Biofuel cell, electrode for biofuel cells, enzyme electrode, and electrode slurry for biofuel cells
The use of a polymer binder with specific structural units in biofuel cells addresses the environmental and binding issues of existing technologies, achieving better output characteristics and reduced environmental impact through improved enzyme immobilization and cost-effectiveness.
Patent Information
- Application Number
- PCT/JP2024/012257
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Biofuel cells using organic solvents like N-methylpyrrolidone for electrode binders face environmental concerns and damage to screen printing equipment, and the binding properties of polyvinylidene fluoride (PVDF) are insufficient, leading to poor enzyme immobilization and output characteristics.
A biofuel cell with electrodes using a polymer binder containing a nonionic ethylenically unsaturated monomer, an anionic ethylenically unsaturated monomer, and a crosslinking agent with multiple ethylenically unsaturated bonds, which provides improved binding and immobilization of enzymes, reducing environmental impact and production costs.
The solution enables biofuel cells with enhanced output characteristics and low environmental impact, suitable for screen printing, and effective enzyme immobilization, resulting in improved power generation performance.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Biofuel cell, electrode for biofuel cell, enzyme electrode, and electrode slurry for biofuel cell
[0001] The present invention relates to a biofuel cell, and an electrode, an enzyme electrode, and an electrode slurry used therein.
[0002] As a next-generation fuel cell, research and development is underway on biofuel cells that use enzymes or microorganisms as electrode catalysts and generate electricity using biomass resources such as sugars, alcohols, and organic waste liquids as fuel (see, for example, Patent Documents 1 and 2). Biofuel cells that use enzymes generally generate electricity by oxidizing and decomposing fuel at the negative electrode (anode) using oxidizing enzymes to extract electrons, and then reducing oxygen at the positive electrode (cathode) using reductases to produce water.
[0003] One known process for easily and inexpensively producing such biofuel cells is a method of patterning electrode materials by screen printing. Specifically, a common method involves preparing a slurry (electrode slurry) by dispersing a conductive material such as carbon powder in a binder (electrode binder) prepared by dissolving polyvinylidene fluoride (PVDF) in an organic solvent such as N-methylpyrrolidone (NMP), screen-printing the slurry onto a substrate, and drying the slurry to form an electrode pattern (see, for example, Patent Document 1).
[0004] Patent No. 6994184 JP 2021-140988 A
[0005] However, electrode binders using NMP, an organic solvent, have raised concerns about damage to screen printing equipment, and the environmental impact of the organic solvent has also been an issue. Furthermore, electrode slurries using PVDF have not necessarily been able to sufficiently bind conductive materials. Furthermore, PVDF has high water repellency, and electrode slurries using PVDF have also presented issues such as insufficient immobilization of enzymes on the electrode and easy deactivation of the enzymes, making it difficult to obtain biofuel cells with sufficient output characteristics.
[0006] The present invention has been made to solve these problems, and aims to provide a biofuel cell that has a low environmental impact, is low cost, and exhibits good output characteristics, as well as a biofuel cell electrode, an enzyme electrode, and a biofuel cell electrode slurry that are suitable for use in the biofuel cell.
[0007] The present invention is based on the discovery that a specific polymer is suitable as an electrode binder when forming electrodes for biofuel cells by screen printing.
[0008] The present invention provides the following means: [1] A biofuel cell that generates electricity through an oxidation-reduction reaction catalyzed by an enzyme, wherein the enzyme is immobilized on at least one of an anode and a cathode, the anode comprising a conductive material (1) and an electrode binder (1), the cathode comprising a conductive material (2) and an electrode binder (2), at least one of the electrode binders (1) and (2) comprising a polymer (A), the polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinker (a3), the crosslinker (a3) having two or more ethylenically unsaturated bonds in one molecule. [2] A biofuel cell that generates electricity through an oxidation-reduction reaction catalyzed by an enzyme, wherein at least one of an anode and a cathode comprises a conductive material and an electrode binder, and an enzyme is immobilized thereon; the electrode binder comprises a polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3); and the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule. [3] A biofuel cell electrode comprising a conductive material and an electrode binder, wherein the electrode binder comprises a polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), and the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule. [4] An enzyme electrode, wherein an enzyme is immobilized on the biofuel cell electrode according to [3].
[0009] [5] An electrode slurry for a biofuel cell, comprising an electrode binder, a conductive material, and an aqueous medium, wherein the electrode binder comprises a polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinker (a3), and the crosslinker (a3) has two or more ethylenically unsaturated bonds in one molecule. [6] The electrode slurry for a biofuel cell according to [5], wherein the content of the electrode binder is 10 to 200 parts by mass per 100 parts by mass of the conductive material.
[0010] According to the present invention, it is possible to provide a biofuel cell, a biofuel cell electrode, and an enzyme electrode that have a low environmental impact and are low cost and exhibit good output characteristics. Furthermore, according to the present invention, it is possible to provide an electrode slurry for a biofuel cell that has a low environmental impact, is suitable for screen printing, and can be used to produce a biofuel cell that exhibits good output characteristics.
[0011] Fig. 1 is a schematic cross-sectional view showing an example of the configuration of a biofuel cell according to an embodiment of the present invention. Fig. 2 is a schematic cross-sectional view showing another example of the configuration of a biofuel cell according to an embodiment of the present invention. Fig. 3 is a schematic cross-sectional view showing an example of the implementation of the biofuel cell of Fig. 1.
[0012] The definitions and meanings of terms and notations used in this specification are provided below. Biofuel cell electrodes, also referred to simply as "electrodes," refer to electrodes in a state before enzymes are immobilized, and are to be distinguished from "enzyme electrodes" on which enzymes are immobilized. The notation "X to Y" (X and Y are numerical values) refers to a numerical range with X as the lower limit and Y as the upper limit. In numerical ranges (e.g., ranges of content, etc.), the lower and upper limits described in stages may be independently combined. The lower and upper limits of numerical ranges may be replaced with numerical values described in the Examples. The content of each structural unit constituting a polymer is determined based on the blending amounts of compounds derived from each structural unit, which are the raw materials for synthesizing the polymer. "(Meth)acrylic" is a general term for acrylic and methacrylic. Similarly, "(meth)acrylate" is a general term for acrylate and methacrylate, and "(meth)acryloyl" is a general term for acryloyl and methacryloyl. The glass transition temperature is the peak-top temperature of the temperature derivative curve in differential scanning calorimetry (DSC). Specifically, it is measured by the method described in the Examples. The median particle diameter D50 is the 50% cumulative particle diameter on a volume basis determined from a particle size distribution curve measured by dynamic light scattering (DLS) for an aqueous dispersion sample.
[0013] [Biofuel Cell] A biofuel cell according to an embodiment of the present invention (hereinafter referred to as the present embodiment) generates electricity through an oxidation-reduction reaction catalyzed by an enzyme. An enzyme is immobilized on at least one of the anode and the cathode. The anode comprises a conductive material (1) and an electrode binder (1), and the cathode comprises a conductive material (2) and an electrode binder (2). At least one of the electrode binders (1) and (2) comprises a polymer (A). The polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinker (a3). The crosslinker (a3) has two or more ethylenically unsaturated bonds per molecule. Forming an electrode using an electrode binder containing the polymer (A) having such a predetermined structure allows for a biofuel cell to be obtained that has low environmental impact, low cost, and excellent output characteristics.
[0014] The electrode on which the enzyme is immobilized may be only one of the anode and the cathode, or both. The enzyme electrode on which the enzyme is immobilized is preferably the enzyme electrode of the present embodiment described below. The biofuel cell of the present embodiment is a biofuel cell that generates power through an oxidation-reduction reaction catalyzed by an enzyme, and it is also preferable that at least one of the anode and the cathode contains a conductive material and an electrode binder, and has an enzyme immobilized thereon. The electrode binder contains a polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), and the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule. That is, either the anode or the cathode may be the enzyme electrode of the present embodiment, or both may be the enzyme electrodes of the present embodiment. When both the anode and the cathode are the enzyme electrodes of this embodiment, the substrates of the enzyme electrodes of the anode and the cathode, the electrode binders (1) and (2), and the conductive materials (1) and (2) may be the same or different. Examples of substrates for enzyme electrodes include paper, cloth, resin films, metal materials, and inorganic materials such as ceramics. When the cathode is not the enzyme electrode of this embodiment, the cathode may be one to which, for example, an oxygen reduction catalyst containing a metal such as platinum is immobilized instead of an enzyme.
[0015] The fuel for a biofuel cell is not particularly limited as long as it is a substance whose oxidation is promoted by an enzyme. Examples of fuels include sugars, alcohols, aldehydes, amino acids, amines, lactic acid, and uric acid. The fuel may be a substance that is hydrolyzed by an enzyme and then oxidized (e.g., starch or cellulose, which is hydrolyzed to glucose). One type of fuel may be used alone, or two or more types may be used in combination. Of these, sugars are preferred from the viewpoints of output stability, ease of handling, and the like. The type of sugar is not particularly limited, and examples include monosaccharides, disaccharides, oligosaccharides, polysaccharides, and sugar alcohols. For example, glucose is preferably used.
[0016] The conductive material (1) and electrode binder (1) constituting the anode, and the conductive material (2) and electrode binder (2) constituting the cathode will be described later.
[0017] FIG. 1 schematically shows an example of the structure of a biofuel cell according to this embodiment. In the biofuel cell 10 shown in FIG. 1, an anode 2 and a cathode 3 are formed on the same surface on one side of a substrate 1 containing a fuel. FIG. 2 also schematically shows another example of the structure of a biofuel cell according to this embodiment. In the biofuel cell 20 shown in FIG. 2, an anode 2 is formed on one side of a substrate 1 containing a fuel, and a cathode 3 is formed on the other (opposite) side. In this case, the substrate 1 also serves as a separator between the anode 2 and the cathode 3.
[0018] The biofuel cell of this embodiment can generate electricity simply by supplying, for example, gum syrup as fuel. In another embodiment, for example, by incorporating sugar as fuel in the substrate in advance, electricity can also be generated using water.
[0019] Another example of an embodiment is one in which the biofuel cell 10 is attached to the skin, as shown in Fig. 3. In the example of Fig. 3, the biofuel cell 10 of the embodiment shown in Fig. 1 is used, and a lead portion 4 is formed on each of the anode 2 and the cathode 3. The lead portion 4 is covered with a cover sheet 5, and the base material 1 is brought into contact with the skin 6, thereby fixing the biofuel cell 10 to the skin 6. The biofuel cell 10 may be fixed to the skin 6 by using an adhesive sheet for the cover sheet 6, or may be fixed to the skin 6 using a separate adhesive tape or the like.
[0020] 3, for example, an enzyme electrode on which lactate oxidase is immobilized can be used as the anode 2, and an enzyme electrode on which bilirubin oxidase is immobilized can be used as the cathode 3. In this case, sweat secreted from the skin 6 is absorbed into the substrate 1, and electricity is generated using the lactic acid contained in the sweat as fuel. The electricity can be extracted to the outside through the lead part 4.
[0021] As described above, when the biofuel cell of this embodiment is applied to a living body, it can also be used as a biosensor. For example, by attaching the biofuel cell to an adherend such as skin, clothing, or a diaper, the amount of substances in bodily fluids such as sweat, urine, blood, tears, and saliva supplied from the adherend can be detected as electric power, and fluctuations in the amount of electric power can be measured, which can be used for health management and measurement and management of exercise volume.
[0022] [Biofuel cell electrode] The electrode of this embodiment is a biofuel cell electrode comprising a conductive material and an electrode binder, wherein the electrode binder comprises a polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinker (a3), wherein the crosslinker (a3) has two or more ethylenically unsaturated bonds per molecule. By using an electrode produced using an electrode binder containing the polymer (A) having such a predetermined structure, a biofuel cell can be obtained that has low environmental impact, low cost, and exhibits good output characteristics.
[0023] The electrode of this embodiment is preferably used in at least one of the anode and cathode of the biofuel cell electrode, and more preferably in both the anode and the cathode, in which case the electrode binder contained in the anode and the electrode binder contained in the cathode may have the same composition or different compositions.
[0024] The electrode is preferably one in which at least a conductive material and the electrode binder are adhered to a substrate. Such an electrode can be produced by applying an electrode slurry containing the electrode binder, a conductive material, and an aqueous medium to the substrate and drying it. Examples of the substrate include cloth, paper, and resin film. The substrate is preferably porous and exhibits good adhesion to the electrode binder so that the conductive material can be adhered at high density. From the viewpoint of consideration for the environmental impact when disposing of the biofuel cell, for example, Japanese paper is preferably used. Furthermore, from the viewpoint of durability, for example, oil-resistant and waterproof paper is preferably used. The electrode slurry may be applied to one side or both sides of the substrate.
[0025] Details of the electrode slurry, as well as the electrode binder, conductive material, and aqueous medium will be described later.
[0026] The method for applying the electrode slurry is not particularly limited. Examples of application methods include screen printing, reverse roll printing, direct roll printing, and doctor blade printing. Among these, screen printing is preferred because it allows for simple and efficient pattern formation. In the case of screen printing, for example, it is also possible to form an electrode pattern in which a lead portion and a plurality of electrodes are printed on a substrate using a conductive material such as carbon paste.
[0027] The electrode slurry applied to the substrate is dried to thoroughly remove the aqueous medium from the electrode slurry. The drying method is not particularly limited as long as the aqueous medium is thoroughly removed. Examples of drying methods include methods using hot air, low-temperature air, reduced pressure or vacuum, (far) infrared radiation, etc. These drying conditions may be combined.
[0028] [Enzyme Electrode] The enzyme electrode of this embodiment is an electrode on which an enzyme is immobilized.
[0029] In the case of an anode enzyme electrode, an enzyme that promotes the oxidation of the fuel in the biofuel cell is used. It may also be used in combination with an enzyme that facilitates the oxidation of the fuel by hydrolysis or the like. Examples of enzymes used in the anode enzyme electrode include, for example, glucose oxidase or a combination of glucose oxidase and glucose dehydrogenase when the fuel is glucose; fructose oxidase or a combination of fructose oxidase and fructose dehydrogenase when the fuel is fructose; invertase or a combination of invertase and glucose dehydrogenase when the fuel is sucrose; amylase or a combination of amylase and glucose dehydrogenase when the fuel is starch; and lactate oxidase when the fuel is lactic acid.
[0030] In the case of a cathode enzyme electrode, an enzyme that promotes the reduction of oxygen is preferably used. Examples of the enzyme used in the cathode enzyme electrode include bilirubin oxidase and laccase.
[0031] The enzyme electrode can be produced, for example, by immobilizing an enzyme on an electrode. Alternatively, the enzyme electrode can be produced by mixing an enzyme with an electrode slurry to form an enzyme-containing electrode slurry, applying the mixture to a substrate, and drying the mixture.
[0032] The method for immobilizing the enzyme on the electrode is not particularly limited, and can be, for example, by applying an enzyme solution to the electrode and drying it. The enzyme can be applied, for example, by dripping or impregnating the enzyme solution. The enzyme may also be applied after applying a mediator.
[0033] The mediator is a redox compound that mediates electron transfer between the electrode and the enzyme, and is appropriately selected depending on the type of fuel and enzyme. The mediator is used by being supported on the electrode or dissolved in the electrolyte. When the mediator is supported on the electrode, the mediator may be added to an electrode slurry and applied to the electrode, or the mediator may be applied after the electrode is formed. The mediator may be supported on either the anode or the cathode, or on both.
[0034] Examples of the mediator include organic sulfur compounds such as thionine, thionine acetic acid, tetrathiafulvalene, and 2,2'-azinobis(3-ethylbenzothiazoline-6-ammonium sulfonate); quinone compounds such as hydroquinone, 1,2-naphthoquinone, and 1,4-naphthoquinone; ferrocene; ferricyanide; osmium complexes; and polymers modified with these compounds. One type of mediator may be used alone, or two or more types may be used in combination.
[0035] The enzyme immobilized on the electrode has a concentration of preferably 0.001 U / cm relative to the electrode in order to sufficiently promote power generation. 2 or more, more preferably 0.01 U / cm 2 More preferably, 0.1 U / cm 2 The amount of enzyme immobilized on the electrode is preferably as large as possible, for example, 2000 U / cm 2 or less, and may be 1000 U / cm 2 It may be less than 500 U / cm 2 It may be the following:
[0036] [Electrode binder for biofuel cells] The electrode binder of this embodiment comprises a polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinker (a3), wherein the crosslinker (a3) has two or more ethylenically unsaturated bonds per molecule. The electrode binder containing the polymer (A) having such a predetermined structure has a low environmental impact and good dispersibility of conductive materials, and can provide an electrode slurry suitable for screen printing. The use of this electrode slurry allows for the production of a biofuel cell that has a low environmental impact, good cost performance, and good output characteristics.
[0037] Hereinafter, the term "electrode binder" refers collectively to the electrode binder (1) constituting the anode and the electrode binder (2) constituting the cathode, and the term "conductive material" refers collectively to the conductive material (1) constituting the anode and the conductive material (2) constituting the cathode.
[0038] The electrode binder of this embodiment contains the polymer (A) and may further contain a water-soluble cellulose derivative (B) and other additives, which will be described later. The content of the polymer (A) in the electrode binder is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 80% by mass or more, and may even be 100% by mass, so that the effects of the present invention can be fully exerted.
[0039] (Polymer (A)) The polymer (A) has a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3). The polymer (A) may have other structural units in addition to the first structural unit, the second structural unit, and the third structural unit. In order to fully exhibit the effects of the present invention, the total of the first structural unit, the second structural unit, and the third structural unit is preferably 80 to 100% by mass, more preferably 85% by mass or more, even more preferably 90% by mass or more, and still more preferably 95% by mass or more, based on 100% by mass of all structural units constituting the polymer (A).
[0040] <First structural unit> The first structural unit constituting the polymer (A) is derived from a nonionic ethylenically unsaturated monomer (a1). The content of the first structural unit in the total amount of the first structural unit, second structural unit, and third structural unit constituting the polymer (A) is preferably 60 to 98% by mass in order to obtain a polymer (A) that fully exhibits the effects of the present invention. It is more preferably 75% by mass or more, even more preferably 90% by mass or more, and more preferably 97% by mass or less, even more preferably 96% by mass or less.
[0041] The nonionic ethylenically unsaturated monomer (a1) from which the first structural unit is derived has one ethylenically unsaturated bond per molecule and has neither an anionic functional group nor a cationic functional group. The nonionic ethylenically unsaturated monomer (a1) may be used alone or in combination of two or more. The nonionic ethylenically unsaturated monomer (a1) is preferably one or more selected from the group consisting of aromatic ethylenically unsaturated compounds, (meth)acrylic acid alkyl esters, and polar group-containing ethylenically unsaturated carboxylic acid esters, and preferably includes all of these.
[0042] The aromatic ethylenically unsaturated compound contributes to good binding properties of the conductive material. Examples of the aromatic ethylenically unsaturated compound include styrene, tert-butylstyrene, α-methylstyrene, p-methylstyrene, 1,1-diphenylethylene, and benzyl (meth)acrylate. The aromatic ethylenically unsaturated compound may be used alone or in combination of two or more. Of these, aromatic vinyl compounds are preferred, and styrene is more preferred.
[0043] The proportion of the aromatic ethylenically unsaturated compound in the nonionic ethylenically unsaturated monomer (a1) is preferably 25 to 70% by mass, more preferably 35% by mass or more, even more preferably 45% by mass or more, and more preferably 65% by mass or less, even more preferably 60% by mass or less, from the viewpoints of the binding property of the conductive material and the adhesion to the substrate.
[0044] The (meth)acrylic acid alkyl ester contributes to the ease of synthesis and durability of the polymer (A). Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate. The (meth)acrylic acid alkyl ester may be used alone or in combination of two or more. Among these, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are preferred, with 2-ethylhexyl acrylate being more preferred. In the (meth)acrylic acid alkyl ester, from the viewpoint of good flexibility of the electrode binder, the alkyl group bonded to the (meth)acryloyloxy group preferably has 2 to 9 carbon atoms, more preferably 4 to 9 carbon atoms, and even more preferably an alkyl group having 4 to 9 carbon atoms bonded to the acryloyloxy group.
[0045] The proportion of the (meth)acrylic acid alkyl ester in the nonionic ethylenically unsaturated monomer (a1) is preferably 20 to 70% by mass, more preferably 30% by mass or more, even more preferably 40% by mass or more, and even more preferably 60% by mass or less, and even more preferably 50% by mass or less, from the viewpoints of the flexibility of the electrode binder, the binding property of the conductive material, and the adhesion to the substrate.
[0046] The polar group-containing ethylenically unsaturated carboxylic acid ester contributes to good polymerizability during synthesis of the polymer (A) and mechanical stability of the electrode binder. Examples of the polar group of the polar group-containing ethylenically unsaturated carboxylic acid ester include a hydroxy group and a cyano group. Examples of the polar group-containing ethylenically unsaturated carboxylic acid ester include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl acrylate, and (meth)acrylonitrile. The polar group-containing ethylenically unsaturated carboxylic acid ester may be used alone or in combination of two or more. Of these, 2-hydroxyethyl (meth)acrylate is preferred, and 2-hydroxyethyl methacrylate is more preferred.
[0047] The proportion of the polar group-containing ethylenically unsaturated carboxylic acid ester in the nonionic ethylenically unsaturated monomer (a1) is preferably 0.50 to 20% by mass, more preferably 1.0% by mass or more, even more preferably 2.0% by mass or more, and even more preferably 15% by mass or less, even more preferably 10% by mass or less, from the viewpoints of good polymerizability during synthesis of the polymer (A), binding properties of the conductive material and adhesion to the substrate, swelling resistance of the electrode binder during use of the battery, etc.
[0048] <Second Structural Unit> The second structural unit constituting the polymer (A) is derived from the anionic ethylenically unsaturated monomer (a2). In order to obtain a polymer (A) that fully exhibits the effects of the present invention, the content of the second structural unit in the total amount of the first structural unit, the second structural unit, and the third structural unit constituting the polymer (A) is preferably 1.5 to 20% by mass, more preferably 3.0% by mass or more, even more preferably 4.5% by mass or more, and more preferably 15% by mass or less, even more preferably 10% by mass or less.
[0049] The anionic ethylenically unsaturated monomer (a2) from which the second structural unit is derived has one ethylenically unsaturated bond per molecule and an anionic functional group. The anionic ethylenically unsaturated monomer (a2) may be used alone or in combination of two or more. Examples of the anionic functional group include a carboxy group, a sulfo group, and a phosphate group. The anionic functional group may form a salt. As the anionic ethylenically unsaturated monomer (a2), one or more selected from the group consisting of ethylenically unsaturated carboxylic acids and salts thereof, and ethylenically unsaturated sulfonic acids and salts thereof are preferably used, and it is more preferable to include both of these.
[0050] Examples of ethylenically unsaturated carboxylic acids and salts thereof include unsaturated monocarboxylic acids such as (meth)acrylic acid and crotonic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid and itaconic acid; half esters of unsaturated dicarboxylic acids, and salts thereof. The ethylenically unsaturated carboxylic acids and salts thereof may be used alone or in combination of two or more. Of these, (meth)acrylic acid and itaconic acid are preferred.
[0051] The proportion of the ethylenically unsaturated carboxylic acid and its salt in the anionic ethylenically unsaturated monomer (a2) is preferably 70 to 99% by mass, more preferably 80% by mass or more, even more preferably 85% by mass or more, and even more preferably 98% by mass or less, even more preferably 95% by mass or less, from the viewpoints of good polymerizability during synthesis of the polymer (A), binding properties of the conductive material, and adhesion to the substrate.
[0052] Examples of ethylenically unsaturated sulfonic acids and salts thereof include parastyrenesulfonic acid and salts thereof. The ethylenically unsaturated sulfonic acids may be used alone or in combination of two or more. Among these, sodium parastyrenesulfonate is preferred.
[0053] The proportion of the ethylenically unsaturated sulfonic acid and its salt in the anionic ethylenically unsaturated monomer (a2) is preferably 1.0 to 30% by mass, more preferably 2.0% by mass or more, even more preferably 3.0% by mass or more, and more preferably 20% by mass or less, even more preferably 15% by mass or less, from the viewpoints of good polymerizability during synthesis of the polymer (A), binding properties of the conductive material, and adhesion to the substrate.
[0054] <Third Structural Unit> The third structural unit constituting the polymer (A) is derived from the crosslinking agent (a3). From the viewpoint of the swelling resistance of the electrode binder during use of the battery, the content of the third structural unit in the total amount of the first structural unit, the second structural unit, and the third structural unit constituting the polymer (A) is preferably 0.010 to 0.50 mass%, more preferably 0.020 mass% or more, even more preferably 0.030 mass% or more, and more preferably 0.30 mass% or less, even more preferably 0.10 mass% or less.
[0055] The crosslinking agent (a3) from which the third structural unit is derived has two or more ethylenically unsaturated bonds in one molecule. The crosslinking agent (a3) may be used alone, or two or more types may be used in combination. The two or more ethylenically unsaturated bonds of the crosslinking agent (a3) can form a crosslinked structure by, for example, an addition reaction between the two or more ethylenically unsaturated bonds and the ethylenically unsaturated bonds of other synthesis raw material compounds of the polymer (A). In other words, the polymer (A) is a crosslinked polymer. Examples of the crosslinking agent (a3) include divinylbenzene, ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and 2-hydroxy-3-acryloyloxypropyl methacrylate. Of these, divinylbenzene is preferred.
[0056] <Glass Transition Temperature> The glass transition temperature of the polymer (A) is preferably −30 to 100° C. from the viewpoints of the binding property of the conductive material, adhesion to the substrate, good flexibility of the electrode binder, etc. It is more preferably −20° C. or higher, even more preferably −10° C. or higher, and more preferably 90° C. or lower, even more preferably 80° C. or lower.
[0057] <Particle size> The polymer (A) exists as dispersed particles in an electrode binder composition containing an aqueous dispersion medium. The suitable particle size of the dispersed particles varies depending on the form and particle size of the conductive material. To ensure that the effects of the present invention are fully exhibited, the median diameter D50 of the particles in the aqueous dispersion is preferably 0.10 to 1.0 μm. It is more preferably 0.15 μm or more, even more preferably 0.20 μm or more, and more preferably 0.80 μm or less, even more preferably 0.50 μm or less.
[0058] <Synthesis Method> The polymer (A) can be produced by polymerizing synthetic raw materials including a nonionic ethylenically unsaturated monomer (a1), an anionic ethylenically unsaturated monomer (a2), and a crosslinking agent (a3). The polymerization method is not particularly limited, and a suitable example is emulsion polymerization. Emulsion polymerization is carried out in an aqueous medium in the presence of a polymerization initiator, with the addition of a surfactant and other additives as necessary. The synthetic raw materials may be charged all at once or may be supplied successively by dropwise addition, for example. The reaction is usually carried out at 30 to 90°C with stirring.
[0059] From the viewpoint of the stability of the polymer (A) in the reaction system, it is preferable to add a basic substance during or after the polymerization reaction as necessary to neutralize and adjust the pH. Preferred examples of the basic substance include ammonia, triethylamine, ethanolamine, morpholine, 2-amino-2-methyl-1-propanol, lithium hydroxide, sodium hydroxide, potassium hydroxide, and calcium hydroxide. The basic substances may be used alone or in combination of two or more.
[0060] The aqueous medium is water, a hydrophilic solvent, or a mixture thereof. Examples of hydrophilic solvents include methanol, ethanol, isopropyl alcohol, N-methylpyrrolidone (NMP), and 1,3-butylene glycol. From the viewpoints of dispersion stability of the synthetic raw materials and the polymer, and reducing the environmental load, water is preferred as the aqueous medium. A mixture of water and a hydrophilic solvent is also preferred, as long as dispersion stability is not impaired. The aqueous medium used in the synthesis of polymer (A) may remain as is after synthesis as the aqueous medium constituting the electrode binder composition.
[0061] The amount of the aqueous medium used is adjusted as appropriate depending on the dispersibility of the synthetic raw materials in the aqueous medium, the viscosity of the reaction system, etc. From the viewpoint of moderate progress of the polymerization reaction, the amount of the aqueous medium used is preferably 50 to 300 parts by mass per 100 parts by mass of the total of the nonionic ethylenically unsaturated monomer (a1), the anionic ethylenically unsaturated monomer (a2), and the crosslinking agent (a3). It is more preferably 80 parts by mass or more, even more preferably 100 parts by mass or more, and more preferably 250 parts by mass or less, even more preferably 200 parts by mass or less.
[0062] The polymerization initiator is not particularly limited, but a radical polymerization initiator can be used, and examples thereof include peroxides such as ammonium persulfate, potassium persulfate, hydrogen peroxide, and tert-butyl hydroperoxide. The polymerization initiators may be used alone or in combination of two or more. Redox polymerization may also be performed using these polymerization initiators in combination with a reducing agent such as sodium bisulfite, Rongalite, or ascorbic acid.
[0063] From the viewpoint of the dispersion stability of the synthesis raw materials and the produced polymer (A) in an aqueous medium, the surfactant is preferably one or more selected from the group consisting of nonionic surfactants and anionic surfactants. Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyalkylene alkyl ethers, sorbitan fatty acid esters, and polyoxyethylene sorbitan fatty acid esters. The nonionic surfactants may be used alone or in combination of two or more. Examples of anionic surfactants include alkylbenzene sulfonates, alkyl sulfates, polyoxyethylene alkyl ether sulfates, and fatty acid salts.
[0064] As the anionic surfactant, a reactive surfactant having an ethylenically unsaturated bond is also suitably used. Examples of the reactive surfactant include compounds represented by the following formulas (1) to (4). The reactive surfactant may be used alone or in combination of two or more. Among these, the compound represented by formula (4) is preferred, and sodium alkylaryl sulfosuccinate is more preferred.
[0065] In formula (1), R 1 is an alkyl group, and p is an integer from 10 to 40. 1 is preferably an alkyl group having 10 to 40 carbon atoms, more preferably a straight chain alkyl group having 10 to 40 carbon atoms.
[0066] In formula (2), R 2 is an alkyl group, and q is an integer from 10 to 12. 2 is preferably an alkyl group having 10 to 40 carbon atoms, more preferably a straight chain alkyl group having 10 to 40 carbon atoms.
[0067] In formula (3), R 3 is an alkyl group, and M 1 is NH 4 Or Na. 3is preferably an alkyl group having 10 to 40 carbon atoms, more preferably a straight chain alkyl group having 10 to 40 carbon atoms.
[0068] In formula (4), R 4 is an alkyl group, and M 2 is NH 4 Or Na. 4 is preferably an alkyl group having 10 to 40 carbon atoms, more preferably a straight chain alkyl group having 10 to 40 carbon atoms.
[0069] The reactive surfactant not only exhibits an emulsifying effect on the reaction system in emulsion polymerization, but also has copolymerizability with the nonionic ethylenically unsaturated monomer (a1), the anionic ethylenically unsaturated monomer (a2), and the crosslinking agent (a3), but in this embodiment, it is not considered to be a structural unit constituting the polymer (A).
[0070] The amount of surfactant added is preferably 0.050 to 1.2 parts by mass per 100 parts by mass of the total of the nonionic ethylenically unsaturated monomer (a1), the anionic ethylenically unsaturated monomer (a2), and the crosslinking agent (a3), from the viewpoints of stable progress of the polymerization reaction, dispersion stability of the synthetic raw materials and the produced polymer (A) in the aqueous medium, adhesion of the conductive material to the substrate, etc. It is more preferably 0.10 parts by mass or more, even more preferably 0.15 parts by mass or more, and more preferably 1.0 part by mass or less, even more preferably 0.50 parts by mass or less.
[0071] Examples of other additives include chain transfer agents such as thiol, thiol glycolic acid and its esters, 3-mercaptopropionic acid and its esters, etc. The addition of other additives is optional, and may be added within a range that allows the production of polymer (A) that does not impair the effects of the present invention.
[0072] (Water-soluble cellulose derivative (B)) The electrode binder of the present embodiment contains the polymer (A) and preferably further contains a water-soluble cellulose derivative (B). The water-soluble cellulose derivative (B) serves to facilitate dispersion of the conductive material in the electrode slurry.
[0073] Examples of the water-soluble cellulose derivative (B) include celluloses and salts thereof such as methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose; polyvinyl alcohol; and polyvinylpyrrolidone. Examples of the salts of celluloses include ammonium salts and alkali metal salts. The water-soluble cellulose derivative (B) may be used alone or in combination of two or more. Among these, carboxymethyl cellulose and its salts are preferred.
[0074] When the water-soluble cellulose derivative (B) is contained in the electrode binder, its content is preferably 1 to 50% by mass from the viewpoint of obtaining good dispersibility of the conductive material without interfering with the function of the polymer (A). It is more preferably 5% by mass or more, even more preferably 10% by mass or more, and more preferably 40% by mass or less, even more preferably 30% by mass or less. The total content of the polymer (A) and the water-soluble cellulose derivative (B) in the electrode binder is preferably 80% by mass or more, more preferably 95% by mass or more, and may be 100% by mass.
[0075] [Electrode binder composition] The electrode binder composition contains the electrode binder of the present embodiment described above and an aqueous medium, and the polymer (A) is dispersed in the aqueous medium. The electrode binder composition can be produced by mixing the electrode binder and the aqueous medium. The mixing method is not particularly limited.
[0076] Examples of the aqueous medium in the electrode binder composition include the same aqueous medium as that used in the synthesis method of polymer (A) described above, and may be the same as or different from that used in the synthesis method of polymer (A). The aqueous medium may contain the aqueous medium used in the synthesis of polymer (A) that remains after the synthesis. From the viewpoints of dispersion stability of the electrode binder in the electrode binder composition, reduction of environmental load, etc., water is preferred as the aqueous medium. A mixture of water and a hydrophilic solvent is also preferred within a range that does not impair dispersion stability.
[0077] The content of the polymer (A) in the electrode binder composition can be appropriately adjusted by optionally adding an aqueous medium during production of the electrode slurry. From the viewpoints of viscosity that is easy to handle, dispersion stability of the polymer (A), and the like, the content is preferably 10 to 80 mass%, more preferably 15 mass% or more, even more preferably 20 mass% or more, and more preferably 70 mass% or less, even more preferably 60 mass% or less.
[0078] [Electrode Slurry] The electrode slurry of this embodiment contains the electrode binder of this embodiment, a conductive material, and an aqueous medium. The electrode slurry can be produced by mixing the electrode binder, the conductive material, and the aqueous medium. The mixing method is not particularly limited, but in order to sufficiently and homogeneously disperse the conductive material, it is preferable to knead the mixture using, for example, a planetary centrifugal mixer.
[0079] The electrode slurry may contain other components in addition to the electrode binder, conductive material, and aqueous medium, as long as the effects of the present invention are not impaired. Examples of other components include surfactants, etc., from the viewpoint of dispersion stability, etc. The total content of the electrode binder, conductive material, and aqueous medium in the electrode slurry is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 80% by mass or more, and may be 100% by mass. The aqueous medium in the electrode slurry is the same as that described above for the aqueous medium in the electrode binder composition.
[0080] Examples of conductive materials include carbon materials and metal materials. Examples of carbon materials include graphite, carbon black, and porous carbon. The conductive materials may be used alone or in combination of two or more. Among these, carbon materials are preferred, and porous carbon is more preferred, from the viewpoints of ease of handling and enzyme immobilization. Examples of porous carbon include mesoporous carbon, and specific examples include mesoporous carbon produced by a template method such as ketjen black, carbon nanotubes, graphene, and MgO-templated carbon. Among these, MgO-templated carbon is preferably used from the viewpoint of good enzyme immobilization.
[0081] The content of the conductive material in the electrode slurry is preferably 40 to 85% by mass, more preferably 45% by mass or more, even more preferably 50% by mass or more, and more preferably 80% by mass or less, even more preferably 75% by mass or less, from the viewpoint of ensuring that a sufficient amount of the conductive material adheres to the substrate.
[0082] The content of the electrode binder in the electrode slurry is preferably 10 to 200 parts by mass, more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, and more preferably 150 parts by mass or less, even more preferably 120 parts by mass or less, and even more preferably 60 parts by mass or less, relative to 100 parts by mass of the conductive material, as an amount sufficient for the conductive material to adhere to the substrate.
[0083] The total content of the electrode binder and the conductive material in the electrode slurry is preferably 40 to 80% by mass, more preferably 45% by mass or more, even more preferably 50% by mass or more, and more preferably 75% by mass or less, even more preferably 70% by mass or less, from the viewpoints of the applicability of the electrode slurry to screen printing, reduction in the amount used, etc.
[0084] The present invention will be described in detail below with reference to examples. The present invention is not limited to the following examples, and various modifications are possible within the scope of the present invention.
[0085] [Production of Polymer (A)] The methods for measuring various physical properties in the following synthesis examples are as follows. <Glass transition temperature> Differential scanning calorimetry (DSC) was measured using a differential scanning calorimeter ("EXSTAR DSC7020", manufactured by Hitachi High-Tech Science Corporation; heating rate 10°C / min, nitrogen gas atmosphere), and the peak top temperature of the DSC temperature derivative curve was taken as the glass transition temperature. <Median diameter D50> The median diameter D50 (volume basis) was determined from a particle size distribution curve measured by dynamic light scattering (DLS).
[0086] (Synthesis Example 1) A reaction vessel equipped with a condenser, thermometer, stirrer, and dropping funnel was charged with 60 parts by mass of ion-exchanged water and heated to 75 ° C. Into this reaction vessel, in the formulation shown in Table 1, a total of 100 parts by mass of nonionic ethylenically unsaturated monomer (a1), anionic ethylenically unsaturated monomer (a2), and crosslinker (a3), 0.20 parts by mass of Eleminol JS-20 (excluding solvent), 0.20 parts by mass of Hitenol 08E, and a mixed solution containing 80 parts by mass of ion-exchanged water were added dropwise over 3 hours and stirred and mixed. At the same time, a solution of 0.40 parts by mass of potassium persulfate dissolved in 10 parts by mass of ion-exchanged water was added dropwise over 3 hours, stirred and mixed, and polymerized. Two hours after the end of the dropwise addition, the reaction product was neutralized with 0.90 parts by mass of ammonia water with a concentration of 25% by mass, to obtain a dispersion of polymer (A1) (polymer (A1) content 40% by mass).
[0087]
[0088] Details of the surfactants in Table 1 are as follows: Eleminol JS-20: sodium alkylaryl sulfosuccinate; "Eleminol (registered trademark) JS-20" manufactured by Sanyo Chemical Industries, Ltd.; anionic reactive surfactant; non-volatile content 38.5% by mass Hitenol 08E: polyoxyethylene oleyl cetyl ether ammonium sulfate; "Hitenol (registered trademark) 08E" manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.; anionic surfactant
[0089] The polymer (A1) had a glass transition temperature of 15° C. and a median diameter D50 of 0.26 μm.
[0090] [Production of Electrode Slurry] The raw materials used in the production of the electrode slurry are as follows: Porous carbon powder: "Knobel (registered trademark) MJ(3)100-00" manufactured by Toyo Tanso Co., Ltd.; BET specific surface area: 390 m 2 / g, total pore volume 0.91 mL / g, micropore volume 0.15 mL / g, mesopore diameter 75 nm, bulk density 0.06 g / mL Electrode binder composition (1): dispersion of polymer (A1) (electrode binder) produced in Synthesis Example 1 (non-volatile content 40% by mass) Electrode binder composition (2): "Kureha KF Polymer L#9305" manufactured by Kureha Corporation; 5 mass% NMP solution of PVDF ("Kureha KF Polymer L#9300": electrode binder) Electrode binder composition (3): styrene-butadiene rubber (electrode binder) latex (non-volatile content 40% by mass) Electrode binder composition (4): PTFE (electrode binder) aqueous dispersion (non-volatile content 60% by mass)
[0091] The porous carbon powder, the electrode binder composition, and the additive medium were blended in the compositions shown in Table 2 and kneaded with a planetary centrifugal mixer to produce electrode slurries 1 to 9. As shown in Table 2, the dispersibility of the porous carbon powder in the obtained electrode slurries was good (◯) for electrode slurries 1 to 8, and poor (×) for electrode slurry 9.
[0092] [Production of Biofuel Cells] Biofuel cells were produced by the following method using electrode slurries 1 to 9. Examples use electrode slurries 1 to 6, and comparative examples use electrode slurries 7 to 9.
[0093] Details of the materials and raw materials used in the construction of the biofuel cell are given below. Substrate (Japanese paper): Water-repellent rice paper; Izumo Japanese paper Substrate (oil-resistant and water-resistant paper): "Oil-resistant and water-resistant paper (3)", manufactured by Lintec Corporation Carbon paste: "JELCON CH-8", manufactured by Jujo Chemical Co., Ltd. AzBTS: 2,2'-azinobis(3-ethylbenzothiazoline-6-ammonium sulfonate); manufactured by Tokyo Chemical Industry Co., Ltd. TTF: tetrathiafulvalene GOD: glucose oxidase; manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Phosphate buffer: 1 mol / L phosphate buffer, pH 7.0 BOD: bilirubin oxidase; manufactured by Amano Enzyme Inc. Triton X-100: polyethylene glycol-tert-octylphenyl ether; "Triton (registered trademark) X-100"; manufactured by Roche Diagnostics; nonionic surfactant
[0094] A carbon paste was screen-printed on the substrate and dried at 120°C for 20 minutes to form a lead. An electrode slurry containing 0.04 g of AzBTS as a mediator was then screen-printed three times onto the lead, followed by drying at 45°C for 30 minutes to form 32 20 mm x 5 mm electrodes. The electrodes were then subjected to UV ozone cleaning for 15 minutes. The electrode pattern consisted of four anodes and four cathodes connected in series and four in parallel. A saturated methanol solution of TTF was dripped onto the anode portion of the electrode, and 20 μL of a solution (10 U / μL) containing GOD dispersed in phosphate buffer was dripped onto each anode. A solution (10 U / μL) containing BOD dispersed in a phosphate buffer solution containing 0.01% Triton X-100 by mass was dropped onto the cathode portion of the electrode, at a rate of 20 μL per cathode. The electrode (patterned electrode) was then dried under reduced pressure for 1 hour to produce an enzyme electrode plate with GOD immobilized on the anode and BOD immobilized on the cathode. The enzyme electrode plates using Japanese paper as the substrate were prepared using electrode slurries 1, 7, and 8, while the enzyme electrode plates using oil-resistant and water-resistant paper were prepared using electrode slurries 1 to 6. Because electrode slurry 9 had poor dispersibility, a biofuel cell was not produced using it (Comparative Example 3).
[0095] In addition, a phosphate buffer solution containing glucose at a concentration of 0.1 mol / L was dropped (1 mL / cm) onto another substrate. 2 ) and dried at 100°C for 30 minutes to prepare a glucose-containing substrate. This glucose-containing substrate was placed on the enzyme electrode of the enzyme electrode plate to produce a biofuel cell.
[0096] [Evaluation of Output Characteristics] The output of each biofuel cell produced by the above method was measured by linear sweep voltammetry (measurement conditions: two-electrode method, scanning potential open circuit voltage 0 V, scanning rate 1 mV / s) to determine the maximum output. The liquid supply during measurement was performed by dropping 1 mol / L phosphate buffer solution (pH 7.0). Table 2 shows the measured maximum output values.
[0097]
[0098] As shown in Table 2, it was confirmed that the biofuel cell produced using electrode slurry 1 exhibited good output characteristics (Example 1). It can also be said that the biofuel cells produced using electrode slurries 2 to 6 exhibited good output characteristics (Examples 2 to 6). On the other hand, the biofuel cells produced using electrode slurries 7 and 8 exhibited poor output characteristics (Comparative Examples 1 and 2). From the above, it can be said that the biofuel cells produced using the electrode slurry containing the aqueous electrode binder of this embodiment exhibit good output characteristics.
[0099] REFERENCE SIGNS LIST 1 substrate 2 anode 3 cathode 4 lead portion 5 covering sheet 6 skin 10, 20 biofuel cell
Claims
1. A biofuel cell that generates electricity through an oxidation-reduction reaction catalyzed by an enzyme, wherein an enzyme is immobilized on at least one of an anode and a cathode, the anode comprising a conductive material (1) and an electrode binder (1), the cathode comprising a conductive material (2) and an electrode binder (2), at least one of the electrode binders (1) and (2) comprising a polymer (A), the polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), and the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
2. A biofuel cell that generates electricity through an oxidation-reduction reaction catalyzed by an enzyme, wherein at least one of an anode and a cathode comprises a conductive material and an electrode binder, and an enzyme is immobilized thereon, the electrode binder comprises a polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), and the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
3. An electrode for a biofuel cell comprising a conductive material and an electrode binder, wherein the electrode binder comprises a polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), and the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
4. An enzyme electrode, comprising the electrode for a biofuel cell according to claim 3 on which an enzyme is immobilized.
5. An electrode slurry for a biofuel cell comprising an electrode binder, a conductive material and an aqueous medium, wherein the electrode binder comprises a polymer (A) having a first structural unit derived from a nonionic ethylenically unsaturated monomer (a1), a second structural unit derived from an anionic ethylenically unsaturated monomer (a2), and a third structural unit derived from a crosslinking agent (a3), and the crosslinking agent (a3) has two or more ethylenically unsaturated bonds in one molecule.
6. The electrode slurry for biofuel cells according to claim 5, wherein the content of the electrode binder is 10 to 200 parts by mass per 100 parts by mass of the conductive material.
Citation Information
Patent Citations
Electrolyte material composition, membrane electrode jointing agent, electrolyte membrane with jointing layer, membrane-electrode assembly, and polymer electrolyte fuel cell
JP2010170837A
Aqueous catalyst paste composition for fuel batteries, and fuel battery
JP2015028932A
Toner
JP2022189436A
Porous membrane for secondary battery, separator for secondary battery, and secondary battery
WO2013005796A1
Cited By
Lactic acid sensor for horse and method for measuring lactic acid in horse
WO2026186673A1