Powder for thermal spraying

The thermal spray powder with composite particles and optimized pore distribution addresses the uniformity and conductivity issues in SOFC and SOEC, enhancing the efficiency of these cells by ensuring uniform component dispersion and improved electrical conductivity.

WO2024204567A1PCT designated stage expired Publication Date: 2024-10-03FUJIMI INCORPORATED
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012706
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing thermal spray powders for solid oxide fuel cells (SOFC) and solid oxide electrolysis cells (SOEC) lack uniformity in component distribution, leading to reduced electrical conductivity and operating efficiency.

Method used

A thermal spray powder comprising composite particles of ion-conductive ceramic and transition metal compound particles, with a specific pore size distribution and bonding structure, is used to improve uniformity and conductivity, featuring a peak in log differential pore volume distribution between 0.15 μm and 1 μm, and a mass ratio of ceramic to transition metal compound particles ranging from 60:40 to 20:80, with zirconia and nickel oxide as preferred materials.

Benefits of technology

The solution enhances the uniformity and electrical conductivity of the thermal spray coating, improving the operating efficiency of SOFC and SOEC by ensuring uniform dispersion of ceramic and transition metal components, thereby increasing power generation and hydrogen production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012706_03102024_PF_FP_ABST
    Figure JP2024012706_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a technique for improving the uniformity of components in a spray coating. The powder for thermal spraying disclosed herein is a powder for thermal spraying for forming an electrode of a solid oxide fuel cell or a solid oxide electrolytic cell. This powder for thermal spraying has a peak in a range of 0.15-1 µm inclusive in a log differential pore volume distribution having a pore diameter of 1 µm or less obtained by a mercury press-in method.
Need to check novelty before this filing date? Find Prior Art

Description

Thermal spray powder

[0001] This application claims priority based on Japanese Patent Application No. 2023-058417, filed on March 31, 2023, the entire contents of which are incorporated herein by reference.

[0002] The present disclosure relates to thermal spray powders.

[0003] Solid oxide fuel cells (SOFCs) and solid oxide electrolysis cells (SOECs) include an air electrode, an anode, and a solid electrolyte layer. In this regard, Patent Document 1 discloses an anode for a solid oxide fuel cell, characterized in that it is obtained by firing a particle mixture of electrolyte material particles having an average particle size D50 of 0.1 to 0.6 μm and nickel oxide particles having an average particle size D50 of 0.5 to 1.5 μm, with the mass ratio of the electrolyte material particles to the nickel oxide particles being 35:65 to 50:50. This document also describes that this configuration can reduce the interfacial resistance between the anode and the electrolyte. Patent Document 2 also discloses a nickel-ion-conductive ceramic mixed powder for use in an anode. This mixed powder contains metallic nickel particles (A) having a median diameter of 10 nm or more and 200 nm or less, and ion-conductive ceramic particles (B) having a median diameter of 10 nm or more and 200 nm or less. This mixed powder is characterized in that the content of elemental nickel in the mixed powder and the content of the ion-conductive ceramic particles are in a volume ratio of [elemental nickel] / [ion-conductive ceramic particles] = 20 / 80 to 80 / 20. The document states that by achieving both high catalytic activity and high conductivity, it is possible to reduce internal resistance and improve the operating efficiency as a functional material.

[0004] JP 2009-266713 A JP 2021-28417 A

[0005] Incidentally, the anode is a porous membrane that contains ion-conductive ceramic particles and metal particles, with voids formed between the particles (see Patent Documents 1 and 2). In such an anode, it is required that the ceramic particles, metal particles, and voids are uniformly dispersed.

[0006] In view of these circumstances, an object of the present invention is to provide a technique for improving the uniformity of components in a thermal spray coating.

[0007] The thermal spray powder disclosed herein is a thermal spray powder for forming electrodes for solid oxide fuel cells or solid oxide electrolysis cells. The thermal spray powder has a peak in the range of 0.15 μm or more and 1 μm or less in the log differential pore volume distribution of pores with diameters of 1 μm or less obtained by mercury intrusion porosimetry. Use of a thermal spray powder with such a configuration can improve the uniformity of the components in the thermal spray coating.

[0008] In a preferred embodiment of the thermal spray powder disclosed herein, the thermal spray powder contains composite particles that include ion-conductive ceramic particles and transition metal compound particles. By using a thermal spray powder with this configuration, the uniformity of the components in the thermal spray coating can be improved and electrical conductivity can be imparted to the thermal spray coating.

[0009] In a preferred embodiment of the thermal spray powder disclosed herein, the composite particles have regions where the primary particles are in contact with each other and where there is no particle interface at the contact points. This configuration makes it easier to achieve the desired pore size distribution in the thermal spray powder. This can further improve the uniformity of the components in the thermal spray coating.

[0010] In another preferred embodiment of the thermal spray powder disclosed herein, the ratio of ceramic particles to transition metal compound particles (ceramic particles:transition metal compound particles) is 60:40 to 20:80. This configuration improves the ionic conductivity of the formed thermal spray coating while suppressing a decrease in the electrical conductivity of the electrodes. This increases the operating efficiency of the SOFC or SOEC.

[0011] In another preferred embodiment of the thermal spray powder disclosed herein, the median diameter (D 50 ) is 10 μm or more and 100 μm or less. This configuration can improve the fluidity of the thermal spray powder.

[0012] In another preferred embodiment of the thermal spray powder disclosed herein, the ceramic particles are zirconia particles containing a rare earth metal oxide. Such ceramic particles are suitable for achieving the effects of the technology disclosed herein. Furthermore, the transition metal compound particles are preferably nickel oxide particles. Such transition metal compound particles are suitable for achieving the effects of the technology disclosed herein.

[0013] In another preferred embodiment of the thermal spray powder disclosed herein, when the thermal spray powder is subjected to a reduction treatment in a hydrogen gas atmosphere at a treatment temperature of 800°C for two hours, and then heated in an air atmosphere from room temperature to 1200°C at a temperature increase rate of 10 K / min and subjected to thermogravimetric analysis, the temperature at which the weight increases by 3% is 470°C or higher and 570°C or lower. With this configuration, when a thermal spray coating formed from this thermal spray powder is used to form an electrode, the conductivity of the electrode can be increased.

[0014] In another preferred embodiment of the thermal spray powder disclosed herein, the peak is in the range of 0.15 μm or more and 0.23 μm or less. This configuration can further improve the uniformity of the components in the thermal spray coating.

[0015] FIG. 1 is a cross-sectional view of an SOFC 10. FIG. 2 is a plan view image of the thermal spray powder of Example 3. FIG. 3 is an enlarged image of FIG. 2. FIG. 4 is a cross-sectional view image of the thermal spray powder of Example 3. FIG. 5 is a plan view image of the thermal spray powder of Example 4. FIG. 6 is an enlarged image of FIG. 5. FIG. 7 is a cross-sectional view image of the thermal spray powder of Example 4. FIG. 8 is a plan view image of the thermal spray powder of a comparative example. FIG. 9 is an enlarged view of FIG. 8. FIG. 10 is a cross-sectional view image of the thermal spray powder of a comparative example. FIG. 11 is a graph showing the log differential pore volume distribution of each example. FIG. 12 is a graph showing the log differential pore volume distribution of each example.

[0016] Preferred embodiments of the technology disclosed herein are described below. Matters necessary for implementing the present invention other than those specifically mentioned in this specification can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The technology disclosed herein can be implemented based on the content disclosed in this specification and the technical common sense in the relevant field. In the specification, the expression "X to Y" indicating a numerical range means "X or more and Y or less" unless otherwise specified, and also means a range "greater than X and less than Y," a range "greater than X and less than Y," and a range "greater than X and less than Y."

[0017] <Definitions> In this specification, the term "thermal spray powder" refers to a powdered material used for thermal spraying. Furthermore, in this specification, the term "composite particle" refers to a particulate matter (in the form of a particle) composed of multiple different materials, which are bonded together and behave as a single particle. Examples of composite particles include granulated particles and granulated sintered particles composed of at least two types of materials. In this specification, the term "primary particle" refers to the smallest unit that can be identified as a granular matter from its appearance among the morphological components that make up the thermal spray powder. Therefore, when the composite particle that makes up the thermal spray powder disclosed herein contains secondary particles, the particles that make up the secondary particles are referred to as primary particles, for example. Here, the term "secondary particle" refers to a particulate matter in which primary particles are bonded three-dimensionally and behave as a single particle. Examples of the "secondary particle" referred to here include granulated particles and particles that have been sintered after granulation (granulated sintered particles).

[0018] Here, "bonding" refers to the direct or indirect bonding of two or more primary particles. Examples of "bonding" include bonding between primary particles due to a chemical reaction, bonding between primary particles due to simple adsorption, bonding using the anchor effect of allowing an adhesive or the like to penetrate the unevenness of the primary particle surface, bonding between primary particles due to the electrostatic attraction effect, and bonding between primary particles formed by melting the surfaces of the primary particles. Furthermore, with regard to secondary particles composed of two or more materials, "bonding" includes bonding between primary particles formed by one material and melting the other material to form the primary particles. Furthermore, in this specification, the term "raw material particles" refers to particles that form the powder in the raw material stage used to produce the thermal spray powder disclosed herein.

[0019] <Method for Measuring Median Diameter> In this specification, the term "median diameter" for a thermal spray powder and primary particles constituting secondary particles (thermal spray powder) refers to the median diameter (D) at an integrated value of 50% in a volume-based particle size distribution measured using a particle size distribution measuring device based on a laser scattering / diffraction method. 50 The median diameter is measured using, for example, a commercially available measuring device.

[0020] The above-mentioned Patent Documents 1 and 2 cite methods such as screen printing and doctor blade methods as means for applying a paste (slurry) for forming an electrode containing a powder material to a substrate. However, the present inventors wanted to form an electrode by thermal spraying a powder material. Thermal spraying is a process in which a powder material is molten or semi-molten and sprayed onto the surface of a substrate to form a film, and is completely different from processes such as screen printing and doctor blade. For this reason, the present inventors investigated the composition of a powder material (thermal spray powder) that is suitable for forming an electrode by thermal spraying and can improve the uniformity of the components in the thermal spray coating.

[0021] <Configuration of Thermal Spray Powder> The thermal spray powder disclosed herein may include, for example, composite particles containing ceramic particles and transition metal compound particles. The thermal spray powder is preferably composed of composite particles containing ceramic particles and transition metal compound particles, but may also include unavoidable impurities resulting from the ceramic particles, transition metal compound particles, or the manufacturing process of the composite particles. The content of the unavoidable impurities relative to the entire thermal spray powder is generally 5% by mass or less, preferably 3% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, and particularly preferably 0.1% by mass or less, and the closer to 0% by mass the better.

[0022] The ceramic particles have, for example, ion conductivity. Here, the ceramic particles preferably have oxide ion conductivity. The ceramic constituting the ceramic particles is appropriately selected from ceramics used for this type of application. Examples of such ceramics include metal oxides. For example, zirconium oxide (zirconia) and cerium oxide (ceria) are preferably used as metal oxides.

[0023] The zirconium oxide may be stabilized zirconia in which one or more stabilizers are dissolved. The stabilized zirconia means zirconia containing a stabilizer. Examples of the stabilizer include scandium oxide (Sc). 2 O 3 ), yttrium oxide (yttria; Y 2 O 3 ), cerium oxide (ceria; CeO 2 ), gadolinium oxide (gadolinium; Gd 2 O 3 ), ytterbium oxide (Yb 2 O 3Examples of suitable ceramic particles include rare earth metal oxides such as zirconia particles containing a rare earth metal oxide; and alkaline earth metal oxides such as calcium oxide (calcia; CaO) and magnesium oxide (magnesia; MgO). Preferably, the ceramic particles are zirconia particles containing a rare earth metal oxide. The effects of the technology disclosed herein are more effectively realized when an electrode (here, a fuel electrode) containing zirconia particles containing a rare earth metal oxide is produced as the ceramic particles. Of these, scandia-stabilized zirconia particles and yttria-stabilized zirconia can be preferably used.

[0024] The cerium oxide here can be doped ceria. The doped ceria can be yttrium oxide (yttria; Y 2 O 3 ), samarium oxide (samaria; Sm 2 O 3 ), gadolinium oxide (gadolinium; Gd 2 O 3 ) or other rare earth metal oxide-doped ceria.

[0025] The median diameter of the ceramic particles is not limited as long as the effects of the technology disclosed herein are achieved. The median diameter is, for example, 0.01 μm to 5 μm, preferably 0.05 μm to 2.5 μm, more preferably 0.1 μm to 1 μm, and even more preferably 0.1 μm to 0.5 μm. By setting the median diameter of the ceramic particles within the above range, the dispersibility of the ceramic particles in the composite particles can be improved, and ultimately, the uniformity of the components in the thermal spray coating can be improved. This can improve the operating efficiency of the SOFC or SOEC.

[0026] The transition metal compounds include substances exhibiting metallic properties, such as alloys, solid solutions, and intermetallic compounds composed of the transition metal element and at least one of other metal elements and metalloid elements, as well as compounds (e.g., oxides) of the transition metal element and a non-metal element. Examples of the transition metal compounds include oxides (transition metal oxides) of 3d transition elements such as titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), and copper (Cu); metals such as precious metal elements, such as ruthenium (Ru), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), platinum (Pt), gold (Au), and silver (Ag); and alloys such as platinum-palladium alloys and platinum-rhodium alloys. Other examples of the transition metal compounds include oxides of 3d transition elements, such as titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), and copper (Cu); metals such as ruthenium (Ru), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), platinum (Pt), gold (Au), and silver (Ag); and alloys such as platinum-palladium alloys and platinum-rhodium alloys. 2 O 3 , Co 3 O 4 ), copper oxide (CuO, Cu 2 O), silver oxide (AgO, Ag 2 O), tungsten oxide (WO, W 2 O 3 , W.O. 3 , W.O. 6) and other oxides (transition metal oxides). Among these, nickel oxide is preferred. Transition metal compound particles (transition metal compound particles) become transition metal particles, for example, by reduction. Therefore, during operation of the SOFC or SOEC, the transition metal compound particles become transition metal particles and exhibit catalytic activity and electronic conductivity. For this reason, the transition metal compound particles are preferably larger than the ceramic particles. For example, the median diameter of the transition metal compound particles may be larger than the median diameter of the ceramic particles. The median diameter of the transition metal compound particles is not limited as long as the effects of the technology disclosed herein are achieved. The median diameter is, for example, approximately 0.01 μm to 10 μm, preferably 0.05 μm to 5 μm, more preferably 0.1 μm to 2 μm, and even more preferably 0.1 μm to 1 μm. By setting the median diameter of the transition metal compound particles within the above range, the dispersibility of the transition metal compound particles in the composite particles can be improved, and ultimately, the uniformity of the components in the thermal spray coating can be improved. This can improve the conductivity of the electrodes of the SOFC or SOEC.

[0027] The mixing ratio (here, mass ratio) of ceramic particles to transition metal compound particles in a thermal spray powder can be a factor that affects the performance of an SOFC or SOEC, the uniformity of components in a thermal spray coating, and the like. From this perspective, the mass ratio of ceramic particles to transition metal compound particles (ceramic particles:transition metal compound particles) is preferably, for example, 80:20 to 20:80, or 70:30 to 30:70. In a preferred embodiment, the mass ratio (ceramic particles:transition metal compound particles) is 60:40 to 20:80. When the mass ratio of ceramic particles to transition metal compound particles (ceramic particles:transition metal compound particles) is 80:20 to 20:80, or 70:30 to 30:70, the electrical conductivity of the electrode in the formed thermal spray coating can be improved while suppressing a decrease in ionic conductivity.

[0028] The composite particles may be particles produced by mixing, for example, ceramic particles and transition metal compound particles. The composite particles are particles containing different materials, namely, ceramic particles and transition metal compound particles, but the ceramic particles and transition metal compound particles are integrated with each other and behave as a single particle. Therefore, for example, if the ceramic particles and transition metal compound particles are well dispersed in the composite particles, the uniformity of the components in the thermal spray coating can be improved.

[0029] The form of the composite particles is not limited as long as the ceramic particles and the transition metal compound particles are integrated and the effects of the technology disclosed herein can be achieved. The composite particles may be, for example, granulated particles. In this case, the granulated particles (secondary particles) can be produced, for example, by combining and mixing ceramic particles (primary particles), transition metal compound particles (primary particles), and other optional components (e.g., binder, solvent, etc.), followed by granulation.

[0030] The composite particles are preferably particles in which primary particles are in contact with each other and have a region where there is no particle interface at the contact point. The composite particles are preferably sintered particles. Sintered particles can be produced by preparing granulated particles from ceramic particles and transition metal compound particles as described above, and then sintering the granulated particles (such particles are sometimes referred to as granulated sintered particles). In the sintered particles, necks are formed at the contact points between the ceramic particles and the transition metal compound particles by sintering, and the necks grow as solid-state diffusion progresses at the necks, resulting in a bond between the ceramic particles and the transition metal compound particles, changing from point contact to surface contact. This bond is achieved, for example, by diffusion of at least a portion of the ceramic particles or the transition metal compound particles. Preferably, the ceramic particles and the transition metal compound particles, which are primary particles, are bonded with a region where there is no particle interface at the contact point. This, for example, improves the conductivity of the electrode. Granulated and sintered particles have higher strength than granulated particles before sintering. Therefore, when the composite particles are granulated and sintered particles, a desired pore size distribution can be achieved and maintained in the thermal spray powder. Therefore, by using such granulated and sintered particles, it is possible to produce a thermal spray coating with improved uniformity of components.

[0031] The median diameter (D) at an integrated value of 50% in the volume-based particle size distribution of the thermal spray powder disclosed herein based on the laser diffraction scattering method is 50 ) is not particularly limited and can be set to a size appropriate for the specifications of the device to be used. The median diameter is, for example, 1 μm or more. As the median diameter increases, for example, the handleability and flowability of the thermal spray material can be improved. From this perspective, the median diameter is appropriately 3 μm or more, preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. On the other hand, if the median diameter is too large, there is a concern that the thermal spray powder may not be sufficiently melted during thermal spraying. From this perspective, the median diameter is, for example, 300 μm or less, preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less.

[0032] When a thermal spray powder is measured by mercury intrusion porosimetry, for example, the pore diameters resulting from voids between primary particles (i.e., voids within composite particles) can be measured in the log differential pore volume distribution in the pore diameter range of 1 μm or less. On the other hand, the pore diameters resulting from voids between secondary particles can be measured in the log differential pore volume distribution in the pore diameter range of more than 1 μm. Therefore, by analyzing the log differential pore volume distribution in the pore diameter range of 1 μm or less, the bonding state (necking state) between ceramic particles and transition metal compound particles in the thermal spray powder and the degree of void formation within the composite particles can be determined.

[0033] The thermal spray powder disclosed herein preferably has a peak in the range of 0.15 μm or more and 1 μm or less in a log differential pore volume distribution for pores with a diameter of 1 μm or less obtained by mercury intrusion porosimetry. This indicates that the ceramic particles and transition metal compound particles in the composite particles are bonded in a favorable state (necking state), and that an appropriate amount of voids are formed within the composite particles. Therefore, by thermally spraying the above-described thermal spray powder, a thermal spray coating with improved component uniformity can be formed. From this perspective, the thermal spray powder preferably has a peak in the range of 0.15 μm to 0.5 μm, more preferably 0.15 μm to 0.3 μm, and even more preferably 0.15 μm to 0.23 μm in a log differential pore volume distribution for pores with a diameter of 1 μm or less obtained by mercury intrusion porosimetry. The term "peak" as used herein refers to a portion that protrudes and has a high height (a portion that occurs frequently) in the log differential pore volume distribution (curve) (see FIG. 11). In other words, a "peak" can also be expressed as a point in the log differential pore volume distribution (curve) where the sign of the slope of the tangent line changes from "+" to "-".

[0034] Mercury intrusion porosimetry is a method for determining the pore size distribution of a powder from the relationship between the pressure applied to infiltrate mercury into the pores of the powder and the amount of mercury intruded into the pores of the powder. Pore size distribution measurement based on mercury intrusion porosimetry is performed, for example, based on JIS R1655:2003 (Method for testing pore size distribution in molded fine ceramics by mercury intrusion porosimetry). The term "log differential pore volume distribution" in this specification is also referred to as log differential pore size frequency distribution, dV / d(logD) (where D represents the pore diameter and V represents the pore volume), and is a commonly used expression format for pore distribution over a relatively wide pore size range.

[0035] The log differential pore volume distribution can be created from the relationship between the amount of mercury intrusion (i.e., pore volume) and the change in unit pore size (which can be a change in unit pressure) obtained by measuring the pore size distribution using mercury intrusion porosimetry. Specifically, the log differential pore volume distribution can be created by dividing the differential pore volume (dV), which is the increase in pore volume, by the logarithmic difference value d (logD) of the pore sizes, and plotting this value against the average pore size in each pore size range (see FIG. 11 ). In this specification, the apex of the peak and other information are determined based on the pore size distribution characteristics obtained by measuring the pore size distribution using mercury intrusion porosimetry in the measurement range of 0.0036 nm to 1 μm. For example, two peaks can be obtained in the log differential pore volume distribution of the thermal spray powder (here, composite particles) disclosed herein (see FIG. 11 ). The larger of the two peaks may be a peak derived from pores between composite particles contained in the thermal spray powder. Meanwhile, the smaller of the two peaks may be a peak derived from pores in the composite particles. In this specification, the "peak" does not refer to a peak derived from gaps between composite particles, but rather to a peak derived from pores in the composite particles, and may be the highest peak in the log differential pore volume distribution (curve) for pore diameters of 1 μm or less.

[0036] After the thermal spray powder is sprayed to form a thermal spray coating, the thermal spray coating can be subjected to a reduction treatment and used as an electrode for an SOFC or SOEC. This reduction treatment reduces the transition metal compound components derived from the transition metal compound particles in the thermal spray coating to transition metal components. The transition metal components are the main component responsible for the electrical conductivity of the electrode, so they are preferably resistant to oxidation. From this perspective, the thermal spray powder disclosed herein is preferably one that has undergone a reduction treatment in a hydrogen gas atmosphere at a temperature of 800°C for two hours, and then heated in an air atmosphere from room temperature (30°C) to 1200°C at a heating rate of 10 K / min. When this reduction treatment is performed, the thermal spray powder exhibits a temperature of 470°C or higher and 570°C or lower at which a 3% weight increase occurs. Alternatively, from the perspective of achieving the effects of the technology disclosed herein, the temperature at which a 3% weight increase occurs is more preferably 470°C or higher and 520°C or lower. The "temperature at which a 3% weight increase occurs" is defined as the "3% weight change point" in the test examples described below.

[0037] Here, when the thermal spray powder is subjected to a predetermined reduction treatment, the transition metal compound particles in the thermal spray powder are reduced to form transition metal particles. In the above-mentioned thermogravimetric analysis, the reduced thermal spray powder is heated in an air atmosphere, causing the transition metal particles to oxidize. This increases the weight of the thermal spray powder. For the reduced thermal spray powder, the fact that the temperature at which the weight increases by 3% in the thermogravimetric analysis falls within the above range indicates that when the thermal spray coating obtained by thermal spraying the thermal spray powder is reduced to form an electrode, the transition metal component in the thermal spray coating is not easily oxidized. Using a thermal spray powder with this characteristic can further improve the conductivity of the electrode.

[0038] <Method for producing thermal spray powder> The thermal spray powder disclosed herein can be prepared, for example, by mixing ceramic particles and transition metal compound particles as raw material particles together with other optional components and combining them. In particular, the thermal spray powder is preferably composed of granulated and sintered particles containing a mixture of ceramic particles and transition metal compound particles. The thermal spray powder may be, for example, a thermal spray powder composed of granulated and sintered particles as secondary particles formed by mixing, granulating, and sintering raw material particles (primary particles), and the primary particles are three-dimensionally bonded together with gaps between them.

[0039] The granulation sintering method is a technique in which raw material particles are granulated into the form of secondary particles and then sintered to bond (sinter) the raw material particles together. In the granulation sintering method, granulation can be carried out by a granulation method such as dry granulation or wet granulation. Examples of granulation methods include tumbling granulation, fluidized bed granulation, stirring frame granulation, crushing granulation, melt granulation, spray granulation, and microemulsion granulation. Among these, spray granulation is a preferred granulation method.

[0040] According to the spray granulation method, a powder material can be produced, for example, by the following procedure. First, raw material particles containing ceramic particles and transition metal compound particles are prepared, and their surfaces are stabilized with a protective agent or the like, as needed. Then, for example, the stabilized raw material particles, along with optional organic materials such as binders and spacer particles, are dispersed in an appropriate solvent to prepare a spray liquid. Here, the raw material particles are dispersed in the solvent using a mixer or disperser, such as a homogenizer or a blade stirrer. Then, droplets are formed from the spray liquid using an ultrasonic atomizer or the like. The droplets are entrained in an airflow and passed through a spray drying device (spray dryer), thereby forming granulated particles. The granulated particles thus obtained are introduced into a predetermined firing furnace and fired. This produces a thermal spray material consisting of granulated and sintered particles in the form of secondary particles formed by primary particles bonded (sintered) with gaps between them. The primary particles may have substantially the same size and shape as the raw material particles, or the raw material particles may be bonded together after growing by firing.

[0041] In the above manufacturing process, when the droplets are dried, the raw material particles and the binder are in a uniformly mixed state. The raw material particles are bound by the binder to form mixed particles. When spacer particles are used, the raw material particles and the spacer particles are bound by the binder in a uniformly mixed state to form mixed particles. When these mixed particles are fired, the binder (and spacer particles) disappear (burn out) and the raw material particles are sintered. This results in the formation of secondary particles in which primary particles are bonded (sintered) with gaps between them. During sintering, depending on their composition, size, etc., some of the raw material particles may become liquid and contribute to bonding with other particles. Therefore, the median diameter of the primary particles may be larger than that of the raw material particles of the starting material. The median diameter of the secondary particles, the median diameter of the primary particles, and the size and proportion of the gaps formed between the primary particles can be designed according to the desired shape of the secondary particles.

[0042] The concentration of the raw material particles in the spray liquid is preferably, for example, 10% by mass to 80% by mass. Examples of binders to be added include polyvinyl alcohol (PVA) and carboxymethyl cellulose (CMC). Examples of the solvent that can be used include water. The amount of binder added is preferably adjusted to a ratio of 0.05% by mass to 10% by mass (e.g., 1% by mass to 5% by mass) relative to the mass of the raw material particles.

[0043] Furthermore, when sintering the granulated particles, the granulated particles are heat-treated (fired) for 1 hour to 10 hours at a predetermined temperature (approximately 600°C to 1600°C (preferably 700°C to 1500°C, more preferably 800°C to 1400°C, and even more preferably 1000°C to 1300°C)) in an air atmosphere; an inert atmosphere such as a nitrogen atmosphere or a rare gas atmosphere; or a vacuum. The predetermined temperature may be, for example, the set temperature of a firing furnace. The temperature and time for heat-treating the granulated particles can be set appropriately so as to produce a thermal spray powder having a desired pore size distribution. The firing temperature and time can also be set appropriately so as to achieve the desired median diameter for the thermal spray powder, the temperature at which a 3% weight increase occurs in thermogravimetric analysis in an air atmosphere, and the like. After the heat treatment, the resulting granulated and sintered particles may be crushed and classified, as necessary.

[0044] <Uses of Thermal Spray Powder> Thermal spray coatings can be produced on various substrates by thermal spraying the thermal spray powder disclosed herein using various thermal spraying methods. The thermal spray powder can be particularly preferably used to produce thermal spray coatings using plasma spraying methods such as atmospheric plasma spraying (APS), low pressure plasma spraying (LPS), and high pressure plasma spraying. The thermal spray powder can also be suitably used for high velocity flame spraying methods such as high velocity oxygen flame (HVOF) thermal spraying, warm spray thermal spraying, and high velocity air flame (HVAF) thermal spraying. The thermal spray powder may be supplied to a thermal spraying device in the form of a powder, or in the form of a slurry in which the powder is dispersed in an appropriate dispersion medium.

[0045] The thermal spray powder disclosed herein is used, for example, to form an electrode of a solid oxide fuel cell (SOFC) or a solid oxide electrolysis cell (SOEC). The thermal spray powder is preferably used as a material for forming an anode of an SOFC or SOEC. An SOFC can extract power (electrical energy) from chemical energy produced by, for example, a combustion reaction between hydrogen and oxygen. An SOEC can cause a chemical reaction that produces hydrogen and oxygen from water (e.g., steam) by applying electrical energy to the water.

[0046] FIG. 1 is a cross-sectional view of an SOFC 10. FIG. 1 shows a stacked structure of electrodes and solid electrolyte layers in the SOFC 10. As shown in FIG. 1, the SOFC 10 includes a fuel electrode 1, an air electrode 2, and a solid electrolyte layer 3. In the SOFC 10, the fuel electrode 1 is the anode, and the air electrode 2 is the cathode. In this specification, the term "anode" refers to an electrode from which electrons flow into an external circuit. The term "cathode" refers to an electrode into which electrons flow from an external circuit.

[0047] In this embodiment, the anode 1 is an electrode where hydrogen reacts with oxide ions. In this embodiment, the reaction between hydrogen and oxide ions produces water and releases electrons. These electrons generate electricity. As shown in FIG. 1 , the anode 1 is provided on one surface of the solid electrolyte layer 3. In this embodiment, the anode 1 is formed using the thermal spray powder disclosed herein.

[0048] The air electrode 2 is an electrode at which oxygen in the air receives electrons. In this embodiment, oxygen in the supplied air receives electrons released from the fuel electrode 1 at the air electrode, generating oxide ions. As shown in FIG. 1 , the air electrode 2 is provided on the other surface of the solid electrolyte layer 3 (in FIG. 1 , the surface opposite to the surface on which the fuel electrode 1 is formed). As the air electrode 2, various air electrodes that have been proposed so far may be used without any particular restrictions. Therefore, a description of the configuration of the air electrode 2 will be omitted here.

[0049] The solid electrolyte layer 3 here is a layer that has the function of conducting oxide ions. In this embodiment, oxide ions generated at the air electrode 2 pass through the solid electrolyte layer 3 and are supplied to the anode 1. As shown in FIG. 1 , the solid electrolyte layer 3 is sandwiched between the anode 1 and the air electrode 2. As the solid electrolyte layer 3, various solid electrolyte layers that have been proposed so far may be used without any particular restrictions. Therefore, a description of the configuration of the solid electrolyte layer 3 will be omitted here.

[0050] The method for manufacturing the SOFC 10 may include, for example, a preparation step, a lamination step, a thermal spraying step, and a firing step. The preparation step is, for example, a step of preparing a green sheet for the solid electrolyte layer 3. In this step, for example, a slurry for forming the solid electrolyte layer 3 may be applied to a carrier sheet, molded into a predetermined shape and dimensions, and dried to prepare the green sheet for the solid electrolyte layer 3. The method for applying the slurry for forming the solid electrolyte layer 3 to the carrier sheet is not particularly limited, and for example, a conventional application method such as a screen printing method or a doctor blade method may be used.

[0051] The lamination step is, for example, a step of laminating a green sheet for the air electrode 2 on one surface of a green sheet for the solid electrolyte layer 3. In this step, for example, a slurry for forming the air electrode 2 is applied to one surface of the green sheet for the solid electrolyte layer 3 (here, the surface opposite the carrier sheet), and the green sheet for the air electrode 2 is laminated on the green sheet for the solid electrolyte layer 3 by forming the slurry into a predetermined shape and size and drying it. Next, the carrier sheet may be removed from the green sheet for the solid electrolyte layer 3. The method for applying the slurry for forming the air electrode 2 to the green sheet for the solid electrolyte layer 3 is not particularly limited, and any conventional coating method such as a screen printing method or a doctor blade method may be used.

[0052] The thermal spraying step is, for example, a step of thermally spraying the thermal spray powder disclosed herein onto the other surface of the green sheet for the solid electrolyte layer 3. In this step, for example, the thermal spray powder is sprayed onto the surface of the green sheet for the solid electrolyte layer 3 opposite to the surface on which the green sheet for the air electrode 2 is laminated. This forms a thermal spray coating of the thermal spray powder disclosed herein, which serves as a precursor for the anode 1.

[0053] The firing step is, for example, a step of firing a laminate of a green sheet of the solid electrolyte layer 3 provided with a thermal spray coating and a green sheet of the air electrode 2. As a result, the anode 1, the air electrode 2, and the solid electrolyte layer 3 are mutually sintered, and a laminate structure of the anode 1, the air electrode 2, and the solid electrolyte layer 3 in the SOFC 10 is formed.

[0054] As described above, the thermal spray powder disclosed herein is a thermal spray powder for forming electrodes of an SOFC or an SOEC. The thermal spray powder preferably contains composite particles of ion-conductive ceramic particles and transition metal compound particles. The thermal spray powder preferably has a peak in the range of 0.15 μm or more and 1 μm or less in a log differential pore volume distribution of pores with a diameter of 1 μm or less obtained by mercury intrusion porosimetry.

[0055] The thermal spray powder contains ceramic particles and transition metal compound particles in the form of composite particles. Therefore, when the thermal spray powder is thermally sprayed, uneven distribution of ceramic components derived from the ceramic particles and transition metal compound components derived from the transition metal compound particles can be suppressed in the thermal spray coating. Furthermore, the thermal spray powder has a log differential pore volume distribution for pores with diameters of 1 μm or less, obtained by mercury intrusion porosimetry, which has a peak in the range of 0.15 μm to 1 μm, thereby achieving a favorable bonding state (necking state) between the ceramic particles and the transition metal compound particles. Therefore, use of the thermal spray powder disclosed herein can improve the uniformity of the components in the thermal spray coating. Furthermore, achieving a favorable bonding state within the granules is thought to create bonds between the transition metal compound particles, resulting in good contact between the transition metals after reduction treatment. Therefore, efficient electron paths (electron passages) between the transition metals can improve the conductivity of the electrode.

[0056] Furthermore, by using the thermal spray powder disclosed herein, it is expected that the uniformity of the components in the thermal spray coating can be improved, and that the three-phase interfaces between voids, the ceramic component (ceramic particles), and the transition metal compound component (transition metal compound particles) can be more uniformly dispersed. By forming an electrode (e.g., anode) for an SOFC or SOEC from such a thermal spray coating, it is expected that both the power generation efficiency in the SOFC and the hydrogen production efficiency in the SOEC will be improved.

[0057] Test examples relating to the present invention will be described below, but it is not intended that the present invention be limited to those shown in the following test examples. In the following description, the notation "%" is based on mass unless otherwise specified.

[0058] <Manufacturing Examples> (Example 1) Starting materials were prepared, including yttria-stabilized zirconia (YSZ) particles as ceramic particles, nickel oxide (NiO) particles as transition metal compound particles, polyvinyl alcohol (PVA) as a binder, and water (ion-exchanged water) as a solvent. The median diameter of the YSZ particles was 0.2 μm. The median diameter of the NiO particles was 0.7 μm. The median diameters of the YSZ particles and the NiO particles were determined by the D σ based on the volume-based particle size distribution measured using a laser diffraction particle size distribution analyzer (Malvern Panalytical, Mastersizer 3000). 50 The median diameters of the YSZ particles and NiO particles were measured under wet dispersion conditions using water, taking into account the dispersion state of each powder during particle size distribution measurement. When the total of the YSZ particles and NiO particles was taken as 100%, the proportion of the YSZ particles was 40% and the proportion of the NiO particles was 60%. When the total starting materials were taken as 100%, the proportion of the PVA was 2% and the proportion of the water was 50%.

[0059] Next, the starting materials were mixed and dispersed to prepare a slurry. This slurry was sprayed into an air stream using an atomizer granulator and dried to produce granulated particles. The granulated particles were then placed in an alumina sagger and fired in an air atmosphere to produce granulated and sintered particles. During this firing, the sagger containing the granulated particles was held at a temperature of 950°C for 4 hours. The granulated and sintered particles were then crushed and classified to obtain a thermal spray powder having a predetermined particle size distribution. This thermal spray powder was designated as the thermal spray powder of this example.

[0060] Example 2 The sintering temperature for sintering the granulated particles was set to 1040° C. Other than this, the same materials and procedures as in Example 1 were used to produce a thermal spray powder according to this example.

[0061] Example 3 The sintering temperature for sintering the granulated particles was set to 1200° C. Other than this, the same materials and procedures as in Example 1 were used to produce a thermal spray powder according to this example.

[0062] Example 4 The sintering temperature for sintering the granulated particles was set to 1300° C. Other than this, the same materials and procedures as in Example 1 were used to produce a thermal spray powder according to this example.

[0063] Comparative Example The granulated particles were fired at a firing temperature of 200° C. Other than this, the same materials and procedures as in Example 1 were used to produce a thermal spray powder according to this example.

[0064] [SEM Observation] Cross-sectional images and planar images were obtained for the thermal spray powders of Examples 1 to 4 and the thermal spray powder of the Comparative Example using a benchtop SEM (Phenom ProX, manufactured by Phenom-World). For reference, FIGS. 2 to 10 show the cross-sectional images and planar images of the thermal spray powders as follows. FIG. 2 is a planar image of the thermal spray powder of Example 3. FIG. 3 is an enlarged image of FIG. 2. FIG. 4 is a cross-sectional image of the thermal spray powder of Example 3. FIG. 5 is a planar image of the thermal spray powder of Example 4. FIG. 6 is an enlarged image of FIG. 5. FIG. 7 is a cross-sectional image of the thermal spray powder of Example 4. FIG. 8 is a planar image of the thermal spray powder of the Comparative Example. FIG. 9 is an enlarged view of FIG. 8. FIG. 10 is a cross-sectional image of the thermal spray powder of the Comparative Example.

[0065] [Measurement of Median Diameter] The volumetric particle size distribution of the thermal spray powders of Examples 1 to 4 and the thermal spray powder of the Comparative Example was measured using a laser diffraction particle size distribution analyzer (Mastersizer 3000, manufactured by Malvern Panalytical) to obtain the median diameter. The results are shown in the "Median Diameter (μm)" column in Table 1. Note that the median diameter of the thermal spray powders was measured under dry dispersion using compressed air, taking into consideration the dispersion state of each powder during particle size distribution measurement.

[0066] [Pore Volume] The pore volumes of the thermal spray powders of Examples 1 to 4 and the comparative example were measured using a mercury intrusion porosimeter (POREMASTER-60, manufactured by Quantachrome Corp.) at a mercury contact angle of 140° and a surface tension of 480 erg / cm. 2(0.480 N / m). Here, the cumulative pore volume (cc / g) of pores with a diameter of 1 μm or less (specifically, pore diameters in the range of 0.0036 μm to 0.98 μm) was measured. The measurement results are shown in the "Pore volume (cc / g)" column in Table 1.

[0067] The cumulative pore volume of pores with diameters of 1 μm or less measured as described above was defined as the "pore volume" of each thermal spray powder. Furthermore, the most frequent diameter (peak top position) of the log differential pore volume distribution was measured within the range of the "pore volume" defined above. The measurement results are shown in the "Peak Top Position (μm)" column of Table 1. Furthermore, FIGS. 11 and 12 are graphs showing the log differential pore volume distribution of each example. FIG. 12 shows an enlarged view of the range of pore diameters of 1 μm or less in the graph of FIG. 11. In FIGS. 11 and 12, the X axis represents "pore diameter (μm)" and the Y axis represents "log differential pore volume (cc / g)." The reason why the cumulative pore volume for pore diameters of 1 μm or less was defined as the “pore volume” of each thermal spray powder is that the pore volume measured in the range of pore diameters greater than 1 μm contains many voids between particles of the thermal spray powder (here, voids between secondary particles).

[0068] [Thermogravimetric Analysis] The thermal spray powders of Examples 1 to 4 and the thermal spray powder of the Comparative Example were subjected to a reduction treatment. Thermogravimetric analysis was performed on each thermal spray powder after the reduction treatment using a thermogravimetric differential thermal analyzer (STA2500 Regulus, manufactured by Netzsch). Specifically, 37.5 mg ± 2.5 mg of each reduced thermal spray powder was placed in an alumina pan, and the temperature was increased from room temperature (30°C) to 1200°C at a heating rate of 10 K / min in an air atmosphere, and the weight change of each thermal spray powder was measured. The temperature at which the weight increased by 3% was defined as the "3% weight change point." The results are shown in Table 1 as "3% weight change point (°C)." Note that in the reduction treatment, each thermal spray powder was held at 800°C for 2 hours in a reducing atmosphere (hydrogen gas atmosphere).

[0069] <Preparation of Thermal Spray Coatings> Thermal spray coatings were prepared by atmospheric pressure plasma spraying using the thermal spray powders of Examples 1 to 4 and the thermal spray powder of the Comparative Example. An aluminum substrate was used as the substrate. The thermal spraying conditions were as follows: Thermal sprayer: SG-100 (manufactured by Praxair) Powder feeder: Model 1264 (manufactured by Praxair) Plasma working gas: Argon (Ar) gas (50 psi (0.34 MPa)); and Helium (He) gas (50 psi (0.34 MPa)) Plasma output: 34 kW Plasma generation voltage: 37 V Plasma generation current: 900 A Thermal spray powder supply rate: 17.5±5 g / min Spraying distance (distance from thermal spray gun to substrate): 120 mm Spray gun traverse speed: 400 mm / s

[0070] [Evaluation of Component Uniformity in Thermal Spray Coating] The thermal spray coatings of each example prepared as described above were subjected to compositional analysis using SEM and energy dispersive X-ray spectroscopy (EDS) (Phenom ProX, manufactured by Pheno-World). Specifically, the following steps (1) to (7) were performed. (1) A composite of an aluminum substrate and a thermal spray coating was cut to obtain a thermal spray coating of the specified dimensions to obtain a test piece. (2) The test piece was immersed in an aqueous sodium hydroxide solution to dissolve the aluminum substrate and isolate the thermal spray coating. (3) The isolated thermal spray coating was subjected to a reduction treatment. The reduction treatment conditions were the same as those described in the "Thermogravimetric Analysis" section above. (4) The thermal spray coating after the reduction treatment was embedded in epoxy resin and subjected to mechanical polishing and cross-section polishing. (5) For the surface polished in (4), the cross-sectional structure of the thermal spray coating was observed and analyzed using an SEM and EDS in a field of view (approximately 27 μm × 27 μm) at a magnification of 10,000 times. Each field of view was divided into 16 sections, and the composition of the thermal spray coating in each divided field of view was quantified using a Phenom ProX (manufactured by Phenom-World). Note that a field of view was selected at any position in the cross-sectional structure of the thermal spray coating, but no field of view was selected from the surface side of the thermal spray coating or the region 20 μm from the substrate side. (6) The procedure in (5) was repeated five times, and the composition of the thermal spray coating in an 80-divided field of view was quantified. (7) The coefficient of variation (standard deviation / average value) was calculated for the quantitative values ​​of Ni atoms in the 80-divided field of view. The results are shown in the "Coefficient of Variation" column in Table 1. The coefficient of variation serves as an index for evaluating the uniformity of the components in the thermal spray coating. Here, the smaller the coefficient of variation, the better the uniformity of the components.

[0071] [Measurement of Electrical Conductivity of Thermal Spray Coating] The electrical conductivity of the thermal spray coatings of Examples 1 to 4 and the comparative example was measured using a low resistivity meter (Loresta GP MCP-T610, manufactured by Mitsubishi Analytech Co., Ltd.). Specifically, the following procedures (1) to (3) were performed. (1) The thermal spray powder of each example was sprayed onto an alumina substrate (30 mm × 30 mm × 5 mm) to produce the thermal spray coating of each example. The thermal spraying conditions were the same as those described in the above section <Preparation of Thermal Spray Coating>. (2) The thermal spray coating was subjected to a reduction treatment to obtain a measurement sample. The reduction conditions were the same as those described in the above section [Thermogravimetric Analysis]. (3) The electrical conductivity of the sample was measured by contacting a measurement probe with the sample under an environment of 21°C temperature and 37% relative humidity. The electrical conductivity was measured at three locations on each sample, and the average value was calculated. The results are shown in Table 1 as "Conductivity (×10 2 The applied properties were evaluated for the thermal spray coatings of Examples 1 to 4 and the thermal spray coating of the comparative example. Specifically, the applied properties were evaluated for the thermal spray coatings of Examples 1 to 4 where the coefficient of variation was less than 0.09 and the electrical conductivity was less than 3×10 2 S / cm or more is marked with "◎", and the coefficient of variation is 0.09 or more and the conductivity is 3×10 2 S / cm or more is marked as "Good", and the coefficient of variation is 0.09 or more and 3 x 10 2 The overall characteristics of the application were evaluated by assigning a grade of "x" to anything below S.

[0072]

[0073] As shown in Table 1, the thermal spray powders of Examples 1 to 4 have a peak in the range of 0.15 μm or more and 1 μm or less in the log differential pore volume distribution for pores with a diameter of 1 μm or less, obtained by mercury intrusion porosimetry. It was found that, when the thermal spray powders of Examples 1 to 4 are used, thermal spray coatings with a smaller coefficient of variation than the thermal spray coatings of the comparative examples (i.e., thermal spray coatings with improved compositional uniformity) can be produced, as shown in Table 1. Furthermore, the thermal spray coatings produced using the thermal spray powders of Examples 1 to 4 had higher electrical conductivity and better applicability than the thermal spray coatings of the comparative examples. These findings demonstrate that the thermal spray powders of Examples 1 to 4 are suitable as thermal spray powders for use in forming electrodes (here, fuel electrodes) for SOFCs or SOECs.

[0074] While specific examples of the technology disclosed herein have been described above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above.

[0075] The technology disclosed herein includes the inventions according to the following items 1 to 9. [Item 1] A thermal spray powder for forming an electrode of a solid oxide fuel cell or a solid oxide electrolysis cell, wherein the thermal spray powder has a peak in the range of 0.15 μm or more and 1 μm or less in a log differential pore volume distribution of pores with a diameter of 1 μm or less obtained by mercury intrusion porosimetry. [Item 2] The thermal spray powder according to item 1, comprising composite particles containing ion-conductive ceramic particles and transition metal compound particles. [Item 3] The thermal spray powder according to item 2, wherein the composite particles have a region where primary particles are in contact with each other and where there is no particle interface at the contact portion. [Item 4] The thermal spray powder according to item 2 or 3, wherein the mass ratio of the ceramic particles to the transition metal compound particles (ceramic particles:transition metal compound particles) is 60:40 to 20:80. [Item 5] A thermal spray powder having a median diameter (D 50) is 10 μm or more and 100 μm or less. [Item 6] The thermal spray powder according to any one of Items 2 to 4, wherein the ceramic particles are zirconia particles containing a rare earth metal oxide. [Item 7] The thermal spray powder according to any one of Items 2 to 4, wherein the transition metal compound particles are nickel oxide particles. [Item 8] The thermal spray powder according to any one of Items 1 to 7, wherein the thermal spray powder has been subjected to a reduction treatment in a hydrogen gas atmosphere at a treatment temperature of 800°C for two hours, and when the thermal spray powder is heated from room temperature to 1200°C at a heating rate of 10 K / min in an air atmosphere and subjected to thermogravimetric analysis, the temperature at which the weight increases by 3% is 470°C or more and 570°C or less. [Item 9] The thermal spray powder according to any one of Items 1 to 8, wherein the peak is in the range of 0.15 μm or more and 0.23 μm or less.

[0076] 1 fuel electrode 2 air electrode 3 solid electrolyte layer 10 SOFC

Claims

1. A thermal spray powder for forming electrodes of a solid oxide fuel cell or a solid oxide electrolysis cell, which has a peak in the range of 0.15 μm or more and 1 μm or less in a log differential pore volume distribution of pores with diameters of 1 μm or less obtained by mercury intrusion porosimetry.

2. The thermal spray powder according to claim 1, comprising composite particles comprising: ion-conductive ceramic particles; and transition metal compound particles.

3. The thermal spray powder according to claim 2, wherein the composite particles have a region where the primary particles are in contact with each other and where there is no particle interface.

4. The thermal spray powder according to claim 2, wherein the mass ratio of the ceramic particles to the transition metal compound particles (ceramic particles:transition metal compound particles) is 60:40 to 20:

80.

5. Median diameter based on laser diffraction scattering method (D 50 3. The thermal spray powder according to claim 1, wherein the average particle size is 10 μm or more and 100 μm or less.

6. The thermal spray powder according to claim 2, wherein the ceramic particles are zirconia particles containing a rare earth metal oxide.

7. The thermal spray powder according to claim 2, wherein the transition metal compound particles are nickel oxide particles.

8. The thermal spray powder according to claim 1 or 2, wherein when the thermal spray powder has been subjected to a reduction treatment in a hydrogen gas atmosphere at a treatment temperature of 800°C for two hours and then heated in an air atmosphere from room temperature to 1200°C at a temperature increase rate of 10 K / min and subjected to thermogravimetric analysis, the temperature at which the weight increases by 3% is 470°C or higher and 570°C or lower.

9. The thermal spray powder according to claim 1 or 2, wherein the peak is in the range of 0.15 μm or more and 0.23 μm or less.

Citation Information

Patent Citations

  • Fuel electrode for solid-oxide fuel cell

    JP2009266713A

  • Nickel-ion conductive ceramic mixed powder and composition thereof

    JP2021028417A

  • Method for producing aromatic diamine compound

    JP2023058417A

  • Powder for flame spray and flame spray material

    JP2016138309A

  • Powder for spray coating

    JP2016156046A