Bright pigment dispersion and method for forming multilayer coating film
The glitter pigment dispersion with a specific composition and application method addresses the issue of uneven luster and sagging in coating films, achieving a uniform and aesthetically pleasing metallic or pearlescent effect on industrial products.
Patent Information
- Application Number
- PCT/JP2024/012976
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Existing coating films for industrial products, such as automobile exterior panels, often fail to achieve a uniform metallic or pearlescent luster and are prone to wrinkles and sagging, especially at edges and vertical areas, due to insufficient film thickness and uneven application.
A glitter pigment dispersion containing a wetting agent, aluminum pigment, and nanocellulose, including phosphate, carboxyl, and sulfonic acid group-containing nanocellulose, is applied in a multilayer coating process, with a specific composition and heating step to ensure uniform orientation and curing, preventing wrinkles and sagging.
The solution achieves a coating film with excellent metallic or pearlescent luster, maintaining uniform thickness and preventing wrinkles and sagging at edges and vertical areas, enhancing the aesthetic appeal of industrial products.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Bright pigment dispersion and method for forming multi-layer coating film
[0001] The present invention relates to a bright pigment dispersion and a method for forming a multilayer coating film.
[0002] The main purpose of applying paint is to protect the material and to add beauty. For industrial products, beauty, especially "texture," is important in terms of enhancing the product's appeal. Consumers desire a wide variety of textures for industrial products, but in recent years, a metallic or pearlescent luster has been in demand in the fields of automobile exterior panels and automobile parts (hereinafter, metallic luster and pearlescent luster will be collectively referred to as "metallic or pearlescent luster").
[0003] Metallic or pearlescent luster is a texture characterized by a surface that does not have a grainy feel like a mirror finish, and which appears shiny when viewed near specular reflection (highlights), and dark when viewed in areas away from specular reflection where the reflected light intensity is relatively low (shades), i.e., a large difference in brightness between the highlight and shade areas.
[0004] Techniques for imparting such metallic or pearlescent luster to the surface of industrial products include metal plating and metal vapor deposition (e.g., Patent Document 1), but if a metallic or pearlescent luster could be imparted by a paint, it would be advantageous from the standpoints of simplicity and cost, and furthermore, if the paint is water-based, it would be even more advantageous from the standpoint of environmental impact.
[0005] Patent Document 2 discloses an aqueous base coating composition that contains a bright pigment obtained by pulverizing a vapor-deposited metal film to form metal flakes, and an aqueous cellulose derivative having an acid value of 20 to 150 mg KOH / g (solid content), the aqueous cellulose derivative being the main binder resin, and the bright pigment content being 20 to 70 mass % in terms of PWC.
[0006] However, the coating film formed by the paint described in Patent Document 2 has insufficient metallic or pearlescent luster.
[0007] On the other hand, Patent Document 3 discloses a glittering pigment dispersion containing water, a scaly aluminum pigment, and a cellulose-based viscosity modifier, in which the solid content is 0.1 to 10 parts by mass per 100 parts by mass of all components of the glittering pigment dispersion, the viscosity measured using a Brookfield viscometer is within the range of 400 to 10,000 mPa·sec at a rotation speed of 6 rpm, and the solid content of the scaly aluminum pigment is 30 to 200 parts by mass per 100 parts by mass of the total of all components other than the scaly aluminum pigment in the solid content.
[0008] The coating film formed using the brilliant pigment dispersion described in Patent Document 3 has excellent metallic luster, but wrinkles may occur at the edge portions where the film thickness tends to be thicker than in the general portions, and sagging may occur in vertical portions.
[0009] Japanese Patent Publication No. 63-272544 Japanese Patent Publication No. 2009-155537 International Publication No. 2017 / 175468
[0010] An object of the present invention is to provide a glitter pigment dispersion that is capable of forming a coating film that has excellent metallic or pearlescent metallic or pearlescent luster, is free from wrinkles at edge portions where the film thickness tends to be thicker than in general portions, and is free from sagging at vertical portions.
[0011] The present invention encompasses the subject matter described in the following paragraphs.
[0012] Item 1. A glittering pigment dispersion containing a wetting agent (A), a glittering pigment (B), nanocellulose (C), and water (D), wherein the glittering pigment dispersion contains 0.1 to 10 parts by mass of solids relative to a total of 100 parts by mass of all components, and the nanocellulose (C) includes at least one selected from the group consisting of phosphate group-containing nanocellulose (C1), carboxyl group-containing nanocellulose (C2), and sulfonic acid group-containing nanocellulose (C3).
[0013] Item 2. The bright pigment dispersion according to Item 1, wherein the bright pigment (B) contains an aluminum pigment.
[0014] Item 3. The glitter pigment dispersion according to Item 1 or 2, wherein the phosphate group-containing nanocellulose (C1) comprises a phosphate group-containing cellulose nanofiber (C11) and / or a phosphate group-containing cellulose nanocrystal (C12).
[0015] Item 4. The cellulose (C) comprises a carboxyl group-containing nanocellulose (C2), and the carboxyl group-containing nanocellulose (C2) comprises a carboxyl group-containing cellulose nanofiber (C21) and / or a carboxyl group-containing cellulose nanocrystal (C22). The brilliant pigment dispersion according to any one of Items 1 to 3.
[0016] Item 5. The cellulose (C) comprises a sulfonic acid group-containing nanocellulose (C3), and the sulfonic acid group-containing nanocellulose (C3) comprises a sulfonic acid group-containing cellulose nanofiber (C31) and / or a sulfonic acid group-containing cellulose nanocrystal (C32). The brilliant pigment dispersion according to any one of Items 1 to 4.
[0017] Item 6. The content ratio of the phosphate group-containing nanocellulose (C1) to at least one selected from the group consisting of carboxyl group-containing nanocellulose (C2) and sulfonic acid group-containing nanocellulose (C3) is in the range of 1 / 99 to 50 / 50 by mass of the phosphate group-containing nanocellulose (C1) to at least one selected from the group consisting of carboxyl group-containing nanocellulose (C2) and sulfonic acid group-containing nanocellulose (C3). The brilliant pigment dispersion according to any one of Items 1 to 5.
[0018] Item 7. A method for forming a multilayer coating film, comprising: step (1): applying a base coating material (X) to a substrate to form an uncured base coating film; step (2): applying the glitter pigment dispersion (Y) described in any one of items 1 to 6 to the base coating film formed in step (1) to form an uncured glitter coating film; step (3): applying a clear coating material (Z) to the glitter coating film formed in step (2) to form an uncured clear coating film; and step (4): simultaneously heating the uncured base coating film formed in step (1), the uncured glitter coating film formed in step (2), and the uncured clear coating film formed in step (3) to cure them.
[0019] According to the present invention, it is possible to provide a brilliant pigment dispersion that can form a coating film that has an excellent metallic or pearlescent luster, is free from wrinkles at edge portions where the film thickness tends to be thicker than in general portions, and is free from sagging at vertical portions.
[0020] As used herein, the singular forms (a, an, the) include both the singular and the plural unless otherwise expressly stated herein or clearly contradicted by context.
[0021] In this specification, the term "comprise" is a concept that encompasses "consist essentially of" and "consist only of."
[0022] In the numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range can be arbitrarily combined with the upper or lower limit of another numerical range. Furthermore, in the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with a value shown in an example or a value that can be unambiguously derived from an example. Furthermore, in this specification, a numerical value connected with "to" means a numerical range that includes the numbers before and after "to" as the upper and lower limits.
[0023] In this specification, the term "edge portion" refers to the edge of an object to be coated. Examples of edge portions include the rim of an object to be coated and a corner formed by the intersection of two surfaces of an object to be coated.
[0024] In this specification, the term "vertical portion" refers to a portion that extends in a substantially vertical direction when the object to be coated is placed at a fixed position.
[0025] In this specification, the "general part" refers to a part that does not come into contact with other members and occupies the majority of the area of the object to be coated or one of its members, such as the main body, excluding edge parts.
[0026] The brilliant pigment dispersion of the present invention is a brilliant pigment dispersion containing a wetting agent (A), a brilliant pigment (B), nanocellulose (C), and water (D), and contains 0.1 to 10 parts by mass of solids relative to a total of 100 parts by mass of all components of the brilliant pigment dispersion, and the nanocellulose (C) contains at least one selected from the group consisting of phosphate group-containing nanocellulose (C1), carboxyl group-containing nanocellulose (C2), and sulfonic acid group-containing nanocellulose (C3).
[0027] Wetting Agent (A) The wetting agent (A) in the glitter pigment dispersion of the present invention is not particularly limited, as long as it is a material that is effective in helping to uniformly orient the glitter pigment dispersion on the substrate when the dispersion is applied to the substrate.
[0028] Materials having such an action may be called wetting agents, leveling agents, surface conditioners, antifoaming agents, surfactants, superwetters, etc. in addition to wetting agents, and the above-mentioned wetting agents also include wetting agents, leveling agents, surface conditioners, antifoaming agents, surfactants, and superwetters.
[0029] Examples of the wetting agent (A) include silicone wetting agents, acrylic wetting agents, vinyl wetting agents, fluorine wetting agents, acetylene diol wetting agents, etc. The wetting agents can be used alone or in appropriate combination of two or more.
[0030] As the wetting agent (A), it is preferable to use an acetylene diol-based wetting agent and / or a wetting agent having an ethylene oxide chain, from the viewpoint of obtaining a glitter pigment dispersion and a multilayer coating film forming method that are excellent in water resistance and can form a metallic or pearlescent luster, and that are also highly stable.
[0031] In particular, it is preferable to use a wetting agent which is an ethylene oxide adduct of acetylene diol as the wetting agent (A).
[0032] Examples of commercially available wetting agents (A) include the Dynol series, Surfynol series, and Tego series manufactured by Evonik Industries, the BYK series manufactured by BYK-Chemie, the Granol series and Polyflow series manufactured by Kyoeisha Chemical Co., Ltd., and the Disparlon series manufactured by Kusumoto Chemical Co., Ltd.
[0033] From the viewpoint of forming a coating film that has excellent metallic or pearlescent metallic or pearlescent luster, is free from wrinkles at edge portions that tend to be thicker than general portions, and is free from sagging at vertical portions, the content of the wetting agent (A) in the brilliant pigment dispersion of the present invention is preferably 1.5 to 30 parts by mass, more preferably 2 to 25 parts by mass, and even more preferably 2.5 to 20 parts by mass in terms of solids content, based on 100 parts by mass of the solids content of the brilliant pigment dispersion.
[0034] Shiny Pigment (B) Examples of the shiny pigment (B) in the shiny pigment dispersion of the present invention include vapor-deposited metal flake pigments, aluminum flake pigments, and optical interference pigments. One or more of these pigments can be appropriately selected and used depending on the texture desired for the resulting coating film. From the viewpoint of obtaining a coating film with excellent metallic luster, vapor-deposited metal flake pigments and aluminum flake pigments are preferred. On the other hand, from the viewpoint of obtaining a coating film with excellent pearlescent luster, optical interference pigments are preferred.
[0035] Vapor-deposited metal flake pigments can be obtained by depositing a metal film on a base substrate, peeling off the base substrate, and then pulverizing the vapor-deposited metal film. Examples of the base substrate include films.
[0036] The metal material of the metal film is not particularly limited, but examples include aluminum, gold, silver, copper, brass, titanium, chromium, nickel, nickel chromium, stainless steel, etc. Among these, aluminum or chromium is particularly preferred from the viewpoints of availability and ease of handling. In this specification, a vapor-deposited metal flake pigment obtained by vapor-depositing aluminum is referred to as a "vapor-deposited aluminum flake pigment," and a vapor-deposited metal flake pigment obtained by vapor-depositing chromium is referred to as a "vapor-deposited chromium flake pigment."
[0037] The vapor-deposited aluminum flake pigment is preferably surface-treated with silica from the viewpoints of storage stability and obtaining a coating film with excellent metallic luster.
[0038] Examples of commercially available products that can be used as the vapor-deposited aluminum flake pigment include the "METALURE" series (trade name, manufactured by Ecart), the "Hydroshine WS" series (trade name, manufactured by Ecart), the "Decomet" series (trade name, manufactured by Schlenk), and the "Metasheen" series (trade name, manufactured by BASF).
[0039] Examples of commercially available vapor-deposited chrome flake pigments that can be used include the "Metalure Liquid Black" series (trade name, manufactured by Ecart).
[0040] The average thickness of the vapor-deposited metal flake pigment is preferably 0.01 to 1.0 μm, more preferably 0.015 to 0.1 μm.
[0041] The average particle size (D50) of the vapor-deposited metal flake pigment is preferably 1 to 50 μm, more preferably 5 to 20 μm.
[0042] The average particle size referred to here means the median diameter of the volume-based particle size distribution measured by a laser diffraction scattering method using a Microtrac particle size distribution analyzer MT3300 (trade name, manufactured by Nikkiso Co., Ltd.) The thickness is defined as the average value of 100 or more measurements obtained by observing the cross section of a coating film containing the effective pigment under a microscope and measuring the thickness using image processing software.
[0043] When the average particle size is equal to or less than the upper limit, no grainy feeling occurs in the multi-layer coating film, and when it is equal to or greater than the lower limit, a large change in brightness from highlight to shade is maintained.
[0044] Aluminum flake pigments are generally produced by pulverizing and grinding aluminum in a ball mill or attritor mill in the presence of a grinding medium using a grinding aid. Grinding aids used in the production process of aluminum flake pigments include higher fatty acids such as oleic acid, stearic acid, isostearic acid, lauric acid, palmitic acid, and myristic acid, as well as aliphatic amines, aliphatic amides, and aliphatic alcohols. The grinding medium used is an aliphatic hydrocarbon such as mineral spirits.
[0045] The above-mentioned aluminum flake pigments can be broadly classified into leafing and non-leafing types depending on the type of grinding aid. In the bright pigment dispersion of the present invention, it is preferable to use non-leafing aluminum pigments from the viewpoint of forming a metallic coating film that has excellent water resistance, high gloss in highlights, and a small particle appearance and is dense. As non-leafing aluminum pigments, those with no particular surface treatment can be used, but those with a resin-coated surface, those with a silica treatment, and those with a surface treatment using phosphoric acid, molybdic acid, or a silane coupling agent can also be used. Those that have undergone one of the above various surface treatments can be used, or those that have undergone multiple types of treatments can also be used.
[0046] Furthermore, the aluminum flake pigment may be a colored aluminum pigment in which the surface of the aluminum flake pigment is coated with a colored pigment and then further coated with a resin, or in which the surface of the aluminum flake pigment is coated with a metal oxide such as iron oxide.
[0047] The aluminum flake pigment preferably has an average particle size in the range of 1 to 100 μm, more preferably in the range of 5 to 50 μm, and particularly preferably in the range of 7 to 30 μm, from the viewpoint of forming a metallic coating film with high gloss in highlights and a fine texture with a small graininess. The thickness is preferably in the range of 0.01 to 1.0 μm, and particularly preferably in the range of 0.02 to 0.5 μm.
[0048] The bright pigment (B) in the bright pigment dispersion of the present invention can also be a combination of the vapor-deposited metal flake pigment and the aluminum flake pigment. In such cases, the blending ratio of the vapor-deposited metal flake pigment to the aluminum flake pigment is 9 / 1 to 1 / 9, preferably 2 / 8 to 8 / 2, by mass.
[0049] As the optical interference pigment, it is preferable to use an optical interference pigment in which a transparent or translucent substrate is coated with titanium oxide. In this specification, a transparent substrate refers to a substrate that transmits at least 90% of visible light. A translucent substrate refers to a substrate that transmits at least 10% to less than 90% of visible light.
[0050] Optical interference pigments are bright pigments in which the surface of a transparent or translucent, scaly substrate, such as mica, artificial mica, glass, iron oxide, aluminum oxide, or various metal oxides, is coated with a metal oxide having a refractive index different from that of the substrate. Examples of the metal oxide include titanium oxide and iron oxide, and optical interference pigments can exhibit a variety of different interference colors depending on the thickness of the metal oxide.
[0051] Specific examples of the light interference pigment include metal oxide-coated mica pigments, metal oxide-coated alumina flake pigments, metal oxide-coated glass flake pigments, and metal oxide-coated silica flake pigments, as shown below.
[0052] Metal oxide-coated mica pigments are pigments that use natural or artificial mica as a base material and have the surface of the base material coated with metal oxide. Natural mica is a scaly base material made by crushing mica ore. Artificial mica is a scaly base material made by crushing mica ore. 2 , MgO, Al 2 O 3 , K. 2 SiF 6 , Na 2 SiF 6 It is synthesized by heating industrial raw materials such as mica, melting them at a high temperature of about 1500°C, and then cooling and crystallizing them. Compared to natural mica, it has fewer impurities and is uniform in size and thickness. 3 AlSi 3O 10 F 2 ), potassium tetrasilicic mica (KMg 2.5 AlSi 4 O 10 F 2 ), sodium tetrasilicic mica (NaMg 2.5 AlSi 4 O 10 F 2 ), Na taeniolite (NaMg 2 LiSi 4 O 10 F 2 ), LiNa taeniolite (LiMg 2 LiSi 4 O 10 F 2 ) are known.
[0053] Metal oxide-coated alumina flake pigments are pigments that use alumina flakes as a base material and the surface of the base material is coated with a metal oxide. Alumina flakes refer to scaly (thin) aluminum oxide, which is colorless and transparent. The alumina flakes do not necessarily have to be composed solely of aluminum oxide, but may also contain oxides of other metals.
[0054] Metal oxide-coated glass flake pigments are pigments whose base material is scaly glass and whose surface is coated with metal oxide. The smooth surface of the base material of the metal oxide-coated glass flake pigments produces strong light reflection.
[0055] The metal oxide-coated silica flake pigment is a pigment in which scaly silica, which is a base material having a smooth surface and a uniform thickness, is coated with a metal oxide.
[0056] The above-mentioned light interference pigment may be subjected to a surface treatment to improve dispersibility, water resistance, chemical resistance, weather resistance, and the like.
[0057] From the viewpoint of obtaining a coating film with excellent pearlescent luster, it is preferable to use the above-mentioned light interference pigment having an average particle size in the range of 5 to 30 μm, particularly 7 to 20 μm.
[0058] The particle size referred to here means the median diameter of the volume-based particle size distribution measured by a laser diffraction scattering method using a Microtrac particle size distribution measuring device MT3300 (trade name, manufactured by Nikkiso Co., Ltd.).
[0059] In order to obtain a coating film with excellent pearlescent luster, it is preferable to use the above-mentioned light interference pigment having a thickness in the range of 0.05 to 1.0 μm, particularly 0.1 to 0.8 μm.
[0060] The luster pigment (B) in the luster pigment dispersion preferably has an average particle size in the range of 1 to 100 μm, more preferably in the range of 5 to 50 μm, and particularly preferably in the range of 7 to 30 μm, from the viewpoint of forming a coating film having a high gloss in highlights, a fine metallic or pearlescent luster with a small particle feel. The thickness is preferably in the range of 0.01 to 1.0 μm, and particularly preferably in the range of 0.02 to 0.5 μm.
[0061] The content of the brilliant pigment (B) in the brilliant pigment dispersion of the present invention is preferably 5 to 80 parts by mass, more preferably 10 to 75 parts by mass, and even more preferably 15 to 70 parts by mass, based on 100 parts by mass of the solid content in the brilliant pigment dispersion, from the viewpoint of forming a coating film that is excellent in metallic or pearlescent metallic or pearlescent luster and that does not cause wrinkles at edge portions where the film thickness tends to be thicker than in general portions, and that does not cause sagging at vertical portions.
[0062] Nanocellulose (C) Nanocellulose (C) includes at least one selected from the group consisting of phosphate group-containing nanocellulose (C1), carboxyl group-containing nanocellulose (C2), and sulfonic acid group-containing nanocellulose (C3).
[0063] Nanocellulose is a term used to refer to nanostructured cellulose, which is made by finely disintegrating cellulose, the main component of plant cell walls, down to the nano level. Specific examples include cellulose nanofibers, cellulose nanocrystals, cellulose nanowhiskers, and bacterial nanocellulose produced by bacteria.
[0064] In this paper, cellulose nanofibers are defined as compounds obtained by subjecting cellulose fibers to mechanical defibration and other processes, and cellulose nanocrystals are defined as compounds obtained by subjecting cellulose fibers to chemical processes such as acid hydrolysis.
[0065] The nanocellulose can be obtained by defibrating a cellulose raw material. Examples of cellulose raw materials include plant materials (e.g., wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, and waste paper), animal materials (e.g., ascidians), algae, microorganisms (e.g., acetic acid bacteria (Acetobacter)), and microbial products. Any of these can be used. Cellulose raw materials derived from plants or microorganisms are preferred, and plant-derived cellulose raw materials are more preferred.
[0066] Phosphate group-containing nanocellulose (C1) The phosphate group-containing nanocellulose (C1) has excellent metallic or pearlescent metallic or pearlescent luster, and from the viewpoint of forming a coating film that does not wrinkle at the edge portions, which tend to be thicker than the general portions, and does not sag at vertical portions, it preferably contains phosphate group-containing cellulose nanofibers (C11) and / or phosphate group-containing cellulose nanocrystals (C12), and more preferably contains phosphate group-containing cellulose nanofibers (C11).
[0067] The phosphate group-containing cellulose nanofibers (C11) have excellent metallic or pearlescent luster and are capable of forming a coating film that is free of wrinkles at edge portions, which tend to be thicker than general portions, and free of sagging at vertical portions. From this viewpoint, the number-average fiber diameter is preferably within the range of 2 to 500 nm, more preferably 2 to 250 nm, and even more preferably 2 to 150 nm. The number-average fiber length is preferably within the range of 0.1 to 20 μm, more preferably 0.1 to 15 μm, and even more preferably 0.1 to 10 μm. The aspect ratio, which is the value obtained by dividing the number-average fiber length by the number-average fiber diameter, is preferably within the range of 50 to 10,000, more preferably 50 to 5,000, and even more preferably 50 to 1,000.
[0068] The number average fiber diameter and the number average fiber length are measured and calculated from an image obtained by, for example, diluting a sample of phosphate group-containing cellulose nanofibers (C11) with water, dispersing the resulting sample, and casting the resulting sample on a carbon film-coated grid that has been hydrophilized, and observing the resulting sample with a transmission electron microscope (TEM).
[0069] The method for producing the phosphate group-containing cellulose nanofibers (C11) is not particularly limited, and may include, for example, a step of introducing phosphate groups into a cellulose raw material and a defibration treatment step. The phosphate group introduction step is a step of reacting a compound having a phosphate group and / or a salt thereof with the cellulose raw material in the presence of urea and / or a derivative thereof. This introduces phosphate groups into the hydroxy groups of the cellulose raw material. The defibration treatment step is a step of pulverizing the fiber raw material into which phosphate groups have been introduced (hereinafter referred to as "phosphate group-introduced cellulose fiber") to the nano-level. The above treatment steps are performed in the order of the phosphate group introduction step and the defibration treatment step. The phosphate group introduction step includes a step of introducing phosphate groups into cellulose, and may optionally include an alkali treatment step, a step of washing away excess reagents, a heat treatment step of cleaving condensed phosphate groups, etc.
[0070] The compound having a phosphate group and / or its salt is a compound containing a phosphorus atom and capable of forming an ester bond with cellulose. Examples of the compound containing a phosphorus atom and capable of forming an ester bond with a hydroxyl group of cellulose include, but are not limited to, at least one selected from phosphoric acid, a salt of phosphoric acid, a dehydration condensation product of phosphoric acid, a salt of a dehydration condensation product of phosphoric acid, diphosphorus pentoxide, and phosphorus oxychloride, or a mixture thereof. All of these compounds may contain water in the form of hydrated water or the like, or may be an anhydrous compound substantially free of water.
[0071] The salts of the phosphate salts and the dehydrated condensates of phosphoric acid may be selected from lithium salts, sodium salts, potassium salts, ammonium salts, organic ammonium salts, and organic phosphonium salts of the phosphoric acid salts and the dehydrated condensates of phosphoric acid, as well as salts with any compound exhibiting basicity, but are not particularly limited thereto.
[0072] The degree of neutralization of the phosphate salt and the salt of the dehydrated condensate of phosphoric acid is not particularly limited.
[0073] Among these, phosphoric acid, sodium salt of phosphoric acid, potassium salt of phosphoric acid, or ammonium salt of phosphoric acid is preferred from the viewpoints of high efficiency of introduction of phosphate groups, easier improvement of defibration efficiency in the defibration step described below, low cost, and ease of industrial application. Phosphoric acid, ammonium dihydrogen phosphate, or sodium dihydrogen phosphate is more preferred.
[0074] Examples of the urea and / or its derivatives include, but are not limited to, urea, thiourea, biuret, phenylurea, benzylurea, dimethylurea, diethylurea, tetramethylurea, benzoleinurea, hydantoin, etc. Among these, urea is preferred because it is low cost, easy to handle, and easily forms hydrogen bonds with fiber raw materials having hydroxyl groups.
[0075] In addition to the above compounds, amides or amines may be included in the reaction system. Examples of amides include formamide, dimethylformamide, acetamide, and dimethylacetamide. Examples of amines include methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine. Among these, triethylamine is known to function as a particularly good reaction catalyst.
[0076] The amount of phosphate groups introduced into the cellulose raw material is not particularly limited, but is preferably 0.10 to 3.65 mmol / g, more preferably 0.20 to 3.00 mmol / g, and even more preferably 0.50 to 2.00 mmol / g per gram (mass) of fine cellulose fiber.
[0077] The content of the phosphate group-containing nanocellulose (C1) in the brilliant pigment dispersion of the present invention is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 7.5 parts by mass, and even more preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the solids in the brilliant pigment dispersion, from the viewpoint of forming a coating film that has excellent metallic or pearlescent metallic or pearlescent luster, does not cause wrinkles at edge portions that tend to be thicker than general portions, and does not cause sagging in vertical portions.
[0078] Carboxyl group-containing nanocellulose (C2) The carboxyl group-containing nanocellulose (C2) has excellent metallic or pearlescent metallic or pearlescent luster, and from the viewpoint of forming a coating film that does not wrinkle at the edge portions, which tend to be thicker than the general portions, and does not sag at vertical portions, it preferably contains carboxyl group-containing cellulose nanofibers (C21) and / or carboxyl group-containing cellulose nanocrystals (C22), and more preferably contains carboxyl group-containing cellulose nanofibers (C21).
[0079] The carboxyl group-containing cellulose nanofiber (C21) preferably has a carboxyl group amount of 0.80 to 1.10 mmol / g, more preferably 0.85 to 1.10 mmol / g, and even more preferably 0.90 to 1.10 mmol / g, relative to the bone dry mass of the cellulose nanofiber.
[0080] Carboxyl group-containing cellulose nanofibers (C21) can be obtained by defibrating oxidized cellulose obtained by introducing carboxyl groups into a cellulose raw material using a known method. One method for introducing carboxyl groups into a cellulose raw material is to oxidize the cellulose raw material in water using an oxidizing agent in the presence of an N-oxyl compound, a bromide, an iodide, or a mixture thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the pyranose ring on the cellulose surface. As a result, carboxyl groups (—COOH) or carboxylate groups (—COO—) can be introduced onto the surface.
[0081] An N-oxyl compound refers to a compound capable of generating a nitroxy radical. Any compound can be used as the N-oxyl compound as long as it promotes the target oxidation reaction. Examples include 2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO).
[0082] The amount of the N-oxyl compound is not particularly limited, as long as it is a catalytic amount capable of oxidizing the raw material cellulose. The amount is preferably 0.01 mmol to 10 mmol, more preferably 0.01 mmol to 1 mmol, and even more preferably 0.05 mmol to 0.5 mmol, per 1 g of bone-dry cellulose. The concentration of the N-oxyl compound in the reaction system is preferably about 0.1 mmol / L to 4 mmol / L.
[0083] Bromides are compounds containing bromine, including alkali metal bromides that can dissociate and ionize in water, while iodides are compounds containing iodine, including alkali metal iodides.
[0084] The amount of bromide or iodide can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is preferably 0.1 mmol to 100 mmol, more preferably 0.1 mmol to 10 mmol, and even more preferably 0.5 mmol to 5 mmol, per 1 g of bone-dry cellulose.
[0085] Any known oxidizing agent can be used, such as halogen, hypohalous acid, halous acid, perhalogen acid or salts thereof, halogen oxide, peroxide, etc. Among these, sodium hypochlorite is preferred because it is inexpensive and has a low environmental impact.
[0086] The amount of the oxidizing agent is preferably 0.5 mmol to 500 mmol, more preferably 0.5 mmol to 50 mmol, and even more preferably 1 mmol to 25 mmol, per 1 g of bone-dry cellulose. For example, the amount of the oxidizing agent is preferably 1 mol to 40 mol per 1 mol of the N-oxyl compound.
[0087] The cellulose oxidation process can proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature is preferably 4°C to 40°C, and may be room temperature, approximately 15°C to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose, causing the pH of the reaction solution to decrease. To efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution during the reaction to maintain the pH of the reaction solution at 8 to 12, preferably about 9 to 12, and more preferably about 10 to 12. Water is preferred as the reaction medium because of its ease of handling and the fact that side reactions are unlikely to occur.
[0088] The reaction time for the oxidation reaction can be appropriately set depending on the degree of progress of the oxidation, and is usually 0.5 to 6 hours.
[0089] Alternatively, the oxidation reaction may be carried out in two stages. For example, the carboxylated cellulose obtained by filtering after the completion of the first stage reaction can be oxidized again under the same or different reaction conditions, thereby enabling efficient oxidation without reaction inhibition by sodium chloride produced as a by-product in the first stage reaction.
[0090] Another example is a method of oxidizing cellulose raw materials by contacting them with an ozone-containing gas, which oxidizes at least the hydroxyl groups at positions 2 and 6 of the pyranose ring and decomposes the cellulose chain.
[0091] The ozone concentration in the ozone-containing gas is 50 g / m 3 ~250g / m 3 It is preferable that the thickness is 50 g / m 3 ~220g / m 3 The amount of ozone added to the cellulose raw material is preferably 0.1 parts by mass to 30 parts by mass, and more preferably 5 parts by mass to 30 parts by mass, when the solid content of the cellulose raw material is taken as 100 parts by mass.
[0092] The ozone treatment temperature is preferably 0° C. to 50° C., more preferably 20° C. to 50° C. The ozone treatment time is not particularly limited, but is about 1 minute to 360 minutes, preferably about 30 minutes to 360 minutes.
[0093] After the ozone treatment, a further oxidation treatment may be carried out using an oxidizing agent. The oxidizing agent used in the further oxidation treatment is not particularly limited, but examples include chlorine compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, the further oxidation treatment can be carried out by dissolving these oxidizing agents in water or a polar organic solvent such as alcohol to prepare an oxidizing agent solution, and then immersing the cellulose raw material in the solution.
[0094] The amount of carboxyl groups, which indicates the degree of modification of oxidized cellulose, can be adjusted by controlling reaction conditions such as the amount of oxidizing agent added and reaction time, as described above. The amount of carboxyl groups is preferably 0.80 to 1.10 mmol / g, more preferably 0.85 to 1.10 mmol / g, and even more preferably 0.90 to 1.10 mmol / g, relative to the bone dry mass of oxidized cellulose. In this specification, when indicating the degree of modification, the amount of carboxyl groups refers to the total amount of carboxyl groups (-COOH) and carboxylate groups (-COO-).
[0095] The amount of carboxyl groups and the like can be calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of a weak acid, where the change in electrical conductivity is gradual, by preparing 60 ml of a 0.5% by mass slurry of oxidized pulp, adding 0.1 M aqueous hydrochloric acid to adjust the pH to 2.5, and then adding 0.05 N aqueous sodium hydroxide dropwise and measuring the electrical conductivity until the pH reaches 11.
[0096] Amount of carboxyl groups [mmol / g pulp] = a [ml] × 0.05 / mass of oxidized pulp [g].
[0097] In principle, the degree of modification does not change during the defibration treatment described below, and therefore the degree of modification of oxidized cellulose can be considered to be the degree of modification of the defibrated cellulose nanofibers. (Defibrillation) The device used for defibration is not particularly limited, but examples include high-speed rotation, colloid mill, high-pressure, roll mill, and ultrasonic types of devices. High-pressure or ultra-high-pressure homogenizers are preferred, and wet high-pressure or ultra-high-pressure homogenizers are more preferred. The device is preferably capable of applying strong shear forces to the cellulose raw material or oxidized cellulose (usually a dispersion). The pressure that the device can apply is preferably 50 MPa or more, more preferably 100 MPa or more, and even more preferably 140 MPa or more. The device is preferably a wet high-pressure or ultra-high-pressure homogenizer that can apply the above pressure and strong shear forces to the cellulose raw material or oxidized cellulose (usually a dispersion). This allows for efficient defibration. The number of treatments (passes) through the defibration device may be one or two or more, with two or more being preferred.
[0098] In the dispersion treatment, oxidized cellulose is usually dispersed in a solvent. The solvent is not particularly limited as long as it can disperse oxidized cellulose, but examples include water, organic solvents (e.g., hydrophilic organic solvents such as methanol), and mixtures thereof. Because the cellulose raw material is hydrophilic, water is preferably used as the solvent.
[0099] The solids concentration of oxidized cellulose in the dispersion is usually 0.1% by mass or more, preferably 0.2% by mass or more, and more preferably 0.3% by mass or more. This ensures an appropriate amount of liquid relative to the amount of cellulose fiber raw material, which is efficient. The upper limit is usually 10% by mass or less, and preferably 6% by mass or less. This allows fluidity to be maintained.
[0100] The order of the defibration treatment and dispersion treatment is not particularly limited, and either may be performed first, or they may be performed simultaneously, but it is preferable to perform the defibration treatment after the dispersion treatment. Each combination of treatments needs to be performed at least once, and may be repeated two or more times.
[0101] Prior to the defibration treatment or dispersion treatment, a pretreatment may be carried out as necessary. The pretreatment may be carried out using a mixing, stirring, emulsifying, or dispersing device such as a high-speed shear mixer.
[0102] The average fiber diameter of the carboxyl group-containing cellulose nanofibers (C21) is preferably 3 nm or more and 500 nm or less, more preferably 3 nm or more and 50 nm or less, and even more preferably 3 nm or more and 20 nm or less. The average fiber length is preferably 60 nm or more and less than 2500 nm, more preferably 75 nm or more and less than 2250 nm, and even more preferably 90 nm or more and less than 900 nm. The average fiber diameter and average fiber length of the carboxyl group-containing cellulose nanofibers (C21) can be measured, for example, by preparing a 0.001 mass% aqueous dispersion of the carboxyl group-containing cellulose nanofibers (C21), spreading this diluted dispersion thinly on a mica sample stage, and heating and drying it at 50°C to prepare an observation sample. The cross-sectional height of the shape image observed with an atomic force microscope (AFM) can be measured to calculate the number average fiber diameter or number average fiber length.
[0103] The average aspect ratio of the carboxyl group-containing cellulose nanofibers (C21) is preferably 20 or more and less than 50, more preferably in the range of 25 to 45, and even more preferably in the range of 30 to 45.
[0104] The content of the carboxyl group-containing nanocellulose (C2) in the brilliant pigment dispersion of the present invention is preferably 1 to 30 parts by mass, more preferably 2 to 25 parts by mass, and even more preferably 3 to 20 parts by mass, based on 100 parts by mass of the solids in the brilliant pigment dispersion, from the viewpoint of forming a coating film that has excellent metallic or pearlescent metallic or pearlescent luster, does not cause wrinkles at edge portions that tend to be thicker than general portions, and does not cause sagging in vertical portions.
[0105] Further, the content ratio of the phosphate group-containing nanocellulose (C1) and the carboxyl group-containing nanocellulose (C2) in the brilliant pigment dispersion of the present invention is excellent in metallic or pearlescent metallic or pearlescent luster, and from the viewpoint of forming a coating film that does not wrinkle at the edge portion where the film thickness tends to be thicker than in the general portion, and does not cause sagging in the vertical portion, the mass ratio ((C1) / (C2)) of the phosphate group-containing nanocellulose (C1) to the carboxyl group-containing nanocellulose (C2) is preferably in the range of 1 / 99 to 50 / 50, more preferably in the range of 3 / 97 to 45 / 55, and even more preferably in the range of 5 / 95 to 40 / 60.
[0106] Sulfonic acid group-containing nanocellulose (C3) The sulfonic acid group-containing nanocellulose (C3) has excellent metallic or pearlescent metallic or pearlescent luster, and from the viewpoint of forming a coating film that does not wrinkle at the edge portions, which tend to be thicker than the general portions, and does not sag at vertical portions, it preferably contains sulfonic acid group-containing cellulose nanofibers (C31) and / or sulfonic acid group-containing cellulose nanocrystals (C32), and more preferably contains sulfonic acid group-containing cellulose nanocrystals (C32).
[0107] The sulfonic acid group-containing cellulose nanocrystals (C32) can be produced by known methods, for example, by a chemical treatment step in which a fiber raw material containing cellulose is chemically treated to introduce sulfo groups, and a step in which the amorphous portion is hydrolyzed with concentrated sulfuric acid or the like.
[0108] The number-average fiber diameter of the sulfonic acid group-containing cellulose nanocrystal (C32) is preferably within the range of 1 to 50 nm, more preferably within the range of 1 to 30 nm, particularly preferably within the range of 1 to 15 nm, and even particularly preferably within the range of 1 to 5 nm, from the viewpoint of forming a coating film that has excellent metallic or pearlescent metallic or pearlescent luster and is free from wrinkles at edge portions, which tend to be thicker than general portions, and free from sagging at vertical portions.
[0109] Furthermore, from the viewpoint of forming a coating film that has excellent metallic or pearlescent metallic or pearlescent luster, is free from wrinkles at edge portions where the film thickness tends to be thicker than in general portions, and is free from sagging at vertical portions, the number-average fiber length of the sulfonic acid group-containing cellulose nanocrystal (C32) is preferably in the range of 10 to 500 nm, more preferably in the range of 10 to 300 nm, particularly preferably in the range of 20 to 250 nm, and even particularly preferably in the range of 30 to 150 nm.
[0110] The number-average fiber diameter and the number-average fiber length are measured and calculated from an image obtained by, for example, diluting sulfonic acid group-containing cellulose nanocrystals (C32) with water, dispersing the diluted sample, and casting the resultant onto a hydrophilized carbon film-coated grid, and observing the resultant grid with a transmission electron microscope (TEM).
[0111] The ratio of the number average fiber length to the number average fiber diameter (number average fiber length / number average fiber diameter) of the sulfonic acid group-containing cellulose nanocrystals (C32) is preferably 3 or more and less than 50, more preferably 5 or more and less than 50, and even more preferably 10 or more and less than 50, from the viewpoint of forming a coating film that has excellent metallic or pearlescent metallic or pearlescent luster and is free from wrinkles at edge portions where the film thickness tends to be thicker than in general portions and free from sagging at vertical portions.
[0112] The content of the sulfonic acid group-containing nanocellulose (C3) in the brilliant pigment dispersion of the present invention is preferably 1 to 30 parts by mass, more preferably 2 to 25 parts by mass, and even more preferably 3 to 20 parts by mass, based on 100 parts by mass of the solids in the brilliant pigment dispersion, from the viewpoint of forming a coating film that has excellent metallic or pearlescent metallic or pearlescent luster, does not cause wrinkles at edge portions that tend to be thicker than general portions, and does not cause sagging in vertical portions.
[0113] Further, the content ratio of the phosphate group-containing nanocellulose (C1) and the sulfonic acid group-containing nanocellulose (C3) in the brilliant pigment dispersion of the present invention is excellent in metallic or pearlescent metallic or pearlescent luster, and from the viewpoint of forming a coating film that does not wrinkle at the edge portion where the film thickness tends to be thicker than the general portion, and does not cause sagging in the vertical portion, the mass ratio of the phosphate group-containing nanocellulose (C1) to the sulfonic acid group-containing nanocellulose (C3) ((C1) / (C3)) is preferably in the range of 1 / 99 to 50 / 50, more preferably in the range of 3 / 97 to 45 / 55, and even more preferably in the range of 5 / 95 to 40 / 60.
[0114] Further, the content ratio of at least one selected from the group consisting of phosphate group-containing nanocellulose (C1), carboxyl group-containing nanocellulose (C2) and sulfonic acid group-containing nanocellulose (C3) in the brilliant pigment dispersion of the present invention is excellent in metallic or pearlescent metallic or pearlescent luster, and at the edge portion where the film thickness tends to be thicker than the general portion, wrinkles do not occur, and from the viewpoint of forming a coating film that does not cause sagging in the vertical portion, the mass ratio of phosphate group-containing nanocellulose (C1) to at least one selected from the group consisting of carboxyl group-containing nanocellulose (C2) and sulfonic acid group-containing nanocellulose (C3) ((C1) / [(C2) and (C3)]), is preferably in the range of 1 / 99 to 50 / 50, more preferably in the range of 3 / 97 to 45 / 55, and even more preferably in the range of 5 / 95 to 40 / 60.
[0115] The content of nanocellulose (C) in the brilliant pigment dispersion of the present invention is preferably 1 to 30 parts by mass, more preferably 2 to 25 parts by mass, and even more preferably 3 to 20 parts by mass, based on 100 parts by mass of the solids in the brilliant pigment dispersion, from the viewpoint of forming a coating film that has excellent metallic or pearlescent metallic or pearlescent luster, does not develop wrinkles at edge portions where the film thickness tends to be thicker than in general portions, and does not develop sagging at vertical portions.
[0116] Brilliant pigment dispersion The brilliant pigment dispersion of the present invention is a brilliant pigment dispersion containing a wetting agent (A), a brilliant pigment (B), nanocellulose (C), and water (D), and contains 0.1 to 10 parts by mass of solids relative to a total of 100 parts by mass of all components of the brilliant pigment dispersion, and the nanocellulose (C) contains at least one selected from the group consisting of phosphate group-containing nanocellulose (C1), carboxyl group-containing nanocellulose (C2), and sulfonic acid group-containing nanocellulose (C3).
[0117] The content of water (D) in the brilliant pigment dispersion of the present invention is preferably within a range of 50 to 95 parts by mass, more preferably within a range of 60 to 90 parts by mass, and even more preferably within a range of 70 to 90 parts by mass, relative to 100 parts by mass of the total of all components of the brilliant pigment dispersion, from the viewpoint of forming a coating film that is excellent in metallic or pearlescent metallic or pearlescent luster and that is free of wrinkles at edge portions where the film thickness tends to be thicker than in general portions and free of sagging at vertical portions.
[0118] Furthermore, from the viewpoint of forming a coating film that has excellent metallic or pearlescent metallic or pearlescent luster, does not develop wrinkles at edge portions that tend to be thicker than general portions, and does not develop sagging at vertical portions, the solid content is preferably in the range of 0.5 to 8 parts by mass, and more preferably in the range of 1.5 to 6 parts by mass, relative to 100 parts by mass of the total of all components of the brilliant pigment dispersion.
[0119] The bright pigment dispersion of the present invention may also contain a resin water dispersion from the viewpoint of water resistance of the resulting coating film.
[0120] Resin Water Dispersion The resin water dispersion is a dispersion in which a resin is dispersed in an aqueous solvent, and may contain, for example, at least one selected from the group consisting of a urethane resin water dispersion, an acrylic resin water dispersion, a polyester resin water dispersion, an olefin resin water dispersion, and a composite of these resins. The water dispersion may be modified.
[0121] Of these, from the viewpoint of the water resistance of the resulting coating film, preferred are urethane resin water dispersions and acrylic resin water dispersions, more preferred are hydroxyl group-containing urethane resin water dispersions and hydroxyl group-containing acrylic resin water dispersions, and especially preferred are hydroxyl group-containing acrylic resin water dispersions.
[0122] The hydroxyl group-containing acrylic resin aqueous dispersion is particularly preferably of the core-shell type.
[0123] When the brilliant pigment dispersion of the present invention contains a resin water dispersion, the content thereof is preferably in the range of 1 to 60 parts by mass, and more preferably in the range of 5 to 40 parts by mass, based on 100 parts by mass of the solid content in the brilliant pigment dispersion.
[0124] Other Components The glittering pigment dispersion may further contain, as necessary, an organic solvent, a pigment other than the glittering pigment (B), a viscosity modifier other than the nanocellulose (C), a binder resin other than the resin aqueous dispersion, a crosslinkable component, a pigment dispersant, an anti-settling agent, an ultraviolet absorber, a light stabilizer, and the like.
[0125] Examples of pigments other than the above-mentioned luster pigment (B) include coloring pigments and extender pigments.
[0126] Examples of the color pigment include titanium oxide, zinc oxide, carbon black, molybdenum red, Prussian blue, cobalt blue, azo pigments, phthalocyanine pigments, quinacridone pigments, isoindoline pigments, threne pigments, perylene pigments, dioxazine pigments, and diketopyrrolopyrrole pigments. Of these, carbon black is preferably used.
[0127] When the brilliant pigment dispersion of the present invention contains a color pigment, the content of the color pigment is preferably in the range of 0.1 to 10 parts by mass, and more preferably in the range of 0.5 to 5 parts by mass, based on 100 parts by mass of the solid content in the brilliant pigment dispersion.
[0128] Examples of the extender pigment include clay, kaolin, barium sulfate, barium carbonate, calcium carbonate, talc, silica, and alumina white.
[0129] When the brilliant pigment dispersion of the present invention contains a body pigment, the content of the extender pigment is preferably in the range of 0.1 to 10 parts by mass, and more preferably in the range of 0.5 to 5 parts by mass, based on 100 parts by mass of the solid content in the brilliant pigment dispersion.
[0130] As viscosity modifiers other than the nanocellulose (C), polyacrylic acid-based viscosity modifiers, polyamide-based viscosity modifiers, mineral-based viscosity modifiers, cellulose-based viscosity modifiers (excluding nanocellulose), polysaccharide-based viscosity modifiers, etc. can be used. Among these, it is preferable to use a polyacrylic acid-based viscosity modifier from the viewpoint of forming a coating film that does not wrinkle at the edge portion, which is likely to be thicker than the general portion, and does not sag at the vertical portion.
[0131] Examples of polyacrylic acid viscosity modifiers include sodium polyacrylate and polyacrylic acid-(meth)acrylic acid ester copolymers.
[0132] Commercially available polyacrylic acid viscosity modifiers include, for example, "Primal ASE-60," "Primal TT615," and "Primal RM5" (all trade names) manufactured by The Dow Chemical Company, and "SN Thickener 613," "SN Thickener 618," "SN Thickener 630," "SN Thickener 634," and "SN Thickener 636" (all trade names) manufactured by San Nopco Ltd. The acid value of the solid content of the polyacrylic acid viscosity modifier is preferably in the range of 30 to 300 mgKOH / g, more preferably 80 to 280 mgKOH / g.
[0133] Examples of polyamide viscosity modifiers include polyamide amine salts and fatty acid polyamides.
[0134] Examples of mineral viscosity modifiers include swellable layered silicates having a 2:1 crystal structure. Specific examples include smectite clay minerals such as natural or synthetic montmorillonite, saponite, hectorite, stevensite, beidellite, nontronite, bentonite, and laponite, swellable mica clay minerals such as Na-type tetrasilicic fluorine mica, Li-type tetrasilicic fluorine mica, Na-salt-type fluorine taeniolite, and Li-type fluorine taeniolite, and vermiculite, as well as substitution products, derivatives, and mixtures thereof.
[0135] Examples of cellulose-based viscosity modifiers (excluding nanocellulose) include carboxymethyl cellulose, methyl cellulose, hydroxyethyl cellulose, hydroxyethyl methyl cellulose, and hydroxypropyl methyl cellulose.
[0136] Examples of polysaccharide viscosity adjusters include guar gum, xanthan gum, and locust bean gum.
[0137] When the brilliant pigment dispersion of the present invention contains a viscosity modifier other than the nanocellulose (C), the content thereof is preferably in the range of 1 to 30 parts by mass, more preferably in the range of 3 to 20 parts by mass, based on 100 parts by mass of the solid content in the brilliant pigment dispersion.
[0138] When the bright pigment dispersion contains the above-mentioned aqueous resin dispersion, the crosslinkable component is a component for crosslinking and curing the dispersion by heating. When the bright pigment dispersion does not contain the above-mentioned aqueous resin dispersion, the crosslinkable component may be a component for self-crosslinking or a component for crosslinking and curing with a part of the colored coating material that forms the colored coating film described below or a part of the clear coating material that forms the clear coating film described below. Examples of crosslinkable components include amino resins, urea resins, polyisocyanate compounds, blocked polyisocyanate compounds, epoxy group-containing compounds, carboxyl group-containing compounds, carbodiimide group-containing compounds, hydrazide group-containing compounds, semicarbazide group-containing compounds, and silane coupling agents. Among these, amino resins, polyisocyanate compounds, and blocked polyisocyanate compounds that can react with hydroxyl groups, and carbodiimide group-containing compounds that can react with carboxyl groups are preferred. Regarding the polyisocyanate compounds and blocked polyisocyanate compounds, those described in the section on clear coating materials below can be used. The above-mentioned crosslinkable components can be used alone or in combination of two or more.
[0139] When the bright pigment dispersion of the present invention contains the above-mentioned crosslinkable component, from the viewpoint of the water resistance of the resulting coating film and the like, the content of the crosslinkable component is preferably within a range of 0.5 to 100 parts by mass, more preferably within a range of 1 to 95 parts by mass, and even more preferably within a range of 2 to 90 parts by mass, in terms of solid content, based on 100 parts by mass of the content of the bright pigment (B) in the bright pigment dispersion of the present invention.
[0140] When the bright pigment dispersion of the present invention contains the binder resin and / or crosslinkable component, the total content of the binder resin and crosslinkable component is, from the viewpoint of the metallic or pearlescent luster and water-resistant adhesion of the resulting coating film, preferably in the range of 1 to 200 parts by mass, more preferably in the range of 2 to 150 parts by mass, and even more preferably in the range of 3 to 100 parts by mass, in terms of solid content, based on 100 parts by mass of the solid content of the bright pigment (B) in the bright pigment dispersion.
[0141] Viscosity The brilliant pigment dispersion of the present invention has an excellent metallic or pearlescent metallic or pearlescent luster, and from the viewpoint of forming a coating film that is free from wrinkles at edge portions where the film thickness tends to be thicker than in general portions and free from sagging in vertical portions, the viscosity at a rotation speed of 6 revolutions per minute (6 rpm) is preferably within the range of 400 to 10,000 mPa sec, more preferably within the range of 500 to 8,000 mPa sec, and even more preferably within the range of 600 to 6,000 mPa sec.
[0142] The viscosity is defined as the viscosity one minute after the start of measurement under certain conditions. Specifically, the prepared bright pigment dispersion is placed in a specified container, and a rotary mixer is used to set the rotation speed to 1,000 rpm and stir and mix until uniform. Measurement is then started at a temperature of 20°C using a Brookfield type viscometer at 6 rpm, and the viscosity is defined as the viscosity one minute after the start (also referred to as the "B6 value" in this specification). The viscometer used here is an "LVDV-I" (trade name, Brookfield, Brookfield type viscometer). A rotation speed of 6 rpm is a common condition for controlling the viscosity of a pseudoplastic liquid.
[0143] Method for forming multilayer coating films The method for forming multilayer coating films of the present invention comprises: step (1): applying a base paint (X) onto an object to be coated to form an uncured base coating film; step (2): applying the glitter pigment dispersion of the present invention onto the base coating film formed in step (1) to form an uncured glitter coating film; step (3): applying an uncured clear paint (Z) onto the glitter coating film formed in step (2) to form a clear coating film; and step (4): simultaneously heating the uncured base coating film formed in step (1), the uncured glitter coating film formed in step (2), and the uncured clear coating film formed in step (3), thereby curing them.
[0144] Substrate The multilayer coating film of the present invention is formed on the substrate shown below.
[0145] Examples of substrates include metal materials such as metals such as iron, zinc, and aluminum, and alloys containing these metals, as well as molded articles made of these metals, and molded articles and films made of glass, plastic, foam, etc. These substrates can be prepared by degreasing or surface treatment as appropriate depending on the material. Examples of such surface treatments include phosphate treatment, chromate treatment, and complex oxide treatment. Furthermore, if the substrate is made of metal, it is preferable that a primer coating film is formed on the surface-treated metal material using a cationic electrodeposition paint or the like. Furthermore, if the substrate is made of plastic, it is preferable that a primer coating film is formed on the degreased plastic material using a primer paint.
[0146] Base Coating (X) As the base coating (X), specifically, a known thermosetting coating composition containing a base resin, a crosslinking agent, a pigment, and a solvent such as an organic solvent and / or water as main components can be used.
[0147] The base resin used in the base coating material (X) may be a thermosetting resin, a room temperature curing resin, or the like, but from the viewpoints of water resistance, chemical resistance, weather resistance, etc., a thermosetting resin is preferred.
[0148] The base resin is preferably a resin having good weather resistance and transparency, and specific examples thereof include acrylic resin, polyester resin, epoxy resin, and urethane resin.
[0149] Examples of the acrylic resin include resins obtained by copolymerizing α,β-ethylenically unsaturated carboxylic acid, (meth)acrylic acid esters having functional groups such as hydroxyl groups, amide groups, methylol groups, and epoxy groups, other (meth)acrylic acid esters, styrene, and the like.
[0150] Examples of polyester resins include polyester resins obtained by a condensation reaction between a polyhydric alcohol such as ethylene glycol, propylene glycol, butylene glycol, 1,6-hexanediol, trimethylolpropane, or pentaerythritol and a polycarboxylic acid component such as adipic acid, isophthalic acid, terephthalic acid, phthalic anhydride, hexahydrophthalic anhydride, or trimellitic anhydride.
[0151] The epoxy resin may be, for example, a so-called bisphenol A type epoxy resin, which is produced by a condensation reaction between bisphenol A and epichlorohydrin.
[0152] Examples of urethane resins include compounds obtained by an addition reaction between a diisocyanate compound and a polyhydric alcohol, and polymerized resins obtained by reacting the above-mentioned acrylic resins, polyester resins, or epoxy resins with a diisocyanate compound.
[0153] The base coating material (X) may be either an aqueous coating material or a solvent-based coating material, but from the viewpoint of reducing VOC emissions, an aqueous coating material is preferable. When the base coating material (X) is an aqueous coating material, the base resin contains a sufficient amount of hydrophilic groups, such as carboxyl groups, hydroxyl groups, methylol groups, amino groups, sulfonic acid groups, polyoxyethylene bonds, etc., most commonly carboxyl groups, to render the resin water-soluble or water-dispersible. The base resin can be rendered water-soluble or water-dispersible by neutralizing the hydrophilic groups to form alkali salts. The amount of hydrophilic groups, such as carboxyl groups, is not particularly limited and can be selected as desired depending on the degree of water solubility or water dispersion, but is generally about 10 mg KOH / g or more, preferably within the range of 30 to 200 mg KOH / g, based on the acid value. Examples of alkaline substances used for neutralization include sodium hydroxide and amine compounds.
[0154] The resin can also be dispersed in water by emulsion polymerization of the polymerizable component in the presence of a surfactant or a water-soluble resin. Furthermore, the resin can also be dispersed in water in the presence of an emulsifier. In this case, the base resin may contain no hydrophilic groups or may contain less hydrophilic groups than the water-soluble resin.
[0155] The crosslinking agent is used to crosslink and cure the base resin by heating, and any of the crosslinking components exemplified in the description of the bright pigment dispersion of the present invention can be used.
[0156] The proportions of the above components in the base coating material (X) can be selected arbitrarily as required, but from the viewpoints of water resistance, finish, etc., it is generally preferred that the base resin and crosslinking agent be within the ranges of 60 to 90% by mass, particularly 70 to 85% by mass, and the latter 10 to 40% by mass, particularly 15 to 30% by mass, based on the total mass of the two components.
[0157] The pigment imparts luster, color, and base hiding properties to the base coating film formed from the base paint (X). The type and amount of the pigment can be adjusted appropriately depending on the hue or brightness desired for the multilayer coating film.
[0158] Examples of the pigment include luster pigments, color pigments, and extender pigments.
[0159] The cured film thickness of the base coating film obtained from the base paint (X) is preferably in the range of 3 μm to 50 μm, more preferably in the range of 5 to 45 μm, and even more preferably in the range of 7 to 40 μm, from the viewpoints of the hiding power of the base and the metallic or pearlescent luster of the multilayer coating film.
[0160] The base paint (X) can be applied according to a conventional method. When the base paint (X) is an aqueous paint, for example, deionized water and, if necessary, additives such as a thickener and an antifoaming agent are added to the base paint (X) to adjust the solids content to about 10 to 70% by mass and the viscosity to 500 to 6,000 cps / 6 rpm (B-type viscometer), and then the surface of the substrate can be sprayed, rotary atomized, or the like. In particular, from the viewpoint of forming a multilayer coating film that does not cause wrinkles at the edge portions, which tend to be thicker than the general portions, it is preferable to set the solids content within the range of 10 to 20% by mass. Electrostatic application can also be performed during application, if necessary.
[0161] From the viewpoint of color stability, etc., the base paint (X) preferably has a black-and-white hiding film thickness of 80 μm or less, more preferably 10 to 60 μm, and even more preferably 15 to 50 μm. In this specification, the "black-and-white hiding film thickness" refers to a value measured with an electromagnetic film thickness meter when a black-and-white checkerboard pattern hiding rate test paper specified in 4.1.2 of JIS K5600-4-1 is attached to a steel plate, the paint is applied at an angle so that the film thickness changes continuously, and after drying or curing, the coated surface is visually observed under diffused daylight, and the minimum film thickness at which the black-and-white boundary of the checkerboard pattern on the hiding rate test paper is no longer visible.
[0162] When the bright pigment dispersion of the present invention is applied onto an uncured base coating film of the base coating material (X), after application of the base coating material (X), the base coating material (X) can be left to stand at room temperature for 15 to 30 minutes, or heated at a temperature of 50 to 100°C for 30 seconds to 10 minutes, and then the bright pigment dispersion of the present invention can be applied.
[0163] Coating of the glitter pigment dispersion (Y) The glitter pigment dispersion (Y) of the present invention can be coated by electrostatic coating, air spray, airless spray, etc. These coating methods may be electrostatically applied as needed. In the method for forming a multilayer coating film of the present invention, rotary atomization electrostatic coating is particularly preferred.
[0164] The dry thickness of the glitter coating film is preferably 0.025 to 3 μm, more preferably 0.15 to 2.5 μm.
[0165] After applying the above-mentioned glitter pigment dispersion (Y), the coating may be left at room temperature for 15 to 30 minutes, or may be heated at a temperature of 50 to 100°C for 30 seconds to 10 minutes, and then the clear coating material (Z) may be applied.
[0166] Clear Coating (Z) Any known thermosetting clear coating composition can be used as the clear coating (Z). Examples of such thermosetting clear coating compositions include organic solvent-based thermosetting coating compositions containing a base resin having a crosslinkable functional group and a curing agent, aqueous thermosetting coating compositions, and powder thermosetting coating compositions.
[0167] Examples of crosslinkable functional groups possessed by the base resin include carboxyl groups, hydroxyl groups, epoxy groups, silanol groups, etc. Types of base resins include acrylic resins, polyester resins, alkyd resins, urethane resins, epoxy resins, fluororesins, etc. Examples of curing agents include polyisocyanate compounds, blocked polyisocyanate compounds, melamine resins, urea resins, carboxyl group-containing compounds, carboxyl group-containing resins, epoxy group-containing resins, and epoxy group-containing compounds.
[0168] Preferred combinations of base resin / curing agent for the clear coating (Z) include carboxyl group-containing resin / epoxy group-containing resin, hydroxyl group-containing resin / polyisocyanate compound, hydroxyl group-containing resin / blocked polyisocyanate compound, and hydroxyl group-containing resin / melamine resin.
[0169] The clear coating (Z) may be a one-component coating, or may be a multi-component coating such as a two-component coating.
[0170] Of these, the clear coating (Z) is preferably a two-component clear coating containing the following hydroxyl group-containing resin and polyisocyanate compound, from the viewpoint of the adhesion of the resulting coating film.
[0171] Hydroxyl-containing resin Any conventionally known resin containing a hydroxyl group can be used without limitation. Examples of the hydroxyl-containing resin include hydroxyl-containing acrylic resins, hydroxyl-containing polyester resins, hydroxyl-containing polyether resins, and hydroxyl-containing polyurethane resins. Preferred examples include hydroxyl-containing acrylic resins and hydroxyl-containing polyester resins, and particularly preferred examples include hydroxyl-containing acrylic resins.
[0172] The hydroxyl value of the hydroxyl-containing acrylic resin is preferably in the range of 80 to 200 mgKOH / g, more preferably in the range of 100 to 180 mgKOH / g, from the viewpoint of the scratch resistance and water resistance of the coating film.
[0173] The weight average molecular weight of the hydroxyl group-containing acrylic resin is preferably in the range of 2,500 to 40,000, more preferably in the range of 5,000 to 30,000, from the viewpoint of the acid resistance and smoothness of the coating film.
[0174] In this specification, the weight average molecular weight is a value calculated from a chromatogram measured by gel permeation chromatography using the molecular weight of standard polystyrene as a reference. The gel permeation chromatograph used was "HLC8120GPC" (manufactured by Tosoh Corporation). Four columns, "TSKgel G-4000HXL," "TSKgel G-3000HXL," "TSKgel G-2500HXL," and "TSKgel G-2000HXL" (all manufactured by Tosoh Corporation, trade names), were used. The measurement was performed under the following conditions: mobile phase: tetrahydrofuran, measurement temperature: 40°C, flow rate: 1 cc / min, and detector: RI.
[0175] The glass transition temperature of the hydroxyl group-containing acrylic resin is preferably −40° C. to 20° C., and particularly preferably within the range of −30° C. to 10° C. If the glass transition temperature is −40° C. or higher, the coating film will have sufficient hardness, and if it is 20° C. or lower, the coating surface smoothness of the coating film can be maintained.
[0176] Polyisocyanate Compound The polyisocyanate compound is a compound having at least two isocyanate groups in one molecule, and examples thereof include aliphatic polyisocyanates, alicyclic polyisocyanates, araliphatic polyisocyanates, aromatic polyisocyanates, and derivatives of the polyisocyanates.
[0177] Examples of the aliphatic polyisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, dimer acid diisocyanate, methyl 2,6-diisocyanatohexanoate (common name: lysine diisocyanate), isocyanate); and aliphatic triisocyanates such as 2-isocyanatoethyl 2,6-diisocyanatohexanoate, 1,6-diisocyanato-3-isocyanatomethylhexane, 1,4,8-triisocyanatooctane, 1,6,11-triisocyanatoundecane, 1,8-diisocyanato-4-isocyanatomethyloctane, 1,3,6-triisocyanatohexane, and 2,5,7-trimethyl-1,8-diisocyanato-5-isocyanatomethyloctane.
[0178] Examples of the alicyclic polyisocyanate include 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), 4-methyl-1,3-cyclohexylene diisocyanate (common name: hydrogenated TDI), 2-methyl-1,3-cyclohexylene diisocyanate, alicyclic diisocyanates such as 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane (common name: hydrogenated xylylene diisocyanate) or mixtures thereof, methylenebis(4,1-cyclohexanediyl)diisocyanate (common name: hydrogenated MDI), and norbornane diisocyanate; 1,3,5-triisocyanatocyclohexane, 1,3,5-trimethylisocyanatocyclohexane, 2-(3-isocyanatopropyl)-2-isocyanatopropyl , 5-di(isocyanatomethyl)-bicyclo(2.2.1)heptane, 2-(3-isocyanatopropyl)-2,6-di(isocyanatomethyl)-bicyclo(2.2.1)heptane, 3-(3-isocyanatopropyl)-2,5-di(isocyanatomethyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 6-(2-isocyanatopropyl)-bicyclo(2.2.1)heptane
[0033] Examples of such alicyclic triisocyanates include alicyclic triisocyanates such as 2-isocyanatoethyl-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, and 6-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane.
[0179] Examples of the araliphatic polyisocyanate include araliphatic diisocyanates such as methylenebis(4,1-phenylene)diisocyanate (common name: MDI), 1,3- or 1,4-xylylene diisocyanate or a mixture thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene (common name: tetramethylxylylene diisocyanate) or a mixture thereof; and araliphatic triisocyanates such as 1,3,5-triisocyanatomethylbenzene.
[0180] Examples of the aromatic polyisocyanate include aromatic diisocyanates such as m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 2,4-tolylene diisocyanate (common name: 2,4-TDI) or 2,6-tolylene diisocyanate (common name: 2,6-TDI) or mixtures thereof, 4,4'-toluidine diisocyanate, and 4,4'-diphenyl ether diisocyanate; aromatic triisocyanates such as triphenylmethane-4,4',4''-triisocyanate, 1,3,5-triisocyanatobenzene, and 2,4,6-triisocyanatotoluene; and aromatic tetraisocyanates such as 4,4'-diphenylmethane-2,2',5,5'-tetraisocyanate.
[0181] Examples of the polyisocyanate derivatives include dimers, trimers, biurets, allophanates, uretdione, uretimine, isocyanurates, oxadiazinetrione, polymethylene polyphenyl polyisocyanate (crude MDI, polymeric MDI), crude TDI, etc. The polyisocyanate derivatives may be used alone or in combination of two or more.
[0182] The above polyisocyanates and derivatives thereof may be used alone or in combination of two or more kinds.
[0183] Among aliphatic diisocyanates, hexamethylene diisocyanate compounds and among alicyclic diisocyanates, 4,4'-methylenebis(cyclohexyl isocyanate) can be preferably used. Among these, derivatives of hexamethylene diisocyanate are particularly suitable from the viewpoints of adhesion, compatibility, etc.
[0184] The polyisocyanate compound may be a prepolymer obtained by reacting the polyisocyanate or a derivative thereof with a compound having an active hydrogen group, such as a hydroxyl group or an amino group, which is reactive with the polyisocyanate under conditions of an excess of isocyanate groups. Examples of the compound reactive with the polyisocyanate include polyhydric alcohols, low-molecular-weight polyester resins, amines, and water.
[0185] Furthermore, as the polyisocyanate compound, a blocked polyisocyanate compound, which is a compound in which the isocyanate group in the above polyisocyanate or its derivative is blocked with a blocking agent, can also be used.
[0186] Examples of the blocking agent include phenol-based agents such as phenol, cresol, xylenol, nitrophenol, ethylphenol, hydroxydiphenyl, butylphenol, isopropylphenol, nonylphenol, octylphenol, and methyl hydroxybenzoate; lactam-based agents such as ε-caprolactam, δ-valerolactam, γ-butyrolactam, and β-propiolactam; aliphatic alcohol-based agents such as methanol, ethanol, propyl alcohol, butyl alcohol, amyl alcohol, and lauryl alcohol; ether-based agents such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, and methoxymethanol; benzyl alcohol, glycolic acid, methyl glycolate, ethyl glycolate, butyl glycolate, lactic acid, methyl lactate, ethyl lactate, butyl lactate, methylol urea, methylol melamine, diacetone alcohol, 2-hydroxyethyl acrylate ... alcohol-based solvents such as methyloxyethyl methacrylate; oxime-based solvents such as formamide oxime, acetamide oxime, acetoxime, methyl ethyl ketoxime, diacetyl monooxime, benzophenone oxime, and cyclohexane oxime; active methylene-based solvents such as dimethyl malonate, diethyl malonate, ethyl acetoacetate, methyl acetoacetate, and acetylacetone; butyl mercaptan, t-butyl mercaptan, hexyl mercaptan, t-dodecyl mercaptan, 2-mercaptobenzothiazole, thiophenol, and methylthiophenol mercaptans such as ethylthiophenol; acid amides such as acetanilide, acetanisidide, acetotoluide, acrylamide, methacrylamide, acetic amide, stearic acid amide, and benzamide; imides such as succinimide, phthalic acid imide, and maleic acid imide; amines such as diphenylamine, phenylnaphthylamine, xylidine, N-phenylxylidine, carbazole, aniline, naphthylamine, butylamine, dibutylamine, and butylphenylamine; imidazoles such as imidazole and 2-ethylimidazole;Examples of the azole compounds include urea-based compounds such as urea, thiourea, ethyleneurea, ethylenethiourea, and diphenylurea; carbamate ester-based compounds such as N-phenylphenylcarbamate; imine-based compounds such as ethyleneimine and propyleneimine; sulfite-based compounds such as sodium bisulfite and potassium bisulfite; and azole-based compounds. Examples of the azole-based compounds include pyrazole or pyrazole derivatives such as pyrazole, 3,5-dimethylpyrazole, 3-methylpyrazole, 4-benzyl-3,5-dimethylpyrazole, 4-nitro-3,5-dimethylpyrazole, 4-bromo-3,5-dimethylpyrazole, and 3-methyl-5-phenylpyrazole; imidazole or imidazole derivatives such as imidazole, benzimidazole, 2-methylimidazole, 2-ethylimidazole, and 2-phenylimidazole; and imidazoline derivatives such as 2-methylimidazoline and 2-phenylimidazoline.
[0187] When blocking (reacting with a blocking agent), a solvent can be added as needed. The solvent used in the blocking reaction is preferably one that is not reactive with isocyanate groups, and examples thereof include ketones such as acetone and methyl ethyl ketone, esters such as ethyl acetate, and N-methyl-2-pyrrolidone (NMP).
[0188] The polyisocyanate compounds may be used either alone or in combination of two or more.
[0189] In the present invention, from the viewpoint of the curability and scratch resistance of the coating film, the equivalent ratio (OH / NCO) of the hydroxyl groups of the hydroxyl group-containing resin to the isocyanate groups of the polyisocyanate compound is preferably within the range of 0.5 to 2.0, more preferably 0.8 to 1.5.
[0190] When a two-component clear coating material containing a hydroxyl group-containing resin and a polyisocyanate compound is used as the clear coating material (Z), the hydroxyl group-containing resin and the polyisocyanate compound are preferably in a separated form from the standpoint of storage stability, and the two are preferably mixed together immediately before use to prepare the coating material.
[0191] A one-component paint may be used as the clear paint (Z). Examples of the combination of base resin / curing agent in a one-component paint include a carboxyl group-containing resin / epoxy group-containing resin, a hydroxyl group-containing resin / blocked polyisocyanate compound, and a hydroxyl group-containing resin / melamine resin.
[0192] The clear coating (Z) may further contain, as required, additives such as solvents such as water and organic solvents, curing catalysts, antifoaming agents, and ultraviolet absorbers.
[0193] A coloring pigment can be appropriately blended into the clear coating (Z) within a range that does not impair transparency. The coloring pigment can be one or a combination of two or more pigments conventionally known for use in inks and coatings. The amount of the pigment added can be determined appropriately, but is 30 parts by mass or less, preferably 0.01 to 10 parts by mass, per 100 parts by mass of the vehicle-forming resin composition in the clear coating.
[0194] The form of the clear coating (Z) is not particularly limited, but it is usually used as an organic solvent-based coating composition. In this case, the organic solvent used can be various organic solvents for coatings, such as aromatic or aliphatic hydrocarbon solvents; ester solvents; ketone solvents; ether solvents, etc. The organic solvent used can be the same as that used in preparing the hydroxyl group-containing resin, or can be added as needed.
[0195] The solid content of the clear coating (Z) is preferably about 30 to 70 mass %, more preferably about 40 to 60 mass %.
[0196] The above-mentioned clear coating material (Z) is applied onto the glossy coating film. The application of the clear coating material (Z) is not particularly limited and can be carried out by the same method as the application of the colored coating material (X), for example, by a coating method such as air spray, airless spray, rotary atomization coating, or curtain coating. These coating methods may employ electrostatic application as necessary. Of these, rotary atomization coating employing electrostatic application is preferred. The amount of application of the clear coating material (Z) is usually preferably an amount that results in a cured film thickness of about 10 to 50 μm.
[0197] Furthermore, when applying the clear coating material (Z), it is preferable to adjust the viscosity of the clear coating material (Z) appropriately using a solvent such as an organic solvent so that it falls within a viscosity range suitable for the coating method, for example, in rotary atomization coating using electrostatic application, it falls within a viscosity range of about 15 to 60 seconds when measured at 20°C using a Ford Cup No. 4 viscometer.
[0198] The method for forming a multilayer coating film of the present invention includes a step of simultaneously heating and curing the base coating film, the glitter coating film, and the clear coating film.
[0199] The heating can be carried out by known means, for example, a drying oven such as a hot air oven, an electric oven, or an infrared induction heating oven. The heating temperature is suitably in the range of 70 to 150°C, preferably 80 to 140°C. The heating time is not particularly limited, but is preferably in the range of 10 to 40 minutes, more preferably 20 to 30 minutes.
[0200] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these examples. Note that "parts" and "%" are all based on mass.
[0201] [1] Preparation of coated object A degreased and zinc phosphate-treated steel plate (JIS G3141, size 400 mm × 300 mm × 0.8 mm) was electrodeposited with the cationic electrodeposition paint "Elecron GT-10" (product name: manufactured by Kansai Paint Co., Ltd., which uses an epoxy resin polyamine-based cationic resin and a blocked polyisocyanate compound as a curing agent) so that the film thickness based on the cured coating was 20 μm, and the coating was heated at 170°C for 20 minutes to crosslink and cure, thereby forming an electrodeposition coating.
[0202] On the electrodeposition coated surface of the steel plate obtained, "TP-90 No. 8101 Gray" (product name, manufactured by Kansai Paint Co., Ltd., hydroxyl group / melamine and blocked isocyanate group curing type one-component organic solvent-based paint) was applied using an air spray so that the film thickness based on the cured film was 40 μm, and after leaving it for 7 minutes, it was heated at 140°C for 30 minutes to form an intermediate coating film, thereby obtaining a coated object.
[0203] [2] Preparation of Paint Preparation of Acrylic Resin Water Dispersion (R-1) Production Example 1 A reaction vessel equipped with a thermometer, thermostat, stirrer, reflux condenser, and dropping device was charged with 70.7 parts of deionized water and 0.52 parts of "Aqualon KH-10" (trade name, Dai-ichi Kogyo Seiyaku Co., Ltd., emulsifier, active ingredient 97%), stirred and mixed in a nitrogen stream, and heated to 80 ° C. Next, 1% of the total amount of the monomer emulsion described below and 5 parts of a 6% aqueous ammonium persulfate solution were introduced into the reaction vessel and maintained at 80 ° C. for 15 minutes. Thereafter, the remaining monomer emulsion was added dropwise over 3 hours to the reaction vessel maintained at the same temperature. After completion of the dropwise addition, the reaction vessel was allowed to age for 1 hour, and then cooled to 30 ° C. while gradually adding 40 parts of a 5% aqueous 2-(dimethylamino)ethanol solution. The mixture was then discharged while filtering through a 100-mesh nylon cloth, yielding an acrylic resin water dispersion (R-1) with a solids concentration of 45%. The resulting acrylic resin water dispersion (R-1) had a hydroxyl value of 43 mgKOH / g and an acid value of 12 mgKOH / g.
[0204] Monomer emulsion: 50 parts of deionized water, 10 parts of styrene, 40 parts of methyl methacrylate, 35 parts of ethyl acrylate, 3.5 parts of n-butyl methacrylate, 10 parts of 2-hydroxyethyl methacrylate, 1.5 parts of acrylic acid, 1.0 part of "Aqualon KH-10," and 0.03 parts of ammonium persulfate were mixed and stirred to obtain a monomer emulsion.
[0205] Preparation of Hydroxyl Group-Containing Polyester Resin Solution (R-2) Preparation Example 2 A reaction vessel equipped with a thermometer, thermostat, stirrer, reflux condenser, and water separator was charged with 174 parts of trimethylolpropane, 327 parts of neopentyl glycol, 352 parts of adipic acid, 109 parts of isophthalic acid, and 101 parts of 1,2-cyclohexanedicarboxylic anhydride. The temperature was raised from 160 ° C. to 230 ° C. over 3 hours, and the resulting condensed water was distilled off using a water separator while maintaining the temperature at 230 ° C. and reacting until the acid value reached 3 mg KOH / g or less. 59 parts of trimellitic anhydride was added to the reaction product, and an addition reaction was carried out at 170 ° C. for 30 minutes. The mixture was then cooled to 50 ° C. or below, and 2-(dimethylamino)ethanol was added in an amount equivalent to the acid groups to neutralize the mixture. Deionized water was then added gradually to obtain a hydroxyl group-containing polyester resin solution (R-2) with a solids concentration of 45%. The resulting hydroxyl group-containing polyester resin solution (R-2) had a hydroxyl value of 128 mgKOH / g, an acid value of 35 mgKOH / g, and a weight average molecular weight of 13,000.
[0206] Preparation of Phosphate Group-Containing Resin Solution (R-3) Preparation Example 3 A mixed solvent of 27.5 parts of methoxypropanol and 27.5 parts of isobutanol was placed in a reaction vessel equipped with a thermometer, thermostat, stirrer, reflux condenser, and dropping device and heated to 110°C. 121.5 parts of a mixture consisting of 25 parts of styrene, 27.5 parts of n-butyl methacrylate, 20 parts of "Isostearyl acrylate" (trade name, branched higher alkyl acrylate, manufactured by Osaka Organic Chemical Industry Ltd.), 7.5 parts of 4-hydroxybutyl acrylate, 15 parts of the following phosphoric acid group-containing polymerizable monomer, 12.5 parts of 2-methacryloyloxyethyl acid phosphate, 10 parts of isobutanol, and 4 parts of t-butyl peroxyoctanoate was added to the mixed solvent over 4 hours, and a mixture of 0.5 parts of t-butyl peroxyoctanoate and 20 parts of isopropanol was then added dropwise over 1 hour. The resulting solution was stirred for 1 hour to obtain a phosphate group-containing resin solution (R-3) with a solids concentration of 50%. The acid value of this resin due to the phosphate group was 83 mg KOH / g, the hydroxyl value was 29 mg KOH / g, and the weight average molecular weight was 10,000.
[0207] Phosphate group-containing polymerizable monomer: 57.5 parts of monobutyl phosphate and 41 parts of isobutanol were placed in a reaction vessel equipped with a thermometer, thermostat, stirrer, reflux condenser, and dropping device, and the mixture was heated to 90°C. 42.5 parts of glycidyl methacrylate was added dropwise over 2 hours, and the mixture was then stirred and aged for an additional 1 hour. 59 parts of isopropanol was then added to obtain a phosphate group-containing polymerizable monomer solution with a solids concentration of 50%. The acid value due to the phosphate group of the resulting monomer was 285 mgKOH / g.
[0208] Preparation of Color Pigment Dispersion (P-1) Preparation Example 4 56 parts (solids content 25 parts) of the hydroxyl group-containing polyester resin solution (R-2) obtained in Preparation Example 2, 1.5 parts of "RAVEN 5000 ULTRA III BEADS" (trade name, carbon black pigment, manufactured by COLUMBIAN CARBON CO.), and 5 parts of deionized water were mixed, and the pH was adjusted to 8.0 with 2-(dimethylamino)ethanol. Next, the resulting mixture was placed in a wide-mouth glass bottle, and glass beads with a diameter of approximately 1.3 mm were added as a dispersion medium, and the bottle was sealed. The mixture was then dispersed for 30 minutes using a paint shaker to obtain Color Pigment Dispersion (P-1).
[0209] Production of a brilliant pigment dispersion (P-2) Production Example 5 In a stirring and mixing vessel, 10.8 parts (solids content: 8 parts) of "GX-3100" (trade name, aluminum pigment paste, manufactured by Asahi Kasei Metals Corporation, metal content: 74%), 35 parts of 2-ethyl-1-hexanol, 8 parts (solids content: 4 parts) of the phosphate group-containing resin solution (R-3) obtained in Production Example 3, and 0.2 parts of 2-(dimethylamino)ethanol were mixed uniformly to obtain a brilliant pigment dispersion (P-2).
[0210] Production of base coating material (X) Production Example 6 62.5 parts of the pigment dispersion paste (P-1) obtained in Production Example 4, 54 parts of the glitter pigment dispersion liquid (P-2) obtained in Production Example 5, 44.4 parts (solid content 20 parts) of the acrylic resin aqueous dispersion (R-1) obtained in Production Example 1, 60 parts (solid content 21 parts) of "U-coat UX-8100" (trade name, urethane emulsion, manufactured by Sanyo Chemical Industries, Ltd., solid content 35%), and 37.5 parts (solid content 30 parts) of "Cymel 325" (trade name, melamine resin, manufactured by Nippon Cytec Industries Co., Ltd., solid content 80%) were uniformly mixed. Next, to the resulting mixture was added "UH-752" (trade name, thickener, manufactured by ADEKA Corporation), 2-(dimethylamino)ethanol, and deionized water to obtain a base coating material (X-1) having a pH of 8.0, a coating material solids content of 25%, and a viscosity of 3000 mPa s when measured at 20°C and 6 rpm using a Brookfield viscometer.
[0211] Production Example 7 62.5 parts of the pigment dispersion paste (P-1) obtained in Production Example 4, 54 parts of the glitter pigment dispersion liquid (P-2) obtained in Production Example 5, 44.4 parts (solid content 20 parts) of the acrylic resin aqueous dispersion (R-1) obtained in Production Example 1, 60 parts (solid content 21 parts) of "U-coat UX-8100" (trade name, urethane emulsion, manufactured by Sanyo Chemical Industries, Ltd., solid content 35%), and 37.5 parts (solid content 30 parts) of "Cymel 325" (trade name, melamine resin, manufactured by Nippon Cytec Industries Co., Ltd., solid content 80%) were uniformly mixed. Next, to the resulting mixture was added "UH-752" (trade name, thickener, manufactured by ADEKA Corporation), 2-(dimethylamino)ethanol, and deionized water to obtain a base coating material (X-2) having a pH of 8.0, a coating material solids content of 14%, and a viscosity of 3500 mPa s when measured at 20°C and 6 rpm using a Brookfield viscometer.
[0212] Preparation of Acrylic Resin Water Dispersion (R-4) Preparation Example 8 A reaction vessel equipped with a thermometer, thermostat, stirrer, reflux condenser, and dropping device was charged with 154 parts of deionized water and 0.52 parts of "Aqualon KH-10," and the mixture was stirred and mixed in a nitrogen stream and heated to 80°C. Next, 1% of the total amount of the monomer emulsion (1) described below and 5.3 parts of a 6% aqueous ammonium persulfate solution were introduced into the reaction vessel and maintained at 80°C for 15 minutes. Thereafter, the remaining monomer emulsion (1) was added dropwise over 3 hours to the reaction vessel maintained at the same temperature, and after completion of the addition, the reaction vessel was aged for 1 hour. Thereafter, the monomer emulsion (2) described below was added dropwise over 1 hour, and after aging for 1 hour, 40 parts of a 5% aqueous dimethylethanolamine solution was gradually added to the reaction vessel while cooling to 30°C. The mixture was then discharged while filtering through a 100-mesh nylon cloth, yielding an acrylic resin water dispersion (R-4) with a solids concentration of 28%. The resulting acrylic resin water dispersion (R-4) had a hydroxyl value of 25 mgKOH / g and an acid value of 33 mgKOH / g.
[0213] Monomer emulsion (1): 42 parts of deionized water, 0.72 parts of "Aqualon KH-10", 2.1 parts of methylenebisacrylamide, 2.8 parts of styrene, 16.1 parts of methyl methacrylate, 28 parts of ethyl acrylate, and 21 parts of n-butyl acrylate were mixed and stirred to obtain a monomer emulsion (1).
[0214] Monomer emulsion (2): A monomer emulsion (2) was obtained by mixing and stirring 18 parts of deionized water, 0.31 parts of "Aqualon KH-10", 0.03 parts of ammonium persulfate, 5.1 parts of methacrylic acid, 5.1 parts of 2-hydroxyethyl acrylate, 3 parts of styrene, 6 parts of methyl methacrylate, 1.8 parts of ethyl acrylate, and 9 parts of n-butyl acrylate.
[0215] Production of Acrylic Resin Solution (R-5) Production Example 9 A typical acrylic resin reaction vessel equipped with a stirrer, thermometer, and reflux condenser was charged with 48 parts of ethylene glycol monobutyl ether, heated and stirred, and maintained at 110 ° C. Into this, 10 parts of styrene, 40 parts of methyl methacrylate, 25 parts of n-butyl methacrylate, 10 parts of 2-hydroxyethyl methacrylate, 3 parts of methacrylic acid, 5 parts of N,N-dimethylaminoethyl methacrylate (solid content, dissolved in 10 parts of deionized water), 10 parts of "NF Bisomer PEM6E" (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., trade name, polyethylene glycol monomethacrylate, molecular weight approximately 350), 4 parts of azobisisobutyronitrile, and a mixture of 20 parts of isobutyl alcohol was added dropwise over 3 hours. After completion of the dropwise addition, the mixture was aged at 110 ° C. for 30 minutes, and then an additional catalyst mixture consisting of 25 parts of ethylene glycol monobutyl ether and 0.5 parts of azobisisobutyronitrile was added dropwise over 1 hour. The mixture was then aged at 110°C for 1 hour and then cooled to obtain an acrylic resin solution (R-5) with a solid content of 50%. The acrylic resin solution (R-5) had a hydroxyl value of 43 mgKOH / g and a weight average molecular weight of about 20,000.
[0216] Production of Color Pigment Dispersion (P-3) Production Example 10 10.2 parts (5.1 parts in terms of solids) of the acrylic resin solution (R-5) obtained in Production Example 9, 3 parts of "RAVEN 5000 ULTRA III BEADS" (trade name, carbon black pigment, manufactured by COLUMBIAN CARBON CO.), and 39.4 parts of deionized water were mixed and dispersed for 2 hours using a paint shaker to obtain a color pigment dispersion (P-3) with a solids content of 15.4%.
[0217] Production of Carboxyl Group-Containing Cellulose Nanofibers (C21) Production Example 11 5 g (bone dry) of bleached softwood-derived dissolving kraft pulp (Buckay DKP) was added to 500 ml of an aqueous solution containing 19.5 mg (0.025 mmol per 1 g of bone dry cellulose) of TEMPO (Sigma-Aldrich) and 514 mg (1.0 mmol per 1 g of bone dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. 8 ml of a 2 M aqueous solution of sodium hypochlorite was added to the reaction system, and the pH was adjusted to 10.3 with a 0.5 N aqueous solution of hydrochloric acid to initiate the oxidation reaction. During the reaction, the pH of the system decreased, but 3.0 N aqueous sodium hydroxide was added sequentially to adjust the pH to 10. After reacting for 2 hours, the mixture was filtered through a glass filter and thoroughly washed with water to obtain carboxylated cellulose. The amount of carboxyl groups in the resulting carboxylated cellulose was 0.94 mmol / g. Subsequently, hydrogen peroxide was added to a 5% (w / v) slurry of oxidized cellulose at 2% (w / v) relative to the oxidized cellulose, and the pH was adjusted to 12 with 1 M sodium hydroxide. This slurry was hydrolyzed at 80°C for 2 hours. This was then adjusted to 4.0% (w / v) with water and treated five times with an ultra-high-pressure homogenizer (20°C, 140 MPa) to obtain a carboxyl group-containing cellulose nanofiber dispersion (C21-1). The carboxyl group content of the carboxyl group-containing cellulose nanofiber dispersion (C21-1) was 0.94 mmol / g, the average fiber diameter was 6.9 nm, the average fiber length was 235 nm, and the aspect ratio was 34.
[0218] Production of Sulfonic Acid Group-Containing Cellulose Nanocrystals (C32) Production Example 12 To deionized water stirred with a magnetic stirrer, "Celluforce NCC" (trade name, manufactured by Celluforce Corporation, number average diameter of 2.3 to 4.5 nm, number average length of 44 to 108 nm, specific surface area of 400 m / g, sulfonic acid group-containing cellulose nanocrystals, solids concentration of 100%) was gradually added so as to give a solids concentration of 4%, and stirring was continued for 2 hours to obtain a sulfonic acid group-containing cellulose nanocrystal dispersion (C32-1).
[0219] Preparation of Glittering Pigment Dispersion Example 1 Into a stirring mixing vessel were added 4,830 parts of distilled water, 15 parts (15 parts solids) of "Dynol-604" (trade name, manufactured by Evonik Industries, acetylene diol-based surface conditioner, solids content 100%), 434.8 parts (200 parts solids) of "Alpaste EMR-B6360" (trade name, manufactured by Toyo Aluminum K.K., 46% solids, non-leafing aluminum flakes, average particle diameter D50: 10.3 μm, thickness: 0.19 μm, surface-silica-treated), 150 parts (3 parts solids) of a phosphate group-containing cellulose nanofiber dispersion (C11-1) (number average fiber diameter 4 nm, amount of phosphate group introduction 1.00 mmol / g, solids concentration 2.0%), 675 parts (27 parts solids) of the carboxyl group-containing cellulose nanofiber dispersion (C21-1) obtained in Production Example 11, and "Primal 118.9 parts (solids content 33.3 parts) of ASE-60 (trade name, manufactured by The Dow Chemical Company, polyacrylic acid-based viscosity modifier, 28% solids aqueous dispersion), 25 parts (solids content 10 parts) of "TINUVIN 479-DW(N)" (trade name, manufactured by BASF Corporation, ultraviolet absorber, 40% solids content), 13.2 parts (solids content 6.6 parts) of "TINUVIN 123-DW(N)" (trade name, manufactured by BASF Corporation, light stabilizer, 50% solids content), and 52.6 parts (solids content 8.1 parts) of the colored pigment dispersion (P-3) obtained in Production Example 10 were added and mixed with stirring to prepare a glittering pigment dispersion (Y-1). The solids content of the resulting glittering pigment dispersion (Y-1) was 4.8%, and the coating viscosity "B6 value" was 1100 mPa s.
[0220] Examples 2 to 10 and Comparative Examples 1 to 6 Bright pigment dispersions (Y-2) to (Y-16) were obtained in the same manner as in Example 1, except that the formulations shown in Table 1 were used.
[0221]
[0222]
[0223]
[0224] (*1) “Xirallic T61-10 Micro Silver”: trade name, manufactured by Merck, 100% solids, titanium oxide-coated alumina flake pigment, average particle size 11.8 μm.
[0225] Comparative Example 7 As the brilliant pigment dispersion (Y-17), a commercially available product "WBC-713T No. 1F7" (product name, manufactured by Kansai Paint Co., Ltd., acrylic melamine resin-based water-based base coat paint, silver paint color, solids content 23%, containing aluminum pigment, no nanocellulose (C)) was used.
[0226] Preparation of Clear Coating (Z) Clear Coating (Z-1) "KINO6510" (trade name: Kansai Paint Co., Ltd., hydroxyl group / isocyanate group curing type acrylic resin / urethane resin based two-component organic solvent type coating) was used as clear coating (Z-1).
[0227] Preparation of Test Plates (1) Preparation of Test Plates for Evaluating Wrinkles, 60° Specular Gloss (60° Gloss), and Flip-Flop Properties Example 11 Base paint (X-1) was electrostatically coated onto the substrate prepared in [1] above in a vertical position using a rotary atomization bell-type coater so that the cured film thickness was 9 μm, and the coating was left to stand for 2 minutes to form an uncured base coating film.
[0228] Next, the glitter pigment dispersion (Y-1) prepared in Example 1 was applied onto the uncured base coating film in a vertical position using a robot bell manufactured by ABB Co., Ltd., at a booth temperature of 23°C and a humidity of 68%, so that the dried coating film would have a thickness of 0.7 µm. After leaving it for 3 minutes, it was preheated in a vertical position at 80°C for 3 minutes to form a glitter coating film.
[0229] Next, a clear coating (Z-1) was applied vertically onto the uncured glossy coating film using a robot bell manufactured by ABB Co., Ltd., under conditions of a booth temperature of 23°C and a humidity of 68%, so that the film thickness of the dried coating film was 35 μm to form a clear coating film. After application, the sample was left at room temperature for 7 minutes, and then heated vertically at 140°C for 30 minutes in a hot air circulation drying oven to simultaneously dry the multi-layer coating film, and a test plate was prepared for evaluating wrinkles, 60° specular gloss (60° gloss), and flip-flop properties.
[0230] Here, the thickness of the dry coating film of the glitter coating film was calculated from the following formula. The same applies to the following examples: x = sc / sg / S * 10000, where x is the film thickness [μm], sc is the coating solid content [g], and sg is the coating specific gravity [g / cm3 ] S: Evaluation area of coating solids [cm 2 ]
[0231] Examples 12 to 21 and Comparative Examples 8 to 14 Test plates for evaluating wrinkles, 60° specular gloss (60° gloss), and flip-flop properties were obtained in the same manner as in Example 11, except that the paints, luster pigment dispersions, and film thicknesses shown in Table 2 were used.
[0232] (2) Preparation of test plate for evaluation of sagging in vertical portions Example 11 Seventeen punch holes, each 5 mm in diameter, were made in a row at 2 cm intervals on the substrate prepared in [1] above, 3 cm from the end of the long side. Each punch hole was made 10 cm away from the 400 mm long side.
[0233] Next, the test substrate was positioned so that the 400 mm side extended horizontally and the 300 mm side extended vertically, and base paint (X-1) was electrostatically applied onto the substrate in a vertical position using a rotary atomization bell-type coater to a cured film thickness of 9 μm, and the coating was left to stand for 2 minutes to form an uncured base coating film.
[0234] Next, the glitter pigment dispersion (Y-1) prepared in Example 1 was applied onto the uncured base coating film in a vertical position using a robot bell manufactured by ABB, under conditions of a booth temperature of 22°C and a humidity of 78%, with a film thickness gradient so as to obtain a dried coating film thickness of approximately 0.5 μm to 4 μm in the longitudinal direction, and the coating was left to stand for 3 minutes. Thereafter, the coating was preheated in a vertical position at 80°C for 3 minutes to form a glitter coating film.
[0235] Next, a clear coating (Z-1) was applied to the uncured glossy coating film in a vertical position using a robot bell manufactured by ABB Co., Ltd., under conditions of a booth temperature of 23°C and a humidity of 68% so that the film thickness of the dried coating film was 35 μm to form a clear coating film. After application, the plate was left at room temperature for 7 minutes, and then heated in a hot air circulation drying oven in a vertical position at 140°C for 30 minutes to simultaneously dry the multi-layer coating film, thereby obtaining a test plate for evaluating sagging in the vertical section.
[0236] Examples 12 to 21 and Comparative Examples 8 to 14 Test plates for evaluating sagging in vertical sections were obtained in the same manner as in Example 11, except that the paint, luster pigment dispersion, and film thickness shown in Table 2 were used.
[0237]
[0238]
[0239] Coating Film Evaluation Each test panel obtained as described above was evaluated for the following items, and the results are shown in Table 2.
[0240] Wrinkles The edge of each test plate was visually inspected and evaluated according to the following criteria. A and B are acceptable. A: No wrinkles observed, excellent coating appearance. B: Almost no wrinkles observed, excellent coating appearance. C: Considerable or significant wrinkles observed, poor coating appearance.
[0241] 60° Specular Gloss (60° Gloss) The 60° gloss value was measured using a gloss meter (micro-TRI-gloss, manufactured by BYK-Gardner). The higher the value, the better. In the examples and comparative examples using aluminum pigments, a value of 122 or more is considered acceptable, and in the examples and comparative examples using optical coherence pigments, a value of 97 or more is considered acceptable.
[0242] Flip-flop properties A multi-angle colorimeter (manufactured by BYK, product name: BYK-mac i) was used to measure the L* value at a light-receiving angle of 15 degrees (L*15 value) and the L* value at a light-receiving angle of 75 degrees (L*75 value), and the FF value of the coating film was calculated and evaluated using the following formula. In Examples and Comparative Examples using aluminum pigments, a value of 8.0 or more was considered acceptable, and in Examples and Comparative Examples using optical coherence pigments, a value of 2.8 or more was considered acceptable. FF value = L*15 value / L*75 value
[0243] For each test plate, the position where sagging of the coating film was observed 3 mm from the lower end of the punch hole was examined, and the film thickness at that position (sagging limit film thickness (μm)) was measured to evaluate sagging of the vertical portion. The larger the sagging limit film thickness, the better the result. A value of 4 μm or more is acceptable.
[0244] In Table 2, the "-" in the sagging limit film thickness for Comparative Example 14 indicates that no sagging occurred at a dry film thickness of 4 μm for the brilliant pigment dispersion (Y-1).
[0245] Although the embodiments and examples of the present invention have been specifically described above, the present invention is not limited to the above-described embodiments, and various modifications based on the technical concept of the present invention are possible.
Claims
1. A glittering pigment dispersion containing a wetting agent (A), a glittering pigment (B), nanocellulose (C) and water (D), wherein the glittering pigment dispersion contains 0.1 to 10 parts by mass of solids per 100 parts by mass of all components in total, and the nanocellulose (C) contains at least one type selected from the group consisting of phosphate group-containing nanocellulose (C1), carboxyl group-containing nanocellulose (C2) and sulfonic acid group-containing nanocellulose (C3).
2. The brilliant pigment dispersion according to claim 1, wherein the brilliant pigment (B) contains an aluminum pigment.
3. The brilliant pigment dispersion according to claim 1 or 2, wherein the phosphate group-containing nanocellulose (C1) comprises a phosphate group-containing cellulose nanofiber (C11) and / or a phosphate group-containing cellulose nanocrystal (C12).
4. The cellulose (C) comprises a carboxyl group-containing nanocellulose (C2), and the carboxyl group-containing nanocellulose (C2) comprises a carboxyl group-containing cellulose nanofiber (C21) and / or a carboxyl group-containing cellulose nanocrystal (C22). The brilliant pigment dispersion according to any one of claims 1 to 3.
5. The cellulose (C) comprises a sulfonic acid group-containing nanocellulose (C3), and the sulfonic acid group-containing nanocellulose (C3) comprises a sulfonic acid group-containing cellulose nanofiber (C31) and / or a sulfonic acid group-containing cellulose nanocrystal (C32). The brilliant pigment dispersion according to any one of claims 1 to 4.
6. The content ratio of the phosphate group-containing nanocellulose (C1) to at least one selected from the group consisting of carboxyl group-containing nanocellulose (C2) and sulfonic acid group-containing nanocellulose (C3) is in the range of 1 / 99 to 50 / 50, in terms of mass ratio of the phosphate group-containing nanocellulose (C1) to at least one selected from the group consisting of the carboxyl group-containing nanocellulose (C2) and the sulfonic acid group-containing nanocellulose (C3). The brilliant pigment dispersion according to any one of claims 1 to 5.
7. A method for forming a multilayer coating film, comprising: step (1): applying a base paint (X) onto a substrate to form an uncured base coating film; step (2): applying the glittering pigment dispersion (Y) described in any one of claims 1 to 6 onto the base coating film formed in step (1) to form an uncured glittering coating film; step (3): applying an uncured clear paint (Z) onto the glittering coating film formed in step (2) to form a clear coating film; and step (4): simultaneously heating the uncured base coating film formed in step (1), the uncured glittering coating film formed in step (2), and the uncured clear coating film formed in step (3) to cure them.
Citation Information
Patent Citations
Synthetic resin molded product
JP1988272544A
Aqueous coating composition and metallic laminated coating film and method for forming the same
JP2009155537A
Bright pigment dispersion and method for forming multilayer coating film
WO2017175468A1
Cosmetic or topical skin preparation containing 3-o-ethyl ascorbic acid
JP2023016083A
Cosmetic or topical skin preparation containing phospholipid
JP2023016084A