inhibitor is 40-50:40-50:0.2-0.6:0.1-0.3; The diol is propylene glycol or isoprene glycol; The phthalic acid is isophthalic acid or terephthalic acid; The polymerization inhibitor is hydroquinone or p-tert-butylcatechol.

[0009] Preferably, the high-toughness polyester resin is prepared according to the following steps: 40-50 parts of mixed dibasic acid, 25-35 parts of mixed diol and 0.01-0.05 parts of antioxidant are added to a reaction kettle, nitrogen is introduced, and the temperature is raised to 150-160° C. under stirring until the system starts to discharge water, and the outlet head temperature is controlled to be above 98° C., and the temperature is kept constant for 1-2 hours until the head temperature drops below 98° C., 0.02-0.06 parts of catalyst are added thereto, and the temperature is continued to be raised to 200-210° C. After reacting for 1 hour, the acid value of the reaction liquid is measured to be 40-50 mgKOH / g, and the heating is stopped, and the temperature is lowered to 175-185° C., and 0.01-0.03 parts of inhibitor hydroquinone are added thereto, and when the temperature drops to 60-70° C., 1-2 parts of amino-containing silane coupling agent are added thereto, and the reaction is stirred for 30-60 minutes, and the temperature is lowered to 20-35° C. to obtain a high-toughness polyester resin; The mixed dibasic acid is composed of succinic acid, terephthalic acid, and adipic anhydride in a mass ratio of 10-15:65-70:5-8; The mixed diol is composed of propylene glycol, neopentyl glycol and triethylene glycol in a mass ratio of 25-35:10-20:40-50; The antioxidant is triphenyl phosphite or dilauryl thiodipropionate; The catalyst is stannous oxalate or stannous octoate; The amino-containing silane coupling agent is silane coupling agent KH-540, aniline methyl trimethoxy silane or phenyl triethoxy silane.

[0010] The preferred high-toughness polyester resin of the present invention uses mixed dibasic acid and mixed dibasic acid as raw materials for esterification reaction, which can form long and short chain segments in the esterification reaction, and form a three-dimensional network structure after being combined with a toughening agent. In particular, a silane coupling agent containing amino groups is added to the three-dimensional network structure, which improves the flexibility and adhesion of the powder coating while improving the adhesion of the powder coating to the coiled material, thereby avoiding cracking and damage of the coating during metal bending, extension, stamping, stretching and other processing.

[0011] Preferably, the colorant is carbon black, iron yellow, iron red, titanium dioxide, ultramarine or phthalocyanine green. The powder coating of the present invention can be toned by adding colorants of different colors.

[0012] Preferably, the filler is barium sulfate or calcium carbonate.

[0013] Preferably, the filler is pretreated with a silane coupling agent; the mass ratio of the filler to the silane coupling agent is 100:1-5; The pre-processing process is as follows: Add the filler into a mixer, heat to 80-90°C while stirring, add the silane coupling agent ethanol solution thereto, stir and disperse the reaction for 30-60 minutes, and cool to obtain the filler pretreated with the silane coupling agent; The silane coupling agent is KH-550, A-151 or KH560; The silane coupling agent ethanol solution is obtained by mixing the silane coupling agent and ethanol in a mass ratio of 1:3-5.

[0014] The filler treated with silane coupling agent can better cooperate with other substances in powder coating, further improve the bonding performance to the coiled material, and avoid cracking and damage of the coating during the bending, extension, stamping, stretching and other processing of the metal.

[0015] The present invention also includes a method for preparing a fast-curing high-toughness lacquer powder coating, comprising the following steps: In parts by weight, 40-50 parts of hydroxyl-terminated and carboxyl-terminated polyester resins, 2-5 parts of glycoluril resins, 1-3 parts of tougheners, 0.1-0.4 parts of benzoin, 0.6-1 parts of acrylate leveling agents, 0.3-0.6 parts of amine-blocked sulfonates, 4.5-5% of polyester curing agent TGIC, 0.6-1 parts of colorants, 3.5-4 parts of fillers, 15-20 parts of hydroxyl polyester resins, 15-20 parts of high-toughness polyester resins and 4-5 parts of isocyanates are added into a reaction kettle and mixed evenly; the mixture is extruded at 90-100° C. by an extruder, cooled and crushed to obtain a flaky material; the flaky material is ground and sieved to obtain a fast-curing high-toughness lacquer powder coating.

[0016] Preferably, 0.1 to 0.5 parts of aluminum oxide are added during the grinding process. It has been found in studies that adding aluminum oxide can prevent the coating from agglomerating.

[0017] Compared with the prior art, the present invention has the following advantages: The fast-curing high-toughness slurry powder coating of the present invention can effectively replace liquid coatings to reduce VOC emissions when sprayed on coiled steel. It can be cured in less than 90 seconds at 240°C, has a fast curing speed, meets the current coil spraying speed requirements, and has good bending resistance. At the same time, the cured paint film has no obvious cracking in the OT bending test, and the sprayed finished product passes the 1T bending test 12 months later, which solves the problem that the color-coated plate cannot be processed in the later stage of powder spraying in the prior art.

[0018] The fast-curing high-toughness velvety paint powder coating of the present invention adopts terminal hydroxyl and terminal carboxyl polyester resins to react with curing agent TGIC and glycoluril resin at the same time, and has both the excellent properties of polyester and the effect of velvety paint; the reaction of hydroxyl polyester resin and isocyanate can better form patterns, and materials such as high-toughness polyester resin and toughening agent can improve the bending performance of the coating film in the later stage, so that there is no obvious cracking during OT testing. DETAILED DESCRIPTION

[0019] The object of the present invention is to provide a fast-curing high-toughness lacquer powder coating and a preparation method thereof. The present invention is further described below in conjunction with specific embodiments.

[0020] The manufacturers and models of some raw materials in the embodiments of the present invention are as follows: Glycol uril resin was purchased from Shanghai Suo Shi Chemical Co., Ltd., model AYSD7114; toughening agent was purchased from Shanghai Suo Shi Chemical Co., Ltd., model AYG82; hydroxy polyester resin was purchased from Zhejiang Chuanhua Tiansong New Materials Co., Ltd., model AYSD0036; high-toughness polyester resin was purchased from Xinzhongfa Polymer Materials Co., Ltd., model AYG330; isocyanate was purchased from Lu'an Korida New Materials Co., Ltd., model AYSD1507.

[0021] Example 1: A fast-curing high-toughness lacquer powder coating is composed of the following raw materials: 40 kg of terminal hydroxyl and terminal carboxyl polyester resin, 2 kg of glycoluril resin, 1 kg of toughening agent, 0.1 kg of benzoin, 0.6 kg of acrylate leveling agent, 0.3 kg of amine-blocked sulfonate, 4.5 kg of polyester curing agent TGIC, 0.6 kg of colorant carbon black, 3.5 kg of barium sulfate, 15 kg of hydroxy polyester resin, 15 kg of high-toughness polyester resin and 4 kg of isocyanate.

[0022] Example 2: A fast-curing high-toughness lacquer powder coating, composed of the following raw materials: 50kg of terminal hydroxyl and terminal carboxyl polyester resin, 5kg of glycoluril resin, 3kg of toughening agent, 0.4kg of benzoin, 1kg of acrylate leveling agent, 0.6kg of amine-blocked sulfonate, 5kg of polyester curing agent TGIC, 1kg of iron yellow colorant, 4kg of calcium carbonate, 20kg of hydroxy polyester resin, 20kg of high-toughness polyester resin and 5kg of isocyanate.

[0023] Example 3: A fast-curing high-toughness lacquer powder coating, composed of the following raw materials: 44 kg of hydroxyl-terminated and carboxyl-terminated polyester resin, 3 kg of glycoluril resin, 1.5 kg of toughening agent, 0.2 kg of benzoin, 0.7 kg of acrylate leveling agent, 0.4 kg of amine-blocked sulfonate, 4.6 kg of polyester curing agent TGIC, 0.7 kg of iron red colorant, 3.6 kg of barium sulfate, 16 kg of hydroxyl polyester resin, 19 kg of high-toughness polyester resin and 4.2 kg of isocyanate; The terminal hydroxyl group and terminal carboxyl group polyester resin has an acid value of 30 mgKOH / g and a hydroxyl value of 30 mgKOH / g.

[0024] Example 4: A fast-curing high-toughness lacquer powder coating, composed of the following raw materials: 46 kg of hydroxyl-terminated and carboxyl-terminated polyester resin, 4 kg of glycoluril resin, 2.5 kg of toughening agent, 0.3 kg of benzoin, 0.8 kg of acrylate leveling agent, 0.5 kg of amine-blocked sulfonate, 4.8 kg of polyester curing agent TGIC, 0.8 kg of phthalocyanine green, 3.8 kg of calcium carbonate, 18 kg of hydroxyl polyester resin, 16 kg of high-toughness polyester resin, 4.5 kg of isocyanate and 0.1 kg of aluminum oxide; The terminal hydroxyl and terminal carboxyl polyester resin has an acid value of 40 mgKOH / g and a hydroxyl value of 20 mgKOH / g; it is prepared according to the following steps: Remove water from isophthalic acid and propylene glycol respectively and set aside; 50 kg of isophthalic acid, 40 kg of propylene glycol and 0.2 kg of stannous octoate are added to a reaction kettle, nitrogen is introduced, the temperature is raised to 105° C. for heat preservation and reaction, a vacuum pump and a condenser are turned on during the reaction to remove water vapor generated by the reaction and promote the reaction, and the hydroxyl value and acid value of the reaction liquid are tested after reacting for 2 hours. When the hydroxyl value of the reaction liquid is 20 mgKOH / g and the acid value is 40 mgKOH / g, 0.1 kg of a polymerization inhibitor hydroquinone is added, the temperature is lowered to 25° C., the material is discharged, and crushed with a crusher to obtain a hydroxyl-terminated and carboxyl-terminated polyester resin; The high-toughness polyester resin is prepared according to the following steps: 40 kg of mixed dibasic acid, 35 kg of mixed diol and 0.01 kg of antioxidant triphenyl phosphite were added to a reaction kettle, nitrogen was introduced, and the temperature was raised to 150° C. under stirring until the system began to discharge water, and the outlet head temperature was controlled to be above 98° C., and the temperature was kept constant for 1 hour until the head temperature dropped to below 98° C., 0.06 kg of catalyst stannous oxalate was added thereto, and the temperature was continued to be raised to 200° C. After reacting for 1 hour, the acid value of the reaction liquid was measured to be 40 mgKOH / g, and the heating was stopped, and the temperature was lowered to 175° C., 0.01 kg of inhibitor hydroquinone was added thereto, and when the temperature dropped to 60° C., 1 kg of silane coupling agent KH-540 was added thereto, and the reaction was stirred for 30 minutes, and the temperature was lowered to 20° C. to obtain a high-toughness polyester resin; The mixed dibasic acid is composed of succinic acid, terephthalic acid and adipic anhydride in a mass ratio of 10:65:5; The mixed diol is composed of propylene glycol, neopentyl glycol and triethylene glycol in a mass ratio of 25:10:40; The calcium carbonate is pretreated with a silane coupling agent, and the pretreatment process is as follows: 3.8 kg of calcium carbonate was added into a mixer, heated to 80° C. under stirring, 152 g of silane coupling agent ethanol solution was sprayed into the mixer, stirred and dispersed for 30 minutes, and cooled to obtain a filler pretreated with a silane coupling agent; The silane coupling agent is KH-550; The silane coupling agent ethanol solution is obtained by mixing the silane coupling agent and ethanol in a mass ratio of 1:3.

[0025] Example 5: A fast-curing high-toughness lacquer powder coating, composed of the following raw materials: 48 kg of hydroxyl-terminated and carboxyl-terminated polyester resin, 4.5 kg of glycoluril resin, 1.5 kg of toughening agent, 0.25 kg of benzoin, 0.9 kg of acrylate leveling agent, 0.5 kg of amine-blocked sulfonate, 4.9 kg of polyester curing agent TGIC, 0.8 kg of titanium dioxide, 3.7 kg of barium sulfate, 17 kg of hydroxyl polyester resin, 17 kg of high-toughness polyester resin, 4.8 kg of isocyanate and 0.5 kg of aluminum oxide; The terminal hydroxyl and terminal carboxyl polyester resin has an acid value of 35 mgKOH / g and a hydroxyl value of 25 mgKOH / g; it is prepared according to the following steps: Remove water from terephthalic acid and diol respectively and set aside; 46 kg of terephthalic acid, 42 kg of isoprene glycol and 0.6 kg of stannous octoate were added to a reaction kettle, nitrogen was introduced, the temperature was raised to 115° C. for heat preservation and reaction, a vacuum pump and a condenser were turned on during the reaction to remove water vapor generated by the reaction and promote the reaction, and the hydroxyl value and acid value of the reaction liquid were tested after the reaction for 1.5 hours. When the hydroxyl value of the reaction liquid was 25 mgKOH / g and the acid value was 35 mgKOH / g, 0.2 kg of polymerization inhibitor p-tert-butylcatechol was added, the temperature was lowered to 28° C., the material was discharged, and crushed with a crusher to obtain a hydroxyl-terminated and carboxyl-terminated polyester resin; The high-toughness polyester resin is prepared according to the following steps: 50 kg of mixed dibasic acid, 25 kg of mixed diol and 0.05 kg of dilauryl thiodipropionate were added to a reaction kettle, nitrogen was introduced, and the temperature was raised to 160° C. under stirring until the system began to discharge water, and the outlet head temperature was controlled to be above 98° C., and the temperature was kept constant for 2 hours until the head temperature dropped to below 98° C., 0.02 kg of stannous octoate was added thereto, and the temperature was continued to be raised to 210° C., and after reacting for 1 hour, the acid value of the reaction liquid was measured to be 50 mgKOH / g, and the heating was stopped, and the temperature was lowered to 185° C., 0.03 kg of inhibitor hydroquinone was added, and when the temperature dropped to 70° C., 2 kg of aniline methyl trimethoxy silane was added thereto, and the reaction was stirred for 60 minutes, and the temperature was lowered to 35° C. to obtain a high-toughness polyester resin; The mixed dibasic acid is composed of succinic acid, terephthalic acid and adipic anhydride in a mass ratio of 15:70:8; The mixed diol is composed of propylene glycol, neopentyl glycol and triethylene glycol in a mass ratio of 35:20:50; The barium sulfate is pretreated with a silane coupling agent; the mass ratio of the filler to the silane coupling agent is 100:5; The pre-processing process is as follows: 3.7 kg of barium sulfate was added into a mixer, heated to 90° C. under stirring, 1.11 kg of silane coupling agent ethanol solution was sprayed therein, stirred and dispersed for reaction for 60 minutes, and cooled to obtain a filler pretreated with a silane coupling agent; The silane coupling agent is A-151; The silane coupling agent ethanol solution is obtained by mixing the silane coupling agent and ethanol in a mass ratio of 1:5.

[0026] Example 6: A fast-curing high-toughness lacquer powder coating, composed of the following raw materials: 45 kg of hydroxyl-terminated and carboxyl-terminated polyester resin, 3 kg of glycoluril resin, 2 kg of toughening agent, 0.3 kg of benzoin, 0.8 kg of acrylate leveling agent, 0.5 kg of amine-blocked sulfonate, 4.6 kg of polyester curing agent TGIC, 0.8 kg of ultramarine, 3.9 kg of calcium carbonate, 18 kg of hydroxyl polyester resin, 16 kg of high-toughness polyester resin, 4.5 kg of isocyanate and 0.3 kg of aluminum oxide; The hydroxyl-terminated and carboxyl-terminated polyester resin has an acid value of 32 mgKOH / g and a hydroxyl value of 24 mgKOH / g; it is prepared according to the following steps: Remove water from terephthalic acid and propylene glycol respectively and set aside; 48 kg of terephthalic acid, 44 kg of propylene glycol and 0.4 kg of stannous octoate were added to a reaction kettle, nitrogen was introduced, the temperature was raised to 108° C. for heat preservation and reaction, a vacuum pump and a condenser were turned on during the reaction to remove water vapor generated by the reaction and promote the reaction, and the hydroxyl value and acid value of the reaction liquid were tested after 1.8 hours of reaction. When the hydroxyl value of the reaction liquid was 24 mgKOH / g and the acid value was 32 mgKOH / g, 0.25 kg of a polymerization inhibitor hydroquinone was added, the temperature was lowered to 30° C., the material was discharged, and crushed with a crusher to obtain a hydroxyl-terminated and carboxyl-terminated polyester resin; The high-toughness polyester resin is prepared according to the following steps: 45 kg of mixed dibasic acid, 30 kg of mixed diol and 0.04 kg of triphenyl phosphite were added to a reaction kettle, nitrogen was introduced, and the temperature was raised to 155° C. under stirring until the system began to discharge water, and the outlet head temperature was controlled to be above 98° C., and the temperature was kept constant for 1.5 hours until the head temperature dropped to below 98° C., 0.04 kg of catalyst stannous octoate was added thereto, and the temperature was continued to be raised to 205° C., and after reacting for 1 hour, the acid value of the reaction liquid was measured to be 46 mgKOH / g, and the heating was stopped, and the temperature was lowered to 180° C., 0.02 kg of inhibitor hydroquinone was added, and when the temperature dropped to 65° C., 1.5 kg of phenyltriethoxysilane was added thereto, and the reaction was stirred for 50 minutes, and the temperature was lowered to 30° C. to obtain a high-toughness polyester resin; The mixed dibasic acid is composed of succinic acid, terephthalic acid, and adipic anhydride in a mass ratio of 14:66:6; The mixed diol is composed of propylene glycol, neopentyl glycol and triethylene glycol in a mass ratio of 32:15:45; The calcium carbonate is pretreated with a silane coupling agent; the mass ratio of the filler to the silane coupling agent is 100:4; The pre-processing process is as follows: 3.9 kg of calcium carbonate was added into a mixer, heated to 86° C. under stirring, 0.78 kg of silane coupling agent ethanol solution was sprayed into the mixer, stirred and dispersed for 50 minutes, and cooled to obtain a filler pretreated with a silane coupling agent; The silane coupling agent is KH560; The silane coupling agent ethanol solution is obtained by mixing the silane coupling agent and ethanol in a mass ratio of 1:4.

[0027] Example 7: The method for preparing the fast-curing high-toughness lacquer powder coating described in Example 1 comprises the following steps: 40kg of terminal hydroxyl and terminal carboxyl polyester resin, 2kg of glycoluril resin, 1kg of toughening agent, 0.1kg of benzoin, 0.6kg of acrylate leveling agent, 0.3kg of amine-blocked sulfonate, 4.5kg of polyester curing agent TGIC, 0.6kg of colorant carbon black, 3.5kg of barium sulfate, 15kg of hydroxy polyester resin, 15kg of high-toughness polyester resin and 4kg of isocyanate were added into a reaction kettle and mixed evenly, extruded at 90°C using an extruder, cooled and crushed to obtain a flaky material, and the obtained flaky material was ground and sieved to obtain a fast-curing high-toughness lacquer powder coating.

[0028] Embodiment 8: The method for preparing the fast-curing high-toughness soft paint powder coating described in Embodiment 2 comprises the following steps: 50kg of hydroxyl-terminated and carboxyl-terminated polyester resin, 5kg of glycoluril resin, 3kg of toughening agent, 0.4kg of benzoin, 1kg of acrylate leveling agent, 0.6kg of amine-blocked sulfonate, 5kg of polyester curing agent TGIC, 1kg of iron yellow colorant, 4kg of calcium carbonate, 20kg of hydroxyl polyester resin, 20kg of high-toughness polyester resin and 5kg of isocyanate were added into a reaction kettle and mixed evenly, extruded at 90-100°C by an extruder, cooled and crushed to obtain a flaky material, and the obtained flaky material was ground and sieved to obtain a fast-curing high-toughness lacquer powder coating.

[0029] Embodiment 9: The method for preparing the fast-curing high-toughness soft paint powder coating described in Embodiment 3 comprises the following steps: 44kg of terminal hydroxyl and terminal carboxyl polyester resin, 3kg of glycoluril resin, 1.5kg of toughening agent, 0.2kg of benzoin, 0.7kg of acrylate leveling agent, 0.4kg of amine-blocked sulfonate, 4.6kg of polyester curing agent TGIC, 0.7kg of iron red colorant, 3.6kg of barium sulfate, 16kg of hydroxy polyester resin, 19kg of high-toughness polyester resin and 4.2kg of isocyanate were added into a reaction kettle and mixed evenly, extruded at 90-100°C by an extruder, cooled and crushed to obtain a flaky material, and the obtained flaky material was ground and sieved to obtain a fast-curing high-toughness lacquer powder coating.

[0030] Embodiment 10: The method for preparing the fast-curing high-toughness soft paint powder coating described in Embodiment 4 comprises the following steps: 46kg of terminal hydroxyl and terminal carboxyl polyester resin, 4kg of glycoluril resin, 2.5kg of toughening agent, 0.3kg of benzoin, 0.8kg of acrylate leveling agent, 0.5kg of amine-blocked sulfonate, 4.8kg of polyester curing agent TGIC, 0.8kg of phthalocyanine green, 3.8kg of calcium carbonate, 18kg of hydroxy polyester resin, 16kg of high-toughness polyester resin and 4.5kg of isocyanate were added into a reaction kettle and mixed evenly, extruded at 90-100°C by an extruder, cooled and crushed to obtain a flaky material, ground the obtained flaky material, added 0.1kg of aluminum oxide during the grinding process, and sieved to obtain a fast-curing high-toughness lacquer powder coating.

[0031] Example 11: The method for preparing the fast-curing high-toughness lacquer powder coating described in Example 5 comprises the following steps: 48kg of terminal hydroxyl and terminal carboxyl polyester resin, 4.5kg of glycoluril resin, 1.5kg of toughening agent, 0.25kg of benzoin, 0.9kg of acrylate leveling agent, 0.5kg of amine-blocked sulfonate, 4.9kg of polyester curing agent TGIC, 0.8kg of titanium dioxide, 3.7kg of barium sulfate, 17kg of hydroxy polyester resin, 17kg of high-toughness polyester resin and 4.8kg of isocyanate were added into a reaction kettle and mixed evenly, extruded at 90-100°C by an extruder, cooled and crushed to obtain a flaky material, which was ground, 0.5kg of aluminum oxide was added during the grinding process, and sieved to obtain a fast-curing high-toughness lacquer powder coating.

[0032] Example 12: The method for preparing the fast-curing high-toughness lacquer powder coating described in Example 6 comprises the following steps: 45kg of terminal hydroxyl and terminal carboxyl polyester resin, 3kg of glycoluril resin, 2kg of toughening agent, 0.3kg of benzoin, 0.8kg of acrylate leveling agent, 0.5kg of amine-blocked sulfonate, 4.6kg of polyester curing agent TGIC, 0.8kg of ultramarine, 3.9kg of calcium carbonate, 18kg of hydroxy polyester resin, 16kg of high-toughness polyester resin and 4.5kg of isocyanate were added into a reaction kettle and mixed evenly, extruded at 90-100°C by an extruder, cooled and crushed to obtain a flaky material, which was ground, 0.3kg of aluminum oxide was added during the grinding process, and sieved to obtain a fast-curing high-toughness lacquer powder coating.

[0033] In the preparation method of the present invention, when mixing is performed in a reaction kettle, the rotation speed of the stirrer is 1100-1300 rpm, the extruder extrude at a temperature of 90° C. in the first zone and 100° C. in the second zone, the main engine screw frequency is set at 40-50 Hz, a vertical mill is used to grind the flakes in the grinding process, the main grinding frequency of the vertical mill is set to 50 Hz, and the auxiliary grinding frequency is set to 35 Hz, aluminum oxide can be added in the process of grinding the flakes, and the powder coating is obtained after screening with a 180-mesh net.

[0034] The fast-curing and high-toughness lacquer powder coatings obtained in Examples 7 to 12 were coated on a galvanized sheet by a one-coating process and cured (the curing temperature was 240°C). The curing time was as shown in Table 1 to obtain a coating with a thickness of 50 μm, and then relevant tests were carried out. The test items and test methods were as follows: Gloss: tested according to GB / T 9754-2007; Pencil hardness: tested according to GB / T 6739-2006; Impact performance: tested according to GB / T 1732-2020; 1000h xenon lamp aging test: tested according to GB / T13448-2019; T-bend performance: tested according to GB / T13448-2019; and tested again after being placed for 12 months.

[0035] Table 1 Performance test results of fast curing high toughness soft paint powder coatings obtained in Examples 7 to 12

[0036] It can be seen from the results in Table 1 that the fast-curing high-toughness lacquer powder coating of the present invention can be quickly cured, has good storage stability, and is resistant to aging. The formed coating has clear reticulated patterns, good bending performance, high flexibility, and good adhesion. The coating will not crack or break during the bending, extension, stamping, stretching and other processing of the metal. In addition, it was found during production that adding aluminum oxide to the powder coating can prevent the powder coating from agglomerating.

Claims

1. A fast-curing high-toughness lacquer powder coating, characterized in that: The invention comprises the following raw materials, in parts by weight: 40-50 parts of hydroxyl-terminated and carboxyl-terminated polyester resins, 2-5 parts of glycoluril resins, 1-3 parts of toughening agents, 0.1-0.4 parts of benzoin, 0.6-1 parts of acrylate leveling agents, 0.3-0.6 parts of amine-blocked sulfonates, 4.5-5 parts of polyester curing agent TGIC, 0.6-1 parts of colorants, 3.5-4 parts of fillers, 15-20 parts of hydroxyl polyester resins, 15-20 parts of high-toughness polyester resins and 4-5 parts of isocyanates.

2. The fast-curing high-toughness lacquer powder coating according to claim 1, characterized in that: It also includes 0.1 to 0.5 parts of aluminum oxide.

3. The fast-curing high-toughness lacquer powder coating according to claim 1, characterized in that: The terminal hydroxyl group and terminal carboxyl group polyester resin has an acid value of 30-40 mgKOH / g and a hydroxyl value of 20-30 mgKOH / g.

4. The fast-curing high-toughness lacquer powder coating according to claim 1, characterized in that: The hydroxyl-terminated and carboxyl-terminated polyester resins are prepared according to the following steps: Remove moisture from phthalic acid and diol respectively and set aside; In parts by weight, phthalic acid, diol and stannous octoate are added to a reaction kettle, nitrogen is introduced, the temperature is raised to 105-115° C. for heat preservation and reaction, a vacuum pump and a condenser are turned on during the reaction to remove water vapor generated by the reaction and promote the reaction, and the hydroxyl value and acid value of the reaction liquid are detected after the reaction for 1.5-2 hours. When the hydroxyl value of the reaction liquid is 20-30 mgKOH / g and the acid value is 30-40 mgKOH / g, a polymerization inhibitor is added, the temperature is lowered to 25-35° C., the material is discharged, and crushed with a crusher to obtain a hydroxyl-terminated and carboxyl-terminated polyester resin; The mass ratio of phthalic acid, diol, stannous octoate and inhibitor is 40-50:40-50:0.2-0.6:0.1-0.3; The diol is propylene glycol or isoprene glycol; The phthalic acid is isophthalic acid or terephthalic acid; The polymerization inhibitor is hydroquinone or p-tert-butylcatechol.

5. The fast-curing high-toughness lacquer powder coating according to claim 1, characterized in that: The high-toughness polyester resin is prepared according to the following steps: 40-50 parts of mixed dibasic acid, 25-35 parts of mixed diol and 0.01-0.05 parts of antioxidant are added to a reaction kettle, nitrogen is introduced, and the temperature is raised to 150-160° C. under stirring until the system starts to discharge water, and the outlet head temperature is controlled to be above 98° C., and the temperature is kept constant for 1-2 hours until the head temperature drops below 98° C., 0.02-0.06 parts of catalyst are added thereto, and the temperature is continued to be raised to 200-210° C. After reacting for 1 hour, the acid value of the reaction liquid is measured to be 40-50 mgKOH / g, and the heating is stopped, and the temperature is lowered to 175-185° C., and 0.01-0.03 parts of inhibitor hydroquinone are added thereto, and when the temperature drops to 60-70° C., 1-2 parts of amino-containing silane coupling agent are added thereto, and the reaction is stirred for 30-60 minutes, and the temperature is lowered to 20-35° C. to obtain a high-toughness polyester resin; The mixed dibasic acid is composed of succinic acid, terephthalic acid, and adipic anhydride in a mass ratio of 10-15:65-70:5-8; The mixed diol is composed of propylene glycol, neopentyl glycol and triethylene glycol in a mass ratio of 25-35:10-20:40-50; The antioxidant is triphenyl phosphite or dilauryl thiodipropionate; The catalyst is stannous oxalate or stannous octoate; The amino-containing silane coupling agent is silane coupling agent KH-540, aniline methyl trimethoxy silane or phenyl triethoxy silane.

6. The fast-curing high-toughness lacquer powder coating according to claim 1, characterized in that: The colorant is carbon black, iron yellow, iron red, titanium dioxide, ultramarine blue or phthalocyanine green.

7. The fast-curing high-toughness lacquer powder coating according to claim 1, characterized in that: The filler is barium sulfate or calcium carbonate.

8. The fast-curing high-toughness lacquer powder coating according to claim 6, characterized in that: The filler is pretreated with a silane coupling agent; the mass ratio of the filler to the silane coupling agent is 100:1-5; The pre-processing process is as follows: Add the filler into a mixer, heat to 80-90°C while stirring, add the silane coupling agent ethanol solution thereto, stir and disperse the reaction for 30-60 minutes, and cool to obtain the filler pretreated with the silane coupling agent; The silane coupling agent is KH-550, A-151 or KH560; The silane coupling agent ethanol solution is obtained by mixing the silane coupling agent and ethanol in a mass ratio of 1:3-5.

9. The method for preparing a fast-curing high-toughness lacquer powder coating according to claim 1, characterized in that: The following steps are involved: In parts by weight, 40-50 parts of terminal hydroxyl and terminal carboxyl polyester resins, 2-5 parts of glycoluril resins, 1-3 parts of tougheners, 0.1-0.4 parts of benzoin, 0.6-1 parts of acrylate leveling agents, 0.3-0.6 parts of amine-blocked sulfonates, 4.5-5% of polyester curing agent TGIC, 0.6-1 parts of colorants, 3.5-4 parts of fillers, 15-20 parts of hydroxy polyester resins, 15-20 parts of high-toughness polyester resins and 4-5 parts of isocyanates are added into a reaction kettle and mixed evenly, extruded at 90-100° C. by an extruder, cooled and crushed to obtain flaky materials, and the obtained flaky materials are ground and sieved to obtain a fast-curing high-toughness lacquer powder coating.

10. The method for preparing a fast-curing high-toughness lacquer powder coating according to claim 9, characterized in that: Add 0.1~0.5 parts of aluminum oxide during the grinding process.

Citation Information

Patent Citations

  • Bifunctional polyester resin for powder coating and preparation method of polyester resin

    CN107868235A

  • Polyester resin and preparation method thereof

    CN108084418A

  • Preparation method of semi-crystalline high-melting point hydroxyl-terminated polyester resin

    CN108752572A

  • High-alkali-resistance powder coating and preparation method thereof

    CN115851084A

  • Instantaneous curing reticulated powder coating for metal coiled material and curing process

    CN118440568A