Metal mask base material, production method for metal mask base material, and production method for metal mask

The use of an iron-nickel alloy metal mask base material with controlled crystal orientation and annealing processes addresses excessive wet etching in metal mask manufacturing, ensuring precise through-hole dimensions and high-definition patterns by maintaining a KAM value of 2.18° or more, effectively preventing warping and enhancing handleability.

WO2024204556A1PCT designated stage expired Publication Date: 2024-10-03TOPPAN HOLDINGS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012684
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-28
Publication Date
2024-10-03

Smart Images

  • Figure JP2024012684_03102024_PF_FP_ABST
    Figure JP2024012684_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This metal mask base material is constituted by an iron-nickel-based alloy. The metal mask base material exhibits a KAM value of not less than 2.18° as obtained by an electron backscatter diffraction method in which a step size is set to 0.5 μm and a crystal grain boundary is considered to be a boundary where the difference in crystal orientation is not less than 5°. The metal mask base material has a thickness of 10-30 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Metal mask substrate, method for manufacturing metal mask substrate, and method for manufacturing metal mask

[0001] The present disclosure relates to a metal mask substrate, a method for manufacturing a metal mask substrate, and a method for manufacturing a metal mask.

[0002] One example of a method for forming pixels in an organic EL display device is a vacuum deposition method. In the vacuum deposition method, a metal mask, which is a metal mask having a plurality of through-holes, is used. Each through-hole has a shape corresponding to the shape of a pixel, and the plurality of through-holes are arranged according to the pixel arrangement. Each through-hole is a passage through which a deposition material for forming the pixel passes. A thin metal plate made of an iron-nickel alloy is used as a material for forming the metal mask (see, for example, Patent Document 1).

[0003] When manufacturing a metal mask from a thin metal plate, a resist layer is first formed on the surface of the thin metal plate, and then a resist pattern is formed from the resist layer. A plurality of through holes are then formed in the thin metal plate by wet etching using the resist pattern.

[0004] International Publication No. 2018 / 235862

[0005] Various electronic devices equipped with organic EL display devices are required to display high-definition images. Therefore, high-definition pixels of organic EL display devices, and therefore metal masks for forming the pixels, are also required. For example, in a metal mask for forming high-definition pixels of about 500 ppi, the maximum dimension of the openings located on the surface of the thin metal plate is reduced to several tens of micrometers. When forming through holes with reduced openings, excessive wet etching occurs in some of the through holes, resulting in a new problem of enlargement of the through holes.

[0006] These problems are not limited to metal masks used to form pixels in organic EL display devices, but are also common to metal masks used to form patterns used in electronic devices and electronic components other than organic EL display devices, for example.

[0007] The metal mask substrate for solving the above problems is a metal plate made of an iron-nickel alloy, which has a step size of 0.5 μm, a KAM value of 2.18° or more as measured by electron backscatter diffraction (EBSD) analysis, and a thickness of 10 μm to 30 μm, when a grain boundary is defined as a boundary where the difference in crystal orientation is 5° or more.

[0008] A method for manufacturing a metal mask substrate that solves the above-mentioned problems is a method for manufacturing a metal mask substrate that is a metal plate made of an iron-nickel alloy. The manufacturing method includes rolling a base material of the metal plate to obtain a rolled material, and annealing the rolled material at a temperature of 720°C or less. In the metal plate, when a step size is set to 0.5 μm and boundaries where the difference in crystal orientation is 5° or more are considered to be grain boundaries, the KAM value obtained by electron backscatter diffraction analysis is 2.18° or more, and the metal plate has a thickness of 10 μm to 30 μm.

[0009] A method for manufacturing a metal mask for solving the above problems includes forming a resist layer on a metal plate, forming a resist pattern from the resist layer, and forming a plurality of through holes in the metal plate by wet etching using the resist pattern. When a step size is set to 0.5 μm and a boundary where a difference in crystal orientation is 5° or more is considered to be a grain boundary, the metal plate has a KAM value of 2.18° or more obtained by electron backscatter diffraction, and has a thickness of 10 μm to 30 μm.

[0010] FIG. 1 is a perspective view of a metal mask substrate. FIG. 2 is a cross-sectional view of the metal mask substrate shown in FIG. 1. FIG. 3 is a plan view schematically showing pixels set on the observation surface of the metal mask substrate when calculating the KAM value. FIG. 4 is a process diagram showing a process in which excessive wet etching progresses locally on the metal mask substrate. FIG. 5 is a process diagram showing a process in which excessive wet etching progresses locally on the metal mask substrate. FIG. 6 is a process diagram showing a process in which excessive wet etching progresses locally on the metal mask substrate. FIG. 7 is a schematic diagram for explaining pitting corrosion that occurs in a metal mask substrate. FIG. 8 is a process diagram showing a process in which excessive wet etching progresses locally on the metal mask substrate. FIG. 9 is a plan view showing the structure of a metal mask. FIG. 10 is an enlarged plan view of a portion of the metal mask shown in FIG. 9. FIG. 11 is a cross-sectional view showing a first example of the structure of the metal mask shown in FIG. 9. FIG. 12 is a cross-sectional view showing a second example of the structure of the metal mask shown in FIG. 9. FIG. 13 is a process diagram showing a step included in a method for manufacturing a metal mask substrate. FIG. 14 is a process diagram showing a step included in a method for manufacturing a metal mask substrate. FIG. 15 is a process diagram showing a step included in a method for manufacturing a metal mask. FIG. 16 is a process diagram showing a step included in a method for manufacturing a metal mask. FIG. 17 is a process diagram showing a step included in a method for manufacturing a metal mask. FIG. 18 is a process diagram showing a step included in a method for manufacturing a metal mask. FIG. 19 is a process diagram showing a step included in a method for manufacturing a metal mask. FIG. 20 is a process diagram showing a step included in a method for manufacturing a metal mask. FIG. 21 is a graph showing the relationship between the KAM value and the incidence of localized etching. FIG. 22 is an SEM image of the surface of a test piece including openings, and includes openings where localized etching has progressed and openings where localized etching has not occurred. FIG. 23 is a graph showing the relationship between annealing temperature and KAM value.

[0011] 1 to 23, one embodiment of a metal mask substrate, a metal mask substrate, and a method for manufacturing a metal mask will be described. The metal mask of this embodiment is an example of a metal mask, and is a vapor deposition mask used to form pixels included in an organic EL display device.

[0012] [Metal Mask Substrate] The metal mask substrate will be described with reference to FIGS. 1 to 8 . The metal mask substrate 10 shown in FIG. 1 is a metal plate made of an iron-nickel alloy. The metal mask substrate 10 has a thickness T of 10 μm or more and 30 μm or less. The metal mask substrate 10 has a front surface 10F and a back surface 10R, which is the surface opposite the front surface 10F. The thickness T of the metal mask substrate 10 is the distance between the front surface 10F and the back surface 10R. From the viewpoint of improving the handleability of the metal mask substrate 10, the thickness of the metal mask substrate 10 is preferably 10 μm or more, and more preferably 15 μm or more. From the viewpoint of preventing the through holes formed in the metal mask substrate 10 from casting a shadow on the vapor deposition material that has entered the through holes, the thickness of the metal mask substrate 10 is preferably 30 μm or less, and more preferably 20 μm or less. The shadow cast by the vapor deposition material is referred to as the shadow effect of the metal mask. From the viewpoint of improving the handleability of the metal mask substrate 10 and suppressing the shadow effect of the metal mask, the thickness of the metal mask substrate 10 is preferably 10 μm or more and 30 μm or less.

[0013] The metal mask substrate 10 preferably contains 35% by mass or more and 36.5% by mass or less of nickel, with the remainder being iron. The metal mask substrate 10 may also contain additive elements other than nickel and iron. The additive elements may be metal elements or non-metal elements. Examples of metal elements include manganese (Mn), magnesium (Mg), aluminum (Al), chromium (Cr), molybdenum (Mo), and cobalt (Co). Examples of non-metal elements include silicon (Si), phosphorus (P), sulfur (S), and chlorine (Cl). The total amount of additive elements in the metal mask substrate 10 may be, for example, 1% by mass or less.

[0014] FIG. 2 shows the cross-sectional structure of the metal mask substrate 10. As shown in FIG. 2, the metal mask substrate 10 is composed of a main layer 10A, a first surface layer 10B1, and a second surface layer 10B2. The main layer 10A is located between the first surface layer 10B1 and the second surface layer 10B2. The first surface layer 10B1 includes the front surface 10F of the metal mask substrate 10. The second surface layer 10B2 includes the back surface 10R of the metal mask substrate 10. The first surface layer 10B1 and the second surface layer 10B2 are each a natural oxide film of an iron-nickel alloy. In contrast, in the main layer 10A, the iron-nickel alloy is not oxidized by the oxidizing agent present around the alloy. Therefore, the oxygen content in each of the surface layers 10B1 and 10B2 is higher than the oxygen content in the main layer 10A. The thickness of each of the surface layers 10B1, 10B2 may be, for example, greater than 0 nm and equal to or less than 10 nm, or greater than 0 nm and equal to or less than 5 nm.

[0015] Among the metal elements contained in metal mask substrate 10, iron and nickel are passively formed by oxidation. First surface layer 10B1 and second surface layer 10B2 contain iron and nickel, and are therefore passively formed. Among the elements that can be contained in metal mask substrate 10, aluminum, chromium, and cobalt are also passively formed by oxidation.

[0016] 3 is a schematic diagram illustrating the KAM value measured on the metal mask substrate 10. In the metal mask substrate 10 of the present disclosure, when the step size is set to 0.5 μm and boundaries where the difference in crystal orientation is 5° or more are considered to be grain boundaries, the KAM value obtained by electron backscatter diffraction is 2.18° or more. According to the metal mask substrate 10 of the present disclosure, the KAM value of the metal mask substrate 10 is 2.18° or more, and therefore, when multiple through holes are formed in the metal mask substrate 10, some of the multiple through holes are prevented from becoming larger.

[0017] When measuring the KAM value of the metal mask substrate 10, first, the surface 10F of the metal mask substrate 10 is prepared, thereby creating an observation surface. At this time, 1 / 10 of the thickness of the metal mask substrate 10 is removed from the surface 10F of the metal mask substrate 10 by buffing and ion milling. Next, using a field emission scanning electron microscope (FE-SEM), the KAM value is measured by electron backscatter diffraction (EBSD) in a 50 μm square measurement area on the observation surface. The step size is set to 0.5 μm, and the KAM value is measured assuming that boundaries with a difference in crystal orientation of 5° or more are regarded as grain boundaries. The KAM value is measured in five non-overlapping measurement areas randomly selected on the observation surface, and the average of the KAM values ​​obtained in each measurement area is set as the KAM value of the metal mask substrate 10.

[0018] As shown in Figure 3, an electron beam is irradiated onto irradiation points SP arranged with a step size SS of 0.5 μm. A hexagonal region in the measurement region centered on the irradiation point SP is defined as a pixel PX, and the crystal orientation at the irradiation point SP included in that pixel PX is considered to be the crystal orientation of that pixel PX. Among the multiple pixels PX included in the measurement region, adjacent pixels PX share one side at the outer edge of the pixel PX.

[0019] When calculating the KAM value, the crystal orientation at each pixel PX is calculated. Next, the average value of the crystal orientations of the six pixels PX adjacent to that pixel PX that belong to the same crystal grain is calculated. At this time, pixels PX whose crystal orientation differs by 5° or more from the crystal orientation of the pixel PX being calculated are recognized as pixels PX that do not belong to the same crystal grain. Next, the difference value between the crystal orientation at the pixel PX being calculated and the average value of the crystal orientations at the adjacent pixels PX is calculated. The absolute value of this difference value is set as the KAM value at the pixel PX being calculated.

[0020] For example, of the multiple pixels PX shown in FIG. 3 , a pixel PX with high-density halftone dots is set as the first pixel PX1. When calculating the KAM value of the first pixel PX1, the average value of the crystal orientations of six second pixels PX2, which are adjacent to the first pixel PX1 and are low-density halftone dots, is calculated. In this case, among the second pixels PX2, those with crystal orientations that differ from the crystal orientation of the first pixel PX1 by 5° or more are excluded from the calculation of the average value. Then, the difference value between the crystal orientation of the first pixel PX1 and the average value of the crystal orientations of the second pixels PX2 is calculated. The absolute value of this difference value is the KAM value of the first pixel PX1.

[0021] The KAM value is calculated for all pixels PX included in the measurement area. Then, the average value for all pixels PX is calculated, and this average value is set as the KAM value for the measurement area. After calculating the KAM values ​​for the five measurement areas, the average value for the five measurement areas is calculated, thereby obtaining the KAM value of the metal mask substrate 10.

[0022] The KAM value is an index that represents the degree of distortion in the crystal lattice contained within a crystal grain. The larger the KAM value within the crystal grain, the greater the distortion of the crystal lattice.

[0023] The mechanism by which localized etching progresses in the metal mask substrate 10 will be described with reference to Figures 4 to 8. Figures 4 to 6 and Figure 8 schematically show the process of wet-etching the metal mask substrate 10 using a second resist pattern formed on the rear surface 10R of the metal mask substrate 10. Figure 7 is a schematic diagram illustrating pitting corrosion that occurs when the metal mask substrate 10 is wet-etched.

[0024] 4, when the metal mask substrate 10 is wet-etched, a second resist pattern RP2 is formed on the rear surface 10R of the metal mask substrate 10. The second resist pattern RP2 has second through holes RP2A. When viewed from the viewpoint facing the rear surface 10R, the second resist pattern RP2 is wet-etched through the second through holes RP2A to form a 1600 μm pattern on the rear surface 10R of the metal mask substrate 10. 2 In order to enable the formation of higher resolution pixels, the area of ​​the opening may be 900 μm or less. 2 It is preferable that:

[0025] 5, when wet-etching the metal mask substrate 10 from the rear surface 10R of the metal mask substrate 10, an etching solution ES is supplied to the second resist pattern RP2. The etching solution ES is, for example, an etching solution containing chloride ions, and may be a ferric chloride solution. The wet etching method may be, for example, spray etching. When the wet etching method is spray etching, the etching solution ES supplied to the second resist pattern RP2 flows in a predetermined direction.

[0026] A part of the etching liquid ES supplied to the second resist pattern RP2 flows into the second through holes RP2A. At this time, as described above, the opening area of ​​the second through holes RP2A is 1600 μm 2 Since the area is small enough to form an opening having an area below this, it is difficult to supply the etching liquid ES uniformly to the entire second through hole RP2A.

[0027] 6, the etching solution ES supplied to a portion of the second through hole RP2A etches a portion of the portion of the back surface 10R that is exposed in the second through hole RP2A. As described above, because back surface 10R of metal mask substrate 10 is included in second surface layer 10B2, a portion of second surface layer 10B2 is etched.

[0028] 7 , when etching solution ES is supplied to second surface layer 10B2, the chloride ion concentration increases only in a portion of second surface layer 10B2. As a result, second surface layer 10B2, which is passive, is locally destroyed by the chloride ions, causing pitting corrosion in a portion of metal mask substrate 10. The portion of main layer 10A exposed from second surface layer 10B2 functions as an anode, and second surface layer 10B2 functions as a cathode. This causes the following reaction:

[0029] (Anode reaction) Fe → Fe 2+ +2e - (Hydrolysis reaction) Fe 2+ +2H 2 O → Fe(OH) 2 +2H + (Cathode reaction) O 2 +2H 2 O+4e - → 4OH - That is, the dissolved iron ions at the anode cause a hydrolysis reaction, which acidifies the pitted area, suppressing passivation and allowing further etching of the pitted area.

[0030] 8, etching proceeds at a higher rate in the portion of main layer 10A exposed from second surface layer 10B2 than in the case where the entire portion exposed from second through hole RP2A is etched. As a result, recess 10AH is formed by localized etching, and therefore, in some of the multiple through holes, the openings located on back surface 10R become larger, and thus the size of the through holes also increases.

[0031] In this regard, according to the metal mask substrate 10 of the present disclosure, the distortion of the crystal lattice in the main layer 10A increases, which in turn increases the distortion of the crystal lattice in the first surface layer 10B1 and the second surface layer 10B2 formed on the surface of the main layer 10A. This roughens the first surface layer 10B1 and the second surface layer 10B2, increasing the number of locations in the first surface layer 10B1 and the second surface layer 10B2 where the etching solution ES can easily penetrate. As a result, the amount of pitting corrosion in the main layer 10A can be distributed among multiple locations, thereby preventing localized etching in a portion of the metal mask substrate 10. In other words, the openings located on the back surface 10R of some of the multiple through holes are prevented from becoming larger, which in turn prevents the through holes from becoming larger.

[0032] The KAM value of the metal mask substrate 10 may be 2.76° or less. This makes it possible to suppress residual strain in the metal mask substrate 10 to a degree that prevents warping of the metal mask substrate 10 after wet etching of the metal mask substrate 10. The KAM value of the metal mask substrate 10 is negatively correlated with the annealing temperature applied to the rolled material in the manufacturing process of the metal mask substrate 10. The KAM value tends to decrease as the annealing temperature increases.

[0033] As described above, if the KAM value of the metal mask substrate 10 is 2.76° or less, the rolled material can be annealed at a temperature that can suppress the strain remaining in the metal mask substrate 10 to a level that does not cause strain in the metal mask substrate 10 after wet etching.

[0034] [Metal Mask] The metal mask will be described with reference to Fig. 9 to Fig. 12. The metal mask 20 shown in Fig. 9 is formed from a metal mask substrate 10 made of an iron-nickel alloy. The maximum thickness of the metal mask 20 is 10 µm or more and 30 µm or less. The metal mask 20 has a rear surface 20R and a plurality of through holes 20H having openings in the rear surface 20R. The rear surface 20R is an example of a first surface. The area of ​​the opening is 1600 µm 2From the viewpoint of enabling the formation of higher resolution pixels, the area of ​​the opening may be 900 μm or less. 2 It is preferable that:

[0035] According to the metal mask 20 of the present disclosure, the KAM value of the metal mask substrate 10, and therefore the KAM value of the metal mask 20, is 2.18° or more. 2 Even when forming through holes 20H having miniaturized openings of 1000 nm or less, excessive wet etching is prevented from progressing locally in the metal mask substrate 10. Therefore, some of the through holes 20H among the plurality of through holes 20H are prevented from becoming larger.

[0036] The metal mask 20 has a back surface 20R and a front surface 20F opposite to the back surface 20R. When a vapor deposition pattern is formed using the metal mask 20, the back surface 20R faces the vapor deposition target, and the front surface 20F faces the vapor deposition source. The metal mask 20 is used to form pixels included in an organic EL display device.

[0037] The metal mask 20 includes a mask portion 20A and a peripheral portion 20B surrounding the mask portion 20A. In the example shown in FIG. 8 , the metal mask 20 includes a plurality of mask portions 20A. A plurality of through holes 20H are formed in each mask portion 20A. Each through hole 20H penetrates the metal mask 20 in the thickness direction of the metal mask 20. Each through hole 20H is a passage for the vapor deposition material. The vapor deposition material passes through the through holes 20H to form a vapor deposition pattern having a predetermined shape on the vapor deposition target. The peripheral portion 20B does not include a through hole 20H. Of the metal mask 20, the peripheral portion 20B has the maximum thickness. The mask portion 20A may or may not have the maximum thickness.

[0038] The metal mask 20 may include an oxide layer composed of an oxide of an iron-nickel-based alloy. The oxide layer includes the back surface 20R of the metal mask 20. That is, the oxide layer corresponds to the second surface layer 10B2 of the metal mask substrate 10 described above. Since the metal mask 20 includes the oxide layer, pitting corrosion is likely to occur in the metal mask substrate 10 used to form the metal mask 20 when the through holes 20H in the metal mask 20 are formed. This increases the effectiveness of the metal mask substrate 10 having a KAM value of 2.18° or greater.

[0039] 10 shows the shape of the through-hole 20H as viewed from a viewpoint facing the rear surface 20R of the metal mask 20. As shown in FIG. 10, the second opening 20H2 of the through-hole 20H may have, for example, a square shape. In the example shown in FIG. 10, the second opening 20H2 has a square shape with curvature at each corner. The center of curvature of each corner is located within the second opening 20H2. In each second opening 20H2, the length L of one side is, for example, 40 μm or less, and therefore the area of ​​the second opening 20H2 is 1600 μm. 2 The shape of the second opening 20H2 is not limited to a square, but may be a quadrangular shape other than a square, or may be a circular shape. 2 If this is the case, the length of one side of the second opening 20H2 is 30 μm or less.

[0040] On the front surface 20F, the second openings 20H2 are arranged according to a predetermined rule. In the example shown in Fig. 9, the second openings 20H2 are arranged in a lattice pattern. The second openings 20H2 may also be arranged in a staggered pattern, for example.

[0041] 11 and 12 show the cross-sectional structure of the metal mask 20 along a plane perpendicular to the front surface 20F of the metal mask 20. Fig. 11 shows the cross-sectional structure of a first example of the metal mask 20, while Fig. 12 shows the cross-sectional structure of a second example of the metal mask 20. Note that Fig. 11 shows the cross-sectional structure of the metal mask 20 when the metal mask substrate 10 is etched only from the front surface 10F. In contrast, Fig. 12 shows the cross-sectional structure of the metal mask 20 when the metal mask substrate 10 is etched from both the front surface 10F and the back surface 10R.

[0042] 11 , in the first example of the metal mask 20, the first opening 20H1 of the through hole 20H is located on the front surface 20F, and the second opening 20H2 is located on the back surface 20R. The through hole 20H has a shape that tapers from the front surface 20F to the back surface 20R. That is, the area of ​​the through hole 20H in a plane perpendicular to the thickness direction monotonically decreases from the front surface 20F to the back surface 20R. The through hole 20H has a substantially arc shape.

[0043] 12 , in the second example of the metal mask 20, the first opening 20H1 of the through hole 20H is located on the front surface 20F, and the second opening 20H2 is located on the back surface 20R. The through hole 20H has a large hole portion 20HL and a small hole portion 20HS. The large hole portion 20HL has a shape that tapers in the direction from the front surface 20F to the back surface 20R, and the small hole portion 20HS has a shape that tapers in the direction from the back surface 20R to the front surface 20F.

[0044] That is, the area of ​​the large hole portion 20HL in a plane perpendicular to the thickness direction monotonically decreases in the direction from the front surface 20F to the back surface 20R, and the area of ​​the small hole portion 20HS monotonically decreases in the direction from the back surface 20R to the front surface 20F. Therefore, the area of ​​the through hole 20H in a plane perpendicular to the thickness direction is smallest at the connection portion between the large hole portion 20HL and the small hole portion 20HS.

[0045] In the case of a metal mask 20 formed using the metal mask substrate 10 of the present disclosure, regardless of whether it is the first or second example described above, the second opening 20H2 is prevented from becoming larger in some of the through holes 20H among the multiple through holes 20H, and therefore the size of the through holes 20H is prevented from becoming larger.

[0046] [Metal Mask Substrate Manufacturing Method] A method for manufacturing a metal mask substrate will be described with reference to FIGS. 13 and 14 . The metal mask substrate manufacturing method of the present disclosure is a method for manufacturing a metal mask substrate, which is a metal plate composed of an iron-nickel alloy. The manufacturing method includes rolling a metal plate base material to obtain a rolled material, and annealing the rolled material at a temperature of 720°C or less. As described above, in the metal plate, when the step size is set to 0.5 μm and boundaries where the difference in crystal orientation is 5° or more are considered to be grain boundaries, the KAM value obtained by electron backscatter diffraction is 2.18° or more. The metal plate has a thickness of 10 μm or more and 30 μm or less. The metal mask substrate manufacturing method will be described in detail below with reference to the drawings.

[0047] 13 , in the method for manufacturing the metal mask substrate 10, first, a base material 31A made of an iron-nickel alloy is prepared. The base material 31A has a strip shape extending along the stretching direction D1. Next, the base material 31A is rolled to obtain a rolled material 31B. In this process, for example, after hot rolling, cold rolling and annealing are alternately performed one or more times to obtain the rolled material 31B.

[0048] When rolling the base material 31A, for example, the base material 31A is transported along the transport direction D2 toward a rolling device 50 equipped with a pair of rolling rollers 51, 52 so that the extension direction D1 of the base material 31A and the transport direction D2 in which the base material 31A is transported are parallel.

[0049] The base material 31A may be, for example, a billet obtained by hot forging a slab. The thickness of the billet may be, for example, 150 mm or more and 250 mm or less. In hot rolling, the billet is rolled until it has a thickness of 3 mm or more and 20 mm or less, thereby obtaining a hot-rolled material. In alternating cold rolling and annealing, the hot-rolled material is rolled until it has a thickness of 10 μm or more and 30 μm or less, thereby obtaining a rolled material 31B. The rolled material 31B is wound around a core C, but the rolled material 31B may also be handled in a strip-like stretched state without being wound around a core C.

[0050] When cold rolling is performed multiple times, the reduction in the final cold rolling may be 30% or more and 95% or less. When cold rolling is performed multiple times, the reduction in the cold rolling may be decreased each time from the first cold rolling to the final cold rolling. The reduction is calculated by the following formula.

[0051] Reduction rate (%)={(T0−T1) / T0}×100 In the above formula, T0 is the thickness of the object to be rolled, and T1 is the thickness of the plate material obtained by rolling.

[0052] 14 , the rolled material 31B obtained by rolling a steel billet is annealed using an annealing device 53. This reduces the residual stress that occurs in the rolled material 31B due to rolling, making it possible to obtain a metal mask substrate 10 with reduced residual stress. As described above, in the method for manufacturing the metal mask substrate 10 of the present disclosure, the rolled material 31B obtained through rolling is annealed at a temperature of 720°C or lower. This makes it possible to obtain a metal mask substrate 10 with a KAM value of 2.18° or higher.

[0053] As described above, if the base material 31A is subjected to hot rolling followed by repeated cold rolling and annealing one or more times, the annealing temperature for the rolled material 31B obtained by these processes is set to a temperature of 720°C or less.

[0054] The rolled material 31B may be annealed at a temperature of 300°C or higher. This allows for the production of a metal mask substrate 10 having a KAM value of 2.76° or lower. From the viewpoint of suppressing warpage of the metal mask substrate 10 after etching and suppressing the occurrence of localized etching, the temperature in the final annealing performed after rolling is preferably 300°C or higher and 720°C or lower. By setting the temperature in the final annealing to 300°C or higher, it is possible to reduce residual stress generated in the rolled material 31B by rolling, thereby making it possible to suppress warpage after etching.

[0055] In the annealing after rolling, the rolled material 31B may be annealed while being pulled along the transport direction D2. That is, tension annealing may be performed on the rolled material 31B. This makes it possible to further reduce residual stress generated in the rolled material 31B by rolling.

[0056] The rolling and annealing steps described above may be modified as follows. For example, rolling may be performed using a rolling mill equipped with multiple pairs of rollers. Furthermore, annealing after rolling may be performed on the rolled material 31B wound around the core C, rather than annealing the rolled material 31B while pulling it along the transport direction D2.

[0057] When the rolled material 31B wound around the core C is annealed after rolling, the metal mask substrate 10 obtained after annealing may warp according to the diameter of the metal mask substrate 10 due to the rolled material 31B being wound around the core C. Therefore, depending on the diameter of the metal mask substrate 10 wound around the core C and the material constituting the base material 31A, it is preferable to anneal the rolled material 31B while pulling it along the transport direction D2.

[0058] [Metal Mask Manufacturing Method] A metal mask manufacturing method will be described with reference to FIGS. 15 to 20 . The method for manufacturing a metal mask 20 of the present disclosure includes forming a resist layer on a metal plate, forming a resist pattern from the resist layer, and forming multiple through holes in the metal plate by wet etching using the resist pattern. As described above, when the step size of the metal plate is set to 0.5 μm and boundaries where the difference in crystal orientation is 5° or more are considered to be grain boundaries, the KAM value obtained by electron backscatter diffraction analysis is 2.18° or more. The metal plate has a thickness of 10 μm or more and 30 μm or less. The metal mask manufacturing method will be described in detail below with reference to the drawings. Note that for convenience of illustration, FIGS. 15 to 20 illustrate the process of forming one through hole in the second example of the metal mask 20 described above.

[0059] As shown in Figure 15, a first resist layer R1 is located on the front surface 10F of the metal mask substrate 10. The first resist layer R1 is formed of, for example, a negative resist. A second resist layer R2 is located on the back surface 10R. The second resist layer R2 is formed of, for example, a negative resist. The first resist layer R1 and the second resist layer R2 may be formed of a positive resist. Each resist layer R1, R2 may be a dry film resist or may be formed of a coating type resist.

[0060] 16, after the first resist layer R1 and the second resist layer R2 are exposed, the first resist layer R1 and the second resist layer R2 are developed. As a result, a first resist pattern RP1 is formed from the first resist layer R1, and a second resist pattern RP2 is formed from the second resist layer R2. A developer such as an aqueous sodium carbonate solution is used to develop each of the resist layers R1 and R2.

[0061] The first resist pattern RP1 has a first through hole RP1A. The first through hole RP1A penetrates the first resist pattern RP1 along the thickness direction of the first resist pattern RP1. The second resist pattern RP2 has a second through hole RP2A. The second through hole RP2A penetrates the second resist pattern RP2 along the thickness direction of the second resist pattern RP2. When viewed from a viewpoint opposite to the plane in which the first resist pattern RP1 extends, the second through hole RP2A is located within the first through hole RP1A.

[0062] As shown in FIG. 17 , a first protective layer PL1 is formed on the surface of the first resist pattern RP1. By forming the first protective layer PL1, the first through holes RP1A are blocked, thereby preventing the etching solution from reaching the metal mask substrate 10 through the first through holes RP1A. Next, the metal mask substrate 10 is etched from the rear surface 10R using the second resist pattern RP2. An etching solution containing chloride ions, for example, is used to etch the metal mask substrate 10. The etching solution may be a ferric chloride solution, as described above. This forms small holes 10HS opening on the rear surface 10R.

[0063] The thickness of the resist patterns RP1 and RP2 may be 10 μm or less, preferably 7 μm or less, and more preferably 5 μm or less. The thinner the resist patterns RP1 and RP2 are, the more easily the etching liquid penetrates into the through holes RP1A and RP2A of the resist patterns RP1 and RP2.

[0064] At this time, each small hole portion 10HS has an opening on the rear surface 10R of the metal mask substrate 10, and the area of ​​each opening is 1600 μm 2 The plurality of small holes 10HS may be formed as follows: That is, the area of ​​each opening located on the rear surface 10R is, for example, 1600 μm 2 Furthermore, the area of ​​each opening may be 900 μm or less. 2 It is preferable that:

[0065] In this case, the area of ​​the openings in the second resist pattern RP2 used to form the openings in the metal mask 20 is also very small, which makes it difficult for the etching solution to penetrate into the openings in the second resist pattern RP2. As a result, etching is likely to vary across the surface of the metal mask substrate 10, making it possible to more significantly obtain the effect of the metal mask substrate 10 having a KAM value of 2.18° or greater.

[0066] 18 , the first protective layer PL1 is removed from the surface of the first resist pattern RP1. The second resist pattern RP2 is also removed from the rear surface 10R of the metal mask substrate 10. Next, the rear surface 10R of the metal mask substrate 10 is covered with the second protective layer PL2. At this time, the second protective layer PL2 is formed on the rear surface 10R so that a portion of the second protective layer PL2 fills the small holes 10HS.

[0067] As shown in FIG. 19 , the metal mask substrate 10 is etched from the surface 10F using the first resist pattern RP1. To etch the metal mask substrate 10, an etching solution containing, for example, chloride ions is used, as in the case of forming the small hole portions 10HS. As described above, the etching solution may be a ferric chloride solution. This forms large hole portions 10HL that open to the surface 10F. The large hole portions 10HL are formed so as to reach portions of the second protective layer PL2 filled in the small hole portions 10HS, thereby connecting the large hole portions 10HL to the small hole portions 10HS.

[0068] 20 , the first resist pattern RP1 is removed from the front surface 10F of the metal mask substrate 10, and the second protective layer PL2 is removed from the back surface 10R. This results in a metal mask 20 having through holes 20H. In the through holes 20H, the large hole portions 20HL correspond to the large hole portions 10HL formed in the metal mask substrate 10, and the small hole portions 20HS correspond to the small hole portions 10HS formed in the metal mask substrate 10. Furthermore, the front surface 20F of the metal mask 20 corresponds to the front surface 10F of the metal mask substrate 10, and the back surface 20R of the metal mask 20 corresponds to the back surface 10R of the metal mask substrate 10.

[0069] When the second protective layer PL2 is formed on the rear surface 10R of the metal mask substrate 10, the second resist pattern RP2 does not have to be removed from the rear surface 10R of the metal mask substrate 10. In this case, the second protective layer PL2 is formed on the second resist pattern RP2. The second protective layer PL2 is formed so that a portion of the second protective layer PL2 fills the small hole portion 10HS and the second through hole RP2A of the second resist pattern RP2. After the large hole portion 10HL is formed in the metal mask substrate 10, the second resist pattern RP2 is removed from the metal mask substrate 10 together with the second protective layer PL2.

[0070] Furthermore, when the first example of the metal mask 20 is manufactured, the process of etching the metal mask substrate 10 from the back surface 10R is omitted. Therefore, the process of forming the second resist pattern RP2 on the back surface 10R is also omitted. Note that when the metal mask substrate 10 is etched from the front surface 10F, a protective layer is formed on the back surface 10R of the metal mask substrate 10.

[0071] [Examples] Examples and comparative examples will be described with reference to FIGS. 21 to 23 and Table 1. [Example 1] A slab made of an iron-nickel alloy and having a thickness of 200 mm was prepared. The slab was then hot forged to produce a steel billet. The steel billet was then hot rolled to a thickness of 400 μm to obtain a hot-rolled material. Subsequently, cold rolling and annealing were alternately performed three times to obtain a rolled material having a thickness of 25 μm. In this process, the reduction ratio in the first cold rolling was set to 70%, the reduction ratio in the second cold rolling was set to 62.5%, and the reduction ratio in the third cold rolling was set to 44.4%. Thus, the total reduction ratio of the rolled material after the three cold rollings on the hot-rolled material before cold rolling was set to 93.8%. The rolled material was then subjected to tension annealing. At this time, the annealing temperature of the rolled material in the tension annealing was set to 620° C., and the holding time was set to 4.5 seconds. As a result, a metal mask substrate of Example 1 having a thickness of 25 μm was obtained.

[0072] Example 2 A metal mask substrate of Example 2 was obtained in the same manner as in Example 1, except that the annealing temperature in the tension annealing was changed to 680°C.

[0073] Example 3 A metal mask substrate of Example 3 was obtained in the same manner as in Example 1, except that the annealing temperature in the tension annealing was changed to 720°C.

[0074] Comparative Example 1 A metal mask substrate of Comparative Example 1 was obtained in the same manner as in Example 1, except that the annealing temperature in the tension annealing was changed to 760°C.

[0075] Comparative Example 2 A metal mask substrate of Comparative Example 2 was obtained in the same manner as in Example 1, except that the annealing temperature in the tension annealing was changed to 800°C.

[0076] Comparative Example 3 A metal mask substrate of Comparative Example 3 was obtained in the same manner as in Example 1, except that the annealing temperature in the tension annealing was changed to 900°C.

[0077] [Evaluation Method] [KAM Value] When measuring the KAM value, first, a 2.5 μm thickness was removed from the surface of each metal mask substrate by buffing and ion milling. This created an observation surface. Next, using an FE-SEM (SU-70, manufactured by Hitachi High-Technologies Corporation) and an OIM (Orientation Imaging Microscopy) crystal orientation measurement device (Digiview 5, manufactured by TSL Solutions Co., Ltd.), the KAM value was measured by the EBSD method for a 50 μm square observation area on the observation surface. In this case, the step size was set to 0.5 μm, and boundaries where the difference in crystal orientation was 5° or more were considered to be grain boundaries. The KAM value was measured for five randomly selected, non-overlapping measurement areas on the observation surface of each metal mask substrate, and the average of the KAM values ​​obtained in each measurement area was set as the KAM value of each metal mask substrate. The KAM value was calculated using data collection software and data analysis software included in the OIM crystal orientation measurement device.

[0078] [Etching] A dry film resist with a thickness of 10 μm was attached to the surface of each metal mask substrate. Next, square through-holes with a side length of 25 μm were formed in the dry film resist by photolithography, thereby obtaining a resist pattern. At this time, the through-hole pitch was set to 50 μm. The metal mask substrate was then etched using a ferric chloride solution to an etching depth of 8 μm. At this time, the concentration of the etching solution was set to 50° Baume, and the temperature of the etching solution was set to 50° C. Subsequently, the resist pattern was removed from the surface of the vapor deposition metal mask substrate to obtain an etched test piece.

[0079] The surface of each test piece was imaged using a laser microscope (VK-X3000, manufactured by Keyence Corporation) to obtain an image of the surface including a plurality of openings. Then, the areas of 1000 openings included in the surface were calculated by image analysis. Of the 1000 openings, the average area of ​​the 10 openings from the smallest opening to the tenth smallest opening was calculated, and this average value was set as the reference value. Then, openings having an area 1.2 times or more larger than the reference value were considered to be openings in which local etching had progressed and were larger than the other openings. Then, the percentage of openings in which local etching had progressed among the 1000 openings was calculated.

[0080] [Evaluation Results] For the metal mask substrates of each Example and Comparative Example, the annealing temperature set during tension annealing, the KAM value, and the incidence rate, which is the percentage of openings where local etching has progressed, are as shown in Table 1 below.

[0081]

[0082] As shown in Table 1, the KAM values ​​of the metal mask substrates were found to be 2.31° in Example 1, 2.23° in Example 2, and 2.18° in Example 3. Also, the KAM values ​​were found to be 2.11° in Comparative Example 1, 2.07° in Comparative Example 2, and 1.92° in Comparative Example 3. Thus, in Examples 1 to 3, the KAM values ​​were found to be 2.18° or more and 2.31° or less. In contrast, in Comparative Examples 1 to 3, the KAM values ​​were found to be 1.92° or more and 2.11° or less.

[0083] Furthermore, it was found that the incidence of localized etching was 0% in Examples 1 to 3, 20.0% in Comparative Example 1, 69.5% in Comparative Example 2, and 95.6% in Comparative Example 3.

[0084] As described above, it was confirmed that the progress of localized etching was suppressed when the KAM value was 2.18° or more. Also, as shown in Fig. 21, it was confirmed that the progress of localized etching was suppressed more rapidly when the KAM value was 2.11° than when the KAM value was greater than 2.11°, and furthermore, it was confirmed that the progress of localized etching did not occur when the KAM value was 2.18° or more.

[0085] 22 is an example of an SEM image of the surface of a test piece obtained from the metal mask substrate of Comparative Example 1. As shown in FIG. 22, the multiple openings located on the surface 40F of the test piece were found to include first openings 40A1, which were not locally etched, and second openings 40A2, which were locally etched. The area of ​​the second openings 40A2 was found to be larger than that of the first openings 40A1, and the depth of the recesses having the second openings 40A2 was found to be deeper than that of the recesses having the first openings 40A1. Furthermore, the bottom of the recesses having the second openings 40A2 was found to be unimaged due to the high surface roughness at the bottom.

[0086] Fig. 23 shows the relationship between the annealing temperature during tension annealing and the KAM value of the metal mask substrate. As shown in Fig. 23, it was confirmed that there is a negative correlation between the annealing temperature during tension annealing and the KAM value of the metal mask substrate. Furthermore, an approximation curve represented by the following formula was obtained from the annealing temperature and the KAM value. In Fig. 23, the approximation curve is indicated by a dashed line.

[0087] y = -0.0014x + 3.1764 Based on the above formula, it was found that the KAM values ​​obtained were as follows. That is, when the annealing temperature was 550 ° C, the KAM value was 2.41 °, when the annealing temperature was 500 ° C, the KAM value was 2.48 °, and when the annealing temperature was 450 ° C, the KAM value was 2.55 °. It was also found that when the annealing temperature was 400 ° C, the KAM value was 2.62 °, when the annealing temperature was 350 ° C, the KAM value was 2.69 °, and when the annealing temperature was 300 ° C, the KAM value was 2.76 °.

[0088] When the annealing temperature in tension annealing is 300°C or higher, warping of the metal mask substrate after wet etching is suppressed. Therefore, from the viewpoint of suppressing warping of the metal mask substrate, it is preferable that the KAM value is 2.76° or less.

[0089] As described above, the metal mask substrate, the method for manufacturing a metal mask substrate, and one embodiment of the method for manufacturing a metal mask can provide the following advantages: (1) When multiple through holes are formed in the metal mask substrate 10, the KAM value of the metal mask substrate 10 is 2.18° or greater, which prevents some of the multiple through holes from becoming larger.

[0090] (2) When the KAM value of the metal mask substrate 10 is 2.76° or less, it is possible to suppress the residual strain of the metal mask substrate to such an extent that the metal mask substrate does not warp after wet etching of the metal mask substrate 10.

[0091] (3) The area of ​​the opening formed on the rear surface 10R of the metal mask substrate 10 is 1600 μm 2 If the KAM value of the metal mask substrate 10 is 2.18° or more, the area of ​​the openings in the second resist pattern RP2 used to form the openings is also very small, making it difficult for the etching solution to penetrate into the openings in the second resist pattern RP2. As a result, etching is likely to vary across the surface of the metal mask substrate 10, making it possible to more significantly obtain the effect of the metal mask substrate 10 having a KAM value of 2.18° or more.

[0092] The above-described embodiment can be modified as follows. [Applications] The metal mask is not limited to a metal mask used to form pixels in an organic EL display device. The metal mask may also be, for example, a mask for forming a pattern used in electronic devices or electronic components other than organic EL display devices. The film formation method using the metal mask may be a vapor deposition method or a sputtering method. The through holes in the metal mask may have an arrangement corresponding to the pattern formed using the metal mask when viewed in plan from the back surface. Such a metal mask enables high-definition patterns, which in turn makes it possible to achieve smaller, lighter, and thinner electronic devices and electronic components that require high-definition patterns.

Claims

1. A metal mask substrate which is a metal plate made of an iron-nickel alloy, the step size of which is set to 0.5 μm, and the boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary has a KAM value of 2.18° or more obtained by electron backscatter diffraction method, and the substrate has a thickness of 10 μm or more and 30 μm or less.

2. The metal mask substrate according to claim 1, wherein the KAM value is 2.76° or less.

3. A method for manufacturing a metal mask substrate, which is a metal plate made of an iron-nickel alloy, comprising: rolling a base material of the metal plate to obtain a rolled material; and annealing the rolled material at a temperature of 720°C or less, wherein, when a step size is set to 0.5 μm in the metal plate and a boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary, a KAM value obtained by electron backscatter diffraction method is 2.18° or more, and the metal plate has a thickness of 10 μm or more and 30 μm or less.

4. The method for manufacturing a metal mask substrate according to claim 3, wherein annealing includes annealing the rolled material at a temperature of 300°C or higher, and the KAM value is 2.76° or less.

5. A method for manufacturing a metal mask, comprising: forming a resist layer on a metal plate; forming a resist pattern from the resist layer; and forming a plurality of through holes in the metal plate by wet etching using the resist pattern, wherein, in the metal plate, a step size is set to 0.5 μm, and when a boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary, a KAM value obtained by electron backscatter diffraction method is 2.18° or more, and the metal plate has a thickness of 10 μm or more and 30 μm or less.

6. The formation of the plurality of through holes includes forming the through holes such that each through hole has an opening on the first surface of the metal plate, and each opening has an area of ​​1600 μm 2 The method for manufacturing a metal mask according to claim 5 , comprising forming the plurality of through holes as follows:

Citation Information

Patent Citations

  • Metal plate for manufacturing vapor deposition mask, manufacturing method of metal plate, vapor deposition mask, manufacturing method of vapor deposition mask, and vapor deposition mask device including vapor deposition mask

    JP2021036076A

  • Cu-Ni-Si-BASED COPPER ALLOY SHEET MATERIAL, PRODUCTION METHOD THEREFOR AND ELECTRIC CONDUCTION COMPONENT

    JP2021110038A

  • Metal mask material and production method therefor

    WO2018043642A1

  • Alloy metal plate and deposition mask including same

    WO2020105910A1

  • Copper alloy, copper alloy plastic-processed material, component for electronic and electric devices, terminal, bus bar, and heat dissipation substrate

    WO2021107096A1