Infrared absorbing particles, infrared absorbing particle dispersion solution, infrared absorbing particle dispersion body, and infrared absorbing laminate

The development of composite oxide-based infrared absorbing particles addresses the inefficiencies in conventional materials by specifically absorbing near-infrared radiation in the 1400 nm to 2100 nm range, enhancing thermal comfort by blocking heat-causing wavelengths while maintaining visible light transparency.

WO2024204328A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO METAL MINING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012227
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional materials for blocking near-infrared rays, such as those used in window applications, lack optimal infrared absorption characteristics, particularly in the 1400 nm to 2100 nm wavelength range, which affects indoor thermal comfort by allowing heat-causing infrared radiation to penetrate.

Method used

Development of novel infrared absorbing particles comprising a composite oxide with specific elemental compositions, including H, Mg, V, Nb, and Ta, which are designed to absorb near-infrared radiation effectively while being transparent in the visible light range, utilizing a specific range of composition ratios and crystal structures to enhance infrared absorption.

Benefits of technology

The novel infrared absorbing particles effectively block heat-causing infrared radiation in the 1400 nm to 2100 nm range, maintaining visible light transparency and providing improved thermal comfort by reducing indoor temperature rises.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012227_03102024_PF_FP_ABST
    Figure JP2024012227_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Infrared absorbing particles each containing a composite oxide, wherein the composite oxide contains an A1 element comprising at least one element selected from H and an alkali metal, an A2 element comprising at least one element selected from Mg and an alkaline earth metal, and a B element comprising at least one element selected from V, Nb and Ta, and the relationships represented by the formulae: 0.002 ≤ (x1+x2) / y ≤ 1.5, 0.001 ≤ x1 / y ≤ 1 and 0.001 ≤ x2 / y ≤ 1 are satisfied when the physical amounts of the A1 element, the A2 element and the B element contained in the composite oxide are x1, x2 and y, respectively.
Need to check novelty before this filing date? Find Prior Art

Description

Infrared absorbing particles, infrared absorbing particle dispersion, infrared absorbing particle dispersion, infrared absorbing laminate

[0001] The present invention relates to infrared absorbing particles, an infrared absorbing particle dispersion, an infrared absorbing particle dispersion, and an infrared absorbing laminate.

[0002] Near-infrared rays contained in sunlight penetrate window materials and enter indoor spaces, raising the surface temperatures of the walls and floors, and thus the indoor air temperature. To maintain a comfortable indoor thermal environment, conventional methods have been to use shading materials in window materials and the like to block the near-infrared rays that enter through windows, thereby preventing the indoor air temperature from rising.

[0003] Patent Document 1 proposes a light-shielding film containing black fine powder including inorganic pigments such as carbon black and titanium black, and organic pigments such as aniline black, as a light-shielding material used in window materials and the like.

[0004] Patent Document 2 discloses a thermal insulation sheet made of a woven fabric in which a strip-shaped film having infrared reflectivity and a strip-shaped film having infrared absorbency are used as warp and weft, respectively. It also describes the use of a synthetic resin film that has been subjected to aluminum vapor deposition processing and further laminated with another synthetic resin film as the infrared reflectivity strip-shaped film.

[0005] In Patent Document 3, the present applicant proposed an infrared-shielding material microparticle dispersion in which infrared material microparticles are dispersed in a medium, the infrared material microparticles containing tungsten oxide microparticles and / or composite tungsten oxide microparticles, and the dispersed particle diameter of the infrared material microparticles is 1 nm or more and 800 nm or less.

[0006] Japanese Unexamined Patent Publication No. 2003-029314 Japanese Unexamined Patent Publication No. 9-107815 International Publication No. 2005 / 037932

[0007] Meanwhile, new infrared absorbing particles having optical properties different from those of conventional materials are being sought, so that the optimum material can be selected depending on the application.

[0008] Therefore, one aspect of the present invention aims to provide novel infrared absorbing particles.

[0009] One aspect of the present invention provides infrared absorbing particles containing a composite oxide, the composite oxide containing: an A1 element which is one or more elements selected from H and alkali metals; an A2 element which is one or more elements selected from Mg and alkaline earth metals; and a B element which is one or more elements selected from V, Nb, and Ta, wherein, when the amount of substance of the A1 element contained in the composite oxide is x1, the amount of substance of the A2 element is x2, and the amount of substance of the B element contained in the composite oxide is y, the infrared absorbing particles satisfy the relationships 0.002≦(x1+x2) / y≦1.5, 0.001≦x1 / y≦1, and 0.001≦x2 / y≦1.

[0010] In one aspect of the present invention, novel infrared absorbing particles can be provided.

[0011] Fig. 1 is a schematic diagram of a composite material production apparatus that can be suitably used when producing infrared absorbing particles using aerosol spraying. Fig. 2 is an explanatory diagram of a reduction treatment apparatus used in the reduction treatment step. Fig. 3 is a schematic diagram of an infrared absorbing particle dispersion. Fig. 4 is a schematic diagram of an infrared absorbing particle dispersion. Fig. 5 is a schematic diagram of an infrared absorbing substrate. Fig. 6 is a schematic diagram of an infrared absorbing laminate. Fig. 7 is a graph of the transmitted light profile of the infrared absorbing particle dispersion according to Example 1, Example 2, and Reference Example 2.

[0012]

[0023] Hereinafter, [1] infrared absorbing particles, [2] a method for producing infrared absorbing particles, [3] infrared absorbing particle dispersion, [4] infrared absorbing particle dispersion, and [5] infrared absorbing laminate will be described in detail in this order. [1] Infrared absorbing particles The inventors of the present invention have conducted studies on novel infrared absorbing particles. The infrared absorbing particles according to the present invention are more preferably near-infrared absorbing particles that absorb, in particular, near-infrared light within the infrared region.

[0013] In investigating new infrared absorbing particles, the inventors of the present invention focused on oxides of Group 5 elements. However, the pentoxides of Group 5 elements (V 2 O 5 , Nb 2 O 5, Ta 2 O 5 Since there are no effective free electrons or holes in the oxide, it has little absorption / reflection characteristics in the infrared region and is therefore not effective as an infrared absorbing material. However, when a cathode element is added to the above oxide to form a composite oxide, free electrons or holes are generated in the composite oxide, and absorption characteristics derived from the free electrons or holes are exhibited in the infrared region. Therefore, it has been discovered that new infrared absorbing particles can be produced.

[0014] Furthermore, the inventors of the present invention have found that there is a specific range within the composition range of the complex oxide that is particularly effective as an infrared absorbing particle. Specifically, they have found that by setting the composition range of the complex oxide within a specific range, the complex oxide is transparent in the visible light region and absorbs in the infrared region.

[0015] The inventors of the present invention further pursued extensive research and discovered that by controlling the composition of the composite oxide within a specific range, it is possible to impart strong absorption to light wavelengths in the infrared region that cause a burning sensation on human skin. It is believed that the burning sensation felt on skin from sunlight (the so-called burning sensation) is largely due to the influence of infrared rays with wavelengths of 1500 nm or more and 2100 nm or less (see, for example, Yoshikazu Ozeki et al., Society of Automotive Engineers of Japan, Inc., Preprint Collection, No. 33-99, 13 (1999)). Therefore, in order for infrared-absorbing particles to absorb light wavelengths that cause a burning sensation on human skin and reduce their transmittance, it is preferable, from the perspective of practicality, that the infrared-absorbing particles reduce or block infrared rays in the wavelength region from around 1400 nm to 2100 nm or less.

[0016] Therefore, by providing a light absorption peak in the wavelength range of 1400 nm or more and 2100 nm or less, infrared absorbing particles can be produced that are transparent in the visible light range, but have high absorption of light wavelengths that cause a burning sensation on human skin, even in the infrared range.

[0017] On the other hand, infrared absorbing particles that are transparent in the visible light region and have a light absorption peak in the wavelength region of 1400 nm or more and 2100 nm or less have not been known up to now.

[0018] In other words, the inventors have found that by providing a light absorption peak in the wavelength region of 1400 nm or more and 2100 nm or less, it is possible to produce novel infrared absorbing particles having optical properties different from those of conventional materials, and have completed the present invention. (Composition of the composite oxide) The infrared absorbing particles of this embodiment can contain a composite oxide.

[0019] The composite oxide contained in the infrared absorbing particles of this embodiment can contain the following A1 element, A2 element, and B element.

[0020] The A1 element is one or more elements selected from H (hydrogen) and alkali metals.

[0021] The A2 element is one or more elements selected from Mg (magnesium) and alkaline earth metals.

[0022] The B element is one or more elements selected from V (vanadium), Nb (niobium), and Ta (tantalum).

[0023] When the amount of substance of the A1 element contained in the composite oxide is x1, the amount of substance of the A2 element is x2, and the amount of substance of the B element is y, it is preferable that the following relationships are satisfied: 0.002≦(x1+x2) / y≦1.5, 0.001≦x1 / y≦1, and 0.001≦x2 / y≦1.

[0024] The infrared absorbing particles of the present embodiment may be composed only of the composite oxide, but even in this case, this does not exclude the case where the infrared absorbing particles of the present embodiment contain inevitable impurities that are mixed in during the manufacturing process, etc.

[0025] As described above, by adding electropositive elements A1 and A2 to an oxide containing B element to form the composite oxide, infrared absorption properties can be exhibited.

[0026] Furthermore, by simultaneously adding the A1 element and the A2 element to an oxide containing the B element and adjusting the composition within a predetermined range, the infrared absorbing particles containing the composite oxide can have a light absorption peak in the wavelength region of 1400 nm or more and 2100 nm or less. This is thought to be because, when the composition of the A1 element and the A2 element is within the predetermined range, free electrons or holes are generated at a density suitable for having a light absorption peak in the wavelength region of 1400 nm or more and 2100 nm or less.

[0027] As described above, the A1 element is preferably one or more elements selected from H and alkali metals. In this specification, alkali metals refer to Li (lithium), Na (sodium), K (potassium), Rb (rubidium), Cs (cesium), and Fr (francium).

[0028] In particular, from the viewpoint of improving the stability of the composite oxide, the A1 element is preferably one or more elements selected from H, Li, Na, K, Rb, and Cs, and more preferably one or more elements selected from Na and K.

[0029] As described above, the element A2 is preferably one or more elements selected from Mg and alkaline earth metals, which in this specification mean calcium (Ca), strontium (Sr), barium (Ba), and radium (Ra).

[0030] In particular, from the viewpoint of improving the stability of the composite oxide, the A2 element is preferably one or more elements selected from alkaline earth metals, and more preferably one or more elements selected from Ca, Sr, and Ba.

[0031] Furthermore, as described above, the B element can be one or more elements selected from V, Nb, and Ta, and is preferably one or more elements selected from Nb and Ta, and more preferably Nb.

[0032] By setting the value of (x1 + x2) / y, which indicates the content ratio of the total amount of the A1 element and the A2 element to the B element in the composite oxide, to 0.002 or more, a sufficient amount of free electrons or holes is generated in the composite oxide, thereby achieving the desired infrared absorption effect. The higher the content of the A1 element and the A2 element, the greater the supply of free electrons and the higher the infrared absorption efficiency, but this effect saturates when the value of (x1 + x2) / y is about 1.5. Furthermore, if the value of (x1 + x2) / y is 1.5 or less, the generation of an impurity phase in the infrared absorbing particles can be avoided. Therefore, as described above, (x1 + x2) / y is preferably 0.002≦(x1 + x2) / y≦1.5, more preferably 0.5≦(x1 + x2) / y≦1.0, even more preferably 0.7≦(x1 + x2) / y≦1.0, and particularly preferably 0.8≦(x1 + x2) / y≦1.0. Furthermore, x1 preferably satisfies 0.1≦x1 / y≦0.8, and x2 preferably satisfies 0.2≦x2 / y≦0.9.

[0033] The composite oxide may be, for example, a compound represented by the general formula A1 x1 A2 x2 B y O z In the general formula, "A1" represents the A1 element, "A2" represents the A2 element, "B" represents the B element, and "O" represents oxygen. As shown in the general formula, the composite oxide is preferably composed of, for example, the A1 element, the A2 element, the B element, and oxygen.

[0034] By adding the A1 element and the A2 element to an oxide containing the B element, free electrons or holes are supplied to the composite oxide, thereby enabling the composite oxide to exhibit infrared absorption properties. Therefore, the amount of oxygen contained in the composite oxide is not particularly limited. However, by setting the oxygen amount within a predetermined range, the amount of free electrons or holes in the composite oxide can be set to a particularly suitable range from the viewpoint of improving infrared absorption properties. Therefore, z / y, which corresponds to the content ratio of oxygen to B element in terms of substance amount in the composite oxide, is preferably 1.0 < z / y < 3.5, more preferably 2.0 < z / y < 3.5, even more preferably 2.0 < z / y ≦ 3.0, and most preferably 2.4 ≦ z / y ≦ 3.0. Note that z corresponds to the substance amount of oxygen contained in the composite oxide.

[0035] As described above, z / y corresponds to the content ratio of oxygen relative to the amount of B in the composite oxide, and is a value that affects the amount of oxygen deficiency or excess oxygen in the composite oxide. As described above, the amount of free electrons or holes in the composite oxide can also be controlled by the amount of oxygen. Therefore, it is preferable to control the value of z / y according to the required infrared absorption characteristics, etc. The value of z / y can be easily controlled by the synthesis conditions of the infrared absorbing particles, etc.

[0036] The above general formula A1 x1 A2 x2 B y O z Preferably, x1, x2, y, and z satisfy the relationship 0<(x1+2x2+5y-2z) / y≦3, more preferably 0<(x1+2x2+5y-2z) / y≦2, and even more preferably 0.1≦(x1+2x2+5y-2z) / y≦1. The above (x1+2x2+5y-2z) / y indicates a guideline for the excess or deficiency of electrons per B element, and when the above range is satisfied, a particularly high infrared absorption effect can be exhibited. (Regarding the Crystal Structure and Lattice Constant of the Complex Oxide) According to studies by the inventors of the present invention, when a complex oxide has a crystal structure selected from cubic, tetragonal, and orthorhombic (rectangular), light transmission in the visible light region is improved and light absorption in the infrared region is improved.

[0037] For this reason, the crystalline structure of the composite oxide is preferably any one selected from cubic, tetragonal, and orthorhombic crystals. By making the crystalline structure of the composite oxide any one selected from cubic, tetragonal, and orthorhombic crystals, the transmittance of light in the visible light region of the infrared absorbing particles is improved, and the absorption of light in the infrared region is improved.

[0038] The composite oxide may have a cubic or orthorhombic crystal structure. By selecting either a cubic or orthorhombic crystal structure as the composite oxide, the infrared absorbing particles are particularly improved in terms of light transmission in the visible light region and absorption of light in the infrared region.

[0039] However, in order to obtain the effect of improving light transmission in the visible light region and improving light absorption in the infrared region, it is sufficient that the complex oxide contains a unit structure of a cubic, tetragonal, or orthorhombic crystal structure, and the complex oxide may partially contain amorphous or other structures.

[0040] In the composite oxide, (x1+x2) / y, which indicates the content ratio of the total amount of substance of the A1 element and the A2 element to the B element, is 1.0, and z / y, which indicates the content ratio of the amount of substance of oxygen to the B element, is 3.0. In this case, the crystalline structure of the composite oxide may be a cubic perovskite structure. Specifically, for example, Na 0.5 Sr 0.5 NbO 3 , K. 0.5 Ba 0.5 NbO 3 etc. may have a cubic perovskite structure.

[0041] A complex oxide having a basic structure of (x1+x2) / y=1.0 and z / y=3.0, where the value of (x1+x2) / y is less than 1.0, may have a cubic perovskite structure with deficiencies in one or more elements selected from the A1 element and the A2 element. Also, a complex oxide having a z / y value of less than 3.0 may have a cubic perovskite structure with oxygen deficiencies. Furthermore, depending on the deficiency state of each element, the complex oxide may have a structure such as (A1, A2)BO 3In some cases, the crystalline structure is a tetragonal, orthorhombic, or monoclinic structure in which the B O blocks and the B O blocks are regularly stacked. In addition, a composite oxide having a z / y value of more than 3.0 and less than 3.5 may have a cubic, tetragonal, or orthorhombic crystalline structure.

[0042] As infrared absorbing particles, materials that have high infrared absorption in the infrared region and low visible light absorption in the visible region are often required. However, since the required performance differs depending on the application, it is not possible to determine in general which of the above-mentioned crystal structures is preferable.

[0043] For example, the composite oxide is Na x1 Sr x2 NbO z In the case of (2.0<z≦3.0), for example, when the value of (x1+x2) is 0.8 or more and less than 1.0, a cubic perovskite structure having deficiencies of Na and Sr elements and, in some cases, oxygen deficiencies may be formed. x1 Sr x2 NbO z (2.0<z≦3.0), (Na,Sr)NbO 3 In some cases, the NbO and NbO blocks are regularly stacked to form a tetragonal or orthorhombic crystal structure. Composite oxides with the above composition and crystal structure tend to have high heat-shielding properties, which are important for window materials and the like. The heat-shielding properties refer to properties determined by the balance between visible light transparency and near-infrared absorption.

[0044] As described above, the relationship between the crystal structure and the infrared absorption characteristics changes depending on the composition of the complex oxide, and therefore the crystal structure of the complex oxide contained in the infrared absorbing particles of this embodiment is not particularly limited, and can be selected depending on the composition of the complex oxide, the required infrared absorption characteristics, etc.

[0045] The lattice constant of the composite oxide is not particularly limited, but when the cubic perovskite structure is used as a reference, the lattice constant of the a-axis is preferably 3.93 Å or more and 4.14 Å or less, more preferably 3.97 Å or more and 4.14 Å or less, and even more preferably 3.98 Å or more and 4.13 Å or less. The lattice constant can be calculated by Rietveld analysis.

[0046] In addition, when the crystal structure is not cubic (i.e., when it is tetragonal, orthorhombic (rectangular), etc.), the lattice constant of the a-axis when the cubic perovskite structure is used as a reference (hereinafter, may be referred to as a "pseudo-cubic lattice constant") can be converted from the value of the lattice constant in the crystal structure. Specifically, the composition of the unit cell of the non-cubic crystal structure is identified. Then, the unit cell volume is calculated based on the lattice constant. Next, the unit cell volume per atom of the B element is calculated. By taking the cube root of the calculated unit cell volume per atom of the B element, it can be converted to a pseudo-cubic lattice constant. (Regarding Particle Characteristics of Infrared Absorbing Particles) The particle characteristics such as particle diameter of the infrared absorbing particles of this embodiment are not particularly limited and can be selected arbitrarily depending on the required infrared absorption characteristics, etc.

[0047] The infrared absorbing particles of this embodiment preferably have a volume-based cumulative 50% particle size of 1 nm or more and 50 nm or less, and a cumulative 90% particle size of 5 nm or more and 100 nm or less, as measured by a particle size distribution measuring device.

[0048] It is generally known that materials containing free electrons or holes exhibit a reflection-absorption response to infrared rays around the solar radiation wavelength range of 200 nm to 2600 nm due to plasma oscillation. It is also known that when powder particles of such materials are made smaller than the wavelength of light, geometric scattering in the visible light range (wavelengths of 380 nm to 780 nm) is reduced, resulting in transparency in the visible light range.

[0049] In this specification, the term "transparency" is used to mean "high transmittance with little scattering of light in the visible light range."

[0050] Therefore, when the infrared absorbing particles of this embodiment are used in an application requiring transparency in the visible light region, it is preferable that the volume-based cumulative 90% particle diameter measured by a particle size distribution measuring device is 100 nm or less. This is because particles having a cumulative 90% particle diameter of 100 nm or less do not completely block light due to scattering, and can maintain visibility in the visible light region while efficiently maintaining transparency. In particular, when transparency in the visible light region is important, it is preferable to further consider scattering by the particles.

[0051] When further reduction in scattering by the infrared-absorbing particles is required, the cumulative 90% particle diameter is more preferably 70 nm or less, and even more preferably 60 nm or less. If the particle diameter of the infrared-absorbing particles is small, scattering of light in the visible light region with wavelengths of 380 nm or more and 780 nm or less due to geometric scattering or Mie scattering is reduced. Therefore, by setting the cumulative 90% particle diameter of the infrared-absorbing particles within the above range, it is possible to more reliably prevent, for example, an infrared-absorbing particle dispersion using the infrared-absorbing particles from becoming like frosted glass and losing clear transparency. When the cumulative 90% particle diameter is 70 nm or less, the geometric scattering or Mie scattering is reduced, and the Rayleigh scattering region is reached. In the Rayleigh scattering region, scattered light is proportional to the sixth power of the particle diameter, so scattering is reduced and transparency is improved as the particle diameter decreases.

[0052] Furthermore, if the cumulative 90% particle diameter is 60 nm or less, scattered light becomes very small, which is preferable. From the viewpoint of avoiding light scattering, a smaller cumulative 90% particle diameter is preferable, and therefore, although the lower limit of the cumulative 90% particle diameter is not particularly limited, the cumulative 90% particle diameter is preferably 5 nm or more. This is because a cumulative 90% particle diameter of 5 nm or more facilitates industrial production.

[0053] As described above, by setting the cumulative 90% particle size to 100 nm or less, for example, the haze of an infrared absorbing particle dispersion in which the infrared absorbing particles of this embodiment are dispersed in a solid medium can be set to 30% or less at a visible light transmittance of 85% or less. By setting the haze to 30% or less, particularly clear transparency can be obtained.

[0054] From the viewpoint of obtaining particularly excellent infrared absorption properties, the cumulative 50% particle diameter of the infrared absorbing particles on a volume basis measured by a particle size distribution measuring device is preferably 1 nm or more, but from the viewpoint of enhancing transparency in the visible light region, the cumulative 50% particle diameter is preferably 50 nm or less for the same reason as for the cumulative 90% particle diameter.

[0055] The volume-based cumulative 50% particle size and cumulative 90% particle size of the infrared absorbing particles can be measured using a particle size distribution measuring device (e.g., UPA-150 manufactured by Nikkiso Co., Ltd.) based on the principle of dynamic light scattering method using frequency analysis.

[0056] Particle size distribution data is expressed as cumulative % or frequency % on a particle size scale, but conversely, it can also be expressed as particle diameter on a cumulative % scale. For example, the particle diameter at the point where a distribution curve expressed as particle diameter on a cumulative % scale intersects the horizontal axis at 10% is called the cumulative 10% particle diameter, and the particle diameter at the point where it intersects the horizontal axis at 50% is called the cumulative 50% particle diameter. Furthermore, the particle diameter at the point where it intersects the horizontal axis at 90% is called the cumulative 90% particle diameter. It is not specifically fixed to 10%, 50%, or 90%, and any cumulative % can be used as needed. The 50% particle diameter is also called the median diameter and is very commonly used. When comparing the particle size distributions of multiple samples, this median diameter is often used because it is necessary to represent the size of the object being measured with a single number. For this reason, the median diameter is often confused with the average particle size, but the definitions are different and the two diameters usually do not coincide. These two diameters will match only when the particle size distribution is symmetrical with respect to the center (50% diameter). [2] Manufacturing method of infrared absorbing particles Next, a manufacturing method of infrared absorbing particles of this embodiment will be described. Since the manufacturing method of infrared absorbing particles of this embodiment can manufacture the infrared absorbing particles already described, some of the matters already described will not be described again.

[0057] The method for producing the infrared absorbing particles of this embodiment is not particularly limited, and they can be produced, for example, by [2-1] solid-phase reaction method or [2-2] production method using aerosol spraying. Each production method will be described below. [2-1] Solid-phase reaction method When synthesizing by the solid-phase reaction method, for example, an A1 element compound or an A1 element simple substance as an A1 element source, an A2 element compound or an A2 element simple substance as an A2 element source, and a B element compound or an B element simple substance as a B element source can be used as raw materials.

[0058] The method for producing infrared absorbing particles of this embodiment may include a mixed powder preparation step (first mixed powder preparation step) of preparing a mixed powder of an A1 element source, an A2 element source, and a B element source.

[0059] The Al element source can be one or more selected from Al element compounds and simple Al element compounds. The Al element compound used as a raw material is preferably one or more selected from oxides, hydroxides, carbonates, nitrates, sulfates, oxalates, organic compounds, sulfides, and chlorides of the Al element.

[0060] The A2 element source can be one or more selected from A2 element compounds and simple A2 elements. The A2 element compound used as a raw material is preferably one or more selected from oxides, hydroxides, carbonates, nitrates, sulfates, oxalates, organic compounds, sulfides, and chlorides of the A2 element.

[0061] Since the preferred A1 and A2 elements have already been explained, the explanation will be omitted here.

[0062] As the B element source, one or more selected from B element compounds and simple B elements can be used. As the B element compound or simple B element source, B element pentoxide (V 2 O 5 , Nb 2 O 5 , Ta 2 O 5 ), dioxide (VO 2 , NbO 2 , TaO 2 ), sesquioxide (V 2 O 3 , Nb 2 O 3 ), elemental metals (V, Nb, Ta), sulfates, ammonium salts, organic compounds, sulfides, chlorides, and hydrates of oxides obtained by dissolving chlorides in a liquid such as alcohol, adding water to hydrolyze the chlorides, and evaporating the solvent. Note that the preferred B element has already been described, and therefore further description will be omitted here.

[0063] In the mixed powder preparation step, the specific procedure for obtaining a mixed powder of an A1 element compound or an A1 element simple substance, an A2 element compound or an A2 element simple substance, and a B element compound or an B element simple substance is not particularly limited. For example, a method can be used in which the A1 element compound or the like serving as the A1 element source, the A2 element compound or the like serving as the A2 element source, and the B element compound or the like serving as the B element source are dry-mixed in powder form to obtain a mixed powder. Alternatively, the A1 element compound or the like serving as the A1 element source can be dissolved in water, wet-mixed with the A2 element compound or the like serving as the A2 element source and the B element compound or the like serving as the B element source, and then dried to obtain a mixed powder.

[0064] In the mixed powder preparation step, it is preferable to mix the elements A1, A2, and B so that the ratio of the amounts of substance of the elements A1, A2, and B in the resulting mixed powder is the same as the ratio of the elements A1, A2, and B in the target composite oxide. That is, it is preferable to mix the elements so that the ratio of the total amount of substance of the elements A1 and A2 (A1 + A2) to the amount of substance of the element B (B) in the target composite oxide satisfies (A1 + A2):B = (x1 + x2):y. As described above, with respect to x1, x2, and y, it is preferable that (x1 + x2) / y satisfies 0.002≦(x1 + x2) / y≦1.5, more preferably 0.5≦(x1 + x2) / y≦1.0, even more preferably 0.7≦(x1 + x2) / y≦1.0, and particularly preferably 0.8≦(x1 + x2) / y≦1.0. Therefore, it is preferable to mix the A1 element compound, the A2 element compound, and the B element compound so as to fall within the above-mentioned preferred range.

[0065] The infrared absorbing particles of this embodiment can also be synthesized in multiple stages to obtain infrared absorbing particles containing a composite oxide of the target composition. In this case, in the first mixed powder preparation step, the A1 element compound or the like serving as the A1 element source, the A2 element compound or the like serving as the A2 element source, and the B element compound or the like serving as the B element source can be mixed to obtain the composition of the intermediate product. When synthesizing the infrared absorbing particles of this embodiment in multiple stages, for example, in the first mixed powder preparation step or the like, a mixture may be prepared using only raw materials for two element sources selected from the A1 element source, the A2 element source, and the B element source. In this case, after the first firing step, an intermediate product containing two elements selected from the A1 element, the A2 element, and the B element is produced.

[0066] The method for producing infrared absorbing particles of this embodiment may include a firing step (first firing step) of firing the mixed powder obtained in the mixed powder preparation step (first mixed powder preparation step).

[0067] The conditions for the firing step are not particularly limited. In the firing step, for example, the mixed powder can be fired in any atmosphere selected from an inert gas atmosphere, a reducing gas atmosphere, a vacuum atmosphere, a mixed gas atmosphere of an inert gas and a reducing gas, and an oxidizing atmosphere containing oxygen.

[0068] For example, when oxygen vacancies are introduced into a composite oxide to make z / y in the general formula smaller than the stoichiometric ratio, the firing atmosphere is preferably a mixed gas atmosphere of an inert gas and a reducing gas. The reducing gas is not particularly limited, but is preferably, for example, hydrogen gas. Furthermore, when hydrogen gas is used as the reducing gas, the volume ratio of hydrogen gas is preferably 1% or more, more preferably 3% or more. There is no particular upper limit to the volume ratio of hydrogen gas, and since the reducing gas can be used alone, it can be up to 100%.

[0069] The inert gas is not particularly limited, but one or more types selected from nitrogen gas, rare gases, and the like can be used.

[0070] The oxidizing atmosphere may be any atmosphere containing oxygen, for example, an atmosphere containing 18% to 100% oxygen by volume, such as air.

[0071] The firing temperature in the firing step is not particularly limited, but the firing temperature is preferably equal to or higher than the temperature at which the produced composite oxide begins to crystallize and equal to or lower than the melting point of the composite oxide. Specifically, the firing temperature is preferably 1000°C or higher and 2100°C or lower.

[0072] The infrared absorbing particles of this embodiment can be synthesized in multiple stages to obtain infrared absorbing particles containing a composite oxide of the target composition. When synthesizing in multiple stages, for example, a B element compound or a simple B element, which is a B element source, can be further added and mixed with the intermediate product obtained in the above-mentioned firing step (first firing step) (second mixed powder preparation step). It is also possible to prepare multiple types of intermediate products with different compositions and mix them in the second mixed powder preparation step. In this case, it is also possible to further add and mix a B element compound or a simple B element, which is a B element source, as needed. When preparing multiple types of intermediate products with different compositions, the above-mentioned mixed powder preparation step (first mixed powder preparation step) and firing step (first firing step) can be performed for each intermediate product. It is also possible for the intermediate product to contain two elements selected from the A1 element, the A2 element, and the B element, and not to contain any of the three elements. In addition, in the second mixed powder preparation step, an A1 element source or an A2 element source other than the B element source can be added as needed.

[0073] The B element compound used in the second mixed powder preparation step is not particularly limited, but the compounds already described in the first mixed powder preparation step can be used, for example. In the second mixed powder preparation step, it is preferable to mix so that the ratio of the total amount of substance of the A1 element and the A2 element to the amount of substance of the B element in the resulting mixed powder is the ratio of the total amount of substance of the A1 element and the A2 element to the amount of substance of the B element in the target composite oxide. In other words, it is preferable to mix so that the ratio of the total amount of substance of the A1 element and the A2 element (A1 + A2) to the amount of substance of the B element (B) in the target composite oxide satisfies (A1 + A2):B = (x1 + x2):y. Mixing can be performed in the same manner as in the mixed powder preparation step, so a detailed description will be omitted here.

[0074] The obtained mixed powder is then subjected to a firing step (second firing step) to prepare the infrared absorbing particles of this embodiment. The conditions for the second firing step are not particularly limited, but the firing atmosphere and firing temperature can be similar to those described for the firing step (first firing step), and therefore will not be described here. The firing conditions for the first firing step and the second firing step may be the same or different.

[0075] Although the method for producing infrared absorbing particles containing a composite oxide in two steps has been described as an example here, infrared absorbing particles containing a composite oxide can also be produced in n steps, which are three or more steps. In this case, the above description of the second mixed powder preparation step and the second firing step can be read as the nth mixed powder preparation step and the nth firing step.

[0076] The n-th mixed powder preparation step can be supplied with an intermediate product obtained by firing the mixed powder prepared in the (n-1)th mixed powder preparation step in the (n-1)th firing step.

[0077] In the n-1th mixed powder preparation step, the intermediate product obtained in the n-2th firing step is used, and the intermediate product can be mixed with a B element compound or simple B element, which is a B element source, in accordance with the composition of the intermediate product to be supplied to the nth step. Other than the above, the configuration can be the same as the second mixed powder preparation step. Therefore, a description thereof will be omitted. In addition to the B element source, an A1 element source or an A2 element source can also be added in the n-1th mixed powder preparation step as necessary.

[0078] In addition, the (n-1)th firing step can be performed under the same firing conditions as the first firing step and the second firing step, except that the mixed powder prepared in the (n-1)th mixed powder preparation step is used, and therefore the explanation will be omitted. Note that the conditions for each firing step may be the same or different.

[0079] By carrying out the steps described above, the infrared absorbing particles of this embodiment can be obtained. After the firing step is completed, the obtained infrared absorbing particles can be crushed, pulverized, sieved, or the like, as needed, to achieve a desired particle size distribution. [2-2] Manufacturing Method Using Aerosol Spraying Hereinafter, a manufacturing method using aerosol spraying will be described for the infrared absorbing particle manufacturing method of this embodiment. Specifically, the manufacturing method using aerosol spraying is a manufacturing method in which infrared absorbing particles are synthesized through a heat treatment step in which an aerosol of raw materials containing an A1 element source, an A2 element source, and a B element source is supplied to an electric furnace, flame, or plasma. (1) Regarding Each Step of the Manufacturing Method Using Aerosol Spraying Therefore, the manufacturing method of infrared absorbing particles of this embodiment using aerosol spraying can include the following raw material preparation step, aerosol formation step, heat treatment step, and reduction treatment step.

[0080] In the raw material preparation step, a raw material containing an A1 element source, an A2 element source, and a B element source can be prepared.

[0081] In the aerosol forming step, the raw material prepared in the raw material preparing step can be aerosolized.

[0082] In the heat treatment process, the aerosolized raw material can be heat treated in a reaction field.

[0083] In the reduction treatment step, the particles obtained in the heat treatment step can be reduced in an atmosphere containing a reducing gas. (Regarding Each Step) Hereinafter, each step of the method for producing infrared absorbing particles of this embodiment will be described. (1-1) Raw Material Preparation Step In the raw material preparation step, a raw material containing an A1 element source, an A2 element source, and a B element source can be prepared.

[0084] In the raw material preparation step, the raw materials can be blended and prepared so that the ratio of the amount of substance of the A1 element to the amount of substance of the A2 element to the amount of substance of the B element contained in the raw materials corresponds to the desired composition of the infrared absorbing particles.

[0085] The state of the raw material prepared in the raw material preparation step is not particularly limited, and may be liquid or powder, and preferably can be formed into an aerosol by spraying, etc. Here, the aerosol means a mixture of minute liquid or solid particles suspended in a gas and the surrounding gas.

[0086] When the raw material is a liquid, the raw material can be prepared by preparing a solution containing, for example, an A1 element source, an A2 element source, and a B element source.

[0087] Alternatively, a solution containing an A1 element source, a solution containing an A2 element source, and a solution containing a B element source may be prepared in advance, and the two solutions may be mixed in the raw material preparation step to form a raw material mixed solution.

[0088] The raw material may be supplied in the form of droplets to the heat treatment step described below. In this case, a solution containing an A1 element source, a solution containing an A2 element source, and a solution containing a B element source may be mixed together immediately before supplying the raw material to a droplet formation section (droplet formation means) that forms the droplets, or within the droplet formation section, to carry out the raw material preparation step. Then, the aerosol formation step described below can be carried out in the droplet formation section.

[0089] For example, if premixing a solution containing an A1 element source, a solution containing an A2 element source, and a solution containing a B element source poses problems such as gelation, it is preferable to prepare each solution in advance as described above and mix them immediately before the aerosol formation step. When the raw material preparation step is performed immediately before the aerosol formation step, the ratio of the amounts of substance of the A1 element, the A2 element, and the B element in the raw material can be adjusted to a desired range by adjusting the concentrations of both solutions and the speeds at which both solutions are sent to the droplet formation section.

[0090] As described above, when the raw material preparation step is carried out immediately before the aerosol formation step, the aerosol formation step and the raw material preparation step do not need to be clearly separated, and both steps can be carried out continuously.

[0091] As described above, in the raw material preparation step, when a solution containing an A1 element source, a solution containing an A2 element source, and a solution containing a B element source are mixed, the specific method for mixing is not particularly limited, and any method can be used.

[0092] The B element source is not particularly limited, and may be any raw material containing the B element, such as a metal element of the B element or a compound of the B element. As the B element source, a salt of the B element or the like may be used, and for example, an alkoxide compound of the B element may be preferably used. As the alkoxide compound of the B element, for example, an ethoxide compound of the B element may be used. As the ethoxide compound of the B element, for example, B(OEt) 5 , or (C 2 H 5 O) 5 B. As the solution containing the B element source, an organic solution containing the B element source can be preferably used because of ease of handling.

[0093] The A1 element source and the A2 element source are not particularly limited, and may be any raw material containing the A1 element or the A2 element. Examples of the A1 element source include the A1 element alone or a compound containing the A1 element. Examples of the A2 element source include the A2 element alone or a compound containing the A2 element. Examples of the solution containing the A1 element source or the A2 element source include a solution of a salt containing the A1 element or a solution of a salt containing the A2 element. The type of salt containing the A1 element or the A2 element is not particularly limited, and one or more types selected from carbonates, acetates, nitrates, hydroxides, alkoxide compounds, etc. of the A1 element and the A2 element can be used. Examples of the alkoxide compound include ethoxide compounds. The salt of the A1 element and the salt of the A2 element may be the same or different.

[0094] As the solution containing the A1 element source and the solution containing the A2 element source, an organic solution containing the A1 element source and an organic solution containing the A2 element source can be preferably used from the viewpoint of ease of handling.

[0095] The ratio of the A1 element and the A2 element to 1 mole of the B element in the obtained infrared absorbing particles, i.e., the doping amount, is determined by the ratio of the B element source to the A1 element and the A2 element source when forming the raw material mixed solution, and can be controlled, for example, by the concentration of the solution containing the B element source, or the concentrations of the solution containing the A1 element source and the solution containing the A2 element source.

[0096] The concentration of the B element source contained in the solution containing the B element source, i.e., the concentration of a salt of the B element, is not particularly limited. For example, the B element concentration of the solution containing the B element source is preferably 0.001 mol / L or more and 10 mol / L or less, more preferably 0.01 mol / L or more and 10 mol / L or less, and even more preferably 0.01 mol / L or more and 1 mol / L or less. This is because, by setting the B element concentration of the solution containing the B element source to 0.001 mol / L or more, a sufficient amount of infrared-absorbing particles can be produced per unit time, and a sufficient amount can be recovered, for example, using a filter, thereby improving productivity. Furthermore, by setting the B element concentration of the solution containing the B element source to 10 mol / L or less, reprecipitation of the dissolved B element source is suppressed, aggregation of the generated particles is suppressed, and the inclusion of coarse infrared-absorbing particles, for example, having a particle diameter greater than 1 μm, can be suppressed. Furthermore, additives such as a pH adjuster or a surfactant can be added to the solution containing the B element source.

[0097] Furthermore, the concentrations of the A1 element source and the A2 element source contained in the solution containing the A1 element source and the solution containing the A2 element source are not particularly limited, and can be selected depending on the desired composition of the infrared absorbing particles to be produced, the concentration of the B element source contained in the solution containing the B element source, etc.

[0098] Any component other than the solution containing the B element source, the solution containing the A1 element source, and the solution containing the A2 element source can be added to the raw material mixed solution.

[0099] Up to this point, the case where the raw material is a liquid has been described as an example, but the raw material may also be solid, for example, powder. When the raw material is a powder, it can be prepared by mixing, for example, a powder of an A1 element compound, a powder of an A2 element compound, and a powder of a B element compound. Alternatively, for example, a precursor powder obtained by adding a B element compound powder to a solution containing an A1 element source and an A2 element source and stirring the mixture, and then removing the solvent by drying or the like, can be used as the raw material.

[0100] When the raw material is solid, the source of B element is not particularly limited, and salts of B element can be used, and for example, oxides of B element such as niobium oxide, tantalum oxide, and vanadium oxide can be preferably used.

[0101] As the A1 element source, the A2 element source, and the B element source, for example, a powder of a salt containing the A1 element, a powder of a salt containing the A2 element, and a powder of a salt containing the B element can be used, respectively. Regarding the salt containing the A1 element, the salt containing the A2 element, and the salt containing the B element, the type of salt is not particularly limited, and for example, one or more types selected from carbonates, acetates, nitrates, hydroxides, etc. can be used. Note that the type of salt for each element source may be different or the same. (1-2) Aerosol Formation Step In the method for producing infrared absorbing particles of this embodiment, it is preferable to supply the raw material prepared in the raw material preparation step in the form of an aerosol to the heat treatment step. Specifically, it is preferable to transport the aerosol by a carrier gas such as oxygen and subject it to the heat treatment step.

[0102] Therefore, the method for producing infrared absorbing particles of this embodiment may also include an aerosol forming step of converting the raw material into an aerosol containing droplets or particles of the raw material.

[0103] The means and method for forming the aerosol in the aerosol forming step are not particularly limited, and can be selected depending on the state of the raw material, etc.

[0104] When the raw material is a liquid, an aerosol can be formed by spraying the liquid toward a carrier gas using various atomizers such as a centrifugal atomizer or a two-fluid nozzle. Alternatively, droplets can be formed by irradiating the liquid with ultrasound.

[0105] When the raw material is a powder, an aerosol can be formed by a device that disperses the raw material powder and supplies the powder into an airflow. For example, the aerosol can be formed by an aerosol forming device that includes a stirring unit such as a rotating brush or stirring blade, and a powder supply unit that includes a piston or screw feeder that delivers the raw material to the stirring unit. The raw material powder supplied from the powder supply unit is dispersed into particles that make up the powder in the stirring unit, and an aerosol can be generated from the raw material powder by sending each particle into a carrier gas. The stirring unit allows the rotation speed of the brush or stirring blade to be selected so that the raw material powder can be dispersed into particles, and it is preferable to rotate it at high speed.

[0106] When forming droplets dispersed in a gas as an aerosol in the aerosol forming process, the size of the formed droplets is not particularly limited, but the diameter of the droplets is preferably 100 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. By making the diameter of the droplets 100 μm or less, it is possible to prevent the obtained infrared absorbing particles from becoming coarse, and it is possible to obtain infrared absorbing particles on the order of nanometers. Note that the lower limit of the size of the droplets formed in the aerosol forming process is not particularly limited. However, since it is difficult to form excessively small droplets and there is a risk of reduced productivity, it is preferable that the droplet size be, for example, 1 μm or more.

[0107] When solid particles dispersed in a gas as an aerosol are formed in the aerosol formation process, the particle size is not particularly limited, but the particle diameter is preferably 100 μm or less, more preferably 10 μm or less, and even more preferably 3 μm or less. By setting the particle diameter to 100 μm or less, it is possible to more reliably perform heat treatment to the interior of the particles. The particle diameter can be measured in the same manner as the particle diameter of the infrared-absorbing particles described above. (1-3) Heat Treatment Process In the heat treatment process, the aerosolized raw material is heat-treated to process the raw material into particles. The heat treatment only needs to be performed at a temperature of 1000°C or higher, and the configuration of the heat source is not particularly limited. Therefore, the heat treatment process can be performed by a method of guiding the raw material into a flame using a carrier gas, a method of guiding the raw material into a tubular electric furnace, a method of guiding the raw material into plasma, or the like. Whether a flame, an electric furnace, or plasma is used, the heat treatment temperature can be 1000°C or higher. By carrying out heat treatment at 1000° C. or higher, the compounds contained in the raw material are decomposed, and the B element, the A1 element, and the A2 element react with each other to form particles.

[0108] The heat treatment temperature is sufficient as long as it can promote the reaction between the B element, the A1 element, and the A2 element, and therefore may be 1000° C. or higher, preferably 1100° C. or higher, and more preferably 1200° C. or higher. There is no particular upper limit to the heat treatment temperature, but from the viewpoint of suppressing energy consumption, it is preferably 4000° C. or lower.

[0109] In the heat treatment step, a flame can be used as described above, and the raw material can be heat-treated using the flame. By using a flame in the heat treatment step and adjusting the temperature of the flame reaction field, the particle size of the resulting particles can be selected.

[0110] When liquid raw materials are sprayed into a carrier gas to form droplets, and the raw materials are introduced into a flame to synthesize particles, the raw material droplets are transported through the flame by a carrier gas such as oxygen gas. When the raw material droplets are transported into the flame, an organic solvent containing the raw material B, Al, and A2 element sources is combusted, and the solvent is decomposed by the combustion reaction. The heat generated by the combustion reaction contributes to the decomposition reaction of the B, Al, and A2 element sources, and the solvent precipitates during the cooling process in the tail flame of the flame field.

[0111] For example, as described above, the B element source may be an ethoxide compound of the B element, and the A1 element source and the A2 element source may be acetates or ethoxide compounds of the A1 element and the A2 element, and these salts decompose in the heat treatment step.

[0112] When a flame is used in the heat treatment process, the conditions for forming the flame are not particularly limited, but the flame can be formed using, for example, a mixed gas containing oxygen and a hydrocarbon. By forming a flame using a mixed gas containing oxygen and a hydrocarbon, a flame with a stable temperature can be formed, and particles with reduced variation in particle size, etc. can be generated.

[0113] The method for adjusting the flame size and temperature is not particularly limited, but it is preferable to adjust the flow rates of the oxygen and flammable gases such as hydrocarbons in the gas mixture supplied to the flame, while maintaining a flow rate ratio that allows the flammable gas to burn. This is because it is possible to adjust the heat power while ensuring the amount of oxygen necessary for the flammable gas to burn.

[0114] For example, when a flame is formed using a gas mixture containing oxygen and propane, the volumetric ratio of the flow rates of propane and oxygen (burner) in the gas mixture is preferably 5 to 8 parts oxygen per 1 part propane, and the flow rate of propane is preferably in the range of 0.5 to 2 L / min. This is because, when the flow rate of propane is 1, by setting the flow rate of oxygen to 5 or more, combustion of propane, which is a flammable gas, can be sufficiently promoted. However, it is preferable to supply 8 or less parts oxygen per 1 part propane to avoid excessive oxygen supply.

[0115] The heat treatment temperature in the flame reaction field also affects the particle size of the resulting particles.

[0116] This is presumably because the thermal energy in the reaction field, such as a flame, is used to sublimate the generated particles, causing them to burst upon sublimation, resulting in particles with a very fine particle size.

[0117] The particles obtained after the heat treatment can be collected, for example, using a filter.

[0118] In the particle synthesis process using aerosol spraying, the raw material prepared in the raw material preparation step may not have the same composition as the particles recovered after heat treatment. Specifically, for example, the ratio of the amounts of the A1, A2, and B elements in the raw material may not match the ratio of the amounts of the A1, A2, and B elements in the constituent materials of the particles recovered after heat treatment. Examples of raw materials prepared in the raw material preparation step include a solution containing an A1 element source, a solution containing an A2 element source, and a solution containing a B element source. This is thought to be because some of the A1 and A2 elements pass through the recovery filter before fully coagulating as a solid after heat treatment, i.e., in the form of vapor, etc., resulting in a loss of some elements in the raw material, and therefore not being contained in the particles recovered by the filter. Therefore, in the raw material preparation step, the raw material may be prepared in anticipation of the loss of one or more elements selected from the A1 and A2 elements in the heat treatment step. Specifically, in the raw material preparation step, the raw material can be prepared so that the ratio of the amount of substance of one or more elements selected from the A1 element and the A2 element to the B element is in excess of the target stoichiometric composition. (1-4) Reduction Treatment Step Particles obtained through the heat treatment step may not exhibit infrared absorption properties. Therefore, the inventors of the present invention conducted an investigation and found that the particles can exhibit infrared absorption properties by further performing a reduction treatment step in which a reduction treatment is performed on the particles obtained through the heat treatment step.

[0119] Therefore, the method for producing infrared absorbing particles of this embodiment may also include a reduction treatment step of reducing the particles obtained in the heat treatment step under an atmosphere containing a reducing gas. Specifically, for example, the method for producing infrared absorbing particles of this embodiment may include a reduction treatment step of reducing the particles obtained in the heat treatment step under an atmosphere containing a reducing gas at a temperature in the range of 1000°C or higher and 1700°C or lower.

[0120] The conditions for the reduction treatment are not particularly limited, but it is preferable to select the conditions for the reduction treatment so that when the infrared absorbing particles after the reduction treatment are analyzed by an X-ray diffraction pattern, a desired crystal structure is synthesized and undesired heterophases are not precipitated. Examples of heterophases include a simple substance of the B element, or an oxide of the B element that does not contain one or more elements selected from the A1 element and the A2 element (for example, a compound represented by the chemical formula B 2 O 5 and oxides represented by the chemical formula BO 2 and oxides represented by the formula:

[0121] In the reduction treatment step, the particles obtained in the heat treatment step can be reduced by increasing and decreasing the temperature in a reducing atmosphere containing a reducing gas, that is, by performing heat treatment.

[0122] During the reduction treatment step, the particles may be stirred or left to stand, and the handling of the particles during the reduction treatment step can be selected as appropriate, but it is preferable to select handling conditions so that the metallic B element does not precipitate.

[0123] The temperature of the reduction treatment (reduction treatment temperature) is preferably 1000°C or higher, more preferably 1100°C or higher, and even more preferably 1200°C or higher.

[0124] The upper limit of the temperature of the reduction treatment is not particularly limited, but is preferably 1700°C or less, more preferably 1600°C or less, and even more preferably 1400°C or less.

[0125] In the case where the raw material is a liquid, the particle size obtained in the aerosol formation step decreases when the raw material concentration is reduced. Since smaller particles are easier to reduce, the temperature in the reduction treatment step can be lowered compared to when the particle size is large. In the reduction treatment step, the temperature can be raised from room temperature to the reduction treatment temperature and then lowered back to room temperature.

[0126] The reduction conditions can be determined based on the optical properties of the infrared absorbing particles to be obtained.

[0127] By setting the temperature of the reduction treatment to 1000° C. or higher, the reduction treatment of the infrared absorbing particles can be advanced, and the infrared absorbing properties can be more reliably exhibited. Furthermore, by setting the temperature to 1700° C. or lower, the B element contained in the infrared absorbing particles can be prevented from being reduced to a simple metal.

[0128] The reducing atmosphere is a mixture of an inert gas such as argon and H 2 It is preferable to use a mixed gas atmosphere with a reducing gas such as H 2 Gas is preferred.

[0129] H as a reducing gas 2 When gas is used, H in a reducing atmosphere 2 The gas content can be appropriately selected. 2 The gas content is preferably in the range of 0.1% to 100% by volume, more preferably 2% to 50% by volume.

[0130] The reduction treatment step time is preferably 60 minutes or more, including the total time from temperature increase to temperature decrease. There is no particular upper limit to the reduction treatment step time, and it is preferable to select the time by conducting a preliminary test or the like so that the reduction does not proceed excessively. Note that the total time from temperature increase to temperature decrease here means the time from starting temperature increase from room temperature, reaching the reduction treatment temperature, and cooling to room temperature. Note that it is preferable that the infrared absorbing particles are placed in the reducing atmosphere described above during this time.

[0131] By carrying out the reduction treatment step in this way, it is possible to convert an unintended heterogeneous phase into the desired crystalline phase in the infrared absorbing particles obtained after the heat treatment step. (2) Apparatus that can be suitably used in the manufacturing method using aerosol spraying (2-1) Composite material manufacturing apparatus An example of the configuration of a composite material manufacturing apparatus that can be suitably used in the manufacturing method of infrared absorbing particles when aerosol spraying is used will be described below.

[0132] FIG. 1 is a diagram schematically illustrating a composite material manufacturing apparatus 10 according to the present embodiment.

[0133] The composite material manufacturing apparatus 10 has a storage section 11 containing a raw material solution, a two-fluid nozzle 12 that forms droplets of the raw material and also forms a flame, and a reaction tube 13 connected to a filter 14 that collects the formed infrared absorbing particles. As already explained, the raw material solution may be a solution containing an A1 element source, an A2 element source, and a B element source.

[0134] A raw material solution and a carrier gas are supplied to the two-fluid nozzle 12 to form an aerosol (aerosol formation process). For example, oxygen and a hydrocarbon are supplied to the two-fluid nozzle 12, which together form a flame reaction field. The formed aerosol can be supplied into the flame and subjected to heat treatment (heat treatment process). A cooling water pipe 131 is arranged around the reaction tube 13, and cooling water is circulated through the pipe. The infrared absorbing particles introduced into the reaction tube 13 are collected by a filter 14, such as a bag filter.

[0135] In addition, an ejector 15 may be provided at the most downstream side to adjust the supply amount of carrier gas.

[0136] Here, an example of the configuration of a composite material apparatus in which droplets of raw material are formed and heat-treated using a flame to form infrared absorbing particles is shown, but the present invention is not limited to this configuration, and the raw material may be a powder or the like, and the heat source used for the heat treatment may be an electric furnace or the like. (2-2) Reduction Treatment Apparatus The reduction treatment apparatus can carry out the reduction treatment step described above.

[0137] The reduction treatment device is not particularly limited as long as it is configured to be able to carry out the reduction treatment step described above, and may include, for example, a container for storing the infrared absorbing particles obtained by the composite material production apparatus described above, a gas pipe for supplying a mixed gas that forms a reducing atmosphere into the container, and a heat source for heating the container.

[0138] It is also possible to introduce a mixed gas that forms a reducing atmosphere into the container and then exhaust it, and place the infrared absorbing particles that are the objects to be treated under a gas flow of the mixed gas. In this case, a supply pipe for the mixed gas and an exhaust pipe can be provided as gas pipes so that such a gas flow can be formed.

[0139] Furthermore, a stirring blade or the like may be used in combination to stir the infrared absorbing particles in the container.

[0140] FIG. 2 is a diagram showing a schematic configuration example of a reduction treatment device, and shows a cross section taken along a plane passing through the central axis of a reaction tube 21 of a reduction treatment device 20.

[0141] The reduction treatment device 20 is a horizontal tubular furnace, and can be used by attaching a gas inlet pipe (not shown) to one opening 21A of the reaction tube 21 and a gas exhaust pipe (not shown) to the other opening 21B of the tubular furnace. Then, by supplying a mixed gas that forms a reducing atmosphere from the opening 21A side, the inside of the reaction tube 21 can be made into a reducing atmosphere.

[0142] A heater 22 can be provided around the reaction tube 21, and the infrared absorbing particles can be placed in a ceramic container 23 such as a boat and placed at a position corresponding to the heater 22 inside the reaction tube 21 of the tubular furnace.

[0143] Using the reduction treatment device 20, a reducing atmosphere is created inside the reaction tube 21, and heating is performed to a desired temperature by the heater 22, thereby performing a reduction treatment on the particles 24 placed in the container 23. Particles recovered in the heat treatment step can be used as the particles 24, and infrared absorbing particles can be obtained by performing a reduction treatment step. [3] Infrared absorbing particle dispersion Next, the infrared absorbing particle dispersion of this embodiment will be described.

[0144] The infrared absorbing particle dispersion of this embodiment can contain a liquid medium and the above-described infrared absorbing particles contained in the liquid medium. That is, as shown in Fig. 3, for example, an infrared absorbing particle dispersion 30 of this embodiment can contain the above-described infrared absorbing particles 31 and a liquid medium 32. The infrared absorbing particles 31 are preferably dispersed in the liquid medium 32.

[0145] 3 is a schematic diagram, and the infrared absorbing particle dispersion of this embodiment is not limited to this form. For example, in FIG. 3, the infrared absorbing particles 31 are represented by circles and are depicted as spherical particles, but the shape of the infrared absorbing particles 31 is not limited to this form and can have any shape. The infrared absorbing particle dispersion 30 can also contain other additives as needed, in addition to the infrared absorbing particles 31 and the liquid medium 32.

[0146] The infrared absorbing particle dispersion liquid of this embodiment can be obtained using the infrared absorbing particles already described, in other words, using infrared absorbing particles obtained by the infrared absorbing particle manufacturing method already described.

[0147] The infrared absorbing particle dispersion may contain, in addition to the infrared absorbing particles and the liquid medium, a dispersant and other additives as desired. The infrared absorbing particle dispersion can be used as an intermediate product of the infrared absorbing particle dispersion or as a coating liquid.

[0148] The liquid medium means a medium that is liquid at the temperature at which it is used, and is preferably a medium that is liquid at room temperature (27° C.) in particular. The liquid medium is not particularly limited and can be selected as desired depending on the application, etc., but it is preferable that the liquid medium contains one or more selected from water, organic solvents, liquid plasticizers, oils and fats, and compounds that are polymerized by curing.

[0149] The infrared absorbing particle dispersion of this embodiment will be described below in the following order: (1) Contained Materials, (2) Manufacturing Method of the Infrared Absorbing Particle Dispersion, (3) Method of Using the Infrared Absorbing Particle Dispersion, and Articles Using the Infrared Absorbing Particle Dispersion. (1) Contained Materials (1-1) Infrared Absorbing Particles The infrared absorbing particle dispersion of this embodiment can contain the infrared absorbing particles described above. Since the infrared absorbing particles have already been described, their description will be omitted here. (1-2) Liquid Medium (1-2-1) Organic Solvent As the organic solvent used as the liquid medium, for example, one or more selected from alcohols, ketones, esters, glycol derivatives, amides, aromatic hydrocarbons, and the like can be suitably used.

[0150] Specifically, the organic solvent may be one or more selected from the following: alcohol-based materials such as methanol, ethanol, 1-propanol, isopropanol, butanol, pentanol, benzyl alcohol, and diacetone alcohol; ketone-based materials such as acetone, methyl ethyl ketone, dimethyl ketone, methyl propyl ketone, methyl isobutyl ketone, cyclohexanone, and isophorone; ester-based materials such as 3-methyl-methoxy-propionate and n-butyl acetate; glycol derivatives such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol isopropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; amides such as formamide, N-methylformamide, dimethylformamide, dimethylacetamide, and N-methyl-2-pyrrolidone; aromatic hydrocarbons such as toluene and xylene; ethylene chloride, chlorobenzene, and the like.

[0151] Among the above organic solvents, it is particularly preferable to use one or more selected from dimethyl ketone, methyl ethyl ketone, methyl isobutyl ketone, toluene, propylene glycol monomethyl ether acetate, n-butyl acetate, etc. (1-2-2) Fats and Oils The fats and oils used as the liquid medium are not particularly limited, but vegetable oils or compounds derived from vegetable oils can be preferably used.

[0152] As the vegetable oil, one or more types selected from drying oils such as linseed oil, sunflower oil, tung oil, and perilla oil; semi-drying oils such as sesame oil, cottonseed oil, rapeseed oil, soybean oil, rice bran oil, and poppy oil; and non-drying oils such as olive oil, coconut oil, palm oil, and dehydrated castor oil can be preferably used.

[0153] As the compound derived from vegetable oil, one or more selected from fatty acid monoesters obtained by direct esterification of fatty acids of vegetable oil with monoalcohols, ethers, etc. can be preferably used.

[0154] Commercially available petroleum-based solvents can also be used as the oils and fats.

[0155] Commercially available petroleum-based solvents that can be used include Isopar (registered trademark) E, Exxol (registered trademark) (hereinafter the same), Hexane, Heptane, E, D30, D40, D60, D80, D95, D110, and D130 (all manufactured by ExxonMobil). (1-2-3) Liquid Plasticizers Examples of liquid plasticizers used as the liquid medium include one or more selected from the group consisting of plasticizers that are compounds of monohydric alcohols and organic acid esters, ester-based plasticizers such as polyhydric alcohol organic acid ester compounds, and phosphoric acid-based plasticizers such as organic phosphoric acid-based plasticizers. Preferably, all of these are liquid at room temperature.

[0156] Among these, plasticizers that are ester compounds synthesized from polyhydric alcohols and fatty acids are preferably used. While there are no particular limitations on the ester compounds synthesized from polyhydric alcohols and fatty acids, for example, glycol-based ester compounds obtained by reacting glycol with a monobasic organic acid are preferably used. As the glycol, one or more selected from triethylene glycol, tetraethylene glycol, tripropylene glycol, etc. are preferably used. Furthermore, as the monobasic organic acid, one or more selected from butyric acid, isobutyric acid, caproic acid, 2-ethylbutyric acid, heptyl acid, n-octylic acid, 2-ethylhexyl acid, pelargonic acid (n-nonylic acid), decylic acid, etc. are preferably used.

[0157] Ester compounds of tetraethylene glycol or tripropylene glycol with a monobasic organic solvent can also be preferably used. Among these, one or more compounds selected from fatty acid esters of triethylene glycol, such as triethylene glycol dihexanate, triethylene glycol di-2-ethylbutyrate, triethylene glycol di-octanate, and triethylene glycol di-2-ethylhexanoate, can be preferably used. Furthermore, fatty acid esters of triethylene glycol can also be preferably used. (1-2-4) Compound Polymerized by Curing As the compound polymerized by curing, used in the infrared absorbing particle dispersion liquid of this embodiment, a monomer or oligomer that forms a polymer by a polymerization reaction induced by heat, light, or water can be preferably used.

[0158] Specific examples of compounds that can be polymerized by curing include methyl methacrylate monomers, acrylate monomers, and styrene resin monomers.

[0159] The liquid media described above can be used in combination of two or more types. Furthermore, if necessary, an acid or alkali may be added to these liquid media to adjust the pH. (1-3) Dispersant In the infrared absorbing particle dispersion liquid of this embodiment, in order to further improve the dispersion stability of the infrared absorbing particles and to prevent the particles from becoming coarse due to re-aggregation, the infrared absorbing particle dispersion liquid of this embodiment can also contain various dispersants, surfactants, coupling agents, etc.

[0160] The dispersant, coupling agent, and surfactant can be selected depending on the application, but are preferably materials having one or more functional groups selected from an amine-containing group, a hydroxyl group, a carboxyl group, a phosphate group, and an epoxy group. These functional groups adsorb to the surface of the infrared-absorbing particles to prevent aggregation and disperse them uniformly. Polymeric dispersants having one or more functional groups selected from these groups in the molecule are more preferably used as the dispersant.

[0161] Preferred examples of commercially available dispersants include SOLSPERSE (registered trademark) 3000, 5000, 9000, 11200, 12000, 13000, 13240, 13650, 13940, 16000, 17000, 18000, 20000, 21000, 24000SC, 24000GR, 26000, 27000, and 280 manufactured by Lubrizol Japan Corporation. 00, 31845, 32000, 32500, 32550, 32600, 33000, 33500, 34750, 35100, 35200, 36600, 37500, 38500, 39000, 41000, 41090, 53095, 55000, 56000, 71000, 76500, J180, J200, M387, etc.; SOLPLUS (registered trademark) (hereinafter the same) D5 10, D520, D530, D540, DP310, K500, L300, L400, R700, etc.; Disperbyk (registered trademark) manufactured by BYK Japan (hereinafter the same) -101, 102, 103, 106, 107, 108, 109, 110, 111, 112, 116, 130, 140, 142, 145, 154, 161, 162, 163, 164, 165, 16 6, 167, 168, 170, 171, 174, 180, 181, 182, 183, 184, 185, 190, 191, 192, 2000, 2001, 2009, 2020, 2025, 2050, 2070, 2095, 2096, 2150, 2151, 2152, 2155, 2163, 2164, Anti-Terra (registered trademark) (hereinafter the same)-U, 203, 204, etc.;BYK (registered trademark) (hereinafter the same) - P104, P104S, P105, P9050, P9051, P9060, P9065, P9080, 051, 052, 053, 054, 055, 057, 063, 065, 066N, 067A, 077, 088, 141, 220S, 300, 302, 306, 307, 310, 315, 320, 322, 323, 325, 330, 331, 333, 337, 340, 345, 346, 347, 348, 350, 354, 355, 358N, 361N, 370, 375, 377, 378, 380N, 381, 392, 410, 425, 430, 1752, 4510, 6919, 9076, 9077, W909, W935, W940, W961, W966, W969, W972, W980, W985, W995, W996, W9010, D ynwet 800, Siclean 3700, UV3500, UV3510, UV3570, etc.; EFKA (registered trademark) manufactured by EFKA Additives (hereinafter the same) 2020, 2025, 3030, 3031, 3236, 4008, 4009, 4010, 4015, 4020, 4046, 4047, 4050, 4055, 4060, 4080, 4300, 4310, 4320, 4330, 43 40, 4400, 4401, 4402, 4403, 4500, 5066, 5220, 6220, 6225, 6230, 6700, 6780, 6782, 7462, 8503, etc.; JONCRYL (registered trademark) manufactured by BASF Japan Ltd. (the same applies hereinafter) 67, 678, 586, 611, 680, 682, 690, 819, -JDX5050, etc.; TERPLUS (registered trademark) manufactured by Otsuka Chemical Co., Ltd. (the same applies hereinafter). MD1000, D 1180, D 1130, etc.; Ajinomoto Fine-Techno Co., Inc., AJISPER (registered trademark) (hereinafter the same) PB-711, PB-821, PB-822, etc.; Kusumoto Chemicals Co., Ltd., Disparlon (registered trademark) (hereinafter the same) 1751N, 1831, 1850, 1860, 1934, DA-400N, DA-703-50, DA-325, DA-375, DA-550, DA-705, DA-725, DA-1401, DA-7301, DN-900, NS-5210, NVI-8514L, etc.;Examples of such products include Alphon (registered trademark) (hereinafter the same) UH-2170, UC-3000, UC-3910, UC-3920, UF-5022, UG-4010, UG-4035, UG-4040, and UG-4070, and Reseda (registered trademark) (hereinafter the same) GS-1015, GP-301, and GP-301S, manufactured by Toagosei Co., Ltd.; and Dianall (registered trademark) (hereinafter the same) BR-50, BR-52, BR-60, BR-73, BR-77, BR80, BR-83, BR-85, BR-87, BR-88, BR-90, BR-96, BR-102, BR-113, and BR-116, manufactured by Mitsubishi Chemical Corporation.

[0162] A liquid dispersant having a glass transition temperature below room temperature can also be used instead of the liquid medium. That is, the infrared-absorbing particle dispersion of this embodiment can contain infrared-absorbing particles and a liquid dispersant, or can be composed of infrared-absorbing particles and a liquid dispersant. Preferred examples of commercially available liquid dispersants include SOLSPERSE (registered trademark) 20000 manufactured by Lubrizol Japan, and Disparlon (registered trademark) DA234, DA325, and DA375 manufactured by Kusumoto Chemicals. (1-4) Other Additives The infrared-absorbing particle dispersion of this embodiment can also contain additives such as various surfactants and resin components to control coatability, leveling, and drying properties. When such additives are added, the infrared-absorbing particle dispersion preferably contains a small amount of the additive in a range of 5% by mass or less of the dispersion. Examples of surfactants include anionic, cationic, nonionic, and amphoteric surfactants.

[0163] Furthermore, in order to impart flexibility to the infrared absorbing particle dispersion obtained using the infrared absorbing particle dispersion, the dispersion may also contain one or more organic resins selected from silicone resins, acrylic resins, polyester resins, polyurethane resins, hydrophilic organic resins containing a polyoxyalkylene group, epoxy resins, etc. When such an organic resin is added, the infrared absorbing particle dispersion preferably contains the organic resin in a small amount within a range of 5% by mass or less of the infrared absorbing particle dispersion.

[0164] Furthermore, in order to impart crack prevention properties to the infrared-absorbing particle dispersion prepared using the infrared-absorbing particle dispersion, the infrared-absorbing particle dispersion may contain one or more resins selected from thermosetting resins, thermoplastic resins, UV-curable resins, etc. When such a resin is added, the infrared-absorbing particle dispersion preferably contains the resin in an amount of 20 mass% or less of the dispersion. More specific examples of the resin include acrylic resins, epoxy resins, polyester resins, amino resins, urethane resins, furan resins, silicone resins, and modified products of these resins. (2) Method for Producing Infrared-Absorbing Particle Dispersion The method for producing the infrared-absorbing particle dispersion of this embodiment is not particularly limited. The infrared-absorbing particle dispersion of this embodiment can be prepared, for example, by adding the infrared-absorbing particles described above, and, if necessary, a dispersant and other additives, to the liquid medium described above and dispersing them. Note that, as described above, a liquid dispersant can also be used instead of the liquid medium.

[0165] The method for dispersing the infrared absorbing particles and the like in the liquid medium is not particularly limited, and examples thereof include pulverization and dispersion methods using devices such as a bead mill, a ball mill, a sand mill, a paint shaker, an ultrasonic homogenizer, etc. Among these, media agitation mills such as a bead mill, a ball mill, a sand mill, and a paint shaker, which use media such as beads, balls, and Ottawa sand, can be preferably used because they can achieve a desired particle size for the infrared absorbing particles in a short period of time.

[0166] By the pulverization-dispersion treatment using a media agitation mill, the infrared absorbing particles are dispersed in the liquid medium, and at the same time, the infrared absorbing particles are atomized due to collisions between the infrared absorbing particles and between the medium and the infrared absorbing particles, and the infrared absorbing particles can be further atomized and dispersed. In other words, the pulverization-dispersion treatment is performed.

[0167] The dispersion concentration of the infrared-absorbing particles in the infrared-absorbing particle dispersion is preferably 0.01% by mass or more and 80% by mass or less. This is because sufficient infrared absorption characteristics can be exhibited by setting the content of the infrared-absorbing particles to 0.01% by mass or more. Furthermore, setting the content to 80% by mass or less allows the infrared-absorbing particles to be uniformly dispersed in the liquid medium. By selecting the appropriate combination of the liquid medium, dispersant, coupling agent, and surfactant, the infrared-absorbing particle dispersion of this embodiment can prevent gelation of the dispersion or particle settling for six months or more, even when placed in a thermostatic chamber at a temperature of 40°C, thereby suppressing particle size increase. (3) Method of Using the Infrared-Absorbing Particle Dispersion and Articles Using the Infrared-Absorbing Particle Dispersion The infrared-absorbing particle dispersion of this embodiment can be used for a variety of purposes without any particular limitations.

[0168] The infrared absorbing particle dispersion of the present embodiment can be used as an infrared absorbing substrate by, for example, applying it to the surface of a suitable substrate to form a dispersion film. The dispersion film is a type of infrared absorbing particle dispersion and a type of dried and solidified product of the infrared absorbing particle dispersion.

[0169] Furthermore, the infrared-absorbing particle dispersion liquid of this embodiment can be dried and, if necessary, pulverized to form a powdered infrared-absorbing particle dispersion (sometimes referred to as a "dispersed powder" in this specification). In other words, the dispersed powder is a type of infrared-absorbing particle dispersion, and is also a type of dried and solidified infrared-absorbing particle dispersion liquid. The dispersed powder can also be a powdered dispersion in which the infrared-absorbing particles are dispersed in a solid medium such as a dispersant. Because the dispersed powder contains a dispersant, the infrared-absorbing particles can be easily redispersed in an appropriate medium by mixing it with the medium.

[0170] The dispersed powder can also be used as a raw material for adding the infrared absorbing particles in a dispersed state to an infrared absorbing product. That is, the dispersed powder in which the infrared absorbing particles of this embodiment are dispersed in a solid medium may be dispersed again in a liquid medium and used as a dispersion liquid for an infrared absorbing product, or the dispersed powder may be kneaded into a resin and used as an infrared absorbing particle dispersion, as described below.

[0171] The infrared absorbing particle dispersion liquid of this embodiment can be used in various applications that utilize light-to-heat conversion.

[0172] For example, a curable ink composition can be prepared by adding an infrared-absorbing particle dispersion to an uncured thermosetting resin, or by adding an uncured thermosetting resin to an infrared-absorbing particle dispersion. The curable ink composition contains the infrared-absorbing particles described above, which function as an auxiliary agent that increases the amount of heat generated by infrared radiation, such as infrared rays. Because the curable ink composition contains a thermosetting resin, when the curable ink composition is irradiated with infrared rays, the infrared-absorbing particles function as an auxiliary agent that increases the amount of heat generated, as described above, and the thermosetting resin can be cured. By providing the curable ink composition on, for example, a substrate, it is possible to increase the adhesion between the cured product of the curable ink composition and the substrate when irradiated with infrared rays, etc.

[0173] Therefore, in addition to being used as a conventional ink, the curable ink composition can also be suitably used in applications such as stereolithography, in which a three-dimensional object is formed by repeatedly applying the ink and curing it by irradiating it with infrared rays or the like to form a layer.

[0174] Alternatively, a thermoplastic resin-containing ink composition can be obtained by adding the infrared absorbing particles of this embodiment to a heat-melted thermoplastic resin, or by dispersing the infrared absorbing particles of this embodiment in an appropriate solvent and then adding a thermoplastic resin that is highly soluble in the solvent.

[0175] For example, by applying a thermoplastic resin-containing ink composition to a substrate and irradiating it with infrared rays or the like, the solvent is removed and the resin is heat-fused, and the cured product of the thermoplastic resin-containing ink composition can be adhered to the substrate. In this case, in the thermoplastic resin-containing ink composition, as in the case of the curable ink composition described above, the infrared-absorbing particles function as an auxiliary agent that increases the amount of heat generated by irradiation with infrared rays or the like.

[0176] Therefore, in addition to its use as a conventional ink, the thermoplastic resin-containing ink composition can be suitably used in applications such as photolithography, in which a three-dimensional object is formed by repeatedly applying the ink, removing the solvent by irradiating the ink with infrared rays or the like, and heat-fusing the resin.

[0177] The curable ink composition and the thermoplastic resin-containing ink composition described above are also examples of the infrared absorbing particle dispersion of this embodiment. [4] Infrared absorbing particle dispersion Next, the infrared absorbing particle dispersion of this embodiment will be described.

[0178] The infrared-absorbing particle dispersion of this embodiment can contain a solid medium and the above-described infrared-absorbing particles contained in the solid medium. Specifically, for example, as schematically shown in FIG. 4 , the infrared-absorbing particle dispersion 40 can contain the above-described infrared-absorbing particles 41 and a solid medium 42, and the infrared-absorbing particles 41 can be disposed in the solid medium 42. The infrared-absorbing particles 41 are preferably dispersed in the solid medium 42. Note that FIG. 4 is a schematic diagram, and the infrared-absorbing particle dispersion of this embodiment is not limited to such a form. For example, in FIG. 4 , the infrared-absorbing particles 41 are represented by circles and are depicted as spherical particles, but the shape of the infrared-absorbing particles 41 is not limited to such a form and can have any shape. In addition to the infrared-absorbing particles 41 and the solid medium 42, the infrared-absorbing particle dispersion 40 can also contain other additives as needed.

[0179] The solid medium means a medium that is solid at the temperature at which it is used, and is preferably a medium that is solid at room temperature (27° C.). Examples of the solid medium that can be used include resin and glass.

[0180] As the solid medium, a resin can be particularly preferably used from the viewpoint of ease of handling.

[0181] When a resin is used as the solid medium, the type of resin is not particularly limited, but the resin can be, for example, one type of resin selected from the group consisting of polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, polyamide resin, polyethylene resin, vinyl chloride resin, polyolefin resin, epoxy resin, polyimide resin, fluororesin, ethylene-vinyl acetate copolymer, polyvinyl acetal resin, and ultraviolet-curable resin, or a mixture of two or more types of resins selected from the above group of resins.

[0182] The content of infrared-absorbing particles in the infrared-absorbing particle dispersion is not particularly limited, but the infrared-absorbing particle dispersion preferably contains infrared-absorbing particles in a proportion of 0.001% by mass or more and 80% by mass or less. This is because a content of infrared-absorbing particles of 0.001% by mass or more can exhibit sufficient infrared-shielding function. Furthermore, by setting the content of infrared-absorbing particles to 80% by mass or less, it is possible to prevent the infrared-absorbing particles from agglomerating together in the solid medium and forming granules, thereby maintaining particularly good transparency. Furthermore, it is advantageous in terms of cost because the amount of infrared-absorbing particles used can be reduced. Furthermore, by setting the content of infrared-absorbing particles to 80% by mass or less, it is possible to increase the proportion of solid medium contained in the infrared-absorbing particle dispersion and thereby increase the strength of the dispersion.

[0183] The shape of the infrared absorbing particle dispersion of this embodiment is not particularly limited and can be selected as desired depending on the application, etc. For example, the infrared absorbing particle dispersion of this embodiment preferably has any of a sheet shape, a board shape, and a film shape.

[0184] The infrared absorbing particle dispersion of this embodiment will be described in the following order: (1) a method for producing the infrared absorbing particle dispersion, (2) an infrared absorbing substrate, and (3) a method for using the infrared absorbing particle dispersion and an article using the infrared absorbing particle dispersion. (1) Method for producing the infrared absorbing particle dispersion The method for producing the infrared absorbing particle dispersion is not particularly limited. The infrared absorbing particle dispersion can be produced, for example, by kneading the infrared absorbing particles described above into a solid medium such as a resin and molding the mixture into a desired shape such as a film or a board.

[0185] The infrared absorbing particle dispersion can also be produced by mixing the above-mentioned infrared absorbing particle dispersion liquid with a solid medium such as a resin. Alternatively, the infrared absorbing particle dispersion can be produced by adding a powder dispersion in which infrared absorbing particles are dispersed in a solid medium, i.e., the above-mentioned dispersed powder, to a liquid medium and mixing it with a solid medium such as a resin.

[0186] The shape of the infrared absorbing particle dispersion of the present embodiment is not particularly limited. For example, when a resin is used as the solid medium, the dispersion may be in the form of a sheet, board, or film having a thickness of 0.1 μm or more and 50 mm or less.

[0187] As described above, when preparing an infrared absorbing particle dispersion by kneading infrared absorbing particles into a solid medium such as a resin, the infrared absorbing particles and the solid medium are heated, mixed, and kneaded together at a temperature near the melting point of the solid medium, for example, the resin (for example, about 200°C or higher and 300°C or lower).

[0188] The material obtained by kneading the infrared absorbing particles into a solid medium can be molded into a desired shape, or it can be first pelletized and then molded into a desired shape such as a film or board by various methods.

[0189] The molding method is not particularly limited, and for example, extrusion molding, inflation molding, solution casting, casting, etc. can be used.

[0190] As described above, when the infrared absorbing particle dispersion is formed into a sheet, board, or film shape, the thickness is not particularly limited and can be selected depending on the application.

[0191] The infrared-absorbing particle dispersion can also be used in a powder state by further pulverizing an infrared-absorbing particle dispersion in which infrared-absorbing particles are dispersed in a solid medium. When this configuration is adopted, the infrared-absorbing particles are sufficiently dispersed in the solid medium in the powdered infrared-absorbing particle dispersion. Therefore, the powdered infrared-absorbing particle dispersion can be used as a so-called masterbatch and dissolved in an appropriate liquid medium or kneaded with resin pellets or the like, thereby easily producing a liquid or solid infrared-absorbing particle dispersion.

[0192] The solid medium serving as the matrix for the above-mentioned sheet, board, or film is not particularly limited and can be selected according to the application. As mentioned above, resins are preferably used from the viewpoint of ease of handling. When a resin is used as the solid medium, one resin selected from the group consisting of polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, polyamide resin, polyethylene resin, vinyl chloride resin, polyolefin resin, epoxy resin, polyimide resin, fluororesin, ethylene-vinyl acetate copolymer, polyvinyl acetal resin, and UV-curable resin, or a mixture of two or more resins selected from the above-mentioned group, can be preferably used. In particular, one or more resins selected from polyethylene terephthalate resin, acrylic resin, polyamide resin, vinyl chloride resin, polycarbonate resin, polyolefin resin, epoxy resin, polyimide resin, etc. can be preferably used as a low-cost, highly transparent, and versatile resin. Furthermore, fluororesins can also be used in consideration of weather resistance. (2) Infrared-Absorbing Substrate The infrared-absorbing particle dispersion of this embodiment also includes the form of an infrared-absorbing substrate having a substrate and a dispersion film containing the above-mentioned infrared-absorbing particles arranged on the surface of the substrate. 5 , which is a cross-sectional schematic view of the substrate and the dispersion film taken along the lamination direction, an infrared-absorbing substrate 50 can have a substrate 51 and a dispersion film 52 containing infrared-absorbing particles. The dispersion film 52 containing infrared-absorbing particles can be disposed on at least one surface 51A of the substrate 51.

[0193] Such an infrared absorbing substrate can be produced, for example, by the following procedure.

[0194] An infrared absorbing particle dispersion is prepared by mixing the above-described infrared absorbing particles, a liquid medium such as an organic solvent such as alcohol or water, a resin binder, and, if desired, a dispersant (dispersion preparation step).

[0195] Next, the infrared absorbing particle dispersion is applied to the surface of an appropriate substrate (application step).

[0196] The liquid medium is removed or the resin binder is cured to form a dispersion film that is an infrared absorbing particle dispersion (dispersion preparation step). Note that both the removal of the liquid medium and the curing of the resin binder may be performed.

[0197] Through the above steps, an infrared absorbing substrate is obtained in which the infrared absorbing particle dispersion is directly laminated on the surface of the substrate.

[0198] The resin binder component can be selected depending on the application, and examples thereof include ultraviolet curable resins, thermosetting resins, room temperature curable resins, thermoplastic resins, and the like.

[0199] The method for producing the infrared absorbing substrate is not limited to the above-mentioned method, and may involve, for example, coating an infrared absorbing particle dispersion liquid containing no resin binder component on the surface of the substrate, and then laminating the infrared absorbing particle dispersion on the surface of the substrate. Alternatively, after forming an infrared absorbing particle dispersion by coating the above-mentioned infrared absorbing particle dispersion liquid containing no resin binder component, a liquid medium containing a binder component may be coated on the layer of the infrared absorbing particle dispersion.

[0200] Therefore, specifically, in the method for producing an infrared absorbing substrate, first, a liquid infrared absorbing particle dispersion liquid in which infrared absorbing particles are dispersed in one or more liquid media selected from an organic solvent, an organic solvent in which a resin is dissolved, an organic solvent in which a resin is dispersed, and water can be applied to the surface of a substrate, and the obtained coating film can be solidified by an appropriate method to obtain an infrared absorbing substrate.

[0201] As the resin, for example, a resin binder can be used. As described above, an infrared-absorbing substrate can also be obtained by applying a liquid infrared-absorbing particle dispersion containing a resin binder to the surface of a substrate and solidifying the resulting coating film by an appropriate method.

[0202] Alternatively, an infrared-absorbing substrate can be obtained by mixing an infrared-absorbing particle dispersion, in which infrared-absorbing particles are dispersed in a powdery solid medium, with a predetermined medium to form a liquid infrared-absorbing particle dispersion, applying the liquid to the surface of a substrate, and solidifying the resulting coating film by an appropriate method.

[0203] Of course, an infrared-absorbing substrate can also be obtained by applying an infrared-absorbing particle dispersion liquid obtained by mixing two or more of the above liquid infrared-absorbing particle dispersion liquids onto the surface of a substrate and solidifying the resulting coating film by an appropriate method.

[0204] The material of the substrate used in the infrared absorbing substrate is not particularly limited as long as it is transparent, but preferably one or more types selected from glass, resin sheets, resin boards, resin films, etc. Note that a transparent body is a material that transmits light in the visible light region, and the degree of transmittance of light in the visible light region can be selected as desired depending on the application of the infrared absorbing substrate, etc.

[0205] The resin used for the resin sheet, resin board, and resin film is not particularly limited and can be selected depending on the required properties such as the surface condition and durability of the sheet, board, or film. Examples of the resin include one or more selected from polyester polymers such as polyethylene terephthalate and polyethylene naphthalate, cellulose polymers such as diacetyl cellulose and triacetyl cellulose, polycarbonate polymers, acrylic polymers such as polymethyl methacrylate, styrene polymers such as polystyrene and acrylonitrile-styrene copolymers, olefin polymers such as polyethylene, polypropylene, polyolefins having a cyclic or norbornene structure, and ethylene-propylene copolymers, vinyl chloride polymers, amide polymers such as aromatic polyamides, imide polymers, sulfone polymers, polyethersulfone polymers, polyetheretherketone polymers, polyphenylene sulfide polymers, vinyl alcohol polymers, vinylidene chloride polymers, vinyl butyral polymers, arylate polymers, polyoxymethylene polymers, epoxy polymers, and transparent polymers such as various binary and ternary copolymers, graft copolymers, and blends thereof. In particular, biaxially oriented polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene-2,6-naphthalate are preferred in terms of mechanical properties, optical properties, heat resistance, and economy. The polyester biaxially oriented film may be a copolymer polyester. (3) Method of Using Infrared-Absorbing Particle Dispersion and Articles Using the Infrared-Absorbing Particle Dispersion The infrared-absorbing particle dispersion and infrared-absorbing substrate of the present embodiment described so far can transmit light in the visible light range and block light in the infrared range. Therefore, they can be used, for example, in window materials in various buildings and vehicles, intended to allow sufficient visible light in while blocking light in the infrared range, thereby suppressing indoor temperature increases while maintaining brightness. In particular, the infrared-absorbing particles described above can have a light absorption peak in the wavelength range of 1400 nm to 2100 nm.Therefore, the infrared absorbing particle dispersion of this embodiment can prevent infrared rays in the above wavelength range from entering a room, and can prevent people's skin from feeling scorching hot.

[0206] The infrared absorbing particle dispersion of this embodiment can also be suitably used in filters that block infrared rays emitted forward from a PDP (plasma display panel).

[0207] Furthermore, since the infrared-absorbing particles of this embodiment have absorption in the infrared region, when an infrared laser is irradiated onto a printed surface containing these infrared-absorbing particles, they absorb infrared light having a specific wavelength. Therefore, an anti-counterfeit printed matter obtained by printing an anti-counterfeit ink containing these infrared-absorbing particles onto one or both sides of a printing substrate can be irradiated with infrared light having a specific wavelength and the reflection or transmission thereof read, thereby enabling the authenticity of the printed matter to be determined from the difference in the amount of reflection or transmission. This anti-counterfeit printed matter is an example of the infrared-absorbing particle dispersion of this embodiment.

[0208] Furthermore, a photothermal conversion layer can be formed by applying an ink containing the above-described infrared-absorbing particle dispersion and a binder component to a substrate, drying the applied ink, and then curing the dried ink. The photothermal conversion layer generates heat at the location irradiated with an infrared laser and can heat adjacent materials. Therefore, the photothermal conversion layer can generate heat only at the desired location with high positional precision when irradiated with an infrared laser. Therefore, the photothermal conversion layer can be used as a localized heating medium in a wide range of fields, including electronics, medicine, agriculture, and machinery. For example, it can be suitably used as a donor sheet used in forming organic electroluminescence elements by laser transfer, thermal paper for thermal printers, or ink ribbons for thermal transfer printers. The photothermal conversion layer is an example of the infrared-absorbing particle dispersion of this embodiment.

[0209] Furthermore, an infrared-absorbing fiber can be produced by dispersing the infrared-absorbing particles described above in an appropriate medium and incorporating the dispersion into one or more locations selected from the surface and the interior of a fiber. Because the infrared-absorbing fiber contains the infrared-absorbing particles, it efficiently absorbs near-infrared rays from sunlight and the like, resulting in an infrared-absorbing fiber with excellent heat retention. Because the infrared-absorbing fiber transmits light in the visible light region, it is an infrared-absorbing fiber with excellent design properties.

[0210] As a result, the infrared absorbing fiber can be used for various applications such as textile products that require heat retention, such as cold weather clothing, sports clothing, stockings, curtains, and other industrial textile products. The infrared absorbing fiber is an example of the infrared absorbing particle dispersion of the present embodiment.

[0211] The infrared-absorbing particle dispersion of this embodiment can also be used in materials such as roofs and exterior walls of agricultural and horticultural greenhouses. The infrared-absorbing particle dispersion of this embodiment transmits visible light, ensuring the light necessary for photosynthesis of plants in the agricultural and horticultural greenhouses. Furthermore, the infrared-absorbing particles of this embodiment can efficiently absorb light other than visible light, such as near-infrared light contained in sunlight, and can therefore be used as a heat-insulating material for agricultural and horticultural facilities. This heat-insulating material for agricultural and horticultural facilities is an example of the infrared-absorbing particle dispersion of this embodiment. [5] Infrared-Absorbing Laminate The infrared-absorbing laminate of this embodiment can have a layered structure including the above-described infrared-absorbing particle dispersion and a transparent substrate. Examples of the infrared-absorbing laminate include a laminate of two or more transparent substrates and the above-described infrared-absorbing particle dispersion. In this case, the infrared-absorbing particle dispersion can be disposed between the transparent substrates and used as an infrared-absorbing interlayer film.

[0212] In this case, specifically, as shown in Fig. 6 which is a cross-sectional schematic diagram along the lamination direction of the transparent substrate and the infrared absorbing particle dispersion, an infrared absorbing laminate 60 can have a plurality of transparent substrates 611, 612 and an infrared absorbing particle dispersion 62. The infrared absorbing particle dispersion 62, which is an infrared absorbing intermediate film, can be disposed between the plurality of transparent substrates 611, 612. Although Fig. 6 shows an example in which two transparent substrates 611, 612 are provided, the present invention is not limited to this embodiment.

[0213] In this case, the infrared absorbing interlayer film preferably has any one of a sheet shape, a board shape, and a film shape.

[0214] The transparent substrate can be suitably one or more selected from glass plates, plastic plates, plastic films, etc. that are transparent in the visible light region. The transparent substrate being transparent in the visible light region means that the substrate transmits light in the visible light region. The degree to which the transparent substrate transmits light in the visible light region can be selected as desired depending on the application of the infrared absorbing laminate, etc.

[0215] When a plastic is used as the transparent substrate, the plastic material is not particularly limited and can be selected depending on the application, and can be, for example, one or more types selected from polycarbonate resin, acrylic resin, polyester resin, polyamide resin, vinyl chloride resin, polyolefin resin, epoxy resin, polyimide resin, ionomer resin, fluororesin, etc. As the polyester resin, polyethylene terephthalate resin can be preferably used.

[0216] The transparent substrate may contain particles having an infrared absorbing function, such as the above-mentioned infrared absorbing particles.

[0217] By using the above-described infrared absorbing particle dispersion as a constituent member of an intermediate layer sandwiched between a plurality of transparent substrates, it is possible to obtain a solar radiation-shading laminated structure that is a type of infrared absorbing laminate that transmits visible light and has an infrared absorbing function.

[0218] The above-mentioned infrared absorbing laminate can also be obtained by bonding and integrating a plurality of transparent substrates facing each other with the infrared absorbing particle dispersion sandwiched therebetween by a known method.

[0219] When the above-described infrared-absorbing particle dispersion is used as an infrared-absorbing interlayer film, which is an intermediate layer sandwiched between a plurality of transparent substrates, the solid medium may be any of those described for the infrared-absorbing particle dispersion. However, from the viewpoint of increasing the adhesive strength between the infrared-absorbing interlayer film and the transparent substrates, the solid medium is preferably a polyvinyl acetal resin.

[0220] The infrared absorbing interlayer film can be produced by the above-mentioned method for producing an infrared absorbing particle dispersion, and can be in the form of, for example, a sheet, board, or film.

[0221] If the infrared-absorbing interlayer film does not have sufficient flexibility or adhesion to the transparent substrate, it is preferable to add a liquid plasticizer for the medium resin (solid medium). For example, if the medium resin used in the infrared-absorbing interlayer film is a polyvinyl acetal resin, adding a liquid plasticizer for the polyvinyl acetal resin is beneficial for improving adhesion to the transparent substrate.

[0222] As the plasticizer, a substance that is used as a plasticizer for a medium resin can be used. For example, plasticizers that can be used in an infrared-absorbing interlayer film in which the medium resin is a polyvinyl acetal resin include plasticizers that are compounds of monohydric alcohols and organic acid esters, ester-based plasticizers such as polyhydric alcohol-organic acid ester compounds, and phosphoric acid-based plasticizers such as organic phosphoric acid-based plasticizers. It is preferable that any of these plasticizers be liquid at room temperature. Among these, plasticizers that are ester compounds synthesized from polyhydric alcohols and fatty acids are preferred.

[0223] The infrared-absorbing interlayer film may also contain at least one selected from the group consisting of a silane coupling agent, a metal salt of carboxylic acid, a metal hydroxide, and a metal carbonate. The metal constituting the metal salt of carboxylic acid, the metal hydroxide, and the metal carbonate is not particularly limited, but is preferably at least one selected from sodium, potassium, magnesium, calcium, manganese, cesium, lithium, rubidium, and zinc. In the infrared-absorbing interlayer film, the content of the at least one selected from the group consisting of a metal salt of carboxylic acid, a metal hydroxide, and a metal carbonate is preferably 1% by mass or more and 100% by mass or less relative to the infrared-absorbing particles.

[0224] Furthermore, the infrared-absorbing interlayer film may contain, in addition to the infrared-absorbing particles described above, at least one type of particle selected from the group consisting of Sb, V, Nb, Ta, W, Zr, F, Zn, Al, Ti, Pb, Ga, Re, Ru, P, Ge, In, Sn, La, Ce, Pr, Nd, Gd, Tb, Dy, Ho, Y, Sm, Eu, Er, Tm, Tb, Lu, Sr, and Ca. The infrared-absorbing interlayer film may contain such particles in an amount of 5% by mass to 95% by mass, where the total of such particles and the infrared-absorbing particles is 100% by mass.

[0225] In the infrared absorbing laminate, at least one intermediate layer disposed between transparent substrates may contain an ultraviolet absorber. Examples of the ultraviolet absorber include one or more compounds selected from the group consisting of compounds having a malonic acid ester structure, compounds having an oxalic acid anilide structure, compounds having a benzotriazole structure, compounds having a benzophenone structure, compounds having a triazine structure, compounds having a benzoate structure, and compounds having a hindered amine structure.

[0226] It goes without saying that the intermediate layer of the infrared absorbing laminate may be composed of only the infrared absorbing intermediate film.

[0227] The infrared-absorbing interlayer film described here is also an example of an infrared-absorbing particle dispersion. The infrared-absorbing laminate of this embodiment is not limited to the above-described configuration in which an infrared-absorbing particle dispersion is disposed between transparent substrates, and can have any configuration as long as it has a laminate structure including an infrared-absorbing particle dispersion and a transparent substrate.

[0228] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. (Evaluation Method) First, the evaluation methods used in the following examples and reference examples will be described. (Cumulative 50% Particle Diameter, Cumulative 90% Particle Diameter) The particle size distribution of the infrared-absorbing particles in the examples and reference examples was measured using a particle size distribution analyzer (Model: UPA-150, manufactured by Nikkiso Co., Ltd.) based on the principle of dynamic light scattering using frequency analysis. The measurement conditions were a particle refractive index of 1.81 and a non-spherical particle shape. Furthermore, the background was measured using methyl isobutyl ketone, and the solvent refractive index was 1.40. The volume-based cumulative 50% particle diameter and cumulative 90% particle diameter were then calculated from the obtained particle size distribution. (Crystal Structure, Lattice Constant) The infrared-absorbing particles obtained by removing the solvent from the infrared-absorbing particle dispersion liquid prepared in the examples and reference examples were used to measure the crystal structure and lattice constant of the composite oxide contained in the infrared-absorbing particles.

[0229] The X-ray diffraction pattern of the infrared absorbing particles was measured by powder X-ray diffraction (θ-2θ method) using a powder X-ray diffractometer (X'Pert-PRO / MPD manufactured by PANalytical, Spectris Inc.) The crystal structure contained in the particles was identified from the obtained X-ray diffraction pattern, and the lattice constant was calculated by Rietveld analysis.

[0230] The Rietveld analysis was performed using an external standard method. The Rietveld analysis was first performed on the X-ray diffraction pattern of a Si standard powder (NIST640c) measured at the same time, and the zero shift value and half width parameter obtained at that time were determined as instrument parameters, and the Rietveld analysis of the infrared absorbing particles, which was the target, was refined.

[0231] Furthermore, for samples in which the crystal structure of the composite oxide was not cubic, the pseudocubic lattice constant, which is the lattice constant of the a-axis when the cubic perovskite structure is used as a reference, was also determined. The unit cell composition and unit cell volume determined when calculating the pseudocubic lattice constant are also shown in Table 1. (Optical Properties of Infrared Absorbing Particle Dispersion) The optical properties of the infrared absorbing particle dispersion in the examples and reference examples were measured as follows.

[0232] First, the infrared-absorbing particle dispersion was diluted with methyl isobutyl ketone as a solvent in a glass cell for measuring a spectrophotometer. At this time, the dilution ratio was set so that the visible light transmittance after dilution was 70%. Next, the transmitted light profile was measured at 5 nm intervals in a wavelength range of 200 nm to 2600 nm using a spectrophotometer (Hitachi High-Tech Science, Model: UH4150). Then, the visible light transmittance and solar transmittance were calculated in a wavelength range of 300 nm to 2100 nm based on JIS R 3106 (2019). In this measurement, the incident direction of the light in the spectrophotometer was perpendicular to the glass cell for measurement. In addition, a blank in which only the solvent methyl isobutyl ketone was placed in the glass cell for measurement was used as the baseline for light transmittance. (Optical Properties of Infrared-Absorbing Substrate) The optical properties of the infrared-absorbing substrate in the examples and reference examples were measured using a spectrophotometer (Hitachi High-Tech Science, Model: UH4150). The transmitted light profile was measured at 5 nm intervals in the wavelength range of 200 nm to 2600 nm, and the visible light transmittance and solar transmittance were calculated in the wavelength range of 300 nm to 2100 nm based on JIS R 3106 (2019). In addition, the wavelength at which the transmittance is lowest (light absorption is strongest) in the near-infrared region (780 nm to 2600 nm) within the measurement range of the transmitted light profile was determined from the transmitted light profile as the "light absorption peak wavelength." (Haze) The haze value of the infrared-absorbing substrate was measured using a haze meter (HM-150N manufactured by Murakami Color Research Laboratory Co., Ltd.) and calculated based on JIS K 7136 (2000). [Example 1] (Infrared-absorbing particles) As a raw material, sodium carbonate (Na 2 CO 3, manufactured by Kanto Chemical Co., Ltd., purity 99.0% or more), strontium carbonate (SrCO 3 , manufactured by Kanto Chemical Co., Ltd., purity 99.5% or more), and niobium oxide (Nb 2 O 5 , manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 99.9% or more) was used. Then, the raw materials were weighed out so that the ratio of the amounts of sodium (Na) as the A1 element, strontium (Sr) as the A2 element, and niobium (Nb) as the B element was Na:Sr:Nb = 0.5:0.5:1.0, and then thoroughly mixed to be uniform. The obtained mixed powder was placed in an alumina boat and fired at a temperature of 1300°C for 3 hours in a mixed atmosphere of 3% by volume hydrogen / 97% by volume argon. As a result, infrared absorbing particles of the composition formula Na 0.5 Sr 0.5 NbO z Particles (hereinafter also referred to as "particles A") containing a composite oxide represented by the formula (1.0<z<3.5) were obtained. Note that the subscript "O" in the above composition formula is "z."

[0233] The concentrations of Na, Sr, and Nb in the obtained infrared-absorbing particles, Particle A, were analyzed using an ICP optical emission spectrometer (Shimadzu Corporation, Model: ICPE-9000). The oxygen concentration was analyzed using a light element analyzer (LECO Corporation, Model: ON-836) by melting the sample in He gas and quantifying the CO gas generated by the reaction with carbon in the analytical crucible using IR absorption spectroscopy. The concentration of each element was analyzed three times and the average value was calculated. When these results were converted to a substance ratio, the atomic ratio was Na / Sr / Nb / O = 0.49 / 0.49 / 1 / 2.93, and the composition formula was Na 0.49 Sr 0.49 NbO 2.93 (Infrared absorbing particle dispersion) 6% by mass of the particles A according to Example 1, 6% by mass of an acrylic polymer dispersant having an amine-containing functional group (an acrylic dispersant with an amine value of 48 mg KOH / g and a decomposition temperature of 250°C), and 88% by mass of methyl isobutyl ketone were mixed. The resulting mixture (slurry) was then passed through a 0.3 mm diameter ZrO 2The mixture was placed in a glass bottle together with the beads, and then loaded into a paint shaker and subjected to a pulverization and dispersion treatment for 10 hours to obtain an infrared absorbing particle dispersion liquid according to Example 1. At this time, the particles A become infrared absorbing particles.

[0234] When the particle size distribution of the infrared absorbing particle dispersion liquid according to Example 1 was measured, the cumulative 50% particle size was 25 nm and the cumulative 90% particle size was 39 nm.

[0235] Furthermore, the solvent (dispersion medium) was removed from the infrared absorbing particle dispersion, and the powder X-ray diffraction pattern of the particles A according to Example 1 was measured. A diffraction peak attributed to a crystalline phase of an orthorhombic perovskite structure was confirmed. Furthermore, Rietveld analysis was performed based on the orthorhombic perovskite structure, and the lattice constants a, b, and c were calculated to be 8.06 Å, 8.06 Å, and 4.06 Å, respectively. The unit cell composition was Na 2 Sr 2 Nb 4 O 12 From this analysis, the unit cell volume per atom of Nb (niobium), which is the B element in this Example 1, is (8.06×8.06×4.06) / 4=65.9 Å. 3 And the pseudocubic lattice constant is (65.9) 1/3 = 4.04 Å.

[0236] The infrared-absorbing particle dispersion according to Example 1 was diluted with a methyl isobutyl ketone solvent, and the optical properties were measured. The visible light transmittance was 70% and the solar radiation transmittance was 40%. The transmitted light profile of the infrared-absorbing particle dispersion is shown in FIG. 7. (Infrared-Absorbing Particle Dispersion) The infrared-absorbing particle dispersion according to Example 1 and an ultraviolet-curable resin (Aronix UV-3701, manufactured by Toagosei Co., Ltd.) were weighed out at a mass ratio of 1:1, and mixed and stirred to prepare an infrared-absorbing substrate-forming dispersion. Then, using a bar coater with bar No. 10, the infrared-absorbing substrate-forming dispersion was applied to a 50 μm-thick PET (polyethylene terephthalate) film (HPE-50, manufactured by Toyobo Co., Ltd.), dried at 70°C for 1 minute, and irradiated with a high-pressure mercury lamp. The infrared-absorbing substrate according to Example 1 was obtained by the above operations. The infrared-absorbing substrate is an example of an infrared-absorbing particle dispersion.

[0237] The optical properties of the obtained infrared-absorbing substrate according to Example 1 were measured, and the visible light transmittance was 71% and the solar radiation transmittance was 46%. Furthermore, the haze was measured and found to be 1.2%. Furthermore, the light absorption peak wavelength was read from the transmittance profile and found to be 1665 nm.

[0238] The evaluation results are shown in Tables 1 and 2. [Examples 2 and 3] The ratio of the amounts of Na, Sr, and Nb when weighing the raw materials sodium carbonate, strontium carbonate, and niobium oxide was changed to Na:Sr:Nb = 0.75:0.25:1.0 (Example 2) and 0.1:0.9:1.0 (Example 3). The firing temperature of the mixed powder was also changed to 1250°C (Example 2) and 1400°C (Example 3). Infrared absorbing particles according to Examples 2 and 3 were prepared under the same conditions as Example 1 except for the above points.

[0239] By the above procedure, the infrared absorbing particles, Na 0.71 Sr 0.24 NbO 2.91 (Example 2) Na 0.10 Sr 0.88 NbO 2.90 Particles containing the composite oxide represented by (Example 2) were obtained. In addition, an infrared absorbing particle dispersion and an infrared absorbing substrate were prepared under the same conditions as in Example 1, except that the infrared absorbing particles produced in each Example were used, and the same evaluations as in Example 1 were carried out. The evaluation results in Examples 2 and 3 are shown in Tables 1 and 2. The transmitted light profile of the infrared absorbing particle dispersion of Example 2 is shown in FIG. 7. [Example 4] In place of sodium carbonate, potassium carbonate (K 2 CO 3 , manufactured by Kanto Chemical Co., Inc., purity of 99.5% or more) was used. The substance amount ratio of K, Sr, and Nb when weighing the raw materials was changed to K:Sr:Nb = 0.5:0.5:1.0. Except for the above points, infrared absorbing particles according to Example 4 were prepared under the same conditions as in Example 1.

[0240] By the above procedure, the infrared absorbing particles, K 0.47 Sr 0.48 NbO 2.89Particles containing a composite oxide represented by the formula (I) were obtained. Furthermore, an infrared absorbing particle dispersion and an infrared absorbing base material were prepared under the same conditions as in Example 1, except that the infrared absorbing particles were used, and the same evaluations as in Example 1 were carried out. The evaluation results in Example 4 are shown in Tables 1 and 2. [Example 5] Infrared absorbing particles were produced and evaluated using the composite material production apparatus 10 shown in Figure 1 and the reduction treatment apparatus shown in Figure 2. Specific conditions are described below.

[0241] The composite material manufacturing apparatus 10 has a storage section 11 containing a solution containing an A1 element source, an A2 element source, and a B element source, which is a raw material solution, a two-fluid nozzle 12 that forms droplets of the raw materials and also forms a flame, and a reaction tube 13 connected to a filter 14 that collects the formed infrared absorbing particles.

[0242] The supply rate of the raw material solution to the two-fluid nozzle 12 was set to 3 g / min. The flow rate of oxygen, which was a carrier gas, was set to 15 L / min, controlled by the ejector 15. The air flow rate in the ejector 15 was controlled to be within the range of 160 L / min to 180 L / min.

[0243] Propane gas and oxygen gas were used to form the flame by the two-fluid nozzle 12, with the flow rate of the propane gas being 1.2 L / min and the flow rate of the oxygen gas being 6.0 L / min.

[0244] As a solution containing a B element source, niobium ethoxide (Nb(OC 2 H 5 ) 5 A solution (solution containing Nb element source) in which sodium acetate (CH 3 , manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 99.9% or more) was dissolved in ethanol was used. 3 A solution (solution containing a Na element source) prepared by dissolving COONa (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 98.5% or higher) in ethanol was used. As a solution containing an A2 element source, strontium acetate 0.5 hydrate ((CH 3 COO) 2 Sr0.5H 2A solution (solution containing a Sr element source) in which niobium (O, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 99.9% or higher) was dissolved in propionic acid was used. A mixed solution of a solution containing a B element source, a solution containing an A1 element source, and a solution containing an A2 element source was used as the raw material, and was stored in storage unit 11. The mixed solution as the raw material was prepared so that the ratio of the amount of substance of Na (Na), which is the A1 element, the amount of substance of Sr (Sr), which is the A2 element, and the amount of substance of niobium (Nb), which is the B element, was Na / Sr / Nb, which was 0.5 / 0.5 / 1.0.

[0245] The raw material solution and oxygen as a carrier gas were supplied from the storage section 11 to the two-fluid nozzle 12 to form an aerosol (aerosol forming step).

[0246] As described above, propane gas and oxygen gas were supplied to the two-fluid nozzle 12 to form a flame reaction field, and the formed aerosol was supplied into the flame and subjected to heat treatment (heat treatment process).

[0247] The particles obtained in the heat treatment step were introduced into a reaction tube 13. A cooling water pipe 131 was arranged around the reaction tube 13, and cooling water was circulated through the pipe. The particles introduced into the reaction tube 13 were collected by a filter 14, which was a bag filter.

[0248] The collected particles were placed in an alumina boat and subjected to a reduction treatment by firing at a temperature of 1200° C. for 3 hours in a mixed atmosphere of 3% by volume hydrogen and 97% by volume argon. 0.30 Sr 0.50 NbO 2.65 In addition, an infrared absorbing particle dispersion and an infrared absorbing substrate were prepared under the same conditions as in Example 1, except that the infrared absorbing particles were used, and the same evaluations as in Example 1 were carried out. The evaluation results in Example 5 are shown in Tables 1 and 2. [Example 6] Tantalum ethoxide (Ta(OC)) was used as the B element source instead of niobium ethoxide. 2 H 5 ) 5The infrared absorbing particles of Example 6 having the composition formula Na were prepared in the same manner as in Example 5, except that the ratio Na / Sr / Ta of the amount of substance of Na (Na), which is the A1 element, the amount of substance of Sr (Sr), which is the A2 element, and the amount of substance of tantalum (Ta), which is the B element, contained in the mixed solution was adjusted to 0.75 / 0.25 / 1.0. 0.67 Sr 0.25 TaO 2.99 In addition, an infrared absorbing particle dispersion and an infrared absorbing base material were prepared under the same conditions as in Example 1, except that the infrared absorbing particles were used, and the same evaluations as in Example 1 were carried out. The evaluation results in Example 6 are shown in Tables 1 and 2. [Reference Example 1] SnCl was added to 340 g of water at 25°C. 4 ・5H 2 54.9 g of tin compound solution was dissolved in tin oxide (Wako Pure Chemical Industries, Ltd., Wako special grade, purity 98% or more). 3 12.7 mL of methanol solution (Yoneyama Pharmaceutical Co., Ltd., special reagent grade, purity 99.8% or higher) containing 4.2 g of NH3 (Wako Pure Chemical Industries, Ltd., JIS special grade, purity 98% or higher) and 16% diluted alkaline solution of NH3 4 An aqueous OH solution (special grade reagent, 30% concentration, manufactured by Wako Pure Chemical Industries, Ltd.) was added dropwise in parallel to the above solution, and a hydroxide containing tin and antimony, which is a precursor of antimony-doped tin oxide (hereinafter abbreviated as ATO) infrared absorbing particles, was generated and precipitated by the above-mentioned dropwise addition.

[0249] From the viewpoint of desired optical properties, the amount of antimony compound added to the tin compound solution was set to 9.5 parts by mass (antimony element equivalent) per 100 parts by mass of tin (IV) oxide, which allows the production of ATO infrared absorbing particles containing approximately 68% by mass of Sn element and approximately 8% by mass of Sb element.

[0250] As described above, aqueous ammonia was used as the alkaline solution used as the precipitant, and the alkaline concentration was 16%, which is 1.6 times the chemical equivalent required for the tin compound and antimony compound to become hydroxides.

[0251] The parallel addition of the methanol solution and the alkaline solution was continued for 25 minutes until the pH of the resulting solution reached 7.5. After the completion of the addition, the solution was stirred for 10 minutes to homogenize the system. The temperature of the solution at this time was kept at 65°C, the same temperature as during the parallel addition.

[0252] Next, the precipitate was washed by repeatedly decanting until the conductivity of the supernatant liquid in the decantation was 1 mS / cm or less, and then filtered.

[0253] Next, the washed precipitate was wetted with an anhydrous ethyl alcohol solution (Wako Pure Chemical Industries, Ltd., special grade reagent, purity 99.5% or higher). During the wet treatment, the mass ratio of the filtered precipitate to the anhydrous ethyl alcohol solution was 1:4 (corresponding to an 80% alcohol content), and the filtered precipitate and the anhydrous ethyl alcohol solution were stirred at room temperature for 1 hour to obtain a precursor. After the wet treatment was completed, the precursor was dried at 90°C for 10 hours to obtain a dried product.

[0254] The ATO infrared absorbing particle precursor that had been subjected to the wet treatment was heated to 700° C. in an air atmosphere and baked for 2 hours, thereby producing the ATO infrared absorbing particles according to Reference Example 1.

[0255] An infrared absorbing particle dispersion liquid and an infrared absorbing base material according to Reference Example 1 were prepared in the same manner as in Example 1, except that the ATO infrared absorbing particles according to Reference Example 1 were used instead of particles A as the infrared absorbing particles, and evaluations were carried out in the same manner as in Example 1. The evaluation results in Reference Example 1 are shown in Tables 1 and 2. [Reference Example 2] (Infrared absorbing particles) As raw materials for preparing an intermediate product, only strontium carbonate and niobium oxide, the same as in Example 1, were used, without using sodium carbonate. When weighing the raw materials, the ratio of the amounts of Sr and Nb was set to Sr:Nb = 2.0:1.0.

[0256] The mixed powder obtained by mixing the raw materials was placed in an alumina boat and fired at 1400°C for 2 hours in an air atmosphere to obtain an intermediate product with the composition formula Sr 4 Nb 2 O 9of strontium niobate was obtained.

[0257] The resulting intermediate product, Sr 4 Nb 2 O 9 The same niobium oxide as in Example 1 and niobium powder (Nb, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity 99.5%) were mixed together. At this time, the mixing was performed so that the ratio of the amounts of Sr and Nb in the powder after mixing, Sr:Nb, was 1.0:1.0. The mixed powder was placed in an alumina crucible and fired at a temperature of 1600°C for 3 hours in a flow of 3 volume% hydrogen gas with argon gas as a carrier, thereby preparing infrared absorbing particles according to Reference Example 2.

[0258] By the above procedure, infrared absorbing particles having the composition formula SrNbO 2.92 Particles containing strontium niobate were obtained. Furthermore, except for using the infrared absorbing particles, an infrared absorbing particle dispersion and an infrared absorbing base material were obtained in the same manner as in Example 1, and evaluations were carried out in the same manner as in Example 1. The evaluation results are shown in Tables 1 and 2. Furthermore, the transmitted light profile of the infrared absorbing particle dispersion is shown in FIG. 7.

[0259]

[0260]

[0261] The results shown in Tables 1 and 2 confirm that the infrared absorbing particle dispersions and the infrared absorbing particle dispersions using the infrared absorbing particles obtained in Examples 1 to 6 have high visible light transmittance and are able to suppress solar radiation transmittance. In other words, it was confirmed that the transmittance in the visible light region is high and the transmittance in the infrared region is able to be suppressed.

[0262] It was also confirmed that the visible light transmittance and solar radiation transmittance were comparable to or superior to ATO of Reference Example 1, which has been conventionally used as infrared absorbing particles. Furthermore, the light absorption peak wavelengths of the infrared absorbing base materials of Examples 1 to 6 were in the range of 1,400 nm or more and 2,100 nm or less.

[0263] That is, it was clear that, even within the infrared region, the infrared absorbing particles have strong absorption at light wavelengths that cause a burning sensation on human skin. Therefore, it was confirmed that the infrared absorbing particles obtained in Examples 1 to 6 are novel infrared absorbing particles that can be used in practical applications.

[0264] Furthermore, the light absorption peak wavelength of the infrared absorbing transparent substrate of Reference Example 2 was 1300 nm. Therefore, it was confirmed that the infrared absorbing particles according to an aspect of the present disclosure of Examples 1 to 6, and the infrared absorbing substrates containing the infrared absorbing particles, etc., are novel substances having optical properties different from those of the conventional infrared absorbing particles of Reference Example 2 and the like, and the infrared absorbing substrates containing the infrared absorbing particles.

[0265] This application claims priority based on Japanese Patent Application No. 2023-055015, filed with the Japan Patent Office on March 30, 2023, the entire contents of which are incorporated herein by reference.

[0266] DESCRIPTION OF SYMBOLS 10 Composite material manufacturing apparatus 11 Storage section 12 Two-fluid nozzle 13 Reaction tube 131 Piping 14 Filter 15 Ejector 20 Reduction treatment device 21 Reaction tube 21A One port 21B Other port 22 Heater 23 Container 24 Particles 30 Infrared absorbing particle dispersion 31 Infrared absorbing particles 32 Liquid medium 40 Infrared absorbing particle dispersion 41 Infrared absorbing particles 42 Solid medium 50 Infrared absorbing substrate 51 Substrate 52 Dispersion film 51A One surface 60 Infrared absorbing laminate 611, 612 Transparent substrate 62 Infrared absorbing particle dispersion

Claims

1. An infrared absorbing particle containing a complex oxide, the complex oxide containing: an A1 element which is one or more elements selected from H and an alkali metal; an A2 element which is one or more elements selected from Mg and an alkaline earth metal; and a B element which is one or more elements selected from V, Nb and Ta, wherein, when the amount of substance of the A1 element contained in the complex oxide is x1, the amount of substance of the A2 element is x2, and the amount of substance of the B element is y, the infrared absorbing particle satisfies the relationships: 0.002≦(x1+x2) / y≦1.5, 0.001≦x1 / y≦1, and 0.001≦x2 / y≦1.

2. The infrared absorbing particles according to claim 1, having a volume-based cumulative 50% particle size of 1 nm or more and 50 nm or less, and a cumulative 90% particle size of 5 nm or more and 100 nm or less, as measured by a particle size distribution measuring device.

3. The infrared absorbing particle according to claim 1 or 2, wherein the A1 element is one or more elements selected from the group consisting of H, Li, Na, K, Rb and Cs.

4. The infrared absorbing particle according to claim 1 or 2, wherein the A2 element is one or more elements selected from the group consisting of Ca, Sr and Ba.

5. An infrared absorbing particle according to claim 1 or 2, wherein the A1 element is one or more elements selected from Na and K, the A2 element is one or more elements selected from Ca, Sr and Ba, and the B element is one or more elements selected from Nb and Ta, and 0.7≦(x1+x2) / y≦1.0 is satisfied.

6. The infrared absorbing particle according to claim 1 or 2, wherein the crystal structure of the composite oxide is a cubic or orthorhombic crystal.

7. An infrared absorbing particle dispersion liquid comprising: a liquid medium; and the infrared absorbing particles according to claim 1 or 2 contained in the liquid medium.

8. The infrared absorbing particle dispersion liquid according to claim 7, wherein the liquid medium contains at least one selected from the group consisting of water, organic solvents, liquid plasticizers, oils and fats, and compounds that are polymerized by curing.

9. An infrared absorbing particle dispersion comprising: a solid medium; and the infrared absorbing particles according to claim 1 or 2 contained in the solid medium.

10. The infrared absorbing particle dispersion according to claim 9, wherein said solid medium is a resin.

11. The infrared absorbing particle dispersion according to claim 10, wherein the resin is one type of resin selected from the group consisting of polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, polyamide resin, polyethylene resin, vinyl chloride resin, polyolefin resin, epoxy resin, polyimide resin, fluororesin, ethylene-vinyl acetate copolymer, polyvinyl acetal resin, and ultraviolet curable resin, or a mixture of two or more types of resins selected from the group of resins.

12. The infrared absorbing particle dispersion of claim 9, having a sheet, board, or film shape.

13. An infrared absorbing laminate having a laminate structure comprising the infrared absorbing particle dispersion according to claim 9 and a transparent substrate.

Citation Information

Patent Citations

  • Light shielding film

    JP2003029314A

  • Information processing apparatus, information processing method, and information processing program

    JP2023055015A

  • Infrared shielding material microparticle dispersion, infrared shield, process for producing infrared shielding material microparticle, and infrared shielding material microparticle

    WO2005037932A1

  • Infrared absorption particle and manufacturing method therefor