Tire rubber composition, method for producing tire rubber composition, tire rubber material, method for producing tire rubber material, and reclaimed rubber
The rubber composition for heavy-duty tires, combining recycled rubber with fumed silica and a silane coupling agent, addresses the trade-off between wear resistance and fuel efficiency, achieving superior performance in wear resistance, breaking strength, and fatigue crack resistance, while being environmentally friendly.
Patent Information
- Application Number
- PCT/JP2024/012319
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Heavy-duty tires face a trade-off between wear resistance and fuel efficiency, and existing rubber compositions containing recycled rubber do not adequately address the requirements for wear resistance, breaking strength, and fatigue crack resistance, especially when blended with recycled materials.
A rubber composition for tires is developed, blending 5-100 parts of recycled rubber containing fumed silica with diene rubber, along with a silane coupling agent, to achieve improved wear resistance, breaking strength, and fatigue crack resistance, while maintaining fuel efficiency, using a method that involves kneading and vulcanizing these components to create a suitable tire rubber material.
The resulting tire rubber material exhibits excellent wear resistance, breaking strength, fatigue crack resistance, and fuel efficiency, making it suitable for heavy-duty tires and environmentally friendly, with properties comparable to or better than those without recycled rubber, and outperforming compositions with carbon black.
Smart Images

Figure JP2024012319_03102024_PF_FP_ABST
Abstract
Description
Rubber composition for tires, method for producing rubber composition for tires, rubber material for tires, method for producing rubber material for tires, and reclaimed rubber
[0001] The present invention relates to a rubber composition for tires, a rubber material for tires, methods for producing the same, and reclaimed rubber.
[0002] Automobile tires are required to have various properties such as wear resistance, low fuel consumption, wet grip, etc. For example, based on environmental regulations such as labeling systems in Japan and Europe and smart way regulations in North America, there is a demand for tires to achieve low fuel consumption, particularly by reducing rolling resistance.
[0003] Among automobile tires, heavy-duty tires used on trucks, buses, etc. are required to have a longer running life and to not develop cracks in the tires when subjected to applied loads, compared to passenger car tires. That is, wear resistance, breaking strength, and fatigue crack resistance are particularly required. However, because there is a trade-off between wear resistance and fuel economy, it is difficult for heavy-duty tires to achieve both wear resistance and fuel economy at the same time.
[0004] From the viewpoint of reducing the burden on the environment and making effective use of resources, recycled rubber obtained by recycling used rubber materials is being used. For example, JIS K 6313 defines recycled rubber as rubber obtained by recycling used rubber from automobile tires, tubes, and other rubber products, and as having specified performance properties.
[0005] However, rubber compositions for tires containing such recycled rubber have reduced properties required for tires, so there has been no incentive to actively incorporate recycled rubber into rubber compositions for tires, and recycled rubber has been viewed as a mere additive that merely increases the volume of the rubber composition for tires.
[0006] Patent Document 1 discloses a rubber composition for tires in which natural rubber is blended with reclaimed rubber containing carbon black, a carbon coupling agent, and wet silica, and discloses that this rubber composition improves tensile break properties and low heat buildup.
[0007] Furthermore, Patent Document 2 discloses a rubber composition in which the hydrogen content of carbon black as a reinforcing filler is reduced, and discloses that this rubber composition can improve fatigue crack resistance.
[0008] JP 2018-123272 A International Publication No. 2016 / 024397
[0009] However, the rubber composition for a tire described in Patent Document 1 has not been evaluated for abrasion resistance and fatigue crack resistance, and there is a problem that the rubber composition for a tire is not suitable for a heavy-duty tire. The rubber composition for a tire described in Patent Document 2 has a problem that the abrasion resistance and fatigue crack resistance are insufficient.
[0010] The present invention has been made in view of the above circumstances, and has an object to provide a rubber material for tires that exhibits a good balance of abrasion resistance, breaking strength, fatigue crack resistance, and fuel economy even when blended with recycled rubber, a rubber composition for tires that is suitable for the rubber material for tires, methods for producing them, and recycled rubber that is suitable for the rubber composition for tires.
[0011] From the above, the aspects of the present invention are as follows.
[0012] [1] A rubber composition for a tire, comprising 5 to 100 parts by mass of recycled rubber containing fumed silica per 100 parts by mass of diene rubber. [2] The rubber composition for a tire according to [1], further comprising 5 to 90 parts by mass of fumed silica. [3] The rubber composition for a tire according to [1], further comprising 0.1 to 30 parts by mass of a silane coupling agent. [4] The rubber composition for a tire according to [2], further comprising 0.1 to 30 parts by mass of a silane coupling agent.
[0013] [5] A rubber material for a tire obtained by vulcanizing the rubber composition for a tire according to any one of [1] to [4]. [6] The rubber material for a tire according to [5], which has a tear strength TS of 40 kN / m or more.
[0014] [7] A method for producing a rubber composition for a tire, comprising a step of kneading a diene rubber and a reclaimed rubber containing fumed silica to obtain a rubber composition for a tire, wherein 5 to 100 parts by mass of the reclaimed rubber containing fumed silica are blended per 100 parts by mass of the diene rubber. [8] A method for producing a rubber composition for a tire according to [7], further comprising blending and kneading a masterbatch obtained by kneading a diene rubber and fumed silica in the step of obtaining a rubber composition for a tire, wherein 5 to 100 parts by mass of the reclaimed rubber containing fumed silica are blended per 100 parts by mass of the total of the diene rubber contained in the masterbatch and the diene rubber blended in the step of obtaining a rubber composition for a tire. [9] A method for producing a rubber composition for a tire according to [7] or [8], further comprising a step of treating a rubber material containing fumed silica to obtain reclaimed rubber containing fumed silica.
[10] The method for producing a rubber composition for a tire according to any one of [7] to [9], wherein, in the step of obtaining a rubber composition for a tire, 5 to 90 parts by mass of fumed silica are further blended and kneaded with respect to 100 parts by mass of the diene rubber blended in the step of obtaining a rubber composition for a tire, or with respect to a total of 100 parts by mass of the diene rubber contained in the masterbatch and the diene rubber blended in the step of obtaining a rubber composition for a tire.
[11] The method for producing a rubber composition for a tire according to any one of [7] to
[10] , wherein, in the step of obtaining a rubber composition for a tire, 0.1 to 30 parts by mass of a silane coupling agent are further blended and kneaded with respect to 100 parts by mass of the diene rubber blended in the step of obtaining a rubber composition for a tire, or with respect to a total of 100 parts by mass of the diene rubber contained in the masterbatch and the diene rubber blended in the step of obtaining a rubber composition for a tire.
[0015]
[12] A method for producing a rubber material for a tire, comprising a step of vulcanizing the rubber composition for a tire obtained by the method for producing a rubber composition for a tire according to any one of [7] to
[11] .
[0016]
[13] A reclaimed rubber containing fumed silica.
[14] The reclaimed rubber according to
[11] , containing 5 parts by mass or more and 90 parts by mass or less of fumed silica per 100 parts by mass of the rubber component contained in the reclaimed rubber.
[0017] According to the present invention, it is possible to provide a rubber material for tires that has good abrasion resistance even when blended with reclaimed rubber, a rubber composition for tires that is suitable for the rubber material for tires, methods for producing them, and reclaimed rubber that is suitable for the rubber composition for tires.
[0018] FIG. 1 is a process diagram of a method for producing a rubber composition for tires and a rubber material for tires using a masterbatch and recycled rubber.
[0019] The present invention will be described in detail below based on specific embodiments in the following order: 1. Rubber composition for tires 1.1. Diene rubber 1.2. Reclaimed rubber 1.3. Fumed silica 1.4. Silane coupling agent 1.5. Other components 2. Method for producing rubber composition for tires 3. Rubber material for tires
[0020] (1. Rubber Composition for Tire) The rubber composition for tire according to this embodiment is a kneaded product used to obtain a rubber material for tire, and contains at least a diene rubber and reclaimed rubber.
[0021] (1.1. Diene-Based Rubber) Examples of diene-based rubbers contained in the rubber composition for a tire according to this embodiment include natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, butyl rubber, ethylene-propylene-diene rubber, chloroprene rubber, etc. Among these, at least one selected from natural rubber and isoprene rubber is preferred, natural rubber or natural rubber and isoprene rubber is more preferred, and natural rubber is even more preferred.
[0022] Examples of natural rubber include natural rubber (NR) and modified natural rubbers such as epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), deproteinized natural rubber (DPNR), and high-purity natural rubber (HPNR). These natural rubbers may be used alone or in combination of two or more.
[0023] (1.2. Reclaimed Rubber) In this embodiment, reclaimed rubber is rubber that has been reclaimed by processing a rubber material. The rubber material before processing (before being reclaimed) is preferably vulcanized rubber, and the vulcanized rubber may be used rubber such as waste, or may be rubber before use. Examples of processing that is performed on the rubber material include crushing and devulcanization. In this embodiment, reclaimed rubber is preferably rubber that has been devulcanized after vulcanization. There are no particular restrictions on used rubber as long as it is an ordinary rubber material, but examples include automobile tires, tubes, etc.
[0024] In this embodiment, the reclaimed rubber contains fumed silica. That is, the rubber material before being reclaimed contains fumed silica. Fumed silica is finely divided silicon dioxide produced by high-temperature hydrolysis of silicon tetrachloride in an oxyhydrogen flame. Therefore, fumed silica is also called dry silica because its production method differs from that of wet silica, which is produced by wet methods such as precipitation and gelation. Fumed silica has a smaller primary particle size of primary aggregates (smallest constituents) and a larger nitrogen adsorption BET specific surface area than wet silica. Fumed silica particles aggregate and fuse together in a beaded shape, forming bulky aggregates.
[0025] By including fumed silica in the recycled rubber, the properties (abrasion resistance, breaking strength, fatigue crack resistance, fuel economy, etc.) of the tire rubber material obtained by compounding the recycled rubber are comparable to those of a tire rubber material of the same composition that does not contain recycled rubber, and are better than the properties of a tire rubber material that contains carbon black. Therefore, tire rubber materials obtained by compounding recycled rubber containing fumed silica are suitable for heavy-duty tires. In other words, the recycled rubber can be used as an additive to improve the properties of tire rubber materials.
[0026] In this embodiment, the BET specific surface area of the fumed silica contained in the reclaimed rubber is 50 m 2 / g or more, 80m 2 / g or more, 120m 2 / g or more, 200m 2 / g or more, 250m 2 / g or more, 300m 2 / g or more, 350m 2 When the BET specific surface area of the fumed silica is within the above range, a sufficient number of silanol groups that serve as reaction sites with other components can be ensured.
[0027] The upper limit of the BET specific surface area of the fumed silica contained in the reclaimed rubber is not particularly limited, but is, for example, 500 m 2 / g. If the BET specific surface area of the fumed silica is too small, the flame temperature during production of the fumed silica must be increased, which tends to result in the loss of the structure unique to fumed silica and the inability to produce fumed silica stably. If the BET specific surface area of the fumed silica is too large, it tends to result in the inability to produce fumed silica stably.
[0028] Fumed silica is divided into hydrophilic and hydrophobic fumed silica based on its properties toward water. Fumed silica has silanol groups on its surface. These silanol groups are chemically active and particularly reactive with water. Therefore, surface treatment (hydrophobic treatment) is sometimes performed to reduce the reactivity with water by reacting the silanol groups with other substances. Hydrophobically treated fumed silica is called hydrophobic fumed silica, while untreated fumed silica is called hydrophilic fumed silica.
[0029] In this embodiment, hydrophobic fumed silica and hydrophilic fumed silica are distinguished by the degree of modified hydrophobicity (M value) shown below. The degree of modified hydrophobicity (M value) is a value obtained by a measurement method utilizing the fact that hydrophobic fumed silica floats in water but is completely suspended in methanol. The method described in the examples of WO 2004 / 099075 can be used to measure the M value. When hydrophobic fumed silica and hydrophilic fumed silica are represented by the M value, hydrophobic fumed silica has an M value of 1 or more, and hydrophilic fumed silica has an M value of less than 1.
[0030] In this embodiment, the fumed silica contained in the reclaimed rubber is preferably hydrophilic fumed silica. When the reclaimed rubber contains hydrophilic fumed silica, the properties of the rubber material for tires obtained by blending the reclaimed rubber tend to be further improved.
[0031] It is known that wet silica reduces the abrasion resistance of rubber materials for tires compared to carbon black, and therefore wet silica is not compounded into heavy-duty tires. In other words, reclaimed rubber made from used heavy-duty tires does not contain wet silica. Furthermore, fumed silica is difficult to mix with rubber components due to its bulkiness, and therefore tires containing fumed silica are not commercially available. In other words, reclaimed rubber made from used tires does not contain fumed silica.
[0032] The rubber composition for tires according to this embodiment is obtained by blending 5 to 100 parts by mass of reclaimed rubber per 100 parts by mass of diene rubber. By blending the amount of reclaimed rubber within the above range, the tire rubber material has properties suitable for heavy-duty tires, and can be an environmentally friendly product with a high degree of recyclability. The amount of reclaimed rubber blended per 100 parts by mass of diene rubber is preferably 7 parts by mass or more, and more preferably 9 parts by mass or more. On the other hand, the amount of reclaimed rubber blended per 100 parts by mass of diene rubber is preferably 70 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 40 parts by mass or less, and particularly preferably 35 parts by mass or less.
[0033] Reclaimed rubber contains a rubber component and fumed silica, and in the manufacturing method of a rubber composition for tires described below, before the diene rubber and reclaimed rubber are kneaded, the rubber component in the reclaimed rubber is distinguished from the diene rubber. After the diene rubber and reclaimed rubber are kneaded, the rubber component is integrated with the diene rubber in the kneaded product. The composition of the rubber component in the reclaimed rubber may be the same as or different from the diene rubber.
[0034] In the reclaimed rubber, the fumed silica is preferably contained in an amount of 5 parts by mass or more and 90 parts by mass or less, more preferably 10 parts by mass or more and 70 parts by mass or less, and even more preferably 15 parts by mass or more and 55 parts by mass or less, per 100 parts by mass of the rubber component.
[0035] The reclaimed rubber may contain components other than the rubber component and fumed silica, such as coupling agents such as silane coupling agents, lubricants (stearic acid, oil, etc.), and fillers (carbon black, wet silica, etc.).
[0036] (1.3. Fumed Silica) The rubber composition for a tire may contain components other than the above-mentioned components (diene rubber and reclaimed rubber). In this embodiment, the rubber composition for a tire is preferably blended with fumed silica in addition to the above-mentioned components. It is believed that blending fumed silica in addition to the above-mentioned components makes it easier to form a structure attributable to fumed silica in the rubber composition for a tire. As a result, the presence of such a structure in the rubber material for a tire obtained by vulcanizing the rubber composition for a tire is believed to improve the abrasion resistance of the rubber material for a tire.
[0037] In the manufacturing method of a rubber composition for tires described below, before the fumed silica and reclaimed rubber are kneaded, the fumed silica is distinguished from the fumed silica in the reclaimed rubber. After the fumed silica and reclaimed rubber are kneaded, the fumed silica is integrated with the fumed silica in the reclaimed rubber in the kneaded mixture.
[0038] The type, physical properties, etc. of the fumed silica to be blended may be the same as or different from the type, physical properties, etc. of the fumed silica contained in the reclaimed rubber. The above explanation regarding the fumed silica contained in the reclaimed rubber can be applied to the blended fumed silica. Therefore, it is preferable that the blended fumed silica is hydrophilic fumed silica. In addition, the BET specific surface area of the blended fumed silica is 50 m, similar to the fumed silica contained in the reclaimed rubber. 2 / g or more, 80m 2 / g or more, 120m 2 / g or more, 200m 2 / g or more, 250m 2 / g or more, 300m 2 / g or more, 350m 2 The upper limit of the BET specific surface area of the fumed silica to be blended is not particularly limited, but it is preferably 500 m 2 / g.
[0039] In the rubber composition for tires, the blending amount of fumed silica is preferably 5 parts by mass or more and 90 parts by mass or less per 100 parts by mass of diene rubber. By blending the amount of fumed silica within the above range, the abrasion resistance and fatigue crack resistance of the rubber material for tires can be improved.
[0040] The amount of fumed silica is preferably 8 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, per 100 parts by mass of diene rubber, while the amount of fumed silica is preferably 80 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 55 parts by mass or less, per 100 parts by mass of diene rubber.
[0041] Furthermore, in the rubber composition for tires, the content of fumed silica, i.e., the total of the blended fumed silica and the fumed silica in the reclaimed rubber, is preferably 5 to 90 parts by mass, more preferably 10 to 70 parts by mass, and even more preferably 15 to 55 parts by mass, per 100 parts by mass of the total of the diene rubber and the rubber components in the reclaimed rubber. If the content of fumed silica is too low, the resulting rubber material for tires tends to have insufficient abrasion resistance and fatigue crack resistance. If the content of fumed silica is too high, the fumed silica does not disperse sufficiently in the diene rubber, and a good kneaded product tends not to be obtained.
[0042] (1.4. Silane Coupling Agent) In this embodiment, the rubber composition for a tire preferably contains a silane coupling agent in addition to the above-described components. By including the silane coupling agent, a crosslinked structure between the diene rubber and the fumed silica is easily formed via the silane coupling agent. As a result, the dispersibility of the fumed silica in the rubber composition for a tire is improved, and the abrasion resistance and fatigue crack resistance of the rubber material for a tire can be improved.
[0043] In the manufacturing method of a rubber composition for tires described below, when a silane coupling agent is contained in the reclaimed rubber, the silane coupling agent is distinguished from the silane coupling agent in the reclaimed rubber before the silane coupling agent and the reclaimed rubber are kneaded together, and after the silane coupling agent and the reclaimed rubber are kneaded together, the silane coupling agent is integrated with the silane coupling agent in the reclaimed rubber in the kneaded mixture.
[0044] The type and physical properties of the silane coupling agent to be blended may be the same as or different from the type and physical properties of the silane coupling agent contained in the reclaimed rubber. The silane coupling agent to be blended is not particularly limited as long as it is one that is commonly used in rubber compositions. In this embodiment, a sulfur-containing silane coupling agent is preferred. Examples of sulfur-containing silane coupling agents include bis-(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, 3-trimethoxysilylpropylbenzothiazole tetrasulfide, γ-mercaptopropyltriethoxysilane, 3-octanoylthiopropyltriethoxysilane, and mercapto-thiocarboxylate oligomer.
[0045] In this embodiment, from the viewpoint of the heat resistance (thermal aging resistance) of the rubber composition for tires, the silane coupling agent to be blended is preferably a blocked mercaptosilane, and particularly preferably a mercapto-thiocarboxylate oligomer.
[0046] Mercapto-thiocarboxylate oligomers are oligomers of thiocarboxylates having a mercapto group. Examples of the molecular structure of mercapto-thiocarboxylate oligomers are shown below. In the molecular structure shown below, the sum (x+y) of the number of repetitions of linking unit A (x) and the number of repetitions of linking unit B (y) is preferably in the range of 3 to 300. Within this range, the mercaptosilane of linking unit B can be bonded to the -CH of linking unit A. 15 Since the mercapto-thiocarboxylate oligomer is covered with the mercapto-thiocarboxylate oligomer, it is possible to prevent the scorch time from becoming shorter and to ensure good reactivity with the fumed silica and diene rubber. A specific example of the mercapto-thiocarboxylate oligomer is "NXT-Z45" manufactured by Momentive.
[0047]
[0048] In the rubber composition for tires, the blending amount of the silane coupling agent is preferably 0.1 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the diene rubber. By blending the amount of the silane coupling agent within the above range, it is possible to easily obtain a rubber material for tires that can realize good fuel economy performance in addition to good abrasion resistance and fatigue crack resistance.
[0049] The amount of the silane coupling agent is preferably 1.5 parts by mass or more, more preferably 2.0 parts by mass or more, and even more preferably 2.5 parts by mass or more, per 100 parts by mass of the diene rubber, while the amount of the silane coupling agent is preferably 27 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, per 100 parts by mass of the diene rubber.
[0050] Furthermore, in the rubber composition for tires, the content of the silane coupling agent, i.e., the total of the silane coupling agent blended and the silane coupling agent in the reclaimed rubber, is preferably 0.1 to 30 parts by mass, more preferably 2.0 to 25 parts by mass, and even more preferably 2.5 to 20 parts by mass, per 100 parts by mass of the total of the diene rubber and the rubber components in the reclaimed rubber. If the content of the silane coupling agent is too low, the dispersibility of the fumed silica in the rubber composition for tires tends to be insufficient. If the content of the silane coupling agent is too high, the silane coupling agents tend to condense with each other, which may result in insufficient improvement in the abrasion resistance and fatigue crack resistance of the resulting rubber material for tires.
[0051] Furthermore, within the range of the amount of silane coupling agent to be compounded per 100 parts by mass of diene rubber or rubber component, it is preferable to increase the amount of silane coupling agent compounded relatively as the BET specific surface area of fumed silica increases. This is because sufficient reaction points with the fumed silica can be secured. Specifically, the amount of silane coupling agent is 0.33 to 1 mg / m relative to the specific surface area of the silica to be added. 2 It is particularly preferable to add it in the range of
[0052] (1.4. Other Components) In this embodiment, the rubber composition for a tire may contain components that are blended into rubber compositions in addition to the above-mentioned components (diene rubber, reclaimed rubber, fumed silica, and silane coupling agent). An example of such a component is a lubricant. Blending a lubricant improves the kneadability of each component, making it easier to obtain a rubber composition for a tire in which each component is well dispersed.
[0053] Examples of lubricants include stearic acid and process oil. Examples of process oil include aromatic oil, paraffin oil, naphthenic oil, etc. The lubricants may be used alone or in combination of two or more.
[0054] The amount of lubricant blended is not limited as long as the effects of the present invention can be obtained. For example, the amount of lubricant blended is preferably 1 part by mass or more and 40 parts by mass or less, more preferably 2 parts by mass or more and 35 parts by mass or less, and even more preferably 3 parts by mass or more and 30 parts by mass or less, per 100 parts by mass of diene rubber.
[0055] If the amount of lubricant is too small, the viscosity will be high and kneading will be poor, which may prevent the abrasion resistance and fatigue crack resistance of the resulting tire rubber material from being sufficiently improved.If the amount of lubricant is too large, shear will not be applied during kneading, which may prevent the fumed silica from being sufficiently dispersed in the diene rubber.
[0056] Furthermore, the rubber composition for tires may contain a reinforcing filler other than fumed silica. Examples of reinforcing fillers include carbon black, wet silica, clay, mica, talc, calcium carbonate, aluminum hydroxide, aluminum oxide, and titanium oxide. When a reinforcing filler is compounded, an appropriate amount of a filler coupling agent may also be compounded. The amount of the reinforcing filler to be compounded is not limited as long as the effects of the present invention can be obtained, and a general compounding amount may be used.
[0057] Furthermore, the rubber composition for a tire may contain various additives such as zinc oxide, an antioxidant, a plasticizer, a processing aid, a liquid polymer, a thermosetting resin, etc. The amount of these additives to be added is not limited as long as the effects of the present invention can be obtained, and may be a general amount.
[0058] (2. Method for producing rubber composition for tire) The rubber composition for tire according to this embodiment is obtained by kneading the diene rubber described above, the reclaimed rubber described above, and, as necessary, other components (fumed silica, silane coupling agent, lubricant, reinforcing filler, various additives). In this embodiment, in the step of kneading the diene rubber and the reclaimed rubber, it is preferable to further add and knead the fumed silica described above and the silane coupling agent described above, and it is also preferable to further add and knead at least one of the lubricant, reinforcing filler, and various additives.
[0059] In this embodiment, the rubber composition for a tire may be produced by kneading predetermined components to prepare a master batch, and then blending and kneading the remaining components into the master batch, or by kneading all of the components together.
[0060] When preparing the masterbatch, the above-described diene rubber is kneaded with other components (fumed silica, silane coupling agent, lubricant, reinforcing filler, various additives, reclaimed rubber, etc.) In this embodiment, it is preferable to prepare the masterbatch by kneading at least the diene rubber and fumed silica, and it is more preferable to prepare the masterbatch by kneading at least the diene rubber, fumed silica, and silane coupling agent.
[0061] In the present embodiment, the masterbatch may contain 13 parts by mass or more and 130 parts by mass or less, 15 parts by mass or more and 110 parts by mass or less, or 20 parts by mass or more and 100 parts by mass or less of fumed silica per 100 parts by mass of diene-based rubber.
[0062] In addition, in this embodiment, the masterbatch may contain, in addition to the fumed silica, 1 part by mass or more and 40 parts by mass or less of a silane coupling agent, 1.5 parts by mass or more and 30 parts by mass or less, or 2 parts by mass or more and 20 parts by mass or less, per 100 parts by mass of diene-based rubber.
[0063] In this embodiment, the masterbatch is preferably a kneaded product to be kneaded with compounding components containing at least a rubber component, i.e., the masterbatch is preferably kneaded with other compounding components containing at least a rubber component to become a part of the rubber composition for a tire.
[0064] When the masterbatch contains fumed silica, the content ratio of fumed silica relative to the rubber component in the masterbatch is preferably higher than the content ratio of fumed silica relative to all rubber components in a rubber composition for a tire containing the masterbatch. That is, the concentration of fumed silica relative to the amount of rubber components in the masterbatch is preferably higher than the concentration of fumed silica relative to the amount of rubber components in the rubber composition for a tire. In other words, in this embodiment, the masterbatch is preferably a kneaded product containing fumed silica at a high concentration.
[0065] As a kneading device for preparing the masterbatch, for example, a Banbury mixer, a kneader, or other known kneading device can be used.
[0066] After preparing the masterbatch, other components are blended with the masterbatch and kneaded to obtain a rubber composition for tires. In this embodiment, it is preferable to knead the masterbatch, reclaimed rubber, diene rubber, and other components, as shown in Figure 1. The masterbatch and other components can be kneaded using a known kneading device such as a Banbury mixer or kneader.
[0067] When all the components are kneaded to produce a rubber composition for tires, all the components may be simultaneously or successively charged into a known kneading device such as a Banbury mixer or a kneader and kneaded.
[0068] The kneading conditions may be set so that the components are thoroughly kneaded.
[0069] (3. Rubber Material for Tires) The rubber material for tires according to this embodiment is a material obtained by vulcanizing the rubber composition for tires described above. Therefore, the rubber material for tires contains the components derived from recycled rubber described above. As a result, the rubber material for tires can exhibit excellent abrasion resistance, breaking strength, fatigue crack resistance, and fuel economy. In other words, despite containing the components derived from recycled rubber, the rubber material for tires according to this embodiment has properties comparable to those of a rubber material for tires of the same composition that does not contain recycled rubber. Furthermore, compared to a rubber material for tires that does not contain recycled rubber but contains carbon black, the rubber material for tires according to this embodiment has an excellent balance of abrasion resistance, breaking strength, fatigue crack resistance, and fuel economy.
[0070] In particular, the tear strength TS of the rubber material for a tire according to the present embodiment is preferably 40 kN / m or more, more preferably 42 kN / m or more, and even more preferably 44 kN / m or more. The upper limit of the tear strength is not particularly limited, but is, for example, 200 kN / m.
[0071] The tear strength TS can be measured in accordance with JIS K6252-1. The curve showing the change in tear force obtained by the measurement is analyzed in accordance with JIS K6274, and the tear strength TS can be calculated from the analysis results. The detailed measurement method will be described in the Examples.
[0072] Therefore, the reclaimed rubber containing the above-mentioned fumed silica effectively functions as an additive for improving the properties of rubber materials.
[0073] The rubber material for a tire according to the present embodiment is excellent in abrasion resistance, breaking strength, fatigue crack resistance, and fuel economy, and therefore can be suitably used for tires for trucks and buses, etc. Also, it can be suitably used for each component of a tire, particularly for the tread, base tread, sidewall, clinch, etc.
[0074] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments and may be modified in various ways within the scope of the present invention.
[0075] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0076] (Experiment 1) (Preparation of Masterbatch) The following components were charged into a pressure kneader with a volume of 0.5 L so that the compounding amounts per 100 parts by mass of diene rubber were as shown in Table 1. After charging, the components were kneaded for about 30 minutes at a rotor rotation speed of 20 to 40 rpm so that the temperature of the kneaded mixture was in the range of 130 to 160°C. The air cylinder pressure was 0.7 MPa. After kneading was completed, the mixture was cooled to room temperature and removed to obtain a masterbatch (Production Example).
[0077] The materials were then charged into a 0.6 L Labo Plastomill (Model BB600, manufactured by Toyo Seiki Seisaku-sho) so that the compounding amounts per 100 parts by mass of diene rubber were as shown in Table 1. After charging, the mixture was kneaded for about 5 to 10 minutes at a rotor rotation speed of 20 to 40 rpm so that the temperature of the kneaded mixture was in the range of 120 to 140°C. After kneading was completed, the mixture was cooled to room temperature and removed to obtain a masterbatch (standard production example). (A) Diene rubber (A-1) Natural rubber (manufactured in Thailand, RSS3) (B) Filler (B-1) Hydrophilic fumed silica (manufactured by Tokuyama, Reolosil QS-30C, nitrogen adsorption BET specific surface area: 300 m 2 / g, tap density: 100 g / L) (B-2) Carbon black (Tokai Carbon, Seast 6, nitrogen adsorption BET specific surface area: 120 m 2 / g, tap density: 400g / L) (C) Silane coupling agent (C-1) Mercapto-thiocarboxylate oligomer (NXT-Z45, manufactured by Momentive) (E) Other components (E-1) Lubricant (stearic acid, NOF Corp., Beads Stearic Acid YR) (E-2) Process oil (Extract No. 4 S (TDAE Oil) manufactured by Showa Shell Sekiyu Co., Ltd.) (E-3) Antioxidant (Ozonone 6C, manufactured by Seiko Chemical Co., Ltd.) (E-4) Lubricant (zinc oxide, Seido Chemical Co., Ltd., zinc oxide type 3)
[0078]
[0079] (Preparation of rubber composition for tires) The obtained masterbatch, the above components as needed, and the reclaimed rubber (E-4) shown below were charged into a 0.6 L volume Labo Plastomill (Model BB600 manufactured by Toyo Seiki Seisaku-sho, Ltd.). After charging, the mixture was kneaded for about 10 minutes at a rotor rotation speed of 20 to 100 rpm so that the temperature of the kneaded mixture was in the range of 130 to 160°C. After kneading was completed, the mixture was cooled to room temperature to obtain a kneaded mixture.
[0080] To the resulting kneaded product, the following (E-5) and (E-6) were added and mixed using a 6-inch roll tester to obtain a rubber composition for tires. The formulation of the resulting rubber composition for tires is shown in Table 2. (D) Reclaimed rubber (D-1) Fumed silica-containing reclaimed rubber (D-2) Carbon black-containing tire reclaimed rubber (Tire Reclaimed Rubber AP, manufactured by Asahi Reclaimed Rubber Co., Ltd.) (E) Other components (E-4) Lubricant (Zinc oxide, manufactured by Seido Chemical, zinc oxide type 3) (E-5) Sulfur (Fine sulfur containing Kinkaji oil, manufactured by Tsurumi Chemical Industry Co., Ltd.) (E-6) Vulcanization accelerator (N-(tert-butyl)-2-benzothiazole sulfenamide (TBBS), manufactured by Sanshin Chemical Industry, Suncerer NS-G)
[0081] The fumed silica-containing reclaimed rubber used was the reclaimed rubber shown below. The tire rubber composition shown in Reference Example 1 in Table 2 was press-vulcanized at 150°C for 10 minutes to obtain a rubber material, which was then heat-aged in a dryer at 80°C for 120 hours. The rubber material after heat aging was then subjected to a devulcanization treatment to obtain reclaimed rubber. The obtained reclaimed rubber satisfied the requirements of JIS K 6313.
[0082]
[0083] (Preparation of tire rubber material) Subsequently, the obtained tire rubber composition was press-vulcanized at 150°C for 10 minutes to obtain a tire rubber material. Test specimens for the following evaluations were prepared from the obtained tire rubber material. The obtained test specimens were used to evaluate the following physical properties.
[0084] (Shore A Hardness) For the test pieces of the obtained tire rubber material, the hardness (Shore A hardness) was measured using a durometer in accordance with JIS K6253 Type A. The results are shown in Table 2.
[0085] (Break Strength) The obtained rubber composition for a tire was vulcanized at 160°C for T90+1 minute using a 2 mm thick mold, and the obtained vulcanized rubber sheet was punched out with a JIS No. 3 dumbbell to prepare a sample. The strength at break (break strength) of this sample was measured using a tensile tester in accordance with JIS K6251. The results are shown in Table 2.
[0086] (Fuel efficiency performance: tan δ at 60°C) Test pieces of the obtained rubber material for tires were measured in accordance with JIS K6394 using a dynamic viscoelasticity tester (VR-7130 manufactured by Ueshima Seisakusho) under the following conditions. Tan δ (60°C) was calculated from the measured value at 60°C. Measurement temperature: 60°C Static strain: 10% Dynamic strain: ±2% Frequency: 10 Hz
[0087] The rolling resistance index was calculated using the following formula, with the calculated tan δ at 60°C of Comparative Example 1 (Standard Example 1) set at 100. The higher the index, the better the rolling resistance. The results are shown in Table 2. (Rolling resistance index) = 100 x (tan δ at 60°C of Standard Example 1) / (tan δ at 60°C of Examples and Comparative Examples)
[0088] (Wear resistance performance: FPS abrasion amount) For the test pieces of the obtained rubber material for tires, the FPS abrasion amount was measured using an FPS abrasion tester (AB-2012 manufactured by Ueshima Seisakusho) under conditions of a temperature of 20°C, a load of 40 N, a slip ratio of 10%, and a test time of 2 minutes. The abrasion index was calculated using the following formula, with the FPS abrasion amount of Comparative Example 1 (Standard Example 1) taken as 100. The higher the index, the better the abrasion resistance performance. The results are shown in Table 2. (Wear index) = 100 × (FPS abrasion amount of Standard Example 1) / (FPS abrasion amount of Examples and Comparative Examples)
[0089] From Table 2, it was confirmed that tire rubber materials containing recycled rubber containing fumed silica exhibit properties comparable to those of tire rubber materials of the same composition that do not contain recycled rubber. It was also confirmed that tire rubber materials containing recycled rubber containing fumed silica have better properties than tire rubber materials containing carbon black.
[0090] (Experiment 2) A rubber material for a tire was obtained by the same method as in Experiment 1, using the masterbatches (Production Example and Standard Production Example) prepared in Experiment 1 and each of the components (A) to (E) so as to obtain the formulation shown in Table 3. Note that, instead of the carbon black-containing tire reclaimed rubber, reclaimed rubber (D-2) was obtained by subjecting a rubber material obtained by vulcanizing the rubber composition shown in Comparative Example 11 (Standard Example 11) in Table 3 to a devulcanization treatment. This reclaimed rubber satisfied the requirements of JIS K 6313. The treatment conditions for vulcanization, heat aging, and devulcanization were the same as those for the fumed silica-containing reclaimed rubber in Experiment 1.
[0091] As shown in Table 3, the composition of Reference Example 11 is the same as the composition of Reference Example 1, the compositions of Examples 11 to 13 are the same as the compositions of Examples 1 to 3, and the compositions of Comparative Examples 11 to 14 are the same as the compositions of Comparative Examples 1 to 4.
[0092]
[0093] Test specimens were prepared from the resulting tire rubber material, and the fatigue crack resistance was evaluated as follows.
[0094] (Fatigue crack resistance: tear strength) Test pieces of the obtained rubber material were punched out into rectangular shapes with long sides of 130 mm and short sides of 40 mm, and a 70 mm long incision was made from the midpoint of the short side in the long side direction to obtain trouser-shaped test pieces. The thickness of the test pieces was 1 mm. A tensile test was conducted on the trouser-shaped test pieces at a tensile speed of 100 mm / min in accordance with JIS K6252-1, and the tear strength until the test piece broke was measured. The measured tear strength was analyzed based on JIS K6274, and the tear strength was calculated. The results are shown in Table 3. In addition, the calculated tear strength TS of Comparative Example 11 (Standard Example 11) was set to 100, and the tear strength index was calculated for Reference Example 11, Examples 11 to 13, and Comparative Examples 12 to 13 using the following calculation formula. The higher the index, the better the fatigue crack resistance. The results are shown in Table 3. (Tensile strength index) = 100 × (tear strength of Examples and Comparative Examples) / (tear strength of Standard Example 11)
[0095] From Table 3, it was confirmed that tire rubber materials containing recycled rubber containing fumed silica exhibit properties comparable to those of tire rubber materials of the same composition that do not contain recycled rubber. It was also confirmed that tire rubber materials containing recycled rubber containing fumed silica have better properties than tire rubber materials containing carbon black.
Claims
1. A rubber composition for tires, comprising 100 parts by mass of diene rubber and 5 parts by mass or more and 100 parts by mass or less of recycled rubber containing fumed silica.
2. The rubber composition for tires according to claim 1, further comprising 5 to 90 parts by mass of fumed silica.
3. The rubber composition for tires according to claim 1, further comprising 0.1 to 30 parts by mass of a silane coupling agent.
4. The rubber composition for tires according to claim 2, further comprising 0.1 to 30 parts by mass of a silane coupling agent.
5. A rubber material for tires obtained by vulcanizing the rubber composition for tires according to any one of claims 1 to 4.
6. The rubber material for tires according to claim 5, which has a tear strength TS of 40 kN / m or more.
7. A method for producing a rubber composition for tires, comprising a step of kneading diene rubber and recycled rubber containing fumed silica to obtain a rubber composition for tires, in which 5 parts by mass or more and 100 parts by mass or less of recycled rubber containing fumed silica are blended per 100 parts by mass of diene rubber.
8. A method for producing a rubber composition for tires according to claim 7, further comprising blending and kneading a master batch obtained by kneading a diene rubber and fumed silica in the step of obtaining a rubber composition for tires, and blending 5 parts by mass or more and 100 parts by mass or less of the recycled rubber containing the fumed silica per 100 parts by mass of the diene rubber contained in the master batch and the diene rubber blended in the step of obtaining a rubber composition for tires.
9. The method for producing a rubber composition for tires according to claim 7, further comprising the step of treating a rubber material containing fumed silica to obtain reclaimed rubber containing said fumed silica.
10. A method for producing a rubber composition for tires according to claim 7, wherein in the step of obtaining the rubber composition for tires, 5 parts by mass or more and 90 parts by mass or less of fumed silica is further blended and kneaded per 100 parts by mass of the diene rubber.
11. A method for producing a rubber composition for tires according to claim 7, wherein in the step of obtaining the rubber composition for tires, 0.1 parts by mass or more and 30 parts by mass or less of a silane coupling agent is further compounded and kneaded relative to 100 parts by mass of the diene rubber.
12. A method for producing a rubber material for tires, comprising a step of vulcanizing a rubber composition for tires obtained by the method for producing a rubber composition for tires according to any one of claims 7 to 11.
13. Reclaimed rubber containing fumed silica.
14. The reclaimed rubber according to claim 13, comprising 5 parts by mass or more and 90 parts by mass or less of fumed silica per 100 parts by mass of the rubber component contained in the reclaimed rubber.
Citation Information
Patent Citations
Desulfurization method for used crosslinked rubber, reclaimed rubber composition therefrom and polymer composition including the same
JP2006232885A
Elastomer composite material containing silica-containing filler and method for manufacturing the same
JP2013537257A
Method for producing silica and carbon black reinforced elastomeric composites and products containing same
JP2018524450A
Method for producing rubber composition
JP2022072813A