Catalyst-carrying electrode
The catalyst-supported electrode with low surface porosity and vapor-deposited layers addresses performance deterioration issues, achieving efficient and durable carbon dioxide conversion to formic acid with improved retention and energy efficiency.
Patent Information
- Application Number
- PCT/JP2024/012414
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional catalyst-supported electrodes experience performance deterioration with repeated use, leading to reduced efficiency in converting carbon dioxide into useful compounds like formic acid, particularly due to high-temperature and high-pressure requirements in existing techniques.
A catalyst-supported electrode with a surface porosity of less than 20% and a vapor-deposited catalyst layer containing elements like Bi or Sn, optionally with an intermediate layer, is designed to improve catalyst performance retention, using a vapor deposition method to enhance durability and reduce thickness variation.
The electrode maintains higher catalyst performance retention and efficiency in converting carbon dioxide to formic acid under mild conditions, reducing equipment space requirements and energy consumption.
Smart Images

Figure JP2024012414_03102024_PF_FP_ABST
Abstract
Description
Catalyst-supported electrode
[0001] The present invention relates to a catalyst-supported electrode.
[0002] There are high hopes for technology that can convert carbon dioxide into useful compounds as a means of solving the problems of global warming and fossil fuel depletion.
[0003] Formic acid is an excellent compound for storing hydrogen and carbon dioxide because it requires low energy for dehydrogenation and is easy to handle, and can be used in the above-mentioned technologies. Hydrogenation reactions and artificial photosynthesis are well-known as representative technologies for producing formic acid from carbon dioxide. However, these technologies have issues, such as the need for high temperature and pressure conditions and the need for energy to concentrate the dilute product.
[0004] Therefore, electrolysis technology, which produces formic acid from carbon dioxide and water using electrical energy, has many advantages, such as the reaction proceeding under mild conditions, the ability to produce relatively high concentrations of formic acid, the absence of the need for hydrogen, and space-saving equipment, and is therefore desirable for social implementation.
[0005] For example, Patent Document 1 describes an electrolytic cell including a catalyst layer containing catalytically active elements dispersed in an ion-conducting polymer. The catalyst layer described in Patent Document 1 is formed by applying an ink containing the catalytically active elements.
[0006] Patent No. 6568326
[0007] There was room for improvement in conventional catalyst-supported electrodes, particularly in the case of catalyst performance degradation after repeated use.
[0008] Therefore, an object of the present invention is to provide a catalyst-supported electrode that is suitable for improving the performance maintenance rate of the catalyst.
[0009] The present invention provides a catalyst-supported electrode for converting carbon dioxide into a reaction product, comprising: a substrate; and a catalyst layer disposed on the substrate and containing an element M1 that functions as a catalytically active species, wherein the surface porosity of the catalyst layer is less than 20%.
[0010] The present invention further provides a catalyst-supported electrode for converting carbon dioxide into a reaction product, comprising: a substrate; and a catalyst layer disposed on the substrate and containing an element M1 that functions as a catalytically active species, wherein the catalyst layer is a vapor-deposited layer.
[0011] The present invention further provides an electrolysis device for converting carbon dioxide into reaction products, the electrolysis device comprising the above catalyst-supported electrode.
[0012] According to the present invention, it is possible to provide a catalyst-supported electrode that is suitable for improving the performance maintenance rate of the catalyst.
[0013] FIG. 1 is a cross-sectional view schematically showing a first example of a catalyst-supported electrode according to this embodiment. FIG. 2 is a cross-sectional view schematically showing a second example of a catalyst-supported electrode according to this embodiment. FIG. 3 is a cross-sectional view schematically showing a third example of a catalyst-supported electrode according to this embodiment. FIG. 4 is a cross-sectional view schematically showing a fourth example of a catalyst-supported electrode according to this embodiment. FIG. 5 is a cross-sectional view schematically showing an example of an electrolysis device 100 according to this embodiment. FIG. 6 shows an SEM image (magnification: 5000 times) and a binarized image of an arbitrary point on the surface of the catalyst layer of electrode sample 1.
[0014] A catalyst-supported electrode according to a first aspect of the present invention is a catalyst-supported electrode for converting carbon dioxide into a reaction product, comprising: a substrate; and a catalyst layer disposed on the substrate and containing an element M1 that functions as a catalytically active species, wherein the surface porosity of the catalyst layer is less than 20%.
[0015] A catalyst-supported electrode according to a second aspect of the present invention is a catalyst-supported electrode for converting carbon dioxide into a reaction product, comprising: a substrate; and a catalyst layer disposed on the substrate and containing an element M1 that functions as a catalytically active species, wherein the catalyst layer is a vapor-deposited layer.
[0016] In a third aspect of the present invention, for example, in the catalyst-supported electrode according to the first aspect, the surface porosity is less than 10%.
[0017] In a fourth aspect of the present invention, for example, in the catalyst-supported electrode according to any one of the first to third aspects, the catalyst layer contains the element M1 as a main component.
[0018] In a fifth aspect of the present invention, for example, in the catalyst-supported electrode according to any one of the first to fourth aspects, the element M1 is Bi or Sn.
[0019] In a sixth aspect of the present invention, for example, in the catalyst-supported electrode according to any one of the first to fifth aspects, the catalyst layer further contains an element M2 different from the element M1.
[0020] In a seventh aspect of the present invention, for example, the catalyst-supported electrode according to any one of the first to sixth aspects further includes an intermediate layer disposed between the substrate and the catalyst layer, wherein the substrate contains an element X, and the intermediate layer contains the element M1 and the element X.
[0021] In an eighth aspect of the present invention, for example, the catalyst-supported electrode according to any one of the first to seventh aspects further comprises a base layer disposed between the substrate and the catalyst layer and in contact with a surface of the substrate, wherein the substrate contains an element X, and the base layer contains the element X.
[0022] In a ninth aspect of the present invention, for example, the catalyst-supported electrode according to any one of the first to sixth aspects further comprises: an underlayer disposed between the substrate and the catalytic layer and in contact with a surface of the substrate; and an intermediate layer disposed between the underlayer and the catalytic layer, wherein the substrate contains element X as a main component, the catalytic layer contains element M1 as a main component, the intermediate layer contains element M1 and element X, and the underlayer contains element X.
[0023] In a tenth aspect of the present invention, for example, in the catalyst-supported electrode according to the ninth aspect, the value of y1 calculated by the following formula (I) is −5.0 or less: y1=(−0.1203)x1+(−0.0426)x2+(−0.0112)x5+(−0.0476)x6+0.1388x7+2.2919 (I) In the formula (I), x1 is the volume ratio (%) of the element M1 in the catalyst layer, x2 is the volume ratio (%) of the element M1 in the intermediate layer, x5 is the thickness (nm) of the catalyst layer, x6 is the thickness (nm) of the intermediate layer, and x7 is the thickness (nm) of the base layer.
[0024] In an eleventh aspect of the present invention, for example, in the catalyst-supported electrode according to the tenth aspect, the value of y3 calculated by the following formulas (II) and (III) is 0.5 or more. y2 = 0.0260x1 + (-0.0286)x2 + 0.1193x3 + (-0.0384)x4 + (-0.1413)x5 + (-0.0247)x6 + 0.2141x7 + 5.5788 (II) y3 = y2 / y1 (III) In the formula (II), x1 is the volume ratio (%) of the element M1 in the catalyst layer, x2 is the volume ratio (%) of the element M1 in the intermediate layer, x3 is the volume ratio (%) of the element X in the intermediate layer, x4 is the volume ratio (%) of the element X in the base layer, x5 is the thickness (nm) of the catalyst layer, x6 is the thickness (nm) of the intermediate layer, and x7 is the thickness (nm) of the base layer.
[0025] In a twelfth aspect of the present invention, for example, in the catalyst-supported electrode according to any one of the seventh to eleventh aspects, the element X is carbon (C).
[0026] In a thirteenth aspect of the present invention, for example, in the catalyst-supported electrode according to any one of the first to twelfth aspects, the thickness of the catalyst layer is 1 nm or more and 5000 nm or less.
[0027] In a fourteenth aspect of the present invention, for example, in the catalyst-supported electrode according to any one of the first to thirteenth aspects, the substrate is porous.
[0028] In a fifteenth aspect of the present invention, for example, in the catalyst-supported electrode according to any one of the first to fourteenth aspects, the catalytically active species is a catalyst that reduces the carbon dioxide.
[0029] An electrolysis device according to a sixteenth aspect of the present invention is an electrolysis device for converting carbon dioxide into a reaction product, comprising the catalyst-supported electrode according to any one of the first to fifteenth aspects.
[0030] The present invention will be described in detail below, but the following description is not intended to limit the present invention to a specific embodiment.
[0031] <Catalyst-supported electrode> Fig. 1 is a cross-sectional view schematically showing a first example of a catalyst-supported electrode according to this embodiment. The catalyst-supported electrode 10 is an electrode having a catalyst for converting carbon dioxide into a reaction product. The catalyst-supported electrode 10 includes a substrate 1 and a catalyst layer 2 disposed on the substrate 1. The catalyst layer 2 contains an element M1 that functions as a catalytically active species. The surface porosity of the catalyst layer 2 is less than 20%.
[0032] The surface porosity of the catalyst layer 2 is the proportion of voids on the surface of the catalyst layer 2. The surface of the catalyst layer 2 is the surface of the catalyst layer 2 opposite the substrate 1, for example, the surface of the catalyst-supported electrode 10. The surface porosity of the catalyst layer 2 can be measured, for example, by the following method. Using a scanning electron microscope (SEM), five or more arbitrary points on the surface of the catalyst layer 2 are observed at a magnification of 5000 times from a direction perpendicular to the surface. From the obtained SEM image, voids present on the surface of the catalyst layer 2 are identified, and the average proportion thereof is determined as the surface porosity.
[0033] The surface porosity of the catalyst layer 2 is preferably less than 10%, 8% or less, 6% or less, 5% or less, less than 5%, 4.5% or less, or even 4.3% or less. A catalyst layer 2 with a surface porosity small enough to satisfy the above numerical range is easily produced by the vapor deposition method described below. A catalyst-supported electrode 10 with a small surface porosity of the catalyst layer 2 reduces deterioration of catalyst performance due to repeated use and is suitable for improving performance retention compared to conventional catalyst-supported electrodes. The lower limit of the surface porosity of the catalyst layer 2 is not particularly limited, and is, for example, 0% or more, 0.5% or more, 1.0% or more, 1.5% or more, 2.0% or more, or even 2.1% or more.
[0034] The catalyst layer 2 has, for example, a vapor-deposited film containing the element M1 that functions as a catalytically active species, and is typically the vapor-deposited film itself. The vapor-deposited layer makes it easy to adjust the surface porosity of the catalyst layer 2 to a small value.
[0035] In another aspect, the present invention provides a catalyst-supported electrode (10) for converting carbon dioxide into a reaction product, the catalyst-supported electrode (10) comprising: a substrate (1); and a catalyst layer (2) disposed on the substrate (1) and containing an element (M1) functioning as a catalytically active species, wherein the catalyst layer (2) is a vapor-deposited layer.
[0036] The catalyst layer 2 is supported on, for example, the substrate 1 (specifically, on one surface of the substrate 1).
[0037] In the catalyst layer 2, the element M1 functions as a catalytically active species in a reaction that electrolyzes carbon dioxide and converts it into a reaction product. The catalytically active species, for example, reduces carbon dioxide. The catalyst-supported electrode 10 is typically a cathode. The reaction product obtained by conversion from carbon dioxide using the catalyst-supported electrode 10 is typically an organic compound. The organic compound is, for example, formic acid. The catalyst-supported electrode 10 may be an electrode for converting carbon dioxide into one type of reaction product, or may be an electrode for converting carbon dioxide into two or more types of reaction products.
[0038] Specifically, the catalyst layer 2 includes a material containing the element M1. The catalyst layer 2 may be made essentially of a material containing the element M1. The material is, for example, a metal catalyst. The metal catalyst may include a simple metal or an alloy. The metal catalyst may include a metal oxide or a metal composite oxide. That is, the metal catalyst may include the element M1 as a simple metal or may include the element M1 as an alloy of the element M1 and another element.
[0039] The catalytic layer 2 may contain the element M1 as a main component. In this specification, "main component" means the component that is contained in the largest amount on a volume basis. The content of the element M1 in the catalytic layer 2 may be 50 vol% or more, 55 vol% or more, 60 vol% or more, 65 vol% or more, or even 70 vol% or more. The content of the element M1 in the catalytic layer 2 may be 100 vol% or less. The content of the element M1 in the catalytic layer 2 is, for example, 50 vol% or more and 100 vol% or less. The catalytic layer 2 may consist essentially of the element M1.
[0040] The content of element M1 in the catalyst layer 2 can be calculated, for example, by measuring the element distribution in the thickness direction of the catalyst layer 2 by repeatedly etching the surface of the catalyst layer 2 and performing X-ray photoelectron spectroscopy (XPS) analysis, or by element mapping of a cross section of the catalyst layer 2 by energy dispersive X-ray analysis (EDX) using a transmission electron microscope (TEM).
[0041] The element M1 is, for example, one element selected from the group consisting of Bi, Sn, V, Cr, Mn, Fe, Co, Ni, Cu, Zr, Nb, Mo, Ru, Rh, Pd, Ag, Cd, Hf, Ta, W, Re, Ir, Pt, Au, Hg, Al, Si, In, Tl, Pb, Sb, Te, U, Sm, Tb, La, Ce, and Nd. The element M1 may be Bi or Sn, or may be Bi.
[0042] The catalytic layer 2 may contain an element M2 different from the element M1. The element M2 may be an element that functions as a catalytically active species, such as an element exemplified as the element M1. With this configuration, the catalyst-supported electrode 10 can further improve the catalyst performance maintenance rate. When the catalytic layer 2 contains two or more elements that function as catalytically active species, the element that is contained in the largest amount by volume among these elements is referred to as the element M1, and the remaining elements are referred to as the elements M2.
[0043] The element M2 may be Bi or Sn, or may be Sn. The element M1 may be Bi and the element M2 may be Sn.
[0044] The catalytic layer 2 may contain the element M1 and the element M2 as simple metals, or may contain an alloy of the element M1 and the element M2. The catalytic layer 2 may contain Bi and Sn as simple metals, or may contain an alloy of Bi and Sn.
[0045] The thickness of the catalyst layer 2 is not particularly limited and is, for example, 1 nm or more and 5000 nm or less. The thickness of the catalyst layer 2 is preferably 4000 nm or less, and may be 3000 nm or less, 2000 nm or less, 1000 nm or less, 800 nm or less, 500 nm or less, 300 nm or less, 200 nm or less, 150 nm or less, or even 110 nm or less. In some cases, the thickness of the catalyst layer 2 may be 100 nm or less, 90 nm or less, 70 nm or less, or even 50 nm or less. The thickness of the catalyst layer 2 is, for example, 10 nm or more. A catalyst layer 2 having a small thickness that satisfies the above numerical range can be easily produced by the vapor deposition method described below. A small thickness of the catalyst layer 2 allows for space-saving equipment.
[0046] The substrate 1 functions as, for example, a support for supporting the catalyst layer 2. The substrate 1 preferably has electrical conductivity. The substrate 1 preferably has gas diffusibility. The substrate 1 may be porous.
[0047] The substrate 1 contains element X. Element X and element M1 are different elements. Element X may be an element that does not function as a catalytically active species. Element X is, for example, one selected from carbon (C), Si, Ni, Pt, Cu, Ti, Cr, F, and Al, and is preferably C. In some cases, element X may be one of the elements exemplified as element M1. The substrate 1 may contain element X as a major component. The content of element X in the substrate 1 may be, for example, 70 vol% or more, 80 vol% or more, 90 vol% or more, or even 95 vol% or more. The content of element X in the substrate 1 may be 100 vol% or less. The substrate 1 may consist essentially of element X. The content of element X in the substrate 1 can be measured in the same manner as the content of element M1 in the catalyst layer 2 described above.
[0048] The substrate 1 may contain carbon as a main component. A known material can be used as the substrate 1, and examples thereof include carbon supports such as carbon paper and carbon cloth. The carbon support is preferably porous. The substrate 1 may also be a glassy carbon (GC) electrode.
[0049] The substrate 1 may further include a microporous layer (MPL) formed on the carbon support. The microporous layer includes, for example, a binder such as Teflon (registered trademark) and carbon particles. Since the surface structure of the catalyst layer 2 tends to depend on the structure of the substrate 1, the surface of the catalyst layer 2 formed on the substrate 1 including the MPL may have a relatively flat structure and a small surface porosity.
[0050] The catalyst layer 2 may be in contact with the substrate 1 .
[0051] The method for manufacturing a catalyst-supported electrode according to this embodiment includes forming a catalyst layer 2 containing an element M1 that functions as a catalytically active species, for example, by a vapor deposition method. For example, the catalyst-supported electrode 10 can be manufactured by the following method. First, a substrate 1 is prepared. Next, a vapor deposition method is performed to form the catalyst layer 2 on the substrate 1. More specifically, a vapor deposition layer containing the element M1 is formed on the substrate 1 by the vapor deposition method. In this manner, the catalyst-supported electrode 10 including the substrate 1 and the catalyst layer 2 can be obtained.
[0052] In this specification, vapor deposition means vapor phase deposition. In other words, the vapor deposition method is synonymous with the vapor phase deposition method. The vapor deposition method is typically a physical vapor deposition method such as a sputtering method. In the sputtering method, for example, a target containing a metal for forming a metal catalyst is used. The conditions for the vapor deposition method can be appropriately set depending on the composition and thickness of the desired catalyst layer 2.
[0053] According to the manufacturing method of this embodiment, the surface porosity of the catalyst layer 2 can be easily adjusted to a small value, and the catalyst-supported electrode of this embodiment can be easily fabricated. Furthermore, unlike conventional coating methods, the manufacturing method of this embodiment does not require the use of solvents such as organic solvents. Therefore, by adopting the manufacturing method of this embodiment, the amount of waste liquid can be reduced. Furthermore, since no organic solvent is used, there is an advantage in that there is no risk of fire caused by the organic solvent. Compared to conventional coating methods, the vapor deposition method not only makes it easy to adjust the surface porosity of the catalyst layer 2 to a small value, but also makes it easy to reduce the thickness of the catalyst layer 2 and tends to suppress thickness variation. The vapor deposition method is suitable for fabricating a catalyst layer 2 over a large area and can be said to have high productivity.
[0054] The method for manufacturing the catalyst-supported electrode 10 is not limited to the above. For example, the catalyst layer 2 may be manufactured by depositing metal particles of the element M1 on the substrate 1 by a spray method or the like. However, from the viewpoint of ensuring mass productivity and large-area capability, it is preferable to manufacture the catalyst layer 2 by a vapor deposition method.
[0055] FIG. 2 is a cross-sectional view schematically illustrating a second example of a catalyst-supported electrode according to this embodiment. The catalyst-supported electrode 20 includes a substrate 1, a catalyst layer 2, and an intermediate layer 3 disposed between the substrate 1 and the catalyst layer 2. The intermediate layer 3 contains an element M1 and an element X. Except for the intermediate layer 3, the configuration of the catalyst-supported electrode 20 is the same as that of the catalyst-supported electrode 10 of the first example. Therefore, elements common to the catalyst-supported electrode 10 of the first example and the catalyst-supported electrode 20 of the second example are denoted by the same reference numerals, and their description may be omitted. In other words, the following descriptions of the examples may be mutually applicable unless technically inconsistent. Furthermore, the examples may be combined with each other unless technically inconsistent.
[0056] The intermediate layer 3 may contain Bi as the element M1 and C (carbon) as the element X.
[0057] The intermediate layer 3 has, for example, a vapor-deposited film containing the element M1 and the element X, and is typically the vapor-deposited film itself.
[0058] The catalyst-supported electrode 20 including the intermediate layer 3 makes it difficult for the catalyst to fall off from the catalyst-supported electrode 20. This makes the catalyst-supported electrode 20 more suitable for improving the performance maintenance rate of the catalyst.
[0059] The intermediate layer 3 may consist essentially of the element M1 and the element X.
[0060] The content of element M1 in intermediate layer 3 may be 60 vol% or more, 70 vol% or more, 80 vol% or more, or even 85 vol% or more. The content of element M1 in intermediate layer 3 may be less than 100 vol% or may be 98 vol% or less. The content of element M1 in intermediate layer 3 is, for example, 70 vol% or more and 98 vol% or less.
[0061] The content of element X in the intermediate layer 3 is, for example, greater than 0 vol% and preferably equal to or greater than 2 vol%. The content of element X in the intermediate layer 3 may be equal to or less than 40 vol%, equal to or less than 30 vol%, equal to or less than 20 vol%, or even equal to or less than 15 vol%. The content of element X in the intermediate layer 3 is, for example, equal to or greater than 2 vol% and equal to or less than 30 vol%.
[0062] The contents of the element M1 and the element X in the intermediate layer 3 can be measured in the same manner as the content of the element M1 in the catalyst layer 2 described above.
[0063] The thickness of the intermediate layer 3 is not particularly limited and is, for example, 1 nm or more and 3000 nm or less. The thickness of the intermediate layer 3 may be preferably 2000 nm or less, 1000 nm or less, 800 nm or less, 500 nm or less, 300 nm or less, 200 nm or less, 100 nm or less, 50 nm or less, or even 45 nm or less. In some cases, the thickness of the intermediate layer 3 may be 40 nm or less, 30 nm or less, or even 20 nm or less. The thickness of the intermediate layer 3 is, for example, 1 nm or more, 2 nm or more, or 5 nm or more. An intermediate layer 3 having a small thickness that satisfies the above numerical range is easily produced by a vapor deposition method.
[0064] The intermediate layer 3 may join the substrate 1 and the catalyst layer 2. The intermediate layer 3 may be in contact with the catalyst layer 2, or may be in contact with the substrate 1 and the catalyst layer 2.
[0065] The catalyst-supported electrode 20 can be manufactured in the same manner as the catalyst-supported electrode 10 of the first example, except that, for example, a vapor deposition method is performed to form the intermediate layer 3 on the substrate 1, and then the catalyst layer 2 is formed on the intermediate layer 3. In detail, a vapor-deposited layer containing the element M1 and the element X is formed on the substrate 1 by the vapor deposition method, and then a vapor-deposited layer containing the element M1 is further formed on the vapor-deposited layer. In this manner, the catalyst-supported electrode 20 including the substrate 1, the catalyst layer 2, and the intermediate layer 3 can be obtained.
[0066] In the manufacturing method of this embodiment, a co-sputtering method may be performed using a target containing carbon together with a target containing metal. The co-sputtering method tends to facilitate the production of the intermediate layer 3 containing the element M1 and the element X.
[0067] 3 is a cross-sectional view schematically showing a third example of a catalyst-supported electrode according to the present embodiment. The catalyst-supported electrode 30 includes a substrate 1, a catalyst layer 2, and an underlayer 4 disposed between the substrate 1 and the catalyst layer 2 and in contact with the surface of the substrate 1. The underlayer 4 contains an element X. Except for the inclusion of the underlayer 4, the configuration of the catalyst-supported electrode 30 is the same as the configuration of the catalyst-supported electrode 10 of the first example.
[0068] The underlayer 4 may contain C (carbon) as the element X.
[0069] The underlayer 4 has, for example, a vapor-deposited film containing the element X, and is typically the vapor-deposited film itself. When the underlayer 4 and the substrate 1 have the same composition, the vapor-deposited film is the underlayer 4, and a structure (e.g., a porous body) that is not a vapor-deposited film is the substrate 1.
[0070] The catalyst-supported electrode 30 including the base layer 4 makes it difficult for the catalyst to fall off from the catalyst-supported electrode 30. This makes the catalyst-supported electrode 30 more suitable for improving the performance maintenance rate of the catalyst.
[0071] The underlayer 4 may contain the element X as a main component. The content of the element X in the underlayer 4 may be 50 vol% or more, 60 vol% or more, 70 vol% or more, 80 vol% or more, 90 vol% or more, or even 95 vol% or more. The underlayer 4 may consist essentially of the element M1 and the element X. The content of the element X in the underlayer 4 can be measured in the same manner as the content of the element M1 in the catalyst layer 2 described above.
[0072] The thickness of the underlayer 4 is not particularly limited and is, for example, 1 nm or more and 1000 nm or less. The thickness of the underlayer 4 may preferably be 800 nm or less, 500 nm or less, 300 nm or less, 100 nm or less, 50 nm or less, 40 nm or less, or even 30 nm or less. In some cases, the thickness of the underlayer 4 may be 20 nm or less, or even 10 nm or less. The thickness of the underlayer 4 is, for example, 1 nm or more, 2 nm or more, or 5 nm or more. An underlayer 4 having a small thickness that satisfies the above numerical range is easy to produce by a vapor deposition method.
[0073] The underlayer 4 may be in contact with the catalyst layer 2 .
[0074] The catalyst-supported electrode 30 can be manufactured in the same manner as the catalyst-supported electrode 10 of the first example, except that, for example, a vapor deposition method is performed to form an underlayer 4 on the substrate 1, and then a catalyst layer 2 is formed on the underlayer 4. In detail, a vapor deposition layer containing element X is formed on the substrate 1 by the vapor deposition method, and then a vapor deposition layer containing element M1 is further formed on the vapor deposition layer. In this manner, the catalyst-supported electrode 30 including the substrate 1, the catalyst layer 2, and the underlayer 4 can be obtained.
[0075] 4 is a cross-sectional view schematically illustrating a fourth example of a catalyst-supported electrode according to this embodiment. The catalyst-supported electrode 40 includes a substrate 1, a catalyst layer 2, a base layer 4 disposed between the substrate 1 and the catalyst layer 2 and in contact with the surface of the substrate 1, and an intermediate layer 3 disposed between the base layer 4 and the catalyst layer 2. Except for the intermediate layer 3 and the base layer 4, the configuration of the catalyst-supported electrode 40 is the same as the configuration of the catalyst-supported electrode 10 of the first example. That is, except for the intermediate layer 3, the configuration of the catalyst-supported electrode 40 is the same as the configuration of the catalyst-supported electrode 30 of the third example. Elements common to the catalyst-supported electrodes of the first to third examples and the catalyst-supported electrode 40 of the fourth example are designated by the same reference numerals, and their description may be omitted.
[0076] In the catalyst-supported electrode 40, the element X may be carbon (C), and the element M1 may be Bi.
[0077] The intermediate layer 3 may bond the catalyst layer 2 and the underlayer 4. The underlayer 4 may bond the substrate 1 and the intermediate layer 3.
[0078] The total thickness of the catalyst layer 2, intermediate layer 3, and underlayer 4 is, for example, 10 nm or more and 5000 nm or less. The total thickness of the catalyst layer 2, intermediate layer 3, and underlayer 4 may be 25 nm or more, 40 nm or more, 50 nm or more, 65 nm, or even 80 nm or more. The total thickness of the catalyst layer 2, intermediate layer 3, and underlayer 4 may be 3000 nm or less, 2000 nm or less, 1000 nm or less, 700 nm or less, 500 nm or less, 300 nm or less, or even 150 nm or less.
[0079] The catalyst-supported electrode of this embodiment may have a structure in which three or more layers are stacked on a substrate 1, as in the catalyst-supported electrode 40 shown in Fig. 4. The three or more layers may have different compositions.
[0080] The catalyst-supported electrode 40 may have a value of y1 calculated by the following formula (I) that is equal to or less than −5.0: y1=(−0.1203)x1+(−0.0426)x2+(−0.0112)x5+(−0.0476)x6+0.1388x7+2.2919 (I)
[0081] x1 is the volume ratio (%) of element M1 in the catalyst layer 2. The value of x1 is, for example, 50 or more, and may be 55 or more, 60 or more, 65 or more, or even 70 or more. The upper limit of x1 is not particularly limited and is, for example, 100. The value of x1 is, for example, 50 or more and 100 or less.
[0082] x2 is the volume ratio (%) of the element M1 in the intermediate layer 3. The value of x2 is, for example, 60 or more, and may be 70 or more, 80 or more, 85 or more, 90 or more, or even 95 or more. The value of x2 may be, for example, less than 100, 99 or less, or even 98 or less. The value of x2 is, for example, 70 or more and less than 100.
[0083] x5 is the thickness (nm) of the catalyst layer 2. The value of x5 is not particularly limited and may be, for example, 5,000 or less, 4,000 or less, 3,000 or less, 2,000 or less, 1,000 or less, 800 or less, 500 or less, 300 or less, 200 or less, 150 or less, 110 or less, 100 or less, or even 90 or less. The value of x5 is, for example, 1 or more, 5 or more, 10 or more, 20 or more, 30 or more, or even 40 or more. The value of x5 is, for example, 1 or more and less than 2,000.
[0084] x6 is the thickness (nm) of the intermediate layer 3. The value of x6 is not particularly limited and may be, for example, 3000 or less, 2000 or less, 1000 or less, 800 or less, 500 or less, 300 or less, 200 or less, 100 or less, 50 or less, 45 or less, or even 40 or less. The value of x6 is, for example, 1 or more, 2 or more, or 5 or more. The value of x6 is, for example, 1 or more and 1000 or less.
[0085] x7 is the thickness (nm) of the underlayer 4. The value of x7 is not particularly limited and may be, for example, 1000 or less, 800 or less, 500 or less, 300 or less, 100 or less, 50 or less, 40 or less, 30 or less, 20 or less, or even 10 or less. The value of x7 is, for example, 1 or more, 2 or more, or 5 or more. The value of x7 is, for example, 1 or more and 1000 or less.
[0086] The value of y1 calculated by formula (I) is preferably −6.0 or less, and may be −7.0 or less, −8.0 or less, −9.0 or less, −10.0 or less, or even −10.8 or less. The lower limit of y1 is not particularly limited and may be, for example, −200.0. The value of y1 may be −180.0 or more, −150.0 or more, −100.0 or more, −80.0 or more, −50.0 or more, −40.0 or more, −30.0 or more, −20.0 or more, or even −17.0 or more. The value of y1 is determined by the CO2 reduction current density (first CO2 reduction current density, unit: mA / cm) when carbon dioxide is reduced in a first electrolysis using the catalyst-supported electrode 40 at a constant voltage of −1.8 V (vs. Ag / AgCl reference electrode) under specific conditions. 2 ) The value of y1 tends to coincide well with the first CO2 reduction current density. When the value of y1 is -5.0 or less, the conversion of carbon dioxide to reaction products proceeds more efficiently, and a sufficient amount of reaction products tends to be obtained.
[0087] The CO reduction current density is the current density (mA / cm) at −1.8 V (vs. Ag / AgCl reference electrode) during carbon dioxide electrolysis. 2 ) × (Faraday efficiency of formic acid production FE HCOOH (%)), where the faradaic efficiency of formic acid production FE HCOOH is the formula: FE HCOOH = 2nF / Q, where n is the amount of formic acid (mol) produced by electrolysis of carbon dioxide, F is the Faraday constant (C / mol), and Q is the total charge (C).
[0088] The catalyst-supported electrode 40 may have a y1 value of −5.0 or less, and a y3 value calculated by the following formulas (II) and (III) of 0.5 or more: y2 = 0.0260x1 + (−0.0286)x2 + 0.1193x3 + (−0.0384)x4 + (−0.1413)x5 + (−0.0247)x6 + 0.2141x7 + 5.5788 (II) y3 = y2 / y1 (III)
[0089] In formula (II), x1, x2, x5, x6, and x7 are the same as x1, x2, x5, x6, and x7 in formula (I) above, and the respective numerical ranges are also as described above.
[0090] x3 is the volume ratio (%) of the element X in the intermediate layer 3. The value of x3 may be, for example, greater than 0, greater than or equal to 1, or greater than or equal to 2. The value of x3 may be, for example, 40 or less, greater than or equal to 30, less than or equal to 20, or less than or equal to 15. The value of x3 is, for example, 2 or more and 30 or less.
[0091] x4 is the volume ratio (%) of the element X in the underlayer 4. The value of x4 is, for example, 50 or more, and may be 60 or more, 70 or more, 80 or more, 90 or more, 95 or more, or even 98 or more. The value of x4 is, for example, 100 or less, and may be 99 or less, or even 98 or less. The value of x4 is, for example, 70 or more and 100 or less, and may be 100.
[0092] The value of y2 calculated by formula (II) is −2.5 or less, and may be −3.5 or less, −5.0 or less, −6.0 or less, −7.0 or less, −8.0 or less, −9.0 or less, or even −10.0 or less. The lower limit of y2 is not particularly limited, and may be, for example, −200.0. The value of y2 may be −180.0 or more, −150.0 or more, −100.0 or more, −80.0 or more, −50.0 or more, −40.0 or more, −30.0 or more, −20.0 or more, or even −15.0 or more. The value of y2 is determined by the CO2 reduction current density (second CO2 reduction current density, unit: mA / cm) obtained by performing a first electrolysis under specific conditions using the catalyst-supported electrode 40 at a constant voltage of −1.8 V (vs. Ag / AgCl reference electrode), and then performing a second electrolysis under the same conditions to reduce carbon dioxide. 2 The value of y2 tends to coincide well with the second CO2 reduction current density. When the value of y2 is -2.5 or less, the catalyst performance retention rate tends to improve.
[0093] The value of y3 calculated by formula (III) is preferably 0.55 or greater, and may be 0.6 or greater, 0.65 or greater, 0.66 or greater, or even 0.67 or greater. The upper limit of y3 is not particularly limited and may be, for example, 1.5. The value of y3 may be 1.4 or less, 1.3 or less, 1.2 or less, or even 1.1 or less. The value of y3 is an index of the catalyst performance maintenance rate when carbon dioxide electrolysis is repeated twice using the catalyst-supported electrode 40 under specific conditions at a constant voltage of −1.8 V (vs. Ag / AgCl reference electrode). The value of y3 tends to closely match the value calculated by (second CO2 reduction current density) / (first CO2 reduction current density). Therefore, the larger the value of y3, the better the catalyst performance maintenance rate of the catalyst-supported electrode 40 tends to be.
[0094] Formulas (I) and (II) were prepared by the following method. First, the configuration of the catalyst-supported electrode, such as the volume ratio of element M1 in catalyst layer 2, the volume ratio of element M1 in intermediate layer 3, the volume ratio of element X in intermediate layer 3, the volume ratio of element X in base layer 4, the thickness of catalyst layer 2, the thickness of intermediate layer 3, and the thickness of base layer 4, was arbitrarily set, and a carbon dioxide reduction reaction was performed by electrolysis. As a result, more than 80 pieces of experimental data were obtained, in which the configuration of the catalyst-supported electrode was correlated with the CO reduction current density. Next, the obtained experimental data was analyzed by PLS (Partial Least Squares) regression, and Formulas (I) and (II) were obtained from experimental data with a generalizability of 0.7 or more.
[0095] The thickness of the catalyst-supported electrode of this embodiment may be, for example, 1 μm to 500 μm, 20 μm to 400 μm, 40 μm to 300 μm, or even 50 μm to 200 μm.
[0096] The catalyst-supported electrode 40 can be manufactured, for example, by performing a vapor deposition method to form an underlayer 4 on a substrate 1. Next, a vapor deposition method is performed to form an intermediate layer 3 on the underlayer 4, and then a vapor deposition method is performed again to form a catalyst layer 2 on the intermediate layer 3. In detail, by the vapor deposition method, a vapor deposition layer containing element X is formed on the substrate 1, a vapor deposition layer containing element M1 and element X is formed on the vapor deposition layer, and a vapor deposition layer containing element M1 is further formed on the vapor deposition layer. In this manner, a catalyst-supported electrode 40 including the substrate 1, the catalyst layer 2, the intermediate layer 3, and the underlayer 4 can be obtained.
[0097] <Electrolysis Device> The electrolysis device of this embodiment includes the above-described catalyst-supported electrode. The electrolysis device converts carbon dioxide into reaction products by electrolysis.
[0098] 5 is a cross-sectional view schematically illustrating an example of the electrolysis device 100 of this embodiment. The electrolysis device 100 includes a current collector 70A, a cathode catalytic electrode 50, an anion exchange membrane 71, a central chamber 72, a cation exchange membrane 73, an anode catalytic electrode 60, and a current collector 70B.
[0099] The cathode catalytic electrode 50 may be the catalyst-supported electrode 10 of this embodiment, or may be the catalyst-supported electrode 20, the catalyst-supported electrode 30, or the catalyst-supported electrode 40. The catalyst-supported electrode 10 serving as the cathode catalytic electrode 50 may be disposed such that the substrate 1 is located on the current collector 70A side and the catalyst layer 2 is located on the anion exchange membrane side.
[0100] The current collector 70A is a cathode-side current collector that contacts the cathode catalytic electrode 50. The current collector 70B is an anode-side current collector that contacts the anode catalytic electrode 60. The current collectors 70A and 70B may have gas flow paths. As the current collectors 70A and 70B, conventionally known current collectors that are generally employed for electrolysis devices can be used. The current collectors 70A and 70B are, for example, graphite current collectors.
[0101] The electrolysis device 100 may include one or more openings for supplying carbon dioxide into or discharging carbon dioxide from the electrolysis device 100. For example, the electrolysis device 100 includes a supply port 6A for sending carbon dioxide to the current collector 70A and a discharge port 7A for discharging carbon dioxide. The electrolysis device 100 may further include one or more openings for supplying water and oxygen into or discharging water and oxygen from the electrolysis device 100. For example, the electrolysis device 100 includes a supply port 6B for sending water to the current collector 70B and a discharge port 7B for discharging water or oxygen.
[0102] The central chamber 72 is typically filled with ion exchange resin beads and is supplied with water. The central chamber 72 is provided with, for example, a supply port 8 through which water is supplied. The central chamber 72 also has a discharge port 9 through which the reaction product is discharged.
[0103] The anion exchange membrane 71 is not particularly limited as long as it is made of a material that has ion conductivity, can transport anion components, and does not have cation conductivity, and known membranes can be used. The anion exchange membrane 71 may be made of an anion exchange resin. The anion exchange resin is not particularly limited as long as it has anion exchange properties. The anion exchange resin may be a solid polymer electrolyte (ionomer) in which a polymer having an anion-conducting functional group is introduced into a polymer base material. Specific examples of anion exchange resins include Sustainion (registered trademark, Dioxide Materials Inc.) and Fumasep (registered trademark, FuMA-Tech Inc.). Specific examples of the anion exchange membrane 71 include Sustainion (registered trademark) 37-50.
[0104] The cation exchange membrane 73 is not particularly limited as long as it is made of a material that has ion conductivity, can transport cationic components (e.g., hydrogen ions), and does not exhibit electronic conductivity, and any known membrane can be used. The cation exchange membrane 73 is preferably a membrane made of a polymer, and may be made of a cation exchange resin.
[0105] The cation exchange resin is not particularly limited as long as it has cation exchange properties. The cation exchange resin may be a solid polymer electrolyte (ionomer) having cationic groups, in which a polymer having cation-conductive functional groups (cationic groups) is introduced into a polymer substrate. Specific examples of cation exchange resins include perfluoroalkyl sulfonic acid resins such as Nafion (registered trademark, DuPont), Flemion (registered trademark, AGC), and Aciplex (registered trademark, Asahi Kasei). Specific examples of the cation exchange membrane 73 include Nafion NR-211 and NR-212.
[0106] The anode catalyst electrode 60 is not particularly limited as long as it can cause an oxidation reaction, and a conductive material can be used. For example, the anode catalyst electrode 60 can be made of iridium, platinum, gold, copper, iron, or the like.
[0107] The electrolysis device 100 may further include known components constituting an electrolysis device. For example, the electrolysis device 100 includes a power supply that applies a voltage between the cathode catalytic electrode 50 and the anode catalytic electrode 60.
[0108] Carbon dioxide can be electrolyzed by supplying carbon dioxide to the cathode catalytic electrode 50 and applying a voltage to the electrolysis device 100 to cause a reaction to proceed at the cathode catalytic electrode 50 and the anode catalytic electrode 60. The carbon dioxide is electrolyzed and converted into a reaction product. The reaction product is typically an organic compound, such as formic acid.
[0109] According to the electrochemical reaction at the cathode catalyst electrode 50, carbon dioxide is reduced to HCOO - ions are generated. The generated HCOO - The ions are supplied to the central chamber 72 through the anion exchange membrane 71. When carbon dioxide is supplied to the cathode catalytic electrode 50 and water is supplied to the anode catalytic electrode 60, an electrochemical reaction occurs at the anode catalytic electrode 60 to generate, for example, hydrogen ions. The generated hydrogen ions are supplied to the central chamber 72 through the cation exchange membrane 73. - For example, formic acid is generated in the central chamber 72 and discharged from the outlet 9.
[0110] The temperature during electrolysis by the electrolysis device 100 is not particularly limited and may be, for example, room temperature. The electrolysis device 100 can convert carbon dioxide into reaction products under mild conditions, and therefore can obtain reaction products with less energy.
[0111] The electrolysis device 100 shows an example of a device that converts carbon dioxide into a reaction product by electrolysis, and the electrolysis device of this embodiment is not limited to the above configuration. In another configuration of the electrolysis device, an electrolytic cell is filled with an electrolyte solution, and a first electrode and a second electrode are arranged in contact with the electrolyte solution. The first electrode or the second electrode is the catalyst-supported electrode of the present invention. The first electrode and the second electrode may be immersed in the electrolyte solution. In addition, a reference electrode in contact with the electrolyte solution may be further provided.
[0112] The electrolyte may be any known electrolyte commonly used for electrolysis devices, such as an aqueous potassium hydrogen carbonate solution, an aqueous sodium hydrogen carbonate solution, or an aqueous sodium hydroxide solution.
[0113] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto.
[0114] Example 1 First, a target composed of Bi was set in the target setting section of the sputtering device. Next, a thoroughly polished glassy carbon (GC) electrode (L-type, GC-3L, EC Frontier) was set in the sample introduction section of the sputtering device. Next, sputtering was performed using the above target, and a catalyst layer composed only of Bi was produced on the GC electrode. The thickness of the catalyst layer was 102 nm.
[0115] In this manner, the catalyst-supported electrode of Example 1 was produced.
[0116] Example 2 First, a target composed of Bi and a target composed of carbon (C) were set in the target mounting section of the sputtering device. Next, a thoroughly polished glassy carbon (GC) electrode (L-type, GC-3L, EC Frontier) was set in the sample introduction section of the sputtering device. Next, co-sputtering was performed using the above two targets, and an intermediate layer composed only of Bi and C was fabricated on the GC electrode. In the co-sputtering method, the power output was controlled so that the Bi content in the intermediate layer was 85% by volume. The thickness of the intermediate layer was 5 nm.
[0117] Next, a sputtering method using only a Bi target was carried out to form a catalyst layer made of only Bi on the intermediate layer, with a thickness of 46 nm.
[0118] In this manner, the catalyst-supported electrode of Example 2 was produced.
[0119] Example 3 First, a target composed of Bi and a target composed of carbon (C) were set in the target mounting section of the sputtering device. Next, a thoroughly polished glassy carbon (GC) electrode (L-type, GC-3L, EC Frontier) was set in the sample introduction section of the sputtering device. Next, co-sputtering was performed using the above two targets, and an intermediate layer composed only of Bi and C was fabricated on the GC electrode. In the co-sputtering method, the power output was controlled so that the Bi content in the intermediate layer was 85% by volume. The thickness of the intermediate layer was 20 nm.
[0120] Next, a Bi target and a Sn target were set in the target mounting section of the sputtering device, and a co-sputtering method using the two targets was performed to produce a catalyst layer composed only of Bi and Sn on the intermediate layer. In this co-sputtering method, the power output was controlled so that the Bi content in the catalyst layer was 70 volume %. The thickness of the catalyst layer was 66 nm.
[0121] In this manner, the catalyst-supported electrode of Example 3 was produced.
[0122] (Example 4) First, a target composed of carbon (C) was set in the target setting section of the sputtering device. Next, a thoroughly polished carbon glassy carbon (GC) electrode (L-type, GC-3L, EC Frontier) was set in the sample introduction section of the sputtering device. Next, a sputtering method using the above C target was performed, and an underlayer composed only of C was formed on the GC electrode. The thickness of the underlayer was 10 nm.
[0123] Next, a Bi target and a Sn target were set in the target mounting section of the sputtering device, and a co-sputtering method using the two targets was performed to produce a catalyst layer composed only of Bi and Sn on the underlayer. In this co-sputtering method, the power output was controlled so that the Bi content in the catalyst layer was 70 volume %. The thickness of the catalyst layer was 66 nm.
[0124] In this manner, the catalyst-supported electrode of Example 4 was produced.
[0125] Example 5 First, a target composed of carbon (C) was set in the target setting section of the sputtering device. Next, a thoroughly polished glassy carbon (GC) electrode (L-type, GC-3L, EC Frontier) was set in the sample introduction section of the sputtering device. Next, a sputtering method using the above C target was performed, and an underlayer composed only of C was formed on the GC electrode. The thickness of the underlayer was 5 nm.
[0126] Next, a Bi target and a carbon (C) target were set in the target mounting section of the sputtering device, and a co-sputtering method using the two targets was performed to produce an intermediate layer composed only of Bi and C on the underlayer. In this co-sputtering method, the power output was controlled so that the Bi content in the intermediate layer was 98% by volume. The thickness of the intermediate layer was 40 nm.
[0127] Next, a sputtering method using a Bi target was carried out to form a catalyst layer made of only Bi on the intermediate layer, with a thickness of 90 nm.
[0128] In this manner, the catalyst-supported electrode of Example 5 was produced.
[0129] Example 6: In the same manner as in Example 5, an underlayer and an intermediate layer were fabricated on a GC electrode. Next, a Bi target and a Sn target were set in the target mounting section of the sputtering device, and co-sputtering using the two targets was performed to fabricate a catalytic layer composed only of Bi and Sn on the intermediate layer. In this co-sputtering method, the power output was controlled so that the Bi content in the catalytic layer was 56% by volume. The thickness of the catalytic layer was 90 nm.
[0130] In this manner, the catalyst-supported electrode of Example 6 was produced.
[0131] Comparative Example 1 10 mg of Bi2O3 powder (US Research Nanomaterials), 180 μL of ultrapure water, 4700 μL of ethanol, and 4 μL of alkaline ionomer (Sustainion (registered trademark) XA-9 5% in EtOH, Dioxide Materials) were thoroughly mixed in an ultrasonic cleaner for 30 minutes to prepare a catalyst ink.
[0132] Next, 1.5 μL of catalyst ink was dropped onto the surface of a thoroughly polished glassy carbon (GC) electrode (L-type, GC-3L, EC Frontier) and dried for 60 minutes to prepare a catalyst layer. In this way, the catalyst-supported electrode of Comparative Example 1 was prepared.
[0133] <Evaluation of Surface Porosity> The surface porosity of the catalyst layer of the catalyst-supported electrode prepared in Example 1-6 was determined by the following method. First, a carbon paper substrate (TGP-H-120, Toray Industries, Inc.) was used instead of the GC electrode, and the amount of catalytically active species supported per unit area (Bi supported amount) was 2 mg / cm. 2 Electrode sample 1-6 corresponding to the catalyst-supported electrode of each example 1-6 was produced by the same method as in each example, except that the catalyst layer was formed so as to have the following structure:
[0134] Next, the surface porosity of the catalytic layer was determined for the obtained electrode samples 1-6. Specifically, any five points on the surface of the catalytic layer of each electrode sample were observed using an SEM at a magnification of 5000 times from a direction perpendicular to the surface. For each obtained SEM image, image analysis software (ImageJ) was used to obtain a binarized image in which the structural portion of the catalytic layer and the void portion were separated within a 10 μm × 10 μm area. The proportion of the void portion was determined by image analysis of the binarized image, and the average value of these five points was calculated to determine the surface porosity of the catalytic layer of electrode samples 1-6. The surface porosity of the catalytic layer in electrode samples 1-6 was considered to be the surface porosity of the catalytic layer of the catalyst-supported electrode in Examples 1-6, respectively.
[0135] 6A and 6B are an SEM image (magnification: 5000 times) and a binarized image of an arbitrary point on the surface of the catalytic layer of electrode sample 1. Fig. 6A is the SEM image. Fig. 6B is the binarized image of Fig. 6A. In Fig. 6B, the black areas indicate voids.
[0136] The surface porosity of the catalyst layer of the catalyst-supported electrode prepared in Comparative Example 1 was determined by the following method. First, a carbon paper substrate (TGP-H-120, Toray Industries, Inc.) was used instead of the GC electrode, and the amount of catalytically active species supported per unit area (BiO supported amount) was 4 mg / cm. 2 An electrode sample C1 corresponding to the catalyst-supported electrode of Comparative Example 1 was produced by the same method as in Comparative Example 1, except that the catalyst layer was formed so as to satisfy the following formula: The surface porosity of the catalyst layer in electrode sample C1 was determined by the method described above for electrode sample C1, and this was considered to be the surface porosity of the catalyst layer of the catalyst-supported electrode of Comparative Example 1.
[0137] <Evaluation of Performance Maintenance Rate> Using the catalyst-supported electrodes prepared in the Examples and Comparative Examples, electrolysis of carbon dioxide was carried out by the following method, and the performance maintenance rate of the catalyst was evaluated.
[0138] First, a working electrode, a counter electrode, and a reference electrode were set in a compact analytical cell (VB2, EC Frontier). The catalyst-supported electrodes of Examples 1-6 and Comparative Example 1 were used as the working electrodes. A platinum electrode (CE-200, EC Frontier) was used as the counter electrode. A silver / silver chloride electrode (RE-1A, EC Frontier) was used as the reference electrode. 15 g of a 0.1 M aqueous potassium bicarbonate solution was added to the cell as the electrolyte. In this way, a test electrolytic cell was assembled.
[0139] Next, CO2 gas was bubbled into the aqueous solution in the cell at a flow rate of 30 mL / min for 30 minutes to replace the gas. After that, a voltage of -1.8 V (vs. Ag / AgCl) was applied for 60 minutes while CO2 gas was continuously supplied into the cell, and an electrolysis test was performed.
[0140] The electrolyte solution after the test was collected and analyzed using high performance liquid chromatography (HPLC) to quantify the concentration of formic acid produced. The faradaic efficiency of formic acid production (FE) was calculated from the formic acid concentration. HCOOH ) was calculated to determine the first CO reduction current density in the catalyst. As described above, the faradaic efficiency for formic acid production (FE HCOOH ) and CO reduction current density were calculated using the following equations: HCOOH = 2nF / Q (n is the amount of formic acid (mol) produced by electrolysis of carbon dioxide, F is the Faraday constant (C / mol), and Q is the total charge (C). CO2 reduction current density = (current density at -1.8 V (vs. Ag / AgCl)) × FE HCOOH
[0141] After the test, each electrode was washed and thoroughly dried, and the test electrolysis cell was reassembled and a second electrolysis test was performed in the same manner. The concentration of formic acid produced in the second electrolysis test was quantified using HPLC, and the second CO reduction current density was calculated.
[0142] The catalyst performance maintenance rate was calculated from the values of the first CO reduction current density and the second CO reduction current density using the following formula: Performance maintenance rate (%) = 100 × (second CO reduction current density) / (first CO reduction current density).
[0143] The configurations of Examples 1 to 6 and Comparative Example 1 are shown in Table 1. The evaluation results of the performance retention rate are shown in Table 2. y1 in Table 2 is the value calculated by the above formula (I), and y3 is the value calculated by formulas (II) and (III). With regard to the amount of catalytic active species supported in Table 2, Examples 1 to 6 are the amount of Bi supported, and Comparative Example 1 is the amount of Bi2O3 supported.
[0144]
[0145]
[0146] In Examples 1-6, in which the surface porosity of the catalyst layer was less than 20%, the catalyst performance retention rate was improved compared to Comparative Example 1. The performance retention rate was further improved by providing an intermediate layer in the catalyst-supported electrode. The performance retention rate was further improved by providing a base in the catalyst-supported electrode. The performance retention rate was further improved by including another element in addition to element M1 in the catalyst layer. The performance retention rate was further improved by including three layers in the catalyst-supported electrode: the catalyst layer, the intermediate layer, and the base layer.
[0147] The catalyst-supported electrode of this embodiment is suitable for an electrolysis device that converts carbon dioxide into reaction products.
Claims
1. A catalyst-supported electrode for converting carbon dioxide into a reaction product, comprising: a substrate; and a catalyst layer disposed on the substrate and including an element M1 functioning as a catalytically active species, the catalyst layer having a surface porosity of less than 20%.
2. A catalyst-supported electrode for converting carbon dioxide into a reaction product, comprising: a substrate; and a catalyst layer disposed on the substrate and containing an element M1 functioning as a catalytically active species, the catalyst layer being a vapor-deposited layer.
3. The catalyst-supported electrode according to claim 1, wherein the surface porosity is less than 10%.
4. The catalyst-supporting electrode according to claim 1 or 2, wherein the catalyst layer contains the element M1 as a main component.
5. The catalyst-supporting electrode according to claim 1 or 2, wherein the element M1 is Bi or Sn.
6. The catalyst-supporting electrode according to claim 1 or 2, wherein the catalyst layer further contains an element M2 different from the element M1.
7. The catalyst-supporting electrode according to claim 1 or 2, further comprising an intermediate layer disposed between the substrate and the catalyst layer, the substrate containing an element X, and the intermediate layer containing the element M1 and the element X.
8. The catalyst-supporting electrode according to claim 1 or 2, further comprising an underlayer disposed between the substrate and the catalyst layer and in contact with a surface of the substrate, the substrate containing element X, and the underlayer containing element X.
9. The catalyst-supporting electrode according to claim 1 or 2, further comprising: an underlayer disposed between the substrate and the catalytic layer and in contact with a surface of the substrate; and an intermediate layer disposed between the underlayer and the catalytic layer, wherein the substrate contains element X as a main component, the catalytic layer contains element M1 as a main component, the intermediate layer contains element M1 and element X, and the underlayer contains element X.
10. The catalyst-supported electrode according to claim 9, wherein the value of y1 calculated by the following formula (I) is −5.0 or less: y1=(−0.1203)x1+(−0.0426)x2+(−0.0112)x5+(−0.0476)x6+0.1388x7+2.2919 (I) In the formula (I), x1 is the volume ratio (%) of the element M1 in the catalyst layer, x2 is the volume ratio (%) of the element M1 in the intermediate layer, x5 is the thickness (nm) of the catalyst layer, x6 is the thickness (nm) of the intermediate layer, and x7 is the thickness (nm) of the base layer.
11. The catalyst-supporting electrode according to claim 10, wherein the value of y3 calculated by the following formulas (II) and (III) is 0.5 or more. y2 = 0.0260x1 + (-0.0286)x2 + 0.1193x3 + (-0.0384)x4 + (-0.1413)x5 + (-0.0247)x6 + 0.2141x7 + 5.5788 (II) y3 = y2 / y1 (III) In the formula (II), x1 is the volume ratio (%) of the element M1 in the catalyst layer, x2 is the volume ratio (%) of the element M1 in the intermediate layer, x3 is the volume ratio (%) of the element X in the intermediate layer, x4 is the volume ratio (%) of the element X in the base layer, x5 is the thickness (nm) of the catalyst layer, x6 is the thickness (nm) of the intermediate layer, and x7 is the thickness (nm) of the base layer.
12. The catalyst-supporting electrode according to claim 7, wherein the element X is carbon (C).
13. The catalyst-supporting electrode according to claim 1 or 2, wherein the thickness of the catalyst layer is 1 nm or more and 5000 nm or less.
14. The catalyst-supporting electrode according to claim 1 or 2, wherein the substrate is porous.
15. The catalyst-supported electrode according to claim 1 or 2, wherein the catalytically active species is a catalyst that reduces the carbon dioxide.
16. An electrolysis device for converting carbon dioxide into reaction products, comprising a catalyst-supported electrode according to claim 1 or 2.
Citation Information
Patent Citations
Bismuth-based catalyst for electrocatalytic CO2 reduction to form formic acid and preparation method and application thereof
CN109518222A
Preparation of electrode for electrochemical reduction of CO2 and electrode and application thereof
CN109652820A
Electrolytic cell for gas production
JP2022160086A
Reduction catalyst
WO2021200544A1
Semiconductor photoelectrode
WO2021234804A1